Ion conductor composition, polymer electrolyte membrane containing same, membrane-electrode assembly, and fuel cell

The introduction of a saccharide compound in the ion conductor composition addresses the challenge of maintaining ionic conductivity in polymer electrolyte membranes under high temperature or low humidity, improving fuel cell performance by stabilizing water content and reducing swelling.

JP2024544568AActive Publication Date: 2024-12-03KOLON INDUSTRIES INC
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024528611
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-26
Filing Date
2022-11-03
Publication Date
2024-12-03
Estimated Expiration
2042-11-03

AI Technical Summary

Technical Problem

Conventional polymer electrolyte membranes face challenges in maintaining high ionic conductivity under high temperature or low humidity conditions, leading to limitations in the operational range of polymer electrolyte membrane fuel cells.

Method used

An ion conductor composition containing a saccharide compound with functional groups capable of interacting with water is introduced to maintain water content in the polymer electrolyte membrane, enhancing ionic conductivity and minimizing interfacial swelling differences.

Benefits of technology

The ion conductor composition improves the activity and ionic conductivity of the polymer electrolyte membrane, maintaining optimal water content and reducing swelling issues, thereby enhancing the performance of fuel cells under varying humidity conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024544568000001_ABST
    Figure 2024544568000001_ABST
Patent Text Reader

Abstract

The ionic conductor composition according to the present invention contains 100 parts by weight of an ionic conductor and 0.05 to 10 parts by weight of a saccharide compound per 100 parts by weight of the ionic conductor.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to an ion conductor composition, a polymer electrolyte membrane, a membrane-electrode assembly, and a fuel cell, and to an ion conductor composition that maintains the water content in a polymer electrolyte membrane under high temperature or low humidity conditions through an ion conductor composition that includes a saccharide compound having a functional group capable of interacting with water, thereby increasing the activity of the electrolyte membrane and improving ion conductivity performance, a polymer electrolyte membrane, a membrane-electrode assembly, and a fuel cell. [Background technology]

[0002] Fuel cells are batteries equipped with a power generation system that directly converts chemical reaction energy, such as the oxidation / reduction reaction of hydrogen and oxygen contained in hydrocarbon fuel materials such as methanol, ethanol, and natural gas, into electrical energy. Due to their high energy efficiency and environmentally friendly characteristics with low pollutant emissions, fuel cells are attracting attention as a next-generation clean energy source that can replace fossil energy.

[0003] Fuel cells have the advantage of being able to produce a wide range of output power due to their stack configuration made up of stacked unit cells, and since they have 4 to 10 times the energy density of small lithium batteries, they are attracting attention as a small and portable power source for mobile use.

[0004] The stack that actually generates electricity in a fuel cell has a structure in which several to several tens of unit cells, each of which is made up of a membrane-electrode assembly (MEA) and a separator (also called a bipolar plate), are stacked. The membrane-electrode assembly generally has a structure in which an electrolyte membrane is sandwiched between an anode electrode (or fuel electrode) and a cathode electrode (or air electrode).

[0005] Fuel cells can be classified into alkaline electrolyte membrane fuel cells, polymer electrolyte membrane fuel cells (PEMFC), etc. depending on the state and type of electrolyte. Among them, polymer electrolyte membrane fuel cells are attracting attention as portable, vehicular, and home power sources due to their advantages such as low operating temperature of less than 100°C, fast start-up and response characteristics, and excellent durability.

[0006] Representative examples of polymer electrolyte membrane fuel cells include the Proton Exchange Membrane Fuel Cell (PEMFC), which uses hydrogen gas as fuel, and the Direct Methanol Fuel Cell (DMFC), which uses liquid methanol as fuel.

[0007] To summarize the reactions that occur in a polymer electrolyte membrane fuel cell, first, when a fuel such as hydrogen gas is supplied to the anode electrode, hydrogen ions (H + ) and electrons (e - The generated hydrogen ions are transferred to the cathode electrode via the polymer electrolyte, and the generated electrons are transferred to the cathode electrode via an external circuit. Oxygen gas is supplied to the cathode electrode, and oxygen combines with the hydrogen ions and electrons to generate water through a reduction reaction of oxygen.

[0008] Meanwhile, there are still many technical barriers to be overcome in order to commercialize polymer electrolyte membrane fuel cells, and essential improvements are to achieve high performance, long life, and low cost. The component that has the greatest impact on this is the membrane-electrode assembly, and among them, the polymer electrolyte membrane is one of the key elements that has the greatest impact on the performance and price of the MEA.

[0009] The requirements for the polymer electrolyte membrane necessary for the operation of the polymer electrolyte membrane fuel cell include high hydrogen ion conductivity, chemical stability, low fuel permeability, high mechanical strength, low moisture content, excellent dimensional stability, etc. Conventional polymer electrolyte membranes tend to have difficulty in normally exhibiting high performance in a specific temperature and relative humidity environment, particularly in a high temperature or low humidity condition. Therefore, the range of use of polymer electrolyte membrane fuel cells using conventional polymer electrolyte membranes is limited.

[0010] In particular, in order to overcome the problem that the high performance of the polymer electrolyte membrane is difficult to be exhibited under high temperature or low humidity conditions, research is being conducted on improving the ionic conductivity of the polymer electrolyte membrane by introducing a hygroscopic material into the polymer electrolyte membrane. Summary of the Invention [Problem to be solved by the invention]

[0011] An object of the present invention is to provide an ion conductor composition that maintains the water content in a polymer electrolyte membrane under low humidity or high temperature conditions through an ion conductor composition containing a saccharide compound having a functional group capable of interacting with water (or forming hydrogen bonds), thereby enhancing the activity of the polymer electrolyte membrane and improving its ion conductivity performance.

