Negative electrode active material for secondary battery and method for producing same
By employing a two-solvent method to form a pitch coating film on nanosilicon and carbon-based materials, the method addresses the challenges of coating uniformity and density, enhancing the performance of negative electrode materials in secondary batteries.
Patent Information
- Application Number
- JP2024536013
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-22
- Filing Date
- 2022-12-09
- Publication Date
- 2024-11-28
- Estimated Expiration
- 2042-12-09
AI Technical Summary
Conventional methods for producing negative electrode materials for secondary batteries face challenges in achieving uniform and dense pitch coating films, leading to reduced initial discharge capacity, efficiency, and lifespan due to issues with solvent usage and physical damage to silicon structures during coating processes.
A method involving the use of two types of solvents to form a pitch coating film on composite materials containing nanosilicon and carbon-based conductive materials, followed by carbonization, to improve coating uniformity and density, resulting in improved negative electrode active materials.
The method enhances the initial discharge capacity, efficiency, and life characteristics of secondary batteries by ensuring a uniform and dense pitch coating film, thereby stabilizing the silicon structure.
Smart Images

Figure 2024544303000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a negative electrode active material for a secondary battery capable of improving the initial discharge capacity (IDC), initial efficiency (ICE) and life characteristics of the secondary battery, and a method for manufacturing the same. [Background technology]
[0002] In recent years, with the rapid spread of electronic devices that use batteries, such as mobile equipment and electric vehicles, the demand for secondary batteries that are small and lightweight yet have a relatively high capacity is increasing, and this trend is accelerating.
[0003] Graphite, a representative material widely used as an anode material for secondary batteries, has the advantages of excellent electrochemical performance (initial capacity) and low cost. However, with repeated charge-discharge cycles, the charge-discharge efficiency and charge capacity rapidly decrease, making it difficult to meet the demands of electronic devices that require high capacity.
[0004] On the other hand, inorganic materials such as silicon (Si), germanium (Ge), and antimony (Sb) have a high theoretical capacity. In particular, silicon has the advantage of a low potential difference with lithium ions. However, due to volume expansion that occurs during charge and discharge cycles, the secondary battery structure is damaged and there is a limit to its lifespan.
[0005] In order to overcome the above limitations, composite materials containing carbon materials and silicon have been used as the active material of negative electrode materials in recent years, but it is difficult to stably bind silicon.
[0006] For this reason, methods have been developed in which pitch is coated as a carbon material on nano silicon particles mixed with a conductive material, or a mixture of nano silicon and pitch is coated on the surface of graphite.
[0007] Meanwhile, typical conventional coating methods that can be used to form a pitch coating film or a coating film containing pitch and nanosilicon are a dry method using a solvent and a wet method using a single solvent.
[0008] First, the dry method involves grinding pitch to submicron size and then coating it using the energy generated by physical friction. However, due to the characteristics of pitch, it is difficult to grind it to submicron size, and the silicon structure is easily damaged during the process of physical friction. In addition, since pitch has a property of easily solidifying itself, there is a problem that the solidified pitch particles remain on the coating film without being coated, which deteriorates the coating property and the quality of the manufactured anode material.
[0009] Next, the wet method is a method in which pitch is dissolved in a solvent, mixed with a material to be coated, and then a condensation process is performed in which the solvent is vaporized under vacuum heating conditions to form a pitch coating film. However, the wet method has limitations in that if the amount of solvent is insufficient during the condensation process, the coating may become less uniform, which may degrade the quality of the manufactured anode material, and a denser coating may not be obtained.
[0010] Therefore, it is necessary to develop a method for producing a high-quality negative electrode active material for a secondary battery that can solve the above problems and improve the initial discharge capacity, initial efficiency, and life characteristics of the secondary battery. Summary of the Invention [Problem to be solved by the invention]
[0011] The present invention is intended to solve the above problems, and aims to provide a method for producing a negative electrode active material for a secondary battery, which can improve the uniformity and denseness of the pitch coating film by using two types of solvents when the negative electrode active material for a secondary battery is a composite material having a coating film containing pitch.
[0012] The present invention also provides a negative electrode material including the negative electrode active material for a secondary battery, and a secondary battery including the same, so that the initial discharge capacity, initial efficiency, and life characteristics of the secondary battery can be improved.
