Manufacturing method of pouch case for secondary battery
By laminating layers and applying heat to the sealant layer after molding, the method addresses the issue of cracks and whitening in secondary battery pouch cases, enhancing durability and stability.
Patent Information
- Application Number
- JP2024535527
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-23
- Filing Date
- 2022-12-22
- Publication Date
- 2024-12-03
AI Technical Summary
The manufacturing of secondary battery pouch cases with deep molding depth and large molding bend leads to excessive tensile stress on the sealant layer, causing severe whitening phenomena that adversely affect durability and insulation, ultimately reducing the stability of the battery.
A method involving the lamination of a base material layer, barrier layer, and sealant layer, followed by molding to form a cup part and applying heat to the sealant layer to reduce cracks and voids, using infrared rays or a heating block to expand the sealant material and fill defects.
Reduces cracks and whitening in the sealant layer, improving the durability and stability of the secondary battery pouch case by enhancing the mechanical strength and sealing properties.
Smart Images

Figure 2024544713000001_ABST
Abstract
Description
[Technical field]
[0001] This application claims the benefit of priority to Korean Patent Application No. 10-2021-0186151, filed December 23, 2021, the entire contents of which are incorporated herein by reference.
[0002] The present invention relates to a method for manufacturing a pouch case for a secondary battery, and more specifically, to a method for manufacturing a pouch case for a secondary battery, which includes a step of reducing cracks in the sealant layer of a molded pouch exterior material for a secondary battery. [Background technology]
[0003] In general, in order to manufacture a pouch case for a secondary battery, a pouch exterior material for a secondary battery is pressed to a specific depth using a punch to form it. The shape of the pouch exterior material for a secondary battery is deformed by the pressure of the punch to form a cup portion, and during this process, pinholes or cracks may occur in the barrier layer of the formed pouch exterior material for a secondary battery, or wrinkles may occur, causing a whitening phenomenon in the sealant layer. The whitening phenomenon of the sealant layer is known as a phenomenon in which the surface appears white due to fine cracks and microvoids generated by tensile stress when the pouch exterior material for a secondary battery is formed.
[0004] Recently, in order to improve the performance of secondary batteries, there is a demand for pouch cases for secondary batteries with a deep molding depth and large molding curvature. However, when a pouch case for secondary batteries with a deep molding depth and large molding curvature is manufactured as described above, excessive tensile stress is applied to the sealant layer disposed on the inside of the pouch case for secondary batteries, causing severe whitening of the sealant layer. The whitening of the sealant layer adversely affects the durability and insulating properties of the pouch case for secondary batteries, and ultimately reduces the stability of the manufactured pouch-type secondary battery.
[0005] Therefore, there is a need for a method for manufacturing a pouch case for a secondary battery that can reduce the degree of whitening of the sealant layer even under molding conditions with a deep molding depth and large molding curvature. Summary of the Invention [Problem to be solved by the invention]
[0006] In order to solve the above problems, an object of the present invention is to provide a method for manufacturing a pouch case for a secondary battery, which can reduce whitening of a sealant layer. [Means for solving the problem]
[0007] In one embodiment of the present invention, there is provided a method for manufacturing a pouch case for a secondary battery, comprising: (S1) a step of preparing a pouch exterior material for a secondary battery including a structure in which a base material layer, a barrier layer, and a sealant layer are laminated in that order; (S2) a step of molding the pouch exterior material for a secondary battery to form a cup portion; and (S3) a step of reducing cracks in the sealant layer of the pouch exterior material for a secondary battery. Effect of the Invention
[0008] According to the present invention, by applying heat to the sealant layer of a molded pouch exterior material for a secondary battery, cracks in the sealant layer are reduced, whitening is decreased, and a pouch case for a secondary battery having improved durability and stability can be manufactured. [Brief description of the drawings]
[0009] The following drawings attached to the specification illustrate preferred embodiments of the present invention and, together with the above-mentioned content of the invention, serve to further understand the technical concept of the present invention. Therefore, the present invention should not be interpreted as being limited only to the matters depicted in such drawings.
