Hydrofluorocarbon compounds containing oxygen and iodine for etching semiconductor structures - Patents.com

The use of an oxygen and iodine-containing etching compound addresses the challenge of achieving high aspect ratios and selectivity in silicon-containing film etching, ensuring minimal distortion and improved etch resistance in semiconductor manufacturing.

JP2024545182AActive Publication Date: 2024-12-05LAIR LIQUIDE SA POUR LETUDE & LEXPLOITATION DES PROCEDES GEORGES CLAUDE
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024534638
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-12-17
Filing Date
2022-12-13
Publication Date
2024-12-05
Estimated Expiration
2042-12-13

AI Technical Summary

Technical Problem

Conventional etching methods for silicon-containing films in semiconductor manufacturing face challenges in achieving high aspect ratios and selectivity, leading to distorted or rough etched structures due to insufficient etch-resistant polymer deposition and oxygen radical etching of amorphous carbon masks.

Method used

A method involving the use of an etching compound containing oxygen and iodine, activated by plasma, which selectively etches silicon-containing films while doping the patterned mask layer with iodine ions to reinforce it, minimizing damage and maintaining a vertical profile.

Benefits of technology

The method achieves high selectivity and high aspect ratios with minimal distortion and roughness, enhancing etch resistance and maintaining pattern integrity in semiconductor structures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024545182000001_ABST
    Figure 2024545182000001_ABST
Patent Text Reader

Abstract

The method includes reacting a silicon-containing film having a silicon-containing layer deposited on the substrate with a patterned mask layer deposited on the silicon-containing layer in a chamber containing the substrate, the silicon-containing film having a silicon-containing layer deposited on the patterned mask layer, with a compound of formula C n H x F y I z O e wherein 0≦n≦10, 0≦x≦21, 0≦y≦21, 1≦z≦4, and 1≦e≦2; activating a plasma to generate an activated etching compound containing oxygen and iodine; and allowing an etching reaction to proceed between the activated etching compound containing oxygen and iodine and the silicon-containing film to selectively etch the silicon-containing film from the patterned mask layer, thereby forming a patterned structure.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of priority under 35 U.S.C. §119(a) and (b) to U.S. patent application Ser. No. 17 / 555,094, filed December 17, 2021, the entire contents of which are incorporated herein by reference.

[0002] The present invention relates to a method for etching silicon-containing films to form patterned structures, in particular a method for etching silicon-containing films comprising the steps of: n H x F y I z O e wherein 0≦n≦10, 0≦x≦21, 0≦y≦21, 1≦z≦4, and 1≦e≦2, is used to etch a silicon-containing film on a patterned mask layer to form a patterned structure, such that iodine from iodine ions generated from the activated oxygen- and iodine-containing etching compound is doped into the patterned mask layer, reinforcing, strengthening, or minimizing damage to the patterned mask layer. [Background technology]

[0003] In the semiconductor industry, etching of stacks of multiple SiO / SiN or SiO / polysilicon (p-Si) layers is important for 3D NAND. See, for example, U.S. Patent Application Publication No. 2011 / 0180941 to Samsung Electronics Co., Ltd. An etchant with high selectivity between the mask and the layer to be etched is essential. Furthermore, the etched structures should have straight vertical profiles without distortion and low line etch roughness (LER).

[0004] Standard hydrofluorocarbons used for etching silicon oxide are cC4F8, C4F6 in combination with an oxidizer (e.g., O2) and a noble gas (e.g., Ar, Kr, Xe). For etching silicon nitride, the above gases are usually mixed with hydrogen-containing fluorocarbons such as CHF2, CHF3, and CH3F.

[0005] However, conventional etch chemistries may be unable to provide features such as holes or trenches with aspect ratios higher than 20:1 required for new applications (e.g., 3D NAND) at least due to insufficient etch-resistant polymer deposition on the sidewalls during the plasma etching process. x F y -polymers, where x ranges from 0.01 to 1 and y ranges from 0.01 to 4, may be susceptible to etching. As a result, the etched patterns may not be vertical and the etched structures may exhibit distortion, dimensional changes, pattern collapse and / or increased roughness.

[0006] The distortion may be due to sidewall etching of the mask layer, which may often be an amorphous carbon (aC) material, which may cause an increase in the opening of the mask and may be etched by oxygen radicals in the plasma, resulting in a distorted or angled / curved etched structure.

[0007] Carbonyl-containing compounds are used as etching gases for etch-back, and / or decomposition of carbonyl-containing compounds is disclosed. Japanese Patent Publication No. 3291885B2 by Y. Toshiharu discloses a dry etching method for etching back a blanket CVD tungsten layer using carbonyl fluoride compound gases such as COF2, COFCl, COFBr, COFI, and (COF)2 to fill a contact hole with good flatness. Furthermore, F-based gases such as SF6, NF3, CF4, ClF3, XeF2, and F2 are commonly used as F sources. U.S. Patent Application Publication No. 2006 / 0140836A1 by O. Masakazuifco discloses a process for decomposing fluorine compounds having iodine in the molecule to render them harmless. Fluorine compounds include compounds such as C2F5IO and C2F4I2O. WO 2009 / 019219 to Uenveren et al. discloses a method for etching SiO2 for self-aligned contacts using hydrofluorocarbons. Although C3F5IO is mentioned, the oxygen is a terminal oxygen bonded to carbon, and no supporting etch examples are disclosed.

[0008] To maximize selectivity to the hard mask and achieve the high aspect ratios (i.e., up to 200:1) required for current applications (e.g., contact etch or 3D NAND), it is important to minimize distortion, CD variation (top vs. bottom), twist, and incomplete etching. Furthermore, the etch is not limited to selectivity to the photoresist mask. aC, SiN, p-Si, SiC, or other forms of Si a C b O c H d N e It is equally important to obtain high selectivity among other materials, such as materials where a>0; b, c, d, and e≧0. Summary of the Invention [Problem to be solved by the invention]

[0009] Therefore, there is a need for suitable etching gas compositions for use in plasma etching applications that maintain selectivity and high aspect ratios over a wide range of process conditions. [Means for solving the problem]

[0010] A method of forming a patterned structure is disclosed, the method comprising: a) introducing into a reaction chamber containing a substrate having a silicon-containing film deposited thereon and a patterned mask layer deposited on the silicon-containing layer, n H x F y I z O e introducing vapor of an etching compound containing oxygen and iodine having the formula: where 0≦n≦10, 0≦x≦21, 0≦y≦21, 1≦z≦4, and 1≦e≦2; b) activating the plasma to produce an activated etching compound containing oxygen and iodine; and c) allowing an etching reaction to proceed between the activated etching compound containing oxygen and iodine and the silicon-containing film to selectively etch the silicon-containing film from the patterned mask layer, thereby forming a patterned structure; Includes.

