Energy storage element
By optimizing the pore volume ratio in the negative electrode active material layer, the power storage element addresses electrolyte depletion in the positive electrode, reducing resistance increase at low temperatures and ensuring effective charge/discharge cycles.
Patent Information
- Application Number
- JP2020171761
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-12
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2040-10-12
AI Technical Summary
Energy storage elements experience a significant increase in resistance at low temperatures after charge/discharge cycles, particularly when a portion of the electrode body is pressed, due to electrolyte depletion in the positive electrode active material layer.
The power storage element is designed such that the ratio of pore volumes in the negative electrode active material layer satisfies the condition A/B ≤ 0.64, where A is the pore volume of pore diameters between 0.01 μm and less than X μm, and B is the pore volume of pore diameters between X μm and 20 μm, with X being the peak pore diameter of the positive electrode active material layer, ensuring sufficient electrolyte flow into the positive electrode layer.
This configuration reduces the rate of resistance increase at low temperatures by preventing electrolyte depletion in the positive electrode active material layer, thereby maintaining efficient charge/discharge performance.
Smart Images

Figure 0007552227000003 
Figure 0007552227000002 
Figure 0007552227000001
Abstract
Description
[Technical field]
[0001] The present invention relates to an energy storage element. [Background technology]
[0002] Due to their high energy density, non-aqueous electrolyte secondary batteries, typified by lithium ion secondary batteries, are widely used in electronic devices such as personal computers and communication terminals, automobiles, etc. In addition, as electricity storage elements other than non-aqueous electrolyte secondary batteries, capacitors such as lithium ion capacitors and electric double layer capacitors, electricity storage elements using electrolytes other than non-aqueous electrolytes, etc. are also widely used.
[0003] As an electric storage element, one having an electrode body in which a positive electrode having a positive electrode active material layer laminated on the surface of a positive electrode substrate and a negative electrode having a negative electrode active material layer laminated on the surface of a negative electrode substrate are stacked with an electrically insulating separator interposed therebetween is widely used. Such an electrode body is housed in a container together with an electrolyte to form an electric storage element (see Patent Documents 1 and 2). In addition, a secondary battery having a compression member that compresses a part of the surface of the electrode body is also known (see Patent Document 3). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2013-73761 A [Patent Document 2] JP 2017-69002 A [Patent Document 3] JP 2010-146759 A Summary of the Invention [Problem to be solved by the invention]
[0005] A storage element is required to have a life performance according to the expected usage environment. For example, in the case of a storage element that may be used at low temperatures, it is required that the resistance is unlikely to increase at low temperatures and the output is unlikely to decrease even if the element is repeatedly charged and discharged. However, in the case of a storage element in which at least a part of the electrode body is pressed, a significant increase in resistance at low temperatures after the charge and discharge cycles may occur.
[0006] An object of the present invention is to provide an electricity storage element in which at least a portion of an electrode assembly is pressed, and in which the rate of increase in resistance at low temperatures after charge / discharge cycles is reduced. [Means for solving the problem]
[0007] An energy storage element according to one aspect of the present invention comprises an electrode body having a positive electrode including a positive electrode active material layer and a negative electrode including a negative electrode active material layer, and an electrolyte, in which at least a portion of the electrode body is compressed in a discharged state and satisfies the following formula 1. A / B≦0.64 1 In formula 1, A is the pore volume of the negative electrode active material layer in the pore diameter range of 0.01 μm or more and less than X μm, B is the pore volume of the negative electrode active material layer in the pore diameter range of X μm or more and 20 μm or less, and X is the pore diameter that shows the maximum value in the pore diameter range of 0.01 μm or more and 20 μm or less in the Log differential pore volume distribution of the positive electrode active material layer. Effect of the Invention
[0008] According to one aspect of the present invention, it is possible to provide an energy storage element in which at least a portion of an electrode body is pressed, and in which the rate of increase in resistance at low temperatures after charge / discharge cycles is reduced. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a perspective view showing an embodiment of an energy storage element. [Diagram 2] FIG. 2 is a schematic diagram showing an embodiment of an electricity storage device configured by assembling a plurality of electricity storage elements. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] First, an overview of the energy storage element disclosed in this specification will be described.
[0011] An energy storage element according to one aspect of the present invention comprises an electrode body having a positive electrode including a positive electrode active material layer and a negative electrode including a negative electrode active material layer, and an electrolyte, in which at least a portion of the electrode body is compressed in a discharged state and satisfies the following formula 1. A / B≦0.64 1 In formula 1, A is the pore volume of the negative electrode active material layer in the pore diameter range of 0.01 μm or more and less than X μm, B is the pore volume of the negative electrode active material layer in the pore diameter range of X μm or more and 20 μm or less, and X is the pore diameter that shows the maximum value in the pore diameter range of 0.01 μm or more and 20 μm or less in the Log differential pore volume distribution of the positive electrode active material layer.
