Graphite oxide, graphene oxide and reduced graphene oxide

By applying shear stress during oxidation and controlling oxygen content, the method addresses defects in graphene oxide production, resulting in improved conductivity of reduced graphene oxide.

JP2024545276APending Publication Date: 2024-12-05DONGJIN SEMICHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024537015
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-12-27
Filing Date
2022-11-01
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Existing methods for producing graphene oxide and reduced graphene oxide result in high defect formation, leading to reduced electrical conductivity due to excessive oxidation and inefficient exfoliation processes.

Method used

Controlled application of shear stress during oxidation with an oxidizing agent to minimize oxygen content in graphene oxide to 25-45 at%, followed by reduction to achieve reduced graphene oxide with less than 5 at% oxygen, using methods like X-ray diffraction and Raman spectroscopy for characterization.

Benefits of technology

The solution effectively reduces defects and enhances the electrical conductivity of reduced graphene oxide, maintaining high conductivity properties while minimizing oxidation reactor formation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024545276000001
    Figure 2024545276000001
  • Figure 2024545276000002
    Figure 2024545276000002
  • Figure 2024545276000003
    Figure 2024545276000003
Patent Text Reader

Abstract

The present invention relates to graphite oxide, graphene oxide, and reduced graphene oxide, and more particularly to graphite oxide, which contains 25 to 45 at % oxygen (O) but is effectively exfoliated from graphite oxide and can achieve excellent powder conductivity after reduction.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to graphite oxide, graphene oxide and reduced graphene oxide. [Background technology]

[0002] Graphite has a layered structure in which carbon atoms are connected in a hexagonal shape to form a two-dimensional layer structure, and these layers are stacked on top of each other to form a layered structure. One layer of this graphite is called graphene.

[0003] Graphene has been called the dream material since the beginning of the new millennium, as it has tensile strength 200 times greater than steel, electron mobility 1,000 times greater than silicon, and thermal conductivity 10 times greater than copper.

[0004] Due to the above-mentioned characteristics of graphene, research is underway to apply it to various fields in the nanomaterial field, such as ink, barrier, heat dissipation, energy, semiconductors, and transparent electrodes.

[0005] Graphene can be produced by various exfoliation methods, among which the chemical exfoliation method is known to be the easiest method for mass production. The graphene chemical exfoliation method produces graphene by oxidizing graphite, exfoliating it in a solution, and then restoring conductivity through a reduction process. The key to the chemical exfoliation method is the technology to efficiently insert an oxidant between the graphite layers to minimize defects on the graphene surface and efficiently reduce it after exfoliation. Summary of the Invention [Problem to be solved by the invention]

[0006] An object of the present invention is to provide a graphene oxide that can minimize defects in reduced graphene.

[0007] Another object of the present invention is to provide a graphite oxide that can minimize defects in reduced graphene.

[0008] It is yet another object of the present invention to provide a reduced graphene oxide having excellent powder conductivity.

[0009] To achieve the above object, graphene oxide according to one embodiment of the present invention is characterized in that it contains oxygen (O) at 25 to 45 at %.

[0010] In this case, the atomic ratio of carbon (C) and oxygen (O) in the graphene oxide can be 1.2:1 to 3:1.

[0011] The graphene oxide may have a D / G ratio of 0.80 to 0.90 in a Raman spectrum measured with a Raman spectrometer.

[0012] The graphene oxide may have properties that satisfy the following Equation 1 when data obtained by X-ray diffraction (XRD) analysis is used.

[0013] [Formula 1]

[0014] JPEG2024545276000001.jpg5126

[0015] In Equation 1, H1 is a peak value of graphene oxide having a maximum peak observed in the 2θ range of 10° to 12° in a data graph obtained by X-ray diffraction (XRD) analysis, and H2 is a peak value of unreacted graphite having a maximum peak observed in the 2θ range of 25° to 28° in a data graph obtained by XRD analysis.

[0016] Graphite oxide according to another embodiment of the present invention includes the graphene oxide.

[0017] The graphite oxide may include the graphene oxide in the form of multiple layers, and the graphene oxide may have an average interlayer distance of 0.7 to 0.9 nm.

[0018] A reduced graphene oxide according to another embodiment of the present invention is obtained by reducing the graphene oxide.

[0019] The reduced graphene oxide may contain oxygen (O) in an amount exceeding 0 at % and not more than 5 at % of the total content.

[0020] The reduced graphene oxide can exhibit a characteristic that the maximum half-width of a peak in the 20 to 26.5° region of an XRD (X-ray diffraction) spectrum is 0.5 to 5°.

