Methods for decomposing polymer compounds, degradable adhesive compositions, methods for decomposing joints, degradable paint compositions, methods for removing paint films from painted surfaces, and methods for recovering fibers contained in fiber-reinforced plastics.
A polymer compound with a divalent group is decomposed using nitrite esters or nitrite and acid solutions, addressing the limitations of poly(diacylhydrazine) degradation and enabling efficient separation and recovery of materials.
Patent Information
- Application Number
- JP2025069490
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2025-04-21
- Publication Date
- 2026-11-02
Smart Images

Figure 2026174911000001_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for decomposing a polymer compound, a decomposable adhesive composition, a method for decomposing a joined body, a decomposable coating composition, a method for removing a coating film from a coated surface, and a method for recovering fibers contained in fiber-reinforced plastic.
Background Art
[0002] In recent years, from the perspective of environmental protection and the like, development of degradable polymer materials represented by biodegradable polymers and photodegradable polymers that can be naturally degraded even after disposal has been actively carried out. However, biodegradable polymers and photodegradable polymers have a problem of being accompanied by deterioration over time under normal use environments.
[0003] For this reason, polymer compounds that do not deteriorate over time during use and can be rapidly degraded at the time of disposal are in demand. As polymer compounds that can be easily degraded by an oxidizing agent at the time of disposal, several examples of poly(diacylhydrazine) obtained by polycondensing a dicarboxylic acid or a reactive derivative thereof (acid chloride or active ester derivative) with hydrazine or a dihydrazide of a dicarboxylic acid have been proposed (see, for example, Patent Documents 1 and 2).
[0004] Since this poly(diacylhydrazine) can be easily degraded by an oxidizing agent as described above, it can not only solve the waste problem of plastic products, but for example, if it is applied to an adhesive composition, the resulting adhesive composition can easily release the joined state by using an oxidizing agent, and if it is applied to a coating composition, it is expected to become a coating composition that can easily peel off the coating film by using an oxidizing agent. In particular, adhesive compositions containing poly(diacylhydrazine) have wide demand in applications such as temporary fixing of electronic components.
[0005] As described above, the property of poly(diacylhydrazine) being easily decomposed by oxidizing agents is expected to lead to various product developments. Incidentally, as described in Patent Documents 1 and 2, poly(diacylhydrazine) is not decomposed by radical oxidizing agents such as oxygen molecules, but is easily decomposed by oxidizing agents such as sodium hypochlorite. However, silicon-based semiconductors lose their function due to halide ions such as sodium hypochlorite, so there are challenges in applying these materials to temporary fixing applications. From this perspective, Patent Document 3 proposes a method of decomposing poly(diacylhydrazine) by treating it with nitrogen oxide gases such as nitrogen dioxide. In this way, diversifying the decomposition methods of poly(diacylhydrazine) makes it possible to broaden its range of applications. [Prior art documents] [Patent Documents]
[0006] [Patent Document 1] Japanese Patent Publication No. 2006-022315 [Patent Document 2] Japanese Patent Publication No. 2011-052075 [Patent Document 3] Japanese Patent Publication No. 2024-045015 [Overview of the project] [Problems that the invention aims to solve]
[0007] This invention has been made in view of the above circumstances, and aims to provide a new method for degrading polymers having an acylhydrazine skeleton, including poly(diacylhydrazine). [Means for solving the problem]
[0008] The inventors have conducted extensive research to solve the above problems and have found that a polymer compound having a divalent group represented by the following chemical formula (1), i.e., a polymer having an acylhydrazine skeleton, can be decomposed by reacting it with (a) a nitrite ester compound or a solution containing the same, or (b) a solution containing a nitrite and an acid. In the decomposition using nitrogen oxides described in Patent Document 3, the decomposition reaction of the polymer occurs when the nitrogen atom adjacent to the acyl group in the acylhydrazine skeleton is nitrosated. However, according to the inventors' research, it has been found that this nitrogen atom adjacent to the acyl group can also be nitrosated by nitrite ester compounds or nitrite produced by the reaction of nitrite and acid, resulting in a decomposition reaction of the polymer. The present invention is based on the above findings and provides the following.
[0009] (1) The present invention is a method for decomposing a polymer compound, characterized by comprising the step of contacting a polymer compound having a divalent group represented by the following chemical formula (1) with (a) a nitrite ester compound or a solution containing the same, or (b) a solution containing a nitrite and an acid. [ka] (In the above chemical formula (1), R represents a hydrogen atom or a monovalent organic group, and the wavy lines indicate bonds to other atoms.)
[0010] (2) The present invention also relates to a method for decomposing a polymer compound as described in item (1), wherein the polymer compound is at least one selected from the group consisting of a cured epoxy resin, a crosslinked vinyl polymer, a vinyl polymer, a polyamide, a polyester, a polyurethane, and a polycarbonate.
[0011] (3) The present invention also relates to a method for decomposing a polymer compound according to item (1) or (2), wherein the nitrite ester compound is isoamyl nitrite.
[0012] (4) The present invention further provides the method for decomposing a polymer compound according to any one of items (1) to (3), wherein the nitrite is an alkali metal salt of nitrous acid.
[0013] (5) The present invention further provides the method for decomposing a polymer compound according to any one of items (1) to (4), characterized in that dimethylacetamide is contained as a solvent constituting the solution containing the nitrite and the acid of the above (i).
[0014] (6) The present invention further provides the method for decomposing a polymer compound according to any one of items (1) to (5), characterized in that the contacting step is performed under heating.
[0015] (7) The present invention is also a decomposable adhesive composition characterized by comprising a polymer compound having a divalent group represented by the following chemical formula (1), and being decomposed by contact with (a) a nitrite ester compound or a solution containing the same, or (b) a solution containing a nitrite and an acid.
