Precipitation hardening stainless steel powder, compound, granulated powder, precipitation hardening stainless steel sintered body, and method for manufacturing the precipitation hardening stainless steel sintered body

The use of a precipitation hardening stainless steel powder with optimized elemental ratios suppresses sinterability and ensures effective binder removal, resulting in a sintered body with enhanced mechanical strength and reduced carbon content.

JP7552080B2Active Publication Date: 2024-09-18SEIKO EPSON CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020100714
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-09-11
Filing Date
2020-06-10
Publication Date
2024-09-18
Estimated Expiration
2040-06-10

AI Technical Summary

Technical Problem

In existing powder metallurgy methods, organic binders are not fully removed during degreasing, leading to carbon atom concentration increases in the sintered body, which deteriorates mechanical properties, especially when using fine metal powder that sintering proceeds faster.

Method used

A precipitation hardening stainless steel powder composition with specific elemental concentrations and a defined δ value is used, optimizing the ratio of elements to suppress sinterability and enhance mechanical strength, allowing for efficient removal of organic binders during firing.

Benefits of technology

The method produces a sintered body with high mechanical strength and reduced carbon atom concentration, maintaining excellent mechanical properties and corrosion resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007552080000002
    Figure 0007552080000002
  • Figure 0007552080000001
    Figure 0007552080000001
Patent Text Reader

Abstract

To provide precipitation-hardened stainless steel powder which allows for production of a sintered body having a high mechanical strength, a compound and granulated powder each including the precipitation-hardened stainless steel powders, and a precipitation-hardened stainless steel sintered body having a high mechanical strength and a method for producing the same.SOLUTION: Precipitation-hardened stainless steel powder includes: Cr of concentration A of 15.00 mass% or more and 17.50 mass% or less; Si of concentration B of 0.30 mass% or more and 1.00 mass% or less; Nb of concentration C of 0.15 mass% or more and 0.45 mass% or less; Ni of concentration D of 3.00 mass% or more and 5.00 mass% or less; Mn of concentration E of 0.05 mass% or more and 1.00 mass% or less; and Cu of concentration F of 3.00 mass% or more and 5.00 mass% or less, wherein a value of δ defined by the following expression (1): δ=3(A+1.5B+0.5C)-2.8(D+0.5E+0.5F)-19.8 is 10.0 mass% or more and 14.0 mass% or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a precipitation hardening stainless steel powder, a compound, a granulated powder, a precipitation hardening stainless steel sintered body, and a method for producing the precipitation hardening stainless steel sintered body. [Background technology]

[0002] In the powder metallurgy method, a composition containing a metal powder and an organic binder is molded into a desired shape, the molded body is degreased to obtain a degreased body, and the degreased body is fired to produce a sintered body. In the process of producing such a sintered body, atomic diffusion occurs between the particles of the metal powder, which gradually densifies the molded body and leads to sintering.

[0003] In such powder metallurgy methods, when the compact is degreased, the compact is heated to thermally decompose the organic binder and remove it. If the organic binder remains in the compact, the properties of the sintered compact are deteriorated, so various methods for removing the organic binder have been studied.

[0004] For example, Patent Document 1 discloses a method of degreasing a molded body containing a metal material powder and a binder containing a polyoxymethylene resin by heating the molded body in an acid-containing atmosphere. By carrying out the degreasing process in an acid-containing atmosphere in this manner, the acid decomposes the binder, so that the binder can be efficiently removed. Therefore, the above-mentioned problems can be reduced. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 4-247802 Summary of the Invention [Problem to be solved by the invention]

[0006] In the method described in Patent Document 1, it is considered that most of the organic binder is removed in the degreasing treatment. However, some of the organic binder remains in the molded body, and is removed in the subsequent firing treatment in parallel with the progress of sintering of the metal material powder. At this time, for example, when the particle size of the metal material powder used is small, the sintering tends to proceed quickly. In other words, sintering may start at a lower temperature. In that case, the organic binder may be trapped in the molded body during the firing treatment. As a result, the carbon atom concentration in the sintered body increases, and there is a concern that the mechanical properties of the sintered body may deteriorate. [Means for solving the problem]

[0007] The precipitation hardening stainless steel powder according to the application example of the present invention is Cr is contained at a concentration A within a range of 15.00 mass% or more and 17.50 mass% or less, Si is contained at a concentration B in the range of 0.30 mass% or more and 1.00 mass% or less, Nb is contained at a concentration C in the range of 0.15 mass% or more and 0.45 mass% or less, Ni is contained at a concentration D in the range of 3.00 mass% or more and 5.00 mass% or less, Mn is contained at a concentration E in the range of 0.05 mass% or more and 1.00 mass% or less, Cu is contained at a concentration F in the range of 3.00 mass% or more and 5.00 mass% or less, The value of δ defined by the following formula (1) is 10.0 mass% or more. 13.5 Mass % or less It is characterized by: δ=3(A+1.5B+0.5C)-2.8(D+0.5E+0.5F)-19.8· (1) [Brief description of the drawings]

[0008] [Figure 1] 1 is a process diagram showing a method for producing a precipitation hardening stainless steel sintered body according to an embodiment. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, embodiments of the precipitation hardening stainless steel powder, compound, granulated powder, precipitation hardening stainless steel sintered body, and method for producing the precipitation hardening stainless steel sintered body of the present invention will be described in detail.

[0010] 1. Precipitation hardening stainless steel powder First, the precipitation hardening stainless steel powder according to the embodiment will be described.

[0011] In powder metallurgy, a composition containing a metal powder and a binder is molded into a desired shape, and then the molded composition is subjected to a degreasing process and a sintering process to obtain a sintered body of a desired shape. Compared to other techniques, powder metallurgy can produce sintered bodies of complex and fine shapes in near-net shapes, i.e., shapes close to the final shape.

[0012] The precipitation hardening stainless steel powder according to the embodiment is a powder made of precipitation hardening stainless steel containing Cr, Si, Nb, Ni, Mn and Cu. In this powder, Cr is contained at a concentration A in the range of 15.00 mass% to 17.50 mass%, Si is contained at a concentration B in the range of 0.30 mass% to 1.00 mass%, Nb is contained at a concentration C in the range of 0.15 mass% to 0.45 mass%, Ni is contained at a concentration D in the range of 3.00 mass% to 5.00 mass%, Mn is contained at a concentration E in the range of 0.05 mass% to 1.00 mass%, and Cu is contained at a concentration F in the range of 3.00 mass% to 5.00 mass%. In this powder, the value of δ defined by the following formula (1) is 10.0 mass% to 14.0 mass%.

[0013] δ=3(A+1.5B+0.5C)-2.8(D+0.5E+0.5F)-19.8 ··· (1)

[0014] Such a precipitation hardening stainless steel powder can suppress sinterability while maintaining the excellent mechanical strength derived from the precipitation hardening stainless steel. Therefore, the temperature at which sintering starts can be increased in the firing process. As a result, the organic binder remaining in the compact can be more reliably removed, and an increase in the carbon atom concentration in the sintered body can be suppressed. Therefore, the precipitation hardening stainless steel powder according to the embodiment can produce a sintered body with high mechanical strength.

