Die-bonding sheet, dicing die-bonding film, semiconductor device, and electronic apparatus
The die-bonding sheet with a tailored thermoplastic resin and inorganic filler composition addresses the dual performance challenge of pick-up and die-bonding, ensuring reliable adhesion and separation in semiconductor manufacturing.
Patent Information
- Application Number
- JP2024018732
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-02-09
- Publication Date
- 2024-10-11
AI Technical Summary
Existing die-bonding sheets fail to achieve both good pick-up performance and die-bonding performance simultaneously due to variations in surface roughness and thermal properties, leading to inconsistent adhesion and peeling issues during the manufacturing process of semiconductor devices.
A die-bonding sheet composed of a thermoplastic resin with specific elastic modulus ranges and a combination of first and second thermoplastic resins with varying molecular weights, along with an inorganic filler, to maintain optimal pick-up and die-bonding performance across different temperature conditions.
The die-bonding sheet achieves both good pick-up performance at lower temperatures and effective die-bonding at higher temperatures, ensuring consistent adhesion and separation of semiconductor chips without thermal degradation.
Smart Images

Figure 2024144135000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a die bond sheet used when manufacturing a semiconductor device having, for example, a semiconductor integrated circuit, and a dicing die bond film provided with the die bond sheet. The present invention also relates to a semiconductor device provided with the die bond sheet. The present invention also relates to an electronic device provided with the semiconductor device. [Background technology]
[0002] Conventionally, a dicing die bond film used in the manufacture of a semiconductor device is known. This type of dicing die bond film includes, for example, a dicing tape and a die bond sheet laminated on the dicing tape and attached to a wafer. The dicing tape has a base layer and an adhesive layer in contact with the die bond sheet. This type of dicing die bond film is used, for example, as follows in the manufacture of a semiconductor device.
[0003] A method for manufacturing a semiconductor device generally includes a front-end process of forming a circuit surface on one side of a wafer using highly integrated electronic circuits, and a back-end process of cutting chips out of the wafer with the circuit surface formed thereon and assembling them.
[0004] The post-process includes, for example, a fragile part forming process in which a fragile part is formed in the semiconductor wafer by laser light or the like to cut the wafer (semiconductor wafer) on which the circuit surface is formed into small chips (dies), a back grinding process in which the surface opposite to the circuit surface of the wafer on which the fragile part is formed is polished and cut, a mounting process in which the surface opposite to the circuit surface of the wafer is attached to a die bond sheet and the semiconductor wafer is fixed to the dicing tape via the die bond sheet, a dicing process in which the dicing tape is stretched in the surface direction to separate the semiconductor wafer into chips (dies) with the fragile part as a boundary and to widen the gap between adjacent chips (dies), a pick-up process in which the die bond sheet is peeled off from the adhesive layer to take out the chip (dies) with the die bond sheet attached, a die bond process in which the chip (dies) with the die bond sheet attached is attached to an adherend via the die bond sheet, and a curing process in which the die bond sheet attached to the adherend is hardened. The semiconductor integrated circuit in the semiconductor device is manufactured, for example, through these processes.
[0005] In the above-mentioned manufacturing method of a semiconductor device, in the pick-up step, the chip (die) with the die bond sheet attached thereto is peeled off from the adhesive layer of the dicing tape, and then in the die bond step, the chip (die) with the die bond sheet attached thereto is heated and pressed against the adherend. These steps are continuously repeated using, for example, one pick-up collet. Therefore, when the pick-up step and the die bond step are repeated, the heat of the pick-up collet, which is increased by heating, is transferred to the die bond sheet. When the temperature of the die bond sheet increases, the above-mentioned peeling in the pick-up step may not occur well due to reasons such as changes in the physical properties of the die bond sheet.
[0006] In response to this, in order to perform the above-mentioned peeling well in the pick-up process, i.e., to improve the pick-up performance, a die-bonding sheet is known in which the surface roughness of the die-bonding sheet on the side in contact with the adhesive layer is designed to a specific value (for example, Patent Document 1).
[0007] Specifically, the die bond sheet described in Patent Document 1 has an arithmetic mean roughness Ra1 of 0.05 to 2.50 μm on the surface in contact with the adhesive layer, and the ratio of the above Ra1 to the arithmetic mean roughness Ra2 of the surface opposite to the surface in contact with the adhesive layer is 1.05 to 28.00. According to the die bond sheet described in Patent Document 1, even if the temperature of the pickup collet rises, the deterioration of the pickup performance can be suppressed. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2022-150243 A Summary of the Invention [Problem to be solved by the invention]
[0009] However, even if a die bond sheet with a designed surface roughness as described above is used, the chip (die) cannot necessarily be well bonded to the adherend through the die bond sheet in the subsequent die bond process. That is, a die bond sheet with a surface roughness simply designed to a specific value cannot achieve both pick-up performance and adhesive performance (die bond performance). Therefore, there is a demand for a die bond sheet that has both good pick-up performance and good die bond performance.
[0010] However, it cannot be said that a die bond sheet having both good pick-up performance and good die bond performance and a dicing die bond film including the die bond sheet have been sufficiently studied yet.
[0011] Therefore, the present invention aims to provide a die bond sheet and a dicing die bond film having both good pickup performance and good die bond performance. The present invention also aims to provide a semiconductor device including the die bond sheet and an electronic device including the semiconductor device. [Means for solving the problem]
[0012] In order to solve the above problems, the die bond sheet according to the present invention has the following features: A die bond sheet containing at least a thermoplastic resin and an inorganic filler, The thermoplastic resin includes a first thermoplastic resin and a second thermoplastic resin having an average molecular weight smaller than that of the first thermoplastic resin, It is characterized in that the elastic modulus at 50°C before curing is 2.0 MPa or more and 10.0 MPa or less, and the elastic modulus at 130°C is 0.1 MPa or more and 1.5 MPa or less.
[0013] The dicing die bond film according to the present invention comprises the above-mentioned die bond sheet and a dicing tape attached to the die bond sheet.
[0014] A semiconductor device according to the present invention includes the above-mentioned die bond sheet. An electronic device according to the present invention includes the semiconductor device described above. Effect of the Invention
[0015] The die bonding sheet and dicing tape according to the present invention can combine good pick-up performance and good die bonding performance. [Brief description of the drawings]
[0016] [Figure 1] FIG. 2 is a cross-sectional view of the dicing die bond film of the present embodiment cut in the thickness direction. [Figure 2A] 1A to 1C are cross-sectional views illustrating a stealth dicing process in a manufacturing method of a semiconductor device. [Figure 2B] 1A to 1C are cross-sectional views illustrating a stealth dicing process in a manufacturing method of a semiconductor device. [Figure 2C] 1A to 1C are cross-sectional views illustrating a stealth dicing process in a manufacturing method of a semiconductor device. [Figure 2D]1A to 1C are cross-sectional views illustrating a back grinding process in a manufacturing method of a semiconductor device. [Figure 3A] 1A to 1C are cross-sectional views each showing a schematic view of a mounting step in a manufacturing method of a semiconductor device. [Figure 3B] 1A to 1C are cross-sectional views each showing a schematic view of a mounting step in a manufacturing method of a semiconductor device. [Figure 4A] 1A to 1C are cross-sectional views each showing a schematic view of an expanding step performed at a low temperature in a method for manufacturing a semiconductor device. [Figure 4B] 1A to 1C are cross-sectional views each showing a schematic view of an expanding step performed at a low temperature in a method for manufacturing a semiconductor device. [Figure 4C] 1A to 1C are cross-sectional views each showing a schematic view of an expanding step performed at a low temperature in a method for manufacturing a semiconductor device. [Figure 5A] 4A to 4C are cross-sectional views illustrating an expansion step at room temperature in the manufacturing method of the semiconductor device. [Figure 5B] 4A to 4C are cross-sectional views illustrating an expansion step at room temperature in the manufacturing method of the semiconductor device. [Figure 6] 1A to 1C are cross-sectional views illustrating a pickup step in a manufacturing method of a semiconductor device. [Figure 7] 1A to 1C are cross-sectional views each showing a schematic diagram of a die bonding step in a manufacturing method of a semiconductor device. [Figure 8] 1A to 1C are cross-sectional views each showing a schematic diagram of a wire bonding step in a manufacturing method of a semiconductor device. [Figure 9] 5A to 5C are cross-sectional views each showing a schematic diagram of an encapsulation step in the manufacturing method of the semiconductor device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, an embodiment of a die bond sheet according to the present invention and a dicing die bond film including the die bond sheet will be described with reference to the drawings.
[0018] 1, the dicing die bond film 1 of this embodiment includes a dicing tape 20 and a die bond sheet 10 that is laminated on an adhesive layer 22 of the dicing tape 20 and adhered to a semiconductor wafer. The die bond sheet 10 is adhered to an adherend such as a circuit board or a semiconductor chip in the manufacture of a semiconductor device having a semiconductor integrated circuit, for example. It should be noted that the figures in the drawings are schematic diagrams and the aspect ratios are not necessarily the same as those of the actual products.
[0019] <Dicing die bond film die bond sheet> The die bond sheet 10 contains at least a thermoplastic resin and an inorganic filler. The thermoplastic resin contains a first thermoplastic resin and a second thermoplastic resin having an average molecular weight smaller than that of the first thermoplastic resin. The elastic modulus of the die bond sheet 10 before curing at 50° C. is 2.0 MPa or more and 10.0 MPa or less, and the elastic modulus at 130° C. is 0.1 MPa or more and 1.5 MPa or less. The die bond sheet 10 may further contain a thermosetting resin.
[0020] The die bond sheet 10 of this embodiment has a modulus of elasticity of 2.0 MPa or more and 10.0 MPa or less at 50° C., so that the pick-up performance in the pick-up step (described in detail later) is good. In addition, the modulus of elasticity of the die bond sheet 10 at 130° C. is 0.1 MPa or more and 1.5 MPa or less, so that the die bond performance in the die bond step (described in detail later) is also good.
[0021] Specifically, the die bond sheet 10 has a tensile modulus (tensile storage modulus E' measured by the following measurement method) of 2.0 MPa or more and 10.0 MPa or less at 50°C before heat curing treatment. Such a tensile modulus may be 3.0 MPa or more, or 4.0 MPa or more. By increasing the tensile modulus at 50°C, better pick-up performance can be exhibited. The tensile modulus may be 9.0 MPa or less, or 8.0 MPa or less.
[0022] Moreover, the die bond sheet 10 has a tensile modulus (tensile storage modulus E' measured by the following measurement method) of 0.1 MPa or more and 1.5 MPa or less at 130°C before the heat curing treatment. Such a tensile modulus may be 1.3 MPa or less, or may be 1.0 MPa or less. By making the tensile modulus at 130°C smaller, better die bond performance can be exhibited. The tensile modulus may be 0.2 MPa or more, or 0.3 MPa or more.
[0023] The tensile modulus of elasticity of the die bond sheet 10 can be increased, for example, by increasing the ratio of the total amount of the thermoplastic resin and the thermosetting resin in the die bond sheet 10, or by decreasing the content of the inorganic filler in the die bond sheet 10. On the other hand, the tensile modulus of elasticity can be decreased, for example, by decreasing the ratio of the total amount of the thermoplastic resin and the thermosetting resin in the die bond sheet 10, or by increasing the content of the inorganic filler in the die bond sheet 10.
