Freestanding film for dry electrode, its manufacturing method, dry electrode including same, and secondary battery
A free-standing film for dry electrodes using PTFE supported by Ox-VGCF addresses uneven solvent evaporation issues, ensuring uniform dispersion and improved electrode quality, thus enhancing battery performance.
Patent Information
- Application Number
- JP2022554708
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-01-10
- Filing Date
- 2022-01-13
- Publication Date
- 2024-09-17
- Estimated Expiration
- 2042-01-13
AI Technical Summary
The manufacturing process of lithium secondary batteries often results in defects such as pinholes and cracks in the electrode active layer due to uneven solvent evaporation, leading to poor electrode quality and increased production costs, especially in thick film coatings.
A free-standing film for dry electrodes is developed using a binder containing fibrous polymer, specifically polytetrafluoroethylene (PTFE), supported by oxidized vapor grown carbon fibers (Ox-VGCF) to ensure uniform dispersion and formation of a conductive network, avoiding shearing forces during mixing.
The solution enables uniform dispersion of PTFE primary particles, enhancing the binding efficiency and forming a robust conductive network, resulting in improved electrode properties and battery performance.
Smart Images

Figure 0007551208000002 
Figure 0007551208000003 
Figure 0007551208000004
Abstract
Description
[Technical field]
[0001] Cross-reference to related applications This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0011774 filed on January 27, 2021, and Korean Patent Application No. 10-2022-0003420 filed on January 10, 2022, and all contents disclosed in the documents of said Korean patent applications are incorporated herein by reference.
[0002] The present invention relates to a freestanding film for a dry electrode, a method for producing the same, and a dry electrode and a secondary battery including the same. [Background technology]
[0003] The rapid increase in the use of fossil fuels has led to an increased demand for alternative and clean energy, and one of the most actively researched fields in this area is the field of electrochemical power generation and storage.
[0004] At present, a representative example of an electrochemical element that uses such electrochemical energy is a secondary battery, and the range of its use is gradually expanding.
[0005] Lithium secondary batteries, which are representative of such secondary batteries, are not only used as an energy source for mobile devices, but are also being used as a power source for electric vehicles and hybrid electric vehicles that can replace vehicles that use fossil fuels such as gasoline vehicles and diesel vehicles, which are one of the main causes of air pollution, and their range of use is expanding to include auxiliary power sources through grid connection.
[0006] The manufacturing process of such lithium secondary batteries is roughly divided into three stages: electrode process, assembly process, and chemical formation process. The electrode process is further divided into active material mixing process, electrode coating process, drying process, rolling process, slitting process, winding process, etc.
[0007] Among these, the active material mixing process is a process of blending a coating material for forming an electrode active layer where an electrochemical reaction actually occurs in the electrode. In detail, the active material, which is an essential element of the electrode, and other additives such as a conductive material and a filler, a binder for binding between particles and adhering to the current collector, and a solvent for imparting viscosity and dispersing particles are mixed to prepare a slurry having fluidity.
[0008] The composition mixed for forming the electrode active layer in this manner may be broadly referred to as an electrode mixture.
[0009] Thereafter, an electrode coating process is performed in which the electrode mixture is applied onto an electrically conductive current collector, and a drying process is performed in which the solvent contained in the electrode mixture is removed. The electrode is then rolled to a predetermined thickness.
[0010] Meanwhile, as the solvent contained in the electrode mixture evaporates during the drying process, defects such as pinholes and cracks may be induced in the already formed electrode active layer. In addition, the inside and outside of the active layer may not be dried uniformly, and particle floating phenomenon due to the difference in solvent evaporation speed, that is, particles in the area that is dried first may float up and form gaps with the area that is dried later, resulting in deterioration of electrode quality. In particular, in the case of thick film coating, it takes more time to evaporate the solvent during electrode drying, and the floating phenomenon of the relatively light conductive material and binder intensifies, which is a fatal disadvantage in that it is difficult to manufacture high-quality electrodes.
[0011] In order to solve the above problems, drying devices capable of controlling the evaporation rate of the solvent while uniformly drying the inside and outside of the active layer have been considered. However, such drying devices are very expensive and require considerable cost and time to operate, which is disadvantageous in terms of manufacturing process.
[0012] Therefore, recently, active research has been conducted into the production of dry electrodes that do not use solvents.
[0013] The dry electrode is generally prepared by laminating a free-standing film, which is prepared in the form of a film and contains an active material, a binder, a conductive material, etc., on a current collector.
[0014] Therefore, the dry electrode is in the spotlight as an innovative technology that can manufacture thick-film electrodes, does not require the use of organic solvents that are harmful to the human body, and can simultaneously solve problems such as high process costs due to long drying times.
[0015] Meanwhile, polytetrafluoroethylene (PTFE) powder is mainly used as a binder when manufacturing such dry electrodes. This PTFE has long fibrous structures with an atomic arrangement of (-CF2-CF2)n neatly aligned inside primary particles with a diameter of less than several hundred nm, and when it receives shear force under certain conditions, it is pulled out into long fibers, and these PTFE nanofibers connect the active material and conductive material like a rope to maintain the shape of the electrode.
[0016] However, the PTFE is easily fiberized even with a very small shear force at room temperature (above 19°C), and has a fatal drawback of coagulating with surrounding PTFE particles even with slight movement.