[0012] Another object of the present invention is to provide a polymer electrolyte membrane comprising the ion conductor composition.

[0013] It is yet another object of the present invention to provide a membrane-electrode assembly which improves the ionic conductivity of a polymer electrolyte membrane while minimizing problems caused by an interfacial difference (difference in swelling degree) between the polymer electrolyte membrane prepared from an ionic conductor composition including a saccharide compound and a catalyst layer having a relatively low water content.

[0014] It is still another object of the present invention to provide a fuel cell comprising the membrane-electrode assembly.

[0015] The object of the present invention is not limited to the object mentioned above, and other objects and advantages of the present invention not mentioned can be understood from the following description and will be more clearly understood from the embodiment of the present invention. In addition, it will be easily understood that the object and advantages of the present invention can be realized by the means and combinations thereof described in the claims. [Means for solving the problem]

[0016] To achieve the above object, one embodiment of the present invention provides an ion conductor composition comprising 100 parts by weight of an ion conductor and 0.05 to 10 parts by weight of a saccharide compound relative to 100 parts by weight of the ion conductor.

[0017] In order to achieve the above object, another embodiment of the present invention provides a polymer electrolyte membrane including the ion conductor composition.

[0018] In order to achieve the above object, still another embodiment of the present invention provides a membrane-electrode assembly including the polymer electrolyte membrane and a catalyst layer disposed on at least one surface of the polymer electrolyte membrane.

[0019] In order to achieve the above object, still another embodiment of the present invention provides a fuel cell including the membrane-electrode assembly. Effect of the Invention

[0020] According to one aspect of the present invention, an ion conductor composition can be provided that maintains the water content in a polymer electrolyte membrane under low humidity or high temperature conditions through the ion conductor composition including a saccharide compound having a functional group capable of interacting with water (or forming hydrogen bonds), thereby enhancing the activity of the polymer electrolyte membrane and improving its ion conductivity performance.

[0021] According to another aspect of the present invention, there is provided a polymer electrolyte membrane comprising the ion conductor composition.

[0022] According to yet another aspect of the present invention, there is provided a membrane-electrode assembly that improves the ionic conductivity of a polymer electrolyte membrane while minimizing problems caused by an interfacial difference (difference in swelling degree) between a polymer electrolyte membrane prepared from an ionic conductor composition including a saccharide compound and a catalyst layer having a relatively low water content.

[0023] According to yet another aspect of the present invention, there is provided a fuel cell comprising the membrane-electrode assembly.

[0024] In addition to the above-mentioned effects, specific effects of the present invention will be described below while explaining specific contents for carrying out the invention. [Brief description of the drawings]

[0025] [Figure 1] FIG. 1 is a cross-sectional view showing a membrane-electrode assembly according to one embodiment of the present invention.

[0026] [Diagram 2] 1 is a schematic diagram showing a fuel cell according to one embodiment of the present invention; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] Hereinafter, each component of the present invention will be described in more detail so that a person having ordinary skill in the art to which the present invention pertains can easily implement the present invention. However, this is merely an example, and the scope of the present invention is not limited to the following content.

[0028] One embodiment of the present invention provides an ion conductor composition comprising 100 parts by weight of an ion conductor and 0.05 to 10 parts by weight of a saccharide compound relative to 100 parts by weight of the ion conductor. According to one aspect of the present invention, the water content in a polymer electrolyte membrane can be maintained under low humidification or high temperature conditions through an ion conductor composition comprising a saccharide compound having a functional group capable of interacting with water (or forming hydrogen bonds), thereby enhancing the activity of the polymer electrolyte membrane and improving ion conductivity performance. According to another aspect of the present invention, problems caused by interfacial differences (swelling degree differences) in a catalyst layer having a relatively low water content can be minimized.

[0029] The configuration of the present invention will be described in more detail below.

[0030] The ion conductor according to the present invention may be one selected from the group consisting of fluorine-based ion conductors, hydrocarbon-based ion conductors, and combinations thereof, and is preferably a hydrocarbon-based ion conductor. When the hydrocarbon-based ion conductor is combined with a saccharide compound, not only can the ion conductivity be further increased with respect to the combination of the fluorine-based ion conductor and the saccharide compound, but the dimensional change rate of the polymer electrolyte membrane can be reduced to improve the dimensional stability, and the water content can be increased to an appropriate level under low humidification conditions. In addition, due to the structural similarity between the hydrocarbon-based ion conductor and the saccharide compound, compatibility is high, making it easier to realize the effect of the saccharide. The ion conductor may be a cation conductor having a cation exchange functional group such as a hydrogen ion, or an anion conductor having an anion exchange functional group such as a hydroxyl ion. The cation exchange functional group may be any one selected from the group consisting of a sulfonic acid group, a carboxyl group, a boronic acid group, a phosphoric acid group, an imide group, a sulfonimide group, a sulfonamide group, a sulfonyl fluoride group, and combinations thereof, and may generally be a sulfonic acid group or a carboxyl group. For example, the fluorine-based ion conductor may be perfluorosulfonic acid (PFSA).