[0021] The reduced graphene oxide may exhibit a weight loss rate of more than 0 at% and less than 20 wt% when the temperature is increased from 25°C to 500°C.

[0022] The reduced graphene oxide may have a density of 0.001 to 0.1 g / mL. Effect of the Invention

[0023] The graphene oxide according to the present invention can be effectively peeled off from graphite oxide even with a small ratio of oxidation reactors, and the reduced graphene oxide according to the present invention obtained by reducing graphene oxide having a small ratio of oxidation reactors can achieve excellent powder conductivity.

[0024] The terms or words used in this specification and the claims should not be interpreted as being limited to their ordinary or dictionary meanings, but should be interpreted as having a meaning and concept that corresponds to the technical idea of ​​the present invention, based on the principle that an inventor can appropriately define the concept of a term in order to explain his / her invention in the best possible manner.

[0025] Therefore, it should be understood that the configurations shown in the embodiments and manufacturing examples described in this specification are merely the most preferred embodiments of the present invention and do not fully represent the technical ideas of the present invention, and therefore there may be various equivalents and modifications that can be substituted for them at the time of filing this application.

[0026] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention may be embodied in various different forms, but is not limited to the embodiments set forth herein, and may be practiced in various different ways.

[0027] The oxygen in graphene oxide is derived from oxidation reactors formed on the graphene surface. The oxidation reactors formed on the graphene surface are formed during the process of peeling off graphene, and after peeling off the graphene, the graphene oxide must be reduced again. In the process of reducing the oxidation reactors of graphene oxide, defects are generated on the graphene surface, which may cause a decrease in the conductive properties of the reduced graphene oxide. Therefore, the less the oxygen, the better.

[0028] The graphene oxide according to one embodiment of the present invention contains oxygen (O) at 25 to 45 at %. That is, in the graphene oxide, 25 to 45% of all atoms are oxygen (O). The oxygen content of the graphene oxide is lower than the oxygen content of conventional graphene oxide, 50 at %, and therefore, the graphene oxide according to the embodiment of the present invention has a smaller ratio of oxidation reactors to be reduced than conventional ones, and defects that deteriorate the conductive properties of graphene generated during the reduction process of graphene oxide can be significantly reduced.

[0029] When the graphene oxide of the present invention contains oxygen at less than 25 at%, an oxidation reactor capable of peeling off graphene is not formed, resulting in a problem that graphene is not sufficiently peeled off through an oxidation reactor, and when the graphene oxide contains oxygen at more than 45 at%, there is no significant difference from the content of conventional graphene oxide, and a problem occurs in that electrical conductivity is significantly reduced during the reduction of graphene oxide, as in conventional graphene oxide. In order to more significantly show the difference in effect from conventional graphene oxide, it is preferable that the graphene oxide contains oxygen at 25 to 35 at%.

[0030] In order to realize a low oxygen content in graphene oxide, a technology is required to effectively exfoliate graphene while using a small amount of oxidant in the process of oxidizing graphite, which is a layered structure of graphene, and for example, this can be solved by applying a physical force to the graphite in the process of adding an oxidant to the graphite and oxidizing it. More specifically, the physical force can be a shear stress, and when a shear stress is applied together with the oxidant in the process of oxidizing graphite, the oxidant can be effectively introduced to the center of the graphite compared to simple diffusion, allowing efficient use of the oxidant, and graphite can be effectively exfoliated even with a small amount of oxidant.

[0031] The oxygen content of the graphene oxide can be analyzed by X-ray photoelectron spectroscopy (XPS), and the ratio of the carbon and oxygen contents of the graphene oxide can be known by XPS.

[0032] The oxygen ratio of the graphene oxide is 25 to 45 at% when expressed as an atomic ratio, and when expressed as an atomic ratio (carbon:oxygen) of carbon (C) and oxygen (O), which are the main components of graphene oxide, the atomic ratio of carbon to oxygen (atomic ratio) may be 1.2:1 to 3:1. Carbon is a basic atom of graphene, and if the ratio of oxygen is lower than the above atomic ratio, there is a problem that graphene oxide cannot be sufficiently exfoliated into a single layer structure from the graphite laminate structure, and if the atomic ratio of oxygen is higher than the above atomic ratio, there is a problem that graphene surface defects frequently occur during the production of reduced graphene oxide, and the conductive properties of the reduced graphene oxide are significantly reduced.

