Method for manufacturing lithium secondary battery and lithium secondary battery manufactured by the same
The method of forming cobalt and boron coatings on lithium composite transition metal oxides addresses the irreversible capacity loss in silicon-based lithium secondary batteries, enhancing capacity and service life by stabilizing the electrode structure and reducing resistance.
Patent Information
- Application Number
- JP2024534102
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-23
- Filing Date
- 2022-12-21
- Publication Date
- 2024-12-05
AI Technical Summary
Lithium secondary batteries face challenges with high irreversible capacity loss during initial charging and discharging due to the use of silicon-based negative electrode materials, leading to reduced capacity and structural collapse, and existing cathode materials like lithium nickel-based oxides are expensive and generate excessive lithium by-products.
A manufacturing method involving the formation of a cobalt and boron coating on a lithium composite transition metal oxide to create a positive electrode active material, which includes a cobalt coating layer formed at 550°C to 700°C and a boron coating layer at 400°C to 500°C, enhancing the electrode's stability and reducing irreversible capacity loss.
The method compensates for irreversible capacity loss, improving the capacity and service life of lithium secondary batteries by using a high-capacity silicon-based negative electrode material without the need for a sacrificial positive electrode material, while maintaining structural integrity and reducing resistance.
Smart Images

Figure 2024545107000001_ABST
Abstract
Description
[Technical field]
[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0186454, filed December 23, 2021, and all contents disclosed in the documents of that Korean patent application are incorporated herein by reference.
[0002] The present invention relates to a method for producing a lithium secondary battery and a lithium secondary battery produced thereby. [Background technology]
[0003] Recently, with the rapid spread of electronic devices using batteries, such as mobile phones, notebook computers, and electric vehicles, the demand for secondary batteries that are small, lightweight, and have a relatively high capacity is rapidly increasing. In particular, lithium secondary batteries are lightweight and have high energy density, and are in the spotlight as a driving power source for portable devices. Therefore, active research and development efforts are being made to improve the performance of lithium secondary batteries.
[0004] Carbonaceous materials such as graphite are mainly used as anode materials for lithium secondary batteries, but carbonaceous materials have a drawback in that it is difficult to increase the capacity of lithium secondary batteries because the capacity per unit mass is low. Therefore, materials that form inter-metallic compounds with lithium, such as silicon, tin, and oxides of these, have been developed and used as non-carbonaceous anode materials that have a higher capacity than carbonaceous materials, but these anode materials have a problem in that they suffer a large irreversible capacity loss during initial charging and discharging.
[0005] To solve this problem, methods have been proposed that use a material that can provide a lithium ion source or reservoir as a positive electrode material and that is electrochemically active after the first cycle so as not to degrade the overall battery performance, thereby solving the irreversible capacity loss of the negative electrode. Specifically, there is a method of using a lithium nickel-based oxide such as Li2NiO2 as a sacrificial positive electrode material or an overdischarge prevention agent in the positive electrode.
[0006] However, most of the lithium nickel-based oxides are expensive and have problems such as generating a large amount of lithium by-products and thus generating a large amount of gas. Therefore, an alternative method is required. Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention aims to provide a method for manufacturing a lithium secondary battery that can ultimately increase capacity without reducing resistance and life characteristics by introducing a low-efficiency cathode material that can compensate for the problem of anode materials that have high irreversible capacity loss during initial charge and discharge. [Means for solving the problem]
[0008] The present invention relates to (1) mixing a transition metal precursor and a lithium source material, and then calcining the mixture to produce a lithium transition metal composite oxide; (2) mixing the lithium composite transition metal oxide with a cobalt-containing raw material and heat-treating the mixture at 550°C to 700°C to form a cobalt coating layer on the lithium composite transition metal oxide; (3) mixing the lithium composite transition metal oxide on which the cobalt coating layer is formed with a boron-containing raw material and heat-treating the mixture at 400°C to 500°C to produce a positive electrode active material including a boron coating layer; (4) coating the positive electrode active material onto a positive electrode current collector to produce a positive electrode; (5) assembling the positive electrode, a negative electrode including a silicon-based negative electrode active material, and a separator, and injecting an electrolyte; The present invention provides a method for producing a lithium secondary battery comprising the steps of:
[0009] The present invention also provides a lithium secondary battery including a positive electrode containing a positive electrode active material, a negative electrode containing a silicon-based negative electrode active material, a separator, and an electrolyte, The positive electrode active material includes a lithium composite transition metal oxide having a cobalt coating layer and a boron coating layer formed thereon, The particle strength of the positive electrode active material is 80 MPa to 250 MPa, The positive electrode active material contains LiOH and Li2CO3 on the surface of the particles, The total content of the LiOH and Li2CO3 is 0.4 wt % to 1.1 wt % based on the total content of the positive electrode active material. Effect of the Invention
[0010] The method for producing a lithium secondary battery according to the present invention uses a high-capacity silicon-based negative electrode active material and compensates for the problem of irreversible capacity loss without a separate sacrificial positive electrode material, thereby making it possible to produce a lithium secondary battery with excellent capacity and life. [Brief description of the drawings]
[0011] [Figure 1] 3 is a photograph of the surface of the positive electrode active materials produced in Examples 1 to 4 taken with a scanning electron microscope (SEM). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] In the following, the present invention will be described in more detail in order to facilitate understanding of the present invention.
[0013] In the present invention, the term "primary particle" refers to a particle unit that does not have grain boundaries when observed at a magnification of 5,000 to 20,000 times using a scanning electron microscope. The term "average particle size of primary particles" refers to the arithmetic mean value calculated after measuring the particle size of primary particles observed in a scanning electron microscope image.
[0014] In the present invention, the "secondary particles" are particles formed by agglomeration of a plurality of primary particles.
[0015] In the present invention, the "average particle size D 50" means the particle size at 50% of the volume cumulative particle size distribution of the lithium composite transition metal oxide powder or the positive electrode active material powder, and means the average particle size of the secondary particles. 50 can be measured using a laser diffraction method. For example, the lithium composite transition metal oxide powder or the positive electrode active material powder is dispersed in a dispersion medium, introduced into a commercially available laser diffraction particle size measuring device (e.g., Microtrac MT 3000), and irradiated with ultrasonic waves of about 28 kHz at an output of 60 W. Then, a volume cumulative particle size distribution graph is obtained, and the particle diameter corresponding to 50% of the volume cumulative amount is obtained.