Chemical Formula
[0016] (8) The present invention also provides a method for separating a joined body, characterized in that, in the joined body bonded by the cured product of the decomposable adhesive composition according to item (7), the cured product is brought into contact with (a) a nitrite ester compound or a solution containing the same, or (b) a solution containing a nitrite and an acid.
[0017] (9) The present invention is also a decomposable coating composition characterized by comprising a polymer compound having a divalent group represented by the following chemical formula (1), and being decomposed by contact with (a) a nitrite ester compound or a solution containing the same, or (b) a solution containing a nitrite and an acid.
Chemical Formula
[0018] (10) The present invention is also a method for removing a coating film from a coated surface, which comprises bringing (a) a nitrite ester compound or a solution containing the same, or (b) a solution containing a nitrite and an acid, into contact with the coated surface provided with a coating film formed from the degradable coating composition according to item (9).
[0019] (11) The present invention is also a method for recovering fibers contained in fiber-reinforced plastics, which comprises bringing (a) a nitrite ester compound or a solution containing the same, or (b) a solution containing a nitrite and an acid, into contact with a fiber-reinforced plastic containing, as a matrix, a polymer compound having a divalent group represented by the following Chemical Formula (1), so as to decompose the matrix and separate and recover the fibers contained in the fiber-reinforced plastic. Advantageous Effects of Invention
[0020] According to the present invention, a new method for decomposing polymers having an acyl hydrazine skeleton, including poly(diacyl hydrazine), is provided. Brief Description of Drawings
[0021] [Figure 1] Figure 1 is the 1H-NMR spectrum of the reaction product obtained in Verification 1 using a model compound. [Figure 2] Figure 2 is the 1H-NMR spectrum of the water-insoluble fraction obtained in Verification 2 using a model compound. [Figure 3] Figure 3 is the 1H-NMR spectrum of the ethyl acetate extract obtained in Verification 2 using a model compound. Mode for Carrying Out the Invention
[0022] The following describes one embodiment of the present invention for decomposing polymer compounds, one embodiment of a degradable adhesive composition, one embodiment of a method for separating a bonded body using the same, one embodiment of a degradable coating composition, one embodiment of a method for removing a coating film using the same, and one embodiment of a method for recovering fibers contained in fiber-reinforced plastics. It should be noted that the present invention is not limited in any way to the following embodiments or models, and can be implemented with appropriate modifications within the scope of the present invention.
[0023] First, one embodiment of the polymer compound decomposition method of the present invention will be described. The polymer compound decomposition method of the present invention is characterized by comprising the step of contacting a polymer compound having a divalent group represented by the following chemical formula (1) with (a) a nitrite ester compound or a solution containing the same, or (b) a solution containing a nitrite and an acid. In the following chemical formula (1), the bonds indicated by the wavy line represent bonds to other atoms. Furthermore, a polymer compound "having a divalent group represented by the following chemical formula (1)" means a polymer compound whose molecule contains the structure represented by the following chemical formula (1). This polymer compound will also be referred to below as the "polymer compound to be decomposed" or simply as the "polymer compound".
[0024] [ka]
[0025] In the above chemical formula (1), R is a hydrogen atom or a monovalent organic group. Examples of such monovalent organic groups include alkyl groups, aryl groups, aralkyl groups, alkylaryl groups, cyano groups, alkylamino groups, acyl groups, heteroatoms to which alkyl or aryl groups are bonded, and carbon chains having 2 to 30 carbon atoms that may have one or more heteroatoms or unsaturated bonds in between, and may also have substituents. Examples of such heteroatoms include oxygen atoms, sulfur atoms, nitrogen atoms, etc.
[0026] When a polymer compound has the structure represented by the above chemical formula (1), it decomposes and becomes low molecular weight via the following chemical reaction upon contact with (a) a nitrite ester compound or a solution containing the same, or (b) a solution containing a nitrite and an acid. In the solution containing the nitrite and acid represented by (b), these react to produce nitrite (HNO2), and this nitrite contributes to the decomposition of the polymer compound. The reason for using (b) above instead of nitrite in this invention is that nitrite is extremely unstable in solution. In addition, in the following chemical reaction equation, R in the above chemical formula (1) is represented as a hydrogen atom for the sake of simplicity, but as mentioned above, R may also be a monovalent organic group. In this case, there is a possibility that a different decomposition reaction that produces other chemical species will proceed in the final stage of the series of chemical reactions without decomposing to an azide (N3-R''), but the CN bond in the above chemical formula (1) will be cleaved and the polymer compound will become low molecular weight.
[0027] [ka]
[0028] As shown in the chemical reaction equation above, a polymer compound having the structure represented by chemical formula (1) is nitrosated upon contact with (a) or (b) above. This nitrosation causes the portion enclosed by the dashed line to become a desirable leaving group. Water molecules present in the environment attack the carbonyl group adjacent to this leaving group, causing the leaving group to detach and the molecule to cleave. The detached compound is then converted to an azide through dehydration. Through these reactions, the polymer compound is decomposed and reduced in molecular weight. For such cleavage to occur, a nitrogen atom bonded to a C=O carbon atom is necessary, and furthermore, another nitrogen atom must be bonded next to this nitrogen atom. That is, the -C(=O)-NN- skeleton will produce this decomposition reaction, which is represented by chemical formula (1) above. For this reason, R in chemical formula (1) can be any group. Similarly, R' and R'' in the chemical reaction equation can also be any group. For example, the diacylhydrazine skeleton described in Patent Documents 1 to 3 above decomposes through a pathway similar to the chemical reaction equations described above, as shown in the following chemical reaction equation. In the case of the following chemical reaction equation as well, the portion enclosed by the dashed line becomes an excellent leaving group, and the carbonyl group adjacent to this leaving group is attacked by a water molecule, causing the leaving group to be removed and the molecule to be cleaved.