[0033] The oxygen content of graphene oxide can be confirmed through Raman spectroscopy, and graphene oxide according to the embodiment of the present invention containing oxygen in the range of 25 to 45 at % may appear in the Raman spectrum with (D peak intensity) / (G peak intensity), i.e., D / G ratio, of 0.80 to 0.90. In the Raman spectrum, the D / G ratio indicates the degree of change in the ordering of carbon structures, and when the D / G ratio of graphene oxide is less than 0.80, there may be a problem that the graphene oxide is not sufficiently peeled off from graphite, and when the D / G ratio of graphene oxide is more than 0.90, there may be a problem that an unnecessary number of oxidation reactors are formed on the graphene oxide, and the electric conductivity property of the reduced graphene oxide may be unnecessary decreased after the graphene oxide is reduced.

[0034] The graphene oxide can be produced by exfoliating graphite oxide, which is obtained by oxidizing graphite. Specifically, the interlayer distance of graphite oxide is increased, and the part with weak interlayer bond energy can be exfoliated into graphene oxide using a physical method such as an ultrasonic grinder.

[0035] The average interlayer distance of the graphene oxide can be confirmed through X-ray diffraction (XRD) analysis. XRD analysis uses Bragg's law, and the 2θ (2 theta) value of XRD is calculated using Bragg's equation and converted into interlayer distance. In the case of the original graphite, a peak point appears in the 26.3° region, and the longer the interlayer distance of the graphite, the more the peak point shifts to the left in the XRD graph. The graphene oxide according to the embodiment of the present invention can satisfy the following mathematical formula 1 when using XRD analysis.

[0036] [Formula 1]

[0037] JPEG2024545276000002.jpg5126

[0038] In the above Equation 1, H1 is a peak value of graphene oxide having a maximum peak observed in a 2θ range of 10° to 12° in a data graph obtained by X-ray diffraction (XRD) analysis, and H2 is a peak value of unreacted graphite having a maximum peak observed in a 2θ range of 25° to 28° in a data graph obtained by XRD analysis.

[0039] Graphite oxide according to another embodiment of the present invention is in a state before being exfoliated into the graphene oxide according to the embodiment of the present invention after oxidizing graphite. The low oxygen content of the graphene oxide of the present invention is derived from the properties of graphite oxide, and each graphene oxide layer constituting the graphite oxide of the present invention has a lower oxygen content than conventional graphite oxide, while having a feature that an oxidation reactor is formed uniformly up to the center of the graphite oxide.

[0040] The characteristics of the graphite oxide according to the embodiment of the present invention can be confirmed through the interlayer distance of the graphite oxide. In the graphite oxide structure in which the graphene oxide is laminated in multiple layers, the average interlayer distance of the graphene oxide means the distance between adjacent graphene oxides. The graphite oxide according to the embodiment of the present invention has a smaller oxygen ratio than that of conventional graphite oxide, so that the average interlayer distance of the graphene oxide can be narrower than that of conventional graphene oxides, and specifically, the average interlayer distance of the graphene oxide according to the embodiment of the present invention can be 0.7 to 0.9 nm. If the average interlayer distance of the oxidized graphene is less than 0.7 nm, a problem may occur in which the graphite oxide is not easily peeled off, and if the average interlayer distance of the graphene oxide is more than 0.9 nm, this means that an unnecessary number of oxidation reactors are formed on the graphene, and many defects may be formed in the process of forming the reduced graphene oxide, which may cause a problem of deteriorating the electrical conductivity properties of the reduced graphene oxide.

[0041] Reduced graphene oxide (rGO) according to another embodiment of the present invention is obtained by reducing the graphene oxide according to the embodiment of the present invention, and is given electrical conductivity by reducing the exfoliated graphene oxide. The reduced graphene oxide according to the embodiment of the present invention is obtained by reducing graphene oxide having a low oxygen ratio (25 to 45 at%), and the ratio of reduced oxidation reactors during the reduction of graphene oxide is lower than that of conventional graphene oxide, so the loss of electrical conductivity during the reduction process is small, and the electrical conductivity (powder conductivity) of the reduced graphene oxide is improved compared to conventional reduced graphene oxide.