[0015] The alloy composition of the precipitation hardening stainless steel powder according to the embodiment will be described in further detail below. In the following description, the precipitation hardening stainless steel powder may be simply referred to as "metal powder."

[0016] 1.1Cr Cr (chromium) is an element that mainly imparts corrosion resistance to the sintered body produced. By using a metal powder containing Cr, the corrosion resistance is increased, and a sintered body with good corrosion resistance can be obtained.

[0017] The Cr concentration A in the metal powder is 15.00% by mass or more and 17.50% by mass or less, preferably 15.20% by mass or more and 16.90% by mass or less, and more preferably 15.50% by mass or more and 16.70% by mass or less. If the Cr concentration A is below the lower limit, the corrosion resistance of the sintered body may be insufficient depending on the overall composition. On the other hand, if the Cr concentration A is above the upper limit, the sinterability may decrease and it may be difficult to increase the density of the sintered body depending on the overall composition, so that the corrosion resistance and mechanical properties of the sintered body may decrease. The mechanical properties of the sintered body refer to properties such as mechanical strength and hardness.

[0018] 1.2 Si Silicon (Si) is an element that mainly imparts corrosion resistance and high mechanical properties to the sintered body produced. By using metal powder containing Si, the corrosion resistance and mechanical properties are improved, resulting in a sintered body with good corrosion resistance.

[0019] The Si concentration B in the metal powder is 0.30% by mass or more and 1.00% by mass or less, preferably 0.35% by mass or more and 0.95% by mass or less, and more preferably 0.40% by mass or more and 0.90% by mass or less. If the Si concentration B is below the lower limit, the corrosion resistance, surface properties, and mechanical properties of the sintered body produced may be reduced depending on the overall composition. On the other hand, if the Si concentration B is above the upper limit, the composition balance may be easily lost depending on the overall composition, and the corrosion resistance, surface properties, and mechanical properties of the sintered body produced may be reduced. The surface properties of the sintered body refer to properties such as mirror finish and smoothness.

[0020] 1.3 Nb Nb (niobium) is an element that causes precipitates to form in the sintered compact to be produced, thereby improving the mechanical properties of the sintered compact. The Nb concentration C in the metal powder is 0.15% by mass or more and 0.45% by mass or less, preferably 0.20% by mass or more and 0.40% by mass or less, and more preferably 0.25% by mass or more and 0.35% by mass or less. If the Nb concentration C is below the lower limit, the precipitation of precipitates in the sintered body is restricted, and the mechanical properties of the sintered body may not be sufficiently improved. On the other hand, if the Nb concentration C exceeds the upper limit, the precipitates are excessively precipitated, the density of the sintered body decreases, and the mechanical properties of the sintered body are deteriorated.

[0021] 1.4 Ni Ni (nickel) is an element that mainly imparts corrosion resistance and heat resistance to the sintered body produced. By using metal powder containing Ni, the corrosion resistance and heat resistance are increased, resulting in a sintered body with good corrosion resistance and surface properties.

[0022] The Ni concentration D in the metal powder is 3.00% by mass or more and 5.00% by mass or less, preferably 3.50% by mass or more and 4.70% by mass or less, and more preferably 3.80% by mass or more and 4.50% by mass or less. If the Ni concentration D is below the lower limit, depending on the overall composition, the corrosion resistance and surface properties of the sintered body to be manufactured may not be sufficiently improved. On the other hand, if the Ni concentration D is above the upper limit, depending on the overall composition, the balance of the composition may be easily lost, and the corrosion resistance and surface properties of the sintered body to be manufactured may be deteriorated.

[0023] 1.5 Mn Manganese (Mn), like Si, is an element that imparts corrosion resistance and high mechanical properties to the sintered body. By using metal powder containing Mn, the corrosion resistance and mechanical properties are improved, resulting in a sintered body with good corrosion resistance and mechanical properties.

[0024] The Mn concentration E in the metal powder is not particularly limited, but is preferably 0.05% by mass to 1.00% by mass, more preferably 0.07% by mass to 0.50% by mass, and even more preferably 0.10% by mass to 0.40% by mass. If the Mn concentration E is below the lower limit, depending on the overall composition, the corrosion resistance, surface properties, and mechanical properties of the sintered body to be produced may not be sufficiently improved, while if the Mn concentration E exceeds the upper limit, the corrosion resistance, surface properties, and mechanical properties may be deteriorated.

[0025] 1.6 Cu Cu (copper) is an element that precipitates intermetallic compounds in the produced sintered compact and improves the mechanical properties of the sintered compact. The Cu concentration F in the metal powder is 3.00% by mass or more and 5.00% by mass or less, preferably 3.10% by mass or more and 4.50% by mass or less, and more preferably 3.20% by mass or more and 4.20% by mass or less. If the Cu concentration F is below the lower limit, the precipitation of intermetallic compounds in the sintered body is restricted, and the mechanical properties of the sintered body may not be sufficiently improved. On the other hand, if the Cu concentration F is above the upper limit, the intermetallic compounds are excessively precipitated, the density of the sintered body decreases, and the mechanical properties of the sintered body are deteriorated.

[0026] 1.7 Value of δ In the precipitation hardening stainless steel powder according to this embodiment, the value of δ defined by the following formula (1) is 10.0 mass % or more and 14.0 mass % or less. δ=3(A+1.5B+0.5C)-2.8(D+0.5E+0.5F)-19.8 ··· (1)

[0027] The value of δ defined by such formula (1) can suppress the sinterability of the precipitation hardening stainless steel powder without impairing the mechanical properties of the sintered body produced using the precipitation hardening stainless steel powder. Specifically, the first term on the right side of formula (1) is a term related mainly to elements that form ferrite, and the second term is a term related mainly to elements that form austenite. Ferrite has a faster diffusion rate during sintering than austenite, and therefore contributes to increasing the sinterability of the precipitation hardening stainless steel powder.

[0028] In view of this, in the present embodiment, the ratio of the concentration of the element that forms ferrite to the concentration of the element that forms austenite is optimized based on formula (1), thereby suppressing the sinterability in the obtained sintered body while maintaining the excellent mechanical strength derived from the precipitation hardened stainless steel. More specifically, by setting the value of δ defined by formula (1) within the above range, it is possible to suppress the sinterability of the precipitation hardened stainless steel powder while maintaining the mechanical strength of the sintered body, and to slow down the diffusion rate compared to the conventional method. This makes it possible to further increase the temperature at which the sintering of the metal powder starts when the compact is subjected to a sintering treatment. As a result, it is possible to more reliably remove the organic binder remaining in the compact before the metal powder starts sintering.

[0029] Note that removal of the organic binder refers to, for example, the volatilization of the organic binder or its decomposition products, or the reaction of carbon atoms contained in the organic binder with oxygen atoms contained in the metal powder or oxygen atoms adsorbed to the metal powder, and the volatilization of the reaction products.