[0011] The disclosed methods may include one or more of the following aspects: step c) comprises modifying or doping the patterned mask layer with iodine from iodine ions generated from an activated etching compound containing oxygen and iodine; · step c) comprises modifying the patterned mask layer; step c) includes doping the patterned mask layer with iodine from iodine ions generated from an activated etching compound containing oxygen and iodine; step c) comprises reinforcing or doping the patterned mask layer with iodine from iodine ions generated from an activated etching compound containing oxygen and iodine; step c) comprises strengthening or doping the patterned mask layer with iodine from iodine ions generated from an activated etching compound containing oxygen and iodine; step c) includes minimizing damage to the patterned mask layer or doping the patterned mask layer with iodine from iodine ions generated from an activated etching compound containing oxygen and iodine; step c) comprises increasing the etch resistance of the patterned mask layer or doping the patterned mask layer with iodine from iodine ions generated from an activated etching compound containing oxygen and iodine; · step c) includes increasing etch selectivity to an underlying layer of the substrate while forming a patterned structure on the substrate; · further comprising the step of introducing an inert gas into the reaction chamber; The inert gas is selected from the group consisting of He, Ar, Xe, Kr, Ne and N2; · The inert gas is Ar; mixing an etching compound containing oxygen and iodine with an inert gas prior to introduction into the chamber to form a mixture; An etching compound containing oxygen and iodine is introduced separately from the inert gas; · Continuously introduce an inert gas and pulse an etching compound containing oxygen and iodine; The inert gas comprises from about 0.01% v / v to about 99.9% v / v of the total volume of the inert gas and the vapor of the oxygen- and iodine-containing etching compound; The inert gas comprises about 90% v / v to about 99% v / v of the total volume of the inert gas and the vapor of the oxygen- and iodine-containing etching compound; · optionally further comprising the step of introducing an oxidant into the reaction chamber; the oxidant is selected from O2, O3, CO, CO2, NO, N2O, NO2, H2O, H2O2, COS, SO2 and combinations thereof; · The oxidant is O2; · The oxidant is O3; mixing an etching compound containing oxygen and iodine with an oxygen-containing gas prior to introduction into the chamber to form a mixture; An etching compound containing oxygen and iodine is introduced separately from the oxygen-containing gas; · successively introducing an oxygen-containing gas and an etching compound containing oxygen and iodine; the oxygen-containing gas comprises from about 0.01% v / v to about 99.9% v / v of the combined volume of the oxygen- and iodine-containing etching compound and the oxygen-containing gas; the oxygen-containing gas comprises from about 0.01% v / v to about 10% v / v of the combined volume of the oxygen- and iodine-containing etching compound and the oxygen-containing gas; The etching compound containing oxygen and iodine is a hydrofluorocarbon compound; The oxygen and iodine containing etching compound is an oxygen and iodine containing hydrofluorocarbon; The etching compound containing oxygen and iodine is an organic fluorine compound; The etching compound containing oxygen and iodine is a fluorine-containing hydrocarbon compound; The etching compound containing oxygen and iodine is a fluorocarbon compound; The etching compound contains oxygen and iodine and does not contain hydrogen; The etching compound containing oxygen and iodine contains hydrogen; · the oxygen and iodine containing etching compound contains fluorine; · The etching compound containing oxygen and iodine does not contain fluorine; The etching compounds containing oxygen and iodine are C3F7IO and its isomers; The etching compound containing oxygen and iodine is C3F7IO, 2-iodo-1-(trifluoromethoxy)tetrafluoroethane (CAS number: 1561-52-0); The etching compound containing oxygen and iodine is C3F7IO, 1,1,1,2-tetrafluoro-2-iodo-2-(trifluoromethoxy)ethane (CAS number: 139604-89-0); The etching compound containing oxygen and iodine is C3F7IO, 1,2,2,2-tetrafluoro-1-trifluoromethoxy-1-iodoethane (CAS number: 69066-98-4); The etching compound containing oxygen and iodine is C3F7IO, 1,1,1,2,2,3,3,3-heptafluoro-3-iodocyl-propane (CAS number: 180613-10-9); Etching compounds containing oxygen and iodine are C3F6I2O, C3F5I3O, C3F4I4O and their isomers; Etching compounds containing oxygen and iodine include C3F7IO, C3F6I2O, C3F5I3O, C3F4I4O, C4F9IO, C4F8I2O, C4F7I3O, C4F6I4O, C5F 11 IO, C5F 10 I2O, C5F9I3O, C5F8I4O, C6F 13 IO, C6F 12 I2O, C6F 11 I3O, C6F 10 I4O, C7F 15 IO, C7F 14 I2O, C7F 13 I3O, C7F 12 I4O, C8F 17 IO, C8F 16 I2O, C8F 15 I3O, C8F 14 I4O, C9F 19 IO, C9F 18 I2O, C9F 17 I3O, C8F 16 I4O, C 10 F 21 I.O., C. 10 F 20 I2O, C10 F 19 I3O, C 10 F 18 I4O and its isomers; Etching compounds containing oxygen and iodine include C4F9IO, C4F9IO, and C5F 11 IO, C5F 11 IO, C6F 13 IO, C7F 15 IO, C8F 17 IO, C9F 19 I.O., C. 10 F 21 IO, and their isomers; Etching compounds containing oxygen and iodine include C3HF6IO, C3HF5I2O, C3HF4I3O, C3HF3I4O, C4HF8IO, C4HF7I2O, C4HF6I3O, C4HF5I4O, C5HF 10 IO, C5HF9I2O, C5HF8I3O, C5HF7I4O, C6HF 12 IO, C6HF 11 I2O, C6HF9I3O, C6HF8I4O, C7HF 14 IO, C7HF 13 I2O, C7HF 12 I3O, C7HF 11 I4O, C8HF 16 IO, C8HF 15 I2O, C8HF 14 I3O, C8HF 10 I4O, C9HF 18 IO, C9HF 17 I2O, C9HF 16 I3O, C9HF 15 I4O, C 10 HF 20 I.O., C. 10 HF 19 I2O, C 10 HF 18 I3O, C 10 HF 17 I4O and its isomers; · An oxygen- and iodine-containing etching compound activated by the plasma reacts with the silicon-containing film to form volatile by-products; · Volatile by-products are removed from the reaction chamber; the silicon-containing film comprises oxygen, nitrogen, carbon, hydrogen, carbon or combinations thereof; The silicon-containing film optionally includes dopants such as B, C, P, As, Ga, In, Sn, Sb, Bi and / or Ge, or combinations thereof; Silicon-containing films include silicon oxide (SiO), silicon nitride (SiN), crystalline Si, polysilicon (p-Si), polycrystalline silicon, amorphous silicon, low dielectric constant SiCOH, SiOCN, SiC, SiON, Si a O b H c C d N e (wherein a>0; b, c, d, and e≧0), comprising alternating layers of SiO and SiN (ONON), or alternating layers of SiO and p-Si (OPOP); The silicon-containing film is SiO x N y H z C k wherein x ranges from 0 to 2, y ranges from 0 to 4, z ranges from 0 to about 1, and k ranges from 0 to 1; The silicon-containing film comprises a SiO layer; The silicon-containing film is a SiN layer; The silicon-containing film comprises alternating layers of SiO and SiN(ONON); The silicon-containing film comprises alternating layers of SiO and p-Si (OPOP); The patterned mask layer is an amorphous carbon layer, a doped amorphous carbon layer, a photoresist layer, an antireflective layer, an organic planarization layer, or a combination thereof; · the patterned mask layer is a layer of CVD, PECVD, ALD, PEALD or spin-on-deposited (SOD) amorphous carbon or doped amorphous carbon, silicon-containing spin-on mask, or carbon-containing spin-on mask; The patterned mask layer is an amorphous carbon (aC) layer; The patterned mask layer is a doped carbon layer; The doped amorphous carbon layer is a boron doped aC layer; The doped amorphous carbon layer is a tungsten doped aC layer; · Alternating layers are selectively etched from a patterned mask layer; · Alternating layers are selectively etched from the aC layer; · Alternating layers are selectively etched from the doped carbon layer; ·Alternating layers of silicon oxide and silicon nitride are selectively etched from the aC layer; · Alternating layers of silicon oxide and silicon nitride are selectively etched from the doped carbon layer; ·Alternating layers of silicon oxide and polysilicon are selectively etched from the aC layer; ·Alternating layers of silicon oxide and polysilicon are selectively etched from the doped carbon layer; · The silicon oxide layer is selectively etched from the patterned mask layer; · The silicon oxide layer is selectively etched from the aC layer; · The silicon oxide layer is selectively etched from the doped carbon layer; · The silicon nitride layer is selectively etched from the patterned mask layer; · The silicon nitride layer is selectively etched from the aC layer; · The silicon nitride layer is selectively etched from the doped carbon layer; · The polysilicon layer is selectively etched from the patterned mask layer; · The polysilicon layer is selectively etched from the aC layer; · The polysilicon layer is selectively etched from the doped carbon layer; · The silicon-containing film is selectively etched from an aC layer, a doped aC layer, a photoresist layer, an antireflective layer, or an organic planarization layer; · The silicon oxide layer is selectively etched from the aC layer, the doped aC layer, the photoresist layer, the antireflective layer or the organic planarization layer; Etching compounds containing oxygen and iodine etch both silicon oxide and silicon nitride layers with high etching rates; An etching chemistry containing oxygen and iodine for plasma etching alternating layers of SiO and SiN (ONON) has a selectivity of about 1:2 to about 2:1 for SiO layers to SiN layers; An oxygen and iodine containing etch chemistry for plasma etching alternating SiO and SiN (ONON) layers has a selectivity of about 1:1 for SiO layers versus SiN layers; An oxygen and iodine containing etch chemistry for plasma etching alternating layers of SiO and p-Si (OPOP) has a selectivity of about 1:2 to about 2:1 for SiO layers to p-Si layers; An oxygen and iodine containing etch chemistry for plasma etching alternating layers of SiO and p-Si (OPOP) has a selectivity of about 1:1 for SiO layers versus p-Si layers; The selectivity of oxygen and iodine-containing etching compounds for plasma etching of SiO2 on patterned mask layers is approximately 70% higher than that of the benchmark gas C4F6 for etching SiO2 on patterned mask layers at a similar etch rate; · the patterned mask layer is a carbon-containing layer, an amorphous carbon layer, a doped amorphous carbon layer, a photoresist layer, an antireflective layer, an organic planarization layer, or a combination thereof; An activated etching compound containing oxygen and iodine selectively etches the silicon-containing film from a landing layer located at the bottom of the silicon-containing film being etched; The landing layer is a buried landing layer located at the bottom of the structure to be etched; The landing layer is an etch stop layer; The landing layer is a silicone layer; The landing layer is a metal layer; The landing layer is the tungsten metal world line of the 3D NAND structure and / or another metal such as W, Cu, Al, Ru, Pt, Ti, Ta, Ni, Co, Mo, Mn, Nb, Cr, Rh, Pd, Ir, V, Au, Ag or combinations thereof; the landing layer is a metal layer selected from W, Cu, Al, Ru, Pt, Ti, Ta, Ni, Co, Mo, Mn, Nb, Cr, Rh, Pd, Ir, V, Au, Ag, or combinations thereof; the landing layer is a metal oxide layer or a metal nitride layer; the landing layer is a metal oxide layer selected from AlO, WO, HfO, TiO, TaO, InO, WO, CrO, RuO, CoO, MoO, ZrO, SnO, or combinations thereof; the landing layer is a metal nitride layer selected from TiN, TaN, HfN, AlN, WN, MoN, NiN, NbN, CrN, RuN, CoN, ZrN, SrN or combinations thereof; The substrate is a Si wafer; The substrate is a crystalline silicon layer; · Forming patterned structures; The patterned structure is a 3D NAND aperture; The patterned structures are contact holes; The patterned structures are 3D NAND contact holes; · The patterned structures are DRAM contacts; · The patterned structures are channel holes; The patterned structure is a 3D NAND channel hole; The patterned structure is a 3D NAND slit contact; · The aperture is a stepped contact; · The aperture is a self-aligning contact; · The aperture is a self-aligned via; · The aperture is a supervia; · further comprising introducing additional etching gas into the reaction chamber; Additional etching gases include cC4F8, C4F8, cC5F8, C5F8, C4F6, CF4, CH3F, CF3H, CH2F2, C3HF7, C3F6, C3H2F6, C3H2F4, C3H3F5, C4HF7, C5HF9, C3F6, C3F8, CF3I, C2F3I, C2F5I, C3F7I, 1-iodoheptafluoropropane (1-C3F7I), 2-iodoheptafluoropropane (2-C3F7I), C4F9I, C3HF7, COS, FNO, FC≡N, CS2, SO2, SF6, trans-1,1,1,4,4,4-hexafluoro-2 -butene (trans-C4H2F6), cis-1,1,1,4,4,4-hexafluoro-2-butene (cis-C4H2F6), hexafluoroisobutene (C4H2F6), trans-1,1,2,2,3,4-hexafluorocyclobutane (trans-C4H2F6), 1,1,2,2,3-pentafluorocyclobutane (C4H3F5), 1,1,2,2-tetrafluorocyclobutane (C4H4F4), and cis-1,1,2,2,3,4-hexafluorocyclobutane (cis-C4H2F6), or a combination thereof; Introducing an etching compound containing oxygen and iodine separately from the additional etching gas; adding about 0.01% v / v to about 99.99% v / v of additional etching gas to the etching compound containing oxygen and iodine; the patterned structure formed in the silicon-containing film has an aspect ratio of about 1:1 to about 200:1; · The iodine doping concentration increases from 0.1% to 99.9% throughout the deposited film; ·Applying RF power to activate the plasma; Activating the plasma with RF power ranging from about 25 W to about 100,000 W; Etching pressure is in the range of about 1mTorr to 10Torr; Etching pressure is 30mTorr; introducing an iodine-containing etching compound at a flow rate ranging from about 0.1 sccm to about 1 slm; The substrate is maintained at a temperature in the range of about -196°C to about 500°C.

[0012] A method of forming a patterned structure is disclosed, the method comprising: a) introducing vapor of C3F7IO into a reaction chamber containing a substrate having a silicon-containing film deposited thereon and a patterned mask layer deposited on the silicon-containing layer; b) activating the plasma to produce activated C3F7IO; and c) allowing an etching reaction to proceed between the activated C3F7IO and the silicon-containing film to selectively etch the silicon-containing film from the patterned mask layer, thereby forming a patterned structure; The disclosed methods may include one or more of the following aspects: step c) comprises modifying the patterned mask layer by doping it with iodine from iodine ions generated from an activated etching compound containing oxygen and iodine; · step c) comprises modifying the patterned mask layer; step c) includes doping the patterned mask layer with iodine from iodine ions generated from an activated etching compound containing oxygen and iodine; · The iodine doping concentration increases from 0.1% to 99.9% throughout the deposited film; The selectivity of an oxygen and iodine-containing etch compound for plasma etching of SiO2 on a patterned mask layer is approximately 70% higher than that of the benchmark gas C4F6 for etching SiO2 on a patterned mask layer at a similar etch rate.

[0013] A method for modifying a surface of a substrate is disclosed, the method comprising: A reaction chamber containing a substrate having a silicon-containing film deposited thereon and a patterned mask layer deposited on the silicon-containing layer is provided with a compound of formula C. n Hx F y I z O e introducing vapor of an etching compound containing oxygen and iodine having the formula: where 4≦n≦10, 0≦x≦21, 0≦y≦21, 1≦z≦4, and 1≦e≦2; Etching the silicon-containing film through the patterned mask layer using an activated etching compound containing oxygen and iodine formed by activating a plasma to form a patterned structure; Includes; Iodine from iodine ions generated from an activated etching compound containing oxygen and iodine is doped into the patterned hard mask layer during formation of the patterned structures on the substrate, thereby strengthening the patterned mask layer and minimizing damage to the patterned mask. The disclosed method may include one or more of the following aspects: Etching compounds containing oxygen and iodine are C3F7IO and its isomers; · The iodine doping concentration increases from 0.1% to 99.9% throughout the deposited film; The selectivity of an oxygen and iodine-containing etch compound for plasma etching of SiO2 on a patterned mask layer is approximately 70% higher than that of the benchmark gas C4F6 for etching SiO2 on a patterned mask layer at a similar etch rate.

[0014] Designation and nomenclature In the following detailed description and claims, a number of abbreviations, symbols and terms that are commonly known in the art are utilized. These include:

[0015] As used herein, the indefinite articles "a" or "an" mean one or more.

[0016] As used herein, in the text or claims, "about" or "approximately" or "approximately" means ±10% of the stated value.

[0017] As used herein, "room temperature" in the text and claims means about 20°C to about 25°C.

[0018] The term "ambient temperature" refers to an environmental temperature of about 20°C to about 25°C.

[0019] The term "substrate" refers to one or more materials on which a process is performed. A substrate may refer to a wafer having one or more materials on which a process is performed. The substrate may be any suitable wafer used in the manufacture of semiconductor, photovoltaic, flat panel, or liquid crystal display thin film transistor (LCD-TFT) devices. The substrate may also have one or more layers of different materials already deposited thereon from a previous manufacturing step. For example, the wafer may include a silicon layer (e.g., crystalline, amorphous, porous, etc.), a silicon-containing layer (e.g., SiO2, SiN, SiON, SiC, SiCN, SiOCN, SiCOH, etc.), a metal-containing layer (e.g., copper, cobalt, ruthenium, tungsten, manganese, platinum, palladium, nickel, ruthenium, gold, etc.), or a combination thereof. Furthermore, the substrate may be flat or patterned. The substrate may be a photoresist film patterned with an organic material. The substrate may include a layer of oxide (e.g., ZrO2-based materials, HfO2-based materials, TiO2-based materials, rare earth oxide-based materials, ternary oxide-based materials, etc.) used as a dielectric material in MEMS, 3D NAND, MIM, Dynamic Random Access Memory (DRAM), or FeRam device applications, or a nitride-based film (e.g., TaN, TiN, NbN) used as an electrode. One skilled in the art will recognize that the term "film" or "layer" as used herein refers to a thickness of any material disposed or extending over a surface, which may be a trench or line. Throughout this specification and claims, the wafer and associated layers thereon are referred to as the substrate.

