Fluoropolymer and Cyclic Olefin Alloys
Fluoropolymer alloys with cyclic olefin copolymers, facilitated by compatibilizers, address the challenges of high-frequency electronics by enhancing mechanical and electrical properties, enabling efficient wireless communication.
Patent Information
- Application Number
- JP2024535667
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-14
- Filing Date
- 2022-12-14
- Publication Date
- 2024-12-05
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing materials used in high-frequency electronics, such as epoxy, polyimide, LCPs, and fluoropolymers, face challenges in achieving high frequency capabilities, processing difficulties, and adhesion issues, while linear polyolefins cannot withstand soldering processes required for electronic circuit manufacturing.
Development of fluoropolymer alloys using cyclic olefin copolymers (COCs) facilitated by compatibilizers, formed through a reaction mixture of functional fluoropolymers, reactive monomers, and cyclic olefins, which enhance electrical, thermal, and mechanical properties.
The resulting alloys exhibit improved mechanical and electrical properties suitable for high-frequency electronics, enabling wireless communication at 1 GHz or higher and overcoming previous material limitations.
Smart Images

Figure 2024545229000021 
Figure 2024545229000022 
Figure 2024545229000023
Abstract
Description
[Technical field]
[0001] FIELD OF THE DISCLOSURE This disclosure relates generally to fluoropolymer alloy compositions for use in applications such as high frequency electronics. In addition to such fluoropolymer alloy compositions, a compatibilizer for use therewith is provided. [Background technology]
[0002] Materials are needed in the field of high frequency electronics for the "fifth generation of communication" (5G). These materials must be able to transmit information and process at higher frequencies. Materials such as epoxy and polyimide have been used for low frequency applications, but these materials could not overcome the stringent requirements to easily achieve the high frequency range required for 5G applications. Other materials such as liquid crystal polymers (LCPs) and fluoropolymers also have difficulties in processing and adhesion. Linear polyolefins have excellent electrical properties, but cannot withstand processes such as soldering to manufacture electronic circuits, which require temperatures above 200°C.
[0003] Thus, there is a need in the art for materials that have suitable electrical, thermal, and mechanical properties for use in high frequency electronic applications. Summary of the Invention
[0004] The present invention described below addresses the above-mentioned problems and others, but it should be noted that not all embodiments of the present invention described herein address each of the above-mentioned problems. The present disclosure provides a compatibilizer that facilitates alloying fluoropolymers with cyclic olefin copolymers (COCs). In some embodiments, alloys containing such compatibilizers have good electrical, thermal, and mechanical properties, making them useful in high frequency electronic devices.
[0005] A first aspect provides a reaction mixture for making a compatibilizer, the reaction mixture comprising: a first functional fluoropolymer; a first COC; a first reactive monomer; and a second reactive monomer.
[0006] A second aspect provides a method of making a compatibilizer for alloying a fluoropolymer with a cyclic olefin, comprising heating the reaction mixture of the first aspect such that at least the first fluoropolymer and the first COC melt.
[0007] A third aspect provides a method of making a compatibilizer for alloying fluoropolymers with cyclic olefins, comprising the steps of reacting an anhydride monomer with a first functional fluoropolymer to form a fluoropolymer dianhydride; and reacting the fluoropolymer dianhydride with functional COC and diamine monomers to form the compatibilizer.
[0008] A fourth aspect provides a reactive polymeric compatibilizer that is the product of the above process according to the second aspect.
[0009] A fifth aspect provides a reactive polymeric compatibilizer that is the product of the above process according to the third aspect.
[0010] A sixth embodiment provides a reactive polymeric compatibilizer comprising a COC group covalently bonded to at least one heterodimeric binding polymer comprising a dianhydride monomer and a diamine monomer, said binding polymer being covalently bonded to a fluoropolymer group.
[0011] A seventh aspect provides a thermoplastic polymer alloy composition comprising: a second fluoropolymer; a compatibilizer; and a second COC.
[0012] An eighth aspect provides a method of forming an alloy of a fluoropolymer and a COC, the method comprising blending a second fluoropolymer, a compatibilizer, and a second cyclic olefin at a temperature such that at least the first fluoropolymer and the first COC are melted.
[0013] A ninth aspect provides an alloy of fluoropolymer and COC that is the product of the process according to the eighth aspect.
[0014] A tenth aspect provides an electronic article capable of wireless communication at or above 1 GHz, comprising a polymer alloy of a fluoropolymer and a cyclic olefin.
[0015] The above summary presents a simplified overview in order to provide a basic understanding of some aspects of the claimed subject matter. This summary is not an extensive overview. It is not intended to identify key or critical elements or to delineate the scope of the claimed subject matter. It is merely intended to present some concepts in a simplified form as a prelude to the more detailed description that is presented below. [Brief description of the drawings]
[0016] [Figure 1] 1 illustrates a scheme for reactively combining a dianhydride monomer, an aromatic diamine, and a PFA having end groups to produce a compatibilizer according to one embodiment. [Diagram 2] 1 illustrates another scheme for producing a compatibilizer in two steps according to one embodiment. [Diagram 3] This represents the final step of the scheme depicted in FIG. [Figure 4] 3 illustrates an alternative final step in the scheme depicted in FIG. 2. [Diagram 5] FIG. 1 illustrates the FTIR characteristics of grafted COC according to one embodiment. [Figure 6] A close-up of FIG. 5 shows the C═O from cyclic anhydrides, showing that increasing the dianhydride increases grafting. [Figure 7]1 is a graph depicting the tensile modulus of compositions according to various embodiments. [Figure 8] 1 is a graph depicting the tensile strength of compositions according to various embodiments. [Figure 9] 1 is a graph depicting elongation of compositions according to various embodiments. [Figure 10] 1 is a graph depicting flexural strength of compositions according to various embodiments. [Figure 11] 1 is a graph depicting flexural modulus of compositions according to various embodiments. [Figure 12] 1 is a graph depicting the % weight loss temperature of compositions according to various embodiments. [Figure 13] 1 is a graph depicting the coefficient of thermal expansion of compositions according to various embodiments. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] definition
[0018] Unless otherwise defined, all terms used herein (including technical and scientific terms) have the same meaning as commonly understood by those skilled in the art in the field of this disclosure. Furthermore, it should be understood that terms such as those defined in commonly used dictionaries should be interpreted as having a meaning consistent with the meaning in the context of the specification, and should not be interpreted in an idealized or overly formal sense unless expressly defined herein. For the sake of brevity and clarity, well-known functions and configurations are not described in detail.
[0019] Where the words "comprise", "comprises" or "comprising" are used in the above description and / or the following claims, unless the context otherwise requires, these terms should be construed as open-ended and not limiting, and each term is used with the understanding and express understanding that it is so interpreted in interpreting the above description and / or the following claims.
[0020] The term "consisting essentially of" means that the claimed subject matter may include, in addition to the recited elements, other elements (steps, structures, components, members, etc.) that do not adversely affect the operability of the claimed subject matter for its intended purpose. Such addition of other elements that do not adversely affect the operability of the claimed subject matter for its intended purpose is not believed to materially alter the basic and novel characteristics of the claimed subject matter.
[0021] A phrase such as "at least one of A and B" should be understood to mean "A only, B only, or both A and B." The same interpretation applies to longer lists (e.g., "at least one of A, B, and C").
[0022] The terms "about" and "approximately" generally refer to an acceptable degree of error or variation in a measured quantity, given the nature or precision of the measurement. Typical degrees of error or variation are, for example, within 20 percent (%), preferably within 10%, more preferably within 5%, and even more preferably within 1% of a given numerical value or numerical range. Unless otherwise stated, numerical values given in this specification are approximate. That is, the term "about" or "approximately" is to be inferred unless otherwise specified.
[0023] The terminology used herein is for the purpose of describing particular embodiments only and is not intended to be limiting. As used herein, the singular forms "a," "an," and "the" are intended to include the plural forms (i.e., "at least one") unless the context clearly dictates otherwise.
[0024] In this specification, terms such as "first" and "second" are used to describe various features or elements, but these features or elements should not be limited by these terms. These terms are used only to distinguish one feature or element from another feature or element. Thus, a first feature or element described below can be referred to as a second feature or element, and similarly, a second feature or element described below can be referred to as a first feature or element, without departing from the teachings of the present disclosure.
[0025] References are made in certain places to standard methodologies, including, but not limited to, measurement methods. It is understood that such standards are revised from time to time and, unless expressly stated otherwise, any reference in this disclosure to such standards shall be construed as referring to the most recently published standard at the time of filing.
[0026] It will be understood that any given element in the disclosed embodiments of the present invention may be realized as a single structure, a single step, or a single material, etc. Likewise, any given element in the disclosed embodiments may be realized as a plurality of structures, steps, or materials, etc.
[0027] Compatibilizer
[0028] Compatibilizers are disclosed, some of whose embodiments find use in making compatible blends of fluoropolymers and COCs. The compatibilizers have four basic functional groups: a fluoropolymer group, a COC group, a first monomer group, and a second monomer group.
[0029] A reaction mixture for making the compatibilizer is also disclosed. The reaction mixture has four components: a first functional fluoropolymer, a first COC, a first reactive monomer, and a second reactive monomer. The reaction mixture is intended to be further processed as described below. Processing results in covalent bonding of the components.
[0030] Cyclic olefin copolymers (COCs) are copolymers of cyclic monomers such as 8,9,10-trinorborn-2-ene (norbornene) or 1,2,3,4,4a,5,8,8a-octahydro-1,4:5,8-dimethanonaphthalene (tetracyclododecane) with ethene. Other cyclic hydrocarbon monomers can be used as well. These polymers have desirable optical properties and are resistant to moisture. They also have good dielectric properties for electronic applications. COCs generally have low dissipation factor and electrical conductivity. When COC resins are pelletized, they are suitable for many standard polymer processing techniques such as single and twin screw extrusion, injection molding, injection and stretch blow molding, compression molding, extrusion coating, biaxial orientation, and thermoforming. COCs are dimensionally stable and show little change after processing.