[0024] The above tensile modulus is measured under the following measurement conditions. Measurement equipment: Solid viscoelasticity measuring equipment For example, "RSA-G2" manufactured by Rheometrics Scientific (TA Instruments) Measurement sample: 200 μm thick (made by laminating die bond sheets) Test piece: 10mm wide, 50mm long strip, initial chuck distance 22.5mm Measurement mode: Tensile mode Frequency 1Hz, heating rate 10℃ / min, distortion 0.1% Measurement temperature range: -20℃ to 200℃ -Read the tensile storage modulus E' [MPa] at 50℃ and 130℃
[0025] The glass transition temperature of the first thermoplastic resin and the glass transition temperature of the second thermoplastic resin may both be 0°C or higher and 30°C or lower. When the glass transition temperatures are within the above ranges, the elastic modulus of the die bond sheet 10 at 50°C can be adjusted (controlled) more easily by changing the ratio of the amounts of the first thermoplastic resin and the second thermoplastic resin. In addition, the breaking elongation and breaking strength of the die bond sheet 10 at -15°C can be adjusted (controlled) more easily. In addition, the peel force (described in detail later) at 50°C between the die bond sheet 10 and the dicing tape 20 can be adjusted (controlled) more easily. When the glass transition temperatures of the first thermoplastic resin and the second thermoplastic resin are 0° C. or higher, the pick-up performance in the pick-up step (described in detail later) can be improved. Also, the breakability of the die bond sheet 10 can be improved. On the other hand, when the glass transition temperatures are 30° C. or lower, the adhesive strength of the die bond sheet 10 to the adherend can be increased.
[0026] The glass transition temperatures of the first and second thermoplastic resins can be increased, for example, by synthesizing each resin with a monomer composition containing an increased amount of monomers that increase the glass transition temperature of each thermoplastic resin, whereas the glass transition temperatures of the first and second thermoplastic resins can be decreased, for example, by synthesizing each resin with a monomer composition containing an increased amount of monomers that decrease the glass transition temperature of each thermoplastic resin.
[0027] The above glass transition temperature is measured before the die bond sheet 10 is subjected to a curing treatment, and is calculated based on the storage modulus E' and loss modulus E'' obtained when measuring the above-mentioned tensile modulus. Specifically, the storage modulus E' and loss modulus E" are measured while increasing the temperature, and Tan δ is calculated for each temperature using the formula Tan δ = E" / E'. A higher Tan δ indicates a higher viscous property. The temperature at which Tan δ is the largest (the apex of the portion where Tan δ shows a peak shape) is defined as the above-mentioned glass transition temperature.
[0028] In this embodiment, the thermoplastic resin includes a first thermoplastic resin and a second thermoplastic resin having different average molecular weights, specifically, the average molecular weight of the first thermoplastic resin is greater than the average molecular weight of the second thermoplastic resin.
[0029] The thermoplastic resin preferably contains an acrylic resin in which at least a (meth)acrylic acid ester monomer is polymerized. More preferably, the thermoplastic resin contains a first acrylic resin and a second acrylic resin having a mass average molecular weight measured by gel permeation chromatography (GPC) smaller than that of the first acrylic resin. Even more preferably, the mass average molecular weight Mw of the first acrylic resin measured by GPC is 500,000 or more and 1,500,000 or less, and the mass average molecular weight Mw of the second acrylic resin is 10,000 or more and 100,000 or less.
[0030] Each of the first acrylic resin and the second acrylic resin as the thermoplastic resin is a polymer obtained by polymerizing at least a (meth)acrylate monomer. In this specification, the term "(meth)acrylic acid" refers to at least one of methacrylic acid and acrylic acid, and the term "(meth)acrylate" refers to at least one of methacrylate (methacrylic acid ester) and acrylate (acrylic acid ester).
[0031] In the above acrylic resins (first acrylic resin and second acrylic resin), it is preferable that the mass ratio of the structural unit of alkyl(meth)acrylate is the highest. Examples of the alkyl(meth)acrylate include C2-C8 alkyl(meth)acrylate, and preferably C2-C4 alkyl(meth)acrylate. The notation C2 in the above C2-C8 alkyl(meth)acrylate represents the number of carbon atoms in the alkyl portion (hydrocarbon portion) of the alkyl(meth)acrylate. Such an alkyl portion is usually a saturated hydrocarbon. For example, the notation C2-C8 represents a carbon number of 2 or more and 8 or less. The same applies below.
[0032] The acrylic resin may further contain a constituent unit derived from a glycidyl group-containing monomer in addition to the constituent unit derived from the alkyl (meth)acrylate monomer. In addition to the constituent units derived from the alkyl (meth)acrylate monomer, the acrylic resin may further contain, for example, constituent units derived from a carboxy group-containing monomer, an acid anhydride monomer, a hydroxy group (hydroxyl group)-containing monomer, a sulfonic acid group-containing monomer, a phosphoric acid group-containing monomer, a polar functional group-containing monomer such as acrylamide or acrylonitrile, or various other polyfunctional monomers.
[0033] The acrylic resin is preferably a copolymer of at least an alkyl(meth)acrylate, particularly an alkyl(meth)acrylate having an alkyl moiety with 8 or less carbon atoms, and a glycidyl group-containing (meth)acrylate.
[0034] When the above-mentioned acrylic resin has a glycidyl group, a carboxy group, a hydroxy group, or the like in the molecule, it may have the above-mentioned glycidyl group, or the like in a side chain, specifically, the above-mentioned glycidyl group, or the like at the terminal of the side chain.
[0035] When the above thermoplastic resin (including the first acrylic resin and the second acrylic resin) is measured by gel permeation chromatography (GPC), since the average molecular weight of the second acrylic resin is smaller than that of the first acrylic resin, the chart showing the molecular weight distribution obtained by the measurement has at least two peaks separated from each other on the low molecular weight side and the high molecular weight side. In the chart showing the molecular weight distribution, the apexes of the two peaks are separated from each other. In other words, even if the bases of the two peaks overlap each other, the chart has two peaks whose apexes are separated from each other. The weight average molecular weight Mw and the like of each of the first acrylic resin and the second acrylic resin are determined by GPC measurement, which will be described in detail later.
[0036] The mass average molecular weight Mw of the first acrylic resin may be 500,000 or more and 1,500,000 or less, or may be 600,000 or more and 1,300,000 or less. When the mass average molecular weight of the first acrylic resin is 500,000 or more, the cohesive force of the die bond sheet 10 can be increased in the die bonding step (described in detail later), and the adhesive force of the die bond sheet 10 can be increased. Also, when the mass average molecular weight of the first acrylic resin is 1,500,000 or less, the wettability of the die bond sheet 10 can be increased in the die bonding step (described in detail later), and the adhesive force of the die bond sheet 10 can be increased. The mass average molecular weight Mw of the second acrylic resin may be 10,000 or more and 100,000 or less, or may be 20,000 or more and 80,000 or less. By making the mass average molecular weight of the second acrylic resin 10000 or more, the reliability of the die bond sheet 10 in the reflow soldering process (described in detail later) can be more sufficiently ensured. Also, by making the mass average molecular weight of the second acrylic resin 100000 or less, the wettability of the die bond sheet 10 in the die bond process (described in detail later) can be further improved.
[0037] The details of the GPC measurement conditions are as follows. [Preparation of measurement samples] (1) A sample of about 0.2 g is obtained from the die bond sheet before hardening treatment. (2) The sample wrapped in the mesh sheet is immersed in about 30 mL of toluene at room temperature for one week. (3) The mesh sheet is removed from the toluene to remove the toluene-insoluble matter remaining in the mesh sheet, thereby obtaining a toluene solution containing a toluene-soluble component. (4) The toluene solution is subjected to a reduced pressure treatment at a temperature of 45° C. or less to remove toluene from the toluene solution, thereby obtaining a solid of the toluene-soluble component. (5) The solid is dissolved in tetrahydrofuran (THF) so that the concentration of the solid is 0.2% by mass to prepare a THF solution, which is then left to stand overnight. (6) The THF solution that has been left overnight is filtered through a membrane filter (0.45 μm), and the resulting filtrate is used as the measurement sample. [GPC measurement conditions] Apparatus: Gel permeation chromatography apparatus (For example, Tosoh's product name "HLC-8220GPC") Columns: 3 in total One TSKgel quadcolumn SuperHZ-L (hereinafter referred to as the first column) manufactured by Tosoh Corporation, and Two TSKgel SuperHAM-M columns (hereafter referred to as the second column) manufactured by Tosoh Corporation Two second columns were connected in series downstream of the first column, and each column was arranged so that an eluent, which will be described later, would flow in from the first column side. Column temperature: 40℃ Eluent: Tetrahydrofuran (THF) Flow rate: Sample pump flow rate 0.3mL / min Reference pump flow rate: 1.0mL / min Injection volume: 10 μL (sample concentration: 0.2% by mass as above) Detector: Refractive index detector (RI) Standard material: Standard polystyrene
[0038] In order to obtain a molecular weight distribution curve by GPC measurement, two kinds of standard polystyrenes with different molecular weights are used as standard substances. Specifically, each standard polystyrene is weighed to a predetermined blend weight, and each weighed standard polystyrene is dissolved in 100 mL of THF to prepare standard polystyrene solution STD1 and standard polystyrene solution STD2. GPC measurement is also performed on these standard polystyrene solutions using the above-mentioned measuring device and under the above-mentioned measuring conditions. The results of the GPC measurement of the measurement sample and the standard polystyrene solution are analyzed using analysis software GPC-8020 Model II (Data Management Version 5.10) manufactured by Tosoh Corporation. In the data analysis using the above analysis software, first, calibration curves (calibration curves with the horizontal axis representing time (min) and the vertical axis representing the logarithm of the mass average molecular weight) for the STD1 and STD2 are created. Data analysis regarding the molecular weight of the measurement sample is performed based on these calibration curves. The data analysis on the molecular weight of the measurement sample is performed after obtaining a molecular weight distribution curve for peak P1 (peak with the highest molecular weight) that is detected earliest on the chromatogram. The data analysis is performed on the molecular weight distribution curve for peak P1 to obtain the mass average molecular weight Mw for peak P1. Since the die bond sheet contains both the first acrylic resin and the second acrylic resin, peak P1 corresponds to the peak of the first acrylic resin. If the falling edge of peak P1, which is detected earliest, overlaps with the rising edge of peak P2, which is detected next to peak P1, a baseline is drawn so as to extend horizontally from the starting point of the rise of peak P1. Next, a line is drawn vertically from the baseline toward the valley (the most depressed part) occurring between the falling edge of peak P1 and the rising edge of peak P2. The area bounded by the line from the starting point of the rise of peak P1 to the valley, the baseline, and the line drawn vertically from the baseline toward the valley is then analyzed to obtain the mass average molecular weight Mw for peak P1. Similarly, the mass average molecular weight Mw is obtained for peak P2. The baseline of peak P2 is drawn so that it extends horizontally from the start of the rise of peak P1 toward the fall of peak P2. A line is drawn vertically from the baseline of peak P2 toward the valley (the most depressed part) that occurs between the fall of peak P1 and the rise of peak P2. Then, the area bounded by the line from the valley to the end of the fall of peak P2, the baseline of peak P2, and the line drawn vertically from the baseline of peak P2 toward the valley is used as the analysis target for peak P2, and the mass average molecular weight Mw is obtained for peak P2. Peak P2 appears to the right of peak P1 in the GPC measurement chart, and corresponds to the peak of the second acrylic resin.