[0029] [ka]
[0030] The polymer compound to be decomposed is not particularly limited as long as it has the structure represented by the above chemical formula (1). Furthermore, the structure represented by the above chemical formula (1) may be included in the main chain as a repeating unit of the polymer compound, may be included in the side chain of the polymer compound, or may be included in a crosslinking structure that crosslinks polymer chains together. Examples of such polymer compounds include cured epoxy resins, crosslinked vinyl polymers, vinyl polymers, polyamides, polyesters, polyurethanes, polycarbonates, etc. Note that cured epoxy resins and crosslinked vinyl polymers, etc., may have multiple polymer chains crosslinked to form cured products with extremely large molecular weights. Strictly speaking, such cured products may not always be called polymer compounds, but in this invention, polymer compounds including such cured products are referred to as polymer compounds.
[0031] The cured epoxy resin is obtained by curing an epoxy resin containing a polyepoxy compound, a compound having multiple ring-opening functional groups that add to epoxy groups, and a curing catalyst such as an amine. The cured epoxy resin in the present invention has the structure represented by the above chemical formula (1) in its molecule. Such a cured epoxy resin can be obtained by using a compound having a divalent group represented by the above chemical formula (1) in its molecule as the compound having multiple ring-opening functional groups that add to epoxy groups. In the present invention, such a "compound having multiple ring-opening functional groups that add to epoxy groups and having a divalent group represented by the above chemical formula (1) in its molecule" is also called an "acylhydrazine skeleton crosslinking agent." In most epoxy resins, a bisphenol compound such as bisphenol A is used as the compound having multiple ring-opening functional groups that add to epoxy groups. For example, by using a compound obtained by the following synthesis route as such a bisphenol compound, the structure represented by the above chemical formula (1) can be introduced into the polymer compound which is the cured epoxy resin. These compounds are examples of the "crosslinking agents having an acylhydrazine skeleton" described above. Although four bisphenol compounds are given as examples below for illustrative purposes, the present invention is not limited to these.
[0032] [ka]
[0033] [ka]
[0034] To synthesize polyphenol compounds such as bisphenol compounds, as described above, a phenolic carboxylic acid hydrazide is synthesized, and then it is oxidatively condensed using an oxidizing agent such as bisacetoxyiodobenzene. Other examples of oxidizing agents that can be used here include potassium persulfate, potassium bisulfate and potassium sulfate double salts, bis(trifluoroacetoxy)iodobenzene, and iodosobenzene.
[0035] The bisphenol compound having a divalent group represented by the above chemical formula (1), obtained by the procedure described above, hardens by reacting with a polyepoxy compound in the presence of a base catalyst such as imidazole, for example, as shown below.
[0036] [ka]
[0037] As shown in the chemical reaction equation above, the main chain of the polymer compound that has reacted and hardened contains a divalent group represented by chemical formula (1) above. As already explained, contact with (a) or (b) above causes the bonds between CN to break, decomposing the compound and reducing its molecular weight. When the hardened product is reduced in molecular weight in this way, it becomes very brittle or soluble in the solvent used, making it easy to remove.
[0038] A crosslinked vinyl polymer can be obtained, for example, by radical polymerization of (A) a monomer having ethylenically unsaturated bonds and (B) a crosslinking agent having two or more ethylenically unsaturated bonds and a divalent group represented by the above chemical formula (1) in the molecule. Such a crosslinking agent can be obtained, for example, by reacting (meth)acryloyl chloride with hydrazine in the presence of a base, as shown in the chemical reaction equation below. In this specification, (meth)acryloyl means acryloyl and / or methacryloyl.
[0039] [ka]
[0040] The crosslinking agent obtained as described above is polymerized with a monomer having an ethylenically unsaturated bond (e.g., vinyl monomer) in the presence of a polymerization initiator such as azobisisobutyronitrile (AIBN), as shown in the chemical reaction equation below, to form a crosslinked vinyl polymer. This crosslinked polymer has a divalent group represented by the above chemical formula (1) in the crosslinked portion, and the crosslinked portion is cleaved upon contact with (a) or (b) above.
[0041] [ka]
[0042] Examples of monomers possessing ethylenically unsaturated bonds include ethylene, styrene, acrylic acid, acrylic acid esters, methacrylic acid esters, acrylamide, N-substituted acrylamide, N,N-disubstituted acrylamide, acrylonitrile, butadiene, vinyl acetate, and the like.
[0043] Furthermore, polymerization initiators include those that generate radicals upon heating, such as persulfates like sodium persulfate, potassium persulfate, and ammonium persulfate; peroxides like hydrogen peroxide, t-butyl peroxide, and methyl ethyl ketone peroxide; and azo compounds such as azonitrile compounds, azoamidine compounds, cyclic azoamidine compounds, azoamide compounds, alkylazo compounds, 2,2'-azobis(2-amidinopropane)dihydrochloride, and 2,2'-azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride.
[0044] The vinyl polymer in the present invention is a compound having the structure represented by the above chemical formula (1) in its main chain. Such a polymer can be obtained, for example, by radical polymerization of a bifunctional vinyl monomer having the structure represented by the above chemical formula (1) as described in the section on crosslinked vinyl polymers, with another vinyl monomer. A suitable chain transfer agent may be used in this process. Details of the method for obtaining such a polymer are given, for example, in Japanese Patent Application Publication No. 2024-143590.