[0010] [Figure 1] FIG. 2 is a diagram illustrating a cross section of a pouch exterior material for a secondary battery. [Diagram 2]FIG. 2 is a diagram illustrating a cross section of a molded pouch exterior material for a secondary battery. [Diagram 3] 3 is an enlarged view of the inner surface of the cup portion of the molded pouch exterior material for a secondary battery shown in FIG. 2. FIG. [Figure 4] FIG. 2 is a plan view of a molded pouch exterior material for a secondary battery. [Diagram 5] 1 is a photograph of the inside of a sealant layer of a comparative example observed with an optical microscope. [Figure 6] 1 is a photograph of the surface of a sealant layer of a comparative example observed with an optical microscope. [Figure 7] 3 is a photograph of the inside of the sealant layer of Example 1 observed with an optical microscope. [Figure 8] 2 is a photograph of the surface of the sealant layer of Example 1 observed with an optical microscope. [Figure 9] 1 is a photograph of the inside of the sealant layer of Example 2 observed with an optical microscope. [Figure 10] 3 is a photograph of the surface of the sealant layer of Example 2 observed with an optical microscope. [Figure 11] 1 is a photograph of the inside of the sealant layer of Example 3 observed with an optical microscope. [Figure 12] 1 is a photograph of the surface of the sealant layer of Example 3 observed with an optical microscope. [Figure 13] 1 is a photograph of the inside of the sealant layer of Example 4 observed with an optical microscope. [Figure 14] 1 is a photograph of the surface of the sealant layer of Example 4 observed with an optical microscope. [Figure 15] 1 is a photograph of the inside of the sealant layer of Example 5 observed with an optical microscope. [Figure 16] 1 is a photograph of the surface of the sealant layer of Example 5 observed with an optical microscope. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, the terms and words used in this specification and the claims should not be interpreted in a limited manner to their ordinary or dictionary meanings, but should be interpreted in a meaning and concept that is consistent with the technical idea of the present invention, in accordance with the principle that inventors can appropriately define the concepts of terms in order to best explain their invention.
[0012] Manufacturing method of pouch case for secondary battery The method for producing a pouch case for a secondary battery according to the present invention includes the following steps (S1) to (S3). (S1) A step of preparing a pouch exterior material for a secondary battery including a structure in which a base layer, a barrier layer, and a sealant layer are laminated in this order. (S2) forming a cup portion by molding the pouch exterior material for a secondary battery (S3) Step of reducing cracks in the sealant layer of the pouch exterior material for the secondary battery
[0013] The inventors of the present invention discovered that after molding a pouch exterior material for a secondary battery to form a cup portion, applying heat to the sealant layer of the pouch exterior material for a secondary battery can reduce cracks in the sealant layer and decrease the whitening phenomenon, and thus completed the present invention.
[0014] Specifically, when heat is applied to the sealant layer of the pouch exterior material for a secondary battery after the pouch exterior material for a secondary battery is molded to form a cup portion, the material contained in the sealant layer expands and defects such as cracks and empty spaces present inside the sealant layer can be filled in. This can significantly improve the durability of the sealant layer, and can also significantly improve the durability of the pouch case for a secondary battery including the sealant layer.
[0015] Steps (S1) to (S3) will be described in detail below with reference to the drawings, but the present invention is not limited to those shown in the drawings.
[0016] First, a pouch exterior material for a secondary battery is prepared, which includes a structure in which a base layer, a barrier layer, and a sealant layer are laminated in this order (S1).
[0017] FIG. 1 is a schematic diagram showing a cross section of a pouch exterior material for a secondary battery.
[0018] Referring to FIG. 1, a pouch exterior material 100 for a secondary battery includes a structure in which a base layer 110, a barrier layer 120, and a sealant layer 130 are laminated in this order.
[0019] The substrate layer 110 is disposed on the outermost side of the pouch case for the secondary battery and serves to protect the barrier layer 120, the sealant layer 130, and the electrode assembly (not shown) and electrolyte (not shown) disposed inside the pouch case for the secondary battery from external substances, air, moisture, etc.