[0012] In the following, the "pore volume in the pore diameter range of 0.01 μm or more and less than X μm in the negative electrode active material layer" is also referred to as the "pore volume A of the negative electrode active material layer." The "pore volume in the pore diameter range of X μm or more and 20 μm or less" is also referred to as the "pore volume B of the negative electrode active material layer." The "pore diameter showing the maximum value in the pore diameter range of 0.01 μm or more and 20 μm or less in the Log differential pore volume distribution of the positive electrode active material layer" is also referred to as the "peak pore diameter X of the positive electrode active material layer."
[0013] The electric storage element according to one aspect of the present invention is an electric storage element in which at least a part of the electrode body is pressed, and the resistance increase rate at a low temperature (for example, -30°C) after the charge / discharge cycle is reduced. The reason for this is unclear, but the following reason is presumed. In general, in an electric storage element, when the active materials of the positive and negative electrodes expand due to the inflow and outflow of ions accompanying charge and discharge, the pore volume of each active material layer of the positive and negative electrodes decreases, and the electrolyte flows out of the pores of each active material layer of the positive and negative electrodes. Then, when the active materials of the positive and negative electrodes contract, the electrolyte flows into the pores of each active material layer. Here, if the electrolyte does not sufficiently return to the pores of the active material layer, a part of the active material layer where the electrolyte is depleted occurs, and the reaction area contributing to charge and discharge decreases, which is thought to cause an increase in resistance. In particular, when at least a part of the electrode body is in a pressed state, the electrolyte is likely to flow out of the active material layer when the active material expands, and is difficult to flow into the active material layer when the active material contracts, so that the electrolyte is likely to run out of the active material layer and the resistance is likely to increase accordingly. At a low temperature of about -30°C, the resistance increase is generally more noticeable in the positive electrode active material layer than in the negative electrode active material layer, so that it is necessary to make the positive electrode active material layer structure such that the electrolyte is unlikely to run out of the active material. In addition, since the inflow of the electrolyte into the pores of the active material layer occurs due to capillary action, it is considered that the smaller the pore diameter, the higher the permeability. In view of the above, in the energy storage element according to one aspect of the present invention, the ratio of the pore volume A in the negative electrode active material layer is reduced to satisfy formula 1. The pore volume A is the volume of pores whose pore diameter is smaller than the peak pore diameter X of the positive electrode active material layer. In the case of such a configuration, the inflow of the electrolyte into the pores of the negative electrode active material layer is relatively suppressed, and the inflow of the electrolyte into the pores of the positive electrode active material layer is easily caused. Therefore, in the energy storage element according to one aspect of the present invention, it is presumed that the resistance increase of the positive electrode active material layer, which is a factor causing the resistance increase especially at low temperatures, is suppressed, and as a result, the resistance increase rate at low temperatures after charge-discharge cycles is reduced for the entire energy storage element.
[0014] The "pressure applied to at least a part of the electrode body in a discharged state" is a value measured by the following method. The electric storage element in a discharged state pressed by a pressure member or the like is placed in a compression tester having a load cell. A load sufficiently smaller than the load applied by the pressure member or the like is applied to the electric storage element by the compression tester. In this state, that is, while maintaining the thickness of the electric storage element, the load applied by the pressure member or the like is released, and the change in the load measured by the compression tester is taken as the load applied to the electrode body. The measured load is divided by the area of the surface of the electric storage element to which the load is applied by the pressure member or the like, and the pressure applied to at least a part of the electrode body is taken as the pressure. Note that a load is usually applied to a pair of opposing surfaces of the electric storage element by a pressure member or the like, and the area of only one of the pair of surfaces is taken as the area of the surface to which the load is applied.
[0015] Specifically, the "discharged state" refers to the following state. First, the storage element is charged at a constant current of 0.05C until it reaches the end-of-charge voltage for normal use, and is placed in a fully charged state. After a 30-minute rest, it is discharged at a constant current of 0.05C until it reaches the lower limit voltage for normal use. This state is called the discharged state. Here, normal use refers to the case where the storage element is used by adopting the charging and discharging conditions recommended or specified for the storage element, and, if a charger for the storage element is provided, the charger is used to use the storage element.