[0016] In the present invention, "particle strength" refers to the force, expressed in pressure units (MPa), at which a particle breaks when a positive active material powder is placed in a micro compression testing machine (MCT-W500, manufactured by Shimadzu) and the particle shape of the positive active material to be measured under a microscope is secured, and then a force is applied to the positive active material particle with a tip. Taking into account the deviation between particles, values measured 30 or more times are mapped, and the average value is used as the particle strength value.
[0017] The method for producing a lithium secondary battery of the present invention includes the following steps (1) to (5).
[0018] (1) mixing a transition metal precursor and a lithium source material, and then calcining the mixture to prepare a lithium composite transition metal oxide; (2) mixing the lithium composite transition metal oxide with a cobalt-containing raw material and heat-treating the mixture at 550°C to 700°C to form a cobalt coating layer on the lithium composite transition metal oxide; (3) mixing the lithium transition metal composite oxide on which the cobalt coating layer is formed with a boron-containing raw material, and heat-treating the mixture at 400°C to 500°C to prepare a positive electrode active material having a boron coating layer; (4) coating the positive electrode active material onto a positive electrode current collector to produce a positive electrode; and (5) Assembling the positive electrode, the negative electrode containing a silicon-based negative electrode active material, and a separator, and injecting an electrolyte.
[0019] To develop high-capacity cells, it is essential to use silicon-based anode active materials with high capacity, but silicon-based anode active materials have the disadvantages of low charge / discharge efficiency of less than 85% and high lithium ion loss rate due to irreversible reactions. This leads to a large loss of lithium in the cathode active material, which can rapidly reduce the capacity of the battery during charge / discharge and can even lead to the collapse of the cathode active material structure.
[0020] Therefore, in the present invention, a low-efficiency positive electrode active material capable of providing lithium to a silicon-based negative electrode active material during initial charge and discharge is developed, so that even if an irreversible event occurs in which lithium ions are not released after being desorbed from the positive electrode active material and inserted into the negative electrode active material, the life and resistance characteristics of the battery are not reduced.
[0021] In addition, they confirmed that by adjusting the cobalt coating conditions, the size of the primary particles of the positive electrode active material can be increased, reducing the amount of fine powder generated during electrode rolling and improving high-temperature life.
[0022] The method for manufacturing a lithium secondary battery according to the present invention provides a cathode material that has low initial charge / discharge efficiency, can reduce the consumption of lithium ions, and has improved output by applying a boron (B) and cobalt (Co) composite coating.
[0023] Each step will be explained in detail below.
[0024] <Production of positive electrode active material> The positive electrode active material of the present invention can be produced by the above steps (1) to (3).
[0025] In step (1), a transition metal precursor and a lithium source material are mixed and then calcined to prepare a lithium composite transition metal oxide, where the precursor may be a commercially available precursor or may be prepared by a precursor preparation method well known in the art.
[0026] For example, the precursor may be prepared by introducing an aqueous solution of a transition metal, an ammonium cation complexing agent, and a basic compound into a reactor and carrying out a coprecipitation reaction while stirring.
[0027] The transition metal aqueous solution may be prepared by dissolving a transition metal-containing source material in a solvent such as water, for example, by dissolving a nickel-containing source material, a cobalt-containing source material, a manganese-containing source material, and / or an aluminum-containing source material in water.
[0028] Meanwhile, the transition metal-containing raw material may be an acetate, carbonate, nitrate, sulfate, halide, sulfide, or oxide of a transition metal.
[0029] Specifically, the nickel-containing source material can be, for example, NiO, NiCO3·2Ni(OH)2·4H2O, NiC2O2·2H2O, Ni(NO3)2·6H2O, NiSO4, NiSO4·6H2O, nickel halides, or combinations thereof.
[0030] The cobalt-containing source material can be, for example, CoSO4, Co(OCOCH3)2·4H2O, Co(NO3)2·6H2O, CoSO4·7H2O, or combinations thereof.
[0031] The manganese-containing source material can be, for example, Mn2O3, MnO2, Mn3O4, MnCO3, Mn(NO3)2, MnSO4·H2O, manganese acetate, manganese halides, or combinations thereof.
[0032] The aluminum-containing source material may be, for example, Al2O3, Al(OH)3, Al(NO3)3, Al2(SO4)3, (HO)2AlCH3CO2, HOAl(CH3CO2)2, Al(CH3CO2)3, aluminum halide, or a combination thereof. However, in the case of Al, it may be added together with the lithium source material in the calcination step described below, without being added to the transition metal aqueous solution.
[0033] Here, the input amount of each of the transition metal-containing raw materials may be determined in consideration of the molar ratio of the transition metal in the final cathode active material to be produced.
[0034] Meanwhile, the ammonium cation complexing agent may include at least one compound selected from the group consisting of NH4OH, (NH4)2SO4, NH4NO3, NH4Cl, CH3COONH4, and (NH4)2CO3, and may be added to the reactor in the form of a solution in which the compound is dissolved in a solvent, where the solvent may be water or a mixture of water and an organic solvent (e.g., alcohol, etc.) that is uniformly miscible with water.
[0035] The basic compound may be at least one compound selected from the group consisting of NaOH, KOH, and Ca(OH)2, and may be added to the reactor in the form of a solution in which the compound is dissolved in a solvent, where the solvent may be water or a mixture of water and an organic solvent (e.g., alcohol, etc.) that is uniformly miscible with water.
[0036] As described above, when the aqueous transition metal solution, the ammonium cation complex forming agent and the basic compound are charged into a reactor and stirred, the transition metal in the aqueous transition metal solution is coprecipitated to produce precursor particles in the form of transition metal hydroxide.
[0037] Here, the aqueous transition metal solution, the ammonium cation complex forming agent and the basic compound are added in amounts such that the pH of the reaction solution falls within a desired range.