[0030] Here, the organic binder contains carbon atoms because it is mainly made of an organic compound. If the organic binder in the compact cannot be sufficiently removed, more carbon atoms than before will remain in the sintered body, which may reduce the mechanical strength of the sintered body. In contrast, in this embodiment, the sinterability of the precipitation hardening stainless steel powder is suppressed, thereby making it possible to increase the efficiency of removing the organic binder in the sintering process. This makes it possible to suppress the carbon atom concentration in the sintered body, making it possible to manufacture a sintered body with high mechanical strength.

[0031] The value of δ is set to 10.0 mass% or more and 14.0 mass% or less, preferably 10.5 mass% or more and 13.5 mass% or less, and more preferably 11.0 mass% or more and 13.0 mass% or less. When the value of δ is below the lower limit, the concentration of elements that form austenite increases. In this case, although the sinterability of the precipitation hardened stainless steel powder decreases, the sinterability tends to become too low, making it difficult to increase the density of the sintered body. This leads to a decrease in the mechanical strength of the resulting sintered body. On the other hand, when the value of δ exceeds the upper limit, the concentration of elements that form ferrite increases. In this case, the sinterability of the precipitation hardened stainless steel powder becomes too high, and the carbon atom concentration in the resulting sintered body increases. This leads to a decrease in the mechanical strength of the sintered body.

[0032] 1.8 Fe Among the elements contained in the precipitation hardening stainless steel powder according to the embodiment, Fe (iron) is the element with the highest content, i.e., the main component, and has a large effect on the properties of the sintered body produced. The Fe content is not particularly limited, but is preferably 50 mass% or more, and more preferably 60 mass% or more.

[0033] 1.9 Other elements The precipitation hardening stainless steel powder according to the embodiment may contain at least one of C, Mo, W, N, S and P in addition to the above-mentioned elements, if necessary.

[0034] C (carbon) is an element that acts as an interstitial element to cause solid solution hardening in the sintered body to be manufactured, and causes precipitation hardening through precipitates containing C or other elements. By using a metal powder containing C, a sintered body with high mechanical properties can be obtained. On the other hand, if the concentration of C, i.e., the carbon atom concentration, is too high, the mechanical properties of the sintered body, such as hardness, decrease. The C concentration in the metal powder is set to 0.07% by mass or less, preferably 0.01% by mass or more and 0.05% by mass or less. If the C concentration exceeds the upper limit, depending on the overall composition, the composition balance is likely to be lost, and the mechanical properties of the sintered body to be produced may be deteriorated.

[0035] Mo (molybdenum) is an element that enhances the corrosion resistance of the sintered body produced. The Mo concentration in the metal powder is not particularly limited, but is preferably 1.00 mass% or less, and more preferably 0.01 mass% or more and 0.50 mass% or less. By setting the Mo concentration within the above range, the corrosion resistance of the sintered body can be further enhanced without causing a significant decrease in the density of the sintered body to be produced.

[0036] W (tungsten) is an element that enhances the heat resistance of the sintered body to be produced. The W concentration in the metal powder is not particularly limited, but is preferably 1.00 mass% or less, and more preferably 0.01 mass% or more and 0.50 mass% or less. By setting the W concentration within the above range, the heat resistance of the sintered body to be produced can be further enhanced without causing a significant decrease in the density of the sintered body.

[0037] N (nitrogen) is an element that improves the mechanical properties such as the yield strength of the produced sintered body. The N concentration in the metal powder is not particularly limited, but is preferably 1.00 mass% or less, more preferably 0.001 mass% or more and 0.50 mass% or less, and even more preferably 0.05 mass% or more and 0.30 mass% or less. By setting the N concentration within the above range, it is possible to further improve the mechanical properties of the sintered body, such as the yield strength, without causing a significant decrease in the density of the sintered body to be produced.

[0038] To manufacture metal powder containing added N, for example, a method of using a nitrided raw material, a method of introducing nitrogen gas into molten metal, a method of subjecting manufactured metal powder to a nitriding treatment, etc. are used.

[0039] S (sulfur) is an element that enhances the machinability of the produced sintered body. The concentration of S in the metal powder is not particularly limited, but is preferably 0.50% by mass or less, and more preferably 0.001% by mass to 0.30% by mass. By setting the concentration of S within the above range, the machinability of the sintered body to be produced can be improved without causing a significant decrease in the density of the sintered body to be produced.

[0040] P (phosphorus) is an element that acts as an interstitial element to cause solid solution hardening in the sintered body to be manufactured, and causes precipitation hardening by forming precipitates in combination with other elements. By using metal powder containing P, sintered bodies with high mechanical properties can be obtained.

[0041] The P concentration in the metal powder is 0.50% by mass or less, preferably 0.001% by mass to 0.35% by mass or less, and more preferably 0.005% by mass to 0.30% by mass or less. If the P concentration is below the lower limit, depending on the overall composition, the mechanical properties of the sintered body may not be sufficiently improved even if P is added. On the other hand, if the P concentration exceeds the upper limit, depending on the overall composition, the balance of the composition may be easily lost, and the mechanical properties of the sintered body produced may be reduced.

[0042] O (oxygen) may be intentionally added or may be unavoidably contained, but its concentration is preferably 0.01% by mass or more and 0.70% by mass or less, and more preferably 0.15% by mass or more and 0.60% by mass or less. By keeping the O concentration in the metal powder within this range, silicon oxide precipitates on the particle surfaces of the metal powder, thereby suppressing the oxidation of elements such as Mn and Cr. As a result, the corrosion resistance and surface properties of the sintered body finally produced can be improved. If the O content falls below the lower limit, the amount of silicon oxide precipitated is reduced, which may cause oxidation of elements such as Mn and Cr. In this case, the corrosion resistance, surface properties, and mechanical properties of the sintered body produced may be degraded. On the other hand, if the O content exceeds the upper limit, oxides of Mn and Cr are also generated at the time of producing the metal powder in addition to silicon oxide. This makes it difficult to increase the density of the sintered body produced, which may result in a decrease in corrosion resistance, surface properties, and mechanical properties.

[0043] Moreover, the O concentration is more preferably 0.20% by mass or more and 0.55% by mass or less, and particularly preferably 0.33% by mass or more and 0.53% by mass or less. By keeping the O concentration in the metal powder within this range, in addition to the above effects, oxygen atoms in the metal powder can react with carbon atoms derived from the organic binder. For example, when oxygen atoms in the metal powder exist as silicon oxide, oxygen atoms and carbon atoms can be removed from the sintered body by the reaction represented by the following formula (2). SiO2+2C→Si+2CO↑ (2) By such a reaction, the carbon atoms derived from the organic binder can be consumed and removed using oxygen atoms. Therefore, by including a predetermined amount of oxygen atoms, the concentration of carbon atoms derived from the organic binder remaining in the sintered body can be suppressed.

[0044] If the O concentration is below the lower limit, the carbon atoms in the sintered body may not be consumed sufficiently, whereas if the O concentration is above the upper limit, the composition balance may be easily lost, and the mechanical strength and corrosion resistance of the sintered body may be reduced.