[0013] The object of the present invention is not limited to the object mentioned above, and other objects and advantages of the present invention not mentioned can be understood from the following description and can be more clearly understood from the embodiments of the present invention. In addition, it is easy to understand that the object and advantages of the present invention can be realized by the means and combinations thereof as set forth in the claims. [Means for solving the problem]
[0014] In order to achieve the above object, according to one aspect of the present invention, (a) mixing nanosilicon, a carbon-based conductive material and a resin matrix to prepare a mixed powder; (b) dissolving a high softening point pitch in a first solvent to produce a pitch solution; (c) adding the mixed powder to the pitch solution and stirring to prepare a dispersion solution containing nanosilicon, a carbon-based conductive material and pitch; (d) adding a second solvent to the dispersion solution to deposit pitch on the composite material including nanosilicon and a carbon-based conductive material to form a pitch coating film; (e) removing the first and second solvents to obtain a dry powder; and (f) carbonizing the dried powder to obtain a negative electrode active material in which a pitch coating film is formed on a composite material containing nanosilicon and amorphous carbon; wherein the first solvent is soluble in the high softening point pitch, the second solvent is insoluble in the high softening point pitch, and the first solvent and the second solvent are miscible with each other.
[0015] According to another aspect of the present invention, (a') dissolving a high softening point pitch in a first solvent to prepare a pitch solution, and then adding graphite to prepare a graphite-pitch solution; (b') separately from (a'), adding and dispersing nanosilicon in a second solvent to prepare a nanosilicon dispersion solution; (c') adding the nanosilicon dispersion solution to the graphite-pitch solution to prepare a mixed solution of graphite, pitch and nanosilicon; (d') further adding the second solvent to the mixed solution of the graphite, pitch and nanosilicon to deposit a mixture of nanosilicon and pitch on the graphite, thereby forming a coating film containing nanosilicon and pitch; (e') removing the first and second solvents to obtain a dry powder; (f') dry-milling the dry powder; and (g') carbonizing the pulverized dry powder to obtain a graphite-silicon-pitch composite as a negative electrode active material for a secondary battery having a structure of a graphite core and a nanosilicon-pitch shell surrounding the core; wherein the first solvent is soluble in the high softening point pitch, the second solvent is insoluble in the high softening point pitch, and the first solvent and the second solvent are miscible with each other.
[0016] According to yet another aspect of the present invention, there can be provided a negative electrode material for a secondary battery, comprising the negative electrode active material for a secondary battery produced according to the method for producing a negative electrode active material for a secondary battery, and a secondary battery including the same. Effect of the Invention
[0017] According to the method for producing a negative electrode active material for a secondary battery of the present invention, the pitch coating film is formed using two types of solvents, which has the effect of improving the uniformity and denseness of the pitch coating film.
[0018] More specifically, according to the method for producing a negative electrode active material for a secondary battery of the present invention, i) a structure in which a pitch coating film is formed on a composite material containing nanosilicon and amorphous carbon; or ii) a structure of a graphite core and a nanosilicon-pitch shell surrounding said core; In producing the negative electrode active material for a secondary battery having the above structure, the use of two types of solvents can improve the coating uniformity and denseness of the pitch coating film.
[0019] The negative electrode material for secondary batteries containing the negative electrode active material for secondary batteries of the present invention has the effect of improving the initial discharge capacity, initial efficiency and life characteristics of the secondary battery.
[0020] The above-mentioned effects and specific effects of the present invention will be described in conjunction with the following description of the preferred embodiment of the invention. [Brief description of the drawings]
[0021] [Figure 1] 1 is a photograph of a composite structure of nanosilicon-amorphous carbon-pitch, which is an anode active material prepared in Example 1 of the present invention, specifically, a SEM image of the surface of the composite structure magnified 5,000 times. [Diagram 2] 1 is a photograph of a composite structure of nanosilicon-amorphous carbon-pitch, which is an anode active material prepared in Example 1 of the present invention, specifically, a SEM image of a cross section of the composite structure magnified 50,000 times. [Diagram 3] 1 is a photograph of a composite structure of nanosilicon-amorphous carbon-pitch, which is an anode active material prepared in Example 1 of the present invention, specifically, a SEM image of a cross section of the composite structure magnified 50,000 times. [Figure 4] 1 is a cross-sectional photograph of a composite structure of graphite-nano silicon-pitch, which is an anode active material prepared in Example 2 of the present invention, specifically, a SEM image of a cross section with a scale bar of 20 μm. [Diagram 5]1 is a cross-sectional photograph of a composite structure of graphite-nano silicon-pitch, which is an anode active material prepared in Example 2 of the present invention, specifically, an EDS mapping image with a scale bar of 20 μm. [Figure 6] 3 is a cross-sectional photograph of a composite structure of graphite-nano silicon-pitch, which is an anode active material prepared in Example 2 of the present invention, specifically, a SEM image of a cross section with a scale bar of 5 μm. [Figure 7] 1 is a cross-sectional photograph of a composite structure of graphite-nano silicon-pitch, which is an anode active material prepared in Example 2 of the present invention, specifically, an EDS mapping image with a scale bar of 5 μm. [Figure 8] 1 is a cross-sectional photograph of a composite structure of graphite-nano silicon-pitch, which is a negative active material prepared in Comparative Example 1 of the present invention, specifically, a SEM image of a cross section with a scale bar of 50 μm. [Figure 9] 1 is a cross-sectional photograph of a composite structure of graphite-nano silicon-pitch, which is an anode active material prepared in Comparative Example 1 of the present invention, specifically, an EDS mapping image with a scale bar of 50 μm. [Figure 10] FIG. 1 is a graph showing floating results of 50 charge / discharge cycles in the evaluation of battery life for half cells prepared using the negative electrode active materials of Examples 1 and 2 of the present invention and Comparative Example 1, in which the horizontal axis represents the number of cycles and the vertical axis represents the discharge capacity (unit: mah / g).