[0017] Therefore, in such dry electrodes, the key is a technology that can uniformly disperse PTFE primary particles under process conditions where no shear force is applied, so there is an urgent need to develop a technology that can realize an electrode by binding active material through fiberization even with only a small amount of PTFE. Summary of the Invention [Problem to be solved by the invention]
[0018] The present invention has been made to solve the above problems, and aims to provide a free-standing film that can improve battery performance by enabling uniform dispersion of PTFE primary particles, thereby increasing the efficiency of PTFE binder application, and by firmly forming a conductive network, and a manufacturing method thereof.
[0019] Another object of the present invention is to provide a dry electrode including the free-standing film, and a secondary battery including the same. [Means for solving the problem]
[0020] A freestanding film according to one embodiment of the present invention is a freestanding film for a dry electrode, and includes an active material, a binder including a fiberized polymer, and a support, and the support is a surface-oxidized carbon fiber (Ox-VGCF).
[0021] Here, the fiberizing polymer is fiberized to bind the active material and the carrier.
[0022] In one specific example, the support may be a carbon fiber having surface oxygen functional groups increased by a surface oxidation treatment, and the support may contain 5 to 15 wt % of surface oxygen functional groups based on the total weight of the support.
[0023] The support may have an average diameter of 50 nm to 500 nm, an average length of 1 μm to 30 μm, and a specific surface area of 10 m 2 / g~150m 2 / g.
[0024] Furthermore, the graphitization degree (ID / IG ratio) of the support may be 0.1 to 2.0.
[0025] In one specific example, the support may be included in an amount of 0.1 wt % to 10 wt % based on the total weight of the freestanding film.
[0026] In one specific example, the fiberizing polymer may be polytetrafluoroethylene (PTFE).
[0027] According to another embodiment of the present invention, the method for producing the free-standing film includes: (a) mixing a binder containing a fiberizing polymer and a support to obtain a mixture; (b) mixing the mixture with an active material and subjecting the mixture to high shear mixing to obtain a fiberizing composition; and (c) forming the fiberizing composition into a film shape; wherein the support is a carbon fiber that has been surface-oxidized (Oxidized Vapour Grown Carbon Fibers).
[0028] Here, the fiberizable polymer may be polytetrafluoroethylene (PTFE).
[0029] In one specific example, the mixing in step (a) can be performed by simply mixing the binder containing the fiberizing polymer and the carrier at 19° C. or less, or by feeding the mixture of the binder containing the fiberizing polymer and the carrier together into a grinder after the mixing.
[0030] Here, the pulverizer may be an air jet mill.
[0031] In this case, the mixture may have a structure in which the primary particles of the fiberizing polymer are uniformly dispersed and supported on the surface of a support.
[0032] In one specific example, the high shear mixing in step (b) can be carried out at a speed ranging from 10 rpm to 500 rpm for 1 minute to 30 minutes.
[0033] In one specific example, the forming in step (c) can be performed by hot rolling using a calendar.
[0034] Meanwhile, a dry electrode according to another embodiment of the present invention includes a current collector, and the free-standing film formed on the current collector, and the current collector has a structure in which a primer layer is coated on a metal foil.
[0035] In addition, according to one embodiment of the present invention, there is provided a secondary battery in which an electrode assembly including the dry electrode, a counter electrode, and a separator is housed in a battery case together with a lithium-containing non-aqueous electrolyte. [Brief description of the drawings]
[0036] [Figure 1] 13 is an SEM image of a reference example. [Diagram 2] 1 is an SEM image of Production Example 1 of the present invention. [Diagram 3] 1 is an SEM image of the fiberization composition according to Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0037] The present invention will now be described in further detail to aid in the understanding of the present invention.
[0038] The terms and words used in this specification and the claims should not be interpreted in a limited manner to their ordinary or dictionary meanings, but should be interpreted in a manner that corresponds to the technical idea of the present invention based on the principle that the inventor can appropriately define the concept of the term in order to best describe his / her invention.
[0039] The terms used in this specification are merely used to describe exemplary embodiments and are not intended to limit the present invention. The singular form includes the plural form unless otherwise clearly indicated in the context.
[0040] In addition, throughout the specification, when a part is said to "comprise" a certain element, this means that it may further include other elements, but not excluding other elements, unless specifically stated to the contrary.
[0041] According to one embodiment of the present invention, there is provided a freestanding film for a dry electrode, the freestanding film including an active material, a binder including a fiberized polymer, and a support, the support being a surface-oxidized carbon fiber (Ox-VGCF).
[0042] Here, the fiberized polymer can bind the active material and the carrier by being fiberized. In this way, in the freestanding film for dry electrodes, the fiberized polymer binds and connects other powders like a rope without a solvent while being fiberized, so the dispersibility of these is very important. If the dispersion is not good, it is impossible to manufacture a freestanding film at all, or even if it is manufactured, it is difficult to ensure the physical properties of the freestanding film, and the active material is likely to be detached during the rolling process, etc., and the life characteristics may be rapidly reduced when the battery is operated after that.
[0043] In relation to this, the inventors of the present application have confirmed that when the binder containing the fiberized polymer is added alone during mixing for manufacturing a free-standing film, the fiberized polymer nanoparticles are present in a dense state as shown in FIG. 1 below, and these primary particles are easily solidified even with a small shear force and are not easily dispersed, so that the free-standing film is not manufactured firmly and the efficiency is greatly reduced, which ultimately affects the electrode properties and deteriorates the battery characteristics.