[0031] In some embodiments of the reaction mixture, the first COC comprises one or more of maleic anhydride, cis-4-cyclohexene-1,2-dicarboxylic anhydride; trans-1,2,3,6-tetrahydrophthalic acid; 5-methyl-3A,4,7,7A-tetrahydro-isobenzofuran-1,3-dione; endo-bicyclo[2.2.2]oct-5-ene-2,3-dicarboxylic anhydride; cis-5-norbornene-endo-2,3-dicarboxylic anhydride; bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic dianhydride; bicyclo[2.2.1]hept-5-ene-2,3-dicarboxylic anhydride; and 5-(2,5-dioxotetrahydrofuryl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride.
[0032] Suitable COCs for use in the reaction mixture include those sold under the trade name COC TOPAS 6017s (TOPAS Advanced Polymers, Raunheim, Germany). COC TOPAS 6017s is an ethylene-norbornene copolymer (CAS 26007-43-2). COC TOPAS 6017s has the following properties listed on the manufacturer's technical data sheet: [Table 1]
[0033] The reaction mixture may include functionalized COC or non-functionalized COC. The functionalized COC includes a functional group. The functional group participates in a reaction with one or more other components. As used herein, "functional group" refers to any reactive group capable of forming a chemical bond with the COC, such as by covalent, hydrogen, or ionic bonding. Suitable functional groups include carboxyl, amine, anhydride, hydroxyl, epoxy, sulfhydryl, siloxane, and oxazoline. In some embodiments, the functionalized COC may have multiple functional groups, including a combination of one or more of carboxyl, amine, anhydride, hydroxyl, epoxy, sulfhydryl, siloxane, and oxazoline.
[0034] In some embodiments of the reaction mixture, the first functionalized COC is an anhydride. Anhydrides are advantageous in that they react with alcohols to form esters and with amines to form amides. The functionalized COC may be a dianhydride (i.e., have two anhydride groups). Dianhydrides are advantageous in that they provide more reactive functional groups. In some embodiments of the reaction mixture, the second monomer is a dicarboxylic acid anhydride. The COC anhydride may be a fluorinated anhydride, such as 4,4'-(hexafluoroisopropylidene)diphthalic anhydride (6FDA). In some embodiments of the reaction, the anhydride is an unsaturated cyclic dianhydride. In one specific embodiment, the functionalized first COC is the reaction product of bicyclo[2.2.1]hept-5-ene-2,3-dicarboxylic anhydride (BCDA) and COC. In a more specific embodiment, the functionalized first COC is the reaction product of BCDA and TOPAS 6017s. In another specific embodiment, the functionalized first COC is the reaction product of BCDA and TOPAS 6015s.
[0035] The functionalized first COC can be prepared in various ways. For example, an anhydride can be grafted onto a COC catalyzed by peroxide catalysis. Suitable peroxide catalysts include dialkyl peroxides. In some embodiments, especially when non-functionalized COC is included in the first COC fraction, the reaction mixture includes a peroxide catalyst capable of catalyzing the functionalization of the first COC with an anhydride. In other embodiments, the COC can be functionalized before being mixed with other components of the reaction mixture.
[0036] In some embodiments of the reaction mixture, the first monomer is an amine. Amine monomers have several advantages, one of which is that amines can react with anhydrides to form amides. In another embodiment, the first monomer is a diamine, which has the advantage of multiple reactive amine groups. In one specific embodiment of the reaction mixture, the first monomer is a dianiline, such as 4,4'-oxydianiline.
[0037] In some embodiments of the reaction mixture, the first monomer is present at 0.1-25 wt%. In some embodiments of the reaction mixture, the first monomer is present at 0.5-10 wt%. In other embodiments of the reaction mixture, the first monomer is present at 0.6-5.0, 0.7-4.0, 0.8-3.0, 0.9-2.5, 1.0-2.4, 1.1-2.3, 1.2-2.2, 1.3-2.1, 1.4-2.0, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, and 2.0 wt%. In one specific embodiment, the first monomer is present at 1.45 wt%. In another specific embodiment, the first monomer is present at 2.0 wt%.
[0038] In some embodiments of the reaction mixture, the second monomer is an anhydride. Anhydrides have the advantages described above for the functionalized first COC in the second monomer, and the anhydrides disclosed as suitable for functionalizing the first COC are also suitable as the second monomer. In one specific embodiment, the second monomer is BCDA. In another specific embodiment, the second monomer is 6FDA. In another specific embodiment, the second monomer is present as BCDA and 6FDA.
[0039] In some embodiments of the reaction mixture, the second monomer is present at 1-25 wt%. In some embodiments of the reaction mixture, the second monomer is present at 1.1-20, 1.2-10, 1.3-9, 1.4-8, 1.5-7, 1.6-6, 1.7-5, 1.8-4.5, 1.9-4, 2.0-3.6, 2.1-3.5, 2.2-3.4, 2.3-3.3, 2.4-3.2, or 2.5-3.1 wt%. In specific embodiments of the reaction mixture, the second monomer is present at 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, or 3.1 wt%.
[0040] In some cases, the first and second monomers may be present in a similar molar ratio. In some embodiments of the reaction mixture, the first and second monomers are present in a molar ratio of 0.5 to 2.0. In other embodiments of the reaction mixture, the first and second monomers are present in a molar ratio of 0.6 to 1.8, 0.7 to 1.6, 0.8 to 1.4, or 0.9 to 1.2. In one specific embodiment, the first and second monomers are present in a molar ratio of 1. The reaction mixture may also include a monomer fraction that includes the first and second monomers (and optionally other monomers of the same nature). In some embodiments of the reaction mixture, the monomer fraction comprises no more than 5% by weight of the mixture. In other embodiments of the reaction mixture, the monomer fraction comprises 4 to 5, 4.1 to 4.9, 4.2 to 4.8, 4.3 to 4.7, or 4.4 to 4.6% by weight of the mixture. In a specific embodiment of the reaction mixture, the monomer fraction comprises 4.5-4.6% by weight of the mixture.
[0041] Ideally, the first COC has mechanical and / or electrical properties suitable for high frequency electronics applications. In some embodiments of the reaction mixture, the first COC has a tensile strength of ≧25 MPa. In other embodiments of the reaction mixture, the first COC has a tensile strength of ≧30, 35, 40, 45, 50, 51, 52, and 53 MPa. In one specific embodiment of the reaction mixture, the first COC has a tensile strength of 54 MPa. In some embodiments of the reaction mixture, the first COC has a Young's modulus of ≧200 MPa. In other embodiments of the reaction mixture, the first COC has a Young's modulus of ≧250, 300, 350, 400, 450, 460, 470, and 480 MPa. In one specific embodiment of the reaction mixture, the first COC has a Young's modulus of 481. In some embodiments of the reaction mixture, the first COC has a flexural modulus of ≧1000 MPa. In another embodiment of the reaction mixture, the first COC has a flexural modulus of ≧1100, 1200, 1300, 1400, 1500, 1600, 1700, 1800, 1900, 2000, 2100, 2200, 2300, 2400, and 2500. In one specific embodiment of the reaction mixture, the first COC has a flexural modulus of 2530. In some embodiments of the reaction mixture, the first COC has a flexural strength of ≧50 MPa. In another embodiment of the reaction mixture, the first COC has a flexural strength of ≧55, 60, 65, 70, 71, 72, 73, 74, and 75 MPa. In one specific embodiment of the reaction mixture, the first COC has a flexural strength of 76 MPa. In some embodiments of the reaction mixture, the first COC has a flexural load of ≧50 N. In another embodiment of the reaction mixture, the first COC has a bending load of ≧60, 70, 80, 90, 100, 110, 120, 121, 122, 123, 124, and 125 N. In a specific embodiment of the reaction mixture, the first COC has a bending load of 126 N. In some embodiments of the reaction mixture, the first COC has a coefficient of thermal expansion of ≦100 μm / (m° C.). All of the above mechanical properties are measured according to the ATSM D638 and ASTM D790 standards.
[0042] In another embodiment of the reaction mixture, the first COC has a coefficient of thermal expansion (CTE) of ≦90, 80, 70, 60, 50, 49, 48, 47, 46, 45, 44, 43, 42, 41, and 40 μm / (m° C.). In one specific embodiment of the reaction mixture, the first COC has a coefficient of thermal expansion of 39 μm / (m° C.). In some embodiments of the reaction mixture, the first COC has a dielectric constant of ≧2.10. In another embodiment of the reaction mixture, the first COC has a dielectric constant of ≧2.15, 2.20, 2.25, 2.30, 2.31, 2.32, and 2.33. In one specific embodiment of the reaction mixture, the first COC has a dielectric constant of 2.335. In some embodiments of the reaction mixture, the first COC has a dissipation factor of ≦0.001. In another embodiment of the reaction mixture, the first COC has a dielectric loss tangent of ≦0.0009, 0.0008, 0.0007, 0.0006, 0.0005, 0.00049, 0.00048. In a specific embodiment of the reaction mixture, the first COC has a dielectric loss tangent of 0.00047. In some embodiments of the reaction mixture, the first COC has a 1% weight loss temperature of ≧350° C. In another embodiment of the reaction mixture, the first COC has a 1% weight loss temperature of ≧360, 370, 380, 390, 391, 392, and 393° C. In a specific embodiment of the reaction mixture, the first COC has a 1% weight loss temperature of 394° C. In some embodiments of the reaction mixture, the first COC has a 5% weight loss temperature of ≧400° C. In another embodiment of the reaction mixture, the first COC has a 5% weight loss temperature of ≧405, 410, 415, 416, and 417° C. In one specific embodiment of the reaction mixture, the first COC has a 5% weight loss temperature of 418° C. In some embodiments of the reaction mixture, the first COC has a melt flow rate at 297° C. of ≦200 (g / 10 min). In another embodiment of the reaction mixture, the first COC has a melt flow rate of ≦190, 180, 170, 160, 150, 140, 130, 120, 110, 109, 108, 107, 106, 105, 104, 103, 102, and 101 g / (10 min). In one specific embodiment of the reaction mixture, the first COC has a melt flow rate of 100.6 g / (10 min).Melt flow rates were measured using a Tinius Olsen Melt Indexer MP1200M (MFR) according to the following method. Whenever MFR is mentioned, it should be assumed that it refers to the MFR measured by this method unless otherwise specified. Approximately 5 g of material is charged into the barrel of the melt flow apparatus (preheated to 297°C). After 300 seconds, a 5 kg weight is added to the plunger, forcing the molten material out of the die. The extrudate is collected and weighed at regular intervals. Melt flow rate values are calculated in g / 10 min. Whenever CTE is mentioned, it should be assumed that it refers to the CTE measured by this method unless otherwise specified.