[0031] Examples of the cationic conductor include a fluorine-based polymer containing the cationic exchange functional group and containing fluorine in the main chain, a hydrocarbon polymer such as benzimidazole, polyamide, polyamideimide, polyimide, polyacetal, polyethylene, polypropylene, acrylic resin, polyester, polysulfone, polyether, polyetherimide, polyester, polyethersulfone, polyetherimide, polycarbonate, polystyrene, polyphenylene sulfide, polyetheretherketone, polyetherketone, polyarylethersulfone, polyphosphazene, or polyphenylquinoxaline, a partially fluorinated polymer such as a polystyrene-graft-ethylenetetrafluoroethylene copolymer or a polystyrene-graft-polytetrafluoroethylene copolymer, a sulfonimide, or a mixture thereof.

[0032] More specifically, when the cation conductor is a hydrogen ion cation conductor, the polymer may contain a cation exchange group selected from the group consisting of a sulfonic acid group, a carboxylic acid group, a phosphoric acid group, a phosphonic acid group, and derivatives thereof in a side chain, and specific examples thereof include fluorine-based polymers including poly(perfluorosulfonic acid), poly(perfluorocarboxylic acid), a copolymer of tetrafluoroethylene and fluorovinyl ether containing a sulfonic acid group, defluorinated sulfurized polyether ketone, or a mixture thereof.

[0033] The anion conductor is a polymer capable of transporting anions such as hydroxy ions, and is commercially available in the form of hydroxide or halide (generally chloride). The anion conductor can be used in industrial water purification, metal separation, catalytic processes, etc.

[0034] The anion conductor may generally be a polymer doped with a metal hydroxide. Specifically, poly(ether sulfone), polystyrene, vinyl polymer, poly(vinyl chloride), poly(vinylidene fluoride), poly(tetrafluoroethylene), poly(benzimidazole), or poly(ethylene glycol) doped with a metal hydroxide may be used.

[0035] The hydrocarbon ion conductor may be a sulfonated polyimide (S-PI), a sulfonated polyarylethersulfone (S-PAES), a sulfonated polyetheretherketone (S-PEEK), a sulfonated polybenzimidazole (S-PBI), a sulfonated polysulfone (S-PSU), a sulfonated polystyrene (S-PS), a sulfonated polyphosphazene, a sulfonated polyquinoxaline, a sulfonated polyketone, a sulfonated polyphenylene oxide, a sulfonated polyethersulfone ... sulfone, sulfonated polyether ketone, sulfonated polyphenylene sulfone, sulfonated polyphenylene sulfide, sulfonated polyphenylene sulfide sulfone, sulfonated polyphenylene sulfide sulfone nitrile, sulfonated polyarylene ether, sulfonated polyarylene ether nitrileThe polyarylene ether nitrile, sulfonated polyarylene ether ether nitrile, sulfonated polyarylene ether sulfone ketone, and mixtures thereof may be any one selected from the group consisting of, however, the technical idea of ​​the present invention is not limited thereto.

[0036] The saccharide compound according to the present invention may be included in an amount of 0.05 to 10 parts by weight, preferably 0.5 to 2.0 parts by weight, and more preferably 0.5 to 1.0 parts by weight, based on 100 parts by weight of the ion conductor. If the amount of the saccharide compound is less than the above range, the water content of the polymer electrolyte membrane may be insufficient under high temperature or low humidity operating conditions, resulting in low hydrogen ion conductivity, and if the amount of the saccharide compound is more than the above range, the swelling degree difference between the catalyst layer and the polymer electrolyte membrane described below may become large, resulting in interface problems. The interface problems mean that the dimensional stability of the polymer electrolyte membrane is reduced.

[0037] The saccharide compound according to the present invention may be one selected from the group consisting of monosaccharides, disaccharides, polysaccharides, and combinations thereof, and may specifically be a monosaccharide.

[0038] The monosaccharide may correspond to a compound represented by the following Chemical Formula 1:

[0039] [C1]

[0040] (CH2O) n

[0041] In the above Chemical Formula 1, n may be 3 to 7, and preferably 4 to 6.

[0042] For example, the monosaccharide may be one selected from the group consisting of aldotriose, ketotriose, aldotetrose, ketotetrose, ribose, dioxyribose, fructose, glucose, galactose, aldoheptose, ketoheptose, and combinations thereof.

[0043] For example, the disaccharide may be one selected from the group consisting of sucrose, lactulose, lactose, trehalose, cellobiose, chitobiose, kojibiose, nigerose, isomaltose, β-trehalose, α,β-trehalose, sophorose, laminaribiose, gentiobiose, turanose, maltulose, isomaltulose, gentiobiulose, mannobiose, melibiose, melibiulose, rutinose, rutinulose, xylobiose, and combinations thereof.

[0044] For example, the polysaccharide may be one selected from the group consisting of starch, glycogen, cellulose, chitin, arabinoxylan, pectin, dextrin, and combinations thereof.

[0045] The solubility of the saccharide compound may be 0 to 1,000 g / L, and preferably 150 to 700 g / L, based on water at 25° C. If the solubility of the saccharide compound in water is below the above range, the saccharide compound may precipitate and act as resistance, and if the solubility exceeds the above range, a problem of leakage from the polymer electrolyte membrane may occur during operation of the fuel cell.

[0046] The saccharide compound contains a functional group (hydroxy group) capable of interacting with water (or forming hydrogen bonds), and thus can maintain the water content in the polymer electrolyte membrane under low humidity or high temperature conditions. Thus, the high water content of the polymer electrolyte membrane under low humidity or high temperature conditions can increase the activity of the polymer electrolyte membrane and improve the ion conductivity performance.

[0047] Another embodiment of the present invention provides a polymer electrolyte membrane comprising the ion conductor composition.