[0039] When the acrylic resin has a glycidyl group in the molecule, the epoxy equivalent of the acrylic resin may be 200 [g / eq] or more and 7000 [g / eq] or less. The epoxy equivalent may be 400 [g / eq] or more and 5000 [g / eq] or less.
[0040] <Epoxy equivalent of acrylic resin> The epoxy equivalent of the acrylic resin is measured by nuclear magnetic resonance analysis (NMR analysis) as follows. [Sample preparation] Weigh out approximately 350 mg of chromium (III) acetylacetonate (molecular weight 349.32 g / mol) as a relaxation reagent, and adjust the volume to 20 mL with CDCl3 to make the concentration 50 mM. Then, weigh out approximately 50 mg of hexamethyldisiloxane sample (molecular weight 162.38 g / mol) as an internal standard, and adjust the volume to 10 mL with chromium (III) acetylacetonate-containing CDCl3 (the above-mentioned solution), to make the quantitative standard solution for NMR measurement. Next, weigh out about 40 mg of the measurement sample, add 0.5 mL of the quantitative standard solution to dissolve it, 13 Measure the epoxy equivalent [g / eq] by C NMR (NNE, absolute quantitative method). [Analyzer] Nuclear Magnetic Resonance Spectrometer [Measurement conditions] Observation frequency: 150MHz ( 13 C) Measurement solvent: CDCl3 Measurement temperature: 300K Chemical shift standard: Measurement solvent ( 13 C: 77.05 ppm) [Epoxy equivalent calculation formula]:
number
[0041] In the die bond sheet 10 of this embodiment, the mass ratio of the second acrylic resin to the first acrylic resin is preferably 1.5 or less, and more preferably 1.0 or less. In other words, it is more preferable that the content of the first acrylic resin is equal to or greater than the content of the second acrylic resin. By making the mass ratio 1.5 or less, the proportion of the first acrylic resin increases, so that the cohesive force of the die bond sheet 10 at high temperatures (e.g., 130°C) is further increased, and the adhesive force of the die bond sheet 10 can be further improved. In addition, the reliability of the die bond sheet 10 in the reflow soldering process (described in detail later) can be more sufficiently guaranteed. The mass ratio may be 0.1 or more, or 0.2 or more. When the mass ratio is 0.1 or more, the die bond sheet 10 can be more satisfactorily cleaved in the expanding step (described later). In addition, the die bond sheet 10 can have better adhesion to the adherend when it is bonded to the adherend.
[0042] The die bond sheet 10 of the present embodiment preferably contains 50.0 mass % or more and 95.0 mass % or less of a thermoplastic resin (particularly the above-mentioned acrylic resin), and more preferably contains 70 mass % or less. By including a larger amount of thermoplastic resin (particularly the above-mentioned acrylic resin) in the die bond sheet 10, there is an advantage that the elastic modulus of the die bond sheet 10 at high temperatures can be easily controlled by changing the type of thermoplastic resin. On the other hand, by including a smaller amount of thermoplastic resin (particularly the above-mentioned acrylic resin) in the die bond sheet 10, the cohesive force after the die bond sheet 10 is thermally cured can be increased, and the reliability of the die bond sheet 10 can be more fully ensured.
[0043] The die bond sheet 10 of the present embodiment preferably contains 20.0% by mass or more of the first acrylic resin, more preferably 30.0% by mass or more, and even more preferably 40.0% by mass or more. The die bond sheet 10 may contain 70.0% by mass or less of the first acrylic resin, and preferably contains 65.0% by mass or less. By the die bond sheet 10 containing 20.0 mass % or more and 65.0 mass % or less of the first acrylic resin, the elastic modulus of the die bond sheet 10 at high temperatures can be easily controlled by changing the type of thermoplastic resin, and both the cohesive strength and wettability of the die bond sheet 10 after it is thermally cured can be appropriately increased.
[0044] The die bond sheet 10 of the present embodiment preferably contains 40.0 mass % or less of the second acrylic resin, more preferably 35.0 mass % or less. The die bond sheet 10 may contain 5.0 mass % or more of the second acrylic resin, preferably 10.0 mass % or more. By the die bond sheet 10 containing 5.0 mass % or more and 40.0 mass % or less of the second acrylic resin, the wettability of the die bond sheet 10 at high temperatures becomes better, and the breakability of the die bond sheet 10 becomes easier to control by changing the type of thermoplastic resin.
[0045] The first acrylic resin and the second acrylic resin may be commercially available products. The first acrylic resin and the second acrylic resin may be synthesized by carrying out a polymerization reaction using an acrylic monomer such as an alkyl (meth)acrylate monomer by a general method.
[0046] The die bond sheet 10 of the present embodiment may have a breaking elongation of 0.2% or more at −15° C. Such breaking elongation may be 2.0% or less, or 1.5% or less. When the breaking elongation at -15°C is 0.2% or more, it is possible to more effectively prevent cracks during processing or transportation of the die bond sheet 10. Moreover, when the breaking elongation is 2.0% or less, the breakability of the die bond sheet 10 in the low-temperature expanding step (described in detail later) can be more improved.
[0047] The above-mentioned breaking elongation at -15°C can be increased, for example, by reducing the amount of the second acrylic resin in the die bond sheet 10. On the other hand, the breaking elongation at -15°C can be decreased, for example, by increasing the amount of the second acrylic resin in the die bond sheet 10.
[0048] The die bond sheet 10 of this embodiment has a breaking strength of 1.0 kg / mm at −15° C. 2 The breaking strength may be 7.5 kg / mm or more. 2 or less, 6.0 kg / mm 2 It may be the following. Breaking strength at -15℃ is 1.0kg / mm 2 By setting the breaking strength to 7.5 kg / mm or more, it is possible to prevent the die bond sheet 10 from cracking during processing or transportation. 2 By satisfying the above, the breakability of the die bond sheet 10 in the low-temperature expanding step (described in detail later) can be improved.
[0049] The above-mentioned breaking strength at -15°C can be increased, for example, by reducing the amount of the second acrylic resin in the die bond sheet 10. On the other hand, the breaking strength can be decreased, for example, by increasing the amount of the second acrylic resin in the die bond sheet 10.
[0050] The breaking elongation (breaking elongation) and breaking strength of the die bond sheet 10 at −15° C. are measured under the following measurement conditions before the die bond sheet 10 is cured. Measurement equipment: Solid viscoelasticity measuring equipment Measurement sample: 20μm thick (if less than 20μm, for example a 5μm die bond sheet, stack so that the total thickness is 20μm) Test piece: Strip shape, width 10 mm, length 50 mm, initial chuck distance 20 mm Pulling speed: 1mm / sec, Measurement temperature: -15℃ (measurement begins after maintaining at -15℃ for 5 minutes) The elongation at break is the breaking elongation (breaking elongation), and the test force at break is the breaking strength.
[0051] The die bond sheet 10 of the present embodiment further contains, for example, a thermosetting resin.
[0052] Examples of the thermosetting resin include epoxy resin, phenol resin, amino resin, unsaturated polyester resin, polyurethane resin, silicone resin, and thermosetting polyimide resin. As the thermosetting resin, only one type or two or more types are adopted. The thermosetting resin may include at least one of an epoxy resin and a phenol resin, or may include a phenol resin.
[0053] In the die bond sheet 10 of the present embodiment, the content of the thermosetting resin is preferably 40 mass% or less, more preferably 30 mass% or less, and further preferably 20 mass% or less. By lowering the content of the thermosetting resin in the die bond sheet 10, the progress of hardening of the die bond sheet 10 can be made relatively slow. In the die bond sheet 10 of the present embodiment, the content of the thermosetting resin is, for example, 5 mass % or more. By increasing the content of the thermosetting resin in the die bond sheet 10, the die bond sheet 10 can be bonded to an adherend with higher adhesive strength, and the heat resistance reliability of the die bond sheet 10 at high temperatures such as during reflow can be improved. In the die bond sheet 10 of the present embodiment, the content of the thermosetting resin may be 0 mass% or more than 0 mass% (i.e., 0 mass% or more). The content of the thermosetting resin is preferably 5 mass% or more, and more preferably 7 mass% or more.
[0054] Examples of the epoxy resin include bisphenol A type, bisphenol F type, bisphenol S type, brominated bisphenol A type, hydrogenated bisphenol A type, bisphenol AF type, biphenyl type, naphthalene type, fluorene type, phenol novolac type, orthocresol novolac type, trishydroxyphenylmethane type (trisphenolmethane type), tetraphenylolethane type, hydantoin type, trisglycidyl isocyanurate type, and glycidylamine type epoxy resins. The epoxy equivalent [g / eq] of the epoxy resin may be, for example, 90 or more and 220 or less.
[0055] Phenol resin can act as a curing agent for epoxy resin. In addition, the hydroxyl group of the phenol resin can crosslink with the glycidyl group. Therefore, when the acrylic resin has a glycidyl group in the molecule, the acrylic resin and the phenol resin can crosslink.
[0056] Examples of the phenol resin include novolac type phenol resin, resol type phenol resin, and polyoxystyrene such as polyparaoxystyrene. Examples of novolac type phenolic resins include phenol novolac resins, phenol aralkyl resins (such as biphenyl aralkyl type resin phenolic resins), cresol novolac resins, tert-butylphenol novolac resins, nonylphenol novolac resins, and phenol xylylene resins. The hydroxyl equivalent weight [g / eq] of the phenolic resin may be, for example, 150 or more and 250 or less. As the phenol resin, a biphenyl aralkyl type resin phenol resin having a relatively large hydroxyl group equivalent is preferable in that the elastic modulus of the die bond sheet 10 can be appropriately low. As the phenolic resin, one kind or two or more kinds may be adopted.
[0057] The die bond sheet 10 of the present embodiment may contain a thermoplastic resin other than the above-mentioned acrylic resin. Examples of the thermoplastic resin other than the above-mentioned acrylic resin include natural rubber, butyl rubber, isoprene rubber, chloroprene rubber, ethylene-vinyl acetate copolymer, ethylene-acrylic acid copolymer, polybutadiene resin, polycarbonate resin, thermoplastic polyimide resin, polyamide resin such as 6-polyamide resin and 6,6-polyamide resin, phenoxy resin, saturated polyester resin such as PET and PBT, polyamideimide resin, and fluororesin. As the thermoplastic resin, one kind or two or more kinds may be adopted.
[0058] The die bond sheet 10 of the present embodiment contains an inorganic filler. By changing the amount of the inorganic filler in the die bond sheet 10, the elasticity and viscosity of the die bond sheet 10 can be more easily adjusted, and the physical properties of the die bond sheet 10, such as electrical conductivity, thermal conductivity, and elastic modulus, can also be adjusted.