[0043] 1: Force 0.100N
[0044] 2: Equilibrate at 35.00℃
[0045] 3: Isothermal for 5.00 min
[0046] 4: marks the end of cycle 0
[0047] 5: Isothermal for 5.00 min
[0048] 6: Ramp 5.00°C / min to 100.00°C
[0049] 7: Isothermal for 3.00 min
[0050] 8: Marks the end of cycle 1
[0051] 9: Ramp 10.00°C / min to 0.00°C
[0052] 10: Marks the end of cycle 2
[0053] 11: Ramp 5.00°C / min to 200.00°C
[0054] 12: Completion of the method
[0055] In some embodiments of the reaction mixture, the first fluoropolymer is functionalized, such as by shearing, which creates reactive end groups, such as COF groups and carboxylic acid groups.
[0056] The first fluoropolymer in the reaction mixture preferably has good heat resistance, good dielectric properties, or both. In some embodiments of the reaction mixture, the first fluoropolymer is one or more of perfluoroalkoxyalkane (PFA), fluorinated ethylene propylene (FEP), polytetrafluoroethylene (PTFE), ethylene-tetrafluoroethylene (ETFE), polyvinylidene fluoride (PVDF), ethylene-tetrafluoroethylene-hexafluoropropylene terpolymer (EFEP), ethylene-chlorotrifluoroethylene (ECTFE), polychlorotrifluoroethylene (PCTFE), tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride terpolymer (THV), tetrafluoroethylene and vinylidene fluoride copolymer (VT), and any combination of the above.
[0057] The first fluoropolymer may be present in the reaction mixture at 1-99 wt%. The first fluoropolymer preferably constitutes a majority (at least 50 wt%) of the compatibilizer composition by weight. In some embodiments of the reaction mixture, the first fluoropolymer is at least 55, 60, 65, 70, 75, 76, 77, 78, 79, or 80 wt%. In other embodiments of the reaction mixture, the first fluoropolymer is present at 65-95, 70-90, 71-89, 72-88, 73-87, 74-86, 75-85, or 76-82 wt%. In specific embodiments, the first fluoropolymer is present at 75, 76, 77, 78, 79, 80, or 81 wt%.
[0058] Method for making a compatibilizer
[0059] Methods for making the compatibilizer are disclosed. Some embodiments of the method can be used to make one or more of the compatibilizer embodiments described above, although not all embodiments of the method may be useful for making each of the compatibilizer embodiments described above. A general embodiment of the method includes heating the reaction mixture described above (e.g., a first fluoropolymer, a first COC, a first reactive monomer, and a second reactive monomer) such that at least the first fluoropolymer and the first COC melt. Heating may melt or reduce the viscosity of the solid components to facilitate mixing and may also functionalize the first COC. In some embodiments, the components of the reaction mixture may be mixed and heated in an extruder, such as a twin screw extruder. In such embodiments, the heat of the extruder initiates the chemical reaction. In some embodiments, the reaction mixture is heated to 315° C. or higher. In some embodiments, the reaction mixture is heated to 330° C. or higher. In yet another embodiment, the reaction mixture is heated to 350° C. FIG. 1 depicts an example scheme for making the compatibilizer according to the present embodiments. As depicted in FIG. 1, the compatibilizer is prepared by a combination of addition and condensation reactions in an extruder.
[0060] Another general method for making the compatibilizer includes reacting an anhydride monomer with a first functional fluoropolymer to form a fluoropolymer dianhydride, and reacting the fluoropolymer dianhydride with a functional COC and a diamine monomer to form a compatibilizer. FIG. 2 shows an example of a scheme for making the compatibilizer according to the present embodiment. As shown in FIG. 2, the functional COC can be made by reacting an anhydride, such as bicyclo[2.2.1]hept-5-ene-2,3-dicarboxylic anhydride, with a non-functional cyclic olefin polymer in the presence of a peroxide catalyst. As mentioned above, the anhydride can be grafted onto the COC by a peroxide-catalyzed reaction. Suitable peroxide catalysts include dialkyl peroxides. Without being bound to a particular theory, it is believed that such an addition reaction increases the reactive groups available to react with other components of the compatibilizer. In the second step of the method, i.e., a condensation reaction, the functional COC can react with the fluoropolymer dianhydride and the diamine monomer to form the compatibilizer.
[0061] Compatibilizer Composition
[0062] In some embodiments, a reactive polymer compatibilizer is disclosed that is the product of any of the methods described above. The reactive polymer compatibilizer is effective in producing a thermoplastic polymer alloy of fluoropolymer and COC. In some embodiments, the reactive polymer compatibilizer is used in an amount of 1-99 wt% to form the thermoplastic polymer alloy. In another embodiment, the reactive polymer compatibilizer is used in an amount of 5-30 wt%. For example, the reactive polymer compatibilizer may be used in an amount of 30, 29, 28, 27, 26, 25, 24, 23, 22, 21, 20, 19, 18, 17, 16, 15, 14, 13, 12, 11, 10, 9, 8, 7, 6, or 5 wt%. In one specific embodiment, the reactive polymer compatibilizer is used in an amount of 10 wt%.
[0063] In another embodiment, the present disclosure provides a reactive polymeric compatibilizer having a COC group covalently bonded to at least one heterodimeric binding polymer comprising a dianhydride monomer and a diamine monomer, in this embodiment, the binding polymer is covalently bonded to a fluoropolymer group.
[0064] In one specific embodiment, the reactive polymeric compatibilizer has formula (I): [ka] wherein m, n, x, y, and z are each independently selected from an integer of ≧1, and the order of each subunit is not important.
[0065] In another specific embodiment, the reactive polymeric compatibilizer has formula (II): [ka] wherein m, n, x, y, and z are each independently selected from an integer of ≧1, and the order of each subunit is not important.
[0066] Fluoropolymer and cyclic olefin copolymer alloy
[0067] A thermoplastic polymer alloy of fluoropolymer and COC is disclosed that has many of the desirable properties of both fluoropolymer and COC. Normally, these two components are not compatible or compatible, but the above-described embodiment of the compatibilizer effectively makes them compatible. In a typical embodiment, the alloy includes a second fluoropolymer (which may or may not be the same as the fluoropolymer used to form the compatibilizer), a second COC (which may or may not be the same as the COC used to form the compatibilizer), and a compatibilizer. Without wishing to be bound by a hypothetical model, it is believed that the second fluoropolymer and the second COC are not chemically altered during the formation of the alloy.
[0068] Ideally, the second COC has mechanical and / or electrical properties suitable for high frequency electronics applications. In some embodiments of the reaction mixture, the second COC has a tensile strength of ≧25 MPa. In other embodiments of the reaction mixture, the second COC has a tensile strength of ≧30, 35, 40, 45, 50, 51, 52, and 53 MPa. In one specific embodiment of the reaction mixture, the second COC has a tensile strength of 54 MPa. In some embodiments of the reaction mixture, the second COC has a Young's modulus of ≧200 MPa. In other embodiments of the reaction mixture, the second COC has a Young's modulus of ≧250, 300, 350, 400, 450, 460, 470, and 480 MPa. In one specific embodiment of the reaction mixture, the second COC has a Young's modulus of 481. In some embodiments of the reaction mixture, the second COC has a flexural modulus of ≧1000 MPa. In another embodiment of the reaction mixture, the second COC has a flexural modulus of ≧1100, 1200, 1300, 1400, 1500, 1600, 1700, 1800, 1900, 2000, 2100, 2200, 2300, 2400, and 2500. In one specific embodiment of the reaction mixture, the second COC has a flexural modulus of 2530. In some embodiments of the reaction mixture, the second COC has a flexural strength of ≧50 MPa. In another embodiment of the reaction mixture, the second COC has a flexural strength of ≧55, 60, 65, 70, 71, 72, 73, 74, and 75 MPa. In one specific embodiment of the reaction mixture, the second COC has a flexural strength of 76 MPa. In some embodiments of the reaction mixture, the second COC has a flexural load of ≧50 N. In another embodiment of the reaction mixture, the second COC has a bending load of ≧60, 70, 80, 90, 100, 110, 120, 121, 122, 123, 124, and 125 N. In one specific embodiment of the reaction mixture, the second COC has a bending load of 126 N. In some embodiments of the reaction mixture, the second COC has a coefficient of thermal expansion of ≦100 μm / (m° C.). All of the above mechanical properties are measured according to the ATSM D638 and ASTM D790 standards.
