Inorganic filler dispersant, inorganic filler masterbatch, resin composition, method for producing same, and molded product

A block copolymer dispersant addresses the dispersion issues of inorganic fillers in acrylic resin compositions, achieving high-gloss and well-colored molded products by effectively dispersing fillers like carbon black.

JP7551365B2Active Publication Date: 2024-09-17TECHNO UMG CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020118204
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-07-09
Publication Date
2024-09-17
Estimated Expiration
2040-07-09

AI Technical Summary

Technical Problem

Acrylic resin compositions face issues with poor dispersion of carbon black and other inorganic fillers, leading to insufficient color development, deterioration of molded appearance, and difficulty in achieving high gloss due to filler aggregation.

Method used

The use of a block copolymer dispersant consisting of aromatic vinyl and vinyl cyanide units for block (A) and (meth)acrylic acid ester units for block (B) to disperse inorganic fillers, such as carbon black, within acrylic resin compositions, combined with an inorganic filler masterbatch and resin composition production methods.

Benefits of technology

The block copolymer effectively disperses inorganic fillers, suppressing aggregation and enhancing the functions of fillers, resulting in high-gloss molded products with improved color development and appearance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007551365000003
    Figure 0007551365000003
  • Figure 0007551365000004
    Figure 0007551365000004
  • Figure 0007551365000002
    Figure 0007551365000002
Patent Text Reader

Abstract

To provide an inorganic filler dispersant and an inorganic filler dispersant masterbatch which enable an inorganic filler to be satisfactorily dispersed in an acrylic resin, suppress generation of an aggregate of the inorganic filler, sufficiently exhibit a function of the inorganic filler, and enable production of a resin composition obtaining a high-gloss molding.SOLUTION: An inorganic filler dispersant is a block copolymer (C) which is composed of a block (A) having an aromatic vinyl unit and a vinyl cyanide unit, and a block (B) having a (meth)acrylate unit. An inorganic filler masterbatch contains the inorganic filler dispersant and an inorganic filler.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an inorganic filler dispersant, an inorganic filler masterbatch, a resin composition, a method for producing the same, and a molded article. [Background technology]

[0002] Molded products made from resin compositions colored black are used in a variety of applications. Acrylic resins such as polymethyl methacrylate (PMMA) are widely used as resins because of their high transparency, excellent color development when colored, and excellent weather resistance. 2. Description of the Related Art In recent years, in the fields of vehicles, building materials, office automation equipment, home appliances and the like, there has been a demand for resin compositions that are highly jet black, have high gloss and are excellent in appearance after molding.

[0003] Acrylic resins have high transparency, so that they can be colored with dyes to give a good jet black color. However, resin compositions containing acrylic resins and dyes have poor weather resistance due to the poor weather resistance of the dyes themselves, and also have the problem of easily contaminating the mold during molding. Therefore, coloring of acrylic resin with pigments, particularly carbon black, has been investigated (Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2011 / 152449 Summary of the Invention [Problem to be solved by the invention]

[0005] However, acrylic resin has low affinity with carbon black, and the poor dispersion of carbon black can lead to problems such as insufficient color development (jet blackness) and deterioration of the molded appearance due to carbon black agglomerates. In particular, when small particles of carbon black are used to improve jet blackness, the surface area of ​​the carbon black increases and agglomerates are likely to form. In addition, because acrylic resin is highly transparent, there is also the problem that it is difficult to develop gloss when colored with carbon black. The same problem occurs when inorganic pigments other than carbon black are used.

[0006] In addition, in order to add functions according to increasingly diverse applications, the addition of inorganic fillers other than inorganic pigments may be required. For example, in order to improve rigidity, the addition of glass fillers, glass beads, carbon fibers, carbon nanotubes, cellulose nanofibers, titanium oxide, wollastonite, etc. may be required. However, the addition of such inorganic fillers also has the same problems as the addition of carbon black, such as problems due to poor dispersion of the inorganic fillers (functions of the inorganic fillers are not fully expressed, and the appearance of the molded product is deteriorated due to aggregates of the inorganic fillers) and problems of difficulty in expressing gloss.

[0007] An object of one aspect of the present invention is to provide an inorganic filler dispersant and an inorganic filler masterbatch capable of producing a resin composition which can satisfactorily disperse an inorganic filler in an acrylic resin, suppress the generation of inorganic filler agglomerates, fully express the function of the inorganic filler (e.g., color development by an inorganic pigment), and give a highly glossy molded article; a resin composition and its production method which can suppress the generation of inorganic filler agglomerates, fully express the function of the inorganic filler, and give a highly glossy molded article; and a resin composition and its production method which can suppress the generation of inorganic filler agglomerates, fully express the function of the inorganic filler, and give a highly glossy molded article; [Means for solving the problem]

[0008] The present invention has the following aspects. [1] An inorganic filler dispersant which is a block copolymer (C) consisting of a block (A) having an aromatic vinyl unit and a vinyl cyanide unit, and a block (B) having a (meth)acrylic acid ester unit. [2] An inorganic filler masterbatch comprising the inorganic filler dispersant of [1] and an inorganic filler. [3] A resin composition comprising the inorganic filler dispersant of [1], an inorganic filler, and an acrylic resin. [4] A method for producing a resin composition, comprising melt-kneading the inorganic filler masterbatch of [2] above with an acrylic resin. [5] A molded article comprising the resin composition according to [3]. Effect of the Invention

[0009] According to the inorganic filler dispersant or inorganic filler masterbatch of the present invention, the inorganic filler can be well dispersed in the acrylic resin, the generation of aggregates of the inorganic filler is suppressed, the functions of the inorganic filler are fully exerted, and a resin composition which can give a highly glossy molded product can be produced. According to the resin composition of the present invention, the generation of aggregates of the inorganic filler is suppressed, the functions of the inorganic filler are fully exerted, and a highly glossy molded article can be obtained. The molded article of the present invention is highly glossy because the generation of aggregates of the inorganic filler is suppressed and the functions of the inorganic filler are fully exerted. [Brief description of the drawings]

[0010] [Figure 1] 1 is a laser microscope image (magnification: 50x) of a molded article of the resin composition of Example 2. [Diagram 2] 1 is a laser microscope image (magnification: 50x) of a molded article of the resin composition of Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] In this specification, number average molecular weight is also referred to as "Mn" and weight average molecular weight is also referred to as "Mw". Mw and Mn are values ​​calculated using standard polystyrene as measured by gel permeation chromatography (hereinafter also referred to as "GPC").

[0012] [Inorganic filler dispersant] The inorganic filler dispersant according to one embodiment of the present invention (hereinafter also referred to as "the present dispersant") is a block copolymer (C). The block copolymer (C) comprises a block (A) having an aromatic vinyl unit and a vinyl cyanide unit, and a block (B) having a (meth)acrylic ester unit. The dispersant is used to disperse inorganic fillers in acrylic resins.