[0022] The dotted or solid circles used to designate specific objects in the black and white photographs in the drawings of this specification are merely illustrative of parts of the specific objects and should not be construed as being limited to the parts represented by the dotted or solid circles. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] The above-mentioned objects, features and advantages will be described in detail with reference to the accompanying drawings, so that those skilled in the art to which the present invention pertains can easily implement the technical idea of the present invention. In describing the present invention, if a detailed description of the known technology according to the present invention is deemed to make the gist of the present invention unclear, the detailed description will be omitted. The terms described below are terms described in consideration of the functions and actions of the present invention, and the meaning of each term should be interpreted based on the overall content of this specification.
[0024] In describing this specification, if a specific description of related publicly known technology is deemed to obscure the gist of this specification, the detailed description will be omitted.
[0025] In this specification, the term "pitch coating film" can be interpreted as referring to both a coating film made of a material consisting of only pitch and a coating film made of a material containing pitch and other components (e.g., nanosilicon), unless otherwise specified.
[0026] When the components in this specification are described as "comprising," "having," "consisting," "disposed," etc., other parts can be added as long as "only" is not used. When a component is expressed in the singular, it includes the plural unless otherwise expressly specified.
[0027] In interpreting the components in this specification, unless otherwise expressly stated, they are interpreted as including a margin of error.
[0028] The method for producing the negative electrode active material for a secondary battery according to the present invention will be described in detail below.
[0029] The negative electrode active material produced according to the method for producing a negative electrode active material for a secondary battery of the present invention is i) A "nano silicon-amorphous carbon-pitch composite structure" having a structure in which a pitch coating film is formed on an amorphous carbon-silicon composite; or ii) A "graphite-nano silicon-pitch composite structure" having a graphite core and a nano silicon-pitch shell surrounding the core.
[0030] Therefore, the composite structure, which is the negative electrode active material for a secondary battery finally produced in the present invention, may have technical commonality in that (1) it has a pitch coating film and (2) two types of solvents are used to increase the density and coatability of the pitch coating film.
[0031] In the conventional wet method, pitch is dissolved and precipitated using one type of solvent, so a uniform coating film cannot be obtained. Therefore, the present inventors have conducted extensive research and found that the uniformity and density of the pitch coating film of the above structure i) or ii) is significantly improved by first dissolving pitch in a solvent (first solvent) that is soluble in pitch, and then forming a pitch coating film on an amorphous carbon-silicon composite material, or by adding a solvent (second solvent) that is insoluble in pitch to form a silicon-pitch shell on a graphite core, and then precipitating pitch, thereby completing the present invention.
[0032] According to one aspect of the present invention, a method for producing a negative electrode active material for a secondary battery can be produced, which is a "nano-silicon-amorphous carbon-pitch composite structure" having a structure in which a pitch coating film is formed on an amorphous carbon-silicon composite material.
[0033] The above manufacturing method includes: (a) mixing nanosilicon, a carbon-based conductive material and a resin matrix to prepare a mixed powder; (b) dissolving a high softening point pitch in a first solvent to produce a pitch solution; (c) adding the mixed powder to the pitch solution and stirring to prepare a dispersion solution containing nanosilicon, a carbon-based conductive material and pitch; (d) adding a second solvent to the dispersion solution to deposit pitch on the composite material including nanosilicon and a carbon-based conductive material to form a pitch coating film; (e) removing the first and second solvents to obtain a dry powder; and (f) carbonizing the dried powder to obtain a negative active material having a pitch coating film formed on a composite material including nanosilicon and amorphous carbon.