[0045] In addition to the above elements, the precipitation hardening stainless steel powder may contain H, Be, B, Al, Co, As, Sn, Se, Zr, Y, Ti, Hf, Ta, Te, Pb, etc. to improve the properties of the sintered body. In this case, the concentrations of these elements are not particularly limited, but are set to a level that does not impair the properties of the sintered body described above, and are preferably less than 0.1 mass% each, and preferably less than 0.2 mass% in total. Note that these elements may be unavoidably contained.

[0046] Furthermore, the precipitation hardening stainless steel powder may contain unavoidable impurities. Examples of impurities include all elements other than those mentioned above. The concentration of each of these impurities may be less than the respective concentrations of Fe, Cr, Si, Nb, Ni, Mn, and Cu. In particular, the concentration of each of these impurities is preferably less than 0.03 mass%, and the total concentration of the impurities is preferably less than 0.30 mass%. Note that these impurities may be intentionally added so long as their concentrations are within the above ranges, since the effects described above are not hindered.

[0047] The tap density of the precipitation hardening stainless steel powder is 3.5 g / cm 3 More than 5.5g / cm 3 Preferably, it is 4.0 g / cm or less. 3 More than 5.0g / cm 3 It is more preferable that the precipitation hardening stainless steel powder is equal to or less than 100%. When a compact is obtained from such a precipitation hardening stainless steel powder, the packing between particles is particularly high. As a result, a particularly dense sintered body can be obtained in the end.

[0048] The specific surface area of ​​precipitation hardening stainless steel powder is 0.10 m 2 / g or more 0.70m 2 / g or less, and 0.15m 2 / g or more 0.50m 2 / g or less is more preferable. With such a precipitation hardening stainless steel powder, the surface activity (surface energy) is optimized, and appropriate sinterability is obtained. This makes it possible to obtain a sufficient sintering rate while suppressing the organic binder, its decomposition products, and the reaction products of carbon atoms from remaining in the sintered body. As a result, a dense sintered body can be obtained while reducing the carbon atom concentration.

[0049] 1.10 Analysis method The composition ratio of the precipitation hardening stainless steel powder according to the embodiment can be determined by, for example, iron and steel-atomic absorption spectrometry as specified in JIS G 1257:2000, iron and steel-ICP optical emission spectrometry as specified in JIS G 1258:2007, iron and steel-spark discharge optical emission spectrometry as specified in JIS G 1253:2002, iron and steel-fluorescent X-ray analysis as specified in JIS G 1256:1997, and gravimetry, titration and absorptiometry as specified in JIS G 1211 to G 1237. Specific examples of the method include a spark discharge optical emission spectrometry analyzer manufactured by SPECTRO, Inc., model: SPECTROLAB, type: LAVMB08A, and an ICP device manufactured by Rigaku Corporation, CIROS120 type.

[0050] In addition, JIS G 1211 to G 1237 are as follows. JIS G 1211:2011 Iron and steel - Carbon determination method JIS G 1212:1997 Iron and steel-Determination of silicon JIS G 1213:2001 Method for determining manganese in iron and steel JIS G 1214:1998 Iron and steel-Determination of phosphorus JIS G 1215:2010 Iron and steel-Determination of sulfur JIS G 1216:1997 Iron and steel - Nickel determination method JIS G 1217:2005 Iron and steel - Chromium determination method JIS G 1218:1999 Iron and steel-Determination of molybdenum JIS G 1219:1997 Iron and steel - Copper determination method JIS G 1220:1994 Iron and steel - Method for quantitative determination of tungsten JIS G 1221:1998 Iron and steel-Determination of vanadium JIS G 1222:1999 Iron and steel-Determination of cobalt JIS G 1223:1997 Iron and steel - Titanium quantitative determination method JIS G 1224:2001 Method for determining aluminum in iron and steel JIS G 1225:2006 Iron and steel-Determination of arsenic JIS G 1226:1994 Iron and steel-Determination of tin JIS G 1227:1999 Method for determining boron in iron and steel JIS G 1228:2006 Iron and steel - Determination of nitrogen JIS G 1229:1994 Steel-lead determination method JIS G 1232:1980 Method for determining zirconium in steel JIS G 1233:1994 Steel - Method for determining selenium JIS G 1234:1981 Method for determining tellurium in steel JIS G 1235:1981 Method for determining antimony in iron and steel JIS G 1236:1992 Method for determining tantalum in steel JIS G 1237:1997 Iron and steel-Determination of niobium

[0051] In addition, when identifying C (carbon) and S (sulfur), the oxygen flow combustion high-frequency induction heating furnace combustion-infrared absorption method specified in JIS G 1211: 2011 is also used. A specific analytical device is the LECO carbon-sulfur analyzer, CS-200. Furthermore, when specifying N (nitrogen) and O (oxygen), the nitrogen determination method for iron and steel specified in JIS G 1228: 2006 and the oxygen determination method for metal materials specified in JIS Z 2613: 2006 are also used. Specific analytical devices include the LECO oxygen / nitrogen analyzer, TC-300 / EF-300.

[0052] In addition, a sintered body manufactured using the precipitation hardening stainless steel powder according to the embodiment can be subjected to various heat treatments to precipitate a martensite crystal structure. The martensite crystal structure imparts high hardness to the sintered body. Whether or not the sintered body has a martensite crystal structure can be determined by, for example, X-ray diffraction.

[0053] The average particle size of the precipitation hardening stainless steel powder is preferably 0.50 μm to 50.00 μm, more preferably 1.00 μm to 30.00 μm, and even more preferably 2.00 μm to 10.00 μm. By using precipitation hardening stainless steel powder with such a particle size, the number of voids remaining in the sintered body is extremely reduced, making it possible to produce a sintered body that is high in density and has excellent mechanical properties. If the average particle size of the precipitation hardening stainless steel powder is below the lower limit, the moldability may decrease when forming a shape that is difficult to form, and the sintered density may decrease. On the other hand, if the average particle size of the precipitation hardening stainless steel powder is above the upper limit, the gaps between the particles may become large during forming, and the sintered density may decrease. The average particle size of the precipitation hardening stainless steel powder is determined as the particle size at which the cumulative amount from the small diameter side is 50% in the cumulative particle size distribution on a mass basis obtained by laser diffraction method.

[0054] The maximum particle size of the precipitation hardening stainless steel powder is not particularly limited as long as the average particle size is within the above range, but is preferably 200 μm or less, and more preferably 150 μm or less. By controlling the maximum particle size of the precipitation hardening stainless steel powder within the above range, the particle size distribution of the precipitation hardening stainless steel powder can be narrowed further, and the sintered body can be made even denser. The maximum particle size mentioned above refers to the particle size at which the cumulative amount from the small diameter side is 99.9% in the cumulative particle size distribution on a mass basis obtained by a laser diffraction method.

[0055] When the minor axis of the particles of the precipitation hardening stainless steel powder is S [μm] and the major axis is L [μm], the average aspect ratio defined by S / L is preferably about 0.4 to 1, more preferably about 0.7 to 1. Precipitation hardening stainless steel powder with such an aspect ratio has a shape relatively close to a sphere, which increases the packing rate when compacted. As a result, the sintered body can be made even denser.

[0056] The major axis is the maximum length that a particle can have in a projected image, and the minor axis is the maximum length that a particle can have in a direction perpendicular to the major axis. The average aspect ratio is the average value of aspect ratios measured for 100 or more particles.