[0044] Therefore, the inventors of the present application have conducted extensive research and confirmed that when a support is first mixed with a binder containing the fiberized polymer and the mixture is used to manufacture a free-standing film, the fiberized polymer is easily dispersed, and in particular, the surface-oxidized carbon fiber (Ox-VGCF) is easily dispersed because the nano-sized fiberized polymer primary particles are easily adsorbed to the support surface due to the increased oxygen functional groups introduced on the surface of the Ox-VGCF. In addition, when such a mixture is subsequently mixed with an active material and fiberized, the active material can be bonded as a whole, and the performance of a dry electrode and a battery using the mixture can be improved, and the present invention has been completed.
[0045] The support may have surface oxygen functional groups increased by 5 to 15 wt %, specifically 8 to 12 wt %, compared to VGCF that has not been surface-oxidized.
[0046] The content of the oxygen functional group on the surface can be measured by elemental analysis. Specifically, the support can be subjected to an elemental analysis device (CHN-coder MT-5, Yanako) to measure the C, H, and N element contents, and the oxygen content (oxygen differential) can be calculated based on the amount of remaining ash.
[0047] In this way, when the surface oxygen functional groups are sufficiently contained, it is preferable because the nano-sized fiberized polymer primary particles are easily adsorbed onto the support surface, but when the content is excessively large, it is not preferable because there is a problem of electrochemical surface side reaction.
[0048] The support may have an average diameter of 50 nm to 500 nm and an average length of 1 μm to 30 μm. More specifically, the support may have an average diameter of 100 nm to 200 nm and an average length of 1 μm to 15 μm.
[0049] If the average diameter is too small, which is outside the above range, the radius of curvature is small, which makes it difficult to support due to the mutual interference between the primary particles of the fiberized polymer, and if it is too thick, the efficiency of dispersion / support is greatly reduced, which is not preferable. Also, if the average length is too long, the powder fluidity is greatly reduced, which reduces the efficiency of dispersion / support, and if it is too short, the ratio of the support particles clumping together increases, which is not preferable for forming a long conductive network between active materials. Therefore, in order to fully disperse the binder containing the fiberized polymer of the present application, it is preferable to use Ox-VGCF, which has a predetermined diameter, excellent linearity, and surface oxygen functional groups, as in the above range.
[0050] The average diameter and length of the support can be measured by SEM. More specifically, the support solution diluted to 1 wt% in acetone solvent is dropped onto a Si wafer and dried, and the wafer is measured by SEM (Scanning Electron Microscopy, JEOL, JSM-7500F) to obtain the average diameter and length of 300 individual particles.
[0051] The specific surface area of the support for uniformly dispersing the fiber-forming polymer is 10 m 2 / g~150m 2 / g, more specifically, 10m 2 / g~100m 2 / g.
[0052] The specific surface area can be measured by the BET (Brunauer-Emmett-Teller) method. For example, it can be measured by the BET 6-point method using a specific surface area measuring device (Belsorp-II mini, Bell Japan Inc.) by nitrogen gas adsorption.
[0053] When the specific surface area is within this range, the fiber-forming polymer can be easily dispersed and supported. If the specific surface area is too small, the fiber-forming polymer cannot be easily dispersed, and if the specific surface area is too large, gas is generated due to a side reaction with the electrolyte, which is not preferable.
[0054] In addition, the support is made of a carbon material having excellent electrical conductivity, is configured in a cylindrical tube shape with excellent linearity, and has a large specific surface area, which can further strengthen the formation of a conductive network between active materials within the freestanding film, making it even more preferable to include the support.
[0055] Furthermore, the support having an increased surface oxygen functional group may have a graphitization degree (ID / IG ratio) of 0.1 to 2.0.
[0056] The graphitization degree (ID / IG ratio) can be obtained through Raman spectroscopy. -1 The nearby G peak is due to the E2g vibration mode of the sp2 bond of carbon, and is at 1350 cm -1 The nearby D peak appears when there is a defect in the sp2 bond of carbon. The lower the ID / IG ratio (D / G Peak Intensity Ratio), the higher the degree of graphitization. Therefore, when carbon-based particles with a high degree of graphitization are used, the capacity and electrical characteristics of the battery can be improved due to the high electrical conductivity of the carbon-based particles.
[0057] Meanwhile, such a support may be included in an amount of 0.1% by weight to 10% by weight, specifically, 0.5% by weight to 10% by weight, based on the total weight of the free-standing film.
[0058] If the content is too high beyond the above range, the active material content may be less than the effective limit, which is undesirable from the viewpoint of energy density. On the other hand, if the content is too low, the fiberized polymer cannot be sufficiently dispersed.
[0059] Meanwhile, the fiber-forming polymer may be polytetrafluoroethylene (PTFE), and the fiber-forming polymer may be contained in an amount of 50% by weight or more, or may be 100% by weight, based on the total weight of the binder.
[0060] In addition, the binder may further include PEO (polyethylene oxide), PVDF (polyvinylidene fluoride), PVDF-HFP (polyvinylidene fluoride-co-hexafluoropropylene), etc., in addition to the polytetrafluoroethylene, or may further include other binders known in the art, depending on whether the dry electrode is a positive electrode or a negative electrode.
[0061] The active material will also vary depending on whether the dry electrode is a positive electrode or a negative electrode.
