Adhesive composition, adhesive, adhesive sheet and display

The adhesive composition with a (meth)acrylic acid ester polymer and long-chain alkylamine stabilizes rust inhibitors to prevent ion migration in touch panels, addressing electrode disconnection and short circuits, ensuring panel reliability.

JP7551372B2Active Publication Date: 2024-09-17LINTEC CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020122223
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-07-16
Publication Date
2024-09-17
Estimated Expiration
2040-07-16

AI Technical Summary

Technical Problem

Conventional adhesives fail to effectively prevent ion migration and resulting short circuits in touch panels with metal electrodes, particularly under high temperature and high humidity conditions, leading to electrode disconnection and dendrite formation.

Method used

An adhesive composition comprising a (meth)acrylic acid ester polymer, a rust inhibitor, and a long-chain alkylamine, which stabilizes the rust inhibitor on the adhesive layer surface, preventing electrode dissolution and dendrite formation, thereby suppressing ion migration.

Benefits of technology

The adhesive composition effectively prevents electrode disconnection and short circuits, maintaining electrode resistance stability even under harsh conditions, thus ensuring the reliability of touch panels.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007551372000009
    Figure 0007551372000009
  • Figure 0007551372000010
    Figure 0007551372000010
  • Figure 0007551372000006
    Figure 0007551372000006
Patent Text Reader

Abstract

To provide an adhesive composition, adhesive, adhesive sheet and display body that can effectively prevent and suppress migration.SOLUTION: The present invention discloses: an adhesive composition containing a (meth)acrylate polymer (A), rust inhibitor (B), and long-chain alkyl amine (C); an adhesive formed by crosslinking the adhesive composition; and an adhesive sheet 1 that includes two release sheets 12a,12b, and an adhesive layer 11 sandwiched between the two release sheets 12a,12b so as to contact the peeling faces of the two release sheets 12a,12b, the adhesive layer 11 composed of the adhesive.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an adhesive composition, an adhesive and an adhesive sheet that can be used in displays such as touch panels, and displays using them. [Background technology]

[0002] In recent years, touch panels have come to be used as displays in many mobile electronic devices such as smartphones and tablet terminals. Touch panel types include resistive and capacitive types, but the capacitive type is mainly used in such mobile electronic devices.

[0003] Recently, efforts have been made to enlarge touch panels, and mesh-shaped metal electrodes, such as copper electrodes or silver electrodes, have been considered as electrode materials for such touch panels. However, when a conventional adhesive is used in contact with a metal electrode, particularly a copper electrode or a silver electrode, ion migration (electrochemical migration; hereinafter simply referred to as "migration") may occur. Specifically, the electrode may dissolve and break at the positive electrode, and dendrites may form at the negative electrode due to precipitation of the positive electrode components, causing a short circuit.

[0004] This migration is particularly likely to occur when voltage is applied to the electrodes under high temperature and humidity conditions. When this type of migration occurs, the resistance value changes and the touch panel will no longer operate normally. In recent years, as electrodes have become finer and their pitches narrower, migration has become more likely to cause disconnections and short circuits in electrodes, making it desirable to fully prevent and suppress migration.

[0005] Incidentally, Patent Document 1 discloses a pressure-sensitive adhesive composition for touch panels, which contains a benzotriazole compound as a rust inhibitor. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2014-177611 A Summary of the Invention [Problem to be solved by the invention]

[0007] However, although benzotriazole compounds as rust inhibitors have the effect of preventing corrosion of metal wiring, they cannot sufficiently prevent or suppress migration.

[0008] The present invention has been made in consideration of the above-mentioned circumstances, and has an object to provide an adhesive composition, an adhesive, an adhesive sheet, and a display material that can effectively prevent or suppress migration. [Means for solving the problem]

[0009] In order to achieve the above-mentioned object, firstly, the present invention provides an adhesive composition comprising a (meth)acrylic acid ester polymer (A), a rust inhibitor (B), and a long-chain alkylamine (C) (Invention 1).

[0010] According to the above invention (Invention 1), the rust inhibitor (B) and the long-chain alkylamine (C) coexist, and the rust inhibitor (B) is easily present stably on the surface of the adhesive layer obtained from the adhesive composition. This prevents or inhibits the dissolution of the positive electrode when the adhesive layer contacts the electrode, and prevents or inhibits the formation of dendrites on the negative electrode. That is, migration in the electrode is effectively prevented or inhibited, and the change in resistance value of the electrode made of metal or metal oxide can be inhibited.

[0011] In the above invention (Invention 1), it is preferable to contain a silane compound (D) having alkoxysilyl groups at both ends (Invention 2).

[0012] In the above inventions (Inventions 1 and 2), it is preferable to contain an alkylene glycol (E) (Invention 3).

[0013] In the above inventions (Inventions 1 to 3), the rust inhibitor (B) is preferably an azole (Invention 4).

[0014] In the above inventions (Inventions 1 to 4), the long-chain alkylamine (C) is preferably a tertiary amine (Invention 5).

[0015] In the above inventions (Inventions 1 to 5), it is preferable to contain a crosslinking agent (F) (Invention 6).

[0016] In the above inventions (Inventions 1 to 6), it is preferable that the (meth)acrylic acid ester polymer (A) does not contain a carboxy group-containing monomer as a monomer unit constituting the polymer (Invention 7).

[0017] In the above inventions (Inventions 1 to 7), the (meth)acrylic acid ester polymer (A) preferably contains 6% by mass or more and 35% by mass or less of a hydroxyl group-containing monomer as a monomer unit constituting the polymer (Invention 8).

[0018] The above inventions (Inventions 1 to 8) may contain an ultraviolet absorbing agent (Invention 9).

[0019] In the above inventions (Inventions 1 to 9), the adhesive composition is preferably for forming an adhesive that comes into contact with an electrode made of a metal or metal oxide (Invention 10).

[0020] Secondly, the present invention provides a pressure-sensitive adhesive (Invention 11) obtained by crosslinking the pressure-sensitive adhesive composition (Inventions 1 to 10).

[0021] Thirdly, the present invention provides an adhesive sheet (Invention 12) comprising two release sheets and an adhesive layer sandwiched between the release sheets so as to be in contact with the release surfaces of the two release sheets, the adhesive layer being made of the adhesive (Invention 11).

[0022] Fourthly, the present invention provides a display comprising a first display member, a second display member, and an adhesive layer for bonding the first display member and the second display member to each other, wherein the first display member and / or the second display member has an electrode made of a metal or metal oxide on at least the surface to be bonded, and the adhesive layer is made of the adhesive (Invention 11) (Invention 13). Effect of the Invention

[0023] The pressure-sensitive adhesive composition, pressure-sensitive adhesive, pressure-sensitive adhesive sheet and display according to the present invention can effectively prevent or suppress migration. [Brief description of the drawings]

[0024] [Figure 1] 1 is a cross-sectional view of a pressure-sensitive adhesive sheet according to one embodiment of the present invention. [Diagram 2] 1 is a cross-sectional view showing a configuration example of a display unit (touch panel). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0025] Hereinafter, an embodiment of the present invention will be described. [Adhesive composition] The adhesive composition according to this embodiment (hereinafter sometimes referred to as "adhesive composition P") contains a (meth)acrylic acid ester polymer (A), a rust inhibitor (B), and a long-chain alkylamine (C), and preferably further contains at least one of a silane compound (D) having alkoxysilyl groups at both ends, an alkylene glycol (E), and a crosslinking agent (F). In this specification, a (meth)acrylic acid ester means both an acrylic acid ester and a methacrylic acid ester. The same applies to other similar terms. In addition, the term "polymer" is also intended to include the concept of a "copolymer."

[0026] The adhesive composition P according to the present embodiment is preferably used to form an adhesive that contacts an electrode made of a metal or metal oxide. By containing the above-mentioned components in the adhesive composition P, when the adhesive obtained from the adhesive composition P contacts an electrode, dissolution of the electrode is prevented or suppressed in the positive electrode, and formation of dendrites is prevented or suppressed in the negative electrode. That is, migration in the electrode is effectively prevented or suppressed (this effect may be referred to as the "migration prevention effect"), and the change in resistance value of the electrode made of a metal or metal oxide can be suppressed. In addition, by effectively preventing or suppressing migration, even when the adhesive contacts, for example, a finely-scaled and narrow-pitch electrode, disconnection or short circuit of the electrode is prevented. In particular, when the electrode is an electrode of a touch panel, driving failure of the touch panel caused by disconnection or short circuit of the electrode is prevented.

[0027] Here, the above-mentioned electrodes include, for example, metal electrodes (including mesh-shaped and grid-shaped) made of copper, copper alloy, silver, silver alloy, etc., transparent conductive films (including patterned ones) made of tin-doped indium oxide (ITO), etc. Among the above-mentioned electrodes, metal electrodes mainly made of non-oxidized metals, specifically, metal electrodes made of copper, copper alloy, silver or silver alloys, are preferred, and metal electrodes made of silver or silver alloys are particularly preferred. Preferred examples of silver alloys include those in which palladium and copper are added to silver. Non-oxidized metals have a higher ionization tendency than metal oxides such as ITO, but according to the adhesive obtained from the adhesive composition P according to this embodiment, even in such cases, disconnection or short circuit of the electrodes is effectively prevented.

[0028] The reason why the above effect occurs is not clear, but is presumed to be as follows. In the adhesive layer obtained from the adhesive composition P, the rust inhibitor (B) and the long-chain alkylamine (C) have a much smaller molecular structure than the crosslinked body of the (meth)acrylic acid ester polymer (A), which has a gigantic molecular structure, and both tend to segregate on the surface layer of the adhesive layer. In addition, the long-chain alkylamine (C) is appropriately distributed on the surface layer of the adhesive layer, and is more likely to stably distribute the rust inhibitor (B) on the surface side of the adhesive layer or around the long-chain alkylamine (C) than the long-chain alkylamine (C). Therefore, in the adhesive layer obtained from the adhesive composition P, the rust inhibitor (B) is more likely to be present stably on the surface of the adhesive layer than an adhesive layer that does not contain the long-chain alkylamine (C). In addition, since the rust inhibitor (B) has a lower molecular weight than the long-chain alkylamine (C), it is presumed that the amount of the rust inhibitor (B) that segregates on the surface of the adhesive layer is large and the proportion of the rust inhibitor (B) present on the surface is high. That is, the coexistence of the rust inhibitor (B) and the long-chain alkylamine (C) makes it easier for the rust inhibitor (B) to be present stably on the surface of the adhesive layer and to effectively exert its effect, which is presumably why the adhesive layer can exert an excellent migration prevention effect.

[0029] The adhesive obtained from the adhesive composition P according to the present embodiment may be an active energy ray curable adhesive that is cured by irradiation with active energy rays, or an active energy ray non-curable adhesive that is not cured by irradiation with active energy rays. In the case of an active energy ray curable adhesive, it is preferable that the adhesive composition P further contains an active energy ray curable component (G).

[0030] (1) Each component (1-1) (Meth)acrylic acid ester polymer (A) The (meth)acrylic acid ester polymer (A) preferably contains a reactive functional group-containing monomer having a reactive functional group in the molecule as a monomer constituting the polymer. By containing this reactive functional group-containing monomer, it reacts with the crosslinking agent (F) described later through the reactive functional group derived from the reactive functional group-containing monomer, thereby forming a crosslinked structure (three-dimensional network structure), and a pressure-sensitive adhesive having a predetermined cohesive strength is obtained.

[0031] The reactive functional group-containing monomer contained in the (meth)acrylic acid ester polymer (A) as a monomer unit constituting the polymer is preferably a monomer having a hydroxyl group in the molecule (hydroxyl group-containing monomer), a monomer having a carboxyl group in the molecule (carboxyl group-containing monomer), a monomer having an amino group in the molecule (amino group-containing monomer), etc. These reactive functional group-containing monomers may be used alone or in combination of two or more kinds.

[0032] Among the above reactive functional group-containing monomers, hydroxyl group-containing monomers are particularly preferred because they have excellent reactivity with the crosslinking agent (F) and have little adverse effect on electrodes.

[0033] Examples of the hydroxyl group-containing monomer include (meth)acrylic acid hydroxyalkyl esters such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate. Among them, from the viewpoint of reactivity with the crosslinking agent (F), 2-hydroxyethyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate are preferred, 2-hydroxyethyl acrylate and 4-hydroxybutyl acrylate are more preferred, and 2-hydroxyethyl acrylate is particularly preferred. These may be used alone or in combination of two or more.

[0034] The (meth)acrylic acid ester polymer (A) preferably contains 6% by mass or more, particularly preferably 9% by mass or more, and more preferably 12% by mass or more of reactive functional group-containing monomers (particularly hydroxyl group-containing monomers) as monomer units constituting the polymer. The (meth)acrylic acid ester polymer (A) preferably contains 35% by mass or less, particularly preferably 30% by mass or less, and more preferably 25% by mass or less of reactive functional group-containing monomers (particularly hydroxyl group-containing monomers) as monomer units constituting the polymer.

[0035] When the (meth)acrylic acid ester polymer (A) contains the reactive functional group-containing monomer as a monomer unit in the above amount, the adhesive strength and cohesive strength of the resulting adhesive are well balanced. In particular, when the reactive functional group-containing monomer is a hydroxyl group-containing monomer, when the (meth)acrylic acid ester polymer (A) contains the hydroxyl group-containing monomer as a monomer unit in the above amount, a predetermined amount of hydroxyl groups, which are hydrophilic groups, remain in the resulting adhesive. This allows moisture to be captured by the hydroxyl groups even if moisture is present, and as a result, the intrusion of moisture into the electrode adjacent to the adhesive layer is suppressed, resulting in a more excellent migration prevention effect.

[0036] It is preferable that the (meth)acrylic acid ester polymer (A) does not contain a carboxyl group-containing monomer as a monomer unit constituting the polymer. Since the carboxyl group is an acid component, there is a concern that the resistance value change due to corrosion of the electrode with which the pressure-sensitive adhesive comes into contact occurs, but by not containing a carboxyl group-containing monomer, corrosion of the electrode can be prevented and the resistance value change can be effectively prevented or suppressed. However, the above-mentioned "not containing a carboxyl group-containing monomer" means that the carboxyl group-containing monomer is allowed to be contained to an extent that the electrode with which the obtained pressure-sensitive adhesive comes into contact is not adversely affected. Specifically, the (meth)acrylic acid ester polymer (A) is allowed to contain a carboxyl group-containing monomer as a monomer unit in an amount of 0.1 mass% or less, preferably 0.01 mass% or less, and more preferably 0.001 mass% or less.

[0037] In addition, the (meth)acrylic acid ester polymer (A) preferably contains a (meth)acrylic acid alkyl ester as a monomer unit constituting the polymer, which allows the polymer to exhibit good adhesiveness.

[0038] In particular, the (meth)acrylic acid ester polymer (A) preferably contains, as monomer units constituting the polymer, a (meth)acrylic acid alkyl ester having an alkyl group having 2 to 20 carbon atoms and having a glass transition temperature (Tg) of 0°C or less as a homopolymer, and a monomer having a glass transition temperature (Tg) of more than 0°C as a homopolymer, in addition to the reactive functional group-containing monomer described above.

[0039] The (meth)acrylic acid ester polymer (A) can exhibit preferable adhesiveness by containing, as a monomer unit constituting the polymer, a (meth)acrylic acid alkyl ester (hereinafter sometimes referred to as "low Tg alkyl acrylate") having a glass transition temperature (Tg) of 0°C or less as a homopolymer and having an alkyl group with 2 to 20 carbon atoms. From this viewpoint, the (meth)acrylic acid ester polymer (A) preferably contains, as a monomer unit constituting the polymer, 30% by mass or more of the low Tg alkyl acrylate, more preferably 40% by mass or more, particularly preferably 50% by mass or more, and even more preferably 60% by mass or more. The (meth)acrylic acid ester polymer (A) preferably contains, as a monomer unit constituting the polymer, 90% by mass or less of the low Tg alkyl acrylate as an upper limit, particularly preferably 80% by mass or less, and even more preferably 70% by mass or less. When the upper limit of the content of the low Tg alkyl acrylate is within the above range, suitable amounts of other monomer components can be introduced into the (meth)acrylic acid ester polymer (A).

[0040] Preferred examples of low Tg alkyl acrylates include ethyl acrylate (Tg-20°C), n-butyl acrylate (Tg-55°C), isobutyl acrylate (Tg-26°C), n-octyl acrylate (Tg-65°C), isooctyl acrylate (Tg-58°C), 2-ethylhexyl acrylate (Tg-70°C), 2-ethylhexyl methacrylate (Tg-10°C), isononyl acrylate (Tg-58°C), isodecyl acrylate (Tg-60°C), isodecyl methacrylate (Tg-41°C), n-lauryl acrylate (Tg-23°C), n-lauryl methacrylate (Tg-65°C), tridecyl acrylate (Tg-55°C), tridecyl methacrylate (-40°C), and isostearyl acrylate (Tg-18°C). Among them, from the viewpoint of more effectively imparting adhesion as a low Tg alkyl acrylate, it is more preferable that the Tg of the homopolymer is -40°C or less, and particularly preferably -50°C or less. Specifically, n-butyl acrylate and 2-ethylhexyl acrylate are particularly preferable, and from the viewpoint of suppressing migration, 2-ethylhexyl acrylate is even more preferable. These may be used alone or in combination of two or more kinds. The alkyl group in the (meth)acrylic acid alkyl ester having 2 to 20 carbon atoms in the alkyl group refers to a linear, branched, or cyclic alkyl group.

[0041] In addition, from the viewpoint of suppressing migration by improving the hydrophobicity of the obtained pressure-sensitive adhesive layer, at least a part of the low Tg alkyl acrylate is preferably a (meth)acrylic acid alkyl ester having 5 or more carbon atoms in the alkyl group, and more preferably a (meth)acrylic acid alkyl ester having 7 or more carbon atoms in the alkyl group. Specifically, 2-ethylhexyl acrylate is particularly preferred. In addition, from the viewpoint of suppressing migration, the proportion of the (meth)acrylic acid alkyl ester having 5 or more carbon atoms in the alkyl group (preferably 7 or more) in the entire low Tg alkyl acrylate is preferably 40% by mass or more, more preferably 60% by mass or more, particularly preferably 80% by mass or more, and most preferably 100% by mass.

[0042] In addition, the (meth)acrylic acid ester polymer (A) contains, as a monomer unit constituting the polymer, a monomer having a glass transition temperature (Tg) as a homopolymer exceeding 0° C. (hereinafter, sometimes referred to as a "hard monomer"), so that the resulting pressure-sensitive adhesive tends to have appropriate cohesive strength and adhesiveness. As a result, the resulting pressure-sensitive adhesive layer tends to suppress defects such as lifting and peeling at the interface with the adherend even after durability conditions.

[0043] Examples of the hard monomer include methyl acrylate (Tg 10° C.), methyl methacrylate (Tg 105° C.), ethyl methacrylate (Tg 65° C.), n-butyl methacrylate (Tg 20° C.), isobutyl methacrylate (Tg 48° C.), t-butyl methacrylate (Tg 107° C.), n-stearyl acrylate (Tg 30° C.), n-stearyl methacrylate (Tg 38° C.), cyclohexyl acrylate (Tg 15° C.), cyclohexyl methacrylate (Tg 66° C.), phenoxyethyl acrylate (Tg 5° C.), phenoxyethyl meth ... Preferred examples of the monomers include acrylic monomers such as acrylate (Tg 54°C), benzyl methacrylate (Tg 54°C), isobornyl acrylate (Tg 94°C), isobornyl methacrylate (Tg 180°C), acryloylmorpholine (Tg 145°C), adamantyl acrylate (Tg 115°C), adamantyl methacrylate (Tg 141°C), dimethylacrylamide (Tg 89°C), acrylamide (Tg 165°C), vinyl acetate (Tg 32°C), and styrene (Tg 80°C), and from the viewpoint of compatibility, acrylic monomers are more preferred. These may be used alone or in combination of two or more.

[0044] In particular, from the viewpoint of imparting suitable cohesive strength and adhesiveness to the resulting pressure-sensitive adhesive and effectively suppressing the occurrence of defects such as lifting and peeling at the interface with the adherend, the glass transition temperature (Tg) of the hard monomer is more preferably 60° C. or higher, and particularly preferably 90° C. or higher. In addition, in consideration of compatibility and copolymerizability with other monomers constituting the (meth)acrylic acid ester polymer (A), the glass transition temperature (Tg) of the hard monomer is preferably 250° C. or lower, more preferably 200° C. or lower, and particularly preferably 150° C. or lower.

[0045] Among the above hard monomers, from the viewpoint of exerting the performance of the hard monomers while preventing adverse effects on other properties such as compatibility with other components, it is preferable to contain at least one selected from the group consisting of methyl methacrylate, isobornyl acrylate, and acryloylmorpholine. In particular, it is preferable to use methyl methacrylate alone or to use isobornyl acrylate and acryloylmorpholine in combination.

[0046] From the viewpoint of imparting suitable cohesive strength and adhesiveness to the resulting pressure-sensitive adhesive, the above-mentioned hard monomer is contained in the (meth)acrylic acid ester polymer (A) in an amount of preferably 5% by mass or more, more preferably 10% by mass or more, and particularly preferably 15% by mass or more, as a monomer constituting the polymer.

[0047] In addition, from the viewpoint of ensuring excellent compatibility between the obtained (meth)acrylic acid ester polymer (A) and other components, the hard monomer is preferably contained in an amount of 50 mass% or less, more preferably 40 mass% or less, and particularly preferably 30 mass% or less, as a monomer constituting the polymer.

[0048] The (meth)acrylic acid ester polymer (A) may contain other monomers as monomer units constituting the polymer, if desired. As the other monomers, monomers not containing reactive functional groups are preferred so as not to interfere with the action of the reactive functional group-containing monomer. Examples of such other monomers include (meth)acrylic acid alkoxyalkyl esters such as methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate. These may be used alone or in combination of two or more.

[0049] The (meth)acrylic acid ester polymer (A) is preferably a solution polymer obtained by a solution polymerization method. By using a solution polymer, a high molecular weight polymer can be easily obtained, and a pressure-sensitive adhesive having excellent durability can be obtained.

[0050] The polymerization mode of the (meth)acrylic acid ester polymer (A) may be a random copolymer or a block copolymer.

[0051] The lower limit of the weight average molecular weight of the (meth)acrylic acid ester polymer (A) is preferably 200,000 or more, particularly preferably 300,000 or more, and more preferably 400,000 or more. When the lower limit of the weight average molecular weight of the (meth)acrylic acid ester polymer (A) is as above, the resulting adhesive has excellent durability, and the rust inhibitor (B) and the long-chain alkylamine (C) are easily segregated and coexist stably on the surface of the adhesive layer. The weight average molecular weight in this specification is a value measured by gel permeation chromatography (GPC) in terms of standard polystyrene.

[0052] The upper limit of the weight average molecular weight of the (meth)acrylic acid ester polymer (A) is preferably not more than 1,200,000, particularly preferably not more than 900,000, and further preferably not more than 750,000. When the upper limit of the weight average molecular weight of the (meth)acrylic acid ester polymer (A) is within the above range, the resulting pressure-sensitive adhesive exhibits suitable adhesive properties.

[0053] In the pressure-sensitive adhesive composition P, the (meth)acrylic acid ester polymer (A) may be used alone or in combination of two or more kinds.

[0054] (1-2) Rust inhibitor (B) The rust inhibitor (B) in this embodiment is preferably one that can coexist suitably with the long-chain alkylamine (C) described later on the surface of the adhesive layer. Such rust inhibitor (B) is likely to be present stably on the surface of the adhesive layer, and therefore effectively exerts its action, contributing to the migration prevention effect. Examples of such rust inhibitor (B) include azoles such as azole compounds, triazole compounds, benzotriazole compounds, thiazole compounds, benzothiazole compounds, imidazole compounds, and benzimidazole compounds, as well as phosphorus compounds and nitrite compounds. Among these, azoles are preferred, and benzotriazole compounds are particularly preferred, from the viewpoint of being easily segregated and coexisting suitably with the long-chain alkylamine (C) on the surface of the adhesive layer and having excellent migration prevention effect. The rust inhibitor (B) may be used alone or in combination of two or more kinds.

[0055] Examples of benzotriazole compounds include 1H-benzotriazole, 1H-tolyltriazole, 1-[N,N-bis(2-ethylhexyl)aminomethyl]benzotriazole, 1-[N,N-bis(2-ethylhexyl)aminomethyl]methylbenzotriazole, carboxybenzotriazole, 2,2'-[[(methyl-1H-benzotriazol-1-yl)methyl]imino]bisethanol, etc. Among them, 1H-benzotriazole, 1H-tolyltriazole, 1-[N,N-bis(2-ethylhexyl)aminomethyl]benzotriazole and 1-[N,N-bis(2-ethylhexyl)aminomethyl]methylbenzotriazole are preferred from the viewpoint of being able to coexist favorably with the long-chain alkylamine (C). These can more effectively suppress the occurrence of migration.

[0056] The content of the rust inhibitor (B) in the adhesive composition P is preferably 0.01 parts by mass or more, more preferably 0.08 parts by mass or more, particularly preferably 0.12 parts by mass or more, and even more preferably 0.15 parts by mass or more, relative to 100 parts by mass of the (meth)acrylic acid ester polymer (A). This makes it easier to segregate moderately on the surface layer of the obtained adhesive layer, and the migration prevention effect is more excellent. In addition, the above content is preferably 2 parts by mass or less, more preferably 1 part by mass or less, particularly preferably 0.5 parts by mass or less, and even more preferably 0.2 parts by mass or less. This allows the rust inhibitor (B) to coexist favorably with the long-chain alkylamine (C) on the surface layer of the obtained adhesive layer, exerting a good migration prevention effect and maintaining good adhesion.

[0057] (1-3) Long-chain alkylamines (C) The long-chain alkylamine (C) in this embodiment is an amine containing a long-chain alkyl group in the molecule. The long-chain alkyl group is preferably linear, but may have a branched chain or a cyclic structure. The carbon number of the long-chain alkyl group is preferably 10 or more, more preferably 12 or more, and particularly preferably 14 or more. The carbon number is preferably 24 or less, more preferably 22 or less, particularly preferably 20 or less, and even more preferably 18 or less. Such a long-chain alkylamine (C) is likely to segregate in the surface layer of the pressure-sensitive adhesive layer together with the above-mentioned rust inhibitor (B), and makes the rust inhibitor (B) more likely to exist stably in the surface layer. As a result, the long-chain alkylamine (C) can exert an excellent migration prevention effect in combination with the rust inhibitor (B).

[0058] The long-chain alkylamine (C) in this embodiment may be a primary amine, a secondary amine, or a tertiary amine, and is preferably a tertiary amine. By using a tertiary amine, the peel strength of the obtained pressure-sensitive adhesive layer from the release sheet can be kept low, and the handling during use is excellent.

[0059] In addition, the long-chain alkylamine (C) in this embodiment preferably has a terminal hydroxyl group, which acts to prevent moisture from penetrating into the electrode adjacent to the resulting pressure-sensitive adhesive layer, thereby providing a more excellent migration prevention effect.

[0060] Furthermore, the long-chain alkylamine (C) in this embodiment preferably contains an oxyethylene structure, and particularly preferably contains a polyoxyethylene structure. That is, the long-chain alkylamine (C) in this embodiment is preferably an oxyethylene long-chain alkylamine, and particularly preferably a polyoxyethylene long-chain alkylamine. Hereinafter, oxyethylene long-chain alkylamine and polyoxyethylene long-chain alkylamine may be collectively referred to as "(poly)oxyethylene long-chain alkylamine".

[0061] As the (poly)oxyethylene long-chain alkylamine, a compound represented by the following general formula (c) is preferred. [ka]

[0062] In the general formula (c), R is a long-chain alkyl group. Furthermore, m and n are each independently an integer of 1 or more, preferably 2 or more, and more preferably 5 or more. Furthermore, m and n are each independently preferably 15 or less, more preferably 12 or less, and particularly preferably 10 or less. This makes it easier to satisfy the sum of the numerical values ​​of m and n described below.

[0063] In the general formula (c), the sum of the numerical values ​​of m and n is an integer of 2 or more. The lower limit of the sum of the numerical values ​​of m and n is preferably 4 or more, more preferably 8 or more, and particularly preferably 12 or more. The upper limit of the sum of the numerical values ​​of m and n is preferably 30 or less, more preferably 24 or less, particularly preferably 20 or less, and even more preferably 15 or less. When the sum of the numerical values ​​of m and n is within the above range, the long-chain alkylamine (C) is likely to segregate together with the above-mentioned rust inhibitor (B) in the surface layer of the pressure-sensitive adhesive layer, and the rust inhibitor (B) is likely to be present stably in the surface layer.

[0064] The weight average molecular weight of the long-chain alkylamine (C) is preferably 250 or more, particularly preferably 350 or more, particularly preferably 500 or more, and more preferably 700 or more. The weight average molecular weight of the long-chain alkylamine (C) is preferably 1400 or less, more preferably 1300 or less, particularly preferably 1200 or less, and more preferably 1000 or less. By having the weight average molecular weight of the long-chain alkylamine (C) within the above range, the long-chain alkylamine (C) is likely to segregate in the surface layer of the pressure-sensitive adhesive layer together with the above-mentioned rust inhibitor (B), and the rust inhibitor (B) can be made to easily exist stably in the surface layer, resulting in a more excellent migration prevention effect.

[0065] The content of the long-chain alkylamine (C) in the adhesive composition P is preferably 0.01 parts by mass or more, more preferably 0.08 parts by mass or more, particularly preferably 0.12 parts by mass or more, and even more preferably 0.15 parts by mass or more, relative to 100 parts by mass of the (meth)acrylic acid ester polymer (A). This makes it easier for the long-chain alkylamine (C) to segregate in the surface layer of the adhesive layer together with the rust inhibitor (B), making the rust inhibitor (B) more likely to be present stably in the surface layer, and the migration prevention effect becomes more excellent. In addition, the above content is preferably 2 parts by mass or less, more preferably 1 part by mass or less, particularly preferably 0.5 parts by mass or less, and even more preferably 0.2 parts by mass or less. This allows the long-chain alkylamine (C) to suitably coexist with the rust inhibitor (B) in the surface layer of the resulting adhesive layer, thereby exerting a good migration prevention effect and maintaining good adhesion.

[0066] (1-4) Silane compounds (D) The adhesive composition P according to the present embodiment has a more excellent migration prevention effect by containing the silane compound (D) having alkoxysilyl groups at both ends. This is believed to be because the alkoxysilyl groups of the silane compound (D) inhibit moisture from penetrating into the electrode adjacent to the adhesive layer obtained.

[0067] The silane compound (D) is an organosilicon compound having alkoxysilyl groups at both ends, and is preferably a compound represented by the following general formula (I). [ka] (R in the formula 1 R is a divalent hydrocarbon group which may have a nitrogen atom. 2 ~R 7 are each independently an alkyl group.

[0068] Above R 1The carbon number of the divalent hydrocarbon group is preferably 1 to 10, particularly preferably 3 to 9, more preferably 4 to 8, and most preferably 5 to 7 from the viewpoint of migration prevention effect in metal electrodes (particularly silver electrodes). The hydrocarbon group is preferably a saturated hydrocarbon group, particularly preferably a chain saturated hydrocarbon group. The hydrocarbon group preferably contains an alkylene group, particularly preferably an alkylene group. The carbon number of the alkylene group is preferably 1 to 10, particularly preferably 3 to 9, more preferably 4 to 8, and most preferably 5 to 7 from the viewpoint of migration prevention effect in metal electrodes (particularly silver electrodes).

[0069] Above R 1 When R has a nitrogen atom, the nitrogen atom may be present in a side chain of the hydrocarbon group, but is preferably present in the main chain of the hydrocarbon group. 1 When has a nitrogen atom, R 1 The number of nitrogen atoms contained therein is preferably 1 to 5, and particularly preferably 2 to 3. The nitrogen atom is preferably an amino group or an amide group, and particularly preferably an amino group, and further preferably exists in the main chain of the hydrocarbon group as a secondary amine or tertiary amine.

[0070] Above R 1 When has a nitrogen atom, R 1 is -(CH) m It is preferred that the skeleton of the group -NH- is included, and -(CH) m -NH-(CH) n More preferably, it contains a - skeleton, in particular, -(CH) m -NH-(CH) n It is preferred that the skeleton of the group -NH- is contained, and more preferably -(CH) m -NH-(CH) n -NH-(CH) p The above m, n and p are positive integers, preferably 1 to 5, and particularly preferably 2 to 4.

[0071] Above R 1 It is preferable that the adhesive does not have a sulfur atom in the main chain. If the adhesive has a sulfur atom in the main chain, metal sulfides are likely to be generated at the interface between the adhesive and an electrode made of a metal (particularly silver) or a metal oxide (particularly ITO) in a durability test environment. This may hinder the migration prevention effect described above.

[0072] Above R 2 ~R 7 The number of carbon atoms in the alkyl group of each of R is preferably 1 to 6, more preferably 1 to 4, further preferably 1 or 2, and most preferably 1. 2 ~R 7 Preferably, all of are the same alkyl group, and most preferably, all are methyl groups.

[0073] The content of the silane compound (D) in the adhesive composition P is preferably 0.01 parts by mass or more as a lower limit, more preferably 0.1 parts by mass or more, particularly preferably 0.16 parts by mass or more, and even more preferably 0.22 parts by mass or more, relative to 100 parts by mass of the (meth)acrylic acid ester polymer (A). The content is preferably 2 parts by mass or less as an upper limit, particularly preferably 1 part by mass or less, and even more preferably 0.5 parts by mass or less. By having the content of the silane compound (D) in the above range, the action of the silane compound (D) is effectively exerted, and the migration prevention effect is more excellent.

[0074] (1-5) Alkylene glycol (E) The adhesive composition P according to the present embodiment has a more excellent migration prevention effect by containing the alkylene glycol (E). This is believed to be because the action of the hydroxyl group of the alkylene glycol (E) inhibits the penetration of moisture into the electrode adjacent to the obtained adhesive layer.

[0075] The alkylene glycol (E) is not particularly limited as long as the above-mentioned effect is exhibited, but preferred examples include alkylene glycol monoalkyl ethers as well as ethylene glycol, propylene glycol, butylene glycol, glycerin, etc. Among them, alkylene glycol monoalkyl ethers are particularly excellent in terms of migration prevention effect.

[0076] The number of carbon atoms in the alkylene group of the alkylene glycol in the alkylene glycol monoalkyl ether is preferably 1 or more, more preferably 2 or more, and particularly preferably 3 or more. The number of carbon atoms in the alkylene group is preferably 10 or less, more preferably 8 or less, and particularly preferably 6 or less. On the other hand, the number of carbon atoms in the alkyl group of the monoalkyl ether in the alkylene glycol monoalkyl ether is preferably 1 or more. The number of carbon atoms in the alkyl group is preferably 8 or less, more preferably 6 or less, and particularly preferably 4 or less, and even more preferably 3 or less.

[0077] Specific examples of the alkylene glycol monoalkyl ether include ethylene glycol monomethyl ether, ethylene glycol monopropyl ether, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol monopropyl ether, diethylene glycol monobutyl ether, polyethylene glycol monomethyl ether, polyethylene glycol monopropyl ether, and polyethylene glycol monobutyl ether; and propylene glycol monoalkyl ethers such as propylene glycol monomethyl ether, propylene glycol monobutyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monobutyl ether, polypropylene glycol monomethyl ether, and polypropylene glycol monobutyl ether. Among these, propylene glycol monoalkyl ethers are preferred, and dipropylene glycol monoalkyl ethers are particularly preferred, and dipropylene glycol monomethyl ether is even more preferred. The alkylene glycol (E) may be used alone or in combination of two or more.

[0078] The content of the alkylene glycol (E) in the adhesive composition P is preferably 0.01 parts by mass or more, more preferably 0.1 parts by mass or more, particularly preferably 0.4 parts by mass or more, and even more preferably 0.8 parts by mass or more, relative to 100 parts by mass of the (meth)acrylic acid ester polymer (A). The content is preferably 5 parts by mass or less, more preferably 3 parts by mass or less, particularly preferably 2 parts by mass or less, and even more preferably 1.5 parts by mass or less, relative to 100 parts by mass of the (meth)acrylic acid ester polymer (A). When the content of the alkylene glycol (E) is within the above range, the action of the alkylene glycol (E) is effectively exerted, and the migration prevention effect is more excellent.

[0079] (1-6) Crosslinking agent (F) The pressure-sensitive adhesive composition P preferably contains a crosslinking agent (F). By containing the crosslinking agent (F), the pressure-sensitive adhesive composition P can crosslink the (meth)acrylic acid ester polymer (A) to form a three-dimensional network structure, thereby improving the cohesive strength of the resulting pressure-sensitive adhesive and improving its durability.

[0080] The crosslinking agent (F) may be any one that reacts with the reactive group of the (meth)acrylic acid ester polymer (A), and examples thereof include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, amine-based crosslinking agents, melamine-based crosslinking agents, aziridine-based crosslinking agents, hydrazine-based crosslinking agents, aldehyde-based crosslinking agents, oxazoline-based crosslinking agents, metal alkoxide-based crosslinking agents, metal chelate-based crosslinking agents, metal salt-based crosslinking agents, and ammonium salt-based crosslinking agents. When the (meth)acrylic acid ester polymer (A) contains a hydroxyl group-containing monomer as a monomer unit constituting the polymer, it is preferable to use an isocyanate-based crosslinking agent that has excellent reactivity with the hydroxyl group. The crosslinking agent (F) may be used alone or in combination of two or more.

[0081] The isocyanate-based crosslinking agent contains at least a polyisocyanate compound. Examples of the polyisocyanate compound include aromatic polyisocyanates such as tolylene diisocyanate, diphenylmethane diisocyanate, and xylylene diisocyanate, aliphatic polyisocyanates such as hexamethylene diisocyanate, alicyclic polyisocyanates such as isophorone diisocyanate and hydrogenated diphenylmethane diisocyanate, and their biuret and isocyanurate forms, as well as adducts which are reactants with low-molecular active hydrogen-containing compounds such as ethylene glycol, propylene glycol, neopentyl glycol, trimethylolpropane, and castor oil. Among these, trimethylolpropane-modified aromatic polyisocyanates, particularly trimethylolpropane-modified tolylene diisocyanate, are preferred from the viewpoint of reactivity with hydroxyl groups.

[0082] The content of the crosslinking agent (F) in the adhesive composition P is preferably 0.001 parts by mass or more as a lower limit, particularly preferably 0.01 parts by mass or more, and even more preferably 0.1 parts by mass or more, relative to 100 parts by mass of the (meth)acrylic acid ester polymer (A). From the viewpoint of the rust inhibitor (B) and the long-chain alkylamine (C) being easily segregated to the surface layer of the adhesive layer, it is preferably 0.3 parts by mass or more, and especially preferably 0.6 parts by mass or more. Moreover, the content is preferably 10 parts by mass or less as an upper limit, particularly preferably 5 parts by mass or less, and even more preferably 1 part by mass or less, and from the viewpoint of increasing the adhesive strength, it is preferably 0.5 parts by mass or less. By the content of the crosslinking agent (F) being in the above range, the cohesive strength of the obtained adhesive becomes favorable, and an adhesive with better adhesiveness is obtained.

[0083] (1-7) Active energy ray-curable component (G) When the adhesive obtained from the adhesive composition P according to the present embodiment is an active energy ray curable adhesive, the adhesive composition P preferably contains an active energy ray curable component (G). By containing the active energy ray curable component (G) in the adhesive composition P, the adhesive obtained by crosslinking (thermal crosslinking) the adhesive composition P becomes an active energy ray curable adhesive. In this active energy ray curable adhesive, it is presumed that the active energy ray curable components (G) polymerize with each other by curing by irradiation with active energy rays after attachment to an adherend, and the polymerized active energy ray curable components (G) are entangled with the crosslinked structure (three-dimensional network structure) of the (meth)acrylic acid ester polymer (A). An adhesive having such a high-order structure has high cohesive force and shows high coating strength, and is therefore more durable.

[0084] The active energy ray curable component (G) is not particularly limited as long as it is a component that is cured by irradiation with active energy rays and can obtain the above-mentioned effects, and may be any of a monomer, an oligomer, or a polymer, or a mixture thereof. Among them, a polyfunctional acrylate monomer that can obtain a pressure-sensitive adhesive having excellent durability can be preferably mentioned.

[0085] Examples of polyfunctional acrylate monomers include bifunctional monomers such as 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, neopentyl glycol adipate di(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, dicyclopentanyl di(meth)acrylate, caprolactone-modified dicyclopentenyl di(meth)acrylate, ethylene oxide-modified phosphoric acid di(meth)acrylate, di(acryloxyethyl)isocyanurate, allylated cyclohexyl di(meth)acrylate, ethoxylated bisphenol A diacrylate, and 9,9-bis[4-(2-acryloyloxyethoxy)phenyl]fluorene; trifunctional types such as diglycerol tetra(meth)acrylate and pentaerythritol tetra(meth)acrylate; pentafunctional types such as propionic acid modified dipentaerythritol tri(meth)acrylate; and hexafunctional types such as dipentaerythritol hexa(meth)acrylate and caprolactone modified dipentaerythritol hexa(meth)acrylate.Among the above, from the viewpoint of imparting suitable cohesive strength and adhesiveness to the obtained pressure-sensitive adhesive and effectively suppressing the occurrence of defects such as lifting and peeling at the interface with the adherend, polyfunctional acrylate monomers containing an isocyanurate structure in the molecule, such as di(acryloxyethyl)isocyanurate, tris(acryloxyethyl)isocyanurate, and ε-caprolactone-modified tris-(2-(meth)acryloxyethyl)isocyanurate, are preferred, polyfunctional acrylate monomers having three or more functions and containing an isocyanurate structure in the molecule are more preferred, and ε-caprolactone-modified tris-(2-(meth)acryloxyethyl)isocyanurate is particularly preferred. These may be used alone or in combination of two or more. In addition, from the viewpoint of compatibility with the (meth)acrylic acid ester polymer (A), the polyfunctional acrylate monomer is preferably one having a molecular weight of less than 1000.

[0086] The active energy ray curable component (G) may be an active energy ray curable acrylate oligomer. Examples of such acrylate oligomers include polyester acrylates, epoxy acrylates, urethane acrylates, polyether acrylates, polybutadiene acrylates, and silicone acrylates.

[0087] The weight average molecular weight of the acrylate oligomer is preferably not more than 50,000, particularly preferably from 1,000 to 50,000, and further preferably from 3,000 to 40,000. These acrylate oligomers may be used alone or in combination of two or more.

[0088] Also, as the active energy ray curable component (G), an adduct acrylate polymer having a group having a (meth)acryloyl group introduced into the side chain can be used. Such an adduct acrylate polymer can be obtained by using a copolymer of a (meth)acrylic acid ester and a monomer having a crosslinkable functional group in the molecule, and reacting a compound having a group reactive with the (meth)acryloyl group and the crosslinkable functional group with a part of the crosslinkable functional group of the copolymer.

[0089] The weight average molecular weight of the adduct acrylate polymer is preferably about 50,000 to 900,000, and particularly preferably about 100,000 to 500,000.

[0090] The active energy ray-curable component (G) may be one selected from the above-mentioned polyfunctional acrylate monomers, acrylate oligomers, and adduct acrylate polymers, or two or more may be combined to be used, or may be combined with other active energy ray-curable components.

[0091] When the adhesive composition P contains an active energy ray curable component (G), the content of the active energy ray curable component (G) is preferably 2 parts by mass or more, more preferably 3 parts by mass or more, and particularly preferably 4 parts by mass or more, relative to 100 parts by mass of the (meth)acrylic acid ester polymer (A). The content is preferably 20 parts by mass or less, more preferably 10 parts by mass or less, particularly preferably 8 parts by mass or less, and even more preferably 6 parts by mass or less. By having the content of the active energy ray curable component (G) within the above range, the adhesive strength of the adhesive after curing with active energy rays can be improved, and the durability of the adhesive can be made more excellent.

[0092] (1-8) Photopolymerization initiator (H) In the case where the adhesive obtained from the adhesive composition P according to the present embodiment is an active energy ray curable adhesive, and ultraviolet rays are used as the active energy rays, it is preferable that the adhesive composition P further contains a photopolymerization initiator (H). By containing the photopolymerization initiator (H) in this way, the active energy ray curable component (G) can be polymerized efficiently, and the polymerization curing time and the irradiation dose of the active energy rays can be reduced.

[0093] Examples of such photopolymerization initiators (H) include benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin-n-butyl ether, benzoin isobutyl ether, acetophenone, dimethylaminoacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-propan-1-one, 4-(2-hydroxyethoxy)phenyl-2-(hydroxy-2-propyl)ketone, benzof Examples of the benzoxanthone include phenone, p-phenylbenzophenone, 4,4'-diethylaminobenzophenone, dichlorobenzophenone, 2-methylanthraquinone, 2-ethylanthraquinone, 2-tertiary-butylanthraquinone, 2-aminoanthraquinone, 2-methylthioxanthone, 2-ethylthioxanthone, 2-chlorothioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, benzyl dimethyl ketal, acetophenone dimethyl ketal, p-dimethylaminobenzoic acid ester, oligo[2-hydroxy-2-methyl-1[4-(1-methylvinyl)phenyl]propanone], 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide, etc. These may be used alone or in combination of two or more.

[0094] When the adhesive composition P contains an active energy ray curable component (G) and a photopolymerization initiator (H), the content of the photopolymerization initiator (H) is preferably 0.1 parts by mass or more as a lower limit, particularly preferably 1 part by mass or more, and more preferably 5 parts by mass or more, relative to 100 parts by mass of the active energy ray curable component (G). The content is preferably 30 parts by mass or less as an upper limit, particularly preferably 20 parts by mass or less, and more preferably 15 parts by mass or less. By having the content of the photopolymerization initiator (H) in the above range, the adhesive strength of the adhesive after curing with active energy rays can be improved, and the durability of the adhesive can be made more excellent.

[0095] (1-9) Various additives If desired, various additives commonly used in acrylic adhesives, such as ultraviolet absorbers, silane coupling agents, antistatic agents, tackifiers, antioxidants, light stabilizers, softeners, fillers, and refractive index adjusters, may be added to the adhesive composition P.

[0096] Examples of the ultraviolet absorbent include compounds such as benzophenone-based, benzotriazole-based, benzoate-based, benzoxazinone-based, triazine-based, phenyl salicylate-based, cyanoacrylate-based, and nickel complex salt-based compounds. Among these, it is preferable to use at least one of a benzophenone-based compound, a benzotriazole-based compound, and a triazine-based compound.

[0097] Examples of the benzophenone-based compound include 2,2-dihydroxy-4-methoxybenzophenone, 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-methoxybenzophenone-5-sulfonic acid hydrate, 2-hydroxy-4-n-octyloxybenzophenone, and the like. Among these, it is preferable to use 2,2-dihydroxy-4-methoxybenzophenone.

[0098] Examples of the benzotriazole-based compounds include 2-(2-hydroxy-5-t-butylphenyl)-2H-benzotriazole, octyl-3-[3-t-butyl-4-hydroxy-5-(5-chloro-2H-benzotriazol-2-yl)phenyl]propionate, 2-ethylhexyl-3-[3-t-butyl-4-hydroxy-5-(5-chloro-2H-benzotriazol-2-yl)phenyl]propionate, and 3-(2H-benzotriazol-2-yl)-5-(1,1-dimethylethyl)-4-hydroxy-benzenepropanoic acid.

[0099] Examples of the triazine-based compound include 2,4-bis[2-hydroxy-4-butoxyphenyl]-6-(2,4-dibutoxyphenyl)-1,3-5-triazine, 2-[4,6-di(2,4-xylyl)-1,3,5-triazin-2-yl]-5-octyloxyphenol, and the like.

[0100] The above ultraviolet absorbents may be used alone or in combination of two or more.

[0101] When the adhesive composition P contains an ultraviolet absorber, the content of the ultraviolet absorber is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, and even more preferably 1.0 parts by mass or more, based on 100 parts by mass of the (meth)acrylic acid ester polymer (A). The content is preferably 15 parts by mass or less, more preferably 12 parts by mass or less, more preferably 8 parts by mass or less, and even more preferably 4 parts by mass or less. When the content of the ultraviolet absorber is within the above range, the adhesive layer is likely to exhibit good ultraviolet absorption properties.

[0102] In addition, the adhesive composition P represents a mixture of various components remaining in the adhesive layer, either as is or after reacting, and components removed during a drying process or the like, such as the polymerization solvent and dilution solvent described below, are not included in the adhesive composition P.

[0103] (2) Manufacturing of adhesive composition The adhesive composition P can be produced by producing a (meth)acrylic acid ester polymer (A), mixing the obtained (meth)acrylic acid ester polymer (A) with a rust inhibitor (B) and a long-chain alkylamine (C), and, if desired, adding a silane compound (D), an alkylene glycol (E), a crosslinking agent (F), an active energy ray-curable component (G), a photopolymerization initiator (H), additives, etc.

[0104] The (meth)acrylic acid ester polymer (A) can be produced by polymerizing a mixture of monomer units constituting the polymer by a normal radical polymerization method. The polymerization of the (meth)acrylic acid ester polymer (A) can be carried out by a solution polymerization method or the like, using a polymerization initiator as desired. Examples of the polymerization solvent include ethyl acetate, n-butyl acetate, isobutyl acetate, toluene, acetone, hexane, methyl ethyl ketone, etc., and two or more of them may be used in combination.

[0105] Examples of the polymerization initiator include azo compounds and organic peroxides, and two or more of them may be used in combination. Examples of the azo compounds include 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), 1,1'-azobis(cyclohexane 1-carbonitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(2,4-dimethyl-4-methoxyvaleronitrile), dimethyl 2,2'-azobis(2-methylpropionate), 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis(2-hydroxymethylpropionitrile), and 2,2'-azobis[2-(2-imidazolin-2-yl)propane].

[0106] Examples of organic peroxides include benzoyl peroxide, t-butyl perbenzoate, cumene hydroperoxide, diisopropyl peroxydicarbonate, di-n-propyl peroxydicarbonate, di(2-ethoxyethyl)peroxydicarbonate, t-butyl peroxyneodecanoate, t-butyl peroxypivalate, (3,5,5-trimethylhexanoyl)peroxide, dipropionyl peroxide, and diacetyl peroxide.

[0107] In the above polymerization step, the weight average molecular weight of the resulting polymer can be adjusted by adding a chain transfer agent such as 2-mercaptoethanol.

[0108] After the (meth)acrylic acid ester polymer (A) is obtained, the rust inhibitor (B), the long-chain alkylamine (C), and, if desired, the silane compound (D), the alkylene glycol (E), the crosslinking agent (F), the active energy ray-curable component (G), the photopolymerization initiator (H), additives, the dilution solvent, etc. are added to the solution of the (meth)acrylic acid ester polymer (A) and mixed thoroughly to obtain a pressure-sensitive adhesive composition P (coating solution) diluted with the solvent.

[0109] Examples of the dilution solvent include aliphatic hydrocarbons such as hexane, heptane, and cyclohexane; aromatic hydrocarbons such as toluene and xylene; halogenated hydrocarbons such as methylene chloride and ethylene chloride; alcohols such as methanol, ethanol, propanol, butanol, and 1-methoxy-2-propanol; ketones such as acetone, methyl ethyl ketone, 2-pentanone, isophorone, and cyclohexanone; esters such as ethyl acetate and butyl acetate; and cellosolve-based solvents such as ethyl cellosolve.

[0110] The concentration and viscosity of the coating solution thus prepared are not particularly limited as long as they are within the range that allows coating, and can be appropriately selected according to the situation. For example, the adhesive composition P is diluted so that the concentration becomes 10 to 40 mass %. In addition, when obtaining the coating solution, the addition of a dilution solvent or the like is not a necessary condition, and if the adhesive composition P has a viscosity that allows coating, it is not necessary to add a dilution solvent. In this case, the adhesive composition P becomes a coating solution in which the polymerization solvent of the (meth)acrylic acid ester polymer (A) itself serves as the dilution solvent.

[0111] [Adhesive] The pressure-sensitive adhesive according to the present embodiment is obtained by crosslinking the above-mentioned pressure-sensitive adhesive composition P. The crosslinking of the pressure-sensitive adhesive composition P can be carried out by a heat treatment. This heat treatment can also serve as a drying treatment for volatilizing the dilution solvent of the applied pressure-sensitive adhesive composition P.

[0112] When heat treatment is performed, the heating temperature is preferably 50 to 150° C., and more preferably 70 to 120° C. The heating time is preferably 30 seconds to 10 minutes, and more preferably 50 seconds to 2 minutes. After the heat treatment, a curing period of about 1 to 2 weeks may be provided at room temperature (e.g., 23° C., 50% RH) as necessary. If this curing period is required, the pressure-sensitive adhesive layer is formed after the curing period has elapsed, and if no curing period is required, the pressure-sensitive adhesive layer is formed after the heat treatment is completed.

[0113] The gel fraction of the pressure-sensitive adhesive according to the present embodiment is preferably 30% or more as a lower limit, particularly preferably 40% or more, and more preferably 45% or more. When the lower limit of the gel fraction of the pressure-sensitive adhesive is as above, the cohesive force is improved and the durability is higher. In addition, the upper limit of the gel fraction is preferably 90% or less, more preferably 80% or less, and particularly preferably 75% or less, and from the viewpoint of further increasing the adhesive strength, it is preferably 65% ​​or less, and more preferably 55% or less. When the upper limit of the gel fraction of the pressure-sensitive adhesive is as above, the pressure-sensitive adhesive does not become too hard and has higher adhesive strength. In addition, the rust inhibitor (B) and the long-chain alkylamine (C) are easily segregated to the surface layer of the pressure-sensitive adhesive layer. The method for measuring the gel fraction of this pressure-sensitive adhesive is as shown in the test example described later.

[0114] [Adhesive sheet] As shown in Fig. 1, the adhesive sheet 1 according to this embodiment is composed of two release sheets 12a, 12b and an adhesive layer 11 sandwiched between the two release sheets 12a, 12b so as to be in contact with the release surfaces of the two release sheets 12a, 12b. However, the release sheets 12a, 12b are not essential components of the adhesive sheet 1, and are peeled off and removed when the adhesive sheet 1 is used. In this specification, the release surface of the release sheet refers to the surface of the release sheet that has releasability, and includes both a surface that has been subjected to a release treatment and a surface that exhibits releasability even without being subjected to a release treatment.

[0115] (1) Adhesive layer The adhesive layer 11 is composed of the adhesive described above. The lower limit of the thickness of the adhesive layer 11 (measured according to JIS K7130) is preferably 5 μm or more, more preferably 10 μm or more, particularly preferably 25 μm or more, and even more preferably 45 μm or more. By setting the lower limit of the thickness of the adhesive layer 11 as above, excellent adhesive strength is fully exhibited. In addition, the upper limit of the thickness of the adhesive layer 11 is preferably 300 μm or less, more preferably 200 μm or less, particularly preferably 100 μm or less, and even more preferably 70 μm or less. By setting the upper limit of the thickness of the adhesive layer 11 as above, the processability is improved. In addition, the rust inhibitor (B) and the long-chain alkylamine (C) are easily segregated to the surface layer of the adhesive layer. The adhesive layer 11 may be formed as a single layer, or may be formed by laminating multiple layers.

[0116] (2) Release sheet The release sheets 12a and 12b are not particularly limited, and known plastic films can be used. For example, polyethylene films, polypropylene films, polybutene films, polybutadiene films, polymethylpentene films, polyvinyl chloride films, vinyl chloride copolymer films, polyethylene terephthalate films, polyethylene naphthalate films, polybutylene terephthalate films, polyurethane films, ethylene vinyl acetate films, ionomer resin films, ethylene-(meth)acrylic acid copolymer films, ethylene-(meth)acrylic acid ester copolymer films, polystyrene films, polycarbonate films, polyimide films, fluororesin films, etc. can be used. Crosslinked films of these can also be used. Furthermore, laminated films of these can also be used.

[0117] The release surfaces of the release sheets 12a and 12b (particularly the surfaces in contact with the adhesive layer 11) are preferably subjected to a release treatment. Examples of release agents used in the release treatment include alkyd-based, silicone-based, fluorine-based, unsaturated polyester-based, polyolefin-based, and wax-based release agents. It is preferable that one of the release sheets 12a and 12b is a heavy release type release sheet having a large release strength, and the other is a light release type release sheet having a small release strength.

[0118] There is no particular limitation on the thickness of the release sheets 12a and 12b, but it is usually about 20 to 150 μm.

[0119] (3) Manufacturing of adhesive sheets In one example of manufacturing the adhesive sheet 1, a coating solution of the adhesive composition P is applied to the release surface of one release sheet 12a (or 12b), a heat treatment is carried out to crosslink the adhesive composition P, and a coating layer is formed, and then the release surface of the other release sheet 12b (or 12a) is superimposed on the coating layer. If a curing period is required, a curing period is left, and if no curing period is required, the coating layer becomes the adhesive layer 11 as is. In this way, the adhesive sheet 1 is obtained. The conditions for the heat treatment and curing are as described above.

[0120] In another manufacturing example of the adhesive sheet 1, the coating liquid of the adhesive composition P is applied to the release surface of one release sheet 12a, and the adhesive composition P is crosslinked by heat treatment to form a coating layer, thereby obtaining the release sheet 12a with the coating layer. The coating liquid of the adhesive composition P is applied to the release surface of the other release sheet 12b, and the adhesive composition P is crosslinked by heat treatment to form a coating layer, thereby obtaining the release sheet 12b with the coating layer. Then, the release sheet 12a with the coating layer and the release sheet 12b with the coating layer are bonded together so that both coating layers are in contact with each other. If a curing period is required, a curing period is provided, and if no curing period is required, the laminated coating layer becomes the adhesive layer 11 as it is. This results in the adhesive sheet 1. According to this manufacturing example, even if the adhesive layer 11 is thick, it can be manufactured stably.

[0121] The coating solution of the pressure-sensitive adhesive composition P can be applied by, for example, bar coating, knife coating, roll coating, blade coating, die coating, gravure coating, or the like.

[0122] (4) Physical properties of adhesive sheets (4-1) Adhesive strength The adhesive strength of the adhesive sheet 1 according to the present embodiment to soda lime glass is preferably 10 N / 25 mm or more as a lower limit, more preferably 15 N / 25 mm or more, and even more preferably 20 N / 25 mm or more. When the lower limit of the adhesive strength is as above, the durability of the adhesive layer 11 becomes more excellent. Furthermore, the upper limit of the adhesive strength is preferably 100 N / 25 mm or less, more preferably 80 N / 25 mm or less, more preferably 60 N / 25 mm or less, and even more preferably 45 N / 25 mm or less. When the upper limit of the adhesive strength is as above, good reworkability is obtained, and re-adhesion is possible even if an adhesion error occurs.

[0123] The above adhesive strength basically refers to the adhesive strength measured by the 180-degree peeling method in accordance with JIS Z0237:2009. The measurement sample is 25 mm wide and 100 mm long, and the measurement sample is attached to the adherend and pressurized at 0.5 MPa and 50°C for 20 minutes, and then left to stand for 24 hours under conditions of normal pressure, 23°C, and 50% RH, and then measured at a peeling speed of 300 mm / min.

[0124] (4-2) Haze value The haze value of the adhesive layer 11 of the adhesive sheet 1 according to this embodiment is preferably 1% or less, more preferably 0.5% or less, particularly preferably 0.3% or less, and even more preferably 0.2% or less. The above haze value of the adhesive layer 11 provides excellent light transmission and is suitable for use in displays. The lower limit of the haze value is not particularly limited, and is preferably 0% or more, and more preferably 0.01% or more.

[0125] The haze value is a characteristic value including the thickness of the pressure-sensitive adhesive layer, and it is preferable that the haze value is satisfied regardless of the thickness of the pressure-sensitive adhesive layer. Here, the haze value in this specification is a value measured in accordance with JIS K7136:2000.

[0126] (4-3) Total light transmittance The total light transmittance of the adhesive layer 11 of the adhesive sheet 1 according to this embodiment is preferably 70% or more, more preferably 80% or more, particularly preferably 90% or more, further preferably 95% or more, and most preferably 99% or more. When the total light transmittance of the adhesive layer 11 is as described above, the adhesive layer 11 has excellent light transmittance and is suitable for use in displays. The upper limit of the total light transmittance is usually 100%. The total light transmittance in this specification is a value measured in accordance with JIS K7361-1:1997.

[0127] (4-4)CIE1976L*a*b* color system The pressure-sensitive adhesive layer 11 of the pressure-sensitive adhesive sheet 1 according to the present embodiment has an absolute value of chromaticity a* defined by the CIE1976 L*a*b* color system of preferably 0 or more, particularly preferably 0.1 or more. The absolute value of the chromaticity a* is preferably 0.8 or less, particularly preferably 0.6 or less, and more preferably 0.4 or less. The absolute value of the chromaticity b* of the pressure-sensitive adhesive layer 11 is preferably 0 or more, particularly preferably 0.1 or more. The absolute value of the chromaticity b* is preferably 0.8 or less, particularly preferably 0.6 or less, and more preferably 0.4 or less. As a result, the pressure-sensitive adhesive layer 11 has a color suitable for display. The methods for measuring the lightness L*, chromaticity a* and b* in this specification are as shown in the test examples described below.

[0128] [Display body] The display according to this embodiment comprises a first display member, a second display member, and an adhesive layer that bonds the first display member and the second display member to each other. The adhesive layer is made of the adhesive according to this embodiment described above. Here, the first display member and / or the second display member has an electrode made of a metal or metal oxide at least on the surface to be bonded (the adhesive layer side). In a preferred configuration, the second display member has the electrode at least on the surface to be bonded.

[0129] Examples of the display include a liquid crystal (LCD) display, a light emitting diode (LED) display, an organic electroluminescence (organic EL) display, electronic paper, etc., and may also be a touch panel. The display may also be a member constituting a part of these.

[0130] The first display member and the second display member may both be rigid and hard. The adhesive layer obtained from the adhesive composition P described above allows the first display member, which is a hard body, and the second display member, which is a hard body, to be bonded together without any problems.

[0131] The first display member is preferably a protective panel made of a glass plate, a plastic plate, or a laminate containing them. The first display member may have a step on the surface on the adhesive layer side. In this case, specifically, it is preferable that the step is caused by a printing layer. This printing layer is generally formed in a frame shape.

[0132] The glass plate is not particularly limited, and examples thereof include chemically strengthened glass, alkali-free glass, quartz glass, soda-lime glass, barium-strontium-containing glass, aluminosilicate glass, lead glass, borosilicate glass, barium borosilicate glass, etc. The thickness of the glass plate is not particularly limited, but is usually 0.1 to 5 mm, and preferably 0.2 to 2 mm.

[0133] The plastic plate is not particularly limited, and examples thereof include an acrylic plate, a polycarbonate plate, etc. The thickness of the plastic plate is not particularly limited, but is usually 0.2 to 5 mm, and preferably 0.4 to 3 mm.

[0134] In addition, various functional layers (electrode layer, silica layer, hard coat layer, anti-glare layer, etc.) may be provided on one or both sides of the above-mentioned glass plate or plastic plate, and optical members may be laminated thereon.

[0135] The material constituting the printing layer is not particularly limited, and known materials for printing are used. The lower limit of the thickness of the printing layer, i.e., the height of the step, is preferably 3 μm or more, more preferably 5 μm or more, particularly preferably 7 μm or more, and most preferably 10 μm or more. By setting the lower limit above, it is possible to sufficiently ensure concealment, such as making the electrical wiring invisible from the viewer side. In addition, the upper limit is preferably 50 μm or less, more preferably 35 μm or less, particularly preferably 25 μm or less, and even more preferably 20 μm or less. By setting the upper limit below the above, it is possible to prevent the step-following ability of the pressure-sensitive adhesive layer relative to the printing layer from deteriorating.

[0136] The second display component is preferably an optical component to which the first display component is to be attached, a display module (e.g., a liquid crystal (LCD) module, a light emitting diode (LED) module, an organic electroluminescence (OLED) module, etc.), an optical component as part of a display module, or a laminate including a display module, and has an electrode made of a metal or metal oxide on at least the surface facing the adhesive layer.

[0137] Examples of the optical member include a film sensor, an electrode film, a metal nanowire film, and a wire grid polarizing film.

[0138] Examples of the electrodes made of the above metals include metal wiring (including mesh-shaped, grid-shaped, and nanowire-shaped) made of silver, silver alloy, copper, copper alloy, etc. In particular, preferred examples include those constituting electrodes of touch panels, and specifically preferred examples include metal wiring contained in film sensors. Among the above metal wirings, metal wiring made of nanoparticles of silver or silver alloy is preferred, and as the silver alloy, silver alloy metal wiring in which palladium and copper are added to silver is particularly preferred. For these metal wirings, the adhesive layer 11 exerts an excellent migration prevention effect.

[0139] Examples of the electrode made of the metal oxide include a patterned transparent conductive film made of a metal oxide such as tin-doped indium oxide (ITO) or zinc oxide. Among the above, a patterned transparent conductive film made of ITO is particularly preferred, and the pressure-sensitive adhesive layer 11 is likely to exhibit an excellent migration prevention effect on the ITO transparent conductive film.

[0140] The wiring width of the positive and negative electrodes in the electrodes made of the above metals or the above metal oxides is preferably 100 μm or less, more preferably 60 μm or less, particularly preferably 45 μm or less, and even more preferably 35 μm or less. The wiring width is preferably 10 μm or more, more preferably 15 μm or more, particularly preferably 20 μm or more, and even more preferably 25 μm or more. When the wiring width is within the above range, the pressure-sensitive adhesive layer of the present embodiment can exhibit an excellent migration prevention effect while contributing to the miniaturization and narrowing of the pitch of the electrodes, and thus contributes to the improvement of the connection reliability of the electrodes.

[0141] The distance between the positive and negative electrodes in the electrodes made of the above metals or metal oxides is preferably 100 μm or less, more preferably 60 μm or less, particularly preferably 45 μm or less, and even more preferably 35 μm or less. The distance between the wires is preferably 10 μm or more, more preferably 15 μm or more, particularly preferably 20 μm or more, and even more preferably 25 μm or more. When the distance between the wires is within the above range, the pressure-sensitive adhesive layer of the present embodiment can exhibit an excellent migration prevention effect while contributing to the miniaturization and narrowing of the pitch of the electrodes, thereby contributing to the improvement of the connection reliability of the electrodes.

[0142] As an example of the display according to this embodiment, a capacitive touch panel 2 is shown in FIG. 2. The touch panel 2 includes a display module 3, a first film sensor 5a laminated thereon via an adhesive layer 4, a second film sensor 5b laminated thereon via a first adhesive layer 11, and a cover material 6 laminated thereon via a second adhesive layer 11. A printed layer 7 is formed on the surface of the cover material 6 facing the second adhesive layer 11, and therefore a step is present depending on the presence or absence of the printed layer 7. In this embodiment, the cover material 6 corresponds to the first display member, and the second film sensor 5b corresponds to the second display member, or the second film sensor 5b corresponds to the first display member, and the first film sensor 5a corresponds to the second display member.

[0143] Considering the migration prevention effect, it is preferable that both the first adhesive layer 11 and the second adhesive layer 11 in the touch panel 2 are the adhesive layer 11 of the adhesive sheet 1. When the first adhesive layer 11 or the second adhesive layer 11 is not the adhesive layer 11 of the adhesive sheet 1, examples of the adhesive constituting the adhesive layer include acrylic adhesives, rubber adhesives, silicone adhesives, urethane adhesives, polyester adhesives, polyvinyl ether adhesives, etc., and among these, acrylic adhesives are preferred.

[0144] The adhesive layer 4 may be formed by the adhesive layer 11 of the adhesive sheet 1, or may be formed by another adhesive or adhesive sheet. In the latter case, examples of the adhesive constituting the adhesive layer 4 include acrylic adhesives, rubber adhesives, silicone adhesives, urethane adhesives, polyester adhesives, polyvinyl ether adhesives, etc., among which acrylic adhesives are preferred.

[0145] In this embodiment, the first film sensor 5a and the second film sensor 5b each include a base film 51 and an electrode 52 formed on the base film 51. The base film 51 is not particularly limited, but examples of the base film that can be used include a polyethylene terephthalate film, an acrylic film, and a polycarbonate film.

[0146] The electrodes 52 are as described above. Generally, one of the electrodes 52 of the first film sensor 5a and the electrodes 52 of the second film sensor 5b forms a circuit pattern in the X-axis direction, and the other forms a circuit pattern in the Y-axis direction.

[0147] In this embodiment, the electrode 52 of the second film sensor 5b is located above the second film sensor 5b in Fig. 2. On the other hand, the electrode 52 of the first film sensor 5a is located above the first film sensor 5a in Fig. 2, but is not limited to this and may be located below the first film sensor 5a.

[0148] An example of a method for manufacturing the touch panel 2 will be described below. A first adhesive sheet 1 and a second adhesive sheet 1 are prepared as the adhesive sheet 1. One release sheet 12a is peeled off from the first adhesive sheet 1, and the exposed adhesive layer 11 (first adhesive layer) is attached to the first film sensor 5a so as to contact the electrode 52 of the first film sensor 5a. Also, one release sheet 12a is peeled off from the second adhesive sheet 1, and the exposed adhesive layer 11 (second adhesive layer 11) is attached to the second film sensor 5b so as to contact the electrode 52 of the second film sensor 5b.

[0149] Then, the other release sheet 12b of the first adhesive sheet 1 is peeled off, and the two are attached together so that the exposed first adhesive layer 11 contacts the surface of the second film sensor 5b opposite to the surface on which the second adhesive layer 11 is laminated (the exposed surface of the base film 51 of the second film sensor 5b). This results in a laminate in which the release sheet 12b, the second adhesive layer 11, the second film sensor 5b, the first adhesive layer 11, and the first film sensor 5a are laminated in this order.

[0150] Next, the adhesive layer 4 provided on the release sheet is attached to the surface of the laminate on the first film sensor 5a side (the exposed surface of the base film 51 of the first film sensor 5a). Next, the release sheet 12b is peeled off from the laminate, and the cover material 6 is attached to the exposed second adhesive layer 11 so that the printed layer 7 side of the cover material 6 is in contact with the second adhesive layer 11. By the above attachment, a structure is obtained in which the cover material 6, the second adhesive layer 11, the second film sensor 5b, the first adhesive layer 11, the first film sensor 5a, the adhesive layer 4, and the release sheet are laminated in this order.

[0151] Next, the release sheet is peeled off from the above-mentioned structure, and the structure is attached to the display module 3 so that the exposed pressure-sensitive adhesive layer 4 contacts the display module 3. In this way, the touch panel 2 shown in FIG. 2 is manufactured.

[0152] Here, when the first adhesive layer 11 and / or the second adhesive layer 11 is made of an active energy ray-curable adhesive, the adhesive layer 11 in the above-mentioned structure or touch panel 2 is irradiated with active energy rays. This causes the active energy ray-curable component (G) in the adhesive layer 11 to polymerize, and the adhesive layer 11 is cured to become a cured adhesive layer. The adhesive layer 11 is usually irradiated with energy rays from one surface side of the above-mentioned structure or touch panel 2, preferably from the surface side of the cover material 6.

[0153] The active energy ray refers to electromagnetic waves or charged particle rays having an energy quantum, and specific examples thereof include ultraviolet rays, electron beams, etc. Among active energy rays, ultraviolet rays are particularly preferred because they are easy to handle.

[0154] The ultraviolet irradiation can be performed by a high pressure mercury lamp, a fusion H lamp, a xenon lamp, etc., and the amount of ultraviolet irradiation is 50 to 1000 mW / cm illuminance. 2 is preferably 100 to 600 mW / cm 2 The light intensity is preferably 50 to 10,000 mJ / cm. 2 is preferably 80 to 5000 mJ / cm 2 More preferably, it is 200 to 2000 mJ / cm 2 On the other hand, the irradiation with the electron beam can be carried out by an electron beam accelerator or the like, and the irradiation dose of the electron beam is preferably about 10 to 1000 krad.

[0155] The gel fraction of the adhesive (adhesive after active energy ray irradiation) constituting the cured adhesive layer is preferably 35% or more as a lower limit, particularly preferably 50% or more, and more preferably 65% ​​or more. When the lower limit of the gel fraction of the adhesive after active energy ray irradiation is as above, the durability is higher. Furthermore, the upper limit of the gel fraction is preferably 90% or less, particularly preferably 80% or less, and more preferably 75% or less. When the upper limit of the gel fraction of the adhesive after active energy ray irradiation is as above, it is possible to prevent the adhesive strength of the cured adhesive layer from decreasing and the durability from deteriorating. The method for measuring the gel fraction of the adhesive after active energy ray irradiation is as shown in the test example described below.

[0156] The adhesive strength of the adhesive sheet having the cured adhesive layer to soda lime glass is preferably 10N / 25mm or more as a lower limit, more preferably 20N / 25mm or more, particularly preferably 30N / 25mm or more, and even more preferably 40N / 25mm or more. When the adhesive strength has the above lower limit, the resulting product (touch panel 2) has high durability. The upper limit of the adhesive strength is not particularly limited, but is usually preferably 100N / 25mm or less, particularly preferably 80N / 25mm or less, and even more preferably 60N / 25mm or less.

[0157] The adhesive strength mentioned above basically refers to the adhesive strength measured by the 180-degree peeling method in accordance with JIS Z0237:2009. The measurement sample is 25 mm wide and 100 mm long, and the measurement sample is attached to the adherend and pressurized at 0.5 MPa and 50°C for 20 minutes, and then irradiated with active energy rays (ultraviolet rays) under the conditions shown in the test example described later. The adhesive strength is then measured at a peeling speed of 300 mm / min after leaving it for 24 hours under conditions of normal pressure, 23°C, and 50% RH.

[0158] Even when the touch panel 2 is placed under high temperature and high humidity conditions and a voltage is applied to the electrodes 52 in this state, migration of the electrodes 52 is effectively suppressed, and changes in the resistance value of the electrodes 52 are also effectively suppressed. This prevents driving defects of the touch panel 2 caused by breaks or short circuits in the electrodes 52.

[0159] Here, the change in resistance value of the electrode 52 will be specifically described. When a soda lime glass and an electrode plate (silver wiring electrode plate in the embodiment) are bonded via the adhesive layer 11 of the adhesive sheet 1 according to the present embodiment, and a durability test is performed on the resulting laminate, the resistance value change rate of the electrode plate calculated by the following formula is preferably less than 50%, particularly preferably less than 30%, and more preferably less than 15%. The lower limit is not particularly limited, but is preferably 0% or more. Similarly, when a soda lime glass and an ITO vapor deposition film are bonded via the adhesive layer 11 of the adhesive sheet 1 according to the embodiment, and a durability test is performed on the resulting laminate, the resistance value change rate of the ITO vapor deposition film calculated by the following formula is preferably less than 200%, particularly preferably less than 150%, and more preferably less than 100%. The lower limit is not particularly limited, but is preferably 0% or more. Resistance change rate (%) = {(RR 0 ) / R 0}×100 (In the formula, R 0 is the initial resistance value (Ω) before the durability test, and R is the resistance value (Ω) after the durability test. The details of the method for measuring the rate of change in resistance value are as shown in the test examples described later.

[0160] The above-described embodiments are described for the purpose of facilitating understanding of the present invention, and are not described for the purpose of limiting the present invention. Therefore, each element disclosed in the above embodiment is intended to include all design modifications and equivalents that fall within the technical scope of the present invention.

[0161] For example, one of the release sheets 12a and 12b may be omitted from the adhesive sheet 1. Furthermore, in the touch panel 2, the printing layer 7 may not be formed on the cover material 6. EXAMPLES

[0162] The present invention will be described in more detail below with reference to examples, but the scope of the present invention is not limited to these examples.

[0163] Example 1 1. Preparation of (meth)acrylic acid ester polymer (A) 60 parts by mass of 2-ethylhexyl acrylate, 20 parts by mass of methyl methacrylate, and 20 parts by mass of 2-hydroxyethyl acrylate were copolymerized by solution polymerization to prepare a (meth)acrylic acid ester polymer (A). The molecular weight of this (meth)acrylic acid ester polymer (A) was measured by the method described below, and the weight average molecular weight (Mw) was 700,000.

[0164] 2. Preparation of adhesive composition 100 parts by mass (solid content equivalent; the same applies below) of the (meth)acrylic acid ester polymer (A) obtained in the above step 1, 0.15 parts by mass of 1H-benzotriazole (B1) as a rust inhibitor (B), and a long-chain alkylamine (C) represented by the following general formula (c): [ka] (weight average molecular weight: 900, carbon number of R: 14 to 18, sum of values ​​of m and n: 15) and 0.15 parts by mass of a silane compound (D) represented by the following structural formula (II): [ka] 0.25 parts by mass of an organosilicon compound (D1) represented by the formula: 1.0 part by mass of dipropylene glycol monomethyl ether as an alkylene glycol (E) and 0.6 parts by mass of trimethylolpropane-modified tolylene diisocyanate (manufactured by Toyochem Co., Ltd., product name "BHS8515") as a crosslinking agent (F) were mixed, thoroughly stirred and diluted with methyl ethyl ketone to obtain a coating solution of an adhesive composition.

[0165] Here, the formulations (solid content equivalent) of the pressure-sensitive adhesive composition when the (meth)acrylic acid ester polymer (A) is taken as 100 parts by mass (solid content equivalent) are shown in Table 1. Details of the abbreviations, components, etc. shown in Table 1 are as follows. [(Meth)acrylic acid ester polymer (A)] 2EHA: 2-ethylhexyl acrylate MMA: Methyl methacrylate HEA: 2-hydroxyethyl acrylate IBXA: Isobornyl acrylate ACMO: N-Acryloylmorpholine BA: n-butyl acrylate [Rust inhibitor (B)] B1: 1H-benzotriazole B2: 1-[N,N-bis(2-ethylhexyl)aminomethyl]methylbenzotriazole [Silane compounds (D)] D1: An organosilicon compound represented by the above structural formula (II) D2: An organosilicon compound represented by the following structural formula (III): [ka] [Active energy ray-curable component (G)] ε-Caprolactone modified tris-(2-acryloxyethyl) isocyanurate [Photopolymerization initiator (H)] 1:1 (mass ratio) mixture of 1-hydroxy-cyclohexyl-phenyl-ketone and benzophenone [Ultraviolet absorber] 2,2-Dihydroxy-4-methoxybenzophenone

[0166] 3. Manufacturing of adhesive sheets The adhesive composition coating solution obtained in step 2 above was applied using a knife coater to the release-treated surface of a heavy-release release sheet (manufactured by Lintec Corporation, product name "SP-PET382150", thickness: 38 μm) in which one side of a polyethylene terephthalate film had been treated with a silicone-based release agent, and then the sheet was heated at 80°C for 1 minute and further heated at 110°C for 1 minute to form a coating layer (thickness: 50 μm).

[0167] Next, the coating layer on the heavy release type release sheet obtained above was attached to a light release type release sheet (manufactured by Lintec Corporation, product name "SP-PET381130"), one side of which was a polyethylene terephthalate film treated with a silicone-based release agent, so that the release-treated surface of the light release type release sheet was in contact with the coating layer, and the sheet was cured for 7 days under conditions of 23°C and 50% RH to produce an adhesive sheet consisting of heavy release type release sheet / adhesive layer (thickness: 50 μm) / light release type release sheet.

[0168] [Examples 2 to 11, Comparative Examples 1 to 7] Pressure-sensitive adhesive sheets were produced in the same manner as in Example 1, except that the types and ratios of the monomers constituting the (meth)acrylic acid ester polymer (A), the weight-average molecular weight of the (meth)acrylic acid ester polymer (A), the type and amount of the rust inhibitor (B), the amount of the long-chain alkylamine (C), the type and amount of the silane compound (D), the amount of the alkylene glycol (E), and the amount of the crosslinking agent (F) were changed as shown in Table 1. Note that, in Example 2, an ultraviolet absorber was further added, and in Examples 6, 7, 9, and 10 and Comparative Examples 6 and 7, an active energy ray-curable component (G) and a photopolymerization initiator (H) were further added.

[0169] The weight average molecular weight (Mw) mentioned above is a polystyrene-equivalent weight average molecular weight measured by gel permeation chromatography (GPC) under the following conditions (GPC measurement). <Measurement conditions> GPC measuring device: Tosoh HLC-8020 GPC columns (passed in the following order): Tosoh Corporation TSK guard column HXL-H TSK gel GMHXL (×2) TSK gel G2000HXL Measurement solvent: Tetrahydrofuran ·Measurement temperature: 40℃

[0170] [Test Example 1] (Measurement of gel fraction) The adhesive sheets obtained in the examples and comparative examples were cut to a size of 80 mm x 80 mm, the adhesive layer was wrapped in a polyester mesh (mesh size 200), and the mass was measured using a precision balance. The mass of the mesh alone was subtracted to calculate the mass of the adhesive alone. This mass was designated as M1.

[0171] Next, the adhesive wrapped in the polyester mesh was immersed in ethyl acetate at room temperature (23°C) for 24 hours. The adhesive was then removed and air-dried for 24 hours in an environment with a temperature of 23°C and a relative humidity of 50%, and then dried in an oven at 80°C for 12 hours. After drying, the mass was weighed using a precision balance, and the mass of the adhesive alone was calculated by subtracting the mass of the mesh alone. The mass at this time was designated M2. The gel fraction (%) was expressed as (M2 / M1) x 100. The results are shown in Table 2.

[0172] The gel fraction was measured before and after ultraviolet (UV) irradiation of the adhesive layer (irradiation from the heavy release type release sheet side) for the pressure-sensitive adhesive sheets of Examples 6, 7, 9, and 10 and Comparative Examples 6 and 7. The ultraviolet irradiation conditions were as follows:

[0173] <Ultraviolet irradiation conditions> -High pressure mercury lamp used ·Illuminance 200mW / cm 2 ,Light intensity 1000mJ / cm 2 The UV illuminance and light intensity meter used is the "UVPF-A1" manufactured by Eye Graphics.

[0174] [Test Example 2] (Haze value measurement) The adhesive layer of the adhesive sheet produced in the examples and comparative examples was attached to glass to prepare a measurement sample. After background measurement was performed on the glass, the haze value (total light haze value;%) of the measurement sample was measured using a haze meter (manufactured by Nippon Denshoku Industries Co., Ltd., product name "NDH-5000") in accordance with JIS K7136:2000. The results are shown in Table 2.

[0175] [Test Example 3] (Measurement of total light transmittance) The adhesive layer of the adhesive sheet produced in the examples and comparative examples was attached to glass to prepare a measurement sample. After background measurement was performed on the glass, the total light transmittance (%) of the measurement sample was measured using a haze meter (manufactured by Nippon Denshoku Industries Co., Ltd., product name "SH-7000") in accordance with JIS K7361-1:1997. The results are shown in Table 2.

[0176] [Test Example 4] (Measurement of L*a*b* color system) The chromaticity a* and chromaticity b* defined by the CIE1976L*a*b* color system were measured for the adhesive layers of the adhesive sheets produced in the Examples and Comparative Examples using a simultaneous photometric spectrophotometer (manufactured by Nippon Denshoku Industries Co., Ltd., product name "SQ2000"). The results are shown in Table 2.

[0177] [Test Example 5] (Measurement of adhesive strength) The light release type release sheet was peeled off from the adhesive sheet obtained in the Examples and Comparative Examples, and the exposed adhesive layer was attached to an easy-adhesion layer of a polyethylene terephthalate (PET) film (manufactured by Toyobo Co., Ltd., product name "PET A4300", thickness: 100 μm) having an easy-adhesion layer to obtain a release sheet / adhesive layer / PET film laminate. The obtained laminate was cut into a width of 25 mm and a length of 100 mm to prepare a sample.

[0178] In an environment of 23°C and 50% RH, the heavy release type release sheet was peeled off from the above sample, and the exposed adhesive layer was attached to soda lime glass (manufactured by Nippon Sheet Glass Co., Ltd.), and then pressure was applied for 20 minutes at 0.5 MPa and 50°C in an autoclave manufactured by Kurihara Seisakusho Co., Ltd. After that, the sample was left for 24 hours under conditions of 23°C and 50% RH, and the adhesive strength (N / 25mm) was measured using a tensile tester (manufactured by Orientec Co., Ltd., Tensilon) at a peel speed of 300 mm / min and a peel angle of 180 degrees. The measurement was performed in accordance with JIS Z0237:2009 under conditions other than those described here. The results are shown in Table 2.

[0179] In addition, the adhesive strength of the pressure-sensitive adhesive sheets of Examples 6, 7, 9, and 10 and Comparative Examples 6 and 7 was also measured after ultraviolet (UV) irradiation. Specifically, after the above autoclave treatment, the adhesive layer was irradiated with ultraviolet light from the soda-lime glass side under the same conditions as in Test Example 1. After that, the adhesive was left for 24 hours under conditions of 23°C and 50% RH, and then the adhesive strength (N / 25 mm; after UV) was measured in the same manner as above. The results are shown in Table 2.

[0180] [Test Example 6] (Evaluation of migration prevention effect) (1) Preparation of silver wiring electrode plate Silver paste (manufactured by Toyochem Co., Ltd., product name "RA FS088") was applied by screen printing onto the easy-adhesion treated surface of a polyethylene terephthalate (PET) film (manufactured by Toray Industries, product name "Lumirror U48", thickness: 125 μm) so that the positive and negative electrode wires were linear and parallel to each other. After that, a heat treatment was performed at 135°C for 30 minutes to harden the silver paste, and an electrode plate with silver wiring (silver wiring electrode plate) was obtained. The width of the positive and negative electrode wires was 30 μm, and the distance between the wires was 30 μm.

[0181] (2) Evaluation of migration prevention effect The light release type release sheet was peeled off from the adhesive sheet obtained in the examples and comparative examples, and the exposed adhesive layer was attached to an easy-adhesion layer of a polyethylene terephthalate (PET) film (manufactured by Toyobo Co., Ltd., product name "PET A4300", thickness: 100 μm) having an easy-adhesion layer, to obtain a laminate of heavy release type release sheet / adhesive layer / PET film. Next, the heavy release type release sheet was peeled off from the laminate, and the exposed adhesive layer was attached to the positive electrode wiring and the negative electrode wiring of the electrodes. Then, the laminate was autoclaved for 20 minutes under conditions of 50°C and 0.5 MPa, and then left for 24 hours under conditions of 23°C and 50% RH, and this was used as a sample.

[0182] For the pressure-sensitive adhesive sheets of Examples 6, 7, 9, and 10 and Comparative Examples 6 and 7, after the autoclave treatment, the pressure-sensitive adhesive layer was irradiated with ultraviolet light from the PET film side under the same conditions as in Test Example 1, and these were used as samples.

[0183] The above sample was left to stand under humid heat conditions of 105°C and 100% RH, and in this state, a voltage of 5 V was applied between the electrodes to perform a migration test. 20 hours after the start of the test, the positive electrode wiring and the negative electrode wiring were observed with an optical microscope (magnification: 10x), and the migration prevention effect was evaluated based on the evaluation criteria shown below. The results are shown in Table 2. Note that no defects such as lifting, peeling, or the generation of air bubbles were observed in any of the samples of the examples and comparative examples. ⊚: No dissolution of the positive electrode wiring or no dendrite formation in the negative electrode wiring was observed. ◯: No dissolution of the positive electrode wiring or no dendrite formation in the negative electrode wiring was observed, but discoloration of the wiring was observed. ×: Dissolution of the positive electrode wiring or formation of dendrites in the negative electrode wiring is observed.

[0184] [Test Example 7] (Evaluation of change in resistance value) The sample prepared in Test Example 6 was used as measurement sample A (silver wiring electrode plate sample).

[0185] In addition, soda lime glass (length 70 mm × width 150 mm × thickness 1.0 mm; manufactured by Nippon Sheet Glass Co., Ltd.) and ITO vapor deposition film (manufactured by Oike Kogyo Co., Ltd., product name "Tetlite TCF KH150NMH2-125-U6 / T2", ITO vapor deposition film side contacts the adhesive layer) were bonded via the adhesive layer of the adhesive sheet obtained in the examples and comparative examples. Then, autoclaving was performed for 20 minutes under conditions of 50°C and 0.5 MPa, and then it was left for 24 hours under conditions of 23°C and 50% RH to obtain measurement sample B (ITO vapor deposition film sample).

[0186] For the pressure-sensitive adhesive sheets of Examples 6, 7, 9 and 10 and Comparative Examples 6 and 7, after the autoclave treatment, the pressure-sensitive adhesive layer was irradiated with ultraviolet light from the soda-lime glass side under the same conditions as in Test Example 1, and these were used as measurement samples.

[0187] For the above measurement sample A, a voltage of 5 V was applied between the positive and negative wiring to obtain the initial resistance R 0 On the other hand, the initial resistance value R of the measurement sample B was measured using a non-contact resistance measuring device (manufactured by Napson, product name "EC-80"). 0 (Ω) was measured.

[0188] Next, the above measurement samples A and B were placed in a humid and hot environment of 105℃ and 100% RH for 3 hours. After that, they were left to stand in a normal temperature and humidity environment of 23℃ and 50% RH for 24 hours, and the resistance value (Ω) was measured in the same manner as the initial resistance value above. This was the resistance value R after the durability test. The resistance value change rate (%) was calculated from the obtained measured values ​​using the following formula. Resistance change rate (%) = {(RR 0 ) / R 0}×100

[0189] The resistance change was evaluated based on the rate of change in resistance calculated above, according to the following criteria. The results are shown in Table 2. <Evaluation criteria for silver wiring electrode plate samples> ◎: Resistance change rate is less than 15% ○: Resistance change rate is 15% or more and less than 30% △: The change rate of resistance value is 30% or more and less than 50% ×: The change rate of resistance value is 50% or more <Evaluation criteria for ITO vapor deposition film samples> ◎: The change rate of resistance value is less than 100% ○: The change rate of resistance value is 100% or more and less than 150% △: The change rate of resistance value is 150% or more and less than 200% ×: The change rate of resistance value is 200% or more

[0190]

Table 1

[0191]

Table 2

[0192] As can be seen from Table 2, according to the adhesive sheet obtained in the examples, migration in the silver wiring electrode plate could be prevented. Further, according to the adhesive sheet obtained in the examples, changes in the resistance values of the silver wiring electrode plate and the ITO vapor deposition film could be suppressed.

Industrial Applicability

[0193] The pressure-sensitive adhesive composition, pressure-sensitive adhesive, and adhesive sheet according to the present invention can be suitably used, for example, in a capacitive touch panel. Further, the display body according to the present invention is suitable, for example, as a capacitive touch panel.

Explanation of Symbols

[0194] 1... Adhesive sheet 11... Adhesive layer 12a, 12b... Release sheet 2... Touch panel 3... Display body module 4... Adhesive layer 5a... First film sensor 5b... Second film sensor 51... Base film 52…Electrode 6…Cover material 7…Printing layer

Claims

1. A (meth)acrylic acid ester polymer (A) as a base polymer, A benzotriazole compound, a long-chain alkylamine (C) which is an amine containing a long-chain alkyl group having 10 or more and 24 or less carbon atoms in the molecule; A silane compound (D) having an alkoxysilyl group at both ends, A crosslinking agent (F); Contains 1. An adhesive composition comprising:

2. A (meth)acrylic acid ester polymer (A) as a base polymer, A benzotriazole compound, a long-chain alkylamine (C) which is an amine containing a long-chain alkyl group having 10 or more and 24 or less carbon atoms in the molecule; A silane compound (D) having an alkoxysilyl group at both ends, A crosslinking agent (F); Contains The weight average molecular weight of the long-chain alkylamine (C) is 500 or more and 1,400 or less.

1. An adhesive composition comprising:

3. A (meth)acrylic acid ester polymer (A) as a base polymer, A benzotriazole compound, A long-chain alkylamine (C); A silane compound (D) having an alkoxysilyl group at both ends, A crosslinking agent (F); Contains The long-chain alkylamine (C) is a compound represented by the following general formula (c): 【Chemistry 1】 (In the formula, R is a long-chain alkyl group having 10 or more and 24 or less carbon atoms. m and n are each independently an integer of 1 or more, and the sum of the values ​​of m and n is 8 or more and 30 or less.) 1. An adhesive composition comprising:

4. The pressure-sensitive adhesive composition according to any one of claims 1 to 3, characterized in that it contains an alkylene glycol (E).

5. 3. The adhesive composition according to claim 1, wherein the long-chain alkylamine (C) is a tertiary amine.

6. The pressure-sensitive adhesive composition according to any one of claims 1 to 5, characterized in that the (meth)acrylic acid ester polymer (A) does not contain a carboxy group-containing monomer as a monomer unit constituting the polymer.

7. The pressure-sensitive adhesive composition according to any one of claims 1 to 6, characterized in that the (meth)acrylic acid ester polymer (A) contains, as a monomer unit constituting the polymer, 6 mass% or more and 35 mass% or less of a hydroxyl group-containing monomer.

8. The pressure-sensitive adhesive composition according to any one of claims 1 to 7, further comprising an ultraviolet absorber.

9. The adhesive composition according to any one of claims 1 to 8, which is an adhesive composition for forming an adhesive to be in contact with an electrode made of a metal or a metal oxide.

10. A pressure-sensitive adhesive obtained by crosslinking the pressure-sensitive adhesive composition according to any one of claims 1 to 9.

11. Two release sheets; a pressure-sensitive adhesive layer sandwiched between the two release sheets so as to be in contact with the release surfaces of the two release sheets; The pressure-sensitive adhesive layer is made of the pressure-sensitive adhesive according to claim 10. A pressure-sensitive adhesive sheet characterized by:

12. A first display member; A second display member; an adhesive layer that bonds the first display member and the second display member to each other; A display comprising: the first display member and / or the second display member has an electrode made of a metal or a metal oxide on at least the surface to be bonded; The pressure-sensitive adhesive layer is made of the pressure-sensitive adhesive according to claim 10. A display characterized by:

Citation Information

Patent Citations

  • Corrosion inhibitor for copper and copper alloy

    JP1998121271A

  • Rust preventive coating, method for forming coating film, and coated article

    JP2013023543A

  • Pressure-sensitive adhesive composition, pressure-sensitive adhesive layer, pressure-sensitive adhesive sheet, optical member and touch panel

    JP2014177611A

  • Curable adhesive composition for polarization film, polarization film and manufacturing method thereof, optical film and image display device

    JP2017021239A

  • Electrically peelable adhesive composition, adhesive sheet, and adhered body

    JP2019059908A