Electrode assembly for lithium secondary battery and lithium secondary battery including the same
The lithium secondary battery design addresses low energy density and irreversible capacity issues by using a specific ratio of lithium metal composite oxide and silicon-based materials, enhancing energy density and stability.
Patent Information
- Application Number
- JP2023513506
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-05-26
- Filing Date
- 2022-05-06
- Publication Date
- 2024-09-17
- Estimated Expiration
- 2042-05-06
AI Technical Summary
Lithium secondary batteries face challenges with low energy density and irreversible capacity loss due to the use of graphite as a negative electrode material and limitations with cobalt-based positive electrode materials, which are costly and unsafe for large-scale applications.
A lithium secondary battery design incorporating a positive electrode with a specific ratio of lithium metal composite oxide and a positive electrode additive, along with a negative electrode containing silicon-based materials, is developed to enhance energy density and stability, using a controlled ratio of positive electrode additives and silicon-containing substances.
The design achieves high energy density and long battery life by optimizing the ratio of positive and negative electrode components, reducing irreversible capacity loss and improving charge/discharge efficiency.
Smart Images

Figure 0007551216000004 
Figure 0007551216000002 
Figure 0007551216000001
Abstract
Description
[Technical field]
[0001] The present invention relates to an electrode assembly for a lithium secondary battery and a lithium secondary battery including the same.
[0002] This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0067353 dated May 26, 2021, and all contents disclosed in the documents of that Korean patent application are incorporated herein by reference. [Background technology]
[0003] Recently, with growing interest in environmental issues, much research has been conducted on electric vehicles (EVs) and hybrid electric vehicles (HEVs) that can replace fossil fuel vehicles such as gasoline and diesel vehicles, which are one of the main causes of air pollution. Nickel-metal hydride (Ni-MH) secondary batteries are mainly used as the power source for such electric vehicles (EVs) and hybrid electric vehicles (HEVs), but active research is being conducted on the use of lithium secondary batteries, which have high energy density, high discharge voltage and output stability, and some have been commercialized.
[0004] Graphite is mainly used as the negative electrode material for such lithium secondary batteries, but since graphite has a small capacity per unit mass of 372 mAh / g, it is difficult to increase the capacity of lithium secondary batteries. For this reason, in order to increase the capacity of lithium secondary batteries, negative electrode materials that form intermetallic compounds with lithium, such as silicon, tin, and oxides of these, have been developed and used as non-carbon-based negative electrode materials that have a higher energy density than graphite. However, such non-carbon-based negative electrode materials have a problem that although they have a large capacity, their initial efficiency is low, resulting in a large amount of lithium consumption during initial charging and discharging, and a large irreversible capacity loss.
[0005] In addition, lithium-containing cobalt oxide (LiCoO2) is mainly used as the positive electrode material for lithium secondary batteries, and the use of lithium-containing manganese oxides such as LiMnO2 with a layered crystal structure and LiMn2O4 with a spinel crystal structure, as well as lithium-containing nickel oxide (LiNiO2), is also being considered.
[0006] However, although LiCoO2 has excellent physical properties such as excellent cycle characteristics and is widely used at present, it is not safe and is expensive due to the limited availability of cobalt as a raw material, so there is a limit to its use in large quantities as a power source in fields such as electric vehicles. In addition, LiNiO2 is difficult to apply to actual mass production processes at reasonable costs due to the characteristics of its manufacturing method, and lithium plating is induced on the negative electrode due to gas generated during charging and discharging, so there is a limit to its safety as well as a decrease in charging and discharging capacity. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Korean Patent Publication No. 10-2018-0023696 Summary of the Invention [Problem to be solved by the invention]
[0008] SUMMARY OF THE PRESENT EMBODIMENTS Accordingly, an object of the present invention is to provide a lithium secondary battery having a high energy density and a long battery life. [Means for solving the problem]
[0009] To solve the above problems, In one embodiment, the present invention comprises: A positive electrode containing a positive electrode active material and a positive electrode additive represented by the following chemical formula 1 in a positive electrode mixture layer; A negative electrode including a carbon material and a silicon (Si)-containing material in a negative electrode mixture layer as a negative electrode active material; A separator located between the positive electrode and the negative electrode, The content of the positive electrode additive is 0.01 to 5 parts by weight based on 100 parts by weight of the positive electrode mixture layer, and The percentage of the positive electrode additive based on the total weight of the positive electrode mixture layer (CR) Lip and the percentage of silicon (Si)-containing material content CR based on the total weight of the negative electrode mixture layer Si Relative to CR Lip / CR Si The electrode assembly for a lithium secondary battery is provided, in which
[0010] [Chemical formula 1] Li p Co (1-q) M 1 q O4
[0011] In the above chemical formula 1, M 1 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; p and q are 5≦p≦7 and 0≦q≦0.5, respectively.
[0012] At this time, the content percentage CR of the positive electrode additive based on the total weight of the positive electrode mixture layer Lip and the percentage of silicon (Si)-containing material content CR based on the total weight of the negative electrode mixture layer Si Relative to CR Lip / CR Si However, it may be 0.05 to 0.20.