[0045] The polyamide in the present invention is a compound having the structure represented by the above chemical formula (1) in its main chain. Examples of such polyamides include polydiacylhydrazine, polyhydrazide, and polyacyl semicarbazide. A suitable example of such polymer is, for example, the one described in Japanese Patent Application Publication No. 2006-22315.
[0046] The polyesters, polyurethanes, and polycarbonates in this invention are compounds having the structure represented by the above chemical formula (1) in their main chain. Such polymers are obtained by reacting a diol compound having the structure represented by the above chemical formula (1) with a polycarboxylic acid derivative, a diisocyanate compound, or a carbonate derivative. Although not particularly limited, the above-mentioned bisphenol compounds and the like can be preferably given as such diol compounds. In this invention, the term "diol compound" is not limited to alcohols, but broadly refers to a compound having two hydroxyl groups.
[0047] Next, we will explain what is represented by (a) or (b) above, namely (a) nitrite ester compounds or solutions containing them, or (b) solutions containing nitrites and acids. These initiate the cleavage reaction described above by nitrosating the nitrogen atom contained in the chemical formula represented by chemical formula (1) above.
[0048] The nitrite ester compound of (a) is a dehydration condensate of nitrite and an alcohol, and is represented by the general formula RON=O. In this general formula, R is preferably an alkyl group, an aryl group, etc., with alkyl groups being more preferred among these. A particularly preferred example in the present invention is isoamyl nitrite, but is not limited to this. If the nitrite ester compound is in liquid form, it may be brought into direct contact with the polymer compound to be decomposed, or it may be dissolved in a solvent before contact as needed. If it is in solid form, it may be dissolved in a solvent before contact. In this case, organic solvents are preferred, with tetrahydrofuran being more preferred.
[0049] In principle, the amount of nitrite ester compound used in the decomposition reaction should be 1 equivalent relative to the portion represented by chemical formula (1) in the polymer to be decomposed. However, in practice, it is preferable to use a large excess amount relative to the portion represented by chemical formula (1) in the polymer to be decomposed. As an example of the temperature in the decomposition reaction, room temperature to about 150°C can be used.
[0050] As previously mentioned, the solution containing the nitrite and acid in (i) contributes to the decomposition of the polymer compound as nitrite produced by their reaction. The nitrite is not particularly limited as long as it is a salt of nitrite and a metal, and examples of such metals include alkali metals and alkaline earth metals. Among these, salts of nitrite and alkali metals are preferred, and sodium nitrite is more preferred. In principle, the amount of nitrite used in the decomposition reaction is 1 equivalent relative to the portion represented by chemical formula (1) in the polymer to be decomposed, but in practice, it is preferable to use a large excess relative to the portion represented by chemical formula (1) in the polymer to be decomposed.
[0051] Examples of acids include inorganic acids and organic acids, with organic acids being preferred. Examples of such organic acids include carboxylic acid compounds and sulfonic acid compounds. Among these, p-toluenesulfonic acid is a particularly preferred acid. The amount of acid used in the decomposition reaction is preferably about 1 to 3 equivalents relative to the nitrite.
[0052] The solvent is not particularly limited as long as it can dissolve the above-mentioned nitrite and acid, but it is preferable that it also has some degree of solubility for the polymer compound to be decomposed. From this viewpoint, a mixed solvent of an organic solvent and water, such as a highly polar protic solvent or aprotic solvent, is preferred. Preferred organic solvents include dimethylformamide, dimethylacetamide, acetonitrile, and dimethyl sulfoxide, with dimethylacetamide being more preferred. The mixing ratio of the organic solvent to water is preferably about 1:1 by volume, but is not particularly limited.
[0053] When carrying out the decomposition reaction using (i) above, it is preferable to do so under heating. In this case, the temperature is preferably around 40 to 150°C, more preferably around 40 to 100°C, and particularly preferably around 60°C.
[0054] The polymer compounds that are decomposed by contact with (a) or (b) above become very brittle or soluble in the solvent used, making them easily removable. Therefore, if the polymer compound was used as an adhesive, it can be easily removed from the bonded object, and if it formed a coating, it can be easily removed from the painted surface.
[0055] <Degradable adhesive composition> Next, the biodegradable adhesive composition of the present invention will be described. The biodegradable adhesive composition of the present invention is characterized by containing a polymer compound having a divalent group represented by the following chemical formula (1), and is characterized by decomposition by contact with (a) a nitrite ester compound or a solution containing the same, or (b) a solution containing a nitrite and an acid. In chemical formula (1), R is a hydrogen atom or a monovalent organic group, and the bonds indicated by the wavy line represent bonds to other atoms. This has been explained in the above-mentioned method for decomposing polymer compounds, so an explanation will be omitted here.
[0056] [ka]
[0057] In other words, the biodegradable adhesive composition of the present invention contains the polymer compound described in the above-mentioned method for decomposing the polymer compound of the present invention. Therefore, the cured product formed with this adhesive composition contains the above-mentioned polymer compound and decomposes and becomes low molecular weight when brought into contact with (a) or (b) above. The decomposed and low molecular weight cured product has already lost its robustness as a cured product and becomes very brittle or soluble in the solvent used, so it can be easily removed. As for (a) or (b) above, they are as described in the above-mentioned method for decomposing the polymer compound, so their explanation is omitted here.