[0020] The term "wafer" or "patterned wafer" refers to a wafer having a stack of silicon-containing films on a substrate and a patterned hard mask layer on the stack of silicon-containing films formed for pattern etching.

[0021] The terms "pattern etch" or "patterned etch" refer to etching a non-planar structure, such as a patterned mask layer on a silicon-containing film stack.

[0022] As used herein, the term "etch" or "etching" refers to the use of plasma to remove material by ion bombardment, remote plasma, or chemical vapor phase reaction between an etching gas and a substrate, and refers to isotropic and / or anisotropic etching processes. Isotropic etching processes involve a chemical reaction between an etching compound and a substrate, which removes a portion of the material on the substrate. This type of etching process includes chemical dry etching, vapor phase chemical etching, thermal dry etching, and the like. Isotropic etching processes produce lateral or horizontal etching profiles in the substrate. Isotropic etching processes produce recesses or horizontal recesses in the sidewalls of preformed apertures in the substrate. Anisotropic etching processes include plasma etching processes (i.e., dry etching processes) in which chemical reactions are accelerated vertically by ion bombardment, resulting in the formation of vertical sidewalls perpendicular to the substrate along the edges of masked features (Manos and Flamm, Thermal etching an Introduction, Academic Press, Inc. 1989 pp. 12-13). Plasma etching processes produce vertical etching profiles in the substrate. The plasma etching process creates vertical vias, apertures, trenches, channel holes, gate trenches, stepped contacts, capacitor holes, contact holes, slit etches, self-aligned contacts, self-aligned vias, supervias, and the like in the substrate.

[0023] The term "mask" refers to a layer that resists etching. A mask layer can be disposed over a layer to be etched. A mask layer also refers to a hard mask layer. A mask layer can be a carbon-containing layer, a silicon-containing layer, a metal-containing layer, a metal oxide-containing layer, or a metal nitride-containing layer.

[0024] The term "etch stop" refers to a layer below the layer being etched that protects the layer below.

[0025] The term "device channel" refers to a layer that is part of the actual device and any damage to it will affect device performance.

[0026] The term "aspect ratio" refers to the ratio of the height of a trench (or a via) to the width of the trench (or the diameter of a via).

[0027] The term "selectivity" refers to the ratio of the etch rate of one material to the etch rate of another material. The terms "selective etch" or "selective etching" refer to etching one material over another, or in other words, an etch selectivity between two materials that is greater than or less than 1:1.

[0028] The term "independently," when used in reference to describing an R group, should be understood to mean that the R group in question is not only independently selected with respect to other R groups having the same or different subscripts or superscripts, but also independently selected with respect to any additional species of the same R group. For example, the formula MR 1 x (NR 2 R 3 ) (4-x) In the above, two or three R 1 The groups may be mutually exclusive or R 2 Or R 3Additionally, unless otherwise specified, it should be understood that the values ​​of R groups are independent of each other when used in different formulas.

[0029] It should be noted that the terms "film" and "layer" may be used interchangeably herein. It is understood that a film may correspond to or relate to a layer, and that a layer may be referred to as a film. Furthermore, one skilled in the art will recognize that the terms "film" or "layer" as used herein refer to a thickness of some material applied or spread over a surface, and that the surface may range from as large as an entire wafer to as small as a trench or line.

[0030] It should be noted that the terms "etching compound" and "etching gas" may be used interchangeably herein. It is understood that an etching compound may correspond to or relate to an etching gas, and an etching gas may refer to an etching compound.

[0031] The terms "via," "aperture," "trench," and "hole" may be used interchangeably and generally refer to an opening in an interlayer dielectric.

[0032] As used herein, the abbreviation "NAND" refers to a "Negated AND" or "Not AND" gate, the abbreviation "2D" refers to a two-dimensional gate structure on a flat substrate, and the abbreviation "3D" refers to a three-dimensional or vertical gate structure in which the gate structures are stacked vertically.

[0033] Standard abbreviations of elements from the periodic table are used herein. It should be understood that elements can be represented by these abbreviations (e.g., Si means silicon, N means nitrogen, O means oxygen, C means carbon, H means hydrogen, F means fluorine, etc.).

[0034] Unique Chemical Abstract Service (CAS) Registry Numbers assigned by the Chemical Abstract Service (ie, "CAS") are provided to aid in better identifying the disclosed molecules.

[0035] It should be noted that silicon-containing films such as silicon nitride and silicon oxide are recited throughout the specification and claims without indicating their appropriate stoichiometry. Silicon-containing films include pure silicon (Si) layers such as crystalline Si, polysilicon (p-Si or polycrystalline Si) or amorphous silicon; silicon nitride (Si k N l ) layer; silicon oxide (Si n O m ) layer; or a mixture thereof, where k, l, m and n are inclusively in the range of 0.1 to 6. Preferably, the silicon nitride is a SiN layer, where k and I are in the range of 0.5 to 1.5, respectively. k N l More preferably, the silicon nitride is Si3N4. Preferably, the silicon oxide is SiN, where n is in the range of 0.5 to 1.5 and m is in the range of 1.5 to 3.5. n O m More preferably, the silicon oxide is SiO2. In the present specification and the following, SiN and SiO are respectively Si k N l and Si n O m It is used to represent a containing layer. The silicon-containing film can also be a silicon oxide-based dielectric material, such as an organic-based or silicon oxide-based low-k dielectric material, such as Black Diamond II or III materials by Applied Materials, Inc., with SiOCH. The silicon-containing film can include SiaObCcNdHe, where a, b, c, d, e range from 0.1 to 6. The silicon-containing film can also include dopants, such as B, C, P, As, Ga, In, Sn, Sb, Bi, and / or Ge.

[0036] Ranges may be expressed herein as from about one particular value, and / or to about another particular value, When such a range is expressed, it should be understood that another embodiment is from the one particular value and / or to the other particular value, along with all combinations within said ranges.

[0037] References herein to "one embodiment" or "an embodiment" mean that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of the invention. The appearances of the phrase "in one embodiment" in various places in the specification do not necessarily all refer to the same embodiment, and separate or alternative embodiments are not necessarily mutually exclusive of other embodiments. The same applies to the term "implementation."

[0038] For a better understanding of the nature and objects of the present invention, the following detailed description should be read in conjunction with the accompanying drawings, in which like elements are given the same or similar reference numerals, and in which: [Brief description of the drawings]

[0039] [Figure 1a] FIG. 1a is a cross-sectional view of an exemplary layer in a 3D NAND stack. [Figure 1b] FIG. 1b is a cross-sectional view of exemplary layers in a 3D NAND stack showing polymer deposited on the sidewalls during etching of the 3D NAND stack. [Figure 1c] FIG. 1c is a cross-sectional view of an exemplary layer in a 3D NAND stack illustrating particles generated during etching of alternating SiO / SiN layers of the 3D NAND stack. [Figure 1d] FIG. 1d is a cross-sectional view of an exemplary layer in a 3D NAND stack illustrating selective etching of SiN exposed on sidewalls in the 3D NAND stack. [Diagram 2] FIG. 2 is a cross-sectional view of an exemplary layer of a DRAM stack. [Figure 3a]FIG. 3a is an exemplary layer cross-sectional view showing a photoresist pattern on a SiO insulating layer around a typical transistor device area for creating a transistor structure. [Figure 3b] FIG. 3b is a cross-sectional view of the exemplary layers of FIG. 3a after etching of the SiO insulating layer. [Figure 4] FIG. 4 shows the etch rate (ER) and selectivity of C3F7IO on four different substrates. [Figure 5a] FIG. 5a is an X-ray photoelectron spectroscopy (XPS) depth profile showing atomic concentration (%) versus Ar etch time of an amorphous carbon pattern mask etched by C3F7IO. [Figure 5b] FIG. 5b is a close-up of the X-ray photoelectron spectroscopy (XPS) depth profile showing atomic concentration (%) versus Ar etch time of an amorphous carbon pattern mask etched by C3F7IO, highlighting the iodine and oxygen doping of the mask. [Figure 6a] FIG. 6a is an X-ray photoelectron spectroscopy (XPS) depth profile showing atomic concentration (%) versus Ar etch time for a silicon substrate etched by C3F7IO. [Figure 6b] Figure 6b is a close-up of the X-ray photoelectron spectroscopy (XPS) depth profile showing the atomic concentration (%) versus Ar etch time of a silicon substrate etched by C3F7IO, highlighting the oxygen doping of the mask. [Figure 7] FIG. 7 is an X-ray photoelectron spectroscopy (XPS) plot of counts per second versus binding energy (eV) for the fluorine (F1s) and iodine (I3d) peaks of an amorphous carbon pattern mask etched by C3F7IO. [Figure 8] FIG. 8 shows the etch rate (ER) and selectivity of C4F6 on four different substrates versus oxygen flow rate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0040] A method is disclosed for plasma etching of semiconductor structures such as trenches, nanolines, nanopillars, channel holes, gate trenches, contacts, stepped contacts, capacitor holes, contact holes, high aspect ratio structures, 3D NAND structures, DRAM structures, slit trenches, self-aligned contacts, vias, self-aligned vias, supervias, etc. in silicon-containing films. The disclosed method comprises: i) reacting a compound of formula C in a reaction chamber containing a substrate having a film deposited thereon and a patterned mask layer deposited on the film. a H b F c I d O e (wherein 0≦a≦10, 0≦b≦21, 0≦c≦21, 1≦d≦4, and 1≦e≦2); ii) activating the plasma to generate an activated etching compound containing oxygen and iodine that can etch the film on the patterned mask layer from the substrate. During the etching of the film, iodine from the activated etching compound containing oxygen and iodine is doped into the patterned mask layer, reinforcing or strengthening the patterned mask layer, thereby minimizing damage to the patterned mask layer. The film here may be a silicon-containing film.

[0041] As shown in the examples below, the iodine ions of the disclosed oxygen-iodine containing etching compounds dissociate from the compounds at low energy (eV) (i.e., <20 eV). As a result, applicants believe that the disclosed etching compounds may be used in dry plasma etching processes that cause less damage to the underlying substrate because they are viable at lower plasma energies. For example, the disclosed oxygen-iodine containing etching compounds may be particularly suitable for low-k etching processes where damage is of particular concern because lower plasma energies cause less damage to the porous low-k material surrounding the etch site. The lower damage to the low-k material may be due to the reduced generation of UV photons and F radicals imparted by the oxygen-iodine containing etching compounds. The disclosed oxygen-iodine containing etching compounds may also prevent loss of critical dimensions and reduce low-k surface roughness. In addition, molecules with two iodine atoms may enhance these benefits, increase doping levels, and preserve the mask layer without damaging the underlying layer.

[0042] Iodine (10.5 eV) has a lower ionization threshold than fluorine (17.4 eV) and the inert gases: Ar (15.8 eV), Xe (12.1 eV), and Kr (14 eV). Therefore, iodine can be ionized by the plasma more easily than fluorine, and iodine-containing etching compounds can increase the plasma density. Iodine is a heavy element (mass 127 amu) and can also behave similarly to the inert gases in the plasma (Kr at 88 amu, Xe at 131 amu, etc.), accelerating toward the wafer. During etching of high aspect ratio structures, many ions cannot reach the bottom of the trench because the deeper the ions penetrate, the weaker their energy becomes. However, the heavy iodine ions can be accelerated toward the wafer by the voltage applied during the plasma etching process and penetrate deep, allowing deep patterned structures with high aspect ratios to be etched. The ionization threshold of fluorine is useful for maintaining it as a neutral species. As a result, fluorine is typically involved in the etching process through chemical reactions. Iodine exhibits lower chemical reactivity than fluorine and is ionized and bombards the surface during the plasma etching process. Also, the bond energy of CI is lower than that of CF, thereby CI bonds are more easily broken in the plasma compared to CF bonds. Therefore, iodine ions can be easily doped into the aC mask layer. Since iodine is a heavy element, it is easier to inject and penetrate deeper into the mask layer than light elements. In addition, due to the fact that the CI bond is weak and the ionization threshold of iodine is low, the atmospheric lifetime of iodine-containing etching compounds is short or negligible, making them good candidates for reducing the global warming potential (GWP) caused by perfluorocarbon compounds. The average bond energies of various bonds are shown in Table 1 (from Huheey et al., Inorganic Chemistry, 4th ed. (1993)).