[0013] The positive electrode additive may have a tetragonal structure with a space group of P42 / nmc.
[0014] The positive electrode active material may be a lithium metal composite oxide represented by the following Chemical Formula 2:
[0015] [Chemical formula 2] Li x [Ni y Co z Mn w M 2 v ]O u
[0016] In the above chemical formula 2, M 2 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; x, y, z, w, v, and u are 1.0≦x≦1.30, 0≦y<0.95, 0 <z≦0.5、0<w≦0.5、0≦v≦0.2、1.5≦u≦4.5である。
[0017] The carbon substance may include one or more selected from the group consisting of natural graphite, artificial graphite, graphene, and carbon nanotubes, and the silicon (Si)-containing substance may include one or more of silicon (Si), silicon monoxide (SiO), and silicon dioxide (SiO2).
[0018] In addition, the carbon material may include at least one of graphene and carbon nanotubes, and may be included in an amount of 0.1 to 10 parts by weight based on 100 parts by weight of the total carbon material.
[0019] The positive electrode mixture layer may contain 0.1 to 5 parts by weight of a conductive material based on the total weight. Here, the positive electrode mixture layer may contain one or more conductive materials selected from the group consisting of natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, and carbon fiber.
[0020] The positive electrode mixture layer may have an average thickness of 50 μm to 300 μm, and the negative electrode mixture layer may have an average thickness of 100 to 300 μm.
[0021] The average area ratio between the negative electrode mixture layer and the positive electrode mixture layer may be 1.0 to 1.1.
[0022] Moreover, in one embodiment, the present invention provides There is provided a lithium secondary battery including the electrode assembly according to the present invention. Effect of the Invention
[0023] The electrode assembly for a lithium secondary battery according to the present invention has a positive electrode additive and a negative electrode active material, respectively, contained in a positive electrode mixture layer and a negative electrode mixture layer, and the positive electrode additive and a negative electrode active material, respectively, are contained in a silicon (Si)-containing material. Lip / CR Si By adjusting the amount of the charge / discharge electrode to a specific range, it is possible to realize high charge / discharge capacity and charge / discharge efficiency during initial charge / discharge, and also to realize excellent capacity retention during subsequent charge / discharge. Thus, a lithium secondary battery including the battery has the advantages of high energy density and long life. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] While the present invention may be modified in many ways and may have a variety of embodiments, a specific embodiment will be described in detail in the detailed description.
[0025] However, it should be understood that this is not intended to limit the invention to the particular embodiment, but includes all modifications, equivalents, and alternatives falling within the spirit and technical scope of the invention.
[0026] In the present invention, the terms "comprise" or "have" are intended to specify the presence of features, numbers, steps, operations, components, parts, or combinations thereof described in the specification, and should be understood as not precluding the presence or additional possibility of one or more other features, numbers, steps, operations, components, parts, or combinations thereof.
[0027] In addition, in the present invention, when a layer, film, region, plate, or other portion is described as being "on" another portion, this includes not only the case where it is "directly on" the other portion, but also the case where there is another portion in between. Conversely, when a layer, film, region, plate, or other portion is described as being "under" the other portion, this includes not only the case where it is "directly under" the other portion, but also the case where there is another portion in between. In addition, in the present application, being "located on" may include not only the case where it is located at the top, but also the case where it is located at the bottom.
[0028] The present invention will now be described in more detail.
[0029] <Electrode assembly for lithium secondary battery> In one embodiment, the present invention comprises: A positive electrode containing a positive electrode active material and a positive electrode additive represented by the following chemical formula 1 in a positive electrode mixture layer; A negative electrode including a carbon material and a silicon (Si)-containing material in a negative electrode mixture layer as a negative electrode active material; A separator located between the positive electrode and the negative electrode, The content of the positive electrode additive is 0.01 to 5 parts by weight based on 100 parts by weight of the positive electrode mixture layer, and The percentage of the positive electrode additive based on the total weight of the positive electrode mixture layer (CR) Lip and the percentage of silicon (Si)-containing material content CR based on the total weight of the negative electrode mixture layer Si Relative to CR Lip / CR Si is 0.03 to 0.30.
[0030] [Chemical formula 1] Li p Co (1-q) M 1 q O4
[0031] In the above chemical formula 1, M 1is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; p and q are 5≦p≦7 and 0≦q≦0.5, respectively.