[0038] When the precursor particles are formed by the above-mentioned method, they are separated from the reaction solution to obtain the precursor. For example, the reaction solution is filtered to separate the precursor from the reaction solution, and the separated precursor is washed with water and dried to obtain the precursor. At this time, steps such as pulverization and / or classification may be performed as necessary.
[0039] The lithium source material may be a lithium-containing sulfate, nitrate, acetate, carbonate, oxalate, citrate, halide, hydroxide, or oxyhydroxide, for example, Li2CO3, LiNO3, LiNO2, LiOH, LiOH·H2O, LiH, LiF, LiCl, LiBr, LiI, CH3COOLi, Li2O, Li2SO4, CH3COOLi, Li3C6H5O7, or a mixture thereof.
[0040] Meanwhile, the lithium source material and the precursor may be mixed so that the molar ratio of Li:total metals in the precursor is 1:1 to 1.2:1, preferably 1:1 to 1.1:1. When the mixing ratio of the lithium source material and the metals in the precursor satisfies the above range, the layered crystal structure of the lithium composite transition metal oxide is well developed, and a positive electrode active material having excellent capacity characteristics and structural stability can be produced.
[0041] After mixing the precursor and the lithium source material, the mixture is fired at 700° C. to 800° C. to form a lithium composite transition metal oxide. The mixture is more preferably fired at 710° C. to 780° C., and even more preferably fired at 730° C. to 760° C., for 5 hours to 20 hours, and more preferably fired for 8 hours to 15 hours. Meanwhile, a source material containing a doping element M can be further mixed during the firing, if necessary.
[0042] In step (2), the lithium composite transition metal oxide is mixed with a cobalt-containing raw material and heat-treated at 550°C to 700°C for 4 to 10 hours to form a cobalt coating layer on the lithium composite transition metal oxide. In the present invention, the introduction of the cobalt coating layer reduces the reactivity between the positive electrode active material surface and the electrolyte, thereby suppressing the deterioration of the surface structure that may occur during the charge / discharge process, and ultimately improving the high-temperature life and resistance increase. However, if the cobalt coating temperature is less than 550°C, the cobalt coating layer cannot be formed normally, and cobalt oxide is formed, which may cause a decrease in capacity and an increase in resistance.
[0043] The cobalt-containing raw material may be one or more selected from the group consisting of Co3O4, Co(OH)2, Co2O3, Co3(PO4)2, CoF3, Co(OCOCH3)2·4H2O, Co(NO3)2·6H2O, Co(SO4)2·7H2O, and CoC2O4.
[0044] The difference between the calcination temperature in step (1) and the heat treatment temperature in step (2) may be less than 100° C. In this case, recrystallization of the lithium transition metal composite oxide may occur during the heat treatment process in step (2), and the size of the primary particles may be increased by adjusting the conditions in step (2).
[0045] In addition, the heat treatment in step (2) may include a first heat treatment and a second heat treatment performed at a temperature lower than that of the first heat treatment. That is, the heat treatment may be performed in two steps, specifically, the first heat treatment may be performed at 650°C to 700°C for 2 hours to 6 hours, and the second heat treatment may be performed at 550°C to 650°C for 1 hour to 3 hours. In this way, when the heat treatment is performed in two steps, it is easier to control the size of the primary particles compared to the case of performing the heat treatment in one step at a predetermined temperature, specifically, the size of the primary particles can be increased by recrystallization of the crystal structure during the first heat treatment at a high temperature, and the cobalt coating layer can be uniformly formed on the surface of the positive electrode active material by performing the second heat treatment at a low temperature.
[0046] In the step (2), the cobalt-containing raw material may be mixed in an amount of 0.5 wt% to 3 wt%, preferably 0.8 wt% to 2 wt%, and more preferably 1.2 wt% to 1.8 wt% based on the total content of the lithium composite transition metal oxide. When the amount of the cobalt-containing raw material is 0.5 wt% to 3 wt% based on the total content of the lithium composite transition metal oxide, it is preferable in that a uniform coating layer can be formed on the surface of the positive electrode active material, lithium migration during charge / discharge is not hindered, and an increase in initial resistance can be suppressed.
[0047] In step (3), the lithium composite transition metal oxide on which the cobalt coating layer is formed is mixed with a boron-containing raw material, and the mixture is heat-treated at 400°C to 500°C, preferably 420°C to 480°C, for 3 to 8 hours to produce a positive electrode active material containing a boron coating layer. The boron coating in step (3) forms an LBO phase (lithium boron oxide phase) on the surface of the positive electrode active material. The LBO phase has high ionic conductivity, which increases the capacity of the battery and reduces resistance, and has low electrical conductivity, which suppresses side reactions between the surface of the positive electrode and the electrolyte. In particular, in the present invention, the heat treatment temperature in step (3) is set to 400°C or higher, which allows the lithium in the lattice to move to the surface, increases the amount of residual lithium, and the residual lithium by-product acts as a resistance layer, thereby reducing the initial efficiency. However, at temperatures above 500°C, soluble lithium is lost as lithium migrates from the lattice to the surface, which can result in a significant decrease in capacity, and the LBO phase cannot be uniformly formed on the surface of the active material, with some boron existing in the form of B2O3, resulting in a decrease in residual lithium and capacity and an increase in resistance during battery operation.
[0048] The boron-containing raw materials include H3BO3, B2O3, B4C, BF3, (C3H7O)3B, (C6H5O)3B, [CH3(CH2)3O]3B, C 13 H 19 It may be any one or more selected from the group consisting of O3, C6H5B(OH)2 and B2F4, and preferably H3BO3.
[0049] In the step (3), the boron-containing raw material may be mixed in an amount of 0.05 wt% to 0.5 wt%, preferably 0.07 wt% to 0.2 wt%, based on the total content of the lithium composite transition metal oxide on which the cobalt coating layer is formed. When the content of the boron-containing raw material is 0.05 wt% to 0.5 wt% based on the total content of the lithium composite transition metal oxide on which the cobalt coating layer is formed, it is preferable in that a uniform coating layer can be formed on the surface of the positive electrode active material.