[0058] The biodegradable adhesive composition of the present invention may be a composition of the type that comprises the above polymer compound and a solvent, and the polymer compound hardens upon evaporation of the solvent, or it may be a composition of the type that comprises a precursor of the above polymer compound and hardens through a chemical reaction. Examples of the latter type of composition include a so-called epoxy adhesive composition comprising a polyepoxy compound, a crosslinking agent having the above acylhydrazine skeleton, and a curing catalyst such as an amine, and a vinyl adhesive composition comprising (A) a monomer having an ethylenically unsaturated bond, (B) a crosslinking agent having two or more ethylenically unsaturated bonds and a divalent group represented by the above chemical formula (1) in the molecule, and (C) a polymerization initiator. However, the biodegradable adhesive composition of the present invention is not limited to these.
[0059] The epoxy adhesive composition comprises a polyepoxy compound, a crosslinking agent having the acylhydrazine skeleton described above, and a curing catalyst such as an amine, and yields a polymer compound having a divalent group represented by the above chemical formula (1) as a cured product. As for the polyepoxy compound, there are many commercially available products for epoxy adhesive composition applications, so they can be obtained and used. As for the crosslinking agent having the acylhydrazine skeleton, a bisphenol compound having a divalent group represented by the above chemical formula (1), as already described, can be preferably mentioned. As for the amine compound as a curing catalyst, imidazole can be preferably mentioned. As already described, these components react to give a cured product that is a polymer compound having a divalent group represented by the above chemical formula (1), and that it decomposes when it comes into contact with (a) or (b) above, so the explanation is omitted here.
[0060] The vinyl adhesive composition comprises (A) a monomer having an ethylenically unsaturated bond, (B) a crosslinking agent having two or more ethylenically unsaturated bonds and a divalent group represented by the above chemical formula (1) in the molecule, and (C) a polymerization initiator, and the cured product yields a polymer compound having a divalent group represented by the above chemical formula (1). As has already been described in the description of the crosslinked vinyl polymer above, the explanation of each of these components is omitted here. Furthermore, as has already been described, this cured product has the structure represented by the above chemical formula (1) and decomposes when it comes into contact with (a) or (b) above.
[0061] <Method for disassembling the joint> In a joint bonded with the cured product of the above-mentioned biodegradable adhesive composition, a method for separating the joint, characterized by contacting the cured product with (a) a nitrite ester compound or a solution containing the same, or (b) a solution containing a nitrite and an acid, is also part of the present invention. As this has already been described in the description of the above-mentioned biodegradable adhesive composition, a further explanation is omitted here.
[0062] <Degradable paint composition> Next, the biodegradable adhesive composition of the present invention will be described. The biodegradable coating composition of the present invention is characterized by containing a polymer compound having a divalent group represented by the following chemical formula (1), and its coating film is characterized by decomposition upon contact with (a) a nitrite ester compound or a solution containing the same, or (b) a solution containing a nitrite and an acid. In chemical formula (1), R is a hydrogen atom or a monovalent organic group, and the wavy line indicates a bond to another atom. This has been explained in the description of the decomposition method of the polymer compound above, so the explanation will be omitted here.
[0063] [ka]
[0064] The biodegradable coating composition of the present invention comprises the above-mentioned polymer compound as a binder, a pigment, and a solvent. As the solvent evaporates, the polymer compound forms a film and creates a coating. As previously explained, this polymer compound decomposes and becomes low molecular weight upon contact with (a) or (b) above.
[0065] <Method for removing paint film from painted surfaces> Another method of removing a coating film from a painted surface, characterized by contacting the painted surface with (a) a nitrite ester compound or a solution containing the same, or (b) a solution containing a nitrite and an acid, is also part of the present invention. This has already been described in the description of the biodegradable adhesive composition, so a further explanation is omitted here.
[0066] <Method for recovering fibers contained in fiber-reinforced plastics> Next, a method for recovering fibers contained in the fiber-reinforced plastic of the present invention will be described. The method for recovering fibers contained in the fiber-reinforced plastic of the present invention is characterized by decomposing the matrix of a fiber-reinforced plastic containing a polymer compound having a divalent group represented by the following chemical formula (1) by contacting it with (a) a nitrite ester compound or a solution containing the same, or (b) a solution containing a nitrite and an acid, and separating and recovering the fibers contained in the fiber-reinforced plastic. In chemical formula (1), R is a hydrogen atom or a monovalent organic group, and the bonds indicated by the wavy line represent bonds to other atoms. This has been explained in the above-mentioned method for decomposing polymer compounds, so an explanation will be omitted here.
[0067] [ka]
[0068] Fiber-reinforced plastics (hereinafter also called FRP) are composite materials that enhance the strength of plastics, which are lightweight but have a low modulus of elasticity and low strength, by combining them with reinforcing materials such as glass fibers and carbon fibers, which have a high modulus of elasticity and high tensile strength. Because they exhibit good mechanical properties, they are used in a wide range of fields, including transportation equipment, housing equipment, swimming pools, and building materials. In particular, carbon fiber reinforced plastics (hereinafter also called CFRP), which use carbon fibers as a reinforcing material, are said to be lightweight and have strength comparable to steel, and are widely used as a material to replace steel plates that have been conventionally used in automobiles and aircraft.
[0069] However, due to its excellent durability and strength, FRP tends to create waste disposal problems. Furthermore, while the carbon fibers used in CFRP exhibit excellent properties, they are very expensive. If carbon fibers could be recovered and reused from discarded CFRP, it would be extremely useful from both an environmental and cost perspective. This invention addresses these needs by contacting FRP containing a polymer compound with a divalent group represented by the above chemical formula (1) as a matrix with (a) or (b) above, thereby decomposing the polymer compound matrix and reducing its molecular weight. Since the low molecular weight matrix can be easily disintegrated, it becomes possible to easily extract the fibers contained within the matrix.