[0032] The electrode assembly for a lithium secondary battery according to the present invention has a structure including a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode, in which the positive electrode has a form in which a positive electrode mixture layer is located on a positive electrode current collector, and the positive electrode mixture layer includes a positive electrode active material that exhibits activity and a positive electrode additive that imparts irreversible capacity. Specifically, the positive electrode mixture layer includes a lithium metal composite oxide represented by the following Chemical Formula 2 as a positive electrode active material capable of reversible intercalation and deintercalation:
[0033] [Chemical formula 2] Li x [Ni y Co z Mn w M 2 v ]O u
[0034] In the above chemical formula 2, M 2 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; x, y, z, w, v, and u are 1.0≦x≦1.30, 0≦y<0.95, 0 <z≦0.5、0<w≦0.5、0≦v≦0.2、1.5≦u≦4.5である。
[0035] The lithium metal composite oxide shown in the above chemical formula 2 is a composite metal oxide containing lithium and nickel, and is LiCoO2, LiCo 0.5 Zinc 0.5 O2, LiCo 0.7 Zinc 0.3 O2, LiNiO2, LiNi 0.5 Co0.5 O2, LiNi 0.6 Co 0.4 O2, LiNi 1 / 3 Co 1 / 3 Al 1 / 3 O2, LiMnO2, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, LiNi 0.8 Co 0.1 Mn 0.1 O2, LiNi 0.6 Co 0.2 Mn 0.2 O2, LiNi 0.9 Co 0.05 Mn 0.05 O2, LiNi 0.6 Co 0.2 Mn 0.1 Al 0.1 O2, and LiNi 0.7 Co 0.1 Mn 0.1 Al 0.1 The gas may contain one or more compounds selected from the group consisting of O2.
[0036] As an example, the positive electrode active material is a lithium metal composite oxide represented by the chemical formula 2, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, LiNi 0.8 Co 0.1 Mn 0.1 O2 or LiNi 0.6 Co 0.2 Mn 0.2 O2 can be used alone or in combination.
[0037] The content of the positive electrode active material may be 85 to 95 parts by weight, specifically 88 to 95 parts by weight, 90 to 95 parts by weight, 86 to 90 parts by weight, or 92 to 95 parts by weight, relative to 100 parts by weight of the positive electrode mixture layer.
[0038] The positive electrode mixture layer contains a positive electrode additive represented by the following Chemical Formula 1:
[0039] [Chemical formula 1] Li p Co(1-q) M 1 q O4
[0040] In the above chemical formula 1, M 1 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; p and q are 5≦p≦7 and 0≦q≦0.5, respectively.
[0041] The positive electrode additive contains an excess of lithium and can provide lithium to replace lithium consumption that occurs due to irreversible chemical and physical reactions at the negative electrode during initial charging, thereby increasing the charging capacity of the battery and reducing the irreversible capacity, thereby improving the life characteristics.
[0042] Among them, the positive electrode additive represented by the above formula 1 has a higher lithium ion content than nickel-containing oxides commonly used in the industry. As a result, the positive electrode additive represented by the above formula 1 can replenish lithium consumed by irreversible chemical and physical reactions occurring in the negative electrode containing a Si-based material (e.g., Si, SiOq (where 0.8≦q≦2.2)) as the negative electrode active material during initial activation of the battery, thereby significantly improving the charge and discharge capacity of the battery. In addition, compared to iron and / or manganese-containing oxides commonly used in the industry, there is no side reaction caused by the elution of transition metals during charging and discharging of the battery, so there is an advantage in that the stability of the battery is excellent. Examples of lithium metal oxides represented by the above formula 1 include Li6CoO4, Li6Co 0.5 Zinc 0.5 O4, Li6Co 0.7 Zinc 0.3 It may also include O4.
[0043] In addition, the positive electrode additive represented by the above formula 1 may have a tetragonal crystal structure, and among them, it may be included in the space group P42 / nmc having a distorted tetrahedral structure formed by cobalt and oxygen elements.
[0044] The content of the positive electrode additive may be 5% by weight or less relative to the total weight of the positive electrode active material, and specifically may be 0.01 to 5% by weight, 0.01 to 4% by weight, 0.01 to 3% by weight, 0.01 to 2% by weight, 0.01 to 1% by weight, 0.1 to 0.9% by weight, 0.3 to 0.9% by weight, 0.2 to 0.7% by weight, 0.5 to 0.9% by weight, 0.01 to 0.5% by weight, 0.1 to 0.4% by weight, 1 to 5 parts by weight, 2 to 4 parts by weight, 0.1 to 2.5 parts by weight, 0.1 to 1 part by weight, or 0.5 to 2.5 parts by weight.
[0045] Moreover, the positive electrode mixture layer may further contain a conductive material, a binder, other additives, and the like, in addition to the positive electrode active material and the positive electrode additive.
[0046] In this case, the conductive material can be used to improve the electrical performance of the positive electrode, and can be one or more carbon materials selected from the group consisting of natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, and carbon fiber. For example, the conductive material may include acetylene black.
[0047] The conductive material may be contained in an amount of 0.1 to 5 parts by weight, specifically 1 to 4 parts by weight, 2 to 4 parts by weight, 1.5 to 5 parts by weight, or 1 to 3 parts by weight, per 100 parts by weight of the composite layer.
[0048] The binder may include one or more resins selected from the group consisting of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethylmethacrylate, and copolymers thereof. As an example, the binder may include polyvinylidene fluoride.
[0049] The mixture layer may contain 1 to 10 parts by weight of the binder, specifically 2 to 8 parts by weight, 2 to 6 parts by weight, 1 to 5 parts by weight, or 2 to 4 parts by weight, based on 100 parts by weight of the total mixture layer.