[0043] [Table 1]

[0044] As mentioned in the comparative examples below, iodine ions dissociate from the disclosed etching compounds at low eV (i.e., <20 eV). However, iodine ions can be implanted into mask features such as the surface and / or body / bulk. This implantation can help strengthen the mask features, minimize damage, improve etch resistance, and maintain shape and profile during the etching process. As shown in the examples below, the composition of the pattern mask is modified after using the disclosed oxygen and iodine containing etching compounds. Applicants believe that iodine ions modify the surface and are incorporated into the bulk of the pattern mask layer by increasing cross-linking with organic mask layers (such as amorphous carbon masks). Due to the doping of iodine ions and cross-linking between carbon, iodine, hydrogen and fluorine atoms, preferably between carbon and iodine, the density of the pattern mask layer is increased, which makes the pattern mask layer stronger. In the following examples, the strengthening effect and improved etch resistance of iodine ions is demonstrated by showing that the etch rate of a patterned mask layer is lower when etched with an iodine-containing etching compound than when etched with conventional etching gases such as cC4F8 and C4F6.

[0045] The crux of the present invention is understanding the effect of iodine on amorphous carbon. Iodine helps preserve the aC mask during etching by modifying and doping the surface of the aC layer. It is also useful in minimizing damage by strengthening the patterned mask layer. During plasma processing, the disclosed iodine-containing gases or precursors can be generated in the following forms: 1) iodine ions (I + , I - );2) Iodine radical (I );3) Iodine-containing polymer ions ( + C x H y I z F d O e , - C x Hy I z F d O e ); and 4) iodine-containing polymer radicals (·C x H y I z F d O e ). The iodine-containing species can be deposited on the carbon-containing layer by controlling the bias power. Furthermore, these chemical forms are deposited as polymer layers that can enhance the EUV absorption of the layer during the patterning process. Doping the carbon matrix with iodine ions and radicals can enhance the EUV absorption of the layer during patterning processes such as resistless lithography. The iodine-containing polymer and / or iodine-doped carbon layers so formed can be utilized to enhance the etch selectivity to the layer being etched, such as a silicon-containing layer.

[0046] The disclosed oxygen and iodine containing etching compounds have the formula C a H b F c I d O e (Wherein, 0≦a≦10, 0≦b≦21, 0≦c≦21, 1≦d≦4, and 1≦e≦2.) has.

[0047] When the disclosed oxygen and iodine containing etching compound contains one oxygen (i.e., e=1), the disclosed oxygen and iodine containing etching compound has the formula C a H b F c I d O (Wherein, 0≦a≦10, 0≦b≦21, 0≦c≦21, and 1≦d≦4.) where an oxygen links two carbons forming a bridge between the two carbons.

[0048] When the disclosed oxygen and iodine containing etching compounds do not contain hydrogen (i.e., b=0), the disclosed oxygen and iodine containing etching compounds have the formula C a F c I d O e (Wherein, 0≦a≦10, 0≦c≦21, 1≦d≦4, and 1≦e≦2.) In this case, when a=3, the disclosed oxygen and iodine containing etching compound has the formula C3F c I d O e where 1≦d≦4, c≦10−d, and 1≦e≦2. Exemplary C3 oxygen and iodine-containing etching compounds that do not contain H include C3F7IO, C3F6I2O, C3F5I3O, C3F4I4O, and isomers thereof.

[0049] Exemplary disclosed oxygen and iodine containing etching compounds that do not contain H include C3F7IO, C3F6I2O, C3F5I3O, C3F4I4O, C4F9IO, C4F8I2O, C4F7I3O, C4F6I4O, C5F 11 IO, C5F 10 I2O, C5F9I3O, C5F8I4O, C6F 13 IO, C6F 12 I2O, C6F 11 I3O, C6F 10 I4O, C7F 15 IO, C7F 14 I2O, C7F 13 I3O, C7F 12 I4O, C8F 17 IO, C8F 16 I2O, C8F 15 I3O, C8F 14 I4O, C9F 19 IO, C9F 18 I2O, C9F 17 I3O, C8F 16 I4O, C 10 F 21 I.O., C. 10 F 20 I2O, C10 F 19 I3O, C 10 F 18 IO and their isomers, where the oxygen connects two carbons and forms a bridge between the two carbons.

[0050] Contains one oxygen and one iodine and no H, general formula C a F 2a+1 Exemplary disclosed etching compounds having IO, where 0≦a≦10, are listed in Table 2. These molecules are commercially available or can be synthesized by methods known in the art. Their structural formulas, CAS numbers, and boiling points are included in Table 2. Compounds having the general formula C, which contain oxygen and iodine but no H, are also disclosed. a F 2a+1 The disclosed etching compounds having IO, where 3≦a≦10, may also include their isomers. More specifically, oxygen links two carbons to form a bridge between the two carbons.

[0051] [Table 2]

[0052] The disclosed oxygen and iodine containing etching compounds can be used to etch silicon oxide (SiO), silicon nitride (SiN), pure silicon (Si), e.g., crystalline Si, polysilicon (p-Si or polycrystalline Si), or amorphous silicon, low dielectric constant SiCOH, SiOCN, SiC, SiON, Si a O b H c C d N e (wherein a>0; b, c, d, and e≧0), or combinations thereof. The silicon-containing film may also include alternating layers of silicon oxide and silicon nitride (ONON) or alternating layers of silicon oxide and polysilicon (OPOP). The silicon-containing film may also include dopants such as B, C, P, As, Ga, In, Sn, Sb, Bi, and / or Ge.

[0053] The disclosed oxygen- and iodine-containing etching compounds, when containing H, can improve the etch rate of SiO and SiN while maintaining high selectivity to the mask layer, but are not limited thereto. The disclosed oxygen- and iodine-containing etching compounds having one H when b=1 can be represented by the formula C a HF c I d O e (wherein 3≦a≦10, 0≦c≦20, 1≦d≦4, y+z≦2n+1, and 1≦e≦2). Exemplary compounds having one H include C3HF6IO, C3HF5I2O, C3HF4I3O, C3HF3I4O, C4HF8IO, C4HF7I2O, C4HF6I3O, C4HF5I4O, C5HF 10 IO, C5HF9I2O, C5HF8I3O, C5HF7I4O, C6HF 12 IO, C6HF 11 I2O, C6HF9I3O, C6HF8I4O, C7HF 14 IO, C7HF 13 I2O, C7HF 12 I3O, C7HF 11 I4O, C8HF 16 IO, C8HF 15 I2O, C8HF 14 I3O, C8HF 10 I4O, C9HF 18 IO, C9HF 17 I2O, C9HF 16 I3O, C9HF 15 I4O, C 10 HF 20 I.O., C. 10 HF 19 I2O, C 10 HF 18 I3O, C 10 HF 17 IO and their isomers.

[0054] The disclosed oxygen and iodine containing etching compounds having two hydrogens where b=2 are represented by the formula C a H2F c I d O ewhere 3≦a≦10, 0≦c≦19, 1≦d≦4, c+d≦2n, and 1≦e≦2. Exemplary compounds include:

[0055] The disclosed oxygen and iodine containing etching compound having three hydrogens where b=3 has the formula C a H3F c I d O e wherein 3≦a≦10, 0≦c≦19, 1≦d≦4, c+d≦2n-1, and 1≦e≦2.

[0056] The disclosed oxygen and iodine containing etching compound having four hydrogens where b=4 has the formula C a H3F c I d O e wherein 3≦a≦10, 0≦c≦19, 1≦d≦4, c+d≦2n-2, and 1≦e≦2.

[0057] Applicants believe that molecules with three or more carbon atoms can provide better etch rates and sidewall protection during the etching process, such as straighter profiles, no bending, no tapering, no kinks, no incomplete etching, and no variation in critical dimensions from the top to the bottom of the etched structure, than molecules with less than three carbons. Applicants also believe that molecules with four or more carbon atoms can provide straighter profiles, with no bending, tapering, kinks, and no incomplete etching, or variation in critical dimensions from the top to the bottom of the etched structure, than molecules with less than four carbons. Applicants believe that molecules with three or more carbons create a thicker passivation layer, and are therefore preferred for sidewall protection.

[0058] The disclosed oxygen and iodine containing etch compounds can provide high selectivity to mask layers, photoresists, etch stop layers and device channel materials and can provide no profile distortion in high aspect ratio structures (HAR), such as DRAM and 3D NAND memory and logic structures having aspect ratios ranging from 1:1 to 200:1. Instead, the disclosed oxygen and iodine containing etch compounds can provide high selectivity to mask layers or silicon-containing films, such as those having aspect ratios ranging from 1:1 to 200:1 in contact etch applications.

[0059] The disclosed oxygen and iodine containing etching compounds can provide a myriad of selectivities for a wide range of process conditions for etching. As used herein, selectivity refers to the etch rate ratio of two different layers. For example, the selectivity for a SiO layer to an aC layer is the etch rate of SiO divided by the etch rate of the aC layer. The disclosed oxygen and iodine containing etching compounds can provide improved selectivity between silicon-containing films and mask materials, reduced damage to the channel region, improved critical dimension uniformity, and reduced profile distortions such as bowing, kinking, tapering, notches, undercuts, and can maintain the same critical dimensions from the top to the bottom of the etched structure and arcing to pattern high aspect ratio structures. The disclosed oxygen and iodine containing etching compounds can etch through alternating layers of p-Si, SiO, and / or SiN, resulting in a vertical etch profile (i.e., selectivity ranging from 2:1 to 1:2 between alternating layers). A plasma of the disclosed oxygen and iodine containing etching compound etches alternating layers of SiO and SiN(ONON) with a selectivity of about 1:2 to about 2:1 for SiO layers to SiN layers. Preferably, a plasma of the disclosed oxygen and iodine containing etching compound etches alternating layers of SiO and SiN(ONON) with a selectivity of about 1:1 for SiO layers to SiN layers.

[0060] The disclosed oxygen and iodine containing etching compounds are provided with a purity of greater than 95% v / v, preferably greater than 99.99% v / v, more preferably greater than 99.999% v / v. The disclosed oxygen and iodine containing etching compounds contain less than 5% by volume of trace gas impurities, including impurity gases such as N2 and / or H2O and / or CO2, less than 150 ppm by volume. Preferably, the water content in the plasma etching gas is less than 20 ppm by weight. Purified products can be produced by distillation and / or passing the gas or liquid through a suitable adsorbent, such as a 4 Å molecular sieve.

[0061] The disclosed oxygen and iodine containing etching compounds contain less than 10% v / v, preferably less than 1% v / v, more preferably less than 0.1% v / v, even more preferably less than 0.01% v / v of any of its isomers, which can be purified by distillation of the gas or liquid to remove the isomers and provide better process repeatability.

[0062] Alternatively, the disclosed oxygen and iodine containing etching compounds may contain 0.01% v / v to 99.99% v / v of the isomer, particularly when the isomer mixture provides improved process parameters or when isolation of the target isomer is difficult or too costly. For example, the disclosed oxygen and iodine containing etching compounds may contain about 50% v / v to about 75% v / v of 2-iodo-1-(trifluoromethoxy)tetrafluoroethane, about 25% v / v to about 50% v / v of 1,1,1,2-tetrafluoro-2-iodo-2-(trifluoromethoxy)ethane, and about 25% v / v to about 50% v / v of 1,2,2,2-tetrafluoro-1-trifluoromethoxy-1-iodoethane. The mixture of isomers may also reduce the need for two or more gas lines to the reaction chamber.

[0063] Some of the disclosed oxygen and iodine-containing etching compounds are gaseous at room temperature and pressure. For non-gaseous (i.e., liquid or solid) compounds, their gaseous form can be generated by evaporating the compound by a conventional evaporation step such as direct evaporation or by bubbling with an inert gas (N2, Ar, He, etc.). The non-gaseous compound can be provided in liquid form to an evaporator that evaporates it before introducing it into the reactor.