[0069] In another embodiment of the reaction mixture, the second COC has a coefficient of thermal expansion of ≦90, 80, 70, 60, 50, 49, 48, 47, 46, 45, 44, 43, 42, 41, and 40 μm / (m° C.). In one specific embodiment of the reaction mixture, the second COC has a coefficient of thermal expansion of 39 μm / (m° C.). In some embodiments of the reaction mixture, the second COC has a dielectric constant of ≧2.10. In another embodiment of the reaction mixture, the second COC has a dielectric constant of ≧2.15, 2.20, 2.25, 2.30, 2.31, 2.32, and 2.33. In one specific embodiment of the reaction mixture, the second COC has a dielectric constant of 2.335. In some embodiments of the reaction mixture, the second COC has a dissipation factor of ≦0.001. In another embodiment of the reaction mixture, the second COC has a dielectric loss tangent of ≦0.0009, 0.0008, 0.0007, 0.0006, 0.0005, 0.00049, 0.00048. In a specific embodiment of the reaction mixture, the second COC has a dielectric loss tangent of 0.00047. In some embodiments of the reaction mixture, the second COC has a 1% weight loss temperature of ≧350° C. In another embodiment of the reaction mixture, the second COC has a 1% weight loss temperature of ≧360, 370, 380, 390, 391, 392, and 393° C. In a specific embodiment of the reaction mixture, the second COC has a 1% weight loss temperature of 394° C. In some embodiments of the reaction mixture, the second COC has a 5% weight loss temperature of ≧400° C. In another embodiment of the reaction mixture, the second COC has a 5% weight loss temperature of ≧405, 410, 415, 416, and 417° C. In one specific embodiment of the reaction mixture, the second COC has a 5% weight loss temperature of 418° C. In some embodiments of the reaction mixture, the second COC has a melt flow rate at 297° C. of ≦200 (g / 10 min). In another embodiment of the reaction mixture, the second COC has a melt flow rate of ≦190, 180, 170, 160, 150, 140, 130, 120, 110, 109, 108, 107, 106, 105, 104, 103, 102, and 101 g / (10 min). In one specific embodiment of the reaction mixture, the second COC has a melt flow rate of 100.6 g / (10 min).The melt flow rate was measured according to the method described above.
[0070] In some alloy embodiments, the second COC is a non-functional COC. In alloy embodiments where the second COC does not chemically react with other components during the alloying process, functional groups are not necessary. In some alloy embodiments, the second COC is the same as the first COC, or the second COC is a less functional version of the first COC. A less functional version of the first COC has fewer or no functional groups.
[0071] In some embodiments of the reaction mixture, the second COC comprises one or more of maleic anhydride, cis-4-cyclohexene-1,2-dicarboxylic anhydride; trans-1,2,3,6-tetrahydrophthalic acid; 5-methyl-3A,4,7,7A-tetrahydro-isobenzofuran-1,3-dione; endo-bicyclo[2.2.2]oct-5-ene-2,3-dicarboxylic anhydride; cis-5-norbornene-endo-2,3-dicarboxylic anhydride; bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic dianhydride; bicyclo[2.2.1]hept-5-ene-2,3-dicarboxylic anhydride; and 5-(2,5-dioxotetrahydrofuryl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride. In one specific embodiment of the alloy, the second COC is TOPAS 6017s (TOPAS Advanced Polymers, Raunheim, Germany).
[0072] In some embodiments of the alloy, the second fluoropolymer is not a sheared fluoropolymer.In some embodiments of the alloy, the second fluoropolymer does not have functional groups.
[0073] In some embodiments of the alloy, the second fluoropolymer comprises at least one of PFA, FEP, PTFE, ETFE, PVDF, EFEP, ECTFE, PCTFE, THV, and VT. Combinations of two or more of the above may be present in the second fluoropolymer fraction. In specific embodiments of the alloy, the second fluoropolymer is PFA, FEP, or PTFE.
[0074] The alloy according to some embodiments includes a third fluoropolymer. In some alloy embodiments, the third fluoropolymer may be any fluoropolymer taught herein as suitable as the second fluoropolymer.
[0075] In some embodiments of the alloy, the compatibilizer is any of the compatibilizers described above.
[0076] In some embodiments of the alloy, the first functional fluoropolymer is a functionalized second functional fluoropolymer. In some such embodiments, the first functional fluoropolymer may be a second functional fluoropolymer that has been pre-sheared to create functional groups.
[0077] Another compatibilizer may be added to the alloy. Bis(oxazoline) compatibilizers are one example of a suitable group of second compatibilizers. In some embodiments, the alloy comprises a second compatibilizer selected from 1,4-bis(4,5-dihydro-2-oxazolyl)benzene and 1,3-bis(4,5-dihydro-2-oxazolyl)benzene. In some embodiments, the alloy comprises about 0.1-10 wt.% of the second compatibilizer. In other embodiments, the alloy comprises 0.2-9, 0.3-8, 0.4-7, 0.5-6, 0.6-5, 0.7-4, 0.8-3, and 0.9-2 wt.% of the second compatibilizer. In one specific embodiment, the alloy comprises 1 wt.% of the second compatibilizer.
[0078] In some embodiments, the alloy includes a filler with a low dielectric tangent to adjust the electrical properties of the alloy. Suitable fillers include Al. 2 O 3 and SiO 2 In some embodiments of the alloy, the amount of filler is 0.1 to 40 wt%. In other embodiments of the alloy, the filler is present at 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, or 40 wt%.
[0079] Ideally, the alloy has mechanical and / or electrical properties suitable for high frequency electronic applications. In some embodiments, the alloy has a 1% weight loss temperature of at least 300°C. In other embodiments, the alloy has a 1% weight loss temperature of at least 310, 320, 330, 340, 350, 360, 370, 380, 390, 400, and 410°C. In other embodiments, the alloy has a 1% weight loss temperature of 330-420°C. In some embodiments, the alloy has a 5% weight loss temperature of at least 390°C. In other embodiments, the alloy has a 5% weight loss temperature of at least 400, 410, 420, 430, 440, 441, 442, 443, 444, 445, 446, and 447°C. In other embodiments, the alloy has a 5% weight loss temperature of 405-450°C. The percent loss at a given temperature was measured using a TA Instruments Q500 Thermogravimetry Instrument (TA Instruments, New Castle, Del.) in the following manner: When referring to the percent loss at a given temperature, it should be assumed that this method is meant unless expressly stated otherwise.
[0080] 1: Equilibrate at 40.00℃
[0081] 2: Ramp 10.00°C / min to 800.00°C
[0082] 3: Marks the end of cycle 1
[0083] 4: Completion of the method
[0084] Ideally, the alloy will be able to withstand deformation under load in high frequency electronics applications. In some embodiments, the alloy has a Young's modulus of ≥ 140 MPa. In other embodiments, the alloy has a Young's modulus of ≥ 225, 250, 260, 280, 300, 350, 400, 410, 420, 430, 450, 470, 475, and 480. For example, in some embodiments, the alloy has a Young's modulus of 140-480 MPa. In other embodiments, the alloy has a Young's modulus of 225-450 MPa. In other embodiments, the alloy has a Young's modulus of 410-472. In one specific embodiment, the alloy has a Young's modulus of 410 MPa. In another specific embodiment, the alloy has a Young's modulus of 430 MPa. In yet another specific embodiment, the alloy has a Young's modulus of 472 MPa. Ideally, the alloy will have a high tensile strength to perform well in high frequency electronics applications. In some embodiments, the alloy has a tensile strength of at least 24 MPa. In other embodiments, the alloy has a tensile strength of ≧25, 30, 35, 38, 40, 45, 48, 50, 52, and 54 MPa. For example, in some embodiments, the alloy has a tensile strength of 24-50 MPa. In other embodiments, the alloy has a tensile strength of 24-48 MPa. In one specific embodiment, the alloy has a tensile strength of 41 MPa. In another specific embodiment, the alloy has a tensile strength of 48 MPa. Ideally, the alloy has an elongation resistance that allows it to perform well in high frequency electronics applications. In some embodiments, the alloy has an elongation of less than 20%. In other embodiments, the alloy has an elongation of 19%, 18%, 17%, and 16% or less. For example, the alloy may have an elongation of 18.5%. In another specific embodiment, the alloy may have an elongation of 17.2%. In yet another embodiment, the elongation of the alloy is only as high as that of the second COC.
[0085] Ideally, the alloy has a bending resistance that allows it to perform well in high frequency electronic applications. In some embodiments, the alloy has a flexural modulus of at least 500 MPa. In other embodiments, the alloy has a flexural modulus of at least 1000 MPa. In yet other embodiments, the alloy has a flexural modulus of at least 1500 MPa. For example, in some embodiments, the alloy has a flexural modulus of at least 500, 700, 900, 1000, 1100, 1500, 1800, 1900, and 2000 MPa. In one specific embodiment, the alloy has a flexural modulus of at least 1823 MPa. In some embodiments, the alloy has a flexural strength of at least 20 MPa. In other embodiments, the alloy has a flexural strength of at least 30, 35, 40, 45, 50, and 55 MPa. In one specific embodiment, the alloy has a flexural strength of 34 MPa. In another specific embodiment, the alloy has a flexural strength of 50 MPa. In some embodiments, the alloy has a flexural load of at least 40 N. In other embodiments, the alloy has a bending load of at least 55, 60, 65, 70, 75, 80, 85, and 90 N. In one specific embodiment, the alloy has a bending load of 58 N. In another specific embodiment, the alloy has a bending load of 84 N. The above-mentioned mechanical properties are measured according to the ATSM D638 and ASTM D790 standards.
[0086] Ideally, the alloy has a thermal expansion resistance that allows it to perform well in high frequency electronics applications. In some embodiments, the alloy has a coefficient of thermal expansion less than 200 μm / (m° C.). In other embodiments, the alloy has a coefficient of thermal expansion less than 225 μm / (m° C.). For example, in some embodiments, the alloy has a coefficient of thermal expansion less than 220, 175, 150, 125, 100, 90, 80, 75, 70, 65, 60, and 55 μm / (m° C.). In one specific embodiment, the alloy has a coefficient of thermal expansion of 66 μm / (m° C.). In another specific embodiment, the alloy has a coefficient of thermal expansion of 74 μm / (m° C.). In some embodiments, the alloy has a coefficient of thermal expansion less than that of the second fluoropolymer.