[0050] In addition, the positive electrode may be a positive electrode current collector having high conductivity without inducing chemical changes in the battery. For example, stainless steel, aluminum, nickel, titanium, calcined carbon, etc. may be used, and in the case of aluminum or stainless steel, those surface-treated with carbon, nickel, titanium, silver, etc. may be used. In addition, the positive electrode current collector may be formed with fine irregularities on the surface to increase the adhesive force of the positive electrode active material, and may be in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc. In addition, the average thickness of the current collector may be appropriately applied in the range of 1 to 500 μm in consideration of the conductivity and total thickness of the positive electrode to be manufactured.
[0051] Meanwhile, the negative electrode includes a negative electrode mixture layer prepared by applying a negative electrode active material onto a negative electrode current collector, drying and pressing the negative electrode active material, and the positive electrode mixture layer may further include an organic binder polymer, an additive, etc., which are the same as those of the positive electrode, as necessary.
[0052] Here, the negative electrode active material may include a carbon material and a silicon (Si)-containing material. The carbon material means a carbon material mainly composed of carbon atoms, and examples of such carbon materials include graphite having a perfect layered crystal structure like natural graphite, soft carbon having a low crystalline layered crystal structure (graphene structure; a structure in which hexagonal honeycomb-shaped carbon planes are arranged in layers), and hard carbon in which such a structure is mixed with a non-crystalline portion, artificial graphite, expanded graphite, carbon fiber, non-graphitizable carbon, carbon black, acetylene black, ketjen black, carbon nanotubes, fullerene, activated carbon, graphene, carbon nanotubes, etc., and preferably, may include one or more selected from the group consisting of natural graphite, artificial graphite, graphene, and carbon nanotubes. More preferably, the carbon material includes natural graphite and / or artificial graphite, and may further include one or more of graphene and carbon nanotubes together with the natural graphite and / or artificial graphite. In this case, the carbon substance may contain 0.1 to 10 parts by weight of graphene and / or carbon nanotubes relative to 100 parts by weight of the total carbon substance, and more specifically, may contain 0.1 to 5 parts by weight, or 0.1 to 2 parts by weight of graphene and / or carbon nanotubes relative to 100 parts by weight of the total carbon substance.
[0053] The silicon (Si)-containing material is a material containing silicon (Si) as a main component as a metal component, and may contain silicon (Si), silicon monoxide (SiO) or silicon dioxide (SiO2) alone or in combination. When silicon monoxide (SiO) and silicon dioxide (SiO2) are uniformly mixed or composited as the silicon (Si)-containing material and contained in the negative electrode composite layer, they may be represented as silicon oxide (SiOx, where 1≦x≦2). In addition, when the silicon (Si)-containing material has a form in which silicon monoxide (SiO) particles and silicon dioxide (SiO2) particles are uniformly mixed, each particle may have the form of a crystalline particle, and when the silicon monoxide (SiO) particles and silicon dioxide (SiO2) particles are composited, each particle may have the form of a crystalline particle or an amorphous particle. In this case, the ratio of the amorphous particles may be 50 to 100 parts by weight, specifically 50 to 90 parts by weight, 60 to 80 parts by weight, or 85 to 100 parts by weight, based on 100 parts by weight of the total silicon (Si)-containing material. In the present invention, the ratio of the amorphous particles contained in the silicon (Si)-containing material can be controlled within the above range, thereby improving the thermal stability and flexibility without deteriorating the electrical properties of the electrode.
[0054] In addition, the negative electrode active material may contain a carbon material and a silicon (Si)-containing material, and may contain 75 to 99 parts by weight of the carbon material and 1 to 25 parts by weight of the silicon (Si)-containing material relative to 100 parts by weight of the total. More specifically, the negative electrode active material may contain 80 to 95 parts by weight of the carbon material and 5 to 20 parts by weight of the silicon (Si)-containing material, 90 to 97 parts by weight of the carbon material and 3 to 10 parts by weight of the silicon (Si)-containing material, 85 to 92 parts by weight of the carbon material and 8 to 15 parts by weight of the silicon (Si)-containing material, 82 to 87 parts by weight of the carbon material and 13 to 18 parts by weight of the silicon (Si)-containing material, or 93 to 98 parts by weight of the carbon material and 2 to 7 parts by weight of the silicon (Si)-containing material relative to 100 parts by weight of the total. By adjusting the contents of the carbon material and silicon (Si)-containing material contained in the negative active material within the above ranges, the present invention can reduce the lithium consumption and irreversible capacity loss during the initial charge and discharge of the battery, and improve the charge capacity per unit mass.
[0055] Furthermore, the negative electrode mixture layer may further contain, as necessary, the conductive material, binder, and other additives mentioned in the positive electrode mixture layer.
[0056] Specifically, the negative electrode mixture layer may contain one or more conductive materials selected from the group consisting of carbon black, acetylene black, ketjen black, carbon fiber, graphene, and carbon nanotubes (e.g., single-walled carbon nanotubes (SWCNT), multi-walled carbon nanotubes (MWCNT), etc.) together with the negative electrode active material. For example, the conductive material may include acetylene black.