[0020] The base layer 110 may include at least one selected from the group consisting of polyethylene, polypropylene, polyethylene terephthalate, and nylon. When the base layer 110 includes the above material, the barrier layer 120, the sealant layer 130, the electrode assembly, the electrolyte, and the like can be effectively protected from external substances, air, moisture, and the like.
[0021] Although not shown in the drawings, the base layer 110 may include two or more layers, specifically, the base layer 110 may include a first layer (not shown) and a second layer (not shown). When the base layer 110 includes two or more layers, the barrier layer 120, the sealant layer 130, the electrode assembly, the electrolyte, and the like may be more effectively protected from external substances, air, or moisture.
[0022] In addition, when the base layer 110 includes the first layer and the second layer, the first layer may include nylon, and the second layer may include polyethylene terephthalate. When the first layer includes nylon, insulation between the barrier layer 120 and the second layer can be further ensured, and when the second layer includes polyethylene terephthalate, foreign matter flowing in from the outside of the pouch case for secondary batteries can be effectively blocked.
[0023] The thickness of the base layer 110 may be 10 μm to 50 μm, specifically 15 μm to 45 μm, and more specifically 18 μm to 35 μm. When the thickness of the base layer 110 satisfies the above numerical range, the base layer 110 will not be damaged and will have excellent insulation properties even when sufficient heat is applied to the sealant layer 130 in step (S3), as described below.
[0024] The barrier layer 120 may function to prevent external substances, air, or moisture from entering the pouch case for the secondary battery.
[0025] The barrier layer 120 may include a metal material, and more specifically, the barrier layer 120 may be an aluminum (Al) alloy. When the barrier layer 120 includes an aluminum alloy, it is possible to effectively block external materials, air, moisture, etc. from entering the pouch case for the secondary battery.
[0026] The thickness of the barrier layer 120 may be 20 μm to 80 μm, specifically 25 μm to 65 μm, and more specifically 30 μm to 60 μm. When the thickness of the barrier layer 120 satisfies the above numerical range, the barrier layer 120 will not be damaged and can have excellent insulation properties even when sufficient heat is applied to the sealant layer 130 in step (S3), as described below.
[0027] The sealant layer 130 is disposed on the innermost side of the pouch case for a secondary battery and may serve to protect the electrode assembly, the electrolyte, etc. Also, the sealant layers 130 may be fused to each other by heat to seal the inside of the pouch case for a secondary battery. As a specific example, when the pouch case for a secondary battery is folded in two parts so that they abut against each other, the sealant layers 130 may come into contact with each other internally, and when heat is applied in that state, the sealant layers 130 may be fused to each other by heat. As a result, the inside of the pouch case for a secondary battery may be sealed.
[0028] The sealant layer 130 may include at least one selected from the group consisting of polyethylene, polypropylene, ethylene propylene copolymer, polypropylene-butylene-ethylene terpolymer, polyethylene-acrylic acid copolymer, and polypropylene-acrylic acid copolymer, and preferably includes polypropylene. When the sealant layer 130 includes such a material, the sealant layers 130 can be effectively fused together by heat, and the electrode assembly and electrolyte disposed inside the pouch case for the secondary battery can be effectively protected.
[0029] The thickness of the sealant layer 130 may be 60 μm to 100 μm, specifically 65 μm to 95 μm, and more specifically 70 μm to 90 μm. When the thickness of the sealant layer 130 satisfies the above numerical range, the sealant layer 130 does not melt easily even when heat is applied to the sealant layer 130 in step (S3), as described below, and a sufficient amount of thermal energy is supplied to effectively reduce or remove defects such as cracks present in the sealant layer 130.
[0030] Meanwhile, although not shown in the drawings, the base layer 110 may include an adhesive layer (not shown). The adhesive layer adheres between the layers to improve the bonding strength. As a result, the base layer 110 can be effectively prevented from being separated from the pouch exterior material 100 for secondary batteries.
[0031] Next, the pouch exterior material 100 for a secondary battery is molded to form a cup portion 210 (S2).
[0032] When the pouch exterior material 100 for a secondary battery is prepared, a stripper and a die are used to fix both ends of the pouch exterior material 100 for a secondary battery. With both ends of the pouch exterior material for a secondary battery fixed, the pouch exterior material 100 for a secondary battery disposed between the both ends is pressed and molded using a punch.