[0013] Block Block (A) is a copolymer having an aromatic vinyl unit and a vinyl cyanide unit. Block (A) may further have other monomer units depending on the desired physical properties, as long as the properties of block (A) are not impaired.

[0014] Examples of aromatic vinyls include styrene, α-methylstyrene, o-, m- or p-methylstyrene, vinylxylene, pt-butylstyrene, ethylstyrene, etc. These aromatic vinyls may be used alone or in combination of two or more. Examples of vinyl cyanides include acrylonitrile, methacrylonitrile, etc. These vinyl cyanides may be used alone or in combination of two or more.

[0015] The other monomers in block (A) may be any monomer capable of copolymerizing with aromatic vinyl and vinyl cyanide, and may include, for example, (meth)acrylic acid esters, maleic anhydride, N-substituted maleimide, (meth)acrylic acid, methacrylic acid, acrylamide, methacrylamide, etc. Examples of (meth)acrylic acid esters include the same as the (meth)acrylic acid esters in block (B) described below. These other monomers may be used alone or in combination of two or more.

[0016] The content of the aromatic vinyl unit is preferably 50 to 95% by mass, more preferably 60 to 80% by mass, based on 100% by mass of all monomer units constituting the block (A). When the content of the aromatic vinyl unit is within the above range, the dispersibility of the inorganic filler is improved.

[0017] The content of the vinyl cyanide unit is preferably 5 to 50 mass%, more preferably 20 to 40 mass%, based on 100 mass% of all monomer units constituting the block (A). When the content of the vinyl cyanide unit is within the above range, the gloss of the molded article becomes better.

[0018] The total content of the aromatic vinyl units and the vinyl cyanide units is preferably 50% by mass or more, more preferably 70% by mass or more, and may be 100% by mass, based on 100% by mass of all monomer units constituting the block (A).

[0019] The Mw of the block (A) is preferably 5,000 to 300,000, more preferably 20,000 to 150,000, and even more preferably 35,000 to 80,000. When the Mw of the block (A) is within the above range, the block (A) is easily adsorbed to the inorganic filler, resulting in good dispersibility, and also reducing adverse effects on the physical properties (such as impact resistance) of the acrylic resin.

[0020] Block The block (B) is a polymer having a (meth)acrylic acid ester unit. The block (B) may further have other monomer units depending on the desired physical properties, as long as the properties of the block (B) are not impaired.

[0021] "(Meth)acrylic acid ester" is a general term for methacrylic acid ester and acrylic acid ester. Examples of methacrylic acid esters include methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, i-propyl methacrylate, n-butyl methacrylate, i-butyl methacrylate, t-butyl methacrylate, amyl methacrylate, isoamyl methacrylate, octyl methacrylate, 2-ethylhexyl methacrylate, decyl methacrylate, lauryl methacrylate, stearyl methacrylate, cyclohexyl methacrylate, benzyl methacrylate, and phenyl methacrylate. Examples of acrylic esters include methyl acrylate, ethyl acrylate, n-propyl acrylate, i-propyl acrylate, n-butyl acrylate, i-butyl acrylate, t-butyl acrylate, amyl acrylate, isoamyl acrylate, octyl acrylate, 2-ethylhexyl acrylate, decyl acrylate, lauryl acrylate, stearyl acrylate, cyclohexyl acrylate, benzyl acrylate, and phenyl acrylate.

[0022] The other monomers in block (B) may be any monomers capable of copolymerizing with the (meth)acrylic acid ester, and examples thereof include aromatic vinyl, vinyl cyanide, maleic anhydride, N-substituted maleimide, (meth)acrylic acid, methacrylic acid, acrylamide, methacrylamide, etc. Examples of the aromatic vinyl and vinyl cyanide include the same as those in block (A). These other monomers may be used alone or in combination of two or more.

[0023] The content of the (meth)acrylic acid ester units is preferably 50% by mass or more, more preferably 70% by mass or more, and may be 100% by mass, based on 100% by mass of all monomer units constituting the block (B).

[0024] The Mw of the block (B) is preferably 20,000 to 300,000, more preferably 20,000 to 150,000, and even more preferably 35,000 to 90,000. When the Mw of the block (B) is within the above range, the inorganic filler adsorbed in the block (A) is easily dispersed in the acrylic resin, and adverse effects on the physical properties (such as impact resistance) of the acrylic resin are reduced.

[0025] [Block copolymer (C)] The block copolymer (C) comprises a block (A) and a block (B). The block copolymer (C) may have one or more blocks (A) and the block copolymer (C) may have one or more blocks (B).

[0026] Examples of the block copolymer (C) include a diblock copolymer represented by AB, a triblock copolymer represented by ABA or BAB, and a tetrablock or higher polyblock copolymer in which A and B are alternately linked. Here, A represents block (A) and B represents block (B). As the structure of the block copolymer (C), a diblock copolymer represented by AB is preferred from the viewpoints of dispersibility in inorganic fillers, adsorption to inorganic fillers, dispersibility in acrylic resins, and ease of production.

[0027] In the block copolymer (C), the mass ratio of block (A) to block (B) (block (A):block (B)) is preferably 10:90 to 90:10, more preferably 20:80 to 80:20, and even more preferably 35:65 to 65:35. When this mass ratio is within the above range, the dispersibility of the inorganic filler, the adsorption to the inorganic filler, and the dispersibility in the acrylic resin are good.

[0028] The Mw of the block copolymer (C) is preferably 25,000 to 350,000, more preferably 30,000 to 250,000, and even more preferably 50,000 to 200,000. When the Mw of the block copolymer (C) is within the above range, the dispersibility of the inorganic filler in the acrylic resin is improved, and adverse effects on the physical properties (such as impact resistance) of the acrylic resin are reduced. The molecular weight dispersity (Mw / Mn) of the block copolymer (C) is preferably 1.0 to 5.0, more preferably 1.0 to 2.5. When the molecular weight dispersity is equal to or less than the above upper limit, the adsorption to inorganic fillers and the dispersibility in acrylic resins are improved.

[0029] [Method for producing block copolymer (C)] The method for producing the block copolymer (C) is not particularly limited, but examples thereof include the following methods. (1) A method of reacting a previously synthesized block (A) (a copolymer of aromatic vinyl and vinyl cyanide) having a reactive functional group at its terminal with a block (B) (a (meth)acrylic acid ester polymer) having a reactive functional group at its terminal. (2) A method of polymerizing a monomer component containing a (meth)acrylic acid ester (or a monomer component containing an aromatic vinyl and a vinyl cyanide) in the presence of a block (A) having a mercapto group (or a block (B) having a mercapto group). (3) A method of sequentially polymerizing the monomers constituting each block of the block copolymer (C) by living radical polymerization. In the above method (1), examples of the reactive functional group include an amino group, a carboxyl group, a hydroxyl group, and an isocyanate group.