[0064] The disclosed oxygen and iodine-containing etching compounds are suitable for plasma etching of semiconductor structures such as channel holes, gate trenches, stepped contacts, slits, capacitor holes, contact holes, self-aligned contacts, self-aligned vias, and supervias in silicon-containing films. Because the disclosed oxygen and iodine-containing etching compounds induce no or only slight damage on the mask with good profile of high aspect ratio structures, the disclosed oxygen and iodine-containing etching compounds are not only compatible with currently available mask materials, but also with next-generation mask materials. In other words, the disclosed oxygen and iodine-containing etching compounds can create vertical etch patterns with minimal or no distortion, pattern collapse, or roughness. To achieve these properties, the disclosed oxygen and iodine-containing etching compounds may deposit an etch-resistant polymer layer during etching to help reduce the direct effect of oxygen and fluorine radicals during the etching process. The disclosed oxygen and iodine containing etching compounds can reduce damage to p-Si or crystalline Si channels and silicon-containing structures during etching.

[0065] The disclosed oxygen and iodine-containing etching compound selectively etches the silicon-containing layer from the buried landing layer or material, which in most applications is the metal layer located at the bottom of the structure to be etched. The disclosed oxygen and iodine-containing etching compound does not etch the landing layer or metal landing layer. The buried landing layer may be an etch stop layer or a diffusion barrier layer. The material of the metal landing layer may be the tungsten metal world lines of the 3D NAND structure, and / or another metal, such as W, Cu, Al, Ru, Pt, Ti, Ta, Ni, Co, Mo, Mn, Pd, Ir, Nb, Cr, Rh, V, Au, Ag, or a combination thereof, and / or an etch stop layer, such as a metal or metal oxide or nitride layer (such as AlO, WO, HfO, TiO, TaO, InO, CrO, RuO, CoO, MoO, ZrO, SnO, TiN, TaN, HfN, AlN, WN, MoN, NiN, NbN, CrN, RuN, CoN, ZrN, SnN, or a combination thereof). The disclosed oxygen and iodine containing etching compounds induce little or no damage to the materials at the bottom of the contact holes, steps and slits (such as the tungsten metal world lines of the 3D NAND structure and / or other metals such as W, Cu, Al, Ru, Pt, Ti, Ta, Ni, Co, Mo, Mn, Pd, Ir, Nb, Cr, Rh, V, Au, Ag, or combinations thereof), and / or etch stop layers such as metal or metal oxide or nitride layers (such as AlO, WO, HfO, TiO, TaO, InO, CrO, RuO, CoO, MoO, ZrO, SnO, TiN, TaN, HfN, AlN, WN, MoN, NiN, NbN, CrN, RuN, CoN, ZrN, SnN, or combinations thereof). Those skilled in the art will recognize that the barrier layers may also be composed of combinations of the aforementioned metals and metal oxides and nitrides, such as Ti / TiN, Ti / TiN / Ti, TiZrN, Ta / TaN, TaN / Cu / TaN, TaN / Ru / TaN, etc.The barrier may also include silicides (TiSiN, TaSiN, TiSi2, MnSiO, etc.), phosphides (CuWP, NiMoP, NiP, etc.), carbides (TaC, TaCN, WCN, etc.), borides (NiMoB, NiB, etc.), or combinations thereof. Preferably, the disclosed oxygen and iodine containing etching compounds are suitably volatile and stable during the etching process for delivery into the reactor / chamber.

[0066] Material compatibility testing is important to determine whether any of the disclosed oxygen and iodine-containing etching compounds will react with the chamber materials and degrade the chamber performance with short-term or long-term use. Important materials associated with some of the chambers, valves, etc. include stainless steel, aluminum, nickel, polychlorotrifluoroethylene (PCTFE), polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), PFA, PP, kalrez, viton, and other metals and polymers. Sometimes these materials are exposed to high temperatures, e.g., temperatures greater than 20°C, and high pressures, e.g., pressures greater than 1 atm, which may enhance their degradation. Measurement methods may include visual inspection, weight measurements, measuring changes on the nanometer scale in scanning electron microscopy (SEM), tensile strength, hardness, etc.

[0067] The disclosed oxygen and iodine containing etching compounds can be used to plasma etch silicon-containing films on substrates. The disclosed plasma etching methods can be useful in the manufacture of semiconductor devices such as NAND or 3D NAND gates, or flash or DRAM memories or transistors such as fin-shaped field-effect transistors (FinFETs), gate-all-around (GAA) FETs, nanowire FETs, nanosheet FETs, fork-sheet FETs, complementary FETs (CFETs), bulk complementary metal oxide semiconductors (bulk CMOS), MOSFETs, fully depleted silicon-on-insulator (FD-SOI) structures. The disclosed oxygen and iodine containing etching compounds can be useful in other areas of applications such as different front end of the line (FEOL) and back end of the line (BEOL) etching applications. Additionally, the disclosed oxygen and iodine containing etching compounds can be used to interconnect memory to logic on a substrate, to etch Si in 3D through silicon via (TSV) etching applications, and in MEMS applications.

[0068] The plasma etching method includes providing a reaction chamber having a substrate disposed therein. The reaction chamber can be any enclosure or chamber in a device in which an etching method is performed, such as, but not limited to, a reactive ion etch (RIE), a capacitively coupled plasma (CCP) with single or multiple frequency RF sources, an inductively coupled plasma (ICP), or a microwave plasma reactor, or other type of etching system capable of selectively removing a portion of a silicon-containing film or generating active species. Those skilled in the art will recognize that different plasma reaction chamber designs provide different electronic temperature control. Suitable commercially available plasma reaction chambers include, but are not limited to, Applied Materials magnetically enhanced reactive ion etcher sold under the trademark eMAX™, or Lam Research Dual CCP reactive ion etcher dielectric etching product line sold under the trademark 2300® Flex™. The RF power therein may be intermittent to control the plasma characteristics and thereby further improve the etching performance (selectivity and damage).

[0069] Alternatively, the plasma treated reactants can be generated outside the reaction chamber. MKS Instruments' ASTRONi® reactive gas generator can be used to treat the reactants prior to passage into the reaction chamber. When operated at 2.45 GHz, 7 kW plasma power, and pressures ranging from about 0.5 Torr to about 10 Torr, the reactant O2 can decompose into two O· radicals. Preferably, the remote plasma can be generated at a power ranging from about 1 kW to about 10 kW, more preferably from about 2.5 kW to about 7.5 kW.

[0070] The reaction chamber may contain one or more substrates. For example, the reaction chamber may contain 1 to 200 silicon wafers with diameters between 25.4 mm and 450 mm. The substrate may be any suitable substrate used in semiconductor, photovoltaic, flat panel or LCD-TFT device manufacturing. Examples of suitable substrates include wafers such as silicon, silica, glass, Ge, SiGe, GeSn, InGaAs, GaSb, InP or GaAs wafers. The wafer will have multiple films or layers thereon from previous manufacturing steps, including silicon-containing films or layers. The layers may be patterned or unpatterned. Examples of suitable layers include, but are not limited to, silicon (amorphous silicon, p-Si, crystalline silicon, any of which may be further p-doped or n-doped with B, C, P, As, Ga, In, Sn, Sb, Bi and / or Ge), silica, silicon nitride, silicon oxide, silicon oxynitride, Si a O b H c C d N e where a>0; b, c, d, e>0; Ge, SiGe, GeSn, InGaAs, GaSb, InP; mask layer materials such as amorphous carbon with or without dopants, anti-reflective coatings, photoresist materials, metal oxides such as AlO, TiO, HfO, ZrO, SnO, TaO, or metal nitride layers such as AlN, ZrN, SnN, HfN, titanium nitride, tantalum nitride, etc., or combinations thereof; silicon nitride, polysilicon, crystalline silicon, silicon carbide, SiON, SiCN, or combinations thereof; device channel materials such as crystalline silicon, epitaxial silicon, doped silicon, Si a O b H c C d N e(wherein a>0; b, c, d, e≧0) or combinations thereof. In one example, the mask layer may be composed of two or more layers, such as a combination of a carbon-containing layer, and / or a silicon-containing layer, and / or a metal-containing layer. In one example, the mask may be SiN and TiN, and the landing layer is Cu, W, or Ru. The silicon oxide layer may form a dielectric material, such as an organic-based or silicon oxide-based low-k dielectric material (e.g., porous SiCOH film). Exemplary low-k dielectric materials are sold by Applied Materials under the trade names Black Diamond II or III. Additionally, layers containing tungsten or precious metals (e.g., platinum, palladium, rhodium, or gold) may be used. Additionally, examples of silicon-containing films include Si a O b H c C d N e where a>0; b, c, d, e>0. Throughout the specification and claims, the wafer and any associated layers thereof are referred to as the substrate.

[0071] The following are exemplary embodiments of substrates to which the disclosed oxygen and iodine containing etching compounds may be applied for etching.

[0072] In one embodiment, the substrate 100 may include a stack of multiple layers, as shown in Figure 1a, which is a cross-sectional view of an exemplary layer in a 3D NAND stack for creating a 3D NAND gate. In Figure 1a, a stack of seven alternating SiO / SiN (i.e., 104a / 104b) layers 104 is located on a silicon wafer 102 (i.e., ONON or terabit cell array transistor (TCAT) technology). In some applications, the wafer 102 may be a buried landing layer or material, such as tungsten metal world lines of a 3D NAND structure and / or another metal, such as W, Cu, Al, Ru, Pt, Ti, Ta, Ni, Co, Mo, Mn, Pd, Ir, Nb, Cr, Rh, V, Au, Ag, or combinations thereof, and / or an etch stop layer or diffusion barrier layer, such as a metal or metal oxide or nitride layer (such as AlO, WO, HfO, TiO, TaO, InO, WO, CrO, RuO, CoO, MoO, TiN, TaN, HfN, AlN, WN, MoN, NiN, NbN, CrN, RuN, CoN, or combinations thereof). One skilled in the art will recognize that the barrier layer, such as Ti / TiN, Ti / TiN / Ti, TiZrN, Ta / TaN, TaN / Cu / TaN, TaN / Ru / TaN, etc., may also be comprised of combinations of the aforementioned metals and metal oxides and nitrides. The barrier may also include silicides (TiSiN, TaSiN, TiSi2, MnSiO, etc.), phosphides (CuWP, NiMoP, NiP, etc.), carbides (TaC, TaCN, WCN, etc.), borides (NiMoB, NiB, etc.), or combinations thereof. Those skilled in the art will recognize that the SiN layer 104b may be replaced by a p-Si layer by some techniques (e.g., SiO / p-Si or pipe-shaped bit cost scalable (p-BICS) techniques). A hardmask layer 106 is located on top of the seven SiO / SiN layers 104. The hardmask layer 106 may be an amorphous carbon (aC) hardmask layer with or without dopants.The hard mask layer 106 may be a layer of CVD, PECVD, ALD, PEALD or spin-on-deposited (SOD) amorphous carbon or doped amorphous carbon, silicon-containing spin-on mask, or carbon-containing spin-on mask. The hard mask layer 106 may contain other elements such as boron, nitrogen, sulfur, chlorine, fluorine, or metals (Al, Zr, Ti, W, Y) as well as C and H to enhance the etch resistance during SiO / SiN layer etching. In this case, the hard mask layer 106 is a doped aC layer, such as a boron doped aC layer, a tungsten doped aC layer, etc. An antireflective coating layer 108 is located on top of the hard mask layer 106. A patterned photoresist layer 110 is located on top of the antireflective coating layer 108 having a pattern 112. Herein, a SiON layer (not shown) may be present between the anti-reflective coating layer 108 and the hard mask layer 106 to transfer the pattern 112 in the photoresist layer 110 to the hard mask layer 106 to form a patterned hard mask layer (not shown). Those skilled in the art will recognize that the stack of layers in the substrate 100 in FIG. 1a is provided for exemplary purposes only, and that the disclosed oxygen- and iodine-containing etching compounds may be used to etch other types of layer stacks. Furthermore, those skilled in the art will recognize that the number of alternating SiO / SiN or SiO / p-Si layers 104 in the substrate 100 stack may vary (i.e., may include more or less than the seven SiO / SiN (104a / 104b) layers described).