[0070] FRP (Fiber Reinforced Plastic) is generally made by impregnating fibers such as glass fibers or carbon fibers with a matrix material, molding it into a desired shape, and then hardening it. Examples of such fibers include glass fibers, carbon fibers, and aramid fibers, with carbon fibers being particularly preferred among them. Examples of these fibers include unidirectional materials in which the fibers are aligned in one direction, woven fabrics such as plain weave, twill weave, and satin weave, and nonwoven fabrics.
[0071] The polymer compound constituting the matrix is not limited as long as it has a divalent group represented by the above chemical formula (1). Preferred examples of such polymer compounds include cured epoxy resins and crosslinked vinyl polymers. FRP using these as the matrix exhibits sufficient durability during use, while the matrix can be easily removed after use by contacting it with (a) or (b) above.
[0072] The cured epoxy resin is obtained by curing an epoxy resin containing a polyepoxy compound, a compound having multiple ring-opening functional groups added to epoxy groups, and a curing catalyst such as an amine. This uncured epoxy resin is impregnated into the aforementioned fibers, and then the epoxy resin is cured to produce FRP.
[0073] For example, in conventional epoxy resins, bisphenol compounds such as bisphenol A are used as compounds having multiple functional groups that undergo ring-opening addition to epoxy groups. It is preferable to introduce a divalent group represented by the above chemical formula (1) into the molecule of such a bisphenol compound. As for such a compound having multiple functional groups that undergo ring-opening addition to epoxy groups, i.e., a crosslinking agent having a diacylhydrazine skeleton, those described in the above explanation of the polymer compound decomposition method of the present invention can be used.
[0074] A crosslinked vinyl polymer is obtained by radical polymerization of (A) a monomer having ethylenically unsaturated bonds and (B) a crosslinking agent having two or more ethylenically unsaturated bonds and a divalent group represented by the above chemical formula (1) within the molecule. A liquid polymerizable composition is prepared by mixing (A) and (B) with a radical polymerization initiator, and this polymerizable composition is impregnated into fibers. The polymerizable composition is then heated to cure it, resulting in FRP. The (A), (B) and radical polymerization initiator can be those described in the above explanation of the polymer compound decomposition method of the present invention. [Examples]
[0075] The present invention will be described in more detail below with reference to examples, but the present invention is not limited in any way to the following examples.
[0076] • Synthesis of model compounds (compounds containing a divalent group represented by the above chemical formula (1)) [ka]
[0077] 0.2044 g, 4.300 mmol of hydrazine monohydrate and 24 mL of an aqueous solution of sodium bicarbonate (2.033 g, 24.19 mmol) were added to a 50 mL round-bottom flask. At 0°C, a solution of 4-methoxybenzoyl chloride (2.067 g, 12.16 mmol) in tetrahydrofuran (THF, 12 mL) was added dropwise, and the mixture was stirred at room temperature for 1 hour. The resulting precipitate was filtered and vacuum-dried to obtain a white solid of diacylhydrazine 1 (yield 1.074 g, yield 89%). This diacylhydrazine 1 is a compound possessing a divalent group represented by the above chemical formula (1), and the effects of the present invention were verified using this as a model compound. In the above chemical reaction equation, the group represented by "Me" is a methyl group. This is the same hereafter.
[0078] • Verification using model compounds 1 (decomposition by isoamyl nitrite) [ka]
[0079] Diacylhydrazine 1 (0.0614 g, 0.204 mmol) and isoamyl nitrite (i-AmONO, 4.0 mL, 30.07 mmol) were added to a 10 mL two-necked round-bottom flask and refluxed for 1 hour. Volatile components were removed by distillation under reduced pressure to obtain 0.0518 g of the reaction product.
[0080] The reactants obtained 1The 1H-NMR spectrum (400 MHz, DMSO-d6) is shown in Figure 1. As shown in Figure 1, diacylhydrazine 1 was almost completely decomposed (signals a, b), and signals for carboxylic acid 2 (signals c, d) and acyl azide 3 (signals e, f) were observed as decomposition products. In addition, the IR spectrum showed 2135 cm⁻¹. -1 A characteristic absorption of acyl azide was observed. From these findings, it can be understood that diacylhydrazine 1, represented by the above chemical formula (1) and possessing a divalent group, reacted with the nitrite ester and was cleaved at the CN bond site, resulting in decomposition. In this decomposition reaction, equimolar products of carboxylic acid 2 and acyl azide 3 should be produced, but in Figure 1... 1 The 1H-NMR spectrum showed that more carboxylic acid 2 (signals c, d) was produced than acyl azide 3 (signals e, f). This is thought to be because acyl azide 3 was hydrolyzed and broken down into carboxylic acid 2.
[0081] • Verification using model compounds 2 (decomposition by nitrites and acids) [ka]
[0082] In a 10 mL round-bottom flask, 1 mL of a mixed solvent of dimethylacetamide (DMAc) and water (volume ratio 1:1), diacylhydrazine 1 (0.1514 g, 0.506 mmol), sodium nitrite (0.0705 g, 1.02 mmol), and p-toluenesulfonic acid monohydrate (0.3842 g, 2.20 mmol) were added, and the mixture was stirred at 60°C for 1 hour. The reaction mixture was poured into 40 mL of water, and the insoluble portion was filtered off to obtain 0.1001 g of a white solid. The filtrate was extracted three times with ethyl acetate (30 mL), the organic layer was washed with saturated sodium chloride aqueous solution, dried over magnesium sulfate, and the solvent was removed by vacuum distillation to obtain 0.058 g of the reaction product. Thus, the reaction product obtained consisted of 0.1001 g of water-insoluble portion and 0.058 g of ethyl acetate extract.