[0050] The mixing in steps (2) and (3) can each be a dry mixing in which mixing is performed without using a solvent.
[0051] In the present invention, the lithium transition metal composite oxide may have a nickel content of 60 mol % or more, preferably 70 mol % or more, and more preferably 80 mol % or more, among transition metals.
[0052] In addition, the lithium composite transition metal oxide may be represented by the following Chemical Formula 1.
[0053] [Chemical formula 1] Li 1+x (Ni a Co b Mn c M d )O2
[0054] In the above Chemical Formula 1, M is at least one selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; x, a, b, c, and d are -0.2≦x≦0.2, 0.50≦a<1, 0 <b≦0.40、0<c≦0.40、0≦d≦0.1、a+b+c+d=1である。
[0055] Preferably, a, b, c and d are 0.60≦a<1, 0 <b≦0.30、0<c≦0.30、0≦d≦0.1、または0.70≦a<1、0<b≦0.20、0<c≦0.20、0≦d≦0.1、または0.80≦a<1、0<b≦0.15、0<c≦0.15、0≦d≦0.05であることができる。
[0056] <Production of positive electrodes> In step (4) of the present invention, the positive electrode active material is coated on a positive electrode current collector to produce a positive electrode. This can be performed according to a typical positive electrode production method, except for using the above-mentioned positive electrode active material. Specifically, the positive electrode can be produced by coating a positive electrode slurry containing the above-mentioned positive electrode active material, a binder, and a conductive material on a positive electrode current collector, followed by drying and rolling.
[0057] The positive electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity. For example, stainless steel; aluminum; nickel; titanium; calcined carbon; or aluminum or stainless steel whose surface has been surface-treated with carbon, nickel, titanium, silver, or the like may be used.
[0058] The solvent of the positive electrode slurry may be an organic solvent such as N-methyl-2-pyrrolidone (NMP) and may be used in an amount that provides a desired viscosity. For example, the positive electrode slurry may be contained in such a manner that the solid content concentration is 10% by weight to 90% by weight, preferably 40% by weight to 85% by weight.
[0059] The binder in the positive electrode slurry is a component that helps to bind the positive electrode material and the conductive material and to bind the current collector, and is usually added in an amount of 1% by weight to 30% by weight based on the total weight of the solid content in the positive electrode slurry. Examples of such binders include polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene termonomer, styrene-butadiene rubber, fluororubber, and various copolymers thereof.
[0060] The conductive material in the positive electrode slurry is a substance that does not cause a chemical change in the battery and provides conductivity, and may be added in an amount of 0.5 wt % to 20 wt % based on the total weight of the solid content of the positive electrode slurry.
[0061] Examples of the conductive material that can be used include carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; graphite powder such as natural graphite, artificial graphite, and graphite with a highly developed crystal structure; conductive fibers such as carbon fibers and metal fibers; conductive powders such as carbon fluoride powder, aluminum powder, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.
[0062] The positive electrode active material may be included in an amount of 80 wt% to 99 wt%, specifically 90 wt% to 99 wt%, based on the total weight of the solid content of the positive electrode slurry. If the content of the positive electrode active material is less than 80 wt%, the energy density may be reduced, resulting in a decrease in capacity.
[0063] <Manufacturing lithium secondary batteries> In step (5) of the present invention, it includes the steps of assembling the positive electrode, the negative electrode containing the silicon-based negative electrode active material, and the separator, and injecting the electrolyte. This can be carried out according to the manufacturing method of a normal lithium secondary battery except for using the above-mentioned positive electrode. For example, a separator is interposed between the positive electrode and the negative electrode containing the silicon-based negative electrode active material and laminated and dried in sequence to manufacture an electrode assembly. Next, after inserting the electrode assembly into a case, a lithium secondary battery can be manufactured by injecting and sealing the electrolyte.
[0064] The negative electrode according to the present invention contains a silicon-based negative electrode active material, and can be manufactured by coating a negative electrode slurry containing a negative electrode active material, a binder, a conductive material, a solvent, etc. on a negative electrode current collector, and then drying and rolling.
[0065] The negative electrode current collector generally has a thickness of 3 μm to 500 μm. Such a negative electrode current collector is not particularly limited as long as it does not cause a chemical change to the battery and has high conductivity. For example, copper, stainless steel, aluminum, nickel, titanium, fired carbon, those with a surface treatment of carbon, nickel, titanium, silver, etc. on the surface of copper or stainless steel, aluminum-cadmium alloy, etc. can be used. Also, similar to the positive electrode current collector, fine irregularities can be formed on the surface to strengthen the binding force of the negative electrode active material, and it can be used in various forms such as films, sheets, foils, meshes, porous bodies, foams, non-woven fabrics, etc.
[0066] In the present invention, the silicon-based negative electrode active material can be any one or more selected from the group consisting of Si, SiO x (0 < x < 2) and Si-containing alloys, and preferably can be SiO.
[0067] The Si-containing alloy can be an alloy of an element selected from Si and an alkali metal, an alkaline earth metal, a Group 13 element, a Group 14 element, a transition metal, a rare earth element, and combinations thereof.
[0068] Silicon-based anode active materials have a capacity approximately 10 times higher than that of graphite, and a mass loading (mg cm -2 ) and improve the fast charging performance of the battery. However, there is a problem of high lithium ion loss rate due to irreversible reaction, but this problem can be solved by applying the above-mentioned positive electrode.
[0069] The negative electrode of the present invention may further include a carbon-based negative electrode active material in addition to the silicon-based negative electrode active material. Any carbon-based negative electrode active material commonly used in lithium ion secondary batteries may be used without particular limitation, and representative examples thereof include crystalline carbon, amorphous carbon, or both. Examples of the crystalline carbon include graphite such as amorphous, plate-like, flake-like, spherical, or fibrous natural graphite and artificial graphite, and examples of the amorphous carbon include soft carbon (low-temperature calcined carbon), hard carbon, mesophase pitch carbide, and calcined coke.
[0070] In the present invention, the silicon-based negative electrode active material may be included in an amount of 1 wt % to 100 wt %, preferably 3 wt % to 10 wt %, based on the total weight of the negative electrode active material.