[0087] Ideally, the alloy has a dielectric constant suitable for high frequency electronic applications. In some embodiments, the alloy has a dielectric constant greater than 2.1. In other embodiments, the alloy has a dielectric constant greater than 2.15, 2.16, 2.17, 2.18, 2.19, 2.0, 2.1, 2.2, 2.25, and 2.3. In a specific embodiment, the alloy has a dielectric constant of 2.17. In another specific embodiment, the alloy has a dielectric constant of 2.3. Ideally, the alloy has a dielectric loss tangent suitable for high frequency electronic applications. In some embodiments, the alloy has a dielectric loss tangent less than 0.001. In other embodiments, the alloy has a dielectric loss tangent less than 0.0009. In yet other embodiments, the alloy has a dielectric loss tangent less than 0.0008. In yet other embodiments, the alloy has a dielectric loss tangent less than 0.0007. In some embodiments of the alloy, the alloy has a lower dielectric loss tangent than the pure second fluoropolymer. For each sample, the sample thickness was measured at 4-5 points using digital calipers and averaged. The sample was then inserted into the cavity. Measurements were made using a Keysight P9374A PNA and NIST SplitC software. If the sample had defects, the best area was used to cover the cavity opening. The dielectric constant and dielectric loss were measured at 16 GHz. References to values of dielectric constant and dielectric loss refer to values obtained by this method unless explicitly stated.
[0088] How the alloy is made
[0089] A method for forming an alloy of a fluoropolymer and a COC is disclosed. It has been found that some embodiments of the method can be used to produce alloys according to some embodiments disclosed above, although not all embodiments of the method may be useful to produce each of the alloy embodiments. In a general embodiment, the method includes blending a second fluoropolymer, a compatibilizer, and a second cyclic olefin at a temperature such that at least the second fluoropolymer and the second COC are melted. Once the fluoropolymer and COC are melted, they can be alloyed in the presence of a compatibilizer (such as those described above). A reactive compatibilizer can be used to reduce the interfacial tension between the two different polymers, i.e., the fluoropolymer and the COC, to form a compatible blend. Figures 3 and 4 depict an example scheme for forming an alloy according to the present embodiments. As depicted in Figures 3 and 4, a fluoropolymer and COC alloy is formed by blending a second compatibilizer, a second fluoropolymer, and a second COC in the presence of a compatibilizer.
[0090] In some embodiments of the method, the blending step is carried out in an extruder, such as a twin screw extruder. In other embodiments, the blending step is carried out at 315° C. or higher. In yet other embodiments, the blending step is carried out at 330° C. or higher. In yet other embodiments, the blending step is carried out at 350° C.
[0091] In some embodiments of the method of forming the alloy, the second fluoropolymer may be any of those described in the above sections. For example, in some embodiments of the method, the second fluoropolymer comprises at least one of perfluoroalkoxyalkane (PFA), fluorinated ethylene propylene (FEP), polytetrafluoroethylene (PTFE), ethylene-tetrafluoroethylene (ETFE), polyvinylidene fluoride (PVDF), ethylene-tetrafluoroethylene-hexafluoropropylene terpolymer (EFEP), ethylene-chlorotrifluoroethylene (ECTFE), polychlorotrifluoroethylene (PCTFE), tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride terpolymer (THV), and tetrafluoroethylene and vinylidene fluoride copolymer (VT). In specific embodiments, such as those shown in Figures 3 and 4, the second fluoropolymer is PFA. In another specific embodiment, the second fluoropolymer is FEP. In yet another specific embodiment, the second fluoropolymer is PTFE.
[0092] Ideally, the COC has suitable mechanical properties for use in high frequency electronic applications. In some embodiments of the method of forming an alloy, the second COC may be any of those described in the sections above. For example, in some embodiments, the second COC comprises one or more of maleic anhydride, cis-4-cyclohexene-1,2-dicarboxylic anhydride; trans-1,2,3,6-tetrahydrophthalic acid; 5-methyl-3A,4,7,7A-tetrahydro-isobenzofuran-1,3-dione; endo-bicyclo[2.2.2]oct-5-ene-2,3-dicarboxylic anhydride; cis-5-norbornene-endo-2,3-dicarboxylic anhydride; bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic dianhydride; bicyclo[2.2.1]hept-5-ene-2,3-dicarboxylic anhydride; and 5-(2,5-dioxotetrahydrofuryl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride. In one specific embodiment, the second COC is TOPAS 6017s (TOPAS Advanced Polymers, Raunheim, Germany).
[0093] In some embodiments, the second COC has a tensile strength of ≧25 MPa. In other embodiments, the second COC has a tensile strength of ≧30, 35, 40, 45, 50, 51, 52, and 53 MPa. In one specific embodiment, the second COC has a tensile strength of 54 MPa. In some embodiments, the second COC has a Young's modulus of ≧200 MPa. In other embodiments, the second COC has a Young's modulus of ≧250, 300, 350, 400, 450, 460, 470, and 480 MPa. In one specific embodiment, the second COC has a Young's modulus of 481. In some embodiments, the second COC has a flexural modulus of ≧1000 MPa. In another embodiment, the second COC has a flexural modulus of ≧1100, 1200, 1300, 1400, 1500, 1600, 1700, 1800, 1900, 2000, 2100, 2200, 2300, 2400, and 2500. In a specific embodiment, the second COC has a flexural modulus of 2530. In some embodiments, the second COC has a flexural strength of ≧50 MPa. In another embodiment, the second COC has a flexural strength of ≧55, 60, 65, 70, 71, 72, 73, 74, and 75 MPa. In a specific embodiment, the second COC has a flexural strength of 76 MPa. In some embodiments, the second COC has a flexural load of ≧50 N. In another embodiment, the second COC has a bending load of ≧60, 70, 80, 90, 100, 110, 120, 121, 122, 123, 124, and 125 N. In one specific embodiment, the second COC has a bending load of 126 N. In some embodiments, the second COC has a coefficient of thermal expansion of ≦100 μm / (m° C.). In another embodiment, the second COC has a coefficient of thermal expansion of ≦90, 80, 70, 60, 50, 49, 48, 47, 46, 45, 44, 43, 42, 41, and 40 μm / (m° C.). In one specific embodiment, the second COC has a coefficient of thermal expansion of 39 μm / (m° C.). All of the above mechanical properties are measured according to the ATSM D638 and ASTM D790 standards.
[0094] In some embodiments of the above method, the second COC has a dielectric constant of ≧2.10. In other embodiments, the second COC has a dielectric constant of ≧2.15, 2.20, 2.25, 2.30, 2.31, 2.32, and 2.33. In a specific embodiment, the second COC has a dielectric constant of 2.335. In some embodiments, the second COC has a dielectric loss tangent of ≦0.001. In other embodiments, the second COC has a dielectric loss tangent of ≦0.0009, 0.0008, 0.0007, 0.0006, 0.0005, 0.00049, and 0.00048. In a specific embodiment, the second COC has a dielectric loss tangent of 0.00047. In some embodiments, the second COC has a 1% weight loss temperature of ≧350° C. In another embodiment, the second COC has a 1% weight loss temperature of ≧360, 370, 380, 390, 391, 392, and 393° C. In one specific embodiment of the reaction mixture, the second COC has a 1% weight loss temperature of 394° C. In some embodiments, the second COC has a 5% weight loss temperature of ≧400° C. In another embodiment, the second COC has a 5% weight loss temperature of ≧405, 410, 415, 416, and 417° C. In one specific embodiment, the second COC has a 5% weight loss temperature of 418° C. In some embodiments, the second COC has a melt flow rate at 297° C. of ≦200 (g / 10 min). In another embodiment, the second COC has a melt flow rate of ≦190, 180, 170, 160, 150, 140, 130, 120, 110, 109, 108, 107, 106, 105, 104, 103, 102, and 101 g / (10 min). In a specific embodiment, the second COC has a melt flow rate of 100.6 g / (10 min). The melt flow rates were calculated as described above.
[0095] In some embodiments of the method of forming the alloy, a second compatibilizer is used. For example, the second compatibilizer may be 1,4-bis(4,5-dihydro-2-oxazolyl)benzene or 1,3-bis(4,5-dihydro-2-oxazolyl)benzene. In specific embodiments, such as those shown in Figures 3 and 4, the second compatibilizer is 1,4-bis(4,5-dihydro-2-oxazolyl)benzene.
[0096] manufactured goods
[0097] Various embodiments of the polymer alloys described herein can be used to make many types of articles of manufacture. In some embodiments, electronic articles capable of wireless communication at 1 GHz or higher are provided, comprising any of the polymer alloys disclosed herein. For example, the electronic articles may be suitable for use in high frequency electronics related to the fifth generation (5G) of communication. In another embodiment, articles of manufacture that can be made using the polymer alloys described herein include, but are not limited to, insulation, such as insulation for communication cables; printed circuit boards; cables, such as coaxial cables, wire / cables for downhole cables, and twisted pair high speed cables for automobiles; wiring; antennas; connectors and tapes, such as tape wraps for electrical insulation, medical devices, electronic, medical, and industrial packaging. EXAMPLES
[0098] Example 1: Alloys with non-grafted COC / PFA compatibilizer
[0099] To form the COC / PFA compatibilized copolymer, the sheared fluorinated PFA, bis[2.2.1]hept-5-ene-2,3-dicarboxylic anhydride, 4,4'-oxydianiline, and reactive grade cyclic olefin copolymer were all mixed homogeneously in one bag. The amount of each chemical component used in the reactive polymeric compatibilizer (RPC) is shown in Table 2. The monomers used were added at 1:1 molar equivalents, totaling less than 5 wt% of the formulation. Once the sample was thoroughly mixed, the mixture was fed into a twin screw extruder (Leistritz ZSE 18HP) at 6 kg / hr. Zones 1-8 were heated from 315°C to 350°C. The screw speed was held constant at 250 RPM. The reactive extrusion process was a combination of addition and condensation reactions as seen in Figure 1. [Table 2]
[0100] After producing the COC / FP RPC blend, the RPC was blended with the COC TOPAS 6017s, PFA or FEP, and 1,4-bis(4,5-dihydro-2-oxazolyl)benzene in a twin screw extruder. The amount of each component used in the two samples is presented in Table 3 below. The sample mixture was fed into the twin screw extruder at 6-6.5 kg / hr. Zones 1-8 were heated to 315-350°C and the screw speed was held constant at 250 RPM for the PFA-based samples and 300 RPM for the FEP-based samples. It can be seen from Figure 2 that the reaction of the initial COC / FP blend was complete. [Table 3]
[0101] The mechanical and thermal properties (as per Table 3 above) of 42052B and 42052C were tested and compared to pure PFA and COC TOPAS 6017s. Initial thermal stability testing was completed on samples of PFA, COC TOPAS 6017s, 42042B, and 42052C on a TA Instruments Thermogravimetric Analyzer. Decomposition temperatures were measured and recorded in Table 4. From the TGA, the 42052B sample was determined to be thermally unstable and not injection moldable. All samples were run using the following method: (1) equilibrate at 45°C, (2) ramp 10°C / min to 800°C, and (3) mark the end of the cycle. [Table 4]
[0102] Samples were gravity fed into a Sumitomo SE750DU injection molding machine. The rotating screw was heated to 600°F to 680°F. PFA, COC TOPAS 6017s, and 42052C were molded into ASTM D638 V-shaped tensile bars, ASTM D790 bend bars, and 6 x 6 cm plates. Each molded part was characterized including mechanical properties, dynamic mechanical analysis, thermomechanical analysis, and electrical properties.