[0030] Among the above methods, the method (3) is preferred since it is easy to control the structure of the block copolymer (C). Examples of living radical polymerization methods include the NMP method (nitroxide-mediated radical polymerization method), the ATRP method (atom transfer radical polymerization method), the TERP method (radical polymerization method using an organotellurium compound), and the RAFT polymerization method (reversible addition-fragmentation chain transfer polymerization method). Among these, the RAFT polymerization method is preferred because it allows polymerization under mild conditions and is compatible with a variety of monomers.

[0031] In the RAFT polymerization process, monomers are polymerized in the presence of a RAFT agent (reversible addition-fragmentation chain transfer agent). The polymerization method in the RAFT polymerization method is not particularly limited, and examples thereof include solution polymerization, suspension polymerization, mini-emulsion polymerization, etc. Among these, mini-emulsion polymerization is preferred from the viewpoints of low VOC and excellent safety of the working environment because no organic solvent is used, and excellent productivity.

[0032] Examples of a method for producing block copolymer (C) by mini-emulsion polymerization using a RAFT polymerization method include a method having a step of mini-emulsifying a mixed liquid containing a monomer constituting block (A) (hereinafter also referred to as "monomer component (a)"), a RAFT agent, a hydrophobic substance, an emulsifier, water, and, if necessary, an initiator; a step of heating the obtained mini-emulsion to a polymerization initiation temperature to polymerize the monomer component (a) to obtain an aqueous dispersion of block (A); and a step of dropping a monomer constituting block (B) (hereinafter also referred to as "monomer component (b)") into the obtained aqueous dispersion of block (A) to polymerize it. Although an example in which the monomer component (a) is polymerized and then the monomer component (b) is polymerized has been shown here, the monomer component (a) may be polymerized after the monomer component (b) has been polymerized. Also, the method for producing the block copolymer (C) is not limited to the above method.

[0033] Monomer component (a) contains aromatic vinyl and vinyl cyanide, and may further contain other monomers. The content (mass%) of each of aromatic vinyl and vinyl cyanide relative to 100 mass% of monomer component (a) is the same as the content of each of aromatic vinyl units and vinyl cyanide units relative to 100 mass% of all monomer units constituting block (A).

[0034] Monomer component (b) contains a (meth)acrylic acid ester and may further contain other monomers. The content (mass%) of the (meth)acrylic acid ester relative to 100 mass% of monomer component (b) is the same as the content of the (meth)acrylic acid ester units relative to 100 mass% of all monomer units constituting block (B).

[0035] The RAFT agent used in the RAFT polymerization method is a compound that causes RAFT polymerization, and is generally a compound having a structure represented by the following formula 1 (thiocarbonylthio compounds such as dithiobenzoates, trithiocarbonates, dithiocarbamates, and xanthates).

[0036] [ka] Z is a functional group that controls the reactivity of the C=S bond and affects the rate of addition and cleavage of radicals, and R is a good homolytic leaving group for the propagating radical that restarts the polymerization reaction.

[0037] The substituents Z and R must be appropriately selected depending on the monomer to be used, and there are many references providing guidance therefor, such as those shown in the following references: Keddie, DJ, Moad, G., Rizzardo, E., Thang, SH: Macromolecules, 45, 5321 (2012).

[0038] More specifically, the RAFT agent includes, but is not limited to, S,S-dibenzyltrithiocarbonate, 2-[(dodecylsulfanylthiocarbonyl)sulfanyl]propanoic acid, 4-cyano-4-(dodecylsulfanylthiocarbonyl)sulfanylpentanoic acid, 2-{[(2-carboxyethyl)sulfanylthiocarbonyl]sulfanyl}propanoic acid, 2'-cyanobutan-2'-yl 4-chloro-3,5-dimethylpyrazole-1-carbodithioate, 4-[(2-carboxyethylsulfanylthiocarbonyl)sulfanyl]-4-cyanopentanoic acid, 3,5-dimethylpyrazole-1-carbodithioate 2'-cyanobutan-2'-yl, Examples of such compounds include cyanomethyl 3,5-dimethylpyrazole-1-carbodithioate, cyanomethyl N-methyl-N-phenyldithiocarbamate, methyl 4-cyano-4-[(dodecylsulfanylthiocarbonyl)sulfanyl]pentanoate, bis[4-(allyloxycarbonyl)benzyl] trithiocarbonate, bis[4-(2,3-dihydroxypropoxycarbonyl)benzyl] trithiocarbonate, bis{4-[ethyl-(2-acetyloxyethyl)carbamoyl]benzyl} trithiocarbonate, bis{4-[ethyl-(2-hydroxyethyl)carbamoyl]benzyl} trithiocarbonate, and bis[4-(2-hydroxyethoxycarbonyl)benzyl] trithiocarbonate.

[0039] The amount of the RAFT agent used is, for example, 0.05 to 3 parts by mass per 100 parts by mass of the total of the monomer components (a) and (b). When the amount of the RAFT agent used is within the above range, it is easy to control the structure of the block copolymer (C).

[0040] When the block copolymer (C) is produced by mini-emulsion polymerization using the RAFT polymerization method, a hydrophobic substance can be used. When the mini-emulsion is produced in the presence of a hydrophobic substance, the production stability of the mini-emulsion polymerization is further improved. If miniemulsion is performed in the absence of a hydrophobic substance, the productivity of block copolymer (C) may decrease due to monomer transfer between micelles caused by Ostwald ripening and coalescence of monomer oil droplets. In addition, monomer transfer may easily generate new small particles without the presence of a RAFT agent, and polymers may be generated by normal radical polymerization instead of living radical polymerization, resulting in the generation of a large amount of polymer that is not a block copolymer.

[0041] Examples of hydrophobic substances include hydrocarbons having 10 or more carbon atoms, alcohols having 10 or more carbon atoms, hydrophobic polymers having Mn of 10,000 or less, hydrophobic monomers (for example, vinyl esters of alcohols having 10 to 30 carbon atoms, vinyl ethers of alcohols having 12 to 30 carbon atoms, (meth)acrylic acid alkyl esters having an alkyl group having 12 to 30 carbon atoms, carboxylic acid vinyl esters having an alkyl group having 10 to 30 carbon atoms (preferably 10 to 22 carbon atoms), p-alkylstyrenes), hydrophobic chain transfer agents, hydrophobic peroxides, etc. These may be used alone or in combination of two or more kinds.

[0042] More specific examples of hydrophobic substances include hexadecane, octadecane, icosane, liquid paraffin, liquid isoparaffin, paraffin wax, polyethylene wax, olive oil, cetyl alcohol, stearyl acrylate, lauryl acrylate, stearyl acrylate, lauryl methacrylate, stearyl methacrylate, polystyrene with Mn of 500 to 10,000, poly(meth)acrylic acid esters, and the like.