[0071] The negative electrode active material may be included in an amount of 80% by weight to 99% by weight based on the total weight of the solid content of the negative electrode slurry.
[0072] The binder is a component that helps bind the conductive material, the negative electrode active material, and the current collector, and may be added in an amount of 1 wt% to 30 wt% based on the total weight of the solid content of the negative electrode slurry. Examples of such binders include polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer, styrene-butadiene rubber, fluororubber, and various copolymers thereof.
[0073] The conductive material is a component for further improving the conductivity of the negative electrode active material, and may be added in an amount of 1 wt% to 20 wt% based on the total weight of the solid content of the negative electrode slurry. Such a conductive material is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity, and examples thereof include carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, or thermal black; graphite powder such as natural graphite, artificial graphite, or graphite with a highly developed crystal structure; conductive fibers such as carbon fibers or metal fibers; conductive powders such as carbon fluoride powder, aluminum powder, or nickel powder; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; or conductive materials such as polyphenylene derivatives.
[0074] The solvent for the negative electrode slurry may include water or an organic solvent such as NMP or alcohol, and may be used in an amount that provides a preferred viscosity when the negative electrode active material, binder, conductive material, etc. are included. For example, the solvent may be included so that the solid content concentration in the slurry containing the negative electrode active material, binder, and conductive material is 50% by weight to 75% by weight, preferably 50% by weight to 65% by weight.
[0075] The separator can be any separator that separates the positive electrode and the negative electrode, provides a path for lithium ions to move, and is generally used as a separator in a lithium secondary battery. In particular, it is preferable that the separator has low resistance to ion movement of the electrolyte and has excellent electrolyte humidification ability. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin-based polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminate structure of two or more layers thereof, can be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of high-melting glass fiber, polyethylene terephthalate fiber, etc. can be used. In addition, a coated separator containing a ceramic component or a polymeric material can be used to ensure heat resistance or mechanical strength, and can be selectively used in a single layer or multilayer structure.
[0076] Examples of the electrolyte include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the manufacture of lithium secondary batteries, but are not limited to these.
[0077] Specifically, the electrolyte may include an organic solvent and a lithium salt.
[0078] The organic solvent can be used without any particular limitation as long as it serves as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the organic solvent can be an ester solvent such as methyl acetate, ethyl acetate, γ-butyrolactone, or ε-caprolactone; an ether solvent such as dibutyl ether or tetrahydrofuran; a ketone solvent such as cyclohexanone; an aromatic hydrocarbon solvent such as benzene or fluorobenzene; dimethylcarbonate (DMC), diethylcarbonate (DEC), ethylmethylcarbonate (EMC), ethylene carbonate (EC), or propylene carbonate (propylene carbonate). Carbonate-based solvents such as ethylene carbonate (PC); alcohol-based solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (R is a C2-C20 straight-chain, branched or cyclic hydrocarbon group that may contain a double bond aromatic ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes may be used. Among them, carbonate-based solvents are preferred, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate) having high ionic conductivity and high dielectric constant that can enhance the charge / discharge performance of the battery and a low-viscosity linear carbonate compound (e.g., ethyl methyl carbonate, dimethyl carbonate or diethyl carbonate) is more preferred. In this case, the cyclic carbonate and the linear carbonate are mixed in a volume ratio of about 1:1 to about 1:9, so that the electrolyte can exhibit excellent performance.
[0079] The lithium salt can be used without any particular limitation as long as it is a compound capable of providing lithium ions used in a lithium secondary battery. Specifically, the lithium salt may be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, LiB(C2O4)2, or a combination thereof. The concentration of the lithium salt is preferably within the range of 0.1 to 2.0M. When the concentration of the lithium salt is within the above range, the electrolyte has appropriate conductivity and viscosity, so that it can exhibit excellent electrolyte performance and lithium ions can move effectively.
[0080] In addition to the electrolyte components, the electrolyte may further include one or more additives such as haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethyl alcohol amine, cyclic ethers, ethylenediamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinoneimine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethyl alcohol, and aluminum trichloride, for the purpose of improving the life characteristics of the battery, suppressing the decrease in battery capacity, and improving the discharge capacity of the battery. Here, the additives may be included in an amount of 0.1% by weight to 5% by weight based on the total weight of the electrolyte.
[0081] <Lithium secondary battery> The lithium secondary battery according to the present invention comprises: A lithium secondary battery including a positive electrode including a positive electrode active material, a negative electrode including a silicon-based negative electrode active material, a separator, and an electrolyte, The positive electrode active material includes a lithium composite transition metal oxide having a cobalt coating layer and a boron coating layer formed thereon, The particle strength of the positive electrode active material is 80 MPa to 250 MPa, The positive electrode active material contains LiOH and Li2CO3 on the surface of the particles, The total content of the LiOH and Li2CO3 is 0.4% by weight to 1.1% by weight based on the total content of the positive electrode active material.
[0082] The lithium secondary battery can be manufactured by the above-mentioned method for manufacturing a lithium secondary battery, and the above-mentioned description of the method for manufacturing a lithium secondary battery can be cited for each configuration.
[0083] In the lithium secondary battery of the present invention, the cobalt coating layer and the boron coating layer included in the positive electrode active material can be confirmed using an electron probe micro analyzer (EPMA).
[0084] The particle strength of the positive electrode active material may be 80 MPa to 250 MPa, preferably 110 MPa to 230 MPa, and more preferably 170 MPa to 200 MPa. When the particle strength is within the above range, cracking of the positive electrode active material during rolling of the electrode is minimized, and side reactions with the electrolyte are reduced, thereby reducing the resistance increase rate of the battery. The lithium secondary battery of the present invention can achieve the above particle strength because the heat treatment process for forming the cobalt coating layer includes a high-temperature heat treatment. Specifically, the step of forming the cobalt coating layer may include two steps, a high-temperature (primary) step and a low-temperature (secondary) step, and recrystallization of the lattice structure occurs during the high-temperature heat treatment, thereby achieving the above particle strength.