[0103] Tensile and flexural properties were completed on an Instron 5582 universal testing machine according to ASTM D638 and ASTM D790 standards. A 10 kN load cell was used to pull the tensile bar to break at a rate of 10 mm / min. The BlueHill2 program was used to calculate Young's modulus, tensile strength, and elongation. A 3-point bending test was performed using a bending bar. For testing, the samples were placed on rollers spaced 50 mm apart using a 1 kN load cell. A bending rod was used to apply load at a rate of 1.35 mm / min. The BlueHill2 program was used to calculate flexural modulus, maximum flexural strength, and maximum flexural load. Mechanical properties showed that the 42052C compatibilized samples were able to retain more than 85% of the properties of the cyclic olefin copolymer. The 42052C samples showed a three-fold increase in properties compared to pure PFA. The results of these tests are presented in Table 5. [Table 5]
[0104] The samples were tested to calculate the coefficient of thermal expansion (CTE) using a TA Instruments TMA Q400. Samples were cut from 6x6 cm injection molded plates. CTE was measured over the temperature range of 10°C to 140 / 150°C. CTE was calculated from the difference in sample height during the temperature change. The CTEs for the three samples and the pure resin are recorded in Table 6. Fluoropolymers are known to have high shrinkage and expansion rates at high temperatures. The 42052C and 42134A samples were found to have lower CTEs than pure PFA and FEP over the measured temperature range. However, the 42134B sample, which is a fluoropolymer rich sample, still showed a very high CTE due to the high fluoropolymer concentration. All samples were measured using the following method: (1) force 0.100 N, (2) equilibrate at 35.00° C., (3) isothermal for 5.00 minutes, (4) mark end of cycle 0, (5) isothermal for 5.00 minutes, (6) ramp 5.00° C. / min to 100.00° C., (7) isothermal for 3.00 minutes, (8) mark end of cycle 1, (9) ramp 10.00° C. / min to 0.00° C., (10) mark end of cycle 2, (11) ramp 5.00° C. / min to 175.00° C., and (12) complete method. [Table 6]
[0105] Dielectric properties were measured on 6 x 6 cm injection molded plates using a Keysight P9374A PNA. Data was analyzed using NIST SplitC software. The dielectric constant and dissipation factor were recorded at 17 GHz and are presented in Table 7. The 42052C sample has a dielectric constant slightly higher than pure PFA but lower than pure COC, and a dissipation factor of less than 0.001, which is better than pure fluoropolymer. [Table 7]
[0106] Example 2: Alloys using COC / PFA compatibilizers with grafted functional groups
[0107] In the second approach, dianhydrides were grafted onto the cyclic olefin copolymer using a high temperature stable dialkyl peroxide. This process is believed to increase the reactive groups available to create copolymers of COC and PFA. Grafting was controlled by increasing the amount of dianhydride (Bicycle[2.2.1]hept-5-ene-2,3-dicarboxylic anhydride; "BCDA") fed into the reactive extrusion process. The compositions are shown in Table 8. The materials were bulk mixed in a plastic bag by hand. The extrusion profile is shown in Table 9. Samples were fed into the TSE at a rate of 4.5 kg / hr with a screw speed of 300 RPM. The grafting of COC is an addition reaction. [Table 8] [Table 9]
[0108] The grafting density was determined by FTIR characterization. Pellets of each sample were pressed at elevated temperature using a heated Carver press to generate a flat sample area. Each sample was characterized on a Perkin Elmer Spectrum 100 FT-IR spectrophotometer using a Universal ATR Sampling Accessory. The transmission plots of each sample are shown in Figure 5. The FTIR spectrum showed the formation of a new band corresponding to cyclic anhydrides, with a peak at 1853 cm -1 and 1775 cm -1 In general, the peaks become more pronounced as the concentration of cyclic anhydride increases, as can be seen in Figure 6.
[0109] Once proper grafting was confirmed, the grafted COC was used to create the next generation RPC. The compositions of the three RPCs are shown in Table 10. The reaction was a condensation reaction and is depicted in Figure 3. The materials were mixed in a plastic bag and fed to the TSE at a screw speed of 300 RPM and a rate of 6.5 kg / hr. Once the RPC was properly extruded, the pellets were dried overnight in an oven at 100°C. The composition of the final COC / FP blend is shown in Table 11. The materials were mixed in a plastic bag and fed to the TSE at a screw speed of 300 RPM and a rate of 6.5 kg / hr. The temperature profile for both the RPC extrusion and the COC / FP blend extrusion to the TSE is shown in Table 12. The chemical structure of the final blend is depicted in Figure 4. [Table 10] [Table 11] [Table 12]
[0110] Once properly formulated, the thermal stability of each COC / FP blend was tested by thermogravimetric analysis. The decomposition temperatures at 1% and 5% by weight were measured and are shown in Table 13. Overall, it can be seen that the FEP-based samples are more thermally stable than the PFA-based samples, which generally have a lower 1% weight loss temperature. The higher graft density of COC has a direct effect on the decomposition temperature of the blend. The 42130A sample, which contains COC with a graft density of 1%, has a 1% weight loss of 414°C and a 5% weight loss of 448°C. For the 42130C and 42130E blends, increasing the graft density to 3% and 5% reduces the 1% weight loss temperature to 374°C and 379°C, and the 5% weight loss temperature to 432°C and 428°C, respectively. Also, the inclusion of PTFE, as in the 42134C sample, reduced the 1% and 5% weight loss temperatures by 20°C. All samples were run in the following manner: (1) equilibrate at 45° C., (2) ramp 10° C. / min to 800° C., and (3) mark the end of the cycle. [Table 13]
[0111] Samples were gravity fed into a Sumitomo SE750DU injection molding machine. The rotating screw was heated to 600°F to 680°F. PFA, COC TOPAS 6017s, and COC / FP blends were molded into ASTM D638 V-shaped tensile bars, ASTM D790 bend bars, and 6 x 6 cm plates. Molded parts were used for characterization including mechanical properties, dynamic mechanical analysis, thermomechanical analysis, and electrical properties.
[0112] Tensile and flexural properties were completed on an Instron 5582 universal testing machine according to ASTM D638 and ASTM D790 standards. A 10 kN load cell was used to pull the tensile bar to break at a rate of 10 mm / min. The BlueHill2 program was used to calculate Young's modulus, tensile strength, and elongation. A 3-point bending test was performed using a bending bar. For testing, the samples were placed on rollers spaced 50 mm apart using a 1 kN load cell. A bending rod was used to apply load at a rate of 1.35 mm / min. The BlueHill2 program was used to calculate flexural modulus, maximum flexural strength, and maximum flexural load. The mechanical properties of the COC / FP blends are recorded in Table 14. The COC-dominant samples exhibited properties of COC, including improved modulus, tensile strength, and elongation. The fluoropolymer-dominant blends showed as much as a two-fold increase in Young's modulus or modulus, making the copolymer stiffer compared to FEP or PFA. The inclusion of PTFE reduces the tensile strength by 7 MPa for the COC / FEP blend and 10.5 MPa for the COC / PFA blend, suggesting that the use of PTFE fillers in applications requiring high flame retardancy may disrupt the polymer alignment, reduce the interaction between the COC and FP, and act as stress points within the blend, weakening the material. [Table 14]
[0113] The samples were tested to calculate the coefficient of thermal expansion (CTE) using a TA Instruments TMA Q400. Samples were cut from 6 x 6 cm injection molded plates. CTE was measured over a temperature range of 10°C to 140 / 150°C. CTE was calculated from the difference in sample height during the temperature change. CTE was recorded for 10 samples and for the pure resin in Table 15. Samples rich in COC, regardless of fluoropolymer, have CTEs below 100 (μm / m*°C). Samples rich in fluoropolymer have very high CTEs. The addition of PTFE did not have a uniform effect on the CTE of the blends. When PTFE was added to the COC / FEP blend, the CTE decreased by 8 (μm / m*°C), whereas when it was added to the COC / PFA blend, the CTE increased by about 20 (μm / m*°C). All samples were run using the following method: (1) force 0.100n, (2) equilibrate at 35.00°C, (3) isothermal for 5.00 minutes, (4) mark end of cycle 0, (5) isothermal for 5.00 minutes, (6) ramp 5.00°C / min to 100.00°C, (7) isothermal for 3.00 minutes, (8) mark end of cycle 1, (9) ramp 10.00°C / min to 0.00°C, (10) mark end of cycle 2, (11) ramp 5.00°C / min to 175.00°C, and (12) complete method. [Table 15]
[0114] The melt flow rate (MFR) of selected FEP blends was measured according to ASTM D1238. The MFR of selected blends was measured at 297°C, 5 min dwell time, and 5 kg weight. The measured MFR is shown in the table below. For COC / FEP blends with predominantly COC, the MFR increases with the graft density of the COC in the RPC. The graft density does not have the same effect for fluoropolymer rich blends. The introduction of PTFE into the COC / FEP blends reduced the MFR by 30 g / 10 min. [Table 16]
[0115] Dielectric properties were measured on 6 x 6 cm injection molded plates using a Keysight P9374A PNA. Data was analyzed using NIST SplitC software. The dielectric constant and dissipation factor were recorded at 17 GHz and are shown in Table 17. The COC-dominant samples have an increased dielectric constant close to that of pure COC. However, the fluoropolymer-rich samples have a decreased dielectric constant of about 2.1. The addition of COC has a positive effect on the dissipation factor, as all but one blend measured values below 0.001, an improvement over the fluoropolymer. The addition of PTFE does not adversely affect the dissipation factor, but does reduce the dielectric constant from 2.301 to 2.295 for the COC / FEP blend and from 2.304 to 2.295 for the COC / PFA blend. [Table 17] [Table 18]
[0116] conclusion
[0117] It will be understood that certain elements disclosed as embodiments of the invention can be embodied as a single structure, a single step, or a single substance, etc. Similarly, certain elements disclosed as embodiments can be embodied as multiple structures, steps, or substances, etc. The above description and accompanying drawings illustrate and describe certain methods, machines, products, and compositions, some of which embody the present invention. These descriptions or illustrations are not intended to limit the scope of the claimed subject matter, but are provided as an aid to understanding the claims, to enable the claimed subject matter to be made and used, and to teach the best mode of using the invention. If the specification and accompanying drawings are construed as disclosing only one or more embodiments, they should not be construed as limiting the claimed subject matter to the one or more embodiments. Examples or embodiments of the invention described herein are not intended to indicate that the claimed subject matter must be identical to the examples or embodiments. Where the invention or embodiments thereof are described as achieving one or more objectives, it is not intended to limit the claimed subject matter to variations that achieve all of those objectives. Any statements herein critical of the prior art are not intended to limit the claimed subject matter to exclude aspects of the prior art. In addition, while this disclosure presents and describes certain embodiments of the disclosed methods, apparatus, manufacture, compositions, and other teachings, it will be understood that the teachings of the disclosure can be used in other various combinations, variations, and environments, and can be modified and varied within the scope of the teachings expressed herein. The headings herein are merely intended to correspond with the suggestions of 37 C.FR §1.77 or to provide organizational queues. These headings are not intended to limit or characterize the inventions described herein.