[0043] The amount of the hydrophobic substance used is preferably 0.1 to 20 parts by mass, more preferably 0.5 to 10 parts by mass, and even more preferably 2 to 10 parts by mass, based on 100 parts by mass of the total of the monomer components (a) and (b). When the amount of the hydrophobic substance used is within the above range, the block copolymer (C) can be stably obtained. In addition, when the block copolymer (C) is used as an inorganic filler master batch, adverse effects such as gas generation and bleed-out are unlikely to occur.

[0044] Examples of the emulsifier include anionic surfactants, nonionic surfactants, and amphoteric surfactants. More specifically, examples of the emulsifier include anionic surfactants such as sulfate esters of higher alcohols (e.g., alcohols having 6 to 30 carbon atoms), alkylbenzenesulfonates, fatty acid sulfonates, phosphates (e.g., ammonium monoglyceride phosphate), fatty acid salts (e.g., dipotassium alkenylsuccinate), and amino acid derivative salts; nonionic surfactants such as alkyl esters, alkyl ethers, and alkyl phenyl ethers of polyethylene glycol; and amphoteric surfactants having a carboxylate, sulfate ester salt, sulfonate, phosphate ester salt, or the like in the anion portion and an amine salt, quaternary ammonium salt, or the like in the cation portion. These emulsifiers may be used alone or in combination of two or more kinds.

[0045] The amount of the emulsifier used is preferably 0.01 to 10 parts by mass, more preferably 0.5 to 10 parts by mass, per 100 parts by mass of the total of the monomer components (a) and (b). When the amount of the emulsifier used is within the above range, the block copolymer (C) can be stably produced.

[0046] The initiator may be any radical polymerization initiator for radical polymerization, and the type is not particularly limited, but examples thereof include azo polymerization initiators, photopolymerization initiators, inorganic peroxides, organic peroxides, and redox initiators combining organic peroxides with transition metals and reducing agents. Among these, azo polymerization initiators, inorganic peroxides, organic peroxides, and redox initiators are preferred, and azo polymerization initiators and organic peroxides are more preferred, in that polymerization can be initiated by heating. These may be used alone or in combination of two or more.

[0047] Examples of the azo polymerization initiator include 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), 1,1'-azobis(cyclohexane-1-carbonitrile), 1-[(1-cyano-1-methylethyl)azo]formamide, 4,4'-azobis(4-cyanovaleric acid), dimethyl 2,2'-azobis( 2-methylpropionate), dimethyl 1,1'-azobis(1-cyclohexanecarboxylate), 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)propionamide], 2,2'-azobis(N-butyl-2-methylpropionamide), 2,2'-azobis(N-cyclohexyl-2-methylpropionamide), 2,2'-azobis[2-(2-imidazolin-2-yl)propane], 2,2'-azobis(2,4,4-trimethylpentane), and the like.

[0048] Examples of inorganic peroxides include potassium persulfate, sodium persulfate, ammonium persulfate, and hydrogen peroxide.

[0049] Examples of organic peroxides include peroxyester compounds, and specific examples thereof include α,α'-bis(neodecanoylperoxy)diisopropylbenzene, cumylperoxyneodecanoate, 1,1,3,3-tetramethylbutylperoxyneodecanoate, 1-cyclohexyl-1-methylethylperoxyneodecanoate, t-hexylperoxyneodecanoate, t-butylperoxyneodecanoate, t-hexylperoxypivalate, t-butylperoxypivalate, 1,1,3,3-tetramethylbutylperoxy -2-ethylhexanoate, 2,5-dimethyl-2,5-bis(2-ethylhexanoylperoxy)hexane, 1-cyclohexyl-1-methylethylperoxy-2-ethylhexanoate, t-hexylperoxy 2-hexylhexanoate, t-butylperoxy 2-hexylhexanoate, t-butylperoxyisobutyrate, t-hexylperoxyisopropylmonocarbonate, t-butylperoxymaleic acid, t-butylperoxy 3,5,5-trimethylhexanoate, t-butylperoxylaurate, 2,5 -Dimethyl-2,5-bis(m-toluoylperoxy)hexane, t-butylperoxyisopropyl monocarbonate, t-butylperoxy2-ethylhexyl monocarbonate, t-hexylperoxybenzoate, 2,5-dimethyl-2,5-bis(benzoylperoxy)hexane, t-butylperoxyacetate, t-butylperoxy-m-toluoylbenzoate, t-butylperoxybenzoate, bis(t-butylperoxy)isophthalate, 1,1-bis(t-hexylperoxy)3,3,5-trimethylcyclohexa 1,1-bis(t-hexylperoxy)cyclohexane, 1,1-bis(t-butylperoxy)3,3,5-trimethylcyclohexane, 1,1-bis(t-butylperoxy)cyclohexane, 1,1-bis(t-butylperoxy)cyclododecane, 2,2-bis(t-butylperoxy)butane, n-butyl 4,4-bis(t-butylperoxy)valerate, 2,2-bis(4,4-di-t-butylperoxycyclohexyl)propane, α,α'-bis(t-butylperoxy)diisopropylbenzene, dicumyl peroxide, 2,Examples of the peroxy groups include 5-dimethyl-2,5-bis(t-butylperoxy)hexane, t-butylcumyl peroxide, di-t-butyl peroxide, cumene hydroperoxide, diisopropylbenzene hydroperoxide, dilauroyl peroxide, diisononanoyl peroxide, t-butyl hydroperoxide, benzoyl peroxide, lauroyl peroxide, dimethylbis(t-butylperoxy)-3-hexyne, bis(t-butylperoxyisopropyl)benzene, bis(t-butylperoxy)trimethylcyclohexane, butyl-bis(t-butylperoxy)valerate, 2-ethylhexaneperoxy acid t-butyl, dibenzoyl peroxide, paramenthane hydroperoxide, and t-butyl peroxybenzoate.

[0050] The redox initiator is preferably a combination of an organic peroxide, ferrous sulfate, a chelating agent, and a reducing agent, such as a combination of cumene hydroperoxide, ferrous sulfate, sodium pyrophosphate, and dextrose, or a combination of t-butyl hydroperoxide, sodium formaldehyde sulfoxylate (Rongalit), ferrous sulfate, and disodium ethylenediaminetetraacetate.

[0051] The amount of the initiator used is preferably 0.03 to 2 parts by mass per 100 parts by mass of the total of the monomer components (a) and (b). If the amount of the initiator used is within the above range, the block copolymer (C) can be stably obtained.

[0052] The mixture can be prepared by mixing the monomer component (a), a RAFT agent, a hydrophobic substance, an emulsifier, water, and, if necessary, an initiator. The mixing method is not particularly limited, but for example, a method of preparing an oil phase by mixing the monomer component (a), a RAFT agent, a hydrophobic substance, and optionally an initiator, and then adding an emulsifier and water to the oil phase and mixing them may be mentioned. The emulsifier and water may be added separately, or they may be mixed in advance and added as an aqueous emulsifier solution. The amount of water used is, for example, 80 to 1000 parts by mass per 100 parts by mass of the monomer component (a).