[0085] The positive electrode active material contains LiOH and Li2CO3 as lithium by-products remaining on the surface of the particles, and the total content of LiOH and Li2CO3 is 0.4 wt% to 1.1 wt%, preferably 0.45 wt% to 1 wt%, more preferably 0.5 wt% to 0.8 wt% based on the total content of the positive electrode active material. When the total content of LiOH and Li2CO3 satisfies the above range, the capacity decrease due to the loss of soluble lithium is not large, and the efficiency can be reduced. The lithium secondary battery of the present invention is subjected to a heat treatment at 400°C to 500°C in the boron coating process of step (3), so that the content of such lithium by-products can be indicated. The content of LiOH and Li2CO3 can be confirmed by pH titration of the positive electrode active material.
[0086] The positive electrode active material is composed of secondary particles formed by agglomeration of primary particles, and the average particle size of the primary particles may be 0.4 μm to 1 μm, preferably 0.4 μm to 0.8 μm. When the average particle size of the primary particles satisfies the above range, the amount of fine powder generated due to cracking of particles during rolling of the electrode is reduced, and the specific surface area that may react with the electrolyte is reduced, which is preferable in that the performance of the battery can be improved. The lithium secondary battery of the present invention includes a high-temperature heat treatment process in the heat treatment process for forming the cobalt coating layer, so that the particle size of the primary particles can be achieved.
[0087] The positive electrode active material has an average particle diameter D 50 When the average particle size is within the above range, particle cracking can be minimized during electrode rolling.
[0088] The lithium secondary battery according to the present invention can be applied to portable devices such as mobile phones, notebook computers, and digital cameras, and to electric vehicles such as hybrid electric vehicles (HEVs).
[0089] According to another embodiment of the present invention, there is provided a battery module including the lithium secondary battery as a unit cell, and a battery pack including the same.
[0090] The battery module or the battery pack may be used as a power source for one or more medium- to large-sized devices including a power tool; an electric vehicle (EV), a hybrid electric vehicle, and a plug-in hybrid electric vehicle (PHEV); or a power storage system.
[0091] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, the embodiments of the present invention will be described in detail so that those skilled in the art can easily carry out the present invention.
[0092] [Examples and Comparative Examples: Production of Positive Electrode Active Material] Example 1. Ni 0.8 Co 0.1 Mn 0.1 The (OH)2 precursor and LiOH were charged into a Henschel mixer (700 L) in amounts such that the molar ratio of (Ni+Co+Mn):Li was 1:1.03, and the center was mixed at a speed of 400 rpm for 20 minutes. The mixed powder was placed in an alumina crucible measuring 330 mm x 330 mm in size and heat-treated at 750 °C for 12 hours in an oxygen (O2) atmosphere to obtain Li. 1.0 Ni 0.8 Co 0.1 Mn 0.1 A lithium composite transition metal oxide with O2 composition was produced.
[0093] The lithium composite transition metal oxide thus prepared was then dry-mixed with 1.5 wt% Co(OH)2 based on the total weight of the lithium composite transition metal oxide. The mixture was first heat-treated at 670°C for 4 hours in an air atmosphere, and then the temperature was lowered to 600°C and second heat-treated for 2 hours to prepare a lithium composite transition metal oxide having a cobalt coating layer formed thereon. This was dry-mixed with 0.2 wt% H3BO3 based on the total weight of the lithium composite transition metal oxide having a cobalt coating layer formed thereon, and then heat-treated at 450°C for 7 hours to prepare a positive electrode active material having a boron coating layer formed thereon.
[0094] Example 2. A positive electrode active material was prepared in the same manner as in Example 1, except that the content of Co(OH)2 was changed to 0.8 wt%.
[0095] Example 3. A positive electrode active material was prepared in the same manner as in Example 1, except that the content of Co(OH)2 was changed to 0.3 wt%.
[0096] Example 4. A positive active material was prepared in the same manner as in Example 1, except that a heat treatment was performed at 630° C. for 6 hours instead of the first and second heat treatments when forming the cobalt coating layer.
[0097] Comparative Example 1 A positive electrode active material was prepared in the same manner as in Example 1, except that the heat treatment temperature during the formation of the boron coating layer was lowered to 380°C.
[0098] Comparative Example 2 A positive electrode active material was prepared in the same manner as in Example 1, except that the heat treatment temperature during the formation of the boron coating was reduced to 300°C.
[0099] Comparative Example 3. A positive electrode active material was prepared in the same manner as in Example 1, except that the heat treatment temperature was increased to 530° C. when forming the boron coating.
[0100] Comparative Example 4. A positive electrode active material was prepared in the same manner as in Example 1, except that a heat treatment was performed at 500° C. for 6 hours instead of the first and second heat treatments when forming the cobalt coating layer.
[0101] [Experimental Example] Experimental Example 1: Measurement of primary particle size Photographs of the surfaces of the positive electrode active materials prepared in Examples 1 to 4 observed by a scanning electron microscope (SEM) are shown in Fig. 1. In addition, the particle sizes of the primary particles observed in the SEM photographs were measured, and the arithmetic average values thereof were calculated and shown in Table 1 below.
[0102] [Table 1]
[0103] From the results in Table 1, it can be seen that the primary particle diameter of the positive electrode active material prepared according to one embodiment of the present invention is 0.4 μm or more.
[0104] Experimental example 2: Evaluation of particle characteristics 3 g of the positive electrode active material powder prepared in Examples 1 to 3 and Comparative Examples 1 to 4 was collected, and the particle strength was measured by gradually increasing pressure applied using a Micro Compression Testing Machine (Shimadzu Corporation, MCT-W500) to measure the pressure at which the particles were destroyed.
[0105] Meanwhile, 3 g of the positive electrode active material powder produced in Examples 1 to 3 and Comparative Examples 1 to 4 was taken, placed in a cylindrical metal mold with a diameter of 2 cm, and pressed under a load of 9 tons, and then a volume cumulative particle size distribution (PSD) was obtained using an S-3500 manufactured by Microtrac Corp. The fine powder generation rate with a particle size of 1 μm or less was converted to weight % with respect to the total weight of the positive electrode active material, and this was shown as the fine powder generation rate in Table 2 below.