[0034] The nanosilicon in step (a) may be in the form of nanosilicon particles commonly used in the present technical field, and for example, the (average) diameter is preferably within the range of 20 to 400 nm, but is not necessarily limited thereto.
[0035] The carbon-based conductive material in step (a) is mixed with the nanosilicon particles and may be included to impart electrical conductivity to the negative electrode active material. The carbon-based conductive material is preferably a carbon-based material that has electrical conductivity without causing a chemical change, and more preferably includes carbon black.
[0036] When the carbon-based conductive material undergoes the carbonization process in step (f), it changes into the form of amorphous carbon, and finally forms an amorphous carbon-silicon composite material.
[0037] The resin matrix in step (a) is included for the purpose of better bonding the carbon-based conductive material and the nanosilicon particles to each other, and may be an organic or aqueous resin matrix. For example, the resin matrix may include phenolic resin, epoxy resin, thermosetting polyimide, polyester, polyurethane, melamine resin, amino resin, dextrin resin, etc., and may include phenolic resin.
[0038] The resin matrix is also removed together with the carbon-based conductive material in the carbonization process (f), so that little or no resin matrix remains in the final negative electrode active material.
[0039] Based on 100 parts by weight of the mixed powder in step (a), the nanosilicon is preferably contained in an amount of 40 to 99 parts by weight, more preferably in an amount of 60 to 95 parts by weight, and most preferably in an amount of 70 to 90 parts by weight, but is not limited thereto, and the content may be appropriately adjusted depending on the properties of the final negative electrode active material.
[0040] Meanwhile, according to a method for producing a negative electrode active material for a secondary battery according to another aspect of the present invention, it is possible to produce a negative electrode active material for a secondary battery, which is a "nano-silicon-amorphous carbon-pitch composite structure" having a structure in which a pitch coating film is formed on an amorphous carbon-silicon composite material.
[0041] The above-mentioned manufacturing method includes: (a') dissolving a high softening point pitch in a first solvent to prepare a pitch solution, and then adding graphite to prepare a graphite-pitch solution; (b') separately from the step (a'), adding and dispersing nanosilicon in a second solvent to prepare a nanosilicon dispersion solution; (c') adding the nanosilicon dispersion solution to the graphite-pitch solution to prepare a mixed solution of graphite, pitch and nanosilicon; (d') further adding the second solvent to the mixed solution of the graphite, pitch and nanosilicon to deposit a mixture of nanosilicon and pitch on the graphite, thereby forming a coating film containing nanosilicon and pitch; (e') removing the first and second solvents to obtain a dry powder; (f') dry-milling the dry powder; and (g') carbonizing the pulverized dry powder to obtain a negative electrode active material for a secondary battery having a structure of a graphite core and a nanosilicon-pitch shell surrounding the core.
[0042] The first solvent may be selected from those that are soluble in the high softening point pitch. For example, the first solvent may include one or more selected from the group consisting of tetrahydrofuran (THF), quinoline, toluene, pyridine, N-methylpyrrolidone (NMP), xylene, chloroform, dimethylsulfoxide, and n-hexane, and is preferably, but not limited to, tetrahydrofuran (THF).
[0043] The second solvent may be selected from those that are insoluble in the high softening point pitch. For example, the second solvent may be one or more selected from the group consisting of ethanol, methanol, acetone, and water, and is preferably, but not limited to, ethanol.
[0044] In addition, in the method for producing a graphite-silicon-pitch composite material of the present invention, since the high softening point pitch dissolved in the first solvent is precipitated by using the second solvent, it is preferable that the first solvent and the second solvent are miscible with each other.
[0045] When steps (a) to (d) or (a') to (d') of the present invention are performed, pitch is deposited on the graphite-silicon composite to form a pitch coating film, or a mixture of silicon and pitch is deposited on graphite to form a coating film. Thereafter, the first and second solvents used in steps (a) to (d) or (a') to (d') are removed to obtain a final graphite-silicon-pitch composite, and step (e) or (e') of obtaining a dry powder can be performed. In step (e) or (e'), the first and second solvents can be vaporized and removed.
[0046] Step (e) or (e') of the present invention may include a primary vaporization step carried out under conditions of a pressure of 0.5 to 1 bar and a temperature of 25 to 40°C; and a secondary vaporization step carried out under conditions of a pressure of 0.5 to 1 bar and a temperature higher than the boiling points of the first and second solvents; however, the operating conditions are not necessarily limited to the pressure and temperature mentioned above.
[0047] For example, when THF is used as the first solvent and ethanol is used as the second solvent, the solvents can be removed by evaporation at a temperature of about 60°C.