[0016] The "peak pore diameter X of the positive electrode active material layer", the "pore volume A of the negative electrode active material layer" and the "pore volume B of the negative electrode active material layer" are values obtained by measuring the pore volume distribution using the mercury intrusion method. Specifically, they are measured by the following method. An AutoPore9600 is used as a measuring device, and the contact angle of mercury is set to 130° and the surface tension to 484 mN / m. The pore diameter range to be measured is set to 20 μm to 0.0055 μm, and the pore volume distribution in this range is measured. The obtained pore distribution is evaluated to obtain the above-mentioned X, A and B. The sample of the positive electrode active material layer or the negative electrode active material layer to be used for measuring the pore volume distribution is prepared by the following method. The storage element is discharged at a current of 0.05 C to the discharge end voltage during normal use. Here, "normal use" refers to a case where the storage element is used by adopting the discharge conditions recommended or specified for the storage element. Dismantle the storage element, take out the positive or negative electrode and use it as the working electrode, and assemble a test battery with metallic Li as the counter electrode. For the positive electrode, the positive electrode potential is 3.0 V vs. Li / Li at a current of 10 mA / g per 1 g of positive electrode active material. + The negative electrode is discharged at a constant current until the negative electrode potential reaches 2.0 V vs. Li / Li at a current of 10 mA / g per 1 g of negative electrode active material. + The battery is charged at a constant current until the positive or negative electrode reaches a constant current of 1000 V. The test battery is disassembled, and the positive or negative electrode is removed. The positive or negative electrode is thoroughly washed with dimethyl carbonate, and then dried under reduced pressure at room temperature. The dried positive or negative electrode is cut to a specified size (e.g., 2 x 2 cm) and used as a sample for measuring the pore volume distribution. The operations from disassembling the storage element to cutting the positive or negative electrode to the specified size are carried out in a dry air atmosphere with a dew point of -40°C or lower.
[0017] It is preferable that the energy storage device according to one aspect of the present invention further satisfies the following formula 1'. 0.30≦A / B≦0.64...1' In formula 1′, A and B have the same meanings as A and B in formula 1.
[0018] When formula 1' is further satisfied, the permeability of the electrolyte between the positive electrode active material layer and the negative electrode active material layer at low temperatures is balanced, and the electrolyte is less likely to run out in both active material layers, and the resistance increase rate at low temperatures after charge-discharge cycles is further reduced.
[0019] In the energy storage element according to one aspect of the present invention, the pressure applied to at least a portion of the electrode assembly in a discharged state is preferably 0.24 MPa or more. By making the pressure 0.24 MPa or more, the distance between the positive and negative electrodes becomes uniform, and non-uniform reactions during charging and discharging are suppressed, thereby suppressing localized deterioration of the active material.
[0020] It is preferable that the positive electrode active material layer contains a transition metal composite oxide containing nickel, cobalt, and manganese or aluminum, and the negative electrode active material layer contains a carbon material. In general, when such a positive electrode active material and a negative electrode active material are used, the resistance increase of the positive electrode active material layer at low temperatures tends to be particularly significant compared to the negative electrode active material layer. Therefore, when such a positive electrode active material and a negative electrode active material are used in the energy storage element according to one aspect of the present invention, the effect of reducing the resistance increase rate at low temperatures after charge and discharge cycles is particularly significant.
[0021] The storage element according to one aspect of the present invention preferably has a rated capacity of 4 Ah or more. In general, in the case of such a large storage element, it is difficult for the electrolyte to flow into the center of the electrode body in a state where at least a part of the electrode body is pressed, and the electrolyte tends to be easily depleted in the positive electrode active material layer. Therefore, when the rated capacity of the storage element according to one aspect of the present invention is 4 Ah or more, the effect of reducing the resistance increase rate at low temperatures after charge and discharge cycles is particularly remarkable.
[0022] "Rated capacity" refers to the capacity (Ah) used to indicate the capacity of a storage element. In other words, the rated capacity is the capacity indicated on the storage element.
[0023] Hereinafter, an energy storage element, an energy storage device, and a method for manufacturing an energy storage element according to an embodiment of the present invention, as well as other embodiments, will be described in detail. Note that the names of the components (elementary components) used in each embodiment may differ from the names of the components (elementary components) used in the background art.
[0024] <Electricity storage element> The electric storage element according to one embodiment of the present invention includes an electrode assembly having a positive electrode, a negative electrode, and a separator, an electrolytic solution, and a container for accommodating the electrode assembly and the electrolytic solution. The electrode assembly is usually a laminated type in which a plurality of positive electrodes and a plurality of negative electrodes are laminated with a separator interposed therebetween, or a wound type in which a positive electrode and a negative electrode are laminated with a separator interposed therebetween and wound. The electrolytic solution is present in a state in which the positive electrode, the negative electrode, and the separator are impregnated. A secondary battery will be described as an example of an electric storage element.
[0025] (positive electrode) The positive electrode has a positive electrode substrate and a positive electrode active material layer disposed on the positive electrode substrate directly or via an intermediate layer.
[0026] The positive electrode substrate is conductive. Whether or not