[0106] In addition, PSD analysis results for the positive electrode active material powders of the Examples and Comparative Examples before pressing were obtained in the same manner as described above except for the pressing process. The strength retention rates calculated by substituting the PSD analysis results before and after pressing into the following formula (a) are shown in Table 2 below.
[0107] Formula (a): Strength retention rate (%) = volume ratio of most frequent particle size after pressing / volume ratio of most frequent particle size before pressing × 100
[0108] [Table 2]
[0109] From the results in Table 2, it can be seen that in Examples 1 to 3, in which boron coating was performed at a temperature of 400°C to 500°C and the first and second heat treatment processes were performed at 550°C to 700°C when forming the cobalt coating layer, positive electrode active materials with excellent particle strength were produced.
[0110] On the other hand, it can be seen that the positive electrode active materials of Comparative Examples 1 to 3, which were boron-coated at temperatures below 400° C. or above 500° C., had poor particle strength compared to the positive electrode active materials of Examples 1 to 3.
[0111] Also, in the case of Comparative Example 4, when the cobalt coating temperature was lowered to 500°C, it was confirmed that the particle strength was significantly inferior to that of Example 1, which was performed under the same conditions except for the cobalt coating temperature. Although the fine powder generation rate was somewhat lower than that of Example 3, considering that a significantly larger amount of cobalt raw material was used in Comparative Example 4 than in Example 3, it can be seen that adjusting the cobalt coating temperature to within the range of 550-700°C is an important factor in improving particle strength.
[0112] Experimental Example 3: Measurement of residual lithium amount 5 g of each of the positive electrode active material powders prepared in Examples 1 to 4 and Comparative Examples 1 to 4 was dispersed in 100 mL of water, and then titrated with 0.1 M HCl to measure the change in pH value, thereby obtaining a pH titration curve. Using the pH titration curve, the amount of LiOH remaining and the amount of Li2CO3 remaining in each positive electrode active material were calculated, and the sum of these values was evaluated as the amount of residual lithium. The measurement results are shown in Table 3 below.
[0113] [Table 3]
[0114] From the results in Table 3, it can be seen that the positive electrode active materials of Examples 1 to 4 have a residual lithium amount of 0.4 wt % or more and 1.1 wt % or less so that the capacity reduction due to lithium loss is not significant and the initial efficiency can be reduced.
[0115] On the other hand, it can be seen that the amount of residual lithium is less than 0.4 wt % in the positive electrode active materials of Comparative Examples 1 to 3 in which boron coating was performed at a temperature less than 400°C or more than 500°C, and in the positive electrode active material of Comparative Example 4 in which cobalt coating was performed at a temperature less than 550°C.
[0116] Experimental example 4: Confirmation of capacitance and initial resistance The positive electrode active materials prepared in Examples 1 to 4 and Comparative Examples 1 to 4, conductive material (carbon black), and binder (polyvinylidene fluoride, PVdF) were mixed in a weight ratio of 97.5:1.0:1.5 in N-methyl-2-pyrrolidone (NMP) solvent to prepare positive electrode slurry (solid content: 50 wt%). The positive electrode slurry was applied to one side of an aluminum current collector, dried at 130°C, and rolled to prepare a positive electrode.
[0117] An electrode assembly was prepared by interposing a 15μm-thick polyethylene separator between lithium metal negative electrodes, and then the electrode assembly was placed inside a battery case, and an electrolyte was injected into the case to prepare a lithium secondary battery. A half cell was prepared by injecting an electrolyte solution prepared by dissolving 1M LiPF6 in a mixed organic solvent of ethylene carbonate (EC): ethyl methyl carbonate (EMC) mixed at a volume ratio of 1:2, and the capacity and resistance of the half cell were measured during 0.1C charge and discharge.
[0118] Specifically, the half cell was charged at a constant current of 0.1 C with a cutoff of 0.05 C at 25° C. up to 4.25 V. Then, the half cell was discharged at a constant current of 0.1 C up to 3.0 V to measure the initial charge / discharge capacity, and the initial resistance was measured by dividing the voltage drop during the initial 10 seconds of discharge by the current value, and the results are shown in Table 4 below.
[0119] [Table 4]
[0120] Referring to Table 4, it can be seen that the batteries using the positive electrode active materials of Examples 1 to 4, which were cobalt-coated at 550° C. to 700° C. and then boron-coated at 400° C. to 500° C., had lower initial resistance and initial charge / discharge efficiency than the batteries using the positive electrode active materials of Comparative Examples 1 and 2, which were boron-coated at a temperature below 400° C., the positive electrode active material of Comparative Example 3, which was boron-coated at a temperature above 500° C., and the positive electrode active material of Comparative Example 4, which was cobalt-coated at a temperature below 550° C. This means that it is advantageous in that it can compensate for irreversible capacity in silicon-based negative electrode active materials, which have low charge / discharge efficiency and a large lithium ion loss rate due to irreversible reactions.
[0121] Experimental example 5: Evaluation of high temperature life characteristics The high-temperature life characteristics of a lithium secondary battery including the positive electrode prepared in Experimental Example 4 and the following silicon-based negative electrode were measured.
[0122] Specifically, the negative electrode active material (composed of 3wt% SiO and 97wt% graphite), binder (SBR-CMC) and conductive material (carbon black) were added to the solvent water in a weight ratio of 95:3.5:1.5 to prepare a negative electrode slurry (solid content: 60wt%). The negative electrode slurry was applied to a copper (Cu) thin film as a negative electrode current collector with a thickness of 6μm, dried and then roll pressed to prepare a negative electrode.
[0123] An electrode assembly was prepared by interposing a 15 μm thick polyethylene separator between the positive electrode and the negative electrode to which the positive electrode active material of each of Examples 1 to 4 and Comparative Examples 1 to 4 was applied, and then the electrode assembly was placed inside a battery case, and an electrolyte was injected into the case to prepare a lithium secondary battery. Here, the electrolyte was prepared by injecting an electrolyte solution prepared by dissolving 1M LiPF6 in a mixed organic solvent in which ethylene carbonate (EC):ethyl methyl carbonate (EMC) was mixed in a volume ratio of 1:2, to prepare a lithium secondary battery.