[0042] The reduced graphene oxide according to the embodiment of the present invention is derived from graphene oxide having a low oxygen content, and the oxygen content of the reduced graphene oxide is also very low. Specifically, the reduced graphene oxide may contain very low oxygen (O) content, such as more than 0 at% and less than 5 at% with respect to the total content including carbon. The oxygen contained in the reduced graphene oxide is derived from the oxidation reactor that is not reduced during the reduction of the graphene oxide, and the reduced graphene oxide does not contain no oxidation reactor at all (more than 0 at%). However, the reduced graphene oxide according to the embodiment of the present invention is obtained by reducing graphene oxide having a low oxygen ratio (25 to 45 at%), and the reduced graphene oxide may contain oxygen at 5 at% or less. If the reduced graphene oxide contains oxygen at more than 5 at%, there may be a problem that the electrical conductivity of the reduced graphene oxide is significantly reduced.

[0043] The oxygen content of reduced graphene oxide can be confirmed through an XRD (X-ray diffraction) spectrum. The reduced graphene oxide of the present invention is derived from graphene oxide with a low oxygen content and has a lower oxygen ratio than conventional reduced graphene oxide, which can be confirmed through the fact that the maximum half-width of the peak in the 20-26.5° region of the XRD (X-ray diffraction) spectrum is 0.5-5°.

[0044] Reduced graphene oxide loses weight due to the oxidation reactor remaining on the surface during heating. The reduced graphene oxide according to the present invention has a very low ratio of remaining oxidation reactor derived from graphene oxide compared to conventional reduced graphene oxide, so that it may exhibit a slight weight loss rate even when heated to a high temperature. For example, the reduced graphene oxide according to the present invention may have a weight loss rate of more than 0 at% and 20 wt% or less when the temperature is increased from 25°C to 500°C. The weight loss rate analysis may be confirmed through thermogravimetric analysis (TGA).

[0045] The reduced graphene oxide according to the embodiments of the present invention may have a density of 0.001 to 0.1 g / mL. The reduced graphene oxide according to the present invention has a low oxygen content, which can be confirmed by its low density compared to conventional reduced graphene oxide.

[0046] The present invention will be described in more detail below through examples, but the present invention is not limited to the following examples.

[0047] [Production Example 1: Production of graphite oxide]

[0048] 1 L of sulfuric acid solution and 40 g of graphite are stirred in a double jacketed reactor and the reactor temperature is cooled to 10°C.

[0049] After the sulfuric acid solution has cooled sufficiently to the center, 160 g of potassium permanganate is added slowly so as not to raise the temperature locally. After the potassium permanganate is added, the solution is stirred in the reaction tank for 30 minutes, during which time the reaction tank is sealed to prevent it from reacting with external moisture.

[0050] After stirring for 30 minutes to stabilize the reaction of potassium permanganate, shear stress is applied to the solution. As an exemplary method for applying shear stress, in this preparation example, a Couette-Taylor reactor is used to apply shear stress to the graphite. To apply the shear stress, the rotation speed of the inner cylinder contained in the Couette-Taylor reactor was set to 1500 rpm, and the rotation time was set to 60 minutes.

[0051] An oxidizing agent (potassium permanganate) is applied with shear stress and an oxidation reaction is carried out until the oxidizing agent is inserted into the center of the graphite. For example, if the reaction is carried out for one hour for a 150 μm graphite particle, the oxidizing agent can be inserted into the center.

[0052] When the oxidation reaction is completed, hydrogen peroxide is added to terminate the oxidation reaction of potassium permanganate. Hydrogen peroxide is added until no more bubbles are generated, producing graphite oxide.

[0053] Metal impurities and acid ions other than the graphite oxide produced are removed. To remove the metal ions, the metal is ionized using an acid such as hydrochloric acid, and the graphite oxide and metal ions are separated through a filter. After sufficient washing, the acid is neutralized with distilled water to wash it off, and the graphite oxide and acid ions are separated through a filter to obtain graphite oxide (Example 1).

[0054] Examples 2 to 4 and Comparative Examples 1 and 2 were produced by varying only the amount of oxidizing agent (potassium permanganate) and the amount of acid (sulfuric acid) from the graphite oxide of Example 1, and are shown in Table 1 below.

[0055] [Table 1]

[0056] [Experimental Example 1-1: Comparison of interlayer distances of graphite oxide]

[0057] For Examples 1 to 4 and Comparative Examples 1 and 2 in Table 1 of Production Example 1, XRD (LabX XRD-6100, SHIMADZU Corporation) analysis was performed, and the average interlayer distance of graphite oxide is shown in Table 2 below.

[0058] [Experimental Example 1-2: Comparison of powder conductivity of graphite oxide]

[0059] Powder conductivity is measured to analyze the electrical conductivity of graphene in powder form. The same amount of powder (0.1g) is placed in a measurement cell, and the conductivity value, which changes depending on the load, can be read through a conductivity probe while applying a load. The results are compared with the powder conductivity value under a 2,000kgf condition.