Claims
1. A reaction mixture for making a compatibilizer, comprising: (a) a first functional fluoropolymer; (b) a first cyclic olefin copolymer; (c) a first reactive monomer; and (d) a second reactive monomer; A reaction mixture comprising:
2. The reaction mixture of claim 1 , wherein the cyclic olefin copolymer comprises a functional group.
3. 3. The reaction mixture of claim 1 or 2, wherein the first cyclic olefin copolymer is an anhydride.
4. The reaction mixture of any one of claims 1 to 3, wherein the first cyclic olefin copolymer is a dianhydride.
5. 5. The reaction mixture of any one of claims 1 to 4, wherein the first cyclic olefin copolymer is a dianhydride and is the product of a process comprising reacting bicyclo[2.2.1]hept-5-ene-2,3-dicarboxylic acid anhydride with a cyclic olefin copolymer.
6. 6. The reaction mixture of any one of claims 1 to 5, wherein the first cyclic olefin copolymer is a dianhydride and is the product of a process comprising reacting an anhydride with a peroxide catalyzed cyclic olefin copolymer.
7. 7. The reaction mixture of any one of claims 1 to 6, wherein the first cyclic olefin copolymer is a dianhydride and is the product of a process comprising reacting bicyclo[2.2.1]hept-5-ene-2,3-dicarboxylic acid anhydride with a peroxide catalyzed cyclic olefin copolymer.
8. 8. The reaction mixture of any one of claims 1 to 7, comprising a peroxide catalyst capable of catalyzing the functionalization of the first cyclic olefin copolymer with an anhydride.
9. The reaction mixture of any one of claims 1 to 8, comprising a peroxide catalyst and wherein the first cyclic olefin copolymer is not a functionalized cyclic olefin copolymer.
10. The reaction mixture of any one of claims 1 to 9, wherein the first monomer is a diamine.
11. The reaction mixture of any one of claims 1 to 10, wherein the first monomer is a dianiline.
12. The reaction mixture of any one of claims 1 to 11, wherein the second monomer is an anhydride.
13. The reaction mixture of any one of claims 1 to 12, wherein the second monomer is a dicarboxylic acid anhydride.
14. The reaction mixture of any one of claims 1 to 13, wherein the second monomer is an unsaturated cyclic dianhydride.
15. 15. The reaction mixture of any one of claims 1 to 14, wherein the second monomer is bicyclo[2.2.1]hept-5-ene-2,3-dicarboxylic anhydride.
16. 16. The reaction mixture of any one of claims 1 to 15, wherein the second monomer is present at about 2.5 to 30 wt %.
17. 17. The reaction mixture of any one of claims 1 to 16, wherein the first cyclic olefin copolymer has a tensile strength of ≧25 MPa.
18. 18. The reaction mixture of any one of claims 1 to 17, wherein the first cyclic olefin copolymer has a Young's modulus of ≧200 MPa.
19. 19. The reaction mixture of any one of claims 1 to 18, wherein the first cyclic olefin copolymer has a flexural modulus of ≧1000 MPa.
20. 20. The reaction mixture of any one of claims 1 to 19, wherein the first cyclic olefin copolymer has a flexural strength of ≧50 MPa.
21. 21. The reaction mixture of any one of claims 1 to 20, wherein the first cyclic olefin copolymer has a flexural load of ≧50N.
22. 22. The reaction mixture of any one of claims 1 to 21, wherein the first cyclic olefin copolymer has a coefficient of thermal expansion of ≦100 μm / (m° C.).
23. 23. The reaction mixture of any one of claims 1 to 22, wherein the first cyclic olefin copolymer has a dielectric constant of ≧2.
1.
24. 24. The reaction mixture of any one of claims 1 to 23, wherein the first cyclic olefin copolymer has a dissipation factor of ≦0.
001.
25. 25. The reaction mixture of any one of claims 1 to 24, wherein the first cyclic olefin copolymer has a 1% weight loss temperature of ≧350°C.
26. 26. The reaction mixture of any one of claims 1 to 25, wherein the first cyclic olefin copolymer has a 5% weight loss temperature of ≧400° C.
27. 27. The reaction mixture of any one of claims 1 to 26, wherein the first cyclic olefin copolymer has a melt flow rate at 297°C of ≦200 (g / 10 min).
28. The reaction mixture of any one of claims 1 to 27, wherein the first fluoropolymer is sheared.
29. 29. The reaction mixture of any one of claims 1 to 28, wherein the first fluoropolymer is one or more of perfluoroalkoxyalkanes (PFA), fluorinated ethylene propylene (FEP), polytetrafluoroethylene (PTFE), ethylene-tetrafluoroethylene (ETFE), polyvinylidene fluoride (PVDF), ethylene-tetrafluoroethylene-hexafluoropropylene terpolymer (EFEP), ethylene-chlorotrifluoroethylene (ECTFE), polychlorotrifluoroethylene (PCTFE), tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride terpolymer (THV), and copolymers of tetrafluoroethylene and vinylidene fluoride (VT).
30. 30. The reaction mixture of any one of claims 1 to 29, wherein the first fluoropolymer is present at about 70-80% by weight and can be present at 1-99%.
31. The reaction mixture of any one of claims 1 to 30, wherein the first monomer is 4,4'-oxydianiline.
32. 32. The reaction mixture of any one of claims 1 to 31, wherein the first monomer is present at 1 to 25 wt%.
33. 2. The reaction mixture of claim 1, wherein the second monomer is 4,4'-(hexafluoroisopropylidene)diphthalic anhydride (6FDA).
34. 2. The reaction mixture of claim 1, wherein the second monomer is present at 1 to 25 weight percent.
35. 2. The reaction mixture of claim 1, wherein the first cyclic olefin copolymer comprises one or more of maleic anhydride, cis-4-cyclohexene-1,2-dicarboxylic anhydride; trans-1,2,3,6-tetrahydrophthalic acid; 5-methyl-3A,4,7,7A-tetrahydro-isobenzofuran-1,3-dione; endo-bicyclo[2.2.2]oct-5-ene-2,3-dicarboxylic anhydride; cis-5-norbornene-endo-2,3-dicarboxylic anhydride; bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic dianhydride; bicyclo[2.2.1]hept-5-ene-2,3-dicarboxylic anhydride; and 5-(2,5-dioxotetrahydrofuryl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride.
36. 36. A method of making a compatibilizer for alloying fluoropolymers with cyclic olefins, comprising the step of heating the reaction mixture of any one of claims 1 to 35 such that at least the first fluoropolymer and the first cyclic olefin copolymer are melted.
37. A method for making a compatibilizer for alloying a fluoropolymer with a cyclic olefin, comprising the steps of: (a) reacting an anhydride monomer with a first functional fluoropolymer to form a fluoropolymer dianhydride; and (b) reacting the fluoropolymer dianhydride with a functional cyclic olefin copolymer and a diamine monomer to form a compatibilizer; The method according to claim 1,
38. 38. The method of any one of claims 36 and 37, comprising reacting an anhydride with a non-functional cyclic olefin polymer in the presence of a peroxide catalyst to produce said functional cyclic olefin copolymer.
39. 39. The method of any one of claims 36 to 38, comprising reacting bicyclo[2.2.1]hept-5-ene-2,3-dicarboxylic anhydride with a non-functional cyclic olefin polymer in the presence of a peroxide catalyst to produce said functional cyclic olefin copolymer.