[0124] Each of the lithium secondary batteries was charged at 0.5 C in CCCV mode at 45° C. up to 4.2 V, and discharged at a constant current of 0.5 C down to 3.0 V, and then subjected to 200 charge-discharge experiments to measure the capacity retention rate and the resistance increase rate. The results are shown in Table 5.
[0125] [Table 5]
[0126] From the results of Table 5, it can be confirmed that the positive electrodes containing the positive electrode active materials of Examples 1 to 4, in combination with the negative electrode containing the Si-based active material, are effective in increasing the capacity retention rate of the battery and decreasing the resistance increase rate in a high temperature environment, compared to the positive electrodes containing the positive electrode active materials of Comparative Examples 1 to 4.
[0127] In addition, when comparing the results between the examples, it can be seen that even though the boron coating was performed at the same temperature, the positive electrode active material of Example 1 among Examples 1 to 3, in which the cobalt coating contents were 1.5 wt %, 0.8 wt %, and 0.3 wt %, respectively, was most advantageous in improving high temperature performance.
[0128] In addition, it can be confirmed that the positive electrode active material of Example 1, in which the heat treatment was performed in two steps by lowering the heat treatment temperature in the middle of the cobalt coating process, is advantageous in improving high-temperature performance compared to the positive electrode active material of Example 4, in which the heat treatment was performed in one step.
[0129] To summarize the above experimental results, the lithium secondary battery manufactured according to an embodiment of the present invention has excellent output characteristics and high-temperature life.
Claims
1. (1) mixing a transition metal precursor and a lithium source material, and then calcining the mixture to produce a lithium transition metal composite oxide; (2) mixing the lithium composite transition metal oxide with a cobalt-containing raw material and heat-treating the mixture at 550° C. to 700° C. to form a cobalt coating layer on the lithium composite transition metal oxide; (3) mixing the lithium composite transition metal oxide on which the cobalt coating layer is formed with a boron-containing raw material and heat-treating the mixture at 400° C. to 500° C. to produce a positive electrode active material including a boron coating layer; (4) coating the positive electrode active material onto a positive electrode current collector to produce a positive electrode; (5) assembling the positive electrode, a negative electrode including a silicon-based negative electrode active material, and a separator, and injecting an electrolyte; A method for producing a lithium secondary battery, comprising:
2. 2. The method for producing a lithium secondary battery according to claim 1, wherein the difference between the firing temperature in step (1) and the heat treatment temperature in step (2) is less than 100°C.
3. 2. The method for producing a lithium secondary battery according to claim 1, wherein the heat treatment in step (2) includes a first heat treatment and a second heat treatment performed at a temperature lower than that of the first heat treatment.
4. 2. The method for producing a lithium secondary battery according to claim 1, wherein in the step (2), the cobalt-containing raw material is mixed in an amount of 0.5% by weight to 3% by weight based on the total content of the lithium composite transition metal oxide.
5. 2. The method of claim 1, wherein in the step (3), the boron-containing raw material is mixed in an amount of 0.05% by weight to 3% by weight based on the total content of the lithium composite transition metal oxide on which the cobalt coating layer is formed.
6. The method for manufacturing a lithium secondary battery according to claim 1 , wherein the lithium composite transition metal oxide is represented by the following Chemical Formula 1: [Chemical formula 1] Li 1+x (N a Co b Mn c M d )O 2 In the above Chemical Formula 1, M is at least one selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; x, a, b, c, and d are -0.2≦x≦0.2, 0.50≦a<1, 0<b≦0.40, 0<c≦0.40, 0≦d≦0.1, and a+b+c+d=1, respectively.
7. The silicon-based negative electrode active material is Si, SiO x 2. The method for producing a lithium secondary battery according to claim 1, wherein the material is at least one selected from the group consisting of (0<x<2) and a Si-containing alloy.
8. A lithium secondary battery comprising a positive electrode including a positive electrode active material, a negative electrode including a silicon-based negative electrode active material, a separator, and an electrolyte, The positive electrode active material includes a lithium composite transition metal oxide having a cobalt coating layer and a boron coating layer formed thereon, The particle strength of the positive electrode active material is 80 MPa to 250 MPa; The positive electrode active material is a material having a particle surface on which LiOH and Li 2 CO 3 Including, The LiOH and Li 2 CO 3 The total content of the positive electrode active material is 0.4% by weight to 1.1% by weight based on the total content of the positive electrode active material.
9. 9. The lithium secondary battery according to claim 8, wherein the positive electrode active material is composed of secondary particles formed by agglomeration of primary particles, and the average particle size of the primary particles is 0.4 μm to 1 μm.
10. The positive electrode active material has an average particle diameter D 50 The lithium secondary battery according to claim 8, wherein the thickness is 8 μm to 20 μm.
11. The lithium secondary battery of claim 8 , wherein the lithium composite transition metal oxide is represented by the following Chemical Formula 1: [Chemical formula 1] Li 1+x (N a Co b Mn c M d )O 2 In the above Chemical Formula 1, M is at least one selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; x, a, b, c, and d are -0.2≦x≦0.2, 0.50≦a<1, 0<b≦0.40, 0<c≦0.40, 0≦d≦0.1, and a+b+c+d=1, respectively.
12. The silicon-based negative electrode active material is Si, SiO x 9. The lithium secondary battery according to claim 8, wherein the lithium secondary battery is at least one selected from the group consisting of (0<x<2) and a Si-containing alloy.
Citation Information
Patent Citations
Production of oxide powder
JP2000044206A
Active material for nonaqueous electrolyte secondary battery, positive electrode plate for nonaqueous electrolyte secondary battery, nonaqueous electrolyte secondary battery and battery pack
JP2012094405A
Lithium ion secondary battery cathode and manufacturing method thereof, and lithium ion secondary battery
JP2014127235A
Positive electrode active material, positive electrode and battery
JP2016033902A
Positive electrode active material for nonaqueous electrolyte secondary battery, method for manufacturing the same, positive electrode for nonaqueous electrolyte secondary battery, and nonaqueous electrolyte secondary battery
JP2018073481A