[0059] Examples of inorganic fillers include fillers containing aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, calcium silicate, magnesium silicate, calcium oxide, magnesium oxide, aluminum oxide, aluminum nitride, boron nitride, silica such as crystalline silica and amorphous silica, etc. Examples of the material of the inorganic filler include simple metals such as aluminum, gold, silver, copper, nickel, etc., and alloys, etc. The inorganic filler may be aluminum borate whiskers, amorphous carbon black, graphite, etc. The shape of the inorganic filler may be various shapes such as spherical, needle-like, flake-like, etc. As the inorganic filler, only one type or two or more types of the above are used.
[0060] As the inorganic filler, silica filler is preferable. Since the -OH group present on the surface of the silica particle and the above-mentioned acrylic resin (containing a glycidyl group in the molecule) easily react with each other by the curing treatment, there is an advantage that the curing of the die bond sheet 10 can be promoted more sufficiently.
[0061] The average particle size of the inorganic filler (average particle size of primary particles) may be, for example, 1 nm or more and 500 nm or less. The average particle size of the inorganic filler is preferably 5 nm or more and 200 nm or less, more preferably 100 nm or less, even more preferably 50 nm or less, particularly preferably 20 nm or less, and most preferably 15 nm or less. In that the breakability of the die bond sheet 10 before the curing treatment can be improved, the average particle size is preferably 500 nm or less, more preferably 200 nm or less, and even more preferably 100 nm or less. In addition, in order to obtain a thinner die bond sheet 10, it is preferable that the average particle size of the inorganic filler is smaller.
[0062] The average particle size (average particle size of primary particles) of the inorganic filler is measured as follows. For example, a dispersion liquid in which the inorganic filler is dispersed is dropped onto a flat plate, and then dried to prepare a measurement sample. An observation image of the inorganic filler particles in the measurement sample is obtained using a field emission scanning electron microscope (FE-SEM). For example, a backscattered electron image is obtained using a scanning electron microscope "HITACHI S-4800" (accelerating voltage 5 kV). Alternatively, a phase contrast image is obtained using a scanning electron microscope "HITACHI SU8020" (accelerating voltage 5 kV). Then, the particle size of each of 1000 or more inorganic fillers is measured by image analysis (ImageJ, Image Pro), and the average value is calculated to measure the average particle size of the inorganic filler. The above dispersion liquid may be prepared by mixing the inorganic filler and a solvent so that the inorganic filler concentration (solid content concentration) is 1 mass % or less. The above dispersion liquid may be prepared, for example, as follows. In detail, the organic components contained in the die bond sheet 10 are burned off by a baking process (for example, 500°C under air conditions for 5 hours). The above dispersion liquid may be prepared by diluting with a solvent so that the concentration of the remaining ash (solid content concentration) is 1 mass% or less. As the solvent, for example, a solvent in which the inorganic filler can be dispersed in the state of primary particles, such as pure water, methanol, ethanol, isopropyl alcohol, methyl ethyl ketone, chloroform, or pH-adjusted water adjusted to a pH away from the isoelectric point of the inorganic filler, may be used.
[0063] In the die-bonding sheet 10, the mass ratio of the inorganic filler to the thermoplastic resin (acrylic resin) is preferably 0.1 or more and 0.5 or less, which allows the die-bonding sheet 10 to have appropriate viscoelasticity.
[0064] The content ratio of the inorganic filler is preferably 5.0 mass % or more, and more preferably 10.0 mass % or more, with respect to the total mass of the die bond sheet 10. The content ratio of the inorganic filler is preferably 30.0 mass % or less, and more preferably 25.0 mass % or less.
[0065] The die bond sheet 10 may contain other components as necessary. Examples of the other components include a curing catalyst, a flame retardant, a silane coupling agent, an ion trapping agent, and a dye. Examples of the flame retardant include antimony trioxide, antimony pentoxide, and brominated epoxy resins. Examples of the silane coupling agent include β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, and γ-glycidoxypropylmethyldiethoxysilane. Examples of the ion trapping agent include hydrotalcites, bismuth hydroxide, and benzotriazole. As the other additives, one kind may be used alone, or two or more kinds may be used in combination.
[0066] The die bond sheet 10 preferably contains the above-mentioned first acrylic resin, the above-mentioned second acrylic resin, a phenol resin, and a silica filler, in that the elasticity and viscosity are easily adjusted.
[0067] The thickness of the die bond sheet 10 is not particularly limited, but is, for example, 1 μm or more and 100 μm or less. Such a thickness may be 3 μm or more, 5 μm or more, or 7 μm or more. The thickness of the die bond sheet 10 may be 50 μm or less, or 40 μm or less. In addition, when the die bond sheet 10 is a laminate, the above thickness is the total thickness of the laminate.
[0068] The die bond sheet 10 may have a single-layer structure, for example, as shown in Fig. 1. In this specification, a single layer means having only a layer formed of the same composition. A form in which a plurality of layers formed of the same composition are laminated is also a single layer. On the other hand, the die bond sheet 10 may have a multi-layer structure in which layers each formed of two or more different compositions are laminated. When the die bond sheet 10 has a multi-layer structure, at least one layer constituting the die bond sheet 10 may contain the above-mentioned first acrylic resin and second acrylic resin.
[0069] Next, an embodiment of the dicing die bond film according to the present invention will be described.
[0070] The dicing die bond film 1 of this embodiment includes the above-mentioned die bond sheet 10 and a dicing tape 20 bonded to the die bond sheet 10. The dicing tape 20 has a base layer 21 and a pressure-sensitive adhesive layer 22 overlapping the base layer 21.
[0071] In the dicing die bond film 1 of this embodiment, when used, the adhesive layer 22 is cured by irradiation with active energy rays (e.g., ultraviolet rays). In detail, in a state in which the die bond sheet 10 having a semiconductor wafer adhered to one surface and the adhesive layer 22 bonded to the other surface of the die bond sheet 10 are laminated, ultraviolet rays or the like are irradiated to at least the adhesive layer 22. For example, ultraviolet rays or the like are irradiated from the side where the base layer 21 is arranged, and the ultraviolet rays or the like reach the adhesive layer 22 after passing through the base layer 21. The adhesive layer 22 is cured by irradiation with ultraviolet rays or the like. Since the adhesive layer 22 hardens after irradiation, the adhesive strength of the adhesive layer 22 can be reduced, so that the die bond sheet 10 (with the semiconductor wafer adhered thereto) can be relatively easily peeled off from the adhesive layer 22 after irradiation.
[0072] <Dicing tape for dicing die bond film> In this embodiment, the dicing tape 20 is usually a long sheet and is stored in a rolled state until it is used. The dicing die bond film 1 of this embodiment is stretched on an annular frame having an inner diameter slightly larger than the silicon wafer to be cut, and is used after being cut.
[0073] The elastic modulus (tensile elastic modulus) of the dicing tape 20 at 50° C. is preferably 10 MPa or more. This allows easy peeling between the adhesive layer 22 and the die bond sheet 10 when the semiconductor chip is picked up using the suction tool J with an increased temperature (for example, 50° C.) in the pick-up step (described in detail later). Therefore, the semiconductor chip can be picked up more satisfactorily. The dicing tape 20 preferably has an elastic modulus (tensile elastic modulus) of 100 MPa or less at 50° C. This can further prevent the pressure-sensitive adhesive layer 22 from cracking in the expanding step (described in detail later).
[0074] The elastic modulus (tensile elastic modulus) of the above dicing tape 20 at 50°C is measured in the same manner as the above-mentioned method for measuring the tensile elastic modulus of the die bond sheet 10 before the adhesive layer 22, which will be described in detail later, is cured with active energy rays.
[0075] The base material layer 21 may be a single layer, or may be configured with multiple layers (for example, three layers). The thickness (total thickness) of the base material layer 21 may be 80 μm or more and 150 μm or less.
[0076] Each layer of the base material layer 21 is, for example, a metal foil, a fiber sheet such as paper or cloth, a rubber sheet, or a resin film. Examples of the fiber sheet constituting the base layer 21 include paper, woven fabric, and nonwoven fabric. Examples of materials for the resin film include polyolefins such as polyethylene (PE), polypropylene (PP), and ethylene-propylene copolymers; ethylene copolymers such as ethylene-vinyl acetate copolymers (EVA), ionomer resins, ethylene-(meth)acrylic acid copolymers, and ethylene-(meth)acrylic acid ester (random, alternating) copolymers; polyesters such as polyethylene terephthalate (PET), polyethylene naphthalate (PEN), and polybutylene terephthalate (PBT); polyacrylates; polyvinyl chloride (PVC); polyurethanes; polycarbonates; polyphenylene sulfide (PPS); polyamides such as aliphatic polyamides and fully aromatic polyamides (aramids); polyether ether ketones (PEEK); polyimides; polyetherimides; polyvinylidene chloride; ABS (acrylonitrile-butadiene-styrene copolymers); cellulose or cellulose derivatives; silicone-containing polymers; and fluorine-containing polymers. These may be used alone or in combination of two or more.
[0077] The base layer 21 is preferably made of a polymeric material such as a resin film. When the base layer 21 has a resin film, the resin film may be subjected to a stretching process or the like to control the deformability such as elongation percentage. The surface of the base layer 21 may be subjected to a surface treatment in order to enhance adhesion with the adhesive layer 22. Examples of the surface treatment that can be used include oxidation treatment by chemical or physical methods such as corona treatment, antistatic treatment, chromic acid treatment, ozone exposure, flame exposure, high-voltage shock exposure, and ionizing radiation treatment. In addition, the base layer 21 may be subjected to a coating treatment using a coating agent such as an anchor coating agent, a primer, an antistatic agent, or an adhesive.
[0078] The back side of the base material layer 21 (the side on which the adhesive layer 22 is not overlapped) may be subjected to a release treatment using a release agent (release agent) such as a silicone-based resin or a fluorine-based resin in order to impart releasability. The base layer 21 is preferably a light-transmitting (ultraviolet ray-transmitting) resin film or the like, since it allows active energy rays such as ultraviolet ray to be applied to the pressure-sensitive adhesive layer 22 from the back side.
[0079] The dicing tape 20 may include a release liner that covers one side of the adhesive layer 22 (the side where the adhesive layer 22 does not overlap the base layer 21) before use. The release liner is used to protect the adhesive layer 22, and is peeled off before the die bond sheet 10 is attached to the adhesive layer 22.
[0080] In this embodiment, the pressure-sensitive adhesive layer 22 contains, for example, an acrylic polymer, an isocyanate compound, and a polymerization initiator. The adhesive layer 22 may have a thickness of 5 μm or more and 40 μm or less. The thickness of the adhesive layer 22 is preferably 10 μm or less in order to more satisfactorily cleave the die bond sheet 10. The shape and size of the adhesive layer 22 are usually the same as those of the base layer 21.
[0081] The acrylic polymer has at least an alkyl (meth)acrylate structural unit, a hydroxyl group-containing (meth)acrylate structural unit, and a polymerizable group-containing (meth)acrylate structural unit in the molecule. The structural units are units that constitute the main chain of the acrylic polymer. Each side chain in the acrylic polymer is included in each structural unit that constitutes the main chain.
[0082] In the acrylic polymer contained in the pressure-sensitive adhesive layer 22, the above-mentioned structural unit is 1 H-NMR, 13 This can be confirmed by NMR analysis such as C-NMR, pyrolysis GC / MS analysis, infrared spectroscopy, etc. The molar ratio of the above-mentioned structural units in the acrylic polymer is usually calculated from the blend amount (charge amount) when the acrylic polymer is polymerized.