[0057] The conductive material may be contained in an amount of 0.1 to 10 parts by weight, specifically 0.1 to 8 parts by weight, 0.1 to 5 parts by weight, or 0.5 to 2 parts by weight, per 100 parts by weight of the composite layer.
[0058] In addition, the binder is for fixing the negative electrode active material, and may be, for example, any one of polyvinylidene fluoride (PVDF), polyacrylic acid (PAA), polymethacrylic acid (PMAA), styrene-butadiene rubber (SBR), carboxymethyl cellulose (CMC), etc., or a mixture of two or more of them.
[0059] The content of the binder may be 0.5 to 5 parts by weight, specifically 0.5 to 4 parts by weight, or 1 to 3 parts by weight, relative to 100 parts by weight of the negative electrode active material.
[0060] In addition, the negative electrode current collector is not particularly limited as long as it has high conductivity without inducing chemical changes in the battery, and for example, copper, stainless steel, nickel, titanium, calcined carbon, etc. can be used. In the case of copper or stainless steel, it is also possible to use a material that has been surface-treated with carbon, nickel, titanium, silver, etc. In addition, the negative electrode current collector can be formed with fine irregularities on the surface to strengthen the binding force with the negative electrode active material, as with the positive electrode current collector, and can be in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc. In addition, the average thickness of the negative electrode current collector can be appropriately applied in the range of 1 to 500 μm, taking into consideration the conductivity and total thickness of the negative electrode to be manufactured.
[0061] Meanwhile, in the electrode assembly for a lithium secondary battery according to the present invention, the average thickness of each composite layer constituting the positive electrode and the negative electrode and / or the average area ratio therebetween may be controlled within a certain range.
[0062] Specifically, the average thickness of the positive electrode composite layer may be 50 μm to 300 μm, and more specifically, may be 100 μm to 200 μm, 80 μm to 150 μm, 120 μm to 170 μm, 150 μm to 300 μm, 200 μm to 300 μm, 150 μm to 190 μm, 130 μm to 160 μm, 100 μm to 150 μm, or 110 μm to 160 μm.
[0063] The negative electrode mixture layer may have an average thickness of 100 μm to 300 μm, and more specifically, may have an average thickness of 100 μm to 250 μm, 100 μm to 200 μm, 100 μm to 180 μm, 100 μm to 150 μm, 120 μm to 200 μm, 140 μm to 200 μm, or 140 μm to 160 μm.
[0064] Furthermore, the ratio NA / PA of the average area PA of the positive electrode mixture layer to the average area NA of the negative electrode mixture layer may be 1.0 to 1.1, specifically, 1.0 to 1.08, 1.0 to 1.06, 1.0 to 1.04, 1.02 to 1.1, 1.04 to 1.1, 1.06 to 1.1, 1.02 to 1.08, or 1.04 to 1.06.
[0065] The present invention controls the average thickness and / or average area ratio of the positive electrode mixture layer and the negative electrode mixture layer to the above range, thereby preventing the content percentage CR of the positive electrode additive contained in the positive electrode mixture layer and the negative electrode mixture layer from decreasing during repeated charging and discharging of the lithium secondary battery. Lip and the percentage of silicon (Si)-containing substances CR Si The ratio of can be easily controlled, and high charge / discharge capacity and charge / discharge efficiency can be realized during initial charge / discharge. Specifically, if the average thickness of the positive electrode composite layer and the negative electrode composite layer exceeds 300 μm, respectively, there may be a problem of reduced safety during high-speed charging and / or overcharging of the lithium secondary battery, and if the average thickness is less than 50 μm and 100 μm, respectively, there is a limit to a significant reduction in the charge / discharge capacity of the lithium secondary battery. In addition, if the average thickness of the positive electrode composite layer is excessively thick and / or the average area is large, and therefore the average area ratio NA / PA is less than 1.0, a considerable amount of gas may be generated and expanded inside the battery during charging / discharging of the lithium secondary battery, resulting in reduced safety, and if the average thickness of the negative electrode composite layer is excessively thick and / or the average area is large, and therefore the average area ratio NA / PA exceeds 1.1, there is a limit to a significant increase in irreversible capacity during charging / discharging of the lithium secondary battery, resulting in a reduction in charge / discharge capacity and output.
[0066] In addition, the electrode assembly for a lithium secondary battery according to the present invention has a positive electrode additive content percentage CR based on the total weight of the positive electrode mixture layer. Lip and the percentage of silicon (Si)-containing material content CR based on the total weight of the negative electrode mixture layer Si Relative to CR Lip / CR Si may be 0.03 to 0.30, specifically, 0.03 to 0.25, 0.03 to 0.20, 0.03 to 0.19, 0.03 to 0.15, 0.03 to 0.1, 0.05 to 0.25, 0.1 to 0.25, 0.12 to 0.2, 0.15 to 0.2, 0.15 to 0.19, 0.05 to 0.2, 0.05 to 0.18, 0.08 to 0.19, 0.09 to 0.17, 0.1 to 0.2, 0.1 to 0.15, or 0.12 to 0.18.