[0073] FIG. 1b is a cross-sectional view of an exemplary layer in the 3D NAND stack of FIG. 1a, showing a polymer deposited on the sidewall of the etched structure or via 112a. The disclosed oxygen- and iodine-containing etching compound may generate fragments during a plasma process suitable for anisotropic etching of the silicon-containing film 104 and deposition of the oxygen- and iodine-containing polymer passivation layer 214 on the sidewall of the etched structure or via 112a as shown in FIG. 1b. The difference between FIG. 1b and FIG. 1a is that in FIG. 1b, the structure or via 112a is formed in the substrate 100 by plasma etching using the disclosed oxygen- and iodine-containing etching compound, which also deposits the polymer passivation layer 214 on the sidewall of the structure or via 112a. The polymer passivation layer 214 also provides smoother sidewalls, less distortion and less deformation at the bottom of the structure or via 212. However, the polymer passivation layer 214 can be easily removed or cleaned by dry or wet etching chemistries known in the art.

[0074] FIG. 1c is a cross-sectional view of an exemplary layer in the 3D NAND stack of FIG. 1a, showing particles 316 generated during alternating SiO / SiN layer etching in the 3D NAND stack. As shown in FIG. 1c, particles 316 generated on the sidewalls of the alternating SiO / SiN (i.e., 104a / 104b) layers 104 can be minimized by using the disclosed oxygen and iodine containing etching compound. The difference between FIG. 1c and FIG. 1b is that in FIG. 1c, the alternating SiO / SiN exposed side has particles 316 generated during plasma etching. Applicants do not believe that the disclosed oxygen and iodine containing etching compound generates the particles 316 shown in FIG. 1c.

[0075] FIG. 1d is a cross-sectional view of an exemplary layer in the 3D NAND stack of FIG. 1a, showing selective isotropic etching of the SiN layer 104b exposed on the sidewall in the 3D NAND stack after an anisotropic etching process. The SiN exposed side in the stack 100 can be selectively etched as shown in FIG. 1d by using the disclosed oxygen and iodine containing etching compound to selectively break the Si-N bond in the SiN layer 104b over the Si-O bond in the SiO layer 104a, forming the selective sidewall SiN etch 418 on the stack in the SiO / SiN layer 104 in the via 112a. The difference between FIG. 1d and FIG. 1b is that in FIG. 1d, the SiN layer exposed on the alternating SiO / SiN sidewall is selectively etched by the disclosed oxygen and iodine containing etching compound to form the selective sidewall SiN etch 418. Typically, the selective sidewall SiN etch 418 is performed by wet etching using a mixture with phosphoric acid. It is known that replacing the wet etching process with a dry plasma etching process greatly improves the economics of the semiconductor device fabrication process because wet etching requires moving the substrate to a different wet etching apparatus. With the disclosed method, all etches, including the selective sidewall SiN etch of FIG. 1d, can be performed in an integrated etching apparatus, which can reduce the cost of semiconductor fabrication.

[0076] In another embodiment, the substrate 200 may include a stack of layers, as shown in FIG. 2, which is a cross-sectional view of an exemplary layer in a DRAM stack for creating a DRAM memory. As shown, a four-layer stack is located on a silicon wafer 202. A hard mask layer 206 is located on top of a large SiO layer 204. An anti-reflective coating layer 208 is located on top of the hard mask layer 206. A patterned photoresist layer 210 is located on top of the anti-reflective coating 208. There may be a SiON layer (not shown) between the anti-reflective coating layer 208 and the hard mask layer 206 to transfer the pattern 212 in the photoresist layer 210 to the hard mask layer 206. Those skilled in the art will recognize that the layer stack in FIG. 2 is provided for exemplary purposes only, and the disclosed oxygen- and iodine-containing etching compounds may be used to etch other layer stacks, for example, stacks in which the hard mask layer 206 is replaced by a TiN layer. Moreover, one of ordinary skill in the art will recognize that the number of layers in the stack can vary (ie, can include more or less than those depicted).

[0077] FIG. 3a is a cross-sectional side view of an exemplary layer showing a photoresist pattern on a SiO insulating layer surrounding a typical transistor device region for fabricating a transistor structure. As shown, a substrate 300 can include a four-layer stack surrounding a transistor gate electrode region supported on a silicon wafer 302. The illustrated transistor region includes two doped silicon regions 306 that function as a source and drain. A transistor gate dielectric 314 resides below the gate electrode 316. The entire transistor, i.e., the transistor gate dielectric 314 and the gate electrode 316, is surrounded by a thin SiN layer 308, which can subsequently function as an etch stop layer during contact etching. Each transistor device region 306 / 316 is separated by a SiO isolation region 304 in the silicon wafer 302 to minimize electrical interference. Those skilled in the art will recognize that layer 302 may be disposed on top of a silicon oxide layer of a silicon-on-insulator (SOI) wafer (not shown). Another SiO layer 310 as an insulating layer is deposited on the transistor and is used to insulate any metal contacts to the transistor device region 306. A patterned photoresist mask 312 is used to pattern the SiO layer 310. Etching is performed in a plasma environment using the disclosed oxygen and iodine containing etching chemistry. The patterned photoresist mask 312 acts as a template to etch the SiO layer 310, and the etch is stopped on the SiN layer 308, as shown in FIG. 3b.

[0078] Figure 3b is a cross-sectional view of the exemplary layers of Figure 3a after etching of SiO layer 310. The difference between Figure 3b and Figure 3a is that in Figure 3b, a structure or via 318 is formed in SiO layer 310 by etching with the disclosed oxygen and iodine containing etching compound. SiO layer 310 may be etched using photoresist layer 312 as a mask layer. The mask layer may be any suitable photoresist mask material such as TiN, aC, etc. Etching may be stopped at the underlying SiN layer 308.

[0079] The disclosed oxygen- and iodine-containing etching compounds may be used to etch the SiN layer 308 using different plasma conditions and different mixtures of etching compounds. Those skilled in the art will recognize that the layer stacks and geometries of Figures 3a and 3b are provided for exemplary purposes only, and that the disclosed oxygen- and iodine-containing etching compounds may be used to etch other types of layer stacks. Furthermore, those skilled in the art will recognize that the number of layers in the stack may vary (i.e., may include more or less than the four layers described).

[0080] Vapor of the disclosed oxygen and iodine-containing etching compound is introduced into a reaction chamber containing a substrate and a silicon-containing film. The vapor can be introduced into the chamber at a flow rate ranging from about 0.1 sccm to about 1 slm, where sccm is standard cubic centimeters per minute and slm is standard liters per minute. For example, for a 200 mm wafer diameter, the vapor can be introduced into the chamber at a flow rate ranging from about 5 sccm to about 50 sccm. Alternatively, for a 450 mm wafer diameter, the vapor can be introduced into the chamber at a flow rate ranging from about 25 sccm to about 250 sccm. One skilled in the art will recognize that the flow rates can vary from tool to tool.

[0081] The disclosed oxygen- and iodine-containing etching compounds can be provided either neat or in blends with inert gases or solvents such as N2, Ar, Kr, Ne, He, Xe, etc. The disclosed oxygen- and iodine-containing etching compounds can be present in various concentrations in the blend. For liquid oxygen- and iodine-containing etching compounds, the vapor form of the oxygen- and iodine-containing etching compound can be produced by evaporating the neat or blended oxygen- and iodine-containing etching compound solution by a conventional evaporation step such as direct distillation or by bubbling. The neat or blended oxygen- and iodine-containing etching compound can be provided in liquid form to an evaporator that evaporates it before introducing it into the reactor.

[0082] Alternatively, the neat or blended oxygen- and iodine-containing etching compound can be vaporized by passing a carrier gas into a vessel containing the disclosed oxygen- and iodine-containing etching compound or by bubbling a carrier gas into the disclosed oxygen- and iodine-containing etching compound. Carrier gases include, but are not limited to, Ar, He, N2, and mixtures thereof. Bubbling with a carrier gas can remove any dissolved oxygen present in the neat or blended iodine-containing etching compound solution. The carrier gas and the disclosed oxygen- and iodine-containing etching compound are then introduced into the reactor as vapor.

[0083] If necessary, the vessel containing the disclosed oxygen-iodine-containing etching compound may be heated to a temperature that allows the oxygen-iodine-containing etching compound to be in liquid phase and have sufficient vapor pressure for delivery to the etching tool. The vessel may be maintained at a temperature ranging, for example, from about 0° C. to about 150° C., preferably from about 25° C. to about 100° C., more preferably from about 25° C. to about 50° C. More preferably, the vessel is maintained at room temperature (about 25° C.) to avoid heating the lines to the etching tool. Those skilled in the art will recognize that the temperature of the vessel may be adjusted in a well-known manner to control the amount of oxygen-iodine-containing compound that is evaporated.

[0084] Additionally, the disclosed oxygen and iodine containing etching compounds can be delivered in purities ranging from 95% to 99.999% by volume and can be purified by well known standard purification techniques for the removal of CO, CO2, N2, HO, HF, H2S, SO2, halides and other hydrocarbons or hydrohalocarbons.

[0085] An inert gas is also introduced into the reaction chamber to receive the plasma. The inert gases include He, Ar, Xe, Kr, Ne, N 2、 or a combination thereof. The etching gas and the inert gas may be mixed prior to introduction into the chamber such that the inert gas comprises from about 0.01% v / v to about 99.9% v / v of the resulting mixture. Alternatively, the inert gas may be continuously introduced into the chamber while the etching gas is intermittently introduced into the chamber.

[0086] The disclosed oxygen-iodine containing etching compound vapor and inert gas are activated by plasma to generate activated etching gas. The oxygen-iodine containing etching compound decomposes into radical form (i.e., activated etching gas) by plasma. The plasma may be generated by applying RF or DC power. The plasma may be generated by RF power ranging from about 25 W to about 100,000 W. The plasma may be generated remotely or within the reactor itself. The plasma may be generated in dual CCP or ICP mode with RF applied at both electrodes. The RF frequency of the plasma may range from 100 KHz to 1 GHz. Different RF sources at different frequencies may be combined and applied at the same electrode. Further plasma RF pulses may be used to control molecular fragmentation and reactions at the substrate. Those skilled in the art will recognize suitable methods and apparatus for such plasma processing.

[0087] The activated etching gas from the chamber exhaust may be measured by a quadrupole mass spectrometer (QMS), optical emission spectrometer, FTIR or other radical / ion measurement tool to determine the type and number of species generated. If necessary, the flow rates of the etching gas and / or inert gas may be adjusted to increase or decrease the number of radical species generated.

[0088] Vapors of the disclosed oxygen and iodine containing etching compounds may be mixed with other gases either prior to introduction into the reaction chamber or in the reaction chamber. Preferably, the gases are mixed prior to introduction into the chamber to provide a uniform concentration of the entrained gases.

[0089] In another option, vapor of the oxygen and iodine containing compound may be introduced into the chamber independently of other gases, such as when two or more gases react or are easier to deliver independently.

[0090] In another alternative, the etching gas, i.e., vapor of an etching compound containing oxygen and iodine, and the inert gas, are the only two gases used during the etching process.

[0091] Exemplary other gases include, but are not limited to, oxidizers such as O2, O3, CO, CO2, NO, N2O, NO2, H2O, H2O2, COS, SO2, and combinations thereof. The disclosed oxygen and iodine containing etching gases and oxidizers may be mixed together prior to being introduced into the reaction chamber.

[0092] Alternatively, the oxidizer can be continuously introduced into the chamber and the etching gas intermittently introduced into the chamber. The oxidizer may comprise from about 0.01% v / v to about 99.99% v / v of the mixture introduced into the chamber (99.99% v / v represents the introduction of nearly pure oxidizer for the continuous introduction option).

[0093] Other exemplary gases with which the disclosed oxygen and iodine containing etching compounds may be used include cC4F8, C4F8, cC5F8, C5F8, C4F6, CF4, CH3F, CF3H, CH2F2, C3HF7, C3F6, C3H2F6, C3H2F4, C3H3F5, C4HF7, C5HF9, C3F6, C3F8, CF3I, C2F3I, C2F5I, C3F7I, 1-iodoheptafluoropropane (1-C3F7I), 2-iodoheptafluoropropane (2-C3F7I), C4F9I, C3HF7, COS, FNO, FC≡N, CS2, SO2, SF6, trans-1, Examples of suitable etchants include 1,1,4,4,4-hexafluoro-2-butene (trans-C4H2F6), cis-1,1,1,4,4,4-hexafluoro-2-butene (cis-C4H2F6), hexafluoroisobutene (C4H2F6), trans-1,1,2,2,3,4-hexafluorocyclobutane (trans-C4H2F6), 1,1,2,2,3-pentafluorocyclobutane (C4H3F5), 1,1,2,2-tetrafluorocyclobutane (C4H4F4), and cis-1,1,2,2,3,4-hexafluorocyclobutane (cis-C4H2F6), or combinations thereof. For example, etching compounds containing about 1% v / v to about 25% v / v of the disclosed oxygen and iodine may be used, with the remainder being C4F6 or cC4F8. As shown in the examples below, the combination of the disclosed oxygen- and iodine-containing etching compounds with conventional etching gases can result in increased etch rates while maintaining higher selectivity between the substrate and the layer being etched in conjunction with the disclosed oxygen- and iodine-containing etching compounds.