[0057] 2. Manufacturing method of sintered precipitation hardening stainless steel Next, a method for producing a precipitation hardening stainless steel sintered body according to an embodiment will be described. FIG. 1 is a process diagram showing a method for producing a precipitation hardened stainless steel sintered body according to an embodiment. The method for producing a precipitation hardened stainless steel sintered body shown in Fig. 1 includes a composition preparation step S1 for preparing a composition for producing the sintered body, a molding step S2 for molding the composition, a degreasing step S3 for degreasing the molded body, and a firing step S4 for firing the degreased body. Each step will be described below in order.

[0058] 2.1 Composition preparation process S1 First, the precipitation hardening stainless steel powder and the organic binder are kneaded with a kneader to obtain a kneaded product, i.e., the compound according to the embodiment. The kneaded product is a composition containing the above-mentioned precipitation hardening stainless steel powder and the organic binder. With such a kneaded product, it is possible to manufacture a sintered body having high mechanical strength, even though an organic binder is used.

[0059] The precipitation hardening stainless steel powder is produced by various powdering methods, such as atomizing methods such as water atomizing, gas atomizing, and high-speed rotating water jet atomizing, reduction methods, carbonyl methods, and pulverization methods.

[0060] Of these, the precipitation hardening stainless steel powder is preferably produced by the atomization method, and more preferably by the water atomization method or the high-speed rotating water flow atomization method. The atomization method is a method for producing metal powder by colliding molten metal with a liquid or gas sprayed at high speed, pulverizing it and cooling it. By producing the precipitation hardening stainless steel powder by such an atomization method, extremely fine powder can be produced efficiently. In addition, the particle shape of the obtained powder becomes close to a spherical shape due to the action of surface tension. Therefore, when molded, a product with a high filling rate can be obtained. In other words, a powder that can be used to produce a high-density sintered body can be obtained.

[0061] When the water atomization method is used as the atomization method, the pressure of the water sprayed toward the molten metal is not particularly limited, but is preferably about 75 MPa or more and 120 MPa or less, and more preferably about 90 MPa or more and 120 MPa or less. The temperature of the atomized water is not particularly limited, but is preferably about 1° C. or higher and 20° C. or lower. Furthermore, the atomized water is often sprayed in a cone shape with an apex on the falling path of the molten metal and an outer diameter that gradually decreases downward. In this case, the apex angle θ of the cone formed by the atomized water is preferably about 10° to 40°, and more preferably about 15° to 35°. This makes it possible to reliably produce the precipitation hardening stainless steel powder having the composition described above.

[0062] Furthermore, water atomization, particularly high-speed rotating water jet atomization, allows the molten metal to be cooled particularly quickly, which makes it possible to obtain high-quality powder over a wide range of alloy compositions. The cooling rate for cooling the molten metal in the atomization method is 1×10 4 °C / s or more, and preferably 1×10 5 It is more preferable that the cooling rate is ℃ / s or more. Such rapid cooling allows homogeneous precipitation hardening stainless steel powder to be obtained. As a result, a high quality sintered body can be obtained.

[0063] The precipitation hardening stainless steel powder thus obtained may be classified as necessary. Examples of the classification method include dry classification such as sieving classification, inertial classification, and centrifugal classification, and wet classification such as sedimentation classification.

[0064] As the organic binder, a resin that can be decomposed in a short time during degreasing or baking is used. Examples of such resins include polyolefins such as polyethylene, polypropylene, and ethylene-vinyl acetate copolymers, acrylic resins such as polymethyl methacrylate and polybutyl methacrylate, styrene resins such as polystyrene, polyesters such as polyvinyl chloride, polyvinylidene chloride, polyamide, polyethylene terephthalate and polybutylene terephthalate, polyethers, polyvinyl alcohol, polyvinylpyrrolidone, or copolymers thereof, various waxes, paraffins, higher fatty acids, higher alcohols, higher fatty acid esters, and higher fatty acid amides, and one or more of these may be used in combination.

[0065] The mixing ratio of the organic binder is preferably about 2% by mass or more and 20% by mass or less of the entire kneaded product, and more preferably about 5% by mass or more and 15% by mass or less. By having the mixing ratio of the organic binder within the above range, a molded body can be formed with good moldability, and the density can be increased, and the shape stability of the molded body can be particularly excellent. In addition, this makes it possible to optimize the difference in size between the molded body and the degreased body, that is, the shrinkage rate, and prevent a decrease in the dimensional accuracy of the sintered body finally obtained. In other words, a sintered body with high density and dimensional accuracy can be obtained.

[0066] In addition, a plasticizer may be added to the kneaded material as necessary. Examples of the plasticizer include phthalic acid esters, adipic acid esters, trimellitic acid esters, and sebacic acid esters, and one or more of these may be mixed and used. Furthermore, in addition to the precipitation hardening stainless steel powder, organic binder, and plasticizer, various additives such as lubricants, antioxidants, degreasing accelerators, surfactants, other metal powders, ceramic powders, etc. may be added to the kneaded product as necessary.

[0067] The kneading conditions vary depending on various conditions such as the alloy composition and particle size of the precipitation hardening stainless steel powder used, the composition of the organic binder, and the amounts of these mixed, but an example can be a kneading temperature of approximately 50°C or higher and 200°C or lower, and a kneading time of approximately 15 minutes or higher and 210 minutes or lower. The kneaded product is pelletized as necessary. The particle size of the pellets is, for example, about 1 mm or more and 15 mm or less.

[0068] In addition, depending on the molding method described later, the granulated powder according to the embodiment may be used instead of the kneaded mixture. These kneaded mixtures and granulated powders are examples of compositions to be subjected to the molding step described later.

[0069] The granulated powder is obtained by subjecting a precipitation hardened stainless steel powder to a granulation process, so that a plurality of metal particles are bound together by an organic binder. That is, the granulated powder is a composition containing the above-mentioned precipitation hardened stainless steel powder and an organic binder. With such a granulated powder, it is possible to produce a sintered body having high mechanical strength, even though an organic binder is used.

[0070] The organic binder used in the production of the granulated powder may be, for example, the organic binders described above.

[0071] The mixing ratio of the organic binder is preferably about 0.2% by mass or more and 10% by mass or less of the total granulated powder, and more preferably about 0.3% by mass or more and 5.0% by mass or less. By setting the mixing ratio of the organic binder within the above range, it is possible to efficiently form the granulated powder while suppressing the granulation of extremely large particles and the remaining of a large amount of ungranulated metal particles. In addition, since the moldability is improved, the shape stability of the molded body can be particularly excellent. In addition, by setting the mixing ratio of the organic binder within the above range, the difference in size between the molded body and the degreased body, that is, the so-called shrinkage rate, can be optimized, and the dimensional accuracy of the finally obtained sintered body can be prevented from decreasing.

[0072] Furthermore, in addition to the precipitation hardening stainless steel powder, organic binder, and plasticizer, the granulated powder may contain various additives such as a lubricant, an antioxidant, a degreasing accelerator, and a surfactant, as well as other metal powders and ceramic powders.