[0083] The water-insoluble portion obtained 1 Figure 2 shows the H-NMR spectrum (400 MHz, DMSO-d6) of the ethyl acetate extract.1 The 1H-NMR spectra (400 MHz, DMSO-d6) are shown in Figure 3. As shown in Figures 2 and 3, no signal for diacylhydrazine 1 (signals a, b) was observed, confirming that diacylhydrazine 1 was completely decomposed. On the other hand, as shown in Figures 2 and 3, signals for carboxylic acid 2 (signals c, d) and acyl azide 3 (signals e, f) were observed as decomposition products. In addition, for the ethyl acetate extract, a signal for amide 6 (signals g, h, i) was also observed, as shown in Figure 3. It was presumed that this amide 6 was produced by the elimination of nitrous oxide from the reaction intermediate.
[0084] Verification using the above model compounds suggests that compounds with a divalent group represented by chemical formula (1) undergo cleavage of their CN bond and subsequent reduction in molecular weight upon contact with a mixture of nitrite esters, nitrites, and acids.
[0085] • Synthesis of Polydiacylhydrazine 9 1 [ka]
[0086] A 10 mL solution of hydrazide 7 (2.503 g, 10.00 mmol) in dimethyl sulfoxide (DMF) was placed in a 50 mL round-bottom flask. Terephthalate chloride 8 (2.030 g, 10.00 mmol) was added all at once, the flask was stoppered, and the mixture was stirred at room temperature for 1 hour. 30 mL of DMF was added and then added dropwise to 400 mL of methanol with vigorous stirring. The resulting precipitate was filtered, washed with methanol, and vacuum-dried to obtain a white powder of polydiacylhydrazine 9 (yield 3.900 g, 95%).
[0087] • Decomposition of Polydiacylhydrazine 9 1 Sodium nitrite (0.7 g, 10 mmol) and p-toluenesulfonic acid monohydrate (3.0 g, 16 mmol) were placed in a 100 mL beaker and dissolved in 10 mL of a mixed solvent of DMAc and water (volume ratio 1:1). Polydiacylhydrazine 9 powder was dispersed in this solution and heated at 60°C, where it completely dissolved in 10 minutes.
[0088] • Synthesis of Polydiacylhydrazine 9 2 A 2 mL solution of hydrazide 7 (308.4 mg, 1.232 mmol) in DMF (2 mL) was placed in a 25 mL sample tube, and terephthalate chloride 8 (250.1 mg, 1.232 mmol) was added all at once. The tube was then capped and stirred at room temperature for 1 hour. This solution was spread onto a glass slide, heated to 140 °C to evaporate the solvent, and a polydiacylhydrazine 9 film was prepared.
[0089] • Decomposition of Polydiacylhydrazine 9 2 Sodium nitrite (0.7g, 10 mmol) and p-toluenesulfonic acid monohydrate (3.0g, 16 mmol) were placed in a 100 mL beaker and dissolved in 20 mL of a mixed solvent of DMAc and water (volume ratio 1:1). A film of polydiacylhydrazine 9 was placed in this solution and heated at 60°C, where it completely dissolved in 20 minutes.
[0090] • Preparation of cured epoxy resin products [ka]
[0091] Bisphenol 10 (5.43 g, 9.29 mmol) and bisphenol A type epoxy resin 11 (epoxy equivalent 187 g / eq, 3.47 g, epoxy 18.56 meq) were placed in a stainless steel beaker and heated to 150°C and stirred to obtain a homogeneous solution. Imidazole (0.12 g, 1.76 mmol) was added to this and stirred, then the solution was spread onto a glass slide, another glass slide was placed on top, a 100 g weight was placed on top, and the mixture was heated on a hot plate at 150°C for 3 hours to obtain a glass bond. In other words, this bond was formed by curing epoxy resin.
[0092] • Decomposition of hardened epoxy resin Sodium nitrite (0.7 g, 10 mmol) and p-toluenesulfonic acid monohydrate (3.0 g, 16 mmol) were placed in a 100 mL beaker and dissolved in 100 mL of a mixed solvent of DMAc and water (volume ratio 1:1). The above-mentioned glass bonded with bisphenol A type epoxy resin 11 cured with bisphenol 10 was placed in this solution and heated at 60°C, where it spontaneously peeled off after 20 hours.
[0093] • Synthesis of superabsorbent polymer 13 (vinyl polymer) [ka]
[0094] Acrylic acid (20 g, 0.28 mol), crosslinking agent 12 having a diacylhydrazine structure (0.4 g, 3 mmol), NaOH (17 g, 0.43 mol), and 4,4'-azobis(4-cyanovaleric acid) (V-501; 1.5 g, 5.4 mmol) were added and dissolved in 200 mL of water. The mixture was degassed by blowing argon over it for 30 minutes. This mixture was placed in a sealed bag and heated at 80°C for 48 hours. After decanting the resulting gel with water, it was added to 3 L of methanol while vigorously stirring with a mechanical stirrer. The resulting solid was filtered and vacuum-dried to obtain a white solid superabsorbent polymer 13 (19 g, yield 95%).
[0095] • Decomposition of superabsorbent polymer 13 (vinyl polymer) 0.01 g of superabsorbent polymer 13 was placed in a 50 mL beaker, and 10 mL of water was added to form a swollen gel. 1 mL of a solution prepared by dissolving sodium nitrite (0.7 g, 10 mmol) and p-toluenesulfonic acid monohydrate (3.0 g, 16 mmol) in 100 mL of water was added, and the mixture was heated to 60°C. A homogeneous aqueous solution was obtained in 5 minutes.