[0048] The polymer electrolyte membrane may be a single membrane, and the thickness of the single membrane may be, for example, 5 to 125 μm, and preferably 5 to 60 μm, although the technical concept of the present invention is not limited to the thickness of the polymer electrolyte membrane, and various thickness ranges may be applied.

[0049] A polymer electrolyte membrane (or reinforced composite membrane) according to yet another embodiment of the present invention may further include a porous support impregnated with a dispersion containing the ion conductor composition. Existing reinforced composite membranes may have excellent mechanical durability compared to single membranes due to the introduction of a porous support, but have problems such as resistance, relatively low ion conductivity, and low water content under high temperature and low humidity conditions. According to one embodiment of the present invention, by impregnating a porous support with a dispersion containing the ion conductor composition, it is possible to increase the ion conductivity and water content to appropriate levels as well as improve dimensional stability.

[0050] The porous support may be one selected from the group consisting of fluorine-based porous supports, hydrocarbon-based porous supports, and combinations thereof.

[0051] The fluorine-based porous support according to one embodiment of the present invention may include a highly fluorinated polymer, preferably a perfluorinated polymer, having excellent resistance to thermal and chemical decomposition, for example, polytetrafluoroethylene (PTFE) or tetrafluoroethylene and CF2=CFC. n F 2n+1 (n is a real number from 1 to 5) or CF2 = CFO-(CF2CF(CF3)O) m C n F 2n+1 (m is a real number of 0 to 15, and n is a real number of 1 to 15).

[0052] The fluorine-based porous support according to another embodiment of the present invention may be expanded polytetrafluoroethylene (e-PTFE) having a microstructure of polymer fibrils or a microstructure in which nodes are connected to each other by fibrils. Also, a film having a microstructure of polymer fibrils without the nodes may be used as the porous support.

[0053] According to yet another embodiment of the present invention, the fluorine-based porous support may include a perfluorinated polymer, which may be obtained by extruding dispersion-polymerized PTFE into a tape in the presence of a lubricant and stretching the resulting material to form a more porous and stronger porous support.

[0054] The amorphous content of PTFE can also be increased by heat treating the e-PTFE at a temperature exceeding the melting point of PTFE (about 342°C). The e-PTFE film produced by the above method can have micropores with various diameters and porosity. The e-PTFE film produced by the above method can have at least 35% micropores, and the diameter of the micropores can be about 0.01 to 1 μm.

[0055] The hydrocarbon-based porous support according to an embodiment of the present invention may be a nonwoven fibrous web made of a plurality of randomly oriented fibers. The nonwoven fibrous web refers to a sheet having a structure of individual fibers or filaments that are interlaid but not in the same manner as a woven fabric. The nonwoven fibrous web may be manufactured by any one method selected from the group consisting of carding, garneting, air-laying, wet-laying, melt blowing, spun bonding, and stitch bonding.

[0056] The fibers may include one or more polymeric materials, and generally, any of those used as fiber-forming polymeric materials may be used, and specifically, hydrocarbon-based fiber-forming polymeric materials may be used. For example, the fiber-forming polymeric material may include any one selected from the group consisting of polyolefins, such as polybutylene, polypropylene, and polyethylene, polyesters, such as polyethylene terephthalate and polybutylene terephthalate, polyamides (nylon-6 and nylon-6,6), polyurethanes, polybutenes, polylactic acids, polyvinyl alcohols, polyphenylene sulfides, polysulfones, fluid crystalline polymers, polyethylene-co-vinyl acetates, polyacrylonitriles, cyclic polyolefins, polyoxymethylenes, polyolefin-based thermoplastic elastomers, and combinations thereof. However, the technical idea of ​​the present invention is not limited thereto.

[0057] The hydrocarbon-based porous support according to an embodiment of the present invention may include a nanoweb in which nanofibers are accumulated in the form of a nonwoven fabric having a plurality of pores.

[0058] The nanofibers are preferably made of a hydrocarbon-based polymer that exhibits excellent chemical resistance, has hydrophobicity, and is not likely to deform due to moisture in a high humidity environment. Specifically, the hydrocarbon-based polymer may be selected from the group consisting of nylon, polyimide, polyaramid, polyetherimide, polyacrylonitrile, polyaniline, polyethylene oxide, polyethylene naphthalate, polybutylene terephthalate, styrene butadiene rubber, polystyrene, polyvinyl chloride, polyvinyl alcohol, polyvinylidene fluoride, polyvinyl butylene, polyurethane, polybenzoxazole, polybenzimidazole, polyamideimide, polyethylene terephthalate, polyphenylene sulfide, polyethylene, polypropylene, copolymers thereof, and mixtures thereof. Among these, polyimide is preferably used because of its excellent heat resistance, chemical resistance, and dimensional stability.

[0059] The nanoweb is an aggregate of nanofibers that are randomly arranged and manufactured by electrospraying. In this case, the nanofibers preferably have an average diameter of 40 to 5000 nm, calculated from the average of diameters of 50 fibers measured using a scanning electron microscope (JSM6700F, JEOL) while taking into account the porosity and thickness of the nanoweb.

[0060] If the average diameter of the nanofibers is less than the above range, the mechanical strength of the porous support may be reduced, and if the average diameter of the nanofibers is more than the above range, the porosity may be significantly reduced and the thickness may be increased.

[0061] The nonwoven fibrous web may have a thickness of 10 to 50 μm, specifically, 15 to 43 μm. If the thickness of the nonwoven fibrous web is less than the above range, the mechanical strength may be reduced, and if it exceeds the above range, the resistance loss may be increased, and the weight and integration may be reduced.