[0083] The constituent unit of the alkyl (meth)acrylate is derived from an alkyl (meth)acrylate monomer. In other words, the molecular structure after the alkyl (meth)acrylate monomer is polymerized is the constituent unit of the alkyl (meth)acrylate. The term "alkyl" refers to the hydrocarbon moiety that is ester-bonded to (meth)acrylic acid. The hydrocarbon of the alkyl portion in the structural unit of the alkyl (meth)acrylate may be a saturated hydrocarbon or an unsaturated hydrocarbon. It is preferable that the alkyl portion does not contain a polar group containing oxygen (O) or nitrogen (N). This can prevent the polarity of the acrylic polymer from increasing excessively. Therefore, the adhesive layer 22 is prevented from having excessive affinity for the die bond sheet 10. Therefore, the dicing tape 20 can be more satisfactorily peeled off from the die bond sheet 10. The number of carbon atoms in the alkyl portion may be 6 or more and 12 or less.
[0084] Examples of the alkyl (meth)acrylate structural unit include hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n- or iso-nonyl (meth)acrylate, decyl (meth)acrylate, and lauryl (meth)acrylate structural units.
[0085] The acrylic polymer has a hydroxyl group-containing (meth)acrylate structural unit, and the hydroxyl group of such a structural unit easily reacts with an isocyanate group. By allowing the acrylic polymer having a hydroxyl group-containing (meth)acrylate structural unit and the isocyanate compound to coexist in the adhesive layer 22, the adhesive layer 22 can be appropriately cured. Therefore, the acrylic polymer can be sufficiently gelled. Therefore, the adhesive layer 22 can exhibit adhesive performance while maintaining its shape.
[0086] The structural unit of the hydroxyl group-containing (meth)acrylate is preferably a structural unit of a hydroxyl group-containing C2-C4 alkyl (meth)acrylate. The term "C2-C4 alkyl" refers to the hydrocarbon moiety ester-bonded to the (meth)acrylic acid and its carbon number. In other words, the hydroxyl group-containing C2-C4 alkyl (meth)acrylate monomer refers to a monomer in which (meth)acrylic acid is ester-bonded to an alcohol having 2 to 4 carbon atoms (usually a dihydric alcohol). The hydrocarbon portion of the C2-C4 alkyl is usually a saturated hydrocarbon. For example, the hydrocarbon portion of the C2-C4 alkyl is a linear saturated hydrocarbon or a branched saturated hydrocarbon. It is preferable that the hydrocarbon portion of the C2-C4 alkyl does not contain a polar group containing oxygen (O), nitrogen (N), or the like.
[0087] Examples of the structural unit of the hydroxyl group-containing C2-C4 alkyl(meth)acrylate include structural units of hydroxybutyl(meth)acrylate such as hydroxyethyl(meth)acrylate, hydroxypropyl(meth)acrylate, hydroxyn-butyl(meth)acrylate, or hydroxyiso-butyl(meth)acrylate. In the structural unit of hydroxybutyl(meth)acrylate, the hydroxyl group (-OH group) may be bonded to the terminal carbon (C) of the hydrocarbon moiety, or may be bonded to a carbon (C) other than the terminal of the hydrocarbon moiety.
[0088] The acrylic polymer contains a structural unit of a polymerizable group-containing (meth)acrylate having a polymerizable unsaturated double bond in the side chain. Since the acrylic polymer contains a structural unit of a polymerizable group-containing (meth)acrylate, the pressure-sensitive adhesive layer 22 can be cured by irradiation with active energy rays (ultraviolet rays, etc.) before the pick-up step. In particular, the irradiation with active energy rays such as ultraviolet rays generates radicals from the photopolymerization initiator, and the action of these radicals can cause a crosslinking reaction between the acrylic polymers. This makes it possible to reduce the adhesive strength of the pressure-sensitive adhesive layer 22 before irradiation. Then, the die-bonding sheet 10 can be peeled off well from the pressure-sensitive adhesive layer 22. The active energy rays include ultraviolet rays, radioactive rays, and electron beams.
[0089] Specifically, the structural unit of the polymerizable group-containing (meth)acrylate may have a molecular structure in which an isocyanate group of an isocyanate group-containing (meth)acrylate monomer is bonded via urethane to a hydroxyl group in the structural unit of the above-mentioned hydroxyl group-containing (meth)acrylate.
[0090] The structural unit of the polymerizable group-containing (meth)acrylate having a polymerizable group can be prepared after the polymerization reaction of synthesizing the acrylic polymer. For example, after the copolymerization of an alkyl (meth)acrylate monomer and a hydroxyl group-containing (meth)acrylate monomer, the hydroxyl group in a part of the structural unit of the hydroxyl group-containing (meth)acrylate and the isocyanate group of the isocyanate group-containing polymerizable monomer are reacted to form a urethane reaction, thereby obtaining the structural unit of the polymerizable group-containing (meth)acrylate.
[0091] The isocyanate group-containing (meth)acrylate monomer preferably has one isocyanate group and one (meth)acryloyl group in the molecule, such as 2-isocyanatoethyl (meth)acrylate.
[0092] The pressure-sensitive adhesive layer 22 of the dicing tape 20 in this embodiment further contains an isocyanate compound. A part of the isocyanate compound may be in a state after being reacted by a urethanization reaction or the like. The isocyanate compound has a plurality of isocyanate groups in the molecule. The isocyanate compound has a plurality of isocyanate groups in the molecule, which allows a crosslinking reaction between the acrylic polymers in the pressure-sensitive adhesive layer 22 to proceed. In detail, one isocyanate group of the isocyanate compound is reacted with a hydroxyl group of an acrylic polymer, and the other isocyanate group is reacted with a hydroxyl group of another acrylic polymer, whereby a crosslinking reaction via the isocyanate compound can proceed.
[0093] Examples of the isocyanate compound include diisocyanates such as aliphatic diisocyanates, alicyclic diisocyanates, and araliphatic diisocyanates.
[0094] Further, examples of the isocyanate compound include polymerized polyisocyanates such as dimers and trimers of diisocyanates, and polymethylene polyphenylene polyisocyanates.
[0095] In addition, the isocyanate compound may be, for example, a polyisocyanate obtained by reacting an excess amount of the above-mentioned isocyanate compound with an active hydrogen-containing compound. Examples of the active hydrogen-containing compound include an active hydrogen-containing low molecular weight compound and an active hydrogen-containing high molecular weight compound. As the isocyanate compound, allophanated polyisocyanate, biuretized polyisocyanate, etc. can also be used. The above isocyanate compounds can be used alone or in combination of two or more.
[0096] The isocyanate compound is preferably a reaction product of an aromatic diisocyanate and an active hydrogen-containing low molecular weight compound. The reaction rate of the isocyanate group in the reaction product of the aromatic diisocyanate is relatively slow, so that the pressure-sensitive adhesive layer 22 containing such a reaction product is prevented from being excessively hardened. The isocyanate compound is preferably one having three or more isocyanate groups in the molecule.
[0097] The polymerization initiator contained in the adhesive layer 22 is a compound capable of initiating a polymerization reaction by the applied heat or light energy. By including a polymerization initiator in the adhesive layer 22, a crosslinking reaction between acrylic polymers can be promoted when heat energy or light energy is applied to the adhesive layer 22. In more detail, a polymerization reaction between polymerizable groups between acrylic polymers having structural units of polymerizable group-containing (meth)acrylate can be initiated to harden the adhesive layer 22. This reduces the adhesive force of the adhesive layer 22, and in the pick-up process, the die bond sheet 10 can be easily peeled off from the hardened adhesive layer 22. As the polymerization initiator, for example, a photopolymerization initiator or a thermal polymerization initiator is used. As the polymerization initiator, a general commercially available product can be used.
[0098] The pressure-sensitive adhesive layer 22 may further contain other components in addition to the above-mentioned components. Examples of the other components include tackifiers, plasticizers, fillers, antioxidants, antioxidants, UV absorbers, light stabilizers, heat stabilizers, antistatic agents, surfactants, and light release agents. The types and amounts of the other components may be appropriately selected depending on the purpose.
[0099] The peel strength between the dicing tape 20 and the die bond sheet 10 may be within a predetermined range. Specifically, the peel strength between the pressure-sensitive adhesive layer 22 of the dicing tape 20 and the die bond sheet 10 at 50° C. may be 0.03 N / 20 mm or more and 0.20 N / 20 mm or less. Since the peeling force is within the above range, even if the temperature of the suction tool J for peeling the semiconductor chip X and the small piece 10' of the die bond sheet from the adhesive layer 22 rises in the pick-up process described in detail later, the semiconductor chip X can be picked up well using the suction tool J.
[0100] The peel strength between the die bond sheet 10 and the adhesive layer 22 (after curing treatment) of the dicing tape 20 is measured as follows. A backing tape (product name "BT-315" manufactured by Nitto Denko Corporation) is attached to the die bond sheet 10 of the dicing die bond film 1. Then, a test piece having a size of 50 mm in width and 120 mm in length is cut out. Using the cut out test piece, a T-peel test is performed using a tensile tester (for example, "Autograph AGS Series" manufactured by Shimadzu Corporation) to measure the peel force [N / 20 mm]. The temperature condition in the measurement is 50°C, and the peel speed is 300 mm / min. Before laminating the backing tape, the adhesive layer of the dicing tape was irradiated with 300 mJ / cm from the base layer side at a temperature of 22°C. 2 (Irradiation intensity 150mW / cm 2 The photocuring process is carried out by irradiating the substrate with ultraviolet light for 2 seconds.
[0101] The dicing die bond film 1 of this embodiment may have a release liner that covers one side of the die bond sheet 10 (the side where the die bond sheet 10 does not overlap the pressure-sensitive adhesive layer 22) before use. The release liner is used to protect the die bond sheet 10, and is peeled off immediately before attaching an adherend (e.g., a semiconductor wafer) to the die bond sheet 10. This release liner can be used as a support material for supporting the die bond sheet 10. The release liner is suitably used when overlaying the die bond sheet 10 on the pressure-sensitive adhesive layer 22. In detail, the die bond sheet 10 is overlaid on the pressure-sensitive adhesive layer 22 in a state in which the release liner and the die bond sheet 10 are laminated, and after overlaying, the release liner is peeled off (transferred), thereby overlaying the die bond sheet 10 on the pressure-sensitive adhesive layer 22.
[0102] Next, a manufacturing method of the die bond sheet 10 and the dicing die bond film 1 of this embodiment will be described.
[0103] <Dicing die bond film manufacturing method> The manufacturing method of the dicing die bond film 1 of this embodiment is as follows: A step of producing a die bond sheet 10; A step of preparing a dicing tape 20; The method includes a step of overlapping the manufactured die bond sheet 10 and the dicing tape 20.
[0104] <Process for producing die bond sheet> The process of producing the die bond sheet 10 includes the following steps: A resin composition preparation step of preparing a resin composition for forming the die bond sheet 10; and a die-bonding sheet forming step of forming the die-bonding sheet 10 from the resin composition.