[0053] In the process of forming the mixed liquid into a mini-emulsion, for example, the mixed liquid is subjected to a shearing treatment. The shearing treatment breaks apart the oil droplets containing the monomer component (a), forming minute oil droplets covered with the emulsifier. This results in a mini-emulsion. The shearing treatment method may be any known method, for example, a method using a high shearing device. The high shearing device capable of forming a mini-emulsion is not particularly limited, but may be, for example, an emulsifying device consisting of a high-pressure pump and an interaction chamber, or a device for forming a mini-emulsion by ultrasonic energy or high frequency. The emulsification device consisting of a high-pressure pump and an interaction chamber is not particularly limited, but examples thereof include the "Pressure Homogenizer" manufactured by SPX Corporation APV, the "Pressure Homogenizer" manufactured by Sanmaru Machinery Industry Co., Ltd., and the "Microfluidizer" manufactured by Powrex Corporation. The device for forming a mini-emulsion by ultrasonic energy or high frequency is not particularly limited, but examples thereof include "Sonic Dismembrator" manufactured by Fisher Scientific and "ULTRASONIC HOMOGENIZER" manufactured by Nippon Seiki Seisakusho Co., Ltd.

[0054] The 50% particle size of the fine oil droplets in the mini-emulsion is preferably 10 to 300 nm, more preferably 30 to 150 nm. When the 50% particle size of the fine oil droplets is within the above range, the reactivity is good and the block (A) can be produced with good productivity. The 50% particle size is the particle size at which the cumulative value is 50% in the volume-based particle size distribution measured by dynamic light scattering. The 50% particle size can be adjusted, for example, by changing the amount of emulsifier used, the amount of water used, the pressure of the pressure homogenizer, etc., and adjusting the shear force of the high shear device.

[0055] By heating the miniemulsion to a polymerization initiation temperature, the monomer component (a) in the minute oil droplets is polymerized to generate fine particles of block (A), thereby obtaining an aqueous dispersion of block (A). The polymerization initiation temperature varies depending on the type of initiator, but is, for example, 50 to 120°C. The polymerization is carried out until the monomer conversion rate reaches 70 to 100%, preferably 80 to 98%.

[0056] Next, the monomer component (b) is added dropwise to the aqueous dispersion of the block (A) and polymerized, thereby obtaining an aqueous dispersion of a block copolymer (C) consisting of the block (A) and the block (B). The polymerization initiation temperature varies depending on the type of initiator, but is, for example, 50 to 120°C. The polymerization is carried out until the monomer conversion rate reaches 70 to 100%, preferably 80 to 98%.

[0057] Thereafter, if necessary, the block copolymer (C) is recovered from the aqueous dispersion of the block copolymer (C). Examples of the recovery method include (i) a method in which an aqueous dispersion is poured into hot water in which a coagulant is dissolved, and the block copolymer (C) is recovered by coagulating it into a slurry state (wet method), and (ii) a method in which an aqueous dispersion of the block copolymer (C) is sprayed into a heated atmosphere, and the block copolymer (C) is recovered semi-directly (spray dry method).

[0058] Examples of the coagulant include, but are not limited to, inorganic acids such as sulfuric acid, hydrochloric acid, phosphoric acid, and nitric acid, and metal salts such as calcium chloride, calcium acetate, and aluminum sulfate.

[0059] Examples of a method for obtaining a dry block copolymer (C) from the block copolymer (C) in a slurry state include (i) a method in which the emulsifier residue and the coagulant residue remaining in the slurry are dissolved into water by washing, and then the slurry is dehydrated using a centrifugal dehydrator or a press dehydrator, and further dried using an air flow dryer or the like, and (ii) a method in which the slurry is simultaneously dehydrated and dried using a squeeze dehydrator, extruder, or the like.

[0060] [Inorganic filler masterbatch] An inorganic filler masterbatch according to one embodiment of the present invention (hereinafter also referred to as "the present masterbatch") contains the present dispersant and an inorganic filler. The present dispersant may be used alone or in combination of two or more kinds.

[0061] Examples of inorganic fillers include calcium carbonate, calcium phosphate, alumina, silica, barium sulfate, calcium sulfate, aluminum hydroxide, magnesium silicate, aluminum silicate, talc, clay, mica, glass microspheres, wollastonite, titanium dioxide, iron oxide, antimony pentoxide, zinc oxide, silica, cadmium sulfide, yellow lead, and carbon black. Among these, titanium dioxide, iron oxide, antimony pentoxide, zinc oxide, silica, cadmium sulfide, calcium carbonate, barium carbonate, barium sulfate, clay, talc, yellow lead, and carbon black also function as inorganic pigments. These inorganic fillers may be used alone or in combination of two or more. In order to impart jet blackness to the resin composition, it is preferable that at least a part of the inorganic filler is carbon black.

[0062] Examples of carbon black include channel black, furnace black, lamp black, thermal black, Ketjen black, and naphthalene black. The carbon black may have a particle surface that has been subjected to a secondary treatment. Examples of the secondary treatment include providing a surface functional group by an oxidation treatment, graphitizing the crystal structure by a heat treatment in an inert atmosphere, and activation treatment with water vapor or carbon dioxide gas. The oxidation treatment includes treatment with any of ozone, nitric acid, nitrous acid, sodium hypochlorite, and hydrogen peroxide. The oxidation treatment generates acidic functional groups such as carboxyl groups and phenolic hydroxyl groups on the carbon black surface, improving the wettability and dispersibility of the carbon black surface.

[0063] The average primary particle size of carbon black is not particularly limited, but is preferably 10 to 20 nm. If the average primary particle size is 10 nm or more, the aggregation of carbon black in the resin composition is further suppressed, and if it is 20 nm or less, jet blackness is easily expressed. The average primary particle size of carbon black is measured by observation with a transmission electron microscope. The pH of carbon black is not particularly limited, but from the viewpoint of dispersibility, it is preferably not more than 6. The pH of carbon black is measured with a pH meter using a mixture of carbon black and distilled water. The dibutyl phthalate (DBP) absorption of carbon black is not particularly limited, but due to color development, it is recommended to use a value between 40 and 60 cm 3 / 100g is preferable. The DBP absorption amount is the amount of dibutyl phthalate absorbed by 100g of carbon black (JIS K6221).

[0064] As the carbon black, commercially available products can be used. Examples of commercially available carbon black include Mitsubishi Carbon Black (registered trademark) #2600, #2300, #1000, #980, #970, #960, #950, #44 (manufactured by Mitsubishi Chemical Corporation), Toka Black (registered trademark) #8500, #8300 (manufactured by Tokai Carbon Co., Ltd.), etc., but are not limited thereto.