[0048] For example, taking into consideration the boiling points of common solvents, a preferred temperature range for the secondary vaporization step may be 40 to 70° C., but is not limited thereto.
[0049] The time for performing the first and second vaporization steps may be appropriately adjusted depending on the amount of the negative active material to be finally prepared.
[0050] The first and second solvents can be dried at a time at a temperature higher than the boiling point to vaporize them. However, since nanosilicon and high softening point pitch are mixed in the first and second solvents, a first vaporization step at room temperature or a temperature slightly higher than room temperature and a second vaporization step at a temperature higher than the boiling point of the solvents may be sequentially performed to remove only the solvent, thereby improving the selectivity of removing the solvent.
[0051] The pitch used as the coating material for the negative electrode material for secondary batteries in the present invention is a high softening point pitch, and for example, the softening point of the pitch of the present invention is preferably 100°C or higher, more preferably 200°C or higher, and most preferably 200 to 300°C. High softening point pitch contains a component with a high boiling point, has excellent crystallinity and high stability, and therefore, when applied to the negative electrode material of secondary batteries, it has the advantage of improving the charge and discharge efficiency of the secondary battery, improving the charge density, and increasing the battery life. In addition, since the high softening point pitch in the present invention is for forming a coating film, it is preferable to select a pitch with a low quinoline insoluble (QI) and a high coking value (CV) related to the carbonization yield, and the specific QI and CV values may vary depending on the selection of the solvent for producing the pitch solution. For example, when tetrahydrofuran (THF) is used as the first solvent to produce a pitch solution as described below, it is preferred that the QI is 0.2% or less and the CV is 58% or more, although this is not necessarily limited thereto.
[0052] In the method for producing the negative active material of the amorphous carbon-nanosilicon-pitch composite structure having the above-mentioned "i) structure", after the step (e), a step (f) of carbonizing the dried powder may be performed.
[0053] Amorphous carbon-nano silicon composite is a micro-sized spherical particle having pores, and when it is pitch-coated, not only is the pitch partially inserted between the pores, but also during the carbonization process, the pitch is further inserted between the pores in the melting section, so there is no need to further process the surface of the particles after coating, and therefore a carbonization process is immediately adopted.
[0054] For example, the carbonization can be carried out in an inert gas atmosphere (e.g., nitrogen atmosphere) by increasing the temperature to 1000 to 1100° C. and maintaining the temperature for about 1 hour, and at this time, the rate of temperature increase may be, for example, 5 to 10° C. If the carbonization temperature is increased, the effect of removing hydrogen, oxygen, etc. from the organic resin is further increased, but if the temperature exceeds 1100° C., there is a problem that SiC is formed, so carbonization at a temperature of 1000 to 1100° C. is preferable.
[0055] In the method for producing a negative electrode active material having a graphite-nano silicon-pitch composite structure having the above-mentioned "ii) structure", after step (e') of the present invention, a step of dry-grinding the dried powder to obtain a graphite-silicon-pitch composite having a structure of a graphite core and a silicon-pitch shell surrounding the core may be performed.
[0056] When the formation of the coating film using the two solutions is completed, the graphite-nano silicon-pitch composite structure is merely precipitated on the graphite surface, and since the precipitated nano silicon-pitch composite is easily separated, further steps are required to form a complete coating film, i.e., a shell.
[0057] Therefore, in order to make the hard core (graphite)-shell (nano silicon-pitch) structure denser and harder, further processing steps such as dry grinding are performed. The grinding method in step (f') of the present invention can be performed using various known methods, preferably, but not limited to, a mechanofusion mixer.
[0058] After step (f') of the present invention, the pulverized dry powder can be carbonized to obtain a negative electrode active material having a structure of a graphite core and a nanosilicon-pitch shell surrounding the core, and the carbonization is the same as that described in the above structure i).
[0059] The present invention will be described in more detail below with reference to examples and experimental examples. However, the following examples and experimental examples are merely illustrative of the present invention, and the content of the present invention is not limited to the following examples and experimental examples.
[0060] 1. Preparation of graphite-silicon-pitch composite [Example 1] (1) Carbon black (Imerys Graphite & Carbon, Super-P product) as a carbon-based conductive material, resol-type phenolic resin (Konan Kasei, KC-4300N) as a resin matrix, and nanosilicon particles (D 50 Average value of 111 nm, D 90 The powder was mixed with the above-mentioned components in a weight ratio of 5:5:90, based on the weight after carbonization, and then spray-dried to obtain 7 g of amorphous carbon-silicon composite powder ([a]).