[0105] In the resin composition preparation step, for example, the first thermoplastic resin, the second thermoplastic resin, the inorganic filler, the solvent, and, if necessary, the thermosetting resin are mixed and each resin is dissolved in the solvent to prepare the resin composition. The viscosity of the composition can be adjusted by changing the amount of the solvent. Commercially available products can be used as these resins.
[0106] In the die-bonding sheet forming step, for example, the resin composition prepared as described above is applied to a release liner. The application method is not particularly limited, and for example, a general application method such as roll coating, screen coating, gravure coating, etc. is adopted. Next, if necessary, the applied composition is solidified by a solvent removal treatment, a curing treatment, etc., to form the die-bonding sheet 10.
[0107] <Process for producing dicing tape> The process for producing the dicing tape includes the following steps: A synthesis step of synthesizing an acrylic polymer; a pressure-sensitive adhesive layer preparation step of preparing a pressure-sensitive adhesive layer 22 by volatilizing a solvent from a pressure-sensitive adhesive composition containing the above-mentioned acrylic polymer, an isocyanate compound, a polymerization initiator, a solvent, and other components appropriately added depending on the purpose; a base layer preparation step of preparing a base layer 21; The method further includes a lamination step of laminating the adhesive layer 22 and the base layer 21 together to laminate the base layer 21 and the adhesive layer 22 together.
[0108] In the synthesis step, for example, an alkyl(meth)acrylate monomer and a hydroxyl group-containing (meth)acrylate monomer are radically polymerized to synthesize an acrylic polymer intermediate. The radical polymerization can be carried out by a general method. For example, the above-mentioned monomers are dissolved in a solvent, stirred under heating, and a polymerization initiator is added to synthesize an acrylic polymer intermediate. In order to adjust the molecular weight of the acrylic polymer, the polymerization may be carried out in the presence of a chain transfer agent. Next, some of the hydroxyl groups of the structural units of the hydroxyl group-containing (meth)acrylate contained in the acrylic polymer intermediate are bonded to the isocyanate groups of the isocyanate group-containing polymerizable monomer by a urethane reaction, whereby some of the structural units of the hydroxyl group-containing (meth)acrylate become structural units of the polymerizable group-containing (meth)acrylate. The urethane reaction can be carried out by a general method. For example, the acrylic polymer intermediate and the isocyanate group-containing polymerizable monomer are stirred while being heated in the presence of a solvent and a urethane catalyst. This allows the isocyanate group of the isocyanate group-containing polymerizable monomer to be urethane-bonded to a part of the hydroxyl groups of the acrylic polymer intermediate.
[0109] In the pressure-sensitive adhesive layer preparation step, for example, an acrylic polymer, an isocyanate compound, and a polymerization initiator are dissolved in a solvent to prepare a pressure-sensitive adhesive composition. The viscosity of the composition can be adjusted by changing the amount of the solvent. Next, the pressure-sensitive adhesive composition is applied to a release liner. As a coating method, for example, a general coating method such as roll coating, screen coating, or gravure coating is adopted. The applied composition is subjected to a solvent removal treatment, a solidification treatment, or the like to solidify the applied pressure-sensitive adhesive composition, thereby preparing the pressure-sensitive adhesive layer 22.
[0110] In the base layer preparation step, the base layer can be prepared by film formation using a general method. Examples of the film formation method include a calendar film formation method, a casting method in an organic solvent, an inflation extrusion method in a closed system, a T-die extrusion method, and a dry lamination method. A co-extrusion molding method may also be used. In addition, a commercially available film or the like may be used as the base layer 21.
[0111] In the lamination step, the pressure-sensitive adhesive layer 22 overlapping the release liner is laminated on the base layer 21. The release liner may remain overlapping the pressure-sensitive adhesive layer 22 until use. In addition, in order to promote the reaction between the crosslinking agent and the acrylic polymer, and also between the crosslinking agent and the surface portion of the base layer 21, an aging treatment step may be carried out for 48 hours in an environment of 50°C after the lamination step.
[0112] Through these steps, the dicing tape 20 can be manufactured.
[0113] <Step of overlapping the die bond sheet 10 and the dicing tape 20> In the step of overlapping the die bond sheet 10 and the dicing tape 20, the die bond sheet 10 is attached to the adhesive layer 22 of the dicing tape 20 manufactured as described above.
[0114] In such attachment, the release liners are peeled off from the adhesive layer 22 of the dicing tape 20 and the die bond sheet 10, and the die bond sheet 10 and the adhesive layer 22 are attached together so that they are in direct contact with each other. For example, they can be attached by pressure bonding. The temperature during attachment is not particularly limited, and is, for example, a temperature above room temperature, 30° C. or higher and 50° C. or lower, and preferably 35° C. or higher and 45° C. or lower. The linear pressure during attachment is not particularly limited, but is preferably 0.1 kgf / cm or higher and 20 kgf / cm or lower, and more preferably 1 kgf / cm or higher and 10 kgf / cm or lower.
[0115] The dicing die bond film 1 manufactured as described above through the above-mentioned steps is used, for example, as an auxiliary tool for manufacturing a semiconductor device having a semiconductor integrated circuit. A specific example of the use will be described below.
[0116] <Method of using dicing die bond film when manufacturing semiconductor device> In a manufacturing method of a semiconductor device, generally, chips are cut out from a semiconductor wafer having a circuit surface formed thereon and assembled. At this time, the dicing die bond film of the present embodiment is used as a manufacturing auxiliary tool.
[0117] A typical method for manufacturing a semiconductor device includes a process of cutting out chips from a semiconductor wafer on which a circuit surface is formed, and assembling the chips. This process includes, for example, a stealth dicing process in which a weak portion is formed by laser light inside a semiconductor wafer to which a backgrind tape has been attached, and the semiconductor wafer is prepared for processing into chips (dies) by a fracturing process; a backgrinding process in which the semiconductor wafer to which the backgrind tape has been attached is ground to reduce the thickness of the semiconductor wafer; a mounting process in which one side of the semiconductor wafer whose thickness has been reduced (for example, the side opposite to the circuit side) is attached to a die bond sheet 10 and the semiconductor wafer is fixed to the dicing tape 20; and a mounting process in which the semiconductor wafer and the die bond sheet 1 are fixed to each other by stretching the dicing tape 20. The dicing process includes an expanding step of fracturing the dicing tape 10 and expanding the gap between the chips, a pick-up step of peeling the die bond sheet 10 from the adhesive layer 22 to take out the semiconductor chip (die) with the die bond sheet 10 attached, a die bond step of bonding the die bond sheet 10 attached to the semiconductor chip (die) to an adherend, a curing step of hardening the die bond sheet 10 attached to the adherend, a wire bonding step of electrically connecting the electrodes of the electronic circuit in the semiconductor chip (die) to the adherend by wires, and a sealing step of sealing the semiconductor chip (die) and wires on the adherend with a thermosetting resin. When any of these steps is performed, at least a part of the dicing tape (dicing die bond film) of this embodiment is used as a manufacturing auxiliary tool.
[0118] In the stealth dicing process, as shown in FIGS. 2A to 2C, weak parts for separating the semiconductor wafer W into small pieces (dies) are formed inside the semiconductor wafer W. More specifically, a backgrind tape G is attached to the circuit surface of the semiconductor wafer W (see FIG. 2A). With the backgrind tape G attached, the semiconductor wafer W is subjected to a grinding process (pre-backgrinding process) using a grinding pad K until it reaches a predetermined thickness (see FIG. 2B). A laser beam is applied to the thinned semiconductor wafer W to form weak parts inside the semiconductor wafer W (see FIG. 2C).
[0119] In the backgrinding process, as shown in FIG. 2D, the semiconductor wafer W with the backgrind tape G attached thereto is further ground to reduce the thickness of the semiconductor wafer W to the thickness of the chip (die) that will be produced by subsequent cutting.
[0120] In the mounting process, as shown in Figures 3A and 3B, the semiconductor wafer W is fixed to the dicing die bond film 1. In detail, while attaching the dicing ring R to the adhesive layer 22 of the dicing tape 20, the semiconductor wafer W whose thickness has been reduced by the above-mentioned cutting process is attached to the exposed surface of the die bond sheet 10 (see Figure 3A). Then, the backgrind tape G is peeled off from the semiconductor wafer W (see Figure 3B).
[0121] In the expanding step, as shown in FIG. 4A to FIG. 4C, the semiconductor wafer W is split by stretching the dicing tape 20, and the interval between the adjacent semiconductor chips (dies) X is expanded. In detail, the dicing ring R is attached to the adhesive layer 22 of the dicing tape 20, and then fixed to the holder H of the expanding device (see FIG. 4A). The dicing die bond film 1 is stretched so as to be expanded in the surface direction by pushing up the push-up member U of the expanding device from the lower side of the dicing die bond film 1 (see FIG. 4B). As a result, the semiconductor wafer W is split under a specific temperature condition. The above temperature condition is, for example, −20° C. or higher and 0° C. or lower, preferably −15° C. or higher and 0° C. or lower, and more preferably −10° C. or higher and −5° C. or lower. The expanded state is released by lowering the push-up member U (see FIG. 4C, low-temperature expanding step up to this point). When the expanding step is performed at such a low temperature, it is necessary to break the die bond sheet 10. The die bond sheet 10 of the present embodiment described above is designed to be broken well at this time. 5A to 5B, the dicing tape 20 is stretched so as to expand its area under higher temperature conditions (for example, 10° C. or higher and 25° C. or lower). As a result, adjacent semiconductor chips X are separated in the planar direction of the film surface after cleavage, and the kerf (spacing) is further expanded (room temperature expansion process).
[0122] In the pick-up process, as shown in Fig. 6, the semiconductor chip X with the die bond sheet piece 10' attached thereto is peeled off from the adhesive layer 22 of the dicing tape 20. More specifically, the pin members P are raised to push up the semiconductor chip X to be picked up through the dicing tape 20. The pushed-up semiconductor chip X is held by a suction jig J. As the suction jig J, for example, a pick-up collet is used.
[0123] In the die bonding process, the semiconductor chip X with the die bond sheet piece 10' attached thereto is bonded to the adherend Z using the above-mentioned suction jig J. In the die bonding process, the semiconductor chip X is generally bonded to the adherend Z under a temperature condition of about 120°C or higher and 150°C or lower. In the die bonding process, as shown in FIG. 7, the semiconductor chips X with the small pieces 10' of the die bonding sheet attached thereto may be stacked multiple times.
[0124] In the pick-up process and the die-bonding process, the suction jig J repeats the operation of picking up the semiconductor chip X and the operation of bonding the semiconductor chip X to the adherend Z under heating conditions. The suction jig J accumulates heat while repeating these operations, and may reach a temperature of, for example, 100°C or higher. If the pick-up process is performed using the suction jig J with an increased temperature, the heat is transferred to the small piece 10' of the die-bonding sheet, and the small piece 10' may be heated to, for example, about 50°C and softened. Then, the small piece 10' may not necessarily be peeled off well from the adhesive layer 22 of the dicing tape 20. In addition, in the die-bonding process, the small piece 10' of the die-bonding sheet is bonded to the adherend Z at a relatively high temperature of around 130°C, so that the small piece 10' needs to adhere well to the adherend Z even at a relatively high temperature. The die bond sheet 10 of this embodiment is configured to have a relatively high elastic modulus at 50° C. and a relatively low elastic modulus at 130° C., so that both the pick-up process and the die bond process can be performed well. That is, the die bond sheet 10 of this embodiment can have both good pick-up performance and good die bond performance.