[0060] The powder conductivity of the graphite oxides of Examples 1 to 4 and Comparative Examples 1 and 2 in Table 1 was measured using a powder resistance characteristic measuring device (HPRM-FA2, HANTech Co., Ltd.) and is shown in Table 2 below.

[0061] [Table 2]

[0062] Referring to Table 2, it can be seen that the graphite oxide according to the embodiment of the present invention has a higher powder conductivity than the comparative example due to the low oxygen content.

[0063] In Comparative Example 1 in Table 2, the content of potassium permanganate is too low to ensure the oxidizing power of the oxidizing agent, so the graphite cannot be oxidized to the center. That is, the carbon / oxygen atomic ratio is high and the D / G ratio is low, which indicates that there is a lot of unreacted graphite and the powder conductivity is low.

[0064] On the other hand, in Comparative Example 2, when the amount of potassium permanganate was excessive, the oxidizing power of the oxidizing agent was sufficient, but the graphite was overoxidized due to the excessive oxidizing agent, which resulted in many defects during reduction, and it was confirmed that the powder conductivity characteristics were reduced.

[0065] [Production Example 2: Production of Graphene Oxide

[0066] The graphite oxide prepared in Preparation Example 1 can be exfoliated into graphene oxide by applying physical energy using an ultrasonic grinder, etc., to the graphite oxide where the interlayer distance is increased and the binding strength is weakened. The graphene oxide (Example 1) can be obtained by exfoliating the graphite oxide through an exfoliation process for more than 1 hour in a 700 W reactor.

[0067] Examples 2 to 15 and Comparative Examples 1 to 3 were produced by varying only the amount of oxidizing agent (potassium permanganate) and the amount of acid (sulfuric acid) from the graphite oxide produced in Example 1, and are shown in Table 3 below.

[0068] [Table 3]

[0069] [Experimental Example 2-1: Comparison of oxygen content in graphene oxide]

[0070] XPS analysis is used to analyze the carbon and oxygen content of graphene oxide. The carbon and oxygen content ratio is calculated by calculating the ratio of bond strength values ​​confirmed by XPS wide scan values, and the bond strength in the C1s and O1s regions is converted into the C / O ratio to confirm the results.

[0071] For Examples 1 to 17 and Comparative Examples 1 to 3 of Preparation Example 2, the oxygen content (at %) and the carbon to oxygen atomic ratio (C / O ratio) of the graphene oxide were measured by XPS and are shown in Table 4 below.

[0072] [Experimental Example 2-2: Comparison of XRD analysis of graphene oxide]

[0073] XRD (LabX XRD-6100, SHIMADZU) analysis was performed on Examples 1 to 17 and Comparative Examples 1 to 3 of Preparation Example 2, and the (H2) / (H1+H2) values ​​are shown in Table 4 below. Here, H1 is the peak value of graphene oxide whose maximum peak is observed in the 10° to 12° 2θ range in the data graph obtained by X-ray diffraction (XRD) analysis, and H2 is the peak value of unreacted graphite whose maximum peak is observed in the 2θ range of 25° to 28° in the data graph obtained by XRD analysis.

[0074] [Experimental Example 2-3: Comparison of Raman spectrum analysis of graphene oxide]

[0075] Raman analysis confirms the degree of change in the regularity of the graphite structure that occurs in the graphite layer, defects, and reactors. In general, the more bonds there are with the reactor, the higher the D / G ratio of graphene oxide becomes, and the D / G ratio is restored when the layer structure is restored after reduction.

[0076] For Examples 1 to 17 and Comparative Examples 1 to 3 of Production Example 2, the D / G ratios (D / Gratio) in the Raman spectra obtained with a Raman spectrometer (LabRAM HR Evolution, HORIBA) are shown in Table 4 below.

[0077] [Experimental Example 2-4: Comparison of powder conductivity of graphene oxide]

[0078] The graphene oxides of Examples 1 to 17 and Comparative Examples 1 to 3 in Production Example 2 were measured for powder conductivity using a powder resistivity characteristic measuring device (HPRM-FA2, HANTech Co., Ltd.), and the results are shown in Table 4 below.

[0079] [Table 4]

[0080] Referring to Table 4, it can be seen that the powder conductivities of Examples 1 to 17, which have a low ratio of oxidation reactors, are superior to the powder conductivities of Comparative Examples 1 to 3.