[0062] In order to prepare a free-standing film for forming the dry positive electrode, the active material is not limited to a lithium transition metal oxide or a lithium metal iron phosphate, as long as it is in the form of a metal oxide, for example, a layered compound such as lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), or a compound substituted with one or more transition metals; a compound represented by the chemical formula Li 1+x Mn 2-x Lithium manganese oxides such as LiMnO3, LiMn2O3, LiMn2O3, and LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, LiFe3O4, V2O5, and Cu2V2O7; and the chemical formula LiNi 1-x M xNi-site type lithium nickel oxide represented by O2 (where M = Co, Mn, Al, Cu, Fe, Mg, Ca, Zr, Ti, B, P, W, Si, Na, K, Mo, V, Nb, Ru or Ga, and x = 0.01 to 0.3); chemical formula LiMn 2-x M x Lithium manganese composite oxide represented by O2 (where M = Co, Ni, Fe, Cr, Zn or Ta, and x = 0.01 to 0.1) or Li2Mn3MO8 (where M = Fe, Co, Ni, Cu or Zn); LiMn2O4 in which part of Li in the chemical formula is substituted with alkaline earth metal ions; lithium metal phosphate LiMPO4 (where M is M = Fe, CO, Ni, or Mn), disulfide compound; Fe2(MoO4)3 and the like can be mentioned, but it is not limited to only these.
[0063] In order to manufacture the free-standing film for forming the dry negative electrode, the active material is carbon such as graphitized carbon and graphite-based carbon; Li x Fe2O3 (0 ≦ x ≦ 1), Li x WO2 (0 ≦ x ≦ 1), Sn x Me 1-x Me’ y O z (Me: Mn, Fe, Pb, Ge; Me’: Al, B, P, Si, elements of Group 1, Group 2, Group 3 of the periodic table, halogen; 0 < x ≦ 1; 1 ≦ y ≦ 3; 1 ≦ z ≦ 8) and other metal composite oxides; lithium metal; lithium alloy; silicon-based alloy; tin-based alloy; SiO, SiO / C, SiO x (1 < x < 2), silicon-based oxides such as SiO2; metal oxides such as SnO, SnO2, PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4, and Bi2O5; conductive polymers such as polyacetylene; Li-Co-Ni-based materials and the like can be used.
[0064] However, the active material for producing the freestanding film may be a positive electrode active material, more specifically, a lithium transition metal oxide, a lithium nickel-manganese-cobalt oxide, an oxide in which a part of the lithium nickel-manganese-cobalt oxide is substituted with another transition metal, a lithium iron phosphate, or the like.
[0065] On the other hand, in the case of a negative electrode using graphite as the main active material, compared to the application of the positive electrode active material, the use of a conductive material with a large specific surface area is unnecessary or the amount of the conductive material can be greatly reduced, and it is easier to realize a dry electrode by fiberizing the PTFE binder compared to the positive electrode. However, since a negative electrode material using a silicon-based active material is generally a relatively high-capacity material compared to a positive electrode material, the thickness of the negative electrode is realized to be thinner than that of the positive electrode in terms of electrode design, which may increase the process difficulty in terms of manufacturing a free-standing film.
[0066] Meanwhile, the freestanding film may further include a conductive material. Here, the conductive material is not particularly limited as long as it has conductivity without inducing a chemical change in the battery. For example, graphite such as natural graphite or artificial graphite; graphene; activated carbon; activated carbon fiber; carbon black such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fiber such as carbon fiber and metal fiber; metal powder such as carbon fluoride, aluminum, and nickel powder; conductive whisker such as zinc oxide and potassium titanate; conductive metal oxide such as titanium oxide; and conductive materials such as polyphenylene derivatives may be used. In particular, in order to uniformly mix the conductive material and improve the conductivity, the freestanding film may include at least one selected from the group consisting of activated carbon, graphite, carbon black, graphene, and single-walled or multi-walled carbon nanotubes, and more specifically, may include carbon black or activated carbon.
[0067] Here, the mixing ratio of the active material, conductive material, and binder containing a fibrous polymer and support may be 60 to 99.8 wt %:0 to 20 wt %:0.2 to 20 wt % by weight of active material:conductive material:binder containing a fibrous polymer and support, more specifically, 80 to 99 wt %:0.1 to 10 wt %:0.9 to 10 wt %.
[0068] If the binder and carrier contents are too high beyond the above range, the binder fiberization polymer is then excessively fiberized and hardened, which may cause loads on the process equipment and a large increase in resistance to the electrode itself. Conversely, if the binder and carrier contents are too low, sufficient fiberization may not be achieved, making it difficult to produce a freestanding film or causing problems such as electrode detachment and other deterioration in electrode properties.
[0069] In addition, if the conductive material content is too high beyond the above range, the active material content is relatively reduced, causing problems of reduced capacity and hindering PTFE fiberization, whereas if the conductive material content is too low, sufficient conductivity cannot be secured or the electrode properties of the free-standing film may be deteriorated, which is undesirable.
[0070] Meanwhile, in some cases, a filler, which is a component that suppresses the expansion of the electrode, may be added to the mixture. The filler is not particularly limited as long as it does not induce chemical changes in the battery and is a fibrous material, and examples of the filler include olefin polymers such as polyethylene and polypropylene; glass fiber, carbon fiber, and other fibrous materials.