[0067] In the present invention, the positive electrode additive and the silicon (Si)-containing material contained in the positive electrode and the negative electrode, respectively, are materials that participate in irreversible reactions. In the present invention, the content percentage of the positive electrode additive CR Lip and the percentage of silicon (Si)-containing material content CR based on the total weight of the negative electrode mixture layer Si Relative to CR Lip / CR Si By controlling the amount of charge and discharge in the above range, high charge and discharge capacity and charge and discharge efficiency can be achieved during the initial charge and discharge.
[0068] Moreover, the separator is an insulating thin film having high ion permeability and mechanical strength, which is interposed between the positive and negative electrodes. The separator is not particularly limited as long as it is one commonly used in the industry, and specifically, a sheet or nonwoven fabric made of chemically resistant and hydrophobic polypropylene, glass fiber, or polyethylene can be used. In some cases, a composite separator made of a porous polymer substrate such as the sheet or nonwoven fabric coated with inorganic particles / organic particles by an organic binder polymer can be used. When a solid electrolyte such as a polymer is used as the electrolyte, the solid electrolyte can also serve as the separator. The pore diameter of the separator may be an average of 0.01 to 10 μm, and the thickness may be an average of 5 to 300 μm.
[0069] <Lithium secondary battery> In one embodiment, the present invention provides a method for producing a composition comprising: A lithium secondary battery including the above-mentioned electrode assembly is provided.
[0070] The lithium secondary battery according to the present invention may have a structure in which the electrode assembly is impregnated with an electrolyte solution containing a lithium salt. Specifically, the electrode assembly may be wound in a jelly roll shape and housed in a cylindrical battery, a prismatic battery, or a pouch battery, or may be folded or stacked and folded and housed in a pouch battery. When the electrode assembly is housed in this manner, an electrolyte solution containing a lithium salt may be injected into the battery to impregnate the electrode assembly with the electrolyte solution, thereby preparing the battery.
[0071] In this case, the lithium salt-containing electrolyte may be composed of an electrolyte and a lithium salt, and the electrolyte may be a non-aqueous organic solvent, an organic solid electrolyte, an inorganic solid electrolyte, or the like.
[0072] Examples of the non-aqueous organic solvent that can be used include aprotic organic solvents such as N-methyl-2-pyrrolidinone, ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, gamma-butyrolactone, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphoric acid triester, trimethoxymethane, dioxolane derivatives, sulfolane, methylsulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl propionate, and ethyl propionate.
[0073] Examples of the organic solid electrolyte that can be used include polyethylene derivatives, polyethylene oxide derivatives, polypropylene oxide derivatives, phosphate polymers, polyagitation lysine, polyester sulfide, polyvinyl alcohol, polyvinylidene fluoride, and polymeric materials containing ionic dissociation groups.
[0074] Examples of the inorganic solid electrolyte that can be used include nitrides, halides, and sulfates of Li, such as Li3N, LiI, Li5Ni2, Li3N-LiI-LiOH, LiSiO4, LiSiO4-LiI-LiOH, Li2SiS3, Li4SiO4, Li4SiO4-LiI-LiOH, and Li3PO4-Li2S-SiS2.
[0075] The lithium salt is a substance that is easily dissolved in a non-aqueous electrolyte, and examples of the lithium salt include LiCl, LiBr, LiI, LiClO4, LiBF4, and LiB 10 Cl 10 , LiPF6, LiCF3SO3, LiCF3CO2, LiAsF6, LiSbF6, LiAlCl4, CH3SO3Li, (CF3SO2)2NLi, lithium chloroborane, lithium lower aliphatic carboxylates, lithium tetraphenylboronate, imides, etc. can be used.
[0076] In addition, for the purpose of improving charge / discharge characteristics, flame retardancy, etc., the electrolyte may contain, for example, pyridine, triethyl phosphite, triethanolamine, cyclic ether, ethylenediamine, n-glyme, hexamethylphosphoric triamide, nitrobenzene derivatives, sulfur, quinoneimine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, aluminum trichloride, etc. In some cases, in order to impart non-flammability, a halogen-containing solvent such as carbon tetrachloride or trifluoroethylene may be further contained, and in order to improve high-temperature storage characteristics, carbon dioxide gas may be further contained, and fluoroethylene carbonate (FEC), propene sultone (PRS), etc. may be further contained.
[0077] <Battery module> Moreover, in one embodiment, the present invention provides a battery module including the above-mentioned secondary battery as a unit cell, and provides a battery pack including the battery module.
[0078] The battery pack can be used as a power source for medium- to large-sized devices that require high temperature stability, long cycle characteristics, and high rate characteristics. Specific examples of such medium- to large-sized devices include power tools powered by electric motors, electric vehicles including electric vehicles (EVs), hybrid electric vehicles (HEVs), and plug-in hybrid electric vehicles (PHEVs), electric bicycles (E-bikes), electric two-wheeled vehicles including electric scooters (E-scooters), electric golf carts, and power storage systems, and more specifically, a hybrid electric vehicle (HEV) can be mentioned, but is not limited to this.