[0065] The present masterbatch may further contain, in addition to the present dispersant and inorganic filler, at least one selected from the group consisting of other additives and other thermoplastic resins. Examples of other additives include various stabilizers such as antioxidants and light stabilizers, lubricants, processing agents, organic pigments, dyes, organic fillers, silicone oils, paraffin oils, plasticizers, release agents, lubricants, antistatic agents, flame retardants, and metal powders.

[0066] Examples of other thermoplastic resins include, but are not limited to, acrylonitrile-styrene copolymers (AS resins), acrylonitrile-α-methylstyrene copolymers (αSAN resins), styrene-maleic anhydride copolymers, acrylonitrile-styrene-N-substituted maleimide terpolymers, styrene-maleic anhydride-N-substituted maleimide terpolymers, resins (ABS resins, ASA resins, SAS resins, AES resins, etc.) obtained by graft polymerizing at least one monomer selected from the group consisting of aromatic vinyl, vinyl cyanide, and (meth)acrylic acid esters in the presence of a rubber polymer (polybutadiene, acrylic rubber, silicone rubber, ethylene propylene diene rubber (EPDM), or a composite rubber thereof, etc.), polycarbonate resins, polybutylene terephthalate (PBT resin), polyethylene terephthalate (PE Examples of suitable elastomers include polyvinyl chloride, polyethylene, polypropylene, and other polyolefins, styrene-butadiene-styrene (SBS), styrene-butadiene (SBR), hydrogenated SBS, styrene-isoprene-styrene (SIS), and other styrene-based elastomers, various olefin-based elastomers, various polyester-based elastomers, polystyrene, methyl methacrylate-styrene copolymer (MS resin), acrylonitrile-styrene-methyl methacrylate copolymer, polyacetal resin, modified polyphenylene ether (modified PPE resin), ethylene-vinyl acetate copolymer, polyphenylene sulfide (PPS resin), polyethersulfone (PES resin), polyetheretherketone (PEEK resin), polyarylate, liquid crystal polyester resin, and polyamide resin (for example, nylon).

[0067] In the present masterbatch, the mass ratio of the present dispersant to the inorganic filler is not particularly limited, but is preferably 20 to 95 parts by mass of the present dispersant and 5 to 80 parts by mass of the inorganic filler, and more preferably 30 to 80 parts by mass of the present dispersant and 20 to 70 parts by mass of the inorganic filler, relative to 100 parts by mass of the total of the present dispersant and the inorganic filler. If the proportion of the present dispersant is equal to or greater than the lower limit, the inorganic filler can be easily dispersed in the acrylic resin when a resin composition is produced using the present masterbatch, and if it is equal to or less than the upper limit, the amount of the masterbatch used in producing the resin composition can be reduced.

[0068] When the inorganic filler contains carbon black, the content of carbon black is preferably 1% by mass or more, more preferably 5% by mass or more, and may be 100% by mass, based on 100% by mass of the inorganic filler. When the content of carbon black is equal to or more than the lower limit, the jet blackness of the resin composition obtained by using the masterbatch is more excellent.

[0069] The total content of the other additives and other thermoplastic resins is not particularly limited, but is, for example, 0 to 30 parts by mass per 100 parts by mass of the total of the present dispersant and the inorganic filler.

[0070] The method for producing the masterbatch is not particularly limited, but is preferably a method of melt-kneading the dispersant and the inorganic filler. For example, the dispersant, the inorganic filler, and at least one selected from the group consisting of additives and other thermoplastic resins as necessary are mixed and dispersed using a V-type blender or Henschel mixer, and the mixture obtained is melt-kneaded using a melt kneader such as a screw extruder, a Banbury mixer, a pressure kneader, or a mixing roll, to produce the masterbatch. After melt-kneading, the melt-kneaded product may be pelletized using a pelletizer, or the melt-kneaded product or its pellets may be pulverized into powder, if necessary.

[0071] [Resin composition] The resin composition according to one embodiment of the present invention (hereinafter also referred to as "the present resin composition") contains the present dispersant, an inorganic filler, and an acrylic resin.

[0072] As the inorganic filler, the same inorganic fillers as those in the present masterbatch can be used. When the present resin composition is obtained using the present masterbatch, the inorganic filler in the present resin composition may be derived only from the present masterbatch, or may further contain an inorganic filler not derived from the present masterbatch.

[0073] The acrylic resin in the present invention is a polymer having a methacrylic acid ester unit. The acrylic resin may further have other monomer units as necessary.

[0074] Examples of the methacrylic acid ester include the same methacrylic acid esters as those in block (B).

[0075] The other monomers may be any monomer capable of copolymerizing with the methacrylic acid ester, and include, but are not limited to, aromatic vinyl, vinyl cyanide, acrylic acid ester, methacrylic acid, acrylic acid, methacrylamide, acrylamide, maleic acid, maleic anhydride, N-substituted maleimide, etc. The aromatic vinyl and vinyl cyanide may be the same as the aromatic vinyl and vinyl cyanide in block (A), respectively. The acrylic acid ester may be the same as the acrylic acid ester in block (B).

[0076] The content of the methacrylic acid ester units in the acrylic resin is preferably 50% by mass or more, more preferably 70% by mass or more, and may be 100% by mass, based on 100% by mass of all monomer units constituting the acrylic resin (the total of the methacrylic acid ester units and other monomer units). If the content of the methacrylic acid ester units is equal to or more than the lower limit, the color development and jet blackness of the resin composition are good.

[0077] The acrylic resin can be produced by polymerizing a methacrylic acid ester and, if necessary, other monomers. Commercially available acrylic resins may also be used.

[0078] The present resin composition may further contain, as necessary, at least one selected from the group consisting of other additives and other thermoplastic resins, in addition to the present dispersant and inorganic filler. The other additives and the other thermoplastic resins may be the same as those in the present masterbatch.

[0079] Among the above-mentioned other thermoplastic resins, a resin obtained by graft polymerizing at least one monomer selected from the group consisting of aromatic vinyl, vinyl cyanide, and (meth)acrylic acid ester in the presence of a rubber polymer is preferred, in that it exhibits good physical properties and improves the dispersibility of inorganic fillers.

[0080] When the present resin composition is obtained by using the present masterbatch and the present masterbatch contains other additives, the other additives in the present resin composition may be only those derived from the present masterbatch, or may further contain additives not derived from the present masterbatch. The same applies to other thermoplastic resins.

[0081] The content of the present dispersant is preferably 1 to 50 parts by mass, more preferably 1 to 25 parts by mass, per 100 parts by mass of the total of the acrylic resin and the other thermoplastic resin. When the content of the present dispersant is within the above range, the dispersibility of the inorganic filler can be sufficiently increased without impairing the inherent physical properties of the resin component consisting of the acrylic resin and the other thermoplastic resin.