[0061] (2) 2 g of high softening point pitch (softening point: 260°C) was dissolved in 300 ml of tetrahydrofuran ([b]).
[0062] (3) The above [a] was added to the above [b], and then dispersed using a stirrer ([c]).
[0063] (4) 100 ml of ethanol was gradually added to the above [c] to precipitate pitch on the surface ([d]).
[0064] (5) Tetrahydrofuran was primarily vaporized from the above [d] under the conditions of pressure, temperature and time (0.7 bar, 35°C and 20 minutes).
[0065] (6) Tetrahydrofuran and ethanol were completely evaporated under the conditions of pressure, temperature and time (0.7 bar, 60° C. and 20 minutes) to obtain a dry powder.
[0066] (7) The dried powder was carbonized at 1000°C for 60 minutes in a nitrogen atmosphere to obtain a nanosilicon-amorphous carbon-pitch composite structure.
[0067] [Example 2] (1') 5 g of high softening point pitch was dissolved in 300 ml of tetrahydrofuran ([a]').
[0068] (2') 26 g of graphite was added to the above [a]' ([b]').
[0069] (3') Nanosilicon particles (D 50 Average value of 111 nm, D 90 158 nm) to prepare a solution, which was then poured into the above [b]' ([c]').
[0070] (4') 100 ml of ethanol was further added to the above [c]' to precipitate a high softening point pitch (softening point: 260°C) ([d]').
[0071] (5') Tetrahydrofuran was primarily vaporized from the above [d]' under the conditions of pressure, temperature and time (0.7 bar, 35°C and 20 minutes).
[0072] (6') Tetrahydrofuran and ethanol were completely evaporated under the conditions of pressure, temperature and time (0.7 bar, 60°C and 20 min) to obtain a dry powder ([e]').
[0073] (7') The dry powder ([e]') was placed in a Mechanofusion mixer and then pulverized.
[0074] (8') The ground, dried powder was carbonized at 1000°C for 60 minutes in a nitrogen atmosphere to obtain a graphite-nano silicon-pitch composite structure.
[0075] [Comparative Example 1] (1”) 5 g of high softening point pitch (softening point: 260°C) was ground using a mixer ([a]”).
[0076] 26 g of graphite was added to a (2”) Mechanofusion mixer and then run for 5 minutes.
[0077] (3) The above [a]" and nanosilicon particles (D) were added to a mechanofusion mixer containing graphite. 50 Average value: 111 nm, D 90 After adding 3 g of nanosilicon pitch (average particle size: 158 nm), the device was operated for 30 minutes to form a nanosilicon-pitch coating film on the graphite.
[0078] (4”) The graphite-nano silicon-pitch powder was collected from the mechanofusion mixer and carbonized at 1000°C for 60 minutes under nitrogen atmosphere to obtain a graphite-nano silicon-pitch composite structure.
[0079] 2. Manufacturing of secondary batteries In order to analyze the electrochemical properties of the negative electrode material for secondary batteries, the amorphous carbon-nano silicon-pitch composite structure prepared in Example 1, and the graphite-nano silicon-pitch composite structures prepared in Example 2 and Comparative Example 1 were used.
[0080] A negative electrode plate was manufactured by using a powder mixed with 15% of the composite structure manufactured in Examples 1-2 and Comparative Example 1 and 85% of artificial graphite as the final active material. The negative electrode plate was manufactured by casting a slurry made by mixing the active material, conductive material (Imerys Graphite & Carbon, Super-P product), and binder (CMC:SBR=3:7) in a weight ratio of 94:1:5 onto a copper foil with a thickness of 10 μm using a doctor blade method, vacuum drying, and rolling to a thickness of 50 μm using a roll press. The manufactured negative electrode plate was manufactured into a coin cell together with lithium metal, and the electrochemical performance was measured in a half cell.
[0081] The charge and discharge conditions were charge CC / CV: 0.01V / 0.01C, discharge CC 1.5V, and the rate limiting was 0.2C.
[0082] Using a half-cell device TOSCAT-3100, the initial charge efficiency (ICE; discharge amount relative to the initial charge amount), initial charge capacity (ICC; initial charge capacity), and initial discharge capacity (IDC; initial discharge capacity) were measured and shown in Table 1 below. The lifespan after 50 cycles was measured and the lifespan characteristics are shown in the graph of FIG. 10 (horizontal axis: number of cycles, vertical axis: discharge capacity).
[0083] 3. Experimental Example [Experimental Example 1 - Observation of the surface of a composite structure] The surfaces of the composite structures of Examples 1 and 2 and Comparative Example 1 were subjected to SEM analysis.