[0125] In the curing step, in order to promote the hardening of the small piece 10' of the die-bonding sheet, a heat treatment is performed at a temperature of, for example, 100° C. or more and 150° C. or less. At this time, pressure can be applied to the small piece 10' of the die-bonding sheet. The heat treatment is performed while applying a pressure of preferably 0.2 MPa or more and 2 MPa or less, more preferably 0.4 MPa or more and 1 MPa or less.
[0126] In the wire bonding process, as shown in Fig. 8, a semiconductor chip X (die) and an adherend Z are connected while being heated. Therefore, the glycidyl group of the above-mentioned acrylic resin contained in the die bond sheet 10 becomes reactive by heating, and the hardening reaction of the die bond sheet 10 can proceed.
[0127] In the sealing process, the semiconductor chip X (die) and the small piece 10' of the die bond sheet are sealed with a thermosetting resin M such as epoxy resin, as shown in Fig. 9. In the sealing process, in order to flow and then harden the thermosetting resin M, the sealing process is performed while applying pressure and heating at a temperature of, for example, 150°C to 200°C.
[0128] After the sealing process, a reflow soldering process may be performed in which the electrodes are electrically connected by molten solder. In the reflow soldering process, a heat treatment is performed at a temperature of 230° C. or more and 270° C. or less, for example.
[0129] In the above-mentioned method for manufacturing a semiconductor device (method for using a dicing die bond film), an example in which a semiconductor wafer W having a weak portion formed therein is fractured into small pieces in an expanding process has been described in detail, but the present invention is not limited to such an example. For example, instead of forming a weak portion inside the semiconductor wafer W, a semiconductor wafer W that has been subjected to a so-called half-cut process may be broken into small pieces in the expanding process. Furthermore, for example, when the above-mentioned pre-backgrinding process is performed on a semiconductor wafer W having a weak portion formed therein or a semiconductor wafer W that has been subjected to a half-cut process, the semiconductor wafer W may be divided into small pieces.
[0130] In addition, in recent years in the semiconductor industry, with further advances in integration technology, there is a demand for thinner semiconductor chips (e.g., a thickness of 20 μm or more and 50 μm or less) and thinner die bond sheets (e.g., a thickness of 1 μm or more and 40 μm or less, preferably 7 μm or less, and more preferably 5 μm or less).
[0131] The die bond sheet and dicing die bond film of this embodiment are as exemplified above, but the present invention is not limited to the die bond sheet and dicing die bond film exemplified above. That is, various forms used in general die bond sheets and dicing die bond films can be adopted within the scope that does not impair the effects of the present invention.
[0132] The matters disclosed in this specification include the following. (1) A die bond sheet containing at least a thermoplastic resin and an inorganic filler, The thermoplastic resin includes a first thermoplastic resin and a second thermoplastic resin having an average molecular weight smaller than that of the first thermoplastic resin, A die bond sheet having an elastic modulus of 2 MPa or more and 10 MPa or less at 50°C before curing, and an elastic modulus of 0.1 MPa or more and 1.5 MPa or less at 130°C before curing. (2) The average molecular weight of the first thermoplastic resin is 500,000 or more and 1,500,000 or less, and the average molecular weight of the second thermoplastic resin is 10,000 or more and 100,000 or less, The die-bonding sheet according to (1) above, wherein the glass transition temperatures of the first thermoplastic resin and the second thermoplastic resin are both 0° C. or higher and 30° C. or lower. (3) The die bond sheet according to (1) or (2) above, having a breaking elongation at -15°C of 0.2% or more and 2.0% or less. (4) Breaking strength at -15℃ is 1.0kg / mm 2 More than 7.5kg / mm 2 The die bond sheet according to any one of (1) to (3) above, which is as follows: (5) The die bond sheet according to any one of (1) to (4) above, wherein the inorganic filler contains silica particles. (6) The die bond sheet according to any one of (1) to (5) above, further comprising a thermosetting resin. (7) A dicing die bond film comprising the die bond sheet according to any one of (1) to (6) above and a dicing tape attached to the die bond sheet. (8) The dicing tape has a base layer and a pressure-sensitive adhesive layer superposed on one surface of the base layer, The pressure-sensitive adhesive layer contains an acrylic polymer having a polymerizable group-containing (meth)acrylate structural unit in the molecule, The dicing die bond film described in (7) above, wherein the peel force between the die bond sheet and the dicing tape at 50°C is 0.03 N / 20 mm or more and 0.20 N / 20 mm or less after the adhesive layer is cured by irradiation with active energy rays. (9) A semiconductor device comprising the die bond sheet according to any one of (1) to (6) above. (10) An electronic device comprising the semiconductor device according to (9) above. EXAMPLES
[0133] The present invention will now be described in more detail with reference to experimental examples, but the present invention is not limited to these.
[0134] A die-bonding sheet was produced as follows. This die-bonding sheet was then attached to a dicing tape to produce a dicing die-bonding film.
[0135] <Preparation of die bond sheet> The raw materials having the composition shown in Tables 1 and 2 were added to methyl ethyl ketone and mixed to obtain a composition for a die-bonding sheet having a solid content concentration of 15% by mass. Details of each raw material are shown below. (1st thermoplastic resin) [SG-P3] First acrylic resin (containing glycidyl groups) Mass average molecular weight: Mw=850,000 Product name: "Teisan Resin SG-P3" manufactured by Nagase Chemtex Corporation Epoxy value: 0.21 [eq / kg] Glass transition temperature Tg: 13℃ [SG-708-6] First acrylic resin (containing carboxyl and hydroxyl groups) Mass average molecular weight: Mw=700,000 Product name: "Teisan Resin SG-708-6" manufactured by Nagase Chemtex Corporation Acid value: 9 [mgKOH / g] Glass transition temperature Tg: 4℃ · [SG-70L] First acrylic resin (containing carboxyl and hydroxyl groups) Mass average molecular weight: Mw=900,000 Product name: "Teisan Resin SG-70L" manufactured by Nagase Chemtex Corporation Acid value: 5 [mgKOH / g] Glass transition temperature Tg: -15℃ (Second thermoplastic resin) [Polymer A] Acrylic resin solution (solid content 70% by mass) in which a copolymer (second acrylic resin) of ethyl acrylate (EA), butyl methacrylate (BMA), and glycidyl methacrylate (GMA) is dissolved in methyl ethyl ketone (MEK) Mass average molecular weight: 70,000 (Mw=70,000), Epoxy equivalent: 444 [g / eq], Glass transition temperature Tg: 11℃ - [Polymer B] Acrylic resin solution (solid content 70% by mass) in which a copolymer (second acrylic resin) of ethyl acrylate (EA), butyl methacrylate (BMA), and glycidyl methacrylate (GMA) is dissolved in methyl ethyl ketone (MEK) Mass average molecular weight: 40,000 (Mw=40,000), Epoxy equivalent: 2029 [g / eq], Glass transition temperature Tg: 2℃ (thermosetting resin) ·[MEHC-7851SS] Biphenyl aralkyl type phenolic resin Product name: "MEHC-7851SS" manufactured by UBE Hydroxyl group equivalent: 203[g / eq] [EPPN-501HY] Trisphenolmethane epoxy resin Product name: "EPPN-501HY" manufactured by Nippon Kayaku Co., Ltd. Epoxy equivalent: 166 [g / eq] (Inorganic filler) [MEK-AC-2140Z] Spherical Silica Dispersion Product name: "MEK-AC-2140Z" manufactured by Nissan Chemical Industries, Ltd. Particles with chemically modified surfaces Dispersion with average particle size of 10 nm to 15 nm and solid content of 40% by mass [MEK-AC-5140Z] Spherical Silica Dispersion Product name: "MEK-AC-5140Z" manufactured by Nissan Chemical Particles with chemically modified surfaces Dispersion with average particle size of 70 nm to 100 nm and solid content of 40% by mass [SO-E2] Spherical Silica Product name: "ADMAFINE SO-E2" manufactured by Admatechs Average particle size 500nm (Silane coupling agent) [KBM-403] 3-Glycidoxypropyltrimethoxysilane Product name: "KBM-403" manufactured by Shin-Etsu Chemical Co., Ltd. [KBM-303] 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane Product name: "KBM-303" manufactured by Shin-Etsu Chemical Co., Ltd.
[0136] A die-bonding sheet composition was prepared using any of the above raw materials according to the blending composition shown in Tables 1 and 2. Then, the die-bonding sheet composition was applied to one side of the release liner (the silicone-treated side of the PET sheet having a thickness of 50 μm) using an applicator. The application was performed so that the thickness after drying was 40 μm, and then the solvent was volatilized from the die-bonding sheet composition by drying at 130° C. for 2 minutes. In this way, a die-bonding sheet overlapping one side of the release liner was obtained.
[0137] <Dicing tape base layer> The following product was used as the resin raw material to produce a base layer (thickness 100 μm) consisting of one layer. Product name: Evaflex P1007 (manufactured by Mitsui DuPont Polychemicals) Ethylene-vinyl acetate copolymer (EVA) Contains 9% by mass of vinyl acetate monomer units
[0138] (Forming of base layer) The substrate layer was formed using an extrusion T-die molding machine. The extrusion temperature was 190° C. The substrate layer was wound into a roll and stored.
[0139] <Adhesive layer of dicing tape> (Preparation of Adhesive Layer (Adhesive Composition)) The following raw materials were mixed to prepare a first resin composition. INA (isononyl acrylate) 150 parts by weight 62 parts by weight of HEA (hydroxyethyl acrylate) 0.4 parts by weight of AIBN (2,2'-azobisisobutyronitrile) 350 parts by weight of ethyl acetate Next, the first resin composition was placed in a round-bottom separable flask of a polymerization experimental apparatus equipped with a round-bottom separable flask (volume 1 L), a thermometer, a nitrogen inlet tube, and a stirring blade. While stirring the first resin composition, the liquid temperature of the first resin composition was adjusted to room temperature (23°C), and the inside of the round-bottom separable flask was replaced with nitrogen gas for 6 hours. Next, while nitrogen gas was flowing into the round-bottom separable flask, the first resin composition was stirred and the liquid temperature of the first resin composition was kept at 62°C for 3 hours. After that, the mixture was further kept at 75°C for 2 hours to carry out the polymerization reaction of the INA, HEA, and AIBN, and the second resin composition was prepared. Then, the flow of nitrogen gas into the round-bottom separable flask was stopped. After the second resin composition was cooled to room temperature, the following raw materials were added to the second resin composition to prepare a third resin composition. 2-Methacryloyloxyethyl isocyanate Compounds with polymerizable carbon-carbon double bonds Product name: Karenz MOI, manufactured by Showa Denko Co., Ltd.) 58 parts by weight Dibutyltin dilaurate IV (Wako Pure Chemical Industries, Ltd.) 0.3 parts by weight The obtained third resin composition was stirred in the air at 50° C. for 24 hours. Finally, the following raw materials were added to 100 parts by mass of the polymer solid content of the third resin composition. Isocyanate compound (product name "Takenate D-101A" (Mitsui Chemicals)) 1.0 part by weight (Trifunctional isocyanate compound) Photopolymerization initiator (product name "Omnirad127", IGM Resins) 3 parts by weight Then, the third resin composition was diluted with ethyl acetate so that the solid content concentration was 20 mass %, thereby preparing a pressure-sensitive adhesive composition.