[0079] The present invention will now be described in more detail with reference to examples and experimental examples.
[0080] However, the following examples and experimental examples are merely illustrative of the present invention, and the contents of the present invention are not limited to the following examples and experimental examples.
[0081] <Examples 1 to 6 and Comparative Examples 1 to 8> Inject N-methylpyrrolidone solvent into the homo mixer, and add LiNi as the positive electrode active material to form the positive electrode mixture layer. 0.8 Co 0.1 Mn 0.1 The positive electrode slurry was prepared by weighing and adding the following amounts of O2, carbon black as a conductive material, PVDF as a binder, and Li6CoO4 as a positive electrode additive as shown in Tables 1 and 2 below, and mixing for 60 minutes at 3,000 rpm. The positive electrode slurry was applied to one side of an aluminum current collector, dried at 100°C, and rolled to prepare a positive electrode. At this time, the total thickness and average area of the positive electrode mixture layer were 130 μm and 1260±50 mm, respectively. 2 The total thickness of the produced positive electrode was about 200 μm.
[0082] In addition, natural graphite and silicon (SiOx, where 1≦x≦2) particles as negative electrode active materials; a mixture of carbon black and single-walled carbon nanotubes (SWCNT) (mixing ratio=1:1 wt. / wt.) as conductive materials; and styrene butadiene rubber (SBR) and carboxymethyl cellulose (CMC) as binders were prepared, and a negative electrode slurry was prepared in the same manner as the positive electrode slurry, with reference to Tables 1 and 2 below. At this time, the graphite used in the preparation of the negative electrode mixture layer was natural graphite (average particle size: 10 to 30 μm), and the silicon (SiOx) particles had an average particle size of 3 to 10 μm. The prepared negative electrode slurry was applied to one side of a copper current collector, dried at 100° C., and rolled to prepare a negative electrode. At this time, the total thickness and average area of the negative electrode mixture layer were 150 μm and 1333±50 mm 2The total thickness of the produced negative electrode was about 250 μm.
[0083] Here, the content percentage CR of the positive electrode additive based on the total weight of the positive electrode mixture layer Lip and the percentage of silicon (SiOx) particles based on the total weight of the negative electrode mixture layer CR Si Relative to CR Lip / CR Si are shown in Tables 1 and 2.
[0084] Next, a separator (thickness: about 16 μm) made of a porous polyethylene (PE) film was placed between the prepared positive and negative electrodes, and E2DVC was injected as an electrolyte to prepare a full cell.
[0085] Here, "E2DVC" refers to a type of carbonate-based electrolyte, a solution in which lithium hexafluorophosphate (LiPF6, 1.0M) and vinyl carbonate (VC, 2% by weight) are mixed with a mixture of ethylene carbonate (EC): dimethyl carbonate (DMC): diethyl carbonate (DEC) = 1:1:1 (volume ratio).
[0086] [Table 1]
[0087] [Table 2]
[0088] <Experimental Example> In order to evaluate the performance of the electrode assembly manufactured according to the present invention, the following experiment was carried out.
[0089] a) Measurement of gas emission amount The cells prepared in Examples 1 to 6 and Comparative Examples 1 to 8 were charged and discharged once at 25°C and 0.1C / 0.1C to perform formation, and the amount of oxygen gas generated was analyzed. The results are shown in Table 3 below.
[0090] b) Evaluation of electrical performance The cells manufactured in Examples 1 to 6 and Comparative Examples 1 to 8 were charged at a temperature of 25° C. with a charge current of 0.05C to a charge end voltage of 4.2 to 4.25V, and then charged until the current density reached 0.01C at 0.02V. Thereafter, the cells were discharged to a charge end voltage of 2V with a discharge current of 0.05C, and one charge / discharge (≒initial charge / discharge) was performed. The charge / discharge capacity of the cell was measured during the charge / discharge, and the initial efficiency was calculated according to the following formula 1. After one charge / discharge, the cells were charged / discharged at a current of 0.5C for 100 cycles, and the charge / discharge capacity of the cell was measured in the same manner as the initial charge / discharge, and the capacity retention rate after 100 charge / discharge cycles was calculated according to the following formula 2. The results are shown in Table 3 below.
[0091] [Formula 1] Initial efficiency (%) = (1st discharge capacity / 1st charge capacity) x 100
[0092] [Formula 2] Capacity retention rate (%) = (100th discharge capacity / 1st discharge capacity) x 100
[0093] [Table 3]
[0094] As shown in Table 3 above, it can be seen that the electrode assembly according to the embodiment of the present invention has the effect of improving the performance of the battery.
[0095] Specifically, the electrode assembly of the embodiment had a high initial charge / discharge capacity and efficiency of 50.7 mAh or more and 80.6% or more, respectively, and maintained a cell capacity of 88% or more even after 100 repeated charge / discharge cycles.In addition, the electrode assembly for a lithium secondary battery generates oxygen gas due to the positive electrode additive according to the following reaction formula, but it was confirmed that the electrode assembly of the embodiment generated less oxygen gas than the electrode assembly of the comparative example, even though the same amount of positive electrode additive was contained in the positive electrode mixture layer.