[0094] Vapor of the disclosed oxygen and iodine containing etching compound and the etching gas may be mixed prior to introduction into the reaction chamber, and the additional etching gas may comprise from about 0.01% v / v to about 99.99% v / v of the mixture introduced into the chamber.

[0095] In one non-limiting plasma etching process, vapors of the disclosed oxygen and iodine-containing compounds, such as C4F9IO, are introduced into a 200 mm dual CCP plasma etching tool using a controlled gas flow device. The controlled gas flow device can be a mass flow controller or bubbler design with inert gas flow to deliver the vapor of the desired molecule. For high boiling point molecules, a special low pressure loss mass flow controller from Brooks Automation (No. GF120XSD), MKS Instruments, etc. can be used. The pressure of the reaction chamber is set to about 30 mTorr. If the vapor pressure is sufficient, heating of the gas source may not be required. The distance between the two CCP electrodes is kept at 1.35 cm, and the top electrode RF power is fixed at 750 W. The bottom electrode RF power is changed to analyze the performance of the molecule. The reaction chamber contains a substrate having a silicon-containing film thereon, similar to that shown in FIG. 1a. The anti-reflective coating layer 108 is patterned / etched by fluorocarbons (e.g., CF4 and CH2F2) and oxygen-containing gases (e.g., O2). The amorphous carbon mask layer 106 is patterned / etched by oxygen-containing gases. The SiO and SiN layers 104 are patterned by a plasma of the disclosed oxygen and iodine-containing etching compounds (e.g., C4F9IO) and argon. Argon is independently introduced into the chamber at a flow rate of 250 sccm. C4F9IO is independently introduced into the chamber at 15 sccm. O2 is independently introduced into the chamber and varied from 0 sccm to 20 sccm to determine the optimal etching conditions. Apertures with aspect ratios of 10:1, preferably 50:1 or more are fabricated, which can be used as channel holes or contact holes or step etching, slit etching in 3D NAND and DRAM. Similar examples may be used for other stack layers as shown in FIG. 2 and FIG. 3a.

[0096] In another non-limiting exemplary plasma etching process, C4F9IO is introduced into a 200 mm dual CCP plasma etching tool using a controlled gas flow device. The controlled gas flow device can be a mass flow controller. For high boiling point molecules, a special low pressure loss mass flow controller from Brooks Automation (No. GF120XSD), MKS Instruments, etc. can be used. The pressure of the reaction chamber is set to about 30 mTorr. If the vapor pressure is sufficient, heating of the gas source may not be required. The distance between the two CCP electrodes is kept at 1.35 cm, and the top electrode RF power is fixed at 750 W. The bottom electrode RF power is changed to analyze the performance of C4F9IO. The reaction chamber contains a substrate 100 having a thick SiO layer 104a thereon, similar to the layer shown in FIG. 2. Prior to this process, the anti-reflective coating layer 108 is removed by a fluorocarbon (e.g., CF4) and an oxygen-containing gas (e.g., O2), and the aC mask layer 106 is removed by an oxygen-containing gas. Argon is independently introduced into the chamber at a 250 sccm flow rate. C4F9IO is independently introduced into the chamber at 15 sccm. O2 is independently introduced into the chamber at 0 sccm to 20 sccm to determine the optimal etching conditions. An aperture with an aspect ratio of 10:1 or more is created, which can be used as a contact hole in a DRAM. Similar examples may be used for other stack layers such as those shown in Figures 1a and 3a.

[0097] The silicon-containing film and the activated etching gas containing oxygen and iodine react to form volatile by-products that are removed from the reaction chamber. The aC mask, anti-reflective coating and photoresist layer are not very reactive to the activated etching gas. Therefore, the activated etching gas selectively reacts with the silicon-containing film to form volatile by-products.

[0098] The temperature and pressure in the reaction chamber are maintained at suitable conditions for the silicon-containing film to react with the activated etching gas. For example, the pressure in the chamber can be maintained at about 0.1 mTorr to about 1000 Torr, preferably about 1 mTorr to about 10 Torr, more preferably about 10 mTorr to about 1 Torr, more preferably about 10 mTorr to about 100 mTorr, as required by the etching parameters. Similarly, the substrate temperature in the chamber can range from about -196°C to about 500°C, preferably about -120°C to about 300°C, more preferably about -100°C to about 50°C, and more preferably about -10°C to about 40°C. The chamber wall temperature can range from about -196°C to about 300°C, depending on the process requirements.

[0099] The reaction between the silicon-containing film and the activated etching gas results in anisotropic removal of the silicon-containing film from the substrate. Nitrogen, oxygen and / or carbon atoms may also be present in the silicon-containing film. Removal may be due to physical sputtering of the silicon-containing film from the plasma ions (enhanced by the plasma) and / or removal of Si by sputtering with SiF, where x is in the range of 1 to 4. x By chemical reaction of the plasma species to convert them into volatile species such as

[0100] The plasma activated vapor of the disclosed oxygen and iodine containing etching compound preferably exhibits high selectivity to the mask and etches through alternating layers of SiO and SiN, resulting in a vertical etch profile without distortion or roughness. This is important for 3D NAND applications. In addition, the plasma activated vapor deposits polymer on the sidewalls, minimizing feature profile deformation. For other applications such as DRAM and 2D NAND, for example, plasma activated etch gases under different process conditions can selectively etch SiO from SiN. The plasma activated etch gases can selectively etch SiO and / or SiN from mask layers such as aC, photoresist, p-Si, or silicon carbide; or from metal contact layers such as Cu, W, Ru; or from channel regions made of SiGe or polysilicon regions.

[0101] The disclosed etching process uses the disclosed oxygen and iodine containing etching compounds to create channel holes, gate trenches, stepped contacts, capacitor holes, contact holes, contact etch, slit etch, self-aligned contacts, self-aligned vias, supervias, etc. in silicon-containing films. The resulting apertures can have aspect ratios ranging from about 10:1 to about 200:1 and diameters ranging from about 5 nm to about 500 nm, preferably less than 100 nm. For example, one skilled in the art will recognize that a channel hole etch creates apertures in silicon-containing films with aspect ratios greater than 50:1.

[0102] A typical material that needs to be etched may be SiO. The process of etching SiO may involve etching trenches in borophosphosilicate glass (BPSG), tetraethylorthosilicate (TEOS), or low deposition rate TEOS (LDTEOS), which are thermal oxides produced by wet or dry processes. The etch stop layer may be silicon nitride or silicon nitride oxygen (SiON) or polysilicon. The mask material used may be aC, p-Si, or photoresist material. The oxygen and iodine containing etching compounds disclosed herein are used to etch SiO, SiN, p-Si, and / or aC substrate films.

[0103] As shown in the examples below, evaluation of dry etching of SiO, SiN, p-Si and aC films using the disclosed oxygen and iodine containing etching compounds shows that HFCs containing oxygen and iodine provide the highest selectivity of silicon oxide over amorphous carbon, silicon nitride and p-Si compared to prior art fluorocarbons. The reason for the high selectivity is believed to be due to the formation of low F / C iodine containing fragments during plasma dissociation of the etching gas, which form a protective polymer film on the substrate. In addition, iodine is ionized and bombards the surface with heavy iodine ions similar to inert gases such as Ar, Kr and Xe. The ionized iodine atoms also modify the surface of the organic hardmask by doping it and improving the etch resistance of the organic hardmask in favor of high aspect ratio etching. Activated oxygen and iodine containing etching compounds generate iodine ions that strengthen the patterned mask layer, thereby reinforcing the patterned mask layer and minimizing damage while forming patterned structures on the substrate. The results of the etching gas shown herein are not only expected for patterned structure etching processes such as contact etching processes, but also show that it may be beneficial for other etching processes on silicon or metal-containing substrates, including low-k etching processes. In addition, in the process of forming patterned structures by etching with the disclosed oxygen- and iodine-containing etching compounds, the surface of the patterned mask layer can be doped with iodine to modify the surface, thereby increasing the etching resistance of the patterned mask layer. In this case, iodine ions from the activated oxygen- and iodine-containing etching compounds are implanted into the patterned mask layer (i.e., the surface and / or body / bulk of the patterned mask layer) while etching the silicon-containing film from the substrate to form the patterned structure. In addition, the disclosed oxygen- and iodine-containing etching compounds are suitable for reducing the global warming potential caused by perfluorocarbon compounds.

[0104] By adjusting the process parameters, the iodine doping concentration can be increased from 0.1 to 99.9% throughout the deposited film, depending on the application.

[0105] The iodine atomic concentration in the substrate material ranges from about 0.1% to about 99.9%, and is a uniform concentration throughout the deposited film.

[0106] The iodine atomic concentration in the substrate material ranges from about 1% to about 50%, and is a uniform concentration throughout the deposited film.

[0107] The iodine atomic concentration in the substrate material ranges from about 2% to about 30%, and is a uniform concentration throughout the deposited film.

[0108] Furthermore, the oxygen in the activated etching compound containing oxygen and iodine can dope the aC mask layer. The oxygen in the activated etching compound containing oxygen and iodine can also reduce or eliminate the use of oxidizing agents. In some embodiments, no oxidizing agent can be introduced. In some embodiments, little oxidizing agent can be used. As mentioned above, oxidizing agents remove the deposited polymer, but can distort the etched structure. With the disclosed etching compound containing oxygen and iodine, little or no oxidizing agent can be applied, so that the etched structure maintains a linear profile. Furthermore, the oxygen in the activated etching compound containing oxygen and iodine can help to incorporate more iodine-containing ions, radicals and species into the mask layer, such as the carbon-containing layer. In addition, the oxygen in the activated etching compound containing oxygen and iodine can also help to increase the etching rate of the silicon-containing layer. EXAMPLES

[0109] The following non-limiting examples are provided to further illustrate embodiments of the present invention, however, the examples are not intended to be comprehensive and are not intended to limit the scope of the invention described herein.

[0110] In the following examples, experiments were performed using a commercial LAM tool 4520XLe 200 mm (CCP dual frequency plasma) or a commercial AMEC 300 mm Primo SSC HD-RIE etcher. Flat wafers were purchased from Advantive Tech. The flat wafers tested were four different substrates:

[0111] Experiments were performed at the Air Liquide R&D Innovation Campus Delaware using a commercial LAM tool 4520XLe 200 mm (CCP dual frequency plasma, 10 gas lines). Flat wafers were purchased from Advantive Tech. The flat wafers tested were: ·2um PECVD TEOS on Si substrate; ·2um PECVD Si3N4 on Si substrate; 300 nm LP-CVD poly-Si on Si substrate; and · 350nm PE-CVD aC on Si substrate.

[0112] In planar tests, the etch rate and selectivity were evaluated through ellipsometry and SEM at different O2 flow rates by measuring the change in etch thickness as a function of etch time. The process test molecule gas flow rate was kept constant at 15 sccm, Ar flow rate at 250 sccm, while O2 flow rates were screened from 0 to 20 sccm. The polymer composition was then investigated by X-ray photoelectron spectroscopy.

[0113] The etching experiments were carried out on four 1.5 × 1.5 cm 3D wafers with four different substrate materials including SiO2, Si3N4, p-Si, and aC. 2This was done on a flat coupon of 200 mm diameter. The coupon is placed on a 200 mm diameter carrier wafer and held in contact using silicone oil or thermal paste. Alternatively, double-sided carbon tape from SPI supplies can be used to attach the coupon onto the carrier wafer.

[0114] Etching tests were performed at a pressure of 30 mTorr and a source power of 750 W (27 MHz), a bias power of 1500 W (2 MHz), and a temperature of 20° C. The feed mixture contained 250 sccm Ar and 15 sccm etch gas, while O2 was varied from 0 to 20 sccm.