[0073] Examples of the granulation process include spray drying, tumbling granulation, fluidized bed granulation, and tumbling fluidized bed granulation. In the granulation process, a solvent that dissolves the binder is used as necessary. Examples of such solvents include inorganic solvents such as water and carbon tetrachloride, and organic solvents such as ketone solvents, alcohol solvents, ether solvents, cellosolve solvents, aliphatic hydrocarbon solvents, aromatic hydrocarbon solvents, aromatic heterocyclic compound solvents, amide solvents, halogenated compound solvents, ester solvents, amine solvents, nitrile solvents, nitro solvents, and aldehyde solvents, and one or a mixture of two or more selected from these solvents is used.

[0074] The average particle size of the granulated powder is not particularly limited, but is preferably about 10 μm to 200 μm, more preferably about 20 μm to 100 μm, and even more preferably about 25 μm to 60 μm. Granulated powder with such a particle size has good flowability and can more faithfully reflect the shape of the mold. The average particle size is determined as the particle size at which the cumulative amount from the small diameter side is 50% in the cumulative particle size distribution on a mass basis obtained by laser diffraction method.

[0075] 2.2 Molding process S2 Next, the kneaded mixture or granulated powder is molded to produce a molded body having the same shape as the desired sintered body. Examples of the molding method include powder compaction, metal powder injection molding, and extrusion molding.

[0076] Of these, the molding conditions in the case of powder compaction method vary depending on various conditions such as the composition and particle size of the precipitation hardening stainless steel powder used, the composition of the organic binder, and the amounts of these mixed, but it is preferable that the molding pressure be approximately 200 MPa or more and 1000 MPa or less.

[0077] Furthermore, the molding conditions in the case of metal powder injection molding vary depending on various conditions, but it is preferable that the material temperature is about 80° C. or more and 210° C. or less, and the injection pressure is about 50 MPa or more and 500 MPa or less.

[0078] In the case of extrusion molding, the molding conditions vary depending on various conditions, but it is preferable that the material temperature is about 80° C. or more and 210° C. or less, and the extrusion pressure is about 50 MPa or more and 500 MPa or less. The shape and dimensions of the green body to be produced are determined taking into account the shrinkage of the green body during the debinding and firing steps described below.

[0079] 2.3 Degreasing process S3 Next, the obtained green body is subjected to a degreasing treatment to obtain a degreased body. Specifically, the degreasing treatment is performed by decomposing and removing the organic binder. Examples of the degreasing treatment include a method of heating the molded body and a method of exposing the molded body to a gas that decomposes the organic binder.

[0080] When the method of heating the molded body is used, the heating conditions of the molded body vary slightly depending on the composition and amount of the organic binder, but are preferably at a temperature of 100°C to 750°C x 0.1 to 20 hours, and more preferably at a temperature of 150°C to 600°C x 0.5 to 15 hours. This allows the molded body to be degreased as necessary and sufficiently without sintering it. As a result, it is possible to prevent a large amount of organic binder components from remaining inside the degreased body.

[0081] The atmosphere in which the molded body is heated is not particularly limited, and examples of the atmosphere include a reducing gas atmosphere such as hydrogen, an inert gas atmosphere such as nitrogen or argon, an oxidizing gas atmosphere such as air, or a reduced pressure atmosphere obtained by reducing the pressure of these atmospheres.

[0082] On the other hand, as a method of exposing a molded body to a gas that decomposes an organic binder, for example, an acid degreasing method is used. The acid degreasing method is a method of degreasing a molded body by heating the molded body in an acid-containing atmosphere and utilizing the catalytic action of the acid. According to the acid degreasing method, the organic binder can be decomposed in a short time even at a low temperature, so that even a molded body with a large volume can be efficiently degreased.

[0083] The acid-containing atmosphere refers to an atmosphere containing an acid capable of decomposing an organic binder. Examples of such acids include nitric acid, oxalic acid, ozone, etc., and one or more of these can be used in combination. In addition, a mixed gas obtained by mixing these acids with other gases may be used. An example of the mixed gas is fuming nitric acid. The atmospheric pressure may be atmospheric pressure, reduced pressure, or pressurized.

[0084] The heating conditions for the molded body vary slightly depending on the composition and amount of the organic binder and the type of acid-containing atmosphere, but are preferably at a temperature of 100°C to 750°C for 0.1 to 20 hours, and more preferably at a temperature of 150°C to 600°C for 0.5 to 15 hours. This allows the molded body to be degreased in a short time even at a relatively low temperature. In addition, the molded body can be prevented from being sintered or oxidized.

[0085] Incidentally, such a debinding step may be carried out in a plurality of separate steps with different debinding conditions, so that the binder in the green body can be decomposed and removed more quickly and without remaining in the green body. If necessary, the degreased body may be subjected to mechanical processing such as cutting, grinding, and cutting. Since the degreased body has a relatively low hardness and is relatively plastic, it can be easily machined while preventing the shape of the degreased body from being distorted. By such machining, a sintered body with high dimensional accuracy can be easily obtained.

[0086] 2.4 Firing process S4 Next, the obtained degreased body is subjected to a sintering treatment. The sintering treatment causes surface diffusion at the interfaces between the particles of the precipitation hardened stainless steel powder, which leads to sintering. As a result, a sintered body is obtained.

[0087] The firing temperature varies depending on the composition and particle size of the precipitation hardening stainless steel powder used to manufacture the compact and the degreased body, but is, for example, about 980° C. to 1330° C., and preferably about 1050° C. to 1260° C. The firing time is from 0.2 hours to 7 hours, and preferably from 1 hour to 6 hours.

[0088] In the firing step, the firing temperature or the firing atmosphere, which will be described later, may be changed midway. By setting the sintering conditions within these ranges, it is possible to sinter the entire degreased body sufficiently while preventing oversintering, which would otherwise cause the crystal structure to become enlarged, and as a result, it is possible to obtain a sintered body that is high in density and has excellent mechanical properties.

[0089] The sintered body thus produced may be subjected to additional treatments as necessary, such as solution treatment, age hardening, double aging, sub-zero treatment, tempering, hot working, and cold working, and one or more of these may be used in combination.

[0090] A specific example of the above-mentioned additional treatment is a solution treatment in which the steel is cooled from a temperature of 1000°C or higher and 1250°C or lower for a period of 30 minutes or longer and 120 minutes or shorter, followed by an age hardening treatment in which the steel is cooled from a temperature of 600°C or higher and 800°C or lower for a period of 6 hours or longer and 48 hours or shorter.