[0071] Furthermore, according to yet another embodiment of the present invention, there is provided a method for producing a free-standing film, comprising the steps of: (a) mixing a binder containing a fiberizing polymer and a support to obtain a mixture; (b) mixing the mixture with an active material and subjecting the mixture to high shear mixing to obtain a fiberizing composition; and (c) forming the fiberizing composition into a film form; wherein the support is a surface-oxidized vapor grown carbon fiber.
[0072] The explanations regarding materials such as the binder, carrier, and active material including the basic fiberized polymer are the same as those described above.
[0073] Meanwhile, the present invention is different from the conventional technology in that, as in step (a), the binder containing the fiberizing polymer is first mixed with the carrier to obtain a mixture, where the mixing is performed without applying a shear force.
[0074] When shear force is applied, fiberization of the fiberizing polymer may occur along with mixing, after which its effectiveness in binding the active material and the conductive material is greatly reduced.
[0075] Specifically, the mixing in step (a) can be performed by simply mixing the binder containing the fiberizing polymer and the carrier at 19° C. or less, or by feeding the mixture of the binder containing the fiberizing polymer and the carrier together into a pulverizer after the mixing, which can be, for example, an air jet mill.
[0076] The reason for mixing at a low temperature of 19° C. or less is that by mixing at a temperature below the phase transition temperature of PTFE, which is mainly used as a fiber-forming polymer, fiberization due to shearing is prevented.
[0077] In addition, when the air jet mill is used, the particles are pulverized by collision between the particles mixed in an air atmosphere rotating at high pressure / high speed, and the application of high shear force from a general impeller-applied mixer is suppressed, so the PTFE primary particles are pulverized without being fiberized by collision, and can be uniformly dispersed / supported on the support surface.
[0078] On the other hand, due to the difference in the mixing method, there may be a certain difference in the resulting mixture structure.
[0079] Specifically, when the binder containing the fiber-forming polymer and the support are simply mixed at 19° C. or less, the binder containing the fiber-forming polymer may be uniformly dispersed and mixed with the support.
[0080] On the other hand, when the binder and carrier mixture is again put into a grinder such as an air jet mill that applies only impact without shear force and is mixed again, the primary particles of the fiberized polymer may be uniformly dispersed and supported on the surface of the carrier as shown in FIG. 2 below.
[0081] In particular, when the binder mixture containing the support and the fiberized polymer is introduced into a grinder such as an air jet mill and mixed so that the primary particles of the fiberized polymer are uniformly dispersed and supported on the surface of the support, it has been confirmed that the dispersion effect is superior to that achieved by applying only simple mixing, thereby further improving the electrode properties and battery performance. More specifically, the mixing can be performed by introducing the mixture into a grinder such as an air jet mill so that the primary particles of the fiberized polymer are uniformly dispersed and supported on the surface of the support.
[0082] Here, the binder containing the fiberizing polymer and the support can be mixed in a ratio of 20:80 to 50:50 on a weight basis.
[0083] If the content of the carrier is too high beyond the above range, the degree of fiberization of the fiberized polymer is not satisfactory, resulting in a problem of deterioration of the quality of the electrode. If the content of the carrier is too low, it is not preferable because a sufficient dispersion effect of the fiberized polymer cannot be obtained.
[0084] Here, the simple mixing may be a process of mixing two to five times, more specifically three times, at 3000 rpm to 5000 rpm for 30 seconds to 1 minute each, using a powder mixer (KM Tech) equipped with a cooler cooled to about 5°C, so as to minimize heat generation from the mixer.
[0085] The above mixing and additional mixing in a grinder are performed so as not to apply shear force. For example, when using a grinder such as an air jet mill (Micronizer, Sturtevant), the feeding condition of the mixture is 4 kgf / cm. 2 ~6kgf / cm 2 Grinding condition is 2kgf / cm 2 ~4kgf / cm 2 It is held.
[0086] The mixture obtained in step (a) is then mixed with an active material and a conductive material.
[0087] Here, in order to ensure uniform dispersion, the mixing in step (b) may be performed using a powder mixer (KM Tech) equipped with a cooler cooled to about 5°C, similar to the premixing, and specifically, may be performed by mixing at 5,000 rpm to 20,000 rpm for 30 seconds to 1 minute, 2 to 5 times, more specifically, 3 times.
[0088] After that, high shear mixing is applied to obtain a fiber composition, where the high shear mixing means the degree to which the fiber polymer can be fiberized, and in detail, the high shear mixing can be performed in the range of 10 rpm to 500 rpm for 1 minute to 30 minutes. Here, the high shear mixing can be performed, for example, by putting the mixture into a twin screw kneader (Irei Shokai Co., Ltd., PBV-0.1L).
[0089] If the shear force is not applied sufficiently, the fiberization of the fiberizing polymer may not be sufficient, whereas if the shear force is too large, the fiberized fiberizing polymer may be broken, which is undesirable.
[0090] The high shear mixing for producing the fiberizing composition can be performed at a mixing temperature of 20 to 120°C, specifically 40 to 120°C, and more specifically 60 to 120°C.
[0091] The structure in which PTFE as the polymer is subjected to a shear force by such high shear mixing to be fibrous and bind the active material and the conductive material is well known in the art.
[0092] Thereafter, when the fiberized composition is formed by the high shear mixing, a step of forming the fiberized composition into a film is carried out, and the forming in step (c) can be carried out by a hot rolling method using a calendar.
[0093] Here, the calender may be a calender roll, and the diameter of the roll may be, for example, 50 to 1000 mm, specifically, 100 to 1000 mm, and more specifically, 100 to 500 mm.