[0033] The molding speed of the pouch exterior material 100 for secondary batteries may be 1 to 100 mm / sec, specifically 5 to 50 mm / sec, and more specifically 10 to 30 mm / sec. When the molding speed satisfies the above numerical range, the pressure applied to the sealant layer 130 per unit time is adjusted to an appropriate level, so that the amount of cracks generated in the sealant layer 130 due to molding can be reduced, and whitening can be reduced.
[0034] When the forming of the pouch exterior material 100 for a secondary battery is completed and the pressed punch is removed, a cup part 210 may be formed between both ends of the pouch exterior material 100 for a secondary battery. The cup part 210 may include a receiving space in which an electrode assembly, etc. can be received.
[0035] FIG. 2 is a schematic diagram showing a cross section of a molded pouch exterior material for a secondary battery.
[0036] 2, the formed pouch exterior material 200 for a secondary battery may include a cup portion 210 and a receiving space 220 defined by the cup portion 210. The cup portion 210 may be formed by being pressed by a punch as described above.
[0037] The cup portion 210 may be in a concave shape including an accommodation space therein, but is not necessarily limited thereto, and the cup portion 210 may be adjusted to various shapes by changing the shape of the punch as necessary.
[0038] The depth d of the cup part 210 may be 4 mm to 10 mm, specifically 5 mm to 9 mm, and more specifically 5.5 mm to 8 mm. The depth d of the cup part 210 may be appropriately adjusted according to the contents to be stored, and even if the depth d of the cup part 210 is formed somewhat deep, cracks can be reduced by applying heat to the sealant layer 130 disposed on the inner surface of the cup part 210 after molding, as described below, and the durability of the manufactured pouch case for a secondary battery can be improved.
[0039] Next, cracks in the sealant layer 130 of the pouch exterior material 100 for a secondary battery are reduced (S3).
[0040] Specifically, heat can be applied to the sealant layer 130 of the pouch exterior material 100 for a secondary battery to reduce cracks in the sealant layer 130. In this case, the material contained in the sealant layer 130 expands due to heat, and defects such as cracks and empty spaces contained in the sealant layer 130 can be filled. This can improve the durability of the manufactured pouch case for a secondary battery.
[0041] In particular, even after the pouch exterior material 100 for a secondary battery has already been formed, when heat is applied to the sealant layer 130, cracks formed in the sealant layer 130 can be filled by the transferred thermal energy. Therefore, even if the molded pouch exterior material 100 for a secondary battery is formed in a state in which the sealant layer 130 has a whitening phenomenon caused by defects such as cracks and has low mechanical strength, the molded pouch exterior material 100 for a secondary battery can be used by improving the mechanical strength of the sealant layer 130 and / or the pouch exterior material 100 for a secondary battery through step (S3) without being discarded.
[0042] When heat is applied to the sealant layer 130 of the pouch exterior material 100 for secondary batteries, the surface temperature of the sealant layer 130 may be 40°C to 110°C, preferably 50°C to 105°C, and more preferably 70°C to 100°C. When the surface temperature of the sealant layer 130 satisfies the above numerical range, cracks formed in the sealant layer 130 may be reduced or completely removed. If the surface temperature of the sealant layer 130 is excessively high, the sealant layer 130 may melt and deform, and if the surface temperature of the sealant layer 130 is excessively low, energy cannot be sufficiently transferred to the sealant layer 130, and the substance contained in the sealant layer 130 cannot expand, making it impossible to reduce cracks.
[0043] The method of applying heat may be, for example, irradiating the sealant layer 130 with infrared rays or using a heating block to conduct heat to the sealant layer 130. The method of irradiating infrared rays has the advantage that heat transfer is uniform.
[0044] The wavelength of the infrared ray may be 1 μm to 100 μm, and the irradiation time of the infrared ray may be 1 to 60 seconds. Preferably, the wavelength of the infrared ray may be 2.5 μm to 50 μm, and the irradiation time of the infrared ray may be 4 to 32 seconds, and more preferably 16 to 32 seconds. When the irradiation time of the infrared ray satisfies the above numerical range, the sealant layer 130 does not melt, and cracks present inside the sealant layer 130 can be reduced and completely removed.