[0081] [Production Example 3: Production of reduced graphene oxide]

[0082] In order to freeze-dry the graphene oxide prepared in Preparation Example 2, the graphene oxide solution is sufficiently frozen and then dried at -80°C and 0.05 mTorr. The drying time varies depending on the amount and surface area of ​​the sample, but is typically one day or more.

[0083] The oxidation reactor must be removed to restore the electrical conductivity of the dried graphene oxide. In this manufacturing example, microwave wavelengths were injected to reduce graphene oxide, and reduced graphene was obtained by irradiating the 2.45 GHz wavelength region at 1,000 W for 5 to 10 seconds (Example 1).

[0084] For the reduced graphene oxide produced in Example 1, the amount of oxidant (potassium permanganate), the amount of acid (sulfuric acid), and the microwave injection time were varied to produce Examples 2 to 26 and Comparative Examples 1 to 3, which are shown in Table 5 below.

[0085] [Table 5]

[0086] [Experimental Example 3-1: Comparison of oxygen content in reduced graphene oxide]

[0087] For Examples 1 to 26 and Comparative Examples 1 to 3 of Preparation Example 3, the oxygen contents (at %) of the reduced graphene oxides were measured by XPS and are shown in Table 6 below.

[0088] [Experimental Example 3-2: XRD analysis comparison of reduced graphene oxide]

[0089] For Examples 1 to 26 and Comparative Examples 1 to 3 of Production Example 3, the maximum half-value widths of the peaks in the 20° to 26.5° region of the XRD spectrum are shown in Table 6 below.

[0090] [Experimental Example 3-3: Comparison of weight loss rate analysis of reduced graphene oxide]

[0091] Regarding Examples 1 to 26 and Comparative Examples 1 to 3 of Production Example 3, the weight loss rates when the temperature was raised from 25° C. to 500° C. are shown in Table 6 below.

[0092] [Experimental Example 3-4: Density comparison of reduced graphene oxide]

[0093] The densities of Examples 1 to 26 and Comparative Examples 1 to 3 in Production Example 3 were measured and are shown in Table 6 below.

[0094] [Experimental Example 3-5: Comparison of powder conductivity of reduced graphene oxide]

[0095] For Examples 1 to 26 and Comparative Examples 1 to 3 of Production Example 3, the powder conductivity was measured using a powder resistance characteristic measuring device (HPRM-FA2, HANTech Co., Ltd.) and is shown in Table 6 below.

[0096] [Table 6]

[0097] Although the preferred embodiments of the present invention have been described in detail above, the scope of the present invention is not limited thereto, and various modifications and improvements made by those skilled in the art using the basic concept of the present invention defined in the following claims also fall within the scope of the present invention.

Claims

1. Graphene oxide containing 25 to 45 at % oxygen (O).

2. 2. The graphene oxide according to claim 1, wherein the atomic ratio of carbon (C) to oxygen (O) is 1.2:1 to 3:

1.

3. 2. The graphene oxide according to claim 1, wherein the (D peak intensity) / (G peak intensity) (D / G ratio) in a Raman spectrum obtained by a Raman spectrometer is 0.80 to 0.

90.

4. The graphene oxide according to claim 1, which satisfies the following formula 1: [Formula 1] In the above formula 1, H1 is a peak value for graphene oxide in which the maximum peak is observed in the range of 2θ from 10° to 12° in a data graph obtained by X-ray diffraction (XRD) analysis, H2 is the peak value of unreacted graphite, the maximum peak of which is observed in the 2θ range of 25° to 28° in a data graph obtained by XRD analysis.

5. Graphite oxide comprising the graphene oxide according to any one of claims 1 to 4.

6. The graphite oxide according to claim 5, wherein the graphene oxide has a multi-layer structure, and an average interlayer distance of the graphene oxide is 0.7 to 0.9 nm.

7. A reduced graphene oxide, obtained by reducing the graphene oxide according to any one of claims 1 to 4.

8. The reduced graphene oxide according to claim 7, containing oxygen (O) in an amount greater than 0 at% and less than or equal to 5 at% relative to the total content.

9. The reduced graphene oxide according to claim 7, wherein the maximum half-width of a peak in the 20 to 26.5° region of an XRD (X-ray diffraction) spectrum is 0.5 to 5°.

10. The weight loss rate when the temperature is increased from 25°C to 500°C exceeds 0 at%. The reduced graphene oxide of claim 7, wherein the reduced graphene oxide is less than or equal to 20 wt%.

11. The reduced graphene oxide of claim 7, having a density of 0.001 to 0.1 g / mL.