[0062] The nonwoven fibrous web has a basic weight of 5 to 30 mg / cm 2 If the basis weight of the nonwoven fibrous web is less than the above range, visible pores may be formed and it may be difficult to function as a porous support, and if it exceeds the above range, it may be manufactured in the form of paper or fabric with almost no pores.

[0063] The porosity can be calculated as a ratio of the air volume in the porous support to the total volume of the porous support according to the following mathematical formula 1. Here, the total volume is calculated by preparing a rectangular sample and measuring its width, length, and thickness, and the air volume can be obtained by measuring the mass of the sample and then subtracting the polymer volume, which is calculated back from the density, from the total volume.

[0064] [Mathematical formula 1]

[0065] Porosity (%) = (air volume in the porous support / total volume of the porous support) x 100

[0066] The porosity of the porous support according to the present invention may be 30 to 90%, and preferably 50 to 85%. If the porosity of the porous support is less than the above range, the impregnation of the ion conductor may be reduced, and if it exceeds the above range, the shape stability may be reduced, which may hinder smooth post-processing.

[0067] Yet another embodiment of the present invention may provide a membrane-electrode assembly comprising the polymer electrolyte membrane and a catalyst layer disposed on at least one surface of the polymer electrolyte membrane.

[0068] The configuration of the present invention will be described in detail below with reference to the drawings.

[0069] FIG. 1 is a cross-sectional view showing a membrane-electrode assembly according to one embodiment of the present invention.

[0070] As shown in FIG. 1, the membrane-electrode assembly 100 according to the present invention includes the polymer electrolyte membrane 50 and the fuel cell electrodes 20 and 20 ′ disposed on both sides of the polymer electrolyte membrane 50 , respectively.

[0071] The electrodes 20, 20' include an electrode substrate 40, 40' and a catalyst layer 30, 30' formed on a surface of the electrode substrate 40, 40'. In order to facilitate diffusion of materials in the electrode substrate 40, 40', a microporous layer (not shown) containing conductive fine particles such as carbon powder or carbon black may be further provided between the electrode substrate 40, 40' and the catalyst layer 30, 30'.

[0072] In the membrane-electrode assembly 100, the electrode 20 that is disposed on one side of the polymer electrolyte membrane 50 and causes an oxidation reaction to generate hydrogen ions and electrons from the fuel transferred to the catalyst layer 30 via the electrode substrate 40 is called an anode.

[0073] The electrode 20′ disposed on the other side of the polymer electrolyte membrane 50 and performing a reduction reaction to generate water from hydrogen ions supplied through the polymer electrolyte membrane 50 and an oxidant transferred to the catalyst layer 30′ via the electrode substrate 40′ is referred to as a cathode electrode.

[0074] The catalyst layers 30, 30' of the anode and cathode electrodes 20, 20' contain a catalyst. The catalyst participates in the cell reaction and can be any catalyst that can be used as a catalyst for a fuel cell. Preferably, a platinum-based metal can be used.

[0075] The platinum-based metal may include one selected from the group consisting of platinum (Pt), palladium (Pd), ruthenium (Ru), iridium (Ir), osmium (Os), platinum-M alloys, non-platinum alloys, and combinations thereof. More preferably, a combination of two or more metals selected from the platinum-based catalytic metal group may be used, but is not limited thereto. Any platinum-based catalytic metal that can be used in this technical field may be used without limitation.

[0076] The M may be at least one selected from the group consisting of palladium (Pd), ruthenium (Ru), iridium (Ir), osmium (Os), gallium (Ga), titanium (Ti), vanadium (V), chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), silver (Ag), gold (Au), zinc (Zn), tin (Sn), molybdenum (Mo), tungsten (W), lanthanum (La), and rhodium (Rh). Specifically, the platinum alloy may be selected from the group consisting of Pt-Pd, Pt-Sn, Pt-Mo, Pt-Cr, Pt-W, Pt-Ru, Pt-Ru-W, Pt-Ru-Mo, Pt-Ru-Rh-Ni, Pt-Ru-Sn-W, Pt-Co, Pt-Co-Ni, Pt-Co-Fe, Pt-Co-Ir, Pt-Co-S, Pt-Co-P, Pt-Fe, Pt-Fe-Ir, Pt-Fe-S, Pt-Fe-P, Pt-Au-Co, Pt-Au-Fe, Pt-Au-Ni, Pt-Ni, Pt-Ni-Ir, Pt-Cr, Pt-Cr-Ir, and combinations thereof, either alone or in combination of two or more thereof.

[0077] Furthermore, the non-platinum alloy may be selected from the group consisting of Ir-Fe, Ir-Ru, Ir-Os, Co-Fe, Co-Ru, Co-Os, Rh-Fe, Rh-Ru, Rh-Os, Ir-Ru-Fe, Ir-Ru-Os, Rh-Ru-Fe, Rh-Ru-Os, and combinations thereof, either alone or in combination of two or more thereof.

[0078] The catalyst may be a catalyst itself (black) or may be supported on a carrier.

[0079] According to the present invention, it is possible to provide a membrane-electrode assembly that improves the ionic conductivity of a polymer electrolyte membrane while minimizing problems caused by an interfacial difference (difference in swelling degree) between a polymer electrolyte membrane prepared from an ionic conductor composition including a saccharide compound and a catalyst layer having a relatively low water content.

[0080] FIG. 2 is a schematic diagram showing a fuel cell according to one embodiment of the present invention.

[0081] An embodiment of the present invention can provide a fuel cell including the membrane-electrode assembly.