[0091] 3. Precipitation hardening stainless steel sintered body As described above, the precipitation hardening stainless steel sintered body according to the present embodiment is a sintered body made of precipitation hardening stainless steel containing Cr, Si, Nb, Ni, Mn and Cu. In the sintered body, Cr is contained at a concentration A in the range of 15.00 mass% to 17.50 mass%, Si is contained at a concentration B in the range of 0.30 mass% to 1.00 mass%, Nb is contained at a concentration C in the range of 0.15 mass% to 0.45 mass%, Ni is contained at a concentration D in the range of 3.00 mass% to 5.00 mass%, Mn is contained at a concentration E in the range of 0.05 mass% to 1.00 mass%, and Cu is contained at a concentration F in the range of 3.00 mass% to 5.00 mass%. In addition, in the sintered body, the value of δ defined by the following formula (1) is 10.0 mass% to 14.0 mass%. δ=3(A+1.5B+0.5C)-2.8(D+0.5E+0.5F)-19.8 ··· (1) According to such a precipitation hardening stainless steel sintered body, an increase in the carbon atom concentration is suppressed, and therefore a sintered body having high mechanical strength derived from the precipitation hardening stainless steel can be obtained. In particular, even when the sintered body is small or has a complex shape, the residual carbon atoms derived from the organic binder are suppressed, and a high-quality sintered body can be obtained.

[0092] The precipitation hardening stainless steel sintered body can be used as a material for constituting all or part of, for example, automobile parts, bicycle parts, railway vehicle parts, ship parts, aircraft parts, and space transport vehicle parts; electronic device parts such as personal computer parts, mobile phone terminal parts, tablet terminal parts, and wearable terminal parts; electrical device parts such as refrigerators, washing machines, and air conditioners; machine parts such as machine tools and semiconductor manufacturing equipment; plant parts such as nuclear power plants, thermal power plants, hydroelectric power plants, refineries, and chemical complexes; watch parts, and decorative items such as metal tableware, jewelry, and eyeglass frames.

[0093] As described above, the method for producing a precipitation hardened stainless steel sintered body according to the present embodiment includes a molding step of molding a compound or granulated powder containing a precipitation hardened stainless steel powder to obtain a molded body, and a sintering step of sintering the molded body to obtain a sintered body. In such a manufacturing method, the carbon atom concentration in the sintered body is preferably lower than that in the precipitation hardened stainless steel powder. This is because the carbon atom concentration in the sintered body is reduced by the reaction between carbon atoms and oxygen atoms as described above. By reducing the carbon atom concentration in the sintered body in this way, the carbon atom concentration in the sintered body can be kept within the above-mentioned range even when a precipitation hardened stainless steel powder with a high carbon atom concentration is used. This allows a sintered body with high mechanical strength to be efficiently manufactured.

[0094] In addition, when the carbon atom concentration in the precipitation hardening stainless steel powder is the first concentration c1 and the carbon atom concentration in the sintered body is the second concentration c2, (c1-c2) / c1 is preferably 70 mass% or less, more preferably 50 mass% or less. This makes it possible to reliably reduce the first concentration c1, thereby increasing the probability that the second concentration c2 will be within the aforementioned range. As a result, it is possible to more reliably manufacture a sintered body with high mechanical strength, hardness, and corrosion resistance derived from the precipitation hardening stainless steel.

[0095] The precipitation hardening stainless steel powder, compound, granulated powder, precipitation hardening stainless steel sintered body, and the manufacturing method thereof according to the present invention have been described above based on preferred embodiments, but the present invention is not limited to these. For example, any additive may be added to the compound and granulated powder. The method for producing a precipitation hardened stainless steel sintered body of the present invention may be obtained by adding any step for any purpose to the above-described embodiment.

[0096] Next, an embodiment of the present invention will be described. 4. Manufacturing of sintered bodies (Sample No. 1) [1] First, precipitation hardening stainless steel powder with the composition shown in Table 1 was prepared by water atomization. The composition of the metal powders shown in Table 1 was identified and quantified using inductively coupled plasma emission spectrometry and a Rigaku Corporation ICP instrument, CIROS120. The carbon and sulfur analyzer, CS-200, manufactured by LECO, was used to identify and quantify C. The oxygen and nitrogen analyzers, TC-300 / EF-300, manufactured by LECO, were used to identify and quantify O.

[0097] [2] Next, the metal powder and the organic binder were weighed and mixed in a mass ratio of 89:11 to obtain a mixed raw material. The organic binder used was a resin obtained by mixing a polyacetal resin containing 2.5 mass% butanediol and polyethylene in a mass ratio of 50:6. [3] Next, the mixed raw materials were kneaded in a kneader to obtain a compound. [4] Next, this compound was molded in an injection molding machine under the molding conditions shown below to produce a molded body. <Molding conditions> ·Material temperature: 180℃ Injection pressure: 11MPa (110kgf / cm 2 )

[0098] [5] Next, the obtained green body was subjected to a degreasing treatment under the degreasing conditions shown below to obtain a degreasing body. <Degreasing conditions> ·Degreasing temperature: 400℃ Degreasing time: 1 hour (holding time at degreasing temperature) Degreasing atmosphere: A mixed gas atmosphere of nitrogen and nitric acid, with a nitric acid concentration of 2% by volume

[0099] [6] Next, the obtained degreased body was subjected to a sintering treatment under the sintering conditions shown below to obtain a sintered body. The shape of the sintered body was a cylinder with a diameter of 10 mm and a thickness of 5 mm. <Firing conditions> Firing temperature: 1300℃ Baking time: 3 hours (holding time at baking temperature) Firing atmosphere: Argon atmosphere

[0100] [7] Next, the obtained sintered body was subjected to solution treatment and age hardening treatment in this order under the conditions shown below. <Solution treatment conditions> ·Heating temperature: 1120℃ Heating time: 30 minutes ·Cooling method: water cooling <Age hardening treatment conditions> ·Heating temperature: 700℃ Heating time: 24 hours ·Cooling method: water cooling

[0101] (Sample No. 2 to 13) Except for changing the composition of the precipitation hardening stainless steel powder as shown in Table 1, sintered bodies were obtained in the same manner as in the case of sample No. 1. Note that the powder of sample No. 5 was produced by gas atomization. In Table 1, among the precipitation hardened stainless steel powders and sintered bodies of each sample number, those that correspond to the present invention are designated as "Examples", and those that do not correspond to the present invention are designated as "Comparative Examples". Although each sintered body contained a small amount of impurities, these are not included in Table 1.

[0102] 5. Evaluation of Precipitation Hardening Stainless Steel Powder and Sintered Body 5.1 Measurement of the average particle size of a powder The average particle size was measured for each powder sample No. shown in Table 1. The measurement results are shown in Table 1.

[0103] 5.2 Measurement of tapped density of powder The tap density was measured for each powder sample No. shown in Table 1. A powder property evaluation device, Powder Tester (registered trademark) PT-X, manufactured by Hosokawa Micron Corporation, was used to measure the tap density. The number of taps was 125. The measurement results are shown in Table 1. Furthermore, since the powder sample No. 5 had a large particle size, the tap density measurement was omitted.

[0104] 5.3 Measurement of the specific surface area of ​​powders The specific surface area was measured for each powder sample No. shown in Table 1. The specific surface area was measured using the BET method, using a BET specific surface area measuring device HM1201-010 manufactured by Mountec Co., Ltd. The amount of the sample was 5 g. The measurement results are shown in Table 1. Furthermore, since the powder sample No. 5 has a large particle size, the measurement of the specific surface area was omitted.