[0082] The content of the inorganic filler is preferably 0.1 to 20 parts by mass, more preferably 0.1 to 5 parts by mass, based on 100 parts by mass of the total of the acrylic resin and the other thermoplastic resin. If the content of the inorganic filler is within the above range, the function of the inorganic filler can be sufficiently imparted without impairing the inherent physical properties of the resin component consisting of the acrylic resin and the other thermoplastic resin. For example, when the inorganic filler contains carbon black, the color development and jet blackness of the resin composition are good.

[0083] The content of the acrylic resin is preferably 40 to 100 parts by mass, more preferably 50 to 100 parts by mass, per 100 parts by mass of the total of the acrylic resin and the other thermoplastic resin. When the content of the acrylic resin is within the above range, the color development and jet blackness are good.

[0084] The content of the other additives is not particularly limited, but is, for example, 0 to 10 parts by mass per 100 parts by mass of the total of the acrylic resin and the other thermoplastic resin.

[0085] <Method of producing resin composition> The resin composition may be produced, for example, by melt-kneading the masterbatch with an acrylic resin. In this process, if necessary, inorganic fillers, other additives, other thermoplastic resins, etc. may be melt-kneaded together with the masterbatch and the acrylic resin. For example, the present resin composition can be produced by mixing and dispersing the present masterbatch, acrylic resin, and, if necessary, at least one selected from the group consisting of inorganic fillers, other additives, and other thermoplastic resins using a V-type blender, Henschel mixer, or the like, and melt-kneading the mixture thus obtained using a melt-kneading machine such as a screw extruder, Banbury mixer, pressure kneader, mixing roll, or the like. After melt-kneading, the melt-kneaded product may be pelletized using a pelletizer, or the like, if necessary. The resin composition may be produced by melt-kneading the dispersant, the inorganic filler, the acrylic resin, and, if necessary, at least one selected from the group consisting of other additives and other thermoplastic resins, without using the masterbatch. The method using the masterbatch is preferred in that the inorganic filler can be more uniformly dispersed.

[0086] [Molded product] A molded article according to one embodiment of the present invention (hereinafter also referred to as "the present molded article") contains the present resin composition. The present molded article can be obtained, for example, by molding the present resin composition by a known molding method. Examples of the molding method include injection molding, press molding, extrusion molding, vacuum molding, and blow molding. The molded article can be used for applications in the fields of vehicles, building materials, office automation, and home appliances. EXAMPLES

[0087] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to the following examples. In the following examples, "%" and "parts" are by weight unless otherwise specified. The various measurement and evaluation methods in the following examples are as follows.

[0088] <50% particle size, 90% particle size> Measurements were performed using a Microtrac (Nanorac 150, manufactured by Nikkiso Co., Ltd.) and ion-exchanged water as the measurement solvent.

[0089] <Monomer conversion rate> 1 g of the latex of block (A) or the latex of block copolymer (C) was heated at 130° C. for 15 minutes to volatilize water and unreacted monomers, and the monomer conversion was determined from the remaining solid content.

[0090] <Mn、Mw> The latex of block (A) or the latex of block copolymer (C) was coagulated at 60 to 95°C using calcium chloride as a coagulant, and the block (A) or the block copolymer (C) was recovered by dehydrating, washing, and drying. The obtained block (A) or block copolymer (C) was dissolved in tetrahydrofuran, and Mw and Mn were determined by GPC in terms of standard polystyrene. The Mn of block (B) can be calculated by subtracting the Mn of block (A) from the Mn of block copolymer (C). The same applies to Mw.

[0091] <Measurement of color development (jet blackness)> Pellets of the resin composition were molded by an injection molding machine (manufactured by The Japan Steel Works, Ltd.) to prepare a test piece of 100 mm×100 mm (thickness 3 mm) (hereinafter referred to as "molded piece 1"). The color tone (L * ) was measured by the SCE method. * The smaller the value, the higher the jet blackness and the better the color development.

[0092] <Gloss measurement> The surface gloss (Gs) of the molded article 1 at an incident angle of 60°, as defined in JIS Z8741, was measured using a digital variable angle gloss meter ("UGV-5D" manufactured by Suga Test Instruments Co., Ltd.).

[0093] <Observation of molded appearance> The appearance of the molded article 1 was observed visually and also observed at a magnification of 50 times using a laser microscope (VK-X1000 manufactured by Keyence Corporation), and evaluated according to the following criteria. ⊚: Almost no carbon black aggregates are observed visually or with a laser microscope. ◯: Carbon black aggregates are not visible to the naked eye, but are slightly visible with a laser microscope. △: Carbon aggregates are visible both visually and with a laser microscope. ×: A large number of carbon black aggregates are observed both visually and by a laser microscope. The developed surface area ratio (Sdr) of the interface was also measured using the same laser microscope. The smaller the developed surface area ratio (Sdr) of the interface, the smoother the surface and the fewer aggregates.

[0094] <Production of Block Copolymer (C-1)> 37.5 parts by mass of styrene, 12.5 parts by mass of acrylonitrile, 2.5 parts by mass of liquid paraffin, 0.1 parts by mass of lauroyl peroxide, and 0.15 parts by mass of 2-[(dodecylsulfanylthiocarbonyl)sulfanyl]propanoic acid were mixed and dissolved. The obtained solution was added to an aqueous solution in which 2 parts by mass of sodium dodecylbenzenesulfonate was dissolved in 200 parts by mass of deionized water, and emulsified to the extent that separation did not occur by stirring for 5 minutes with a homomixer device (HIGH-FLEX DISPERSER HG92 manufactured by SMT). The obtained emulsion was treated four times at 50 MPa using a small pressure homogenizer (Econizer 02 manufactured by Sanmaru Machinery Co., Ltd.) to obtain a mini-emulsion (aqueous dispersion of monomer fine particles). The 50% particle size of the monomer fine particles in the obtained mini-emulsion was 70 nm, and the 90% particle size was 90 nm.

[0095] The obtained mini-emulsion was placed in a reactor equipped with a cooling tube, a jacket heater, and a stirrer, and the atmosphere was replaced with nitrogen, and then the reaction was carried out at 80°C for 360 minutes to obtain a latex of block (A-1). The monomer conversion was 93%, Mw was 116,000, Mn was 87,000, and the molecular weight distribution (Mw / Mn) was 1.3.

[0096] To the obtained latex of block (A-1), 50 parts by mass of methyl methacrylate was added dropwise over 60 minutes at 80° C., and the mixture was further reacted for 300 minutes at 80° C. to obtain a latex of block copolymer (C-1) in which block (A-1) was copolymerized with block (B-1). The monomer conversion was 96%, and the block copolymer (C-1) had Mw of 255,000, Mn of 181,000, and molecular weight distribution (Mw / Mn) of 1.4.