[0045] The area to which the heat is applied may be the entire area of the sealant layer 130 disposed on the inner surface of the cup portion 210, and in this case, defects such as cracks and microvoids present inside the sealant layer 130 may be generally reduced or eliminated.
[0046] In addition, the area to which heat is applied may be a portion of the sealant layer 130 disposed on the inner surface of the cup portion 210. Specifically, when the area to which heat is applied is a portion of the sealant layer 130 that is bent by molding in the (S2) step, it is possible to reduce whitening in areas where defects such as cracks and microvoids are concentrated in the pouch exterior material 100 for secondary batteries, and to improve the mechanical strength or durability of the sealant layer 130.
[0047] The region to which heat is applied may be, for example, at least one of a first region 300A, a second region 300B, and a third region 300C described below, and is preferably the first region 300A.
[0048] FIG. 3 is an enlarged view of the inner side surface of the cup portion 210 of the molded pouch exterior material 200 for a secondary battery shown in FIG.
[0049] 1 to 3, the inner surface of the cup part 210 includes a first region 300A, a second region 300B, and a third region 300C. In addition, the first region 300A, the second region 300B, and the third region 300C may each be a part of the sealant layer 130.
[0050] The first region 300A is the upper end of the inner surface of the cup portion 210, the second region 300B is the center of the inner surface of the cup portion 210, and the third region 300C is the lower end of the inner surface of the cup portion 210.
[0051] Specifically, the first region 300A may be a region from 0.2d to 0.3d from the top end of the cup portion 210 based on the depth d of the cup portion 210, the second region 300B may be a region from 0.4d to 0.5d from an end of the first region 300A, and the third region 300C may be a region from 0.2d to 0.3d from an end of the second region 300B.
[0052] The first region 300A is a region where the cup portion 210 starts to be formed and where bending occurs due to punching in step (S2). The first region 300A is a region where many defects such as cracks occur, and the degree of whitening may increase and the mechanical strength may decrease.
[0053] The second region 300B is a central portion of the inner surface of the cup part 210, where bending does not occur, and the third region 300C is a lower end portion of the inner surface of the cup part 210, where bending does not occur. The second region 300B and the third region 300C are less deformed by molding than the first region 300A, so that defects such as cracks are relatively less likely to occur. This can reduce the degree of whitening of the second region 300B and the third region 300C, and can somewhat increase the mechanical strength.
[0054] Meanwhile, the area to which the heat is applied may be the first area 300A, which is the upper end of the inner surface of the cup portion 210, and as a specific example of a method of applying heat, the area to which the infrared rays are applied may be the first area 300A, which is the upper end of the inner surface of the cup portion 210.
[0055] As described above, the first region 300A is a region where many defects such as cracks occur due to the large degree of deformation caused by molding, and the infrared rays are irradiated to the first region 300A, thereby effectively reducing or removing defects such as cracks and empty spaces present in the sealant layer 130. As a result, relatively weak parts of the pouch case for a secondary battery to be manufactured can be reinforced, and the durability of the pouch case for a secondary battery can be improved.
[0056] The region to which heat is applied may be an edge of the cup portion 210, which extends horizontally in the sealant layer 130. The edge of the cup portion 210, which extends horizontally in the sealant layer 130, may be more susceptible to cracks than other portions because it extends vertically during molding, and by applying heat after molding, the formed cracks can be removed in a concentrated manner to improve durability. Regions H1 and H2 to which heat is applied are illustrated in FIG. 4 as examples.
[0057] The present invention will now be described in detail with reference to examples, but the present invention is not limited to the following examples.
[0058] Example 1 (S1) Step: Preparing a pouch exterior material for a secondary battery including a structure in which a base layer, a barrier layer, and a sealant layer are laminated in this order A pouch exterior material for a secondary battery was prepared, including a structure in which a 15 μm-thick nylon layer was laminated as a first layer of the base material layer, a 12 μm-thick polyethylene terephthalate layer was laminated as a second layer of the base material layer, a 40 μm-thick aluminum alloy layer was laminated as a barrier layer, and an 80 μm-thick polypropylene layer was laminated as a sealant layer. Adhesive layers were disposed between the first layer and the second layer, and between the barrier layer and the first layer.