[0105] 5.4 Measurement of carbon atom concentration in sintered bodies The carbon atom concentration was measured for the sintered body of each sample number shown in Table 1. The measurement results are shown in Table 1.

[0106] 5.5 Evaluation of mechanical strength of sintered bodies Test pieces as specified in ISO 2740:2009 were cut out from the sintered body of each sample number shown in Table 1. The tensile strength of the test pieces was measured by the test method as specified in JIS Z 2241:2011. Next, the tensile strength measured for the sintered body of Sample No. 10 was set to 1, and the relative values ​​of the tensile strengths measured for the sintered bodies of each of the Examples and Comparative Examples were calculated. The calculated relative values ​​were then evaluated according to the following evaluation criteria.

[0107] <Evaluation criteria for tensile strength> A: Very high tensile strength (relative value greater than 1.1) B: High tensile strength (relative value is greater than 1 and less than 1.1) C: Low tensile strength (relative value is greater than 0.9 and less than 1) D: The tensile strength is very low (relative value is 0.9 or less) The evaluation results are shown in Table 1.

[0108] 5.6 Evaluation of hardness of sintered body For each sintered body of sample No. shown in Table 1, the Vickers hardness was measured. Next, the Vickers hardness measured for the sintered body of Sample No. 10 was set to 1, and the relative values ​​of the Vickers hardness measured for the sintered bodies of each of the Examples and Comparative Examples were calculated. The calculated relative values ​​were then evaluated according to the following evaluation criteria.

[0109] <Hardness evaluation criteria> A: Very high hardness (relative value > 1.1) B: High hardness (relative value is greater than 1 and less than 1.1) C: Low hardness (relative value is greater than 0.9 and less than 1) D: Very low hardness (relative value 0.9 or less) The evaluation results are shown in Table 1.

[0110] 5.7 Evaluation of relative density of sintered bodies The density of the sintered body of each sample No. shown in Table 1 was measured by a method based on Archimedes' method. The relative density of the sintered body was calculated from the measured density and the true density of the soft magnetic powder. Next, the calculated relative density was evaluated based on the following evaluation criteria.

[0111] <Relative density evaluation criteria> A: Relative density is 98.0% or more B: Relative density is less than 98.0% The evaluation results are shown in Table 1.

[0112] 5.8 Evaluation of corrosion resistance of sintered body The corrosion rate of the sintered body of each sample No. shown in Table 1 was measured in accordance with the sulfuric acid corrosion test method for stainless steel specified in JIS G 0591: 2012. Note that boiled 5 mass% sulfuric acid was used as the sulfuric acid. Next, the corrosion degree measured for the sintered compact of each sample No. was compared with the corrosion degree measured for the sintered compact of sample No. 10 (unit: g / m 2 / h) was set to 1. The calculated relative values ​​were then evaluated according to the following evaluation criteria.

[0113] <Corrosion resistance evaluation criteria> A: The relative corrosion rate of the sintered body is less than 0.75. B: The relative corrosion rate of the sintered body is 0.75 or more and less than 1.00. C: The relative corrosion rate of the sintered body is 1.00 or more and less than 1.25. D: The relative corrosion rate of the sintered body is 1.25 or more. The evaluation results are shown in Table 1.

[0114] [Table 1]

[0115] As is clear from Table 1, the sintered bodies of the examples had good mechanical strength, hardness and corrosion resistance. In addition, in each Example, the carbon atom concentration in the sintered body was lower than that in the powder, which suggests that in each Example, the reaction products of carbon atoms were efficiently removed during the sintering process, resulting in improved mechanical properties and improved corrosion resistance. In the above, a sintered body was obtained by using a molded body manufactured by injection molding using a compound containing precipitation hardening stainless steel powder. On the other hand, a sintered body was also obtained by using a molded body manufactured by pressure molding using a granulated powder containing precipitation hardening stainless steel powder. As a result, the same tendency as when a compound was used was observed. [Explanation of symbols]

[0116] S1...composition preparation process, S2...molding process, S3...degreasing process, S4...baking process

Claims

1. Cr is contained at a concentration A in the range of 15.00 mass% or more and 17.50 mass% or less, Si is contained at a concentration B in the range of 0.30 mass% or more and 1.00 mass% or less, Nb is contained at a concentration C in the range of 0.15 mass% or more and 0.45 mass% or less, Ni is contained at a concentration D in the range of 3.00 mass% or more and 5.00 mass% or less, Mn is contained at a concentration E in the range of 0.05 mass% or more and 1.00 mass% or less, Cu is contained at a concentration F in the range of 3.00 mass% or more and 5.00 mass% or less, The value of δ defined by the following formula (1) is 10.0 mass% or more and 13.5 mass% or less. The present invention relates to a precipitation hardening stainless steel powder. δ=3(A+1.5B+0.5C)-2.8(D+0.5E+0.5F)-19.8・ ...(1)

2. 2. The composition according to claim 1, wherein O is contained in a concentration ranging from 0.01% by mass to 0.70% by mass. Precipitation hardening stainless steel powder.

3. 3. The composition according to claim 2, wherein O is contained in a concentration ranging from 0.33% by mass to 0.53% by mass. Precipitation hardening stainless steel powder.

4. 4. Any one of claims 1 to 3, wherein the average particle size is 0.50 μm or more and 50.00 μm or less. Item 3. The precipitation hardening stainless steel powder according to item 1.

5. A precipitation hardening stainless steel powder according to any one of claims 1 to 4 and an organic binder. A compound comprising:

6. A precipitation hardening stainless steel powder according to any one of claims 1 to 4 and an organic binder. A granulated powder comprising:

7. Cr is contained at a concentration A in the range of 15.00 mass% or more and 17.50 mass% or less, Si is contained at a concentration B in the range of 0.30 mass% or more and 1.00 mass% or less, Nb is contained at a concentration C in the range of 0.15 mass% or more and 0.45 mass% or less, Ni is contained at a concentration D in the range of 3.00 mass% or more and 5.00 mass% or less, Mn is contained at a concentration E in the range of 0.05 mass% or more and 1.00 mass% or less, Cu is contained at a concentration F in the range of 3.00 mass% or more and 5.00 mass% or less, The value of δ defined by the following formula (1) is 10.0 mass% or more and 13.5 mass% or less. A precipitation hardening stainless steel sintered body characterized by the above. δ=3(A+1.5B+0.5C)-2.8(D+0.5E+0.5F)-19.8・ ...(1)

8. The compound according to claim 5 or the granulated powder according to claim 6 is molded to obtain a molded body. and sintering the molded body to obtain a sintered body; The carbon atom concentration in the sintered body is A method for producing a sintered body of precipitation hardening stainless steel, characterized in that the carbon atom concentration is smaller than that in .

Citation Information

Patent Citations

  • A method for producing a sintered component and a sintered component

    CN105829560A

  • Thermoplastic composition for manufacturing molded metal and manufacture thereof

    JP1992247802A

  • Precipitation hardening stainless steel powder and sintered body thereof

    JP2015175054A

  • Metal powder for powder metallurgy, compound, granulated powder and sintered body

    JP2016125124A

  • Metal powder for powder metallurgy, compound, granulated powder and sintered body

    JP2016128592A