[0096] [ka]
[0097] From these results, the electrode assembly for a lithium secondary battery according to the present invention has a ratio CR of the content percentage of the positive electrode additive and the silicon (Si)-containing material as the negative electrode active material contained in the positive electrode mixture layer and the negative electrode mixture layer, respectively. Lip / CR Si Within a specific range, the ratio and / or efficiency of reversible and irreversible reactions of lithium ions in the electrode assembly can be controlled, so that high charge / discharge capacity and charge / discharge efficiency can be realized during initial charge / discharge, and capacity retention is excellent during subsequent charge / discharge. A lithium secondary battery including the same has the advantages of high energy density and long life.
[0098] Although the present invention has been described above with reference to preferred embodiments thereof, it will be understood that a person skilled in the art or having ordinary knowledge in the art can make various modifications and variations to the present invention without departing from the spirit and technical scope of the present invention as described in the claims below.
[0099] Therefore, the technical scope of the present invention should not be limited to the contents described in the detailed description of the specification, but should be defined by the claims.
Claims
1. A positive electrode including a positive electrode active material and a positive electrode additive represented by the following chemical formula 1 in a positive electrode mixture layer; a negative electrode including a carbon material and a silicon (Si)-containing material as a negative electrode active material in a negative electrode mixture layer; A separator located between the positive electrode and the negative electrode, The content of the positive electrode additive is 0.01 to 5 parts by weight based on 100 parts by weight of the positive electrode mixture layer, and The percentage of the positive electrode additive based on the total weight of the positive electrode mixture layer CR Lip and the content percentage CR of silicon (Si)-containing material based on the total weight of the negative electrode mixture layer Si Relative to CR Lip / CR Si is 0.03 to 0.30, The negative electrode active material includes 75 to 99 parts by weight of the carbon material and 1 to 25 parts by weight of the silicon (Si)-containing material, based on 100 parts by weight of the negative electrode active material. [Chemical formula 1] Li p Co (1-q) M 1 q O 4 In the above Chemical Formula 1, M 1 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; p and q are 5≦p≦7 and 0≦q≦0.5, respectively.
2. The percentage of the positive electrode additive based on the total weight of the positive electrode mixture layer CR Lip and the content percentage CR of silicon (Si)-containing material based on the total weight of the negative electrode mixture layer Si Relative to CR Lip / CR Si 2. The electrode assembly for a lithium secondary battery according to claim 1, wherein is 0.05 to 0.
20.
3. The positive electrode additive has a space group of P4 22. The electrode assembly for a lithium secondary battery according to claim 1, having a tetragonal structure in which N is a cubic lattice constant.
4. 2. The electrode assembly for a lithium secondary battery according to claim 1, wherein the positive electrode active material is a lithium metal composite oxide represented by the following Chemical Formula 2: [Chemical formula 2] Li x [Ni y Co z Mn w M 2 v ]O u In the above Chemical Formula 2, M 2 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; x, y, z, w, v, and u are within the ranges of 1.0≦x≦1.30, 0≦y<0.95, 0<z≦0.5, 0<w≦0.5, 0≦v≦0.2, and 1.5≦u≦4.5, respectively.
5. 2. The electrode assembly for a lithium secondary battery according to claim 1, wherein the carbon material comprises at least one material selected from the group consisting of natural graphite, artificial graphite, graphene, and carbon nanotubes.
6. 6. The electrode assembly for a lithium secondary battery according to claim 5, wherein the carbon material comprises at least one of graphene and carbon nanotubes, and is contained in an amount of 0.1 to 10 parts by weight based on 100 parts by weight of the total carbon material.
7. 2. The electrode assembly for a lithium secondary battery according to claim 1, wherein the positive electrode mixture layer contains 0.1 to 5 parts by weight of a conductive material based on the total weight of the positive electrode mixture layer.
8. 2. The electrode assembly for a lithium secondary battery according to claim 1, wherein the positive electrode mixture layer contains one or more conductive materials selected from the group consisting of natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, and carbon fiber.
9. Silicon (Si)-containing materials include silicon (Si), silicon monoxide (SiO) and silicon dioxide (SiO 2 2. The electrode assembly for a lithium secondary battery according to claim 1, comprising at least one of the following:
10. The average thickness of the positive electrode mixture layer is 50 μm to 300 μm, 2. The electrode assembly for a lithium secondary battery according to claim 1, wherein the average thickness of the negative electrode mixture layer is 100 to 300 μm.
11. 2. The electrode assembly for a lithium secondary battery according to claim 1, wherein an average area ratio of the negative electrode mixture layer to the positive electrode mixture layer is 1.0 to 1.
1.
12. A lithium secondary battery comprising the electrode assembly according to claim 1.
Citation Information
Patent Citations
Power storage device
JP2015088268A
Lithium ion secondary battery and manufacturing method thereof
JP2018185905A
Lithium ion secondary battery
JP2019046689A