[0096] Preparation of CFRP (vinyl crosslinked material 14) [ka]
[0097] A monomer mixture was prepared by mixing N,N-dimethylacrylamide, a crosslinking agent 12 having a diacylhydrazine structure, and AIBN in a molar ratio of 95:5:2. A mold was made from a 1 mm thick polytetrafluoroethylene (PTFE) sheet, and a carbon fiber sheet was laid in the mold. This was then covered and fixed with a PTFE sheet. The monomer mixture was poured into the mold to impregnate the carbon fiber sheet, and then sealed by vacuum degassing. This was placed in a constant temperature bath and heated at 40°C for one day, then heated at 100°C for 3 hours to prepare CFRP (i.e., vinyl crosslinked material 14). The CFRP was removed and washed with diethyl ether.
[0098] • Decomposition of the vinyl crosslinked material 14 Sodium nitrite (0.7 g, 10 mmol) and p-toluenesulfonic acid monohydrate (3.0 g, 16 mmol) were placed in a 100 mL beaker and dissolved in 100 mL of a mixed solvent of DMAc and water (volume ratio 1:1). The CFRP obtained by the above procedure was wrapped in a polyester net and suspended in the above solution and heated at 60°C. The CFRP matrix (vinyl crosslinked material 14) disappeared, leaving only the carbon fiber sheet.
[0099] • Synthesis of polystyrene-15 [ka]
[0100] Styrene (105 mg, 1.01 mmol), crosslinking agent 12 with a diacylhydrazine structure (14 mg, 0.10 mmol), azobisisobutyronitrile (AIBN; 10 mg, 0.06 mmol), and DMAc (0.5 mL) were added to an 8φ glass tube with a rounded bottom and homogeneously dissolved. This solution was frozen with liquid nitrogen and then thawed in a vacuum three times to remove air, before being sealed and heated at 65°C for 48 hours. The sealed tube was opened, methylene chloride was added to separate the insoluble portion by filtration, and the filtrate was added dropwise to 100 mL of methanol with vigorous stirring. The precipitate was filtered, washed with methanol, and then vacuum dried to obtain a white powder of polystyrene 15 (77 mg, yield 73%) with diacylhydrazine introduced into the main chain.
[0101] • Decomposition of polystyrene 15 When polystyrene-15 powder, with diacylhydrazine introduced into the main chain, was dispersed in isoamyl nitrite (4.0 mL, 30 mmol) and refluxed for 1 hour, it completely dissolved.
Claims
1. A method for decomposing a polymer compound, characterized by comprising the step of contacting a polymer compound having a divalent group represented by the following chemical formula (1) with (a) a nitrite ester compound or a solution containing the same, or (b) a solution containing a nitrite and an acid. 【Chemistry 1】 (In the above chemical formula (1), R is a hydrogen atom or a monovalent organic group, and the wavy lines indicate bonds to other atoms.)
2. The method for decomposing a polymer compound according to claim 1, wherein the polymer compound is at least one selected from the group consisting of a cured epoxy resin, a crosslinked vinyl polymer, a vinyl polymer, a polyamide, a polyester, a polyurethane, and a polycarbonate.
3. The method for decomposing a polymer compound according to claim 1, wherein the nitrite ester compound is isoamyl nitrite.
4. The method for decomposing a polymer compound according to claim 1, wherein the nitrite is an alkali metal salt of nitrite.
5. The method for decomposing a polymer compound according to claim 1, characterized in that the solution comprising the nitrite and acid described above (i) contains dimethylacetamide as the solvent.
6. The method for decomposing a polymer compound according to claim 1, characterized in that the contact step is performed under heating.
7. A biodegradable adhesive composition characterized by containing a polymer compound having a divalent group represented by the following chemical formula (1), and decomposing upon contact with (a) a nitrite ester compound or a solution containing the same, or (b) a solution containing a nitrite and an acid. 【Chemistry 2】 (In the above chemical formula (1), R is a hydrogen atom or a monovalent organic group, and the wavy lines indicate bonds to other atoms.)
8. A method for separating a bonded body, characterized in that the bonded body is bonded with a cured product of the biodegradable adhesive composition described in claim 7, and the cured product is brought into contact with (a) a nitrite ester compound or a solution containing the same, or (b) a solution containing a nitrite and an acid.
9. A biodegradable paint composition characterized by containing a polymer compound having a divalent group represented by the following chemical formula (1), and decomposing by contact with (a) a nitrite ester compound or a solution containing the same, or (b) a solution containing a nitrite and an acid. 【Transformation 3】 (In the above chemical formula (1), R is a hydrogen atom or a monovalent organic group, and the wavy lines indicate bonds to other atoms.)
10. A method for removing a coating film from a painted surface, characterized by contacting the painted surface having a coating film formed with the degradable coating composition described in claim 9 with (a) a nitrite ester compound or a solution containing the same, or (b) a solution containing a nitrite and an acid.
11. A method for recovering fibers contained in fiber-reinforced plastic, characterized by contacting a fiber-reinforced plastic containing a polymer compound having a divalent group represented by the following chemical formula (1) as a matrix with (a) a nitrite ester compound or a solution containing the same, or (b) a solution containing a nitrite and an acid, to decompose the matrix and separate and recover the fibers contained in the fiber-reinforced plastic. 【Chemistry 4】 (In the above chemical formula (1), R is a hydrogen atom or a monovalent organic group, and the wavy lines indicate bonds to other atoms.)
Citation Information
Patent Citations
Degradable polyamide
JP2006022315A
Method for producing poly(diacylhydrazine) and poly(diacylhydrazine)
JP2011052075A
Method for decomposing polymer compound, decomposable adhesive composition and method for separating joint body using the same, decomposable coating composition and method for removing coating layer using the same, and method for recovering fiber included in fiber-reinforced plastic
JP2024045015A