[0059] (S2) Step: Forming a cup portion by molding the pouch exterior material for secondary batteries The pouch exterior material for a secondary battery was placed in a molding device so that the base layer was placed at the bottom and the sealant layer was placed at the top, and then both ends of the pouch exterior material for a secondary battery were fixed using a stripper and a die, and the pouch exterior material for a secondary battery was molded using a punch to form a cup portion. Here, the molding speed was 15 mm / sec, and the molding depth was 5.7 mm.
[0060] (S3) Step: Reducing cracks in the sealant layer of the pouch exterior material for the secondary battery to manufacture a pouch case for the secondary battery. Heat was applied to the sealant layer of the molded pouch exterior material for secondary batteries to reduce cracks present in the sealant layer. In the examples, a method of irradiating the sealant layer with infrared rays using an infrared lamp was used.
[0061] The molded pouch exterior material for secondary batteries was placed in place, and an infrared lamp was placed at a position 5 cm away from it. The wavelength of the infrared lamp was set to 2.5 to 50 μm, and the output of the infrared lamp was set to 200 W.
[0062] Using the infrared lamp, infrared rays were irradiated to the upper and lower ends of the edge of the cup part where the length of the sealant layer extends in the horizontal direction (areas indicated by H1 and H2 in FIG. 4). The infrared rays were irradiated for 4 seconds, and the infrared rays were irradiated so that the surface temperature of the sealant layer reached about 40°C.
[0063] Example 2 A pouch case for a secondary battery was manufactured in the same manner as in Example 1, except that in step (S3), the infrared ray irradiation time using an infrared lamp was 12 seconds and the infrared ray irradiation was performed so that the surface temperature of the sealant layer reached about 60°C.
[0064] Example 3 A pouch case for a secondary battery was manufactured in the same manner as in Example 1, except that in step (S3), the infrared ray irradiation time using an infrared lamp was 20 seconds and the infrared ray irradiation was performed so that the surface temperature of the sealant layer reached about 80°C.
[0065] Example 4 A pouch case for a secondary battery was manufactured in the same manner as in Example 1, except that in step (S3), the infrared ray irradiation time using an infrared lamp was 28 seconds, and the infrared ray irradiation was performed so that the surface temperature of the sealant layer reached about 100°C.
[0066] Example 5 A pouch case for a secondary battery was manufactured in the same manner as in Example 1, except that in step (S3), the infrared ray irradiation time using an infrared lamp was 50 seconds and the infrared ray irradiation was performed so that the surface temperature of the sealant layer reached about 150°C.
[0067] Comparative Example A pouch case for a secondary battery was produced in the same manner as in Example 1, except that infrared rays were not irradiated using an infrared lamp in the step (S3).
[0068] Experimental example - Crack level evaluation The sealant layers of the pouch cases for secondary batteries of Examples 1 to 5 and Comparative Example were evaluated for crack levels. Figure 4 shows the positions where the crack levels were evaluated.
[0069] 4 is a plan view of the molded pouch exterior material for secondary batteries. A portion M corresponding to the upper end of the inner surface of the cup portion 410 was cut into a size of 3 cm x 2.5 cm at a horizontal distance of about 2 cm from one apex P of the cup portion 410 of each pouch exterior material for secondary batteries 400 to prepare a test piece. The test piece was attached to a slide glass, and then cracks were observed using an optical microscope.
[0070] Optical microscope photographs of Examples 1 to 5 and Comparative Example are shown in FIGS. 5 to 16, and the experimental results are summarized in Table 1 below.
[0071] [Table 1]
[0072] In Table 1, the crack levels inside the sealant layer and on the surface of the sealant layer were determined by visually checking the presence of cracks in photographs taken with an optical microscope, and the level was indicated on a scale of 0 to 5. The level increases from 0 to 5, indicating a greater number of cracks.