[0082] As shown in FIG. 2, a fuel cell 200 according to the present invention may include a fuel supply unit 210 for supplying a mixed fuel obtained by mixing fuel and water, a reforming unit 220 for reforming the mixed fuel to generate a reformed gas containing hydrogen gas, a stack 230 for generating electrical energy by electrochemically reacting the reformed gas containing hydrogen gas supplied from the reforming unit 220 with an oxidant, and an oxidant supply unit 240 for supplying an oxidant to the reforming unit 220 and the stack 230.

[0083] The stack 230 may include a plurality of unit cells that generate electrical energy by conducting an oxidation / reduction reaction between the reformed gas including hydrogen gas supplied from the reformer 220 and an oxidant supplied from the oxidant supplying unit 240.

[0084] Each unit cell means a unit cell that generates electricity, and may include the membrane-electrode assembly that oxidizes / reduces oxygen in a reformed gas containing hydrogen gas and an oxidant, and a separator plate (also called a bipolar plate, hereinafter referred to as "separator plate") for supplying the reformed gas containing hydrogen gas and the oxidant to the membrane-electrode assembly. The separator plates are disposed on both sides of the membrane-electrode assembly. In this case, the separator plates located at the outermost sides of the stack are also referred to as end plates.

[0085] Of the separation plates, the end plate may be provided with a pipe-shaped first supply pipe 231 for injecting the reformed gas containing hydrogen gas supplied from the reforming section 220, and a pipe-shaped second supply pipe 232 for injecting oxygen gas, and the other end plate may be provided with a first exhaust pipe 233 for discharging the reformed gas containing hydrogen gas that is ultimately left unreacted in the multiple unit cells to the outside, and a second exhaust pipe 234 for discharging the oxidant that is ultimately left unreacted in the unit cells to the outside.

[0086] In the fuel cell, the separator, the fuel supply section, and the oxidant supply section constituting the electricity generating section are the same as those used in ordinary fuel cells, and therefore detailed description thereof will be omitted in this specification.

[0087] Hereinafter, the embodiments of the present invention will be described in detail so that a person having ordinary skill in the art to which the present invention pertains can easily carry out the embodiments. However, this is merely an example, and the scope of the present invention is not limited to the following contents.

[0088] [Production Example: Production of a Polymer Electrolyte Membrane Containing an Ion Conductor Composition]

[0089] Polymer electrolyte membranes containing the ion conductor compositions according to the examples and comparative examples were prepared according to the compositions shown in Table 1. The polymer electrolyte membranes were prepared by a conventional method for preparing a polymer electrolyte membrane.

[0090] <Comparative Example 1-1>

[0091] A Nafion dispersion (D2020; Dupont, 20 wt% Nafion) was cast onto a glass plate using a doctor blade to prepare a single-layer polymer electrolyte membrane.

[0092] <Comparative Example 1-2>

[0093] Glucose was added to a Nafion dispersion (D2020; Dupont, 20 wt% Nafion) in an amount of 0.01 parts by weight per 100 parts by weight of the Nafion dispersion, and the Nafion dispersion to which glucose was added was stirred at room temperature for 3 hours. The stirred Nafion dispersion was cast on a glass substrate using a doctor blade to prepare a polymer electrolyte membrane in the form of a single membrane.

[0094] <Comparative Example 1-3>

[0095] Glucose was added to a Nafion dispersion (D2020; Dupont, 20 wt% Nafion) in an amount of 11 parts by weight per 100 parts by weight of the Nafion dispersion, and the Nafion dispersion to which glucose was added was stirred at room temperature for 3 hours. The stirred Nafion dispersion was cast on a glass substrate using a doctor blade to prepare a polymer electrolyte membrane in the form of a single membrane.

[0096] <Comparative Example 2-1>

[0097] A dispersion liquid prepared by dissolving sulfonated polyarylene ether sulfone (S-PAES) with an IEC (Ion Exchange Capacity) of 1.3 meq / g in DMAc (Dimethylacetamide) was cast on a glass plate using a doctor blade to prepare a single-layer polymer electrolyte membrane.

[0098] <Comparative Example 3-1>

[0099] A polymer electrolyte membrane (or reinforced composite membrane) was prepared by impregnating PTFE (Poly-Terafluoroethylene; 80% porosity, 0.45 μm pore size, 15 μm thickness) into a Nafion dispersion (D2020; Dupont, 20 wt% Nafion) for 1 hour and then drying the mixture.

[0100] <Example 1-1>

[0101] Glucose was added to a Nafion dispersion (D2020; Dupont, 20 wt% Nafion) in an amount of 0.1 parts by weight per 100 parts by weight of the Nafion dispersion, and the Nafion dispersion to which glucose was added was stirred at room temperature for 3 hours. The stirred Nafion dispersion was cast on a glass substrate using a doctor blade to prepare a polymer electrolyte membrane in the form of a single membrane.

[0102] <Example 1-2>

[0103] Glucose was added to a Nafion dispersion (D2020; Dupont, 20 wt% Nafion) in an amount of 0.5 parts by weight per 100 parts by weight of the Nafion dispersion, and the Nafion dispersion to which glucose was added was stirred at room temperature for 3 hours. The stirred Nafion dispersion was cast on a glass substrate using a doctor blade to prepare a polymer electrolyte membrane in the form of a single membrane.

[0104] <Example 1-3>

[0105] Glucose was added to a Nafion dispersion (D2020; Dupont, 20 wt% Nafion) in an amount of 1.0 part by weight per 100 parts by weight of the Nafion dispersion, and the Nafion dispersion to which glucose was added was stirred at room temperature for 3 hours. The stirred Nafion dispersion was cast on a glass substrate using a doctor blade to prepare a polymer electrolyte membrane in the form of a single membrane.