40. A reactive polymeric compatibilizer which is the product of the process of any one of claims 36 to 39.
41. A reactive polymeric compatibilizer comprising a cyclic olefin copolymer group covalently bonded to at least one heterodimeric binding polymer comprising a dianhydride monomer and a diamine monomer, said binding polymer being covalently bonded to a fluoropolymer group.
42. (a) a second fluoropolymer; (b) a compatibilizer; and (c) a second cyclic olefin copolymer 1. A thermoplastic polymer alloy composition comprising:
43. 43. The composition of claim 42, wherein the second cyclic olefin copolymer has a tensile strength of > 25 MPa.
44. The composition of any one of claims 42-43, wherein the second cyclic olefin copolymer has a Young's modulus of ≧200 MPa.
45. The composition of any one of claims 42 to 44, wherein the second cyclic olefin copolymer has a flexural modulus of ≧1000 MPa.
46. The composition of any one of claims 42 to 45, wherein the second cyclic olefin copolymer has a flexural strength of ≧50 MPa.
47. The composition of any one of claims 42 to 46, wherein the second cyclic olefin copolymer has a flexural load of ≧50N.
48. 48. The composition of any one of claims 42 to 47, wherein the second cyclic olefin copolymer has a coefficient of thermal expansion of ≦100 μm / (m° C.).
49. The composition of any one of claims 42 to 48, wherein the second cyclic olefin copolymer has a dielectric constant of ≧2.
1.
50. 50. The composition of any one of claims 42 to 49, wherein the second cyclic olefin copolymer has a dissipation factor of ≦0.
001.
51. The composition of any one of claims 42 to 50, wherein the second cyclic olefin copolymer has a 1% weight loss temperature of ≧350° C.
52. The composition of any one of claims 42 to 51, wherein the second cyclic olefin copolymer has a 5% weight loss temperature of ≧400° C.
53. The composition of any one of claims 42 to 52, wherein the second cyclic olefin copolymer has a melt flow rate at 297°C of ≦200 (g / 10 min).
54. The composition of any one of claims 42 to 53, wherein the second cyclic olefin copolymer is a non-functional cyclic olefin copolymer.
55. The composition of any one of claims 42 to 54, wherein the second fluoropolymer is not a sheared fluoropolymer.
56. The composition of any one of claims 42 to 55, wherein the second fluoropolymer has no functional groups.
57. The composition according to any one of claims 42 to 56, wherein the second fluoropolymer comprises at least one of perfluoroalkoxyalkane (PFA), fluorinated ethylene propylene (FEP), polytetrafluoroethylene (PTFE), ethylene-tetrafluoroethylene (ETFE), polyvinylidene fluoride (PVDF), ethylene-tetrafluoroethylene-hexafluoropropylene terpolymer (EFEP), ethylene-chlorotrifluoroethylene (ECTFE), polychlorotrifluoroethylene (PCTFE), tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride terpolymer (THV), and copolymer of tetrafluoroethylene and vinylidene fluoride (VT).
58. The composition of any one of claims 42 to 57, comprising a third fluoropolymer.
59. 59. The composition of any one of claims 42 to 58, comprising a third fluoropolymer selected from perfluoroalkoxyalkanes (PFA), fluorinated ethylene propylene (FEP), polytetrafluoroethylene (PTFE), ethylene-tetrafluoroethylene (ETFE), polyvinylidene fluoride (PVDF), ethylene-tetrafluoroethylene-hexafluoropropylene terpolymers (EFEP), ethylene-chlorotrifluoroethylene (ECTFE), polychlorotrifluoroethylene (PCTFE), tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride terpolymers (THV), and copolymers of tetrafluoroethylene and vinylidene fluoride (VT).
60. The composition according to any one of claims 42 to 59, wherein the compatibilizer is a compatibilizer according to any one of claims 40 to 41.
61. 61. The composition of any one of claims 42 to 60, wherein the compatibilizer is a compatibilizer of any one of claims 40 to 41, and the first cyclic olefin copolymer is the same compound as the second cyclic olefin copolymer.
62. 62. The composition of any one of claims 42 to 61, wherein the compatibilizer is the compatibilizer of any one of claims 40 to 41, and the first cyclic olefin copolymer is a functionalized version of the second cyclic olefin copolymer.
63. The composition of any one of claims 42 to 62, wherein the compatibilizer is the compatibilizer of claim 40 or 41, and the first functional fluoropolymer is a functionalized version of the second functional fluoropolymer.
64. 64. The composition of any one of claims 42 to 63, comprising a second compatibilizer selected from 1,4-bis(4,5-dihydro-2-oxazolyl)benzene and 1,3-bis(4,5-dihydro-2-oxazolyl)benzene.
65. 65. The composition of any one of claims 42 to 64, comprising about 0.1 to 10 wt. % of a second compatibilizer selected from 1,4-bis(4,5-dihydro-2-oxazolyl)benzene and 1,3-bis(4,5-dihydro-2-oxazolyl)benzene.
66. A 2 O 3 and SiO 2 The composition according to any one of claims 42 to 65, comprising at least one of:
67. The composition of any one of claims 42 to 66, having a 1% weight loss temperature of at least 330°C.
68. The composition of any one of claims 42 to 67, having a 5% weight loss temperature of at least 400°C.
69. The composition of any one of claims 42 to 68, having a Young's modulus of about 140 to 480 MPa.
70. 70. The composition of any one of claims 42 to 69, having a Young's modulus of about 225 to 450 MPa.
71. The composition of any one of claims 42 to 70, having a tensile strength of at least 24 MPa.
72. The composition of any one of claims 42 to 71, having a tensile strength of 24 to 48 MPa.
73. The composition of any one of claims 42 to 72, having an elongation of less than about 20%.
74. The composition of any one of claims 42-73, wherein the elongation is only about as great as the elongation of the second cyclic olefin copolymer.
75. The composition of any one of claims 42 to 74, having a flexural modulus of at least 500 MPa.
76. The composition according to any one of claims 42 to 75, having a flexural modulus of 200 to 900 MPa.
77. The composition of any one of claims 42 to 76, having a flexural strength of at least 20 MPa.
78. The composition of any one of claims 42 to 77, having a flexural load of at least 40N.
79. The composition of any one of claims 42 to 78, having a coefficient of thermal expansion of less than about 200 μm / (m° C.).
80. The composition of any one of claims 42 to 79, having a coefficient of thermal expansion of less than about 100 μm / (m° C.).
81. The composition of any one of claims 42 to 80, having a dielectric constant greater than 2.
1.
82. The composition of any one of claims 42 to 81, having a dielectric loss tangent of less than 0.
001.
83. 1. A method for forming an alloy of a fluoropolymer and a cyclic olefin copolymer, comprising the steps of: blending a second fluoropolymer, a compatibilizer, and a second cyclic olefin at a temperature such that at least the first fluoropolymer and the first cyclic olefin copolymer are melted; The method according to claim 1,
84. The method of claim 83, wherein the compatibilizer is a compatibilizer according to any one of claims 40 to 41.
85. The method of any one of claims 83 to 84, wherein the blending step is carried out in an extruder.
86. The method of any one of claims 83 to 85, wherein the blending step is carried out in a twin screw extruder.
87. The method of any one of claims 83 to 86, wherein the second fluoropolymer comprises at least one of perfluoroalkoxyalkanes (PFA), fluorinated ethylene propylene (FEP), polytetrafluoroethylene (PTFE), ethylene-tetrafluoroethylene (ETFE), polyvinylidene fluoride (PVDF), ethylene-tetrafluoroethylene-hexafluoropropylene terpolymer (EFEP), ethylene-chlorotrifluoroethylene (ECTFE), polychlorotrifluoroethylene (PCTFE), tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride terpolymer (THV), and copolymers of tetrafluoroethylene and vinylidene fluoride (VT).
88. 88. The method of any one of claims 83 to 87, wherein the second cyclic olefin copolymer has a tensile strength of ≧25 MPa.
89. 89. The method of any one of claims 83 to 88, wherein the second cyclic olefin copolymer has a Young's modulus of ≧200 MPa.
90. 90. The method of any one of claims 83 to 89, wherein the second cyclic olefin copolymer has a flexural modulus of ≧1000 MPa.
91. 91. The method of any one of claims 83 to 90, wherein the second cyclic olefin copolymer has a flexural strength of ≧50 MPa.
92. 92. The method of any one of claims 83 to 91, wherein the second cyclic olefin copolymer has a flexural load of ≧50N.
93. 93. The method of any one of claims 83 to 92, wherein the second cyclic olefin copolymer has a coefficient of thermal expansion of ≦100 μm / (m° C.).
94. 94. The method of any one of claims 83 to 93, wherein the second cyclic olefin copolymer has a dielectric constant of ≧2.
1.
95. 95. The method of any one of claims 83 to 94, wherein the second cyclic olefin copolymer has a dissipation factor of ≦0.
001.
96. 96. The method of any one of claims 83 to 95, wherein the second cyclic olefin copolymer has a 1% weight loss temperature of ≧350° C.
97. 97. The method of any one of claims 83 to 96, wherein the second cyclic olefin copolymer has a 5% weight loss temperature of ≧400° C.
98. 98. The method of any one of claims 83 to 97, wherein the second cyclic olefin copolymer has a melt flow rate at 297°C of ≦200 (g / 10 min).
99. 99. The method of any one of claims 83 to 98, comprising the step of including at least one second compatibilizer selected from 1,4-bis(4,5-dihydro-2-oxazolyl)benzene and 1,3-bis(4,5-dihydro-2-oxazolyl)benzene.
100. An electronic article capable of wireless communication at 1 GHz or higher, comprising a polymer alloy of a fluoropolymer and a cyclic olefin.
101. The article of claim 100, wherein the polymer alloy is a polymer alloy according to any one of claims 42 to 82.
Citation Information
Patent Citations
Backlight device
JP2012009187A
Method for producing composition
JP2022041941A
Film
JP2022041942A
Microporous sheet product and methods for making and using the same
WO2016073558A1
Chemically compatibilized fluoropolymer blends
WO2021039997A1