[0094] The surface temperature of the calender roll may be from 20 to 200°C, specifically from 40 to 150°C, and more specifically from 60 to 150°C.
[0095] Such calender rolls can apply shear pressure to ultimately produce a free-standing film.
[0096] The freestanding film thus produced may have a thickness of 10 to 1000 μm, specifically, 50 to 500 μm, and more specifically, 100 to 500 μm.
[0097] That is, the free-standing film for a dry electrode according to the present invention can be manufactured thick and is suitable for manufacturing a thick-film electrode.
[0098] Meanwhile, according to yet another embodiment of the present invention, there is provided a dry electrode including a current collector and a free-standing film formed on the current collector, the current collector having a structure in which a primer layer is coated on a metal foil.
[0099] The PTFE polymer used in the manufacture of the freestanding film can be manufactured in the form of a film by binding the active material and the conductive material through fiberization, but since it does not have adhesive strength to the current collector, the current collector coated with the primer layer can be used to ensure the adhesive strength between the current collector and the freestanding film.
[0100] The current collector is not particularly limited as long as it has high conductivity without inducing chemical changes in the battery, and can be, for example, stainless steel, aluminum, nickel, titanium, calcined carbon, copper, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. The current collector can also be processed into a mesh shape or have fine projections and recesses on its surface to increase the adhesive force of the positive electrode active material, and can be in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.
[0101] The primer layer may be coated entirely or partially on the current collector, and more particularly, may be coated entirely on the current collector.
[0102] Such a primer layer may include a conductive material and a binder, and the conductive material is not limited as long as it is a conductive material, and may be, for example, a carbon-based material such as carbon black, carbon nanotubes, graphene, graphite, etc. The binder may include a fluorine-based binder (including PVDF and PVDF copolymers) that is soluble in a solvent, an acrylic binder, and a water-based binder.
[0103] The free-standing film and the current collector coated with the primer layer can be bonded together by lamination.
[0104] The lamination can also be performed by a lamination roll, where the lamination roll is maintained at a temperature of 80°C to 200°C.
[0105] Meanwhile, according to another embodiment of the present invention, there is provided a secondary battery including the dry electrode.
[0106] Specifically, an electrode assembly including the dry electrode, the separator, and the counter electrode is housed in a battery case together with an electrolyte. Other configurations of the secondary battery are well known in the art, and therefore will not be described here.
[0107] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, the present invention will be described in detail based on examples, comparative examples, and experimental examples in order to facilitate understanding by those skilled in the art of the present invention. EXAMPLES
[0108] <Reference example> Polytetrafluoroethylene (PTFE) was used as a binder. The sample was placed on the carbon tape while being careful not to apply maximum shear force, and the SEM image was taken and shown in Figure 1 below.
[0109] <Production of Oxidized Grown Carbon Fibers (Ox-VGCF) with increased surface oxygen functional groups through surface oxidation treatment> Commercial VGCF (Showadenko, VGCF-H) was mixed with a 30 wt% HNO3 solution and oxidized at 60°C for 8 hours while stirring. After thorough washing with distilled water, it was dried in a vacuum oven at 150°C for 24 hours to obtain a surface-oxidized carbon fiber support (Ox-VGCF) (surface oxygen functional group content: about 10.3 wt%, average diameter: 150 nm, average length: 6 μm, specific surface area: 13 m). 2 / g, graphitization degree: 0.42).
[0110] The content of surface oxygen functional groups was measured by elemental analysis. Specifically, the support was subjected to an elemental analysis instrument (CHN-coder MT-5, Yanako) to measure the C, H, and N element contents, and the oxygen content (Oxygen Differential) was calculated based on the amount of remaining ash.
[0111] The average diameter and length of the support were determined by dropping the support solution, which had been diluted to 1 wt % in acetone solvent, onto a Si wafer, drying it, and measuring it with a SEM (Scanning Electron Microscopy, JEOL, JSM-7500F) to determine the average diameter and length for 300 individual particles.
[0112] The specific surface area was measured by the BET 6-point method using nitrogen gas adsorption with a specific surface area measuring device (Belsorp-II mini, Bell Japan Inc.).
[0113] The degree of graphitization (ID / IG ratio) was measured by analyzing the Raman spectrum using a Raman spectrum measuring device (NRS-2000B, Jasco) with an Ar ion laser having a wavelength of 514.5 nm.
[0114] <Production Example 1> Polytetrafluoroethylene (PTFE) and carbon fibers with increased surface oxygen functional groups (Ox-VGCF) were prepared in a weight ratio of 1:1 as a binder, and a mixture was prepared by premixing three times at 5000 rpm for 1 minute each using a powder mixer (KM Tech) equipped with a cooler cooled to 5°C. The mixture was then pulverized / dispersed / supported using an air jet mill (Sturtevant, Micronizer), where the feeding condition was 5 kgf / cm. 2 Grinding condition is 3kgf / cm 2 It was.
[0115] The SEM image of the mixture prepared above is shown in FIG.
[0116] <Production Example 2> Polytetrafluoroethylene (PTFE) as a binder and carbon fiber with increased surface oxygen functional groups (Oxidized Vapour Grown Carbon Fibers, Ox-VGCF) were prepared in a weight ratio of 1:1, and a mixture was prepared by premixing three times at 5000 rpm for 1 minute each using a powder mixer (KM Tech) equipped with a cooler cooled to 5°C.