[0073] As a result of the experiment, it was confirmed that in the comparative example, infrared rays were not irradiated after the pouch outer casing for secondary batteries was formed, and in the cases of Examples 1 and 2, the time for infrared irradiation was somewhat short, so that although some of the cracks inside the sealant layer and on the surface of the sealant layer were filled, they were not completely filled and some of them remained.
[0074] In the case of Examples 3 and 4, it was confirmed that after the pouch exterior material for secondary batteries was formed, the time for infrared irradiation was appropriately set, and a sufficient level of heat was transferred to the sealant layer, thereby causing the internal material of the sealant layer to expand and removing all cracks.
[0075] In the case of Example 5, after forming the pouch exterior material for a secondary battery, infrared rays were irradiated to transfer a sufficient level of heat to the sealant layer, which caused the internal material of the sealant layer to expand and all cracks to be removed, but physical deformation such as curling occurred in the base material layer or barrier layer of the pouch exterior material for a secondary battery. [Explanation of symbols]
[0076] 100 Pouch exterior material for secondary batteries 110 Base material layer 120 Barrier Layer 130 Sealant Layer 200 Pouch exterior material for secondary batteries 210 Cup section 220 Containment Space 300A 1st area 300B 2nd area 300C 3rd area 400 Pouch exterior material for secondary batteries 410 Cup section 420 Containment Space M Measurement site P Vertex
Claims
1. (S1) preparing a pouch exterior material for a secondary battery including a structure in which a base layer, a barrier layer, and a sealant layer are laminated in this order; (S2) forming a cup portion by molding the pouch exterior material for a secondary battery; (S3) a step of reducing cracks in the sealant layer of the secondary battery pouch exterior material.
2. The method for manufacturing a pouch case for a secondary battery according to claim 1 , wherein in the step (S3), heat is applied to the sealant layer to reduce cracks in the sealant layer.
3. 3. The method for manufacturing a pouch case for a secondary battery according to claim 2, wherein in the step (S3), a surface temperature of the sealant layer is 40° C. to 110° C.
4. The method for producing a pouch case for a secondary battery according to claim 2 , wherein in the step (S3), heat is applied to the sealant layer by irradiating it with infrared rays.
5. 5. The method for manufacturing a pouch case for a secondary battery according to claim 4, wherein the infrared ray has a wavelength of 1 to 100 μm, and the infrared ray irradiation time is 1 to 60 seconds.
6. 3. The method for manufacturing a pouch case for a secondary battery according to claim 2, wherein in the step (S3), the region to which heat is applied is an edge of a cup portion extending horizontally in length in the sealant layer.
7. 2. The method for manufacturing a pouch case for a secondary battery according to claim 1, wherein in the step (S2), the depth of the cup portion is 4 mm to 10 mm.
8. 2. The method for producing a pouch case for a secondary battery according to claim 1, wherein in the step (S2), a speed for forming the pouch exterior material for a secondary battery is 1 to 100 mm / sec.
9. 2. The method for producing a pouch case for a secondary battery according to claim 1, wherein the sealant layer includes at least one selected from the group consisting of polyethylene; polypropylene; ethylene-propylene copolymer; polypropylene-butylene-ethylene terpolymer; polyethylene-acrylic acid copolymer; and polypropylene-acrylic acid copolymer.
10. The method for manufacturing a pouch case for a secondary battery according to claim 1, wherein the sealant layer has a thickness of 60 μm to 100 μm.
11. The method for producing a pouch case for a secondary battery according to claim 1 , wherein the barrier layer is an aluminum (Al) alloy.
12. 2. The method for producing a pouch case for a secondary battery according to claim 1, wherein the barrier layer has a thickness of 20 μm to 80 μm.
13. 2. The method for producing a pouch case for a secondary battery according to claim 1, wherein the base layer comprises at least one selected from the group consisting of polyethylene; polypropylene; polyethylene terephthalate; and nylon.
Citation Information
Patent Citations
Method of manufacturing thin battery
JP2002231196A
Outer package body for battery and its manufacturing method
JP2002343311A
Manufacturing method of flat electrochemical cell
JP2008041403A
Battery packaging material
JP2016225301A
Forming apparatus for pouche
KR101837234B1