[0097] <Production of Block Copolymer (C-2)> Block copolymer (C-2) was obtained by carrying out the same procedure as in the production of block copolymer (C-1), except that the amount of 2-[(dodecylsulfanylthiocarbonyl)sulfanyl]propanoic acid was 0.3 parts by mass and the amount of lauroyl peroxide was 0.2 parts by mass. The monomer conversion rate when obtaining the latex of block (A-2) was 92%, Mw of block (A-2) was 61000, Mn was 48000, and molecular weight distribution (Mw / Mn) was 1.3. The monomer conversion rate when obtaining the latex of block copolymer (C-2) was 94%, Mw of block copolymer (C-2) was 128000, Mn was 98000, and molecular weight distribution (Mw / Mn) was 1.3.

[0098] <Production of Block Copolymer (C-3)> Block copolymer (C-3) was obtained by carrying out the same operation as in the production of block copolymer (C-1), except that styrene was 24.75 parts by mass, acrylonitrile was 8.25 parts by mass, methyl methacrylate was 67 parts by mass, 2-[(dodecylsulfanylthiocarbonyl)sulfanyl]propanoic acid was 0.3 parts by mass, and lauroyl peroxide was 0.2 parts by mass. The monomer conversion rate when obtaining the latex of block (A-3) was 91%, and the monomer conversion rate when obtaining the latex of block copolymer (C-3) was 92%. The Mw of block (A-3) was 43,000, the Mn was 34,000, and the molecular weight distribution (Mw / Mn) was 1.3, and the Mw of block copolymer (C-3) was 124,000, the Mn was 95,000, and the molecular weight distribution (Mw / Mn) was 1.3.

[0099] <Production of Block Copolymer (C-4)> Block copolymer (C-4) was obtained by carrying out the same operation as in the production of block copolymer (C-1), except that styrene was 50.25 parts by mass, acrylonitrile was 16.75 parts by mass, methyl methacrylate was 33 parts by mass, 2-[(dodecylsulfanylthiocarbonyl)sulfanyl]propanoic acid was 0.3 parts by mass, and lauroyl peroxide was 0.2 parts by mass. The monomer conversion rate when obtaining the latex of block (A-4) was 95%, and the monomer conversion rate when obtaining the latex of block copolymer (C-4) was 93%. The Mw of block (A-3) was 93,000, the Mn was 67,000, and the molecular weight distribution (Mw / Mn) was 1.4, and the Mw of block copolymer (C-4) was 141,000, the Mn was 99,000, and the molecular weight distribution (Mw / Mn) was 1.4.

[0100] <Examples 1 to 4 and Comparative Examples 1 to 3> [Manufacturing of inorganic filler master batches] A carbon black master batch (inorganic filler master batch) was obtained by melt-kneading 100 parts by mass of a carbon black dispersant (any one of block copolymers (C-1) to (C-4), SAN (S100N manufactured by Techno UMG Co., Ltd.) and PMMA (VH5 manufactured by Mitsubishi Chemical Co., Ltd.) with 10 parts by mass of carbon black (#1000 manufactured by Mitsubishi Chemical Co., Ltd.) in a twin-screw extruder (TEX-28V manufactured by Japan Steel Works, Ltd.).

[0101] [Production of resin composition] The graft polymer (MUX-60 manufactured by Techno UMG Co., Ltd.), acrylic resin (VH5 manufactured by Mitsubishi Chemical Corporation), and the carbon black master batch or carbon black (#1000 manufactured by Mitsubishi Chemical Corporation) obtained above were melt-kneaded in a twin-screw extruder (TEX-28V manufactured by The Japan Steel Works, Ltd.) to obtain a resin composition having the composition shown in Table 1. The obtained resin compositions were evaluated for color development (jet blackness), gloss, and molded appearance. The results are shown in Table 1. Laser microscope images of molded products 1 using the resin compositions of Example 2 and Comparative Example 1 are shown in Figs. 1 and 2.

[0102] [Table 1]

[0103] The materials shown by the abbreviations in Table 1 are as follows. MUX-60: MUX-60 manufactured by Techno UMG Co., Ltd., a graft polymer obtained by polymerizing methyl methacrylate and alkyl acrylate in the presence of polybutadiene-polybutyl acrylate composite rubber. PMMA: VH5, polymethyl methacrylate, manufactured by Mitsubishi Chemical Corporation. C-1 to C-4: block copolymers (C-1) to (C-4), respectively. SAN: S100N manufactured by Techno UMG Co., Ltd., acrylonitrile-styrene copolymer. #1000: Mitsubishi Chemical Corporation #1000, average primary particle size 18 nm, pH = 3.5, DBP absorption 56 cm 3 / 100g. A blank space in Table 1 indicates that the material was not included.

[0104] As shown in Table 1, in Examples 1 to 4 in which the graft copolymer (C) was used as a carbon black dispersant, molded articles having excellent color development and molded appearance and high gloss were obtained. On the other hand, in Comparative Example 1 in which SAN was used instead of the graft copolymer (C), the color development and appearance of the molded article were poor. In Comparative Example 1, in which PMMA was used instead of the graft copolymer (C), and Comparative Example 3, in which no carbon black dispersant was used, the color development, molding appearance, and gloss of the molded product were poor. [Industrial Applicability]

[0105] The inorganic filler dispersant of the present invention can disperse the inorganic filler well in the acrylic resin, and therefore, a resin composition containing the inorganic filler dispersant of the present invention, an inorganic filler, and an acrylic resin can suppress the generation of aggregates of the inorganic filler, fully exert the functions of the inorganic filler, and produce a highly glossy molded product. The inorganic filler dispersant of the present invention is particularly useful in pigmenting acrylic resins with carbon black.

Claims

1. An inorganic filler dispersant comprising a block copolymer (C) including a block (A) having an aromatic vinyl unit and a vinyl cyanide unit, and a block (B) having a (meth)acrylic acid ester unit, wherein the molecular weight dispersity of the block copolymer (C), expressed as weight average molecular weight (Mw) / number average molecular weight (Mn), is 1.0 to 2.

5.

2. The inorganic filler dispersant according to claim 1, wherein the weight average molecular weight (Mw) of the block (A) is 20,000 to 150,000.

3. The inorganic filler dispersant according to claim 1 or 2, wherein a mass ratio of the block (A) to the block (B) (the block (A):the block (B)) is 20:80 to 80:

20.

4. An inorganic filler masterbatch comprising the inorganic filler dispersant according to any one of claims 1 to 3 and an inorganic filler.

5. A resin composition comprising the inorganic filler dispersant according to any one of claims 1 to 3, an inorganic filler, and an acrylic resin.

6. A method for producing a resin composition, comprising melt-kneading the inorganic filler masterbatch according to claim 4 with an acrylic resin.

7. A molded article comprising the resin composition according to claim 5.

Citation Information

Patent Citations

  • Chlorinated vinyl chloride resin composition

    JP1989210450A

  • Chlorinated vinyl chloride resin composition

    JP1990110157A

  • Dispersant for carbon black

    JP1994148927A

  • Coated molded product, resin molded product, recycled resin material, and their manufacturing process

    JP2004025831A

  • Water-soluble tool materials for composite structures

    JP2005500909A