[0106] <Example 1-4>

[0107] Sucrose was added to a Nafion dispersion (D2020; Dupont, 20 wt% Nafion) in an amount of 0.5 parts by weight per 100 parts by weight of the Nafion dispersion, and the Nafion dispersion to which sucrose was added was stirred at room temperature for 3 hours. The stirred Nafion dispersion was cast on a glass substrate using a doctor blade to prepare a polymer electrolyte membrane in the form of a single membrane.

[0108] <Example 1-5>

[0109] Maltose was added to a Nafion dispersion (D2020; Dupont, 20 wt% Nafion) in an amount of 0.5 parts by weight per 100 parts by weight of the Nafion dispersion, and the Nafion dispersion to which maltose was added was stirred at room temperature for 3 hours. The stirred Nafion dispersion was cast on a glass substrate using a doctor blade to prepare a polymer electrolyte membrane in the form of a single membrane.

[0110] <Examples 1-6>

[0111] Starch was added to a Nafion dispersion (D2020; Dupont, 20 wt% Nafion) in an amount of 0.5 parts by weight per 100 parts by weight of the Nafion dispersion, and the Nafion dispersion to which the starch was added was stirred at room temperature for 24 hours. The stirred Nafion dispersion was cast on a glass substrate using a doctor blade to prepare a polymer electrolyte membrane in the form of a single membrane.

[0112] <Example 2-1>

[0113] Sulfonated polyarylene ether sulfone (S-PAES) with an IEC (Ion Exchange Capacity) of 1.3 meq / g was dissolved in DMAc (Dimethylacetamide) to prepare an S-PAES dispersion, to which 1.0 part by weight of glucose was added per 100 parts by weight of the S-PAES dispersion, and the S-PAES dispersion to which glucose was added was stirred at room temperature for 3 hours. The stirred S-PAES dispersion was cast on a glass plate with a doctor blade to prepare a polymer electrolyte membrane in the form of a single membrane.

[0114] <Example 2-2>

[0115] Sulfonated polyarylene ether sulfone (S-PAES) with an IEC (Ion Exchange Capacity) of 1.3 meq / g was dissolved in DMAc (Dimethylacetamide) to prepare an S-PAES dispersion, and 0.5 parts by weight of sucrose was added to 100 parts by weight of the S-PAES dispersion, and the S-PAES dispersion to which sucrose was added was stirred at room temperature for 3 hours. The stirred S-PAES dispersion was cast on a glass plate with a doctor blade to prepare a polymer electrolyte membrane in the form of a single membrane.

[0116] <Example 2-3>

[0117] Sulfonated polyarylene ether sulfone (S-PAES) with an IEC (Ion Exchange Capacity) of 1.3 meq / g was dissolved in DMAc (Dimethylacetamide) to prepare an S-PAES dispersion, to which 0.5 parts by weight of maltose was added per 100 parts by weight of the S-PAES dispersion, and the S-PAES dispersion to which maltose was added was stirred at room temperature for 3 hours. The stirred S-PAES dispersion was cast on a glass plate with a doctor blade to prepare a polymer electrolyte membrane in the form of a single membrane.

[0118] <Example 2-4>

[0119] Sulfonated polyarylene ether sulfone (S-PAES) with an IEC (Ion Exchange Capacity) of 1.3 meq / g was dissolved in DMAc (Dimethylacetamide) to prepare an S-PAES dispersion, to which 0.5 parts by weight of starch was added per 100 parts by weight of the S-PAES dispersion, and the S-PAES dispersion to which the starch was added was stirred at room temperature for 6 hours. The stirred S-PAES dispersion was cast on a glass plate with a doctor blade to prepare a polymer electrolyte membrane in the form of a single membrane.

[0120] <Example 3-1>

[0121] Glucose was added to a Nafion dispersion (D2020; Dupont, 20 wt% Nafion) in an amount of 1.0 part by weight per 100 parts by weight of the Nafion dispersion, and the Nafion dispersion to which glucose was added was stirred at room temperature for 3 hours. PTFE (Poly-Terafluoroethylene; 80% porosity, 0.45 μm pore size, 15 μm thickness) was impregnated into the stirred Nafion dispersion for 1 hour, and then a polymer electrolyte membrane (or reinforced composite membrane) was manufactured through a drying process.

[0122] [Table 1]

[0123] [Experimental example: Ion conductivity, moisture content, and dimensional stability evaluation experiment]

[0124] The polymer electrolyte membranes prepared using the ion conductor compositions prepared in the Examples and Comparative Examples were measured for ion conductivity, water content, and dimensional stability, and the results are shown in Table 2. The respective measurement methods are as follows.

[0125] 1) Ionic conductivity (high temperature / low humidity conditions: 80℃ / 50%RH)

[0126] The ionic conductivity of the polymer electrolyte membranes according to the comparative examples and examples was measured using a measuring device (Solatron-1280 Impedance / Gain-Phase analyzer, Solartron) at a measuring temperature of 80° C. In particular, the ohmic resistance or bulk resistance was measured using a four point probe AC ​​impedance spectroscopic method, and then the ionic conductivity was calculated according to the following [Equation 2].

[0127] [Mathematical formula 2]

[0128]

number

[0129] In the above mathematical formula 2, σ is the ionic conductivity (S / cm), R is the ohmic resistance of the electrolyte membrane (Ω), L is the distance between the electrodes (cm), and S is the area in the electrolyte through which a certain current flows (cm 2 ) applies.