[0117] <Production Example 3> Polytetrafluoroethylene (PTFE) as a binder and commercial carbon fiber (Showadenko, VGCF-H) without surface oxidation treatment as a carrier were prepared in a weight ratio of 1:1, and a mixture was prepared by premixing three times at 5000 rpm for 1 minute each using a powder mixer (KM Tech) equipped with a cooler cooled to 5°C. The mixture was then crushed / dispersed / supported using an air jet mill (Sturtevant, Micronizer), where the feeding condition was 5 kgf / cm. 2 Grinding condition is 3kgf / cm 2It was.
[0118] <Production Example 4> Polytetrafluoroethylene (PTFE) as a binder and commercial activated carbon (Kuraray, YP-80F) as a carrier were prepared in a weight ratio of 1:1, and a mixture was premixed three times at 5000 rpm for 1 minute each using a powder mixer (KM Tech) equipped with a cooler cooled to 5°C. The mixture was then crushed / dispersed / supported using an air jet mill (Sturtevant, Micronizer), where the feeding conditions were 5 kgf / cm. 2 Grinding condition is 3kgf / cm 2 It was.
[0119] <Production Example 5> Polytetrafluoroethylene (PTFE) as a binder and commercial activated carbon (Kuraray, YP-80F) as a support were prepared in a weight ratio of 1:1, and a mixture was prepared by premixing three times at 5000 rpm for 1 min each using a powder mixer (KM Tech) equipped with a cooler cooled to 5°C.
[0120] <Production Example 6> Polytetrafluoroethylene (PTFE) as a binder and commercial carbon black (Imerys, Super C45) as a carrier were prepared in a weight ratio of 1:1, and a mixture was prepared by premixing three times at 5000 rpm for 1 minute each using a powder mixer (KM Tech) equipped with a cooler cooled to 5°C. The mixture was then pulverized / dispersed / supported using an air jet mill (Sturtevant, Micronizer), where the feeding conditions were 5 kgf / cm. 2 Grinding condition is 3kgf / cm 2 It was.
[0121] <Production Example 7> Polytetrafluoroethylene (PTFE) as a binder and commercial activated carbon (Kuraray, YP-80F) as a support were prepared in a weight ratio of 1:1, and a mixture was prepared by premixing three times at 5000 rpm for 1 min each using a powder mixer (KM Tech) equipped with a cooler cooled to 5°C.
[0122] <Production Example 8> Polytetrafluoroethylene (PTFE) and commercial activated carbon (Kuraray, YP-80F) were used as the binder, and commercial carbon fiber (Showadenko, VGCF-H) without surface oxidation treatment was used as the support in a weight ratio of 2:1:1. The mixture was premixed three times at 5,000 rpm for 1 min each using a powder mixer (KM Tech) equipped with a cooler cooled to 5°C.
[0123] <Example 1> 96 g of LiMn2O4 positive active material and 4 g of the mixture prepared in Preparation Example 1 as a conductive material and binder were dispersed three times at 10,000 rpm for 1 minute each using a powder mixer (KM Tech Co., Ltd.) equipped with a cooler cooled to 5°C. The mixture was then added to a high-shear mixer Twin Screw Kneader (Irie Shokai Co., Ltd., PBV-0.1L) and mixed at 100 rpm at a temperature of 90°C for 3 minutes to prepare a fiberized composition.
[0124] An SEM image of the fiber composition is shown in FIG.
[0125] Referring to FIG. 3, it can be seen that the PTFE binder is uniformly fiberized throughout.
[0126] The fiberization composition was put into a wrap calendar (roll diameter: 200 mm, roll temperature: 100° C., 20 rpm) and the roll gap was adjusted to finally prepare a free-standing film having a thickness of 200 μm.
[0127] <Example 2> A free-standing film having a thickness of 200 μm was prepared in the same manner as in Example 1, except that the mixture prepared in Preparation Example 2 was used as the conductive material and the binder in Example 1.
[0128] <Comparative Example 1> A free-standing film having a thickness of 200 μm was prepared in the same manner as in Example 1, except that the mixture prepared in Preparation Example 3 was used as the conductive material and the binder in Example 1.
[0129] <Comparative Example 2> A free-standing film having a thickness of 200 μm was prepared in the same manner as in Example 1, except that the mixture prepared in Preparation Example 4 was used as the conductive material and the binder in Example 1.
[0130] <Comparative Example 3> A free-standing film having a thickness of 200 μm was prepared in the same manner as in Example 1, except that the mixture prepared in Preparation Example 5 was used as the conductive material and the binder in Example 1.
[0131] <Comparative Example 4> A free-standing film having a thickness of 200 μm was prepared in the same manner as in Example 1, except that the mixture prepared in Preparation Example 6 was used as the conductive material and the binder.
[0132] <Comparative Example 5> A free-standing film having a thickness of 200 μm was prepared in the same manner as in Example 1, except that the mixture prepared in Preparation Example 7 was used as the conductive material and the binder.
[0133] <Comparative Example 6> A free-standing film having a thickness of 200 μm was prepared in the same manner as in Example 1, except that the mixture prepared in Preparation Example 8 was used as the conductive material and the binder.
[0134] <Experimental Example 1> The free-standing film was placed on one side of an aluminum foil (20 μm, Primer Coated Al Foil, Dongwon Systems) coated with a primer layer containing a mixture of carbon black and PVDF binder, and laminated using a lamination roll maintained at 120° C. to prepare an electrode.