[0084] In Fig. 1, which is the analysis result of Example 1, it was observed that the pitch was uniformly and densely coated on the amorphous carbon and nanosilicon composite to form a spherical composite structure. Figs. 2 and 3 are enlarged photographs of Fig. 1, and the white parts on the surfaces of the spherical particles shown by dotted circles in Figs. 2 and 3 are pitch coating films, and the parts shown by solid circles in Fig. 3 are amorphous carbon-nanosilicon composites. As a result of observing the photographs of Figs. 2 and 3, it was confirmed that a thin and uniform pitch coating film was formed on the surface of the amorphous carbon-nanosilicon composite.
[0085] From the analysis results of Example 2, shown in Figures 4 to 7, it was observed that a graphite core was present between the layers, and a shell formed of pitch-nano silicon was uniformly and densely coated on top of the graphite core. The dark intermediate parts in the black and white drawings of Figures 4 and 6 are graphite, and the relatively light white parts are the shell formed of pitch-nano silicon, while the purple parts in the EDS mapping images of Figures 5 and 7 are graphite (labeled as carbon (C) in the color label) and the yellow parts are the pitch-silicon shell (labeled as silicon (Si) in the color label).
[0086] On the other hand, in Comparative Example 1, the coating film was formed by a dry method. When large-sized pitch was mixed, the pitch itself could act as a core, not a coating, so it was necessary to crush the pitch very finely, and step (1)" of Comparative Example 1 was carried out.
[0087] In this way, in Comparative Example 1, as a result of crushing the pitch into small particles, pitch particles of 50 to 100 μm level and fractions of 0.1 to 1 μm level were mixed, and the crushed pitch particles clumped together, and pitch lumps consisting of only pitch, not nanosilicon-pitch shells, were observed (the area indicated by the dotted circle in FIG. 8 and the yellow area in FIG. 9, labeled with silicon (Si) in the color label), and graphite lumps without any pitch coating were also observed (the area indicated by the solid circle in FIG. 8 and the red area in FIG. 9, labeled with carbon (C) in the color label).
[0088] [Experimental Example 2 - Evaluation of battery performance] In order to analyze the electrochemical properties of the negative electrode material for secondary batteries, the amorphous carbon-nano silicon-pitch composite structure prepared in Example 1, and the graphite-nano silicon-pitch composite structures prepared in Example 2 and Comparative Example 1 were used.
[0089] A negative electrode plate was manufactured by using a powder obtained by mixing 15% of the composite structures manufactured in Examples 1 and 2 and Comparative Example 1 with 85% of artificial graphite as the final active material. The negative electrode plate was manufactured by casting a slurry obtained by mixing the active material, conductive material (superP), and binder (CMC:SBR=3:7) in a weight ratio of 94:1:5 onto a copper foil of 10 microns thickness using a doctor blade method, vacuum drying, and rolling to a thickness of 50 microns using a roll press. The manufactured negative electrode plate was manufactured into a coin cell together with lithium metal, and the electrochemical performance of the half cell was measured.
[0090] The charge and discharge conditions were charge CC / CV: 0.01V / 0.01C, discharge CC 1.5V, and the rate limiting was 0.2C.
[0091] Using a half-cell device TOSCAT-3100, the initial charge efficiency (ICE; discharge amount relative to the initial charge amount), initial charge capacity (ICC; initial charge capacity), and initial discharge capacity (IDC; initial discharge capacity) were measured and shown in Table 1 below. The lifespan after 50 cycles was measured and the lifespan characteristics are shown in the graph of FIG. 10 (horizontal axis: number of cycles, vertical axis: discharge capacity).
[0092] [Table 1]
[0093] As can be seen from Table 1 above, it was confirmed that the performance of the secondary batteries of Examples 1 and 2 according to the present invention was significantly superior to the performance of the secondary battery of Comparative Example 1.
[0094] Although the examples of the present specification have been described in more detail above, the present specification is not necessarily limited to these examples, and various modifications and implementations are possible within the scope of the technical idea of the present specification. Therefore, the examples disclosed in the present specification are for the purpose of explanation, not for the purpose of limiting the technical idea of the present invention, and the scope of the technical idea of the present invention is not limited by these examples. Therefore, it should be understood that the above-mentioned examples are illustrative in all respects and not limiting. The present specification and the scope of protection of the present invention should be interpreted according to the claims, and all technical ideas within the scope equivalent thereto should be interpreted as being included in the scope of the present specification and the present invention.