[0130] 2) Moisture content

[0131] The polymer electrolyte membranes according to the comparative example and the examples were washed several times with deionized water, and the washed polymer electrolyte membranes were dried in a vacuum dryer at 120° C. for 24 hours and then weighed (W dry The same membrane was then immersed in deionized water for 24 hours, taken out, the water present on the surface was removed, and the weight was measured again (W wet The water absorption rate was calculated using the following mathematical formula 3.

[0132] [Mathematical formula 3]

[0133]

number

[0134] 3) Low humidity moisture content

[0135] The polymer electrolyte membranes according to the comparative example and the examples were washed several times with deionized water, and the washed polymer electrolyte membranes were dried in a vacuum dryer at 120° C. for 24 hours and then weighed (W dry Next, the same film was placed on a balance inside a chamber at 25°C and 50% relative humidity, and left for 24 hours, after which its weight was measured (W wet ) and the water absorption rate was calculated according to the above mathematical formula 3.

[0136] 4) Dimensional stability

[0137] The dimensional stability of the polymer electrolyte membranes according to the comparative examples and examples was measured in the same manner as the water absorption rate measurement method, but instead of measuring the weight, the volume change of the polymer electrolyte membrane was measured, and then the dimensional stability (or dimensional change rate) was calculated according to the following Equation 4.

[0138] [Mathematical formula 4]

[0139]

number

[0140] [Table 2]

Claims

1. 100 parts by weight of an ionic conductor; The ionic conductor composition comprises 0.05 to 10 parts by weight of a saccharide compound relative to 100 parts by weight of the ionic conductor.

2. The saccharide compound is 2. The ionic conductor composition according to claim 1, which is one selected from the group consisting of monosaccharides, disaccharides, polysaccharides, and combinations thereof.

3. The ionic conductor composition according to claim 2 , wherein the monosaccharide is a compound represented by the following chemical formula 1: [Chemical formula 1] (CH 2 O) n In the above formula 1, n is an integer of 3 to 7.

4. The monosaccharide is 3. The ionic conductor composition according to claim 2, which is one selected from the group consisting of aldotriose, ketotriose, aldotetrose, ketotetrose, ribose, dioxyribose, fructose, glucose, galactose, aldoheptose, ketoheptose, and combinations thereof.

5. The disaccharide is 3. The ionic conductor composition according to claim 2, which is one selected from the group consisting of sucrose, lactulose, lactose, trehalose, cellobiose, chitobiose, kojibiose, nigerose, isomaltose, β-trehalose, α,β-trehalose, sophorose, laminaribiose, gentiobiose, turanose, maltulose, isomaltulose, gentiobiulose, mannobiose, melibiose, melibiulose, rutinose, rutinulose, xylobiose, and combinations thereof.

6. The polysaccharide is 3. The ionic conductor composition according to claim 2, which is one selected from the group consisting of starch, glycogen, cellulose, chitin, arabinoxylan, pectin, dextrin, and combinations thereof.

7. The ion conductor is 2. The ionic conductor composition according to claim 1, which is one selected from the group consisting of fluorine-based ionic conductors, hydrocarbon-based ionic conductors, and combinations thereof.

8. The hydrocarbon ion conductor is Sulfonated polyimide (S-PI), sulfonated polyarylethersulfone (S-PAES), sulfonated polyetheretherketone (S-PEEK), sulfonated polybenzimidazole (S-PBI), sulfonated polysulfone (S-PSU), sulfonated polystyrene (S-PS), sulfonated polyphosphazene (S-PS), polyphosphazene, sulfonated polyquinoxaline, sulfonated polyketone, sulfonated polyphenylene oxide, sulfonated polyether sulfone, sulfonated polyether ketone, sulfonated polyphenylene sulfone, sulfonated polyphenylene sulfide sulfonated polyphenylene sulfide sulfone, sulfonated polyphenylene sulfide sulfone nitrile, sulfonated polyarylene ether, sulfonated polyarylene ether nitrile, sulfonated polyarylene ether ether nitrile8. The ionic conductor composition according to claim 7, which is any one selected from the group consisting of polyarylene ether ether nitrile, sulfonated polyarylene ether sulfone ketone, and mixtures thereof.

9. The fluorine-based ion conductor is 8. The ionic conductor composition according to claim 7, which is perfluorosulfonic acid (PFSA).

10. 2. The ionic conductor composition according to claim 1, wherein the solubility of the saccharide compound is 0 to 1000 g / L in water at 25° C.

11. A polymer electrolyte membrane comprising the ion conductor composition of claim 1.

12. The polymer electrolyte membrane is The polymer electrolyte membrane of claim 11, further comprising a porous support impregnated with a dispersion containing the ion conductor composition.

13. The porous support is 13. The polymer electrolyte membrane according to claim 12, which is one selected from the group consisting of a fluorine-based porous support, a hydrocarbon-based porous support, and a combination thereof.

14. The polymer electrolyte membrane according to claim 11; a catalyst layer disposed on at least one surface of the polymer electrolyte membrane; A membrane-electrode assembly comprising:

15. A fuel cell comprising the membrane-electrode assembly according to claim 14.

Citation Information

Patent Citations

  • Proton conductive polymer electrolyte membrane, polymer electrolyte membrane-electrode assembly, manufacturing method for them, and fuel cell using it

    JP2006031970A

  • Polymer electrolyte membrane for fuel cells, membrane electrode assembly containing the same, and fuel cell

    JP2014522552A

  • Polymer electrolyte membrane for fuel cell, membrane electrode assembly and fuel cell including the same

    KR1020120139066A