[0135] A coin-type half cell was fabricated using the above electrode, lithium metal as a counter electrode, and an electrolyte containing 1M LiPF6 in a solvent of ethylene carbonate (EC): dimethyl carbonate (DMC): (diethyl carbonate) DEC = 1: 2: 1.
[0136] The coin-type half cell prepared above was charged and discharged at a current condition of 0.2 C rate at 25° C. in the voltage range of 3.0 to 4.30 V, and the ratio of the discharge capacity when charged and discharged at a current condition of 2.0 C rate was measured. The results are shown in Table 1 below.
[0137] [Table 1]
[0138] Referring to Table 1 above, it can be seen that excellent battery characteristics can be obtained when the carbon fiber having an increased surface oxygen functional group by surface oxidation treatment according to the present invention is used together, and even more excellent effects can be obtained when the carbon fiber is additionally mixed using an air jet mill.
[0139] Furthermore, when examining Comparative Example 1, it can be seen that even when non-oxidized VGCF is used, a certain degree of dispersion effect is exhibited and an improved effect is shown, but it is not sufficient, and it can be confirmed that not only when activated carbon or carbon black is used, but also when activated carbon and VGCF are used together, the effect is significantly inferior to that of the present invention. [Industrial Applicability]
[0140] According to the present invention, a surface-oxidized carbon fiber (Ox-VGCF) support is mixed with a binder containing a fiberizing polymer and used to manufacture a free-standing film, so that the primary particles of the fiberizing polymer are uniformly dispersed / supported in the mixture for manufacturing the free-standing film, and the free-standing film can be uniformly and firmly bonded due to the fiberization of the fiberizing polymer, thereby improving the electrode properties and thus improving the battery performance.
[0141] Furthermore, the use of the carrier can further strengthen the conductive network between the active materials, which is advantageous for improving the battery performance.
Claims
1. A free-standing film for a dry electrode of a lithium secondary battery, comprising: The free-standing film includes an active material, a binder including a fiberized polymer, and a support; The support is a surface-oxidized carbon fiber (Ox-VGCF), A free-standing film, wherein the fiberized polymer is polytetrafluoroethylene (PTFE).
2. 2. The freestanding film of claim 1, wherein the fiberized polymer is fiberized to bind the active material and the support.
3. 3. The freestanding film according to claim 1, wherein the support is a carbon fiber having surface oxygen functional groups increased by a surface oxidation treatment.
4. 4. The freestanding film of claim 3, wherein the support comprises surface oxygen functional groups at 5 to 15 wt %, based on the total weight of the support.
5. 5. The freestanding film of claim 1, wherein the supports have an average diameter of 50 nm to 500 nm and an average length of 1 μm to 30 μm.
6. The specific surface area of the support is 10 m 2 / g ~ 150m 2 6. The freestanding film of claim 1, wherein the elastic modulus is 1 / g.
7. 7. The freestanding film according to claim 1, wherein the support has a degree of graphitization of 0.1 to 2.
0.
8. 8. The freestanding film of claim 1, wherein the support is present in an amount of 0.1% to 10% by weight, based on the total weight of the freestanding film.
9. A method for producing a free-standing film according to any one of claims 1 to 8, comprising the steps of: (a) mixing a binder comprising a fiberizing polymer and a support to obtain a mixture; (b) mixing the mixture with an active material and subjecting it to high shear mixing to obtain a fiberized composition; and (c) forming the fiberizing composition into a film form; The support is a surface-oxidized carbon fiber (Ox-VGCF), The method for producing a free-standing film, wherein the fiberized polymer is polytetrafluoroethylene (PTFE).
10. The method for producing a freestanding film according to claim 9, wherein the mixing in step (a) is performed by simply mixing the binder containing the fiberizing polymer and the carrier at 19°C or less, or by feeding the mixture of the binder containing the fiberizing polymer and the carrier together into a grinder after the mixing.
11. The method for producing a freestanding film according to claim 10, wherein the grinder is an air jet mill.
12. The method for producing a freestanding film according to any one of claims 9 to 11, wherein the mixture has a structure in which primary particles of the fiberizing polymer are uniformly dispersed and supported on the surface of the support.
13. The method for producing a freestanding film according to any one of claims 9 to 12, wherein the high shear mixing in step (b) is carried out at a speed ranging from 10 rpm to 500 rpm for a period ranging from 1 minute to 30 minutes.
14. The method for producing a freestanding film according to any one of claims 9 to 13, wherein the forming in step (c) is carried out by a hot rolling method using a calendar.
15. A current collector and the free-standing film according to claim 1 formed on the current collector, The current collector has a structure in which a primer layer is coated on a metal foil, forming a dry electrode for a lithium secondary battery.
16. A secondary battery including the dry electrode of the lithium secondary battery according to claim 15, The electrode assembly including the dry electrode, the counter electrode, and the separator is housed in a battery case together with a lithium-containing non-aqueous electrolyte.
Citation Information
Patent Citations
Electrochemical capacitor and electrode layer used therefor, and method of manufacturing the electrode layer
JP2011029408A
Positive electrode active material, and positive electrode containing the same, lithium secondary battery
JP2012528451A
Conductive auxiliary agent dispersion liquid for electrode material of lithium ion secondary battery
JP2013077479A
Composite positive electrode active material, method of preparing the same, and positive electrode and lithium battery containing the composite positive electrode active material
JP2014170739A