Claims
1. (a) mixing nanosilicon, a carbon-based conductive material and a resin matrix to prepare a mixed powder; (b) dissolving a high softening point pitch in a first solvent to prepare a pitch solution; (c) adding the mixed powder to the pitch solution and stirring to prepare a dispersion solution containing nanosilicon, a carbon-based conductive material and pitch; (d) adding a second solvent to the dispersion solution to deposit pitch on the composite material including nanosilicon and carbon-based conductive material to form a pitch coating film; (e) removing the first and second solvents to obtain a dry powder; and (f) carbonizing the dried powder to obtain a negative active material having a pitch coating film formed on a composite material including nanosilicon and amorphous carbon; The first solvent is soluble in the high softening point pitch, The second solvent is insoluble in the high softening point pitch, The first solvent and the second solvent are miscible with each other. A method for producing a negative electrode active material for a secondary battery.
2. (a') dissolving a high softening point pitch in a first solvent to prepare a pitch solution, and then adding graphite to prepare a graphite-pitch solution; (b') separately from (a'), adding and dispersing nanosilicon in a second solvent to prepare a nanosilicon dispersion solution; (c') adding the nanosilicon dispersion solution to the graphite-pitch solution to prepare a mixed solution of graphite, pitch and nanosilicon; (d') adding the second solvent to the mixed solution of the graphite, pitch and nanosilicon to deposit the mixture of nanosilicon and pitch on the graphite, thereby forming a coating film containing nanosilicon and pitch; (e') removing the first and second solvents to obtain a dry powder; (f') dry-milling the dry powder; and (g') carbonizing the pulverized dry powder to obtain a negative electrode active material for a secondary battery having a structure of a graphite core and a nanosilicon-pitch shell surrounding the core; The first solvent is soluble in the high softening point pitch, The second solvent is insoluble in the high softening point pitch, The first solvent and the second solvent are miscible with each other. A method for producing a negative electrode active material for a secondary battery.
3. Based on 100 parts by weight of the mixed powder in step (a), the nanosilicon is included in an amount of 40 to 99 parts by weight. The method for producing the negative electrode active material for a secondary battery according to claim 1 .
4. The carbon-based conductive material in step (a) includes carbon black; The method for producing the negative electrode active material for a secondary battery according to claim 1 .
5. The resin matrix in step (a) includes at least one of a phenolic resin, an epoxy resin, a thermosetting polyimide, a polyester, a polyurethane, a melamine resin, an amino resin, and a dextrin resin; The method for producing the negative electrode active material for a secondary battery according to claim 1 .
6. The high softening point pitch has a softening point of 200 to 300° C. The method for producing the negative electrode active material for a secondary battery according to claim 1 or 2.
7. The step (e) or the step (e′) A primary vaporization step carried out under conditions of a pressure of 0.5 to 1 bar and a temperature of 25 to 40° C.; and a secondary vaporization step carried out under conditions of a pressure of 0.5 to 1 bar and a temperature higher than the boiling points of the first and second solvents; The method for producing the negative electrode active material for a secondary battery according to claim 1 or 2.
8. The first solvent includes at least one selected from the group consisting of tetrahydrofuran (THF), quinoline, toluene, pyridine, N-methylpyrrolidone (NMP), xylene, chloroform, dimethyl sulfoxide, and n-hexane; The method for producing the negative electrode active material for a secondary battery according to claim 1 or 2.
9. The second solvent is at least one selected from the group consisting of ethanol, methanol, acetone, and water. The method for producing the negative electrode active material for a secondary battery according to claim 1 or 2.
10. The first solvent comprises tetrahydrofuran and the second solvent comprises ethanol; The method for producing the negative electrode active material for a secondary battery according to claim 1 or 2.
11. The carbonization is carried out at a temperature of 1000 to 1100 ° C. The method for producing the negative electrode active material for a secondary battery according to claim 1 or 2.
12. The step (f') is carried out using a mechanofusion mixer. The method for producing the negative electrode active material for a secondary battery according to claim 2 .
13. The negative electrode active material for a secondary battery produced according to the production method of claim 1 or 2, Negative electrode material for secondary batteries.
14. The negative electrode active material for a secondary battery produced according to the production method of claim 1 or 2, A secondary battery including a negative electrode material for a secondary battery.
Citation Information
Patent Citations
Manufacture of carbonaceous powder for lithium ion secondary battery negative electrode active material
JP1999121007A
Coated carbonaceous particles particularly useful as electrode material in electrical storage cells and method for making same
JP2005515957A
Carbon-coated silicon particle power as positive electrode material for lithium-ion batteries and its production method
JP2007519182A
Method for producing carbonaceous particles
JP2013528898A
Negative electrode active material and secondary battery including the same
JP2016081920A