[0115] To demonstrate reproducibility, each etching test was repeated at least three times. The standard deviation of the average of the triplicate measurements is shown as the error bar in the chart. The composition of the polymer was then examined by X-ray photoelectron spectroscopy (XPS).

[0116] Example 1 Plasma-enhanced dry etching using C3F7IO [ka] C3F7IO, 2-iodo-1,1,2,2-tetrafluoro-1-(trifluoromethoxy)ethane, was applied to plasma etching of silicon oxide SiO2.

[0117] [Table 3]

[0118] Figure 4 shows the etch rate (ER) and selectivity of C3F7IO for four different substrates, namely SiO, SiN, p-Si, and aC, at different O2 flow rates (0-20 sccm). The ER of SiO2 and aC are inversely proportional: the ER of SiO2 increases and the ER of aC decreases with decreasing O2 flow rate. It is shown that the highest SiO2 / aC selectivity is about 17:1 at O2=0 sccm, with the ER of SiO2 being about 535 nm min. Table 4 shows a comparison with the standard etching gas C4F6, which is a benchmark commonly used in the industry. C3F7IO shows about 70% higher SiO2 / aC selectivity than the benchmark gas (C4F6) at similar etch rates. Of note are the differences in the carbon number of the two molecules (C3 vs. C4) and the F / C ratio of the two etching compounds: C3F7IO has an F / C ratio=2.33 and C4F6 has an F / C ratio=1.5. Generally, according to the literature, the higher the F / C ratio, the lower the selectivity due to the lower number of carbon atoms forming polymers to protect the pattern mask. However, C3F7IO shows high selectivity even with a low carbon number due to the presence of elements containing iodine and oxygen in the etching compound. Figure 8 shows the etch rates of SiO, SiN, p-Si and aC using C4F6.

[0119] [Table 4]

[0120] XPS Data Analysis: To simulate the formation of a polymer layer on the top surface and sidewalls during the plasma etching process, the process conditions were adjusted: aC and Si bare coupons were etched at 30 mTorr for 60 seconds with a power supply of 750 W (27 MHz) and no bias power at the substrate (0 W, 2 MHz). The process was delivered with a mixture containing 125 sccm Ar and 30 sccm C3F7IO, no O2, as described in Table 5. Due to the lack of bias power, the ions that reach the substrate may not have enough energy to etch the substrate. Additionally, neutral and activated species that reach the substrate surface will attach to the surface based on their sticking coefficients, resulting in the deposition of a thin polymer layer on top. This thin polymer layer can contribute to sidewall passivation and often provides selectivity.

[0121] [Table 5]

[0122] For XPS depth profiling, monoatomic Ar was used to minimize chemical damage and to avoid possible knock-on of iodine atoms during Ar sputtering, which can occur during sputtering of organic materials such as fluorocarbon polymers and amorphous carbon. + Instead, we used Ar1000, a large cluster ion gas with an ion energy of 5 keV. + was used. Figure 5a shows the depth profile on the aC substrate. Figure 5b shows a magnified view of Figure 3a without C1s. Table 6 shows the XPS results of etching carbon-containing substrates using C3F7IO.

[0123] [Table 6]

[0124] [Table 7]

[0125] Fluorocarbon compounds containing oxygen and iodine exhibit interesting behavior during etching of carbon-containing masks compared to Si-containing materials. XPS data show that iodine modifies the carbon surface and penetrates deeper into the aC mask, similar to a doping effect, helping to protect the hardmask layer during etching. Table 7 shows the XPS results of etching silicon-containing substrates using C3F7IO. On Si substrates, the structure C x F y I z O k A thin polymer layer with iodine is observed superficially, but after an etching time of about 20 seconds the iodine content drops to zero. Meanwhile, in the aC layer iodine can be seen deeper and at a lower percentage (<2%). Also, oxygen from C3F7IO is incorporated in the bulk of the aC mask layer at a percentage of 2-3%. By adjusting the process parameters, the iodine doping concentration can be increased from 0.1 to 99.9% throughout the deposited film, depending on the application.

[0126] Comparing the F1s and I3d peaks in the XPS shown in Table 5, the depth profile on the aC substrate (in Figure 7, the y-axis shows counts per second and the x-axis shows binding energy (eV)) is: Fluorine is deposited on the surface to form a thin IFC (iodo-fluorocarbon) polymer (F1s is Ar etching for up to 120 seconds), Iodine penetrates deeper into aC mask (I3d etches up to 500 seconds) This shows that.

[0127] Thus, the iodine and oxygen species help protect the aC mask during etching by modifying the surface and doping the aC layer with iodine. The iodine also strengthens the aC mask, thereby minimizing damage. Additionally, the oxygen-containing species help retain and incorporate a higher percentage of iodine into the patterned mask, improving the etch resistance of the patterned mask.

[0128] Each etching test was repeated three times to demonstrate reproducibility. The standard deviation of the average of the triplicate measurements is shown as an error bar in FIG. 4. The subject matter described herein may be described in the context of example implementations for processing one or more computing application functions / operations for a computing application having a user-interactive component, although the subject matter is not limited to these particular embodiments. Rather, the techniques described herein may be applied to any suitable type of user-interactive component execution management method, system, platform, and / or apparatus.

[0129] It will be understood that many additional changes in the details, materials, steps, and arrangements of parts described and illustrated herein to explain the nature of the invention may be made by those skilled in the art within the principles and scope of the invention as set forth in the appended claims. Accordingly, it is not intended that the invention be limited to the specific embodiments in the examples given above and / or in the accompanying drawings.

[0130] Although embodiments of the present invention have been shown and described, they may be modified by those skilled in the art without departing from the spirit and teachings of the present invention. The embodiments described herein are merely exemplary and not limiting. Many variations and modifications of the compositions and methods are possible and are within the scope of the present invention. Thus, the scope of protection is not limited to the embodiments described herein, but only by the claims, including all equivalents of the subject matter of the claims.

Claims

1. 1. A method of forming a patterned structure, comprising: a) introducing into a reaction chamber containing a substrate having a silicon-containing film deposited thereon and a patterned mask layer deposited on the silicon-containing layer, n H x F y I z O e introducing vapor of an etching compound containing oxygen and iodine having the formula: where 0≦n≦10, 0≦x≦21, 0≦y≦21, 1≦z≦4, and 1≦e≦2; b) activating the plasma to produce an activated etching compound containing oxygen and iodine; and c) allowing an etching reaction to proceed between the activated oxygen and iodine containing etching compound and the silicon-containing film to selectively etch the silicon-containing film from the patterned mask layer, thereby forming the patterned structure; The method includes:

2. 2. The method of claim 1, wherein step c) comprises modifying or doping the patterned mask layer with iodine from iodine ions generated from the activated oxygen and iodine containing etching compound.

3. The method further includes the step of introducing an inert gas into the reaction chamber, the inert gas being selected from the group consisting of He, Ar, Xe, Kr, Ne, and N. 2 The method of claim 1 , wherein the compound is selected from the group consisting of:

4. O 2 , O 3 , CO, CO 2 , NO, N 2 O, NO 2 , H 2 O, H 2 O 2 , COS, SO 2 10. The method of claim 1, optionally further comprising introducing an oxidizing agent selected from the group consisting of:

5. The etching compound containing oxygen and iodine is C 3 F 7 10. The method of claim 1, wherein the aryl group is 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 3

6. The silicon-containing film may be silicon oxide (SiO), silicon nitride (SiN), crystalline Si, polysilicon (p-Si), polycrystalline silicon, amorphous silicon, low dielectric constant SiCOH, SiOCN, SiC, SiON, Si a O b H c C d N e 2. The method of claim 1 , comprising alternating layers of SiO and SiN (ONON), or alternating layers of SiO and p-Si (OPOP), where a>0; and b, c, d, and e>0.

7. 7. The method of claim 1, wherein the oxygen and iodine containing etching compound plasma etches alternating layers of SiO and SiN (ONON) with a selectivity of about 1:2 to about 2:1 for SiO layers versus SiN layers.

8. 7. The method of any one of claims 1 to 6, wherein the oxygen and iodine containing etching compound plasma etches alternating layers of SiO and p-Si (OPOP) with a selectivity of about 1:2 to about 2:1 for SiO layers versus p-Si layers.

9. 7. The method of any one of claims 1 to 6, wherein the patterned mask layer is a carbon-containing layer, an amorphous carbon layer, a doped amorphous carbon layer, a photoresist layer, an anti-reflective layer, an organic planarization layer, or a combination thereof.

10. and introducing an additional etching gas into the reaction chamber, the additional etching gas being cC 4 F 8 , C 4 F 8 , cC 5 F 8 , C 5 F 8 , C 4 F 6 , C.F. 4 , C.H. 3 F, C.F. 3 H, C.H. 2 F 2 , C 3 H.F. 7 , C 3 F 6 , C 3 H 2 F 6 , C 3 H 2 F 4 , C 3 H 3 F 5 , C 4 H.F. 7 , C 5 H.F. 9 , C 3 F 6 , C 3 F 8 , C.F. 3 I.C. 2 F 3 I.C. 2 F 5 I.C. 3 F 7 I, 1-iodoheptafluoropropane (1-C 3 F 7 I), 2-iodoheptafluoropropane (2-C 3 F 7 I), C4F9I, C 3 H.F. 7 , COS, FNO, FC≡N, CS 2 , S.O. 2 , S.F. 6 , trans-1,1,1,4,4,4-hexafluoro-2-butene (trans-C 4 H 2 F 6 ), cis-1,1,1,4,4,4-hexafluoro-2-butene (cis-C 4 H 2 F 6 ), hexafluoroisobutene (C 4 H 2 F 6 ), trans-1,1,2,2,3,4-hexafluorocyclobutane (trans-C 4 H 2 F 6 ), 1,1,2,2,3-pentafluorocyclobutane (C 4 H 3 F 5 ), 1,1,2,2-tetrafluorocyclobutane (C 4 H 4 F 4 ), and cis-1,1,2,2,3,4-hexafluorocyclobutane (cis-C 4 H 2 F 6 7. The method of claim 1, wherein the compound is selected from the group consisting of:

11. 7. The method of claim 1, wherein the patterned features formed in the silicon-containing film have an aspect ratio of about 1:1 to about 200:

1.

12. 1. A method of forming a patterned structure, comprising: a) introducing C into a reaction chamber containing a substrate having a silicon-containing film deposited thereon and a patterned mask layer deposited on the silicon-containing layer; 3 F 7 introducing vapor of IO; b) Activating the plasma to generate activated C 3 F 7 generating an IO; and c) the activated C 3 F 7 allowing an etching reaction to proceed between an IO and the silicon-containing film to selectively etch the silicon-containing film from the patterned mask layer, thereby forming the patterned structure; The method includes:

13. The step c) The activated C 3 F 7 modifying the patterned mask layer by doping the patterned mask layer with iodine from iodine ions generated from IO. The method of claim 12, comprising:

14. 1. A method for modifying a surface of a substrate, comprising the steps of: A reaction chamber containing a substrate having a silicon-containing film deposited thereon and a patterned mask layer deposited on the silicon-containing layer, the reaction chamber being provided with a compound of formula C. n H x F y I z O e introducing vapor of an etching compound containing oxygen and iodine having the formula: where 4≦n≦10, 0≦x≦21, 0≦y≦21, 1≦z≦4, and 1≦e≦2; Etching the silicon-containing film through the patterned mask layer using an activated etching compound containing oxygen and iodine formed by activating a plasma to form a patterned structure; Including; wherein iodine from iodine ions generated from the activated oxygen and iodine containing etching compound is doped into a patterned hard mask layer during formation of the patterned structures on the substrate, thereby strengthening the patterned mask layer and minimizing damage to the patterned mask.

15. The etching compound containing oxygen and iodine is C 3 F 7 15. The method of claim 14, wherein said aryloxycarbonyl group is 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29

Citation Information

Patent Citations

  • Dry etching

    JP1993326460A

  • Dry etching method

    JP1995335624A

  • Method of decomposing fluoride compound

    JP2004249285A

  • Manufacturing method of semiconductor device and apparatus thereof

    JP2005072518A

  • Iodine-containing compounds for etching semiconductor structures

    JP2020515047A