[0140] <Preparation of dicing tape> The above-mentioned adhesive composition was applied to one surface of the base layer using an applicator so that the thickness after drying was 10 μm. After the adhesive composition was applied, a heat drying treatment was performed at 110 ° C for 3 minutes to form an adhesive layer. In this way, a dicing tape was produced.
[0141] <Manufacture of dicing die bond film> (Laminating the die bond sheet and dicing tape) The adhesive layer of the dicing tape was attached to the die bond sheet (the side on which the release liner was not laminated) of the die bond sheet. Then, the release liner was peeled off from the die bond sheet to prepare a dicing die bond film equipped with the die bond sheet.
[0142] In the above manner, the die bond sheet and the dicing die bond film of the examples and the comparative examples were manufactured. Details of each die bond sheet are shown in Tables 1 and 2. In Tables 1 and 2, the blending amounts [parts by mass] of the first thermoplastic resin, the second thermoplastic resin, the thermosetting resin, the inorganic filler (silica filler), etc. are shown in terms of solid content.
[0143] [Table 1]
[0144] [Table 2]
[0145] <Measurement of tensile modulus of die bond sheet> The die bond sheets before the heat curing treatment of each example and each comparative example were laminated to a thickness of 200 μm. Next, this laminated sample was cut into a strip shape with a width of 10 mm and a length of 50 mm with a cutter knife to obtain a test piece. Using a solid viscoelasticity measuring device (measurement device: RSA-G2, Rheometrics Scientific Co. (TA Instruments Co.), the dynamic storage modulus was measured in a tensile mode in a temperature range from -20 ° C to 200 ° C under the conditions of a frequency of 1 Hz, a heating rate of 10 ° C / min, an initial chuck distance of 22.5 mm, and a strain of 0.1%. Then, the values at 50 ° C and 130 ° C were read, and these values were taken as the tensile modulus (tensile storage modulus) [MPa] at 50 ° C and 130 ° C.
[0146] <Measurement of breaking elongation (breaking elongation) and breaking strength of die bond sheet at low temperature> The breaking elongation (breaking elongation) and breaking strength of the die bond sheet were measured under the above-mentioned measurement conditions. Specifically, the die bond sheet before the heat curing treatment of each Example and each Comparative Example was coated to a thickness of 20 μm to prepare a sheet sample, or laminated to prepare a laminated sheet sample. Next, this sample was cut into a strip shape of 10 mm in width and 50 mm in length with a cutter knife to prepare a test piece. A tensile test was performed using a solid viscoelasticity measuring device (measurement device: RSA-G2, Rheometrics Scientific Co., Ltd. (TA Instruments Co., Ltd.) under the conditions of a temperature of -15°C, a tensile speed of 1 mm / sec, and an initial chuck distance of 20 mm. Note that the measurement was started after holding at -15°C for 5 minutes. The elongation at break was taken as the breaking elongation (breaking elongation). The test force at break was also confirmed as the breaking strength.
[0147] <Evaluation of peel strength (peel strength between die bond sheet and adhesive layer of dicing tape)> The peel strength between the die bond sheet and the pressure-sensitive adhesive layer of the dicing tape was measured according to the above-mentioned test conditions. Specifically, after bonding a backing tape to the die bond sheet of the dicing die bond film, a test piece with a width of 50 mm and a length of 120 mm was cut out. Using the cut out test piece, a T-type peel test was performed to measure the peel force [N / 20 mm]. The temperature condition for the measurement was 50°C, and the peel speed was 300 mm / min. Before laminating the backing tape, the adhesive layer of the dicing tape was irradiated with 300 mJ / cm from the base layer side at a temperature of 22°C. 2 (Irradiation intensity 150mW / cm 2 The adhesive layer was then cured by irradiating it with ultraviolet light for 2 seconds. It is believed that the pick-up performance will be good if the peel strength is 0.05 [N / 20 mm] or more and 0.20 [N / 20 mm] or less.
[0148] <Evaluation of pick-up performance (Picking up a small piece of a die bond sheet with a semiconductor chip from a dicing tape> Using each of the manufactured dicing die bond films, a mounting process, a low-temperature expanding process for cleaving the semiconductor wafer, a room-temperature expanding process for spacing the chips, and a die bond process were carried out as follows. In the mounting process, the semiconductor wafer held by the wafer processing tape (product name "UB-3083D", manufactured by Nitto Denko Corporation) was attached to the adhesive layer of the dicing die bond film, and then the wafer processing tape was peeled off from the semiconductor wafer. The semiconductor wafer had a thickness of 50 μm, and was subjected to half-cut processing to form a dividing groove (width 25 μm, each section in a grid shape of 10 mm × 10 mm) for small pieces, and was thinned through pre-back grinding processing. The above-mentioned attachment was performed using a laminator, with an attachment speed of 10 mm / sec, a temperature condition of 60°C, and a pressure condition of 0.15 MPa. The surface of the semiconductor wafer opposite to the surface on which the dividing groove was formed was attached to the adhesive layer of the dicing die bond film. The low-temperature expansion step was carried out in a low-temperature expansion unit of a die separator (product name "Die Separator DDS2300", manufactured by Disco Corporation) using the die separator. Specifically, a ring frame was attached to the adhesive layer of the dicing die bond film to which the semiconductor wafer was attached, and the dicing die bond film was set in the device. In the low-temperature expansion unit of the device, the dicing tape was expanded together with the semiconductor wafer. In this low-temperature expansion step, the temperature was -15°C, the expansion speed was 200 mm / sec, and the expansion amount was 12 mm. In this way, the semiconductor wafer was cut into small pieces on the dicing tape, and multiple semiconductor chips with die bond sheets were obtained. The room temperature expansion step was carried out in a room temperature expansion unit in a die separator device (product name "Die Separator DDS2300", manufactured by Disco Corporation) after the above-mentioned low temperature expansion step. Specifically, the dicing tape of the dicing die bond film in a state accompanied by the diced semiconductor wafer (multiple semiconductor chips) was expanded in the room temperature expansion unit of the same device. In this room temperature expansion step, the temperature was 23°C, the expansion speed was 1mm / sec, and the expansion amount was 10mm. Thereafter, the dicing sheet was thermally shrunk in a heat expander unit to obtain an evaluation sample. The conditions of the thermal shrinkage were an expansion amount of 10mm, a heat temperature of 250°C, an air volume of 40L / min, a heat distance of 20mm, and a rotation speed of 3° / sec.
[0149] At a temperature of 22°C, the dicing tape was applied with a 300mJ / cm2 pressure to the adhesive layer from the base layer side. 2 (Irradiation intensity 150mW / cm 2 The adhesive layer was cured by irradiating it with ultraviolet light for 10 seconds. After that, 1000 chips were picked up with a die bonder and the pick-up ability was evaluated. If two or more chips could not be picked up, it was judged as defective (×), and if one or less chips could not be picked up, it was judged as good (◯). Pickup was performed using a die bonder (manufactured by Shinkawa, product name "Die Bonder SPA-300") with 5 pins and a pickup height of 350 μm. The die bond temperature was 130°C.
[0150] <Evaluation of die bonding performance> (Shear adhesive strength of die bond sheet at 130℃) Each die bond sheet was attached to a bare chip (silicon chip) of 0.5 mm thickness and 3 mm x 3 mm size under the following conditions: temperature 80°C, speed 10 mm / s, and pressure 0.15 MPa. Furthermore, each die bond sheet was bonded to a bare chip (0.5 mm, 10 mm x 10 mm) to obtain each test piece. A die bonder (manufactured by Shinkawa Co., Ltd., product name "Die Bonder SPA-300") was used for bonding. The bonding conditions were: stage temperature 130°C, die bond load 0.2 MPa, and die bond time 1 second. Next, a shear tester (Dage, Dage4000) was used to apply a shear force to each test piece, and the shear adhesive strength (MPa) was measured. The measurement conditions were a speed of 500 μm / s, a measurement gap of 100 μm, and a stage temperature of 130° C. The measurement was performed 20 seconds after placing the test piece on the measurement stage. A measured value of 0.02 MPa or more was judged as good (◯), and a value less than this was judged as poor (×).
[0151] As can be seen from the above evaluation results, the die bond sheets of the examples were able to combine good pick-up performance and good die bond performance. On the other hand, the die bond sheet of the comparative example could not achieve both good pick-up performance and good die bond performance.
[0152] By using the die bond sheet (dicing die bond film) of the embodiment having the above-mentioned physical properties in the manufacture of semiconductor devices, so-called NAND type flash memories and the like can be manufactured efficiently. [Industrial Applicability]
[0153] The die bond sheet and dicing die bond film of the present invention are suitably used, for example, as auxiliary tools when manufacturing a semiconductor device having a semiconductor integrated circuit. [Explanation of symbols]
[0154] 1: Dicing die bond film, 10: Die bond sheet, 20: dicing tape, 21: Base material layer, 22: Adhesive layer.
Claims
1. A die bond sheet containing at least a thermoplastic resin and an inorganic filler, The thermoplastic resin includes a first thermoplastic resin and a second thermoplastic resin having an average molecular weight smaller than that of the first thermoplastic resin, A die bond sheet having an elastic modulus of 2.0 MPa or more and 10.0 MPa or less at 50°C before curing, and an elastic modulus of 0.1 MPa or more and 1.5 MPa or less at 130°C.
2. The average molecular weight of the first thermoplastic resin is 500,000 or more and 1,500,000 or less, and the average molecular weight of the second thermoplastic resin is 10,000 or more and 100,000 or less, The die bond sheet according to claim 1 , wherein the glass transition temperatures of the first thermoplastic resin and the second thermoplastic resin are both 0° C. or higher and 30° C. or lower.
3. The die bond sheet according to claim 1 or 2, wherein the breaking elongation at -15 ° C. is 0.2% or more and 2.0% or less.
4. Breaking strength at -15°C is 1.0 kg / mm 2 Over 7.5kg / mm 2 The die bond sheet according to claim 1 or 2, wherein:
5. The die bond sheet according to claim 1 or 2, wherein the inorganic filler contains silica particles.
6. A dicing die bond film comprising the die bond sheet according to claim 1 or 2 and a dicing tape attached to the die bond sheet.
7. The dicing die bond film according to claim 6, wherein the peel strength between the die bond sheet and the dicing tape at 50°C is 0.03 N / 20 mm or more and 0.20 N / 20 mm or less.
8. A semiconductor device comprising the die bond sheet according to claim 1 or 2.
9. An electronic device comprising the semiconductor device according to claim 8.
Citation Information
Patent Citations
Dicing die attach film and method for manufacturing the same, and semiconductor package and method for manufacturing the same
JP2022150243A
Cited By
Game machine
JP2024159849A
Game machine
JP2024159850A
Game machine
JP2024161101A
Game machine
JP2024161102A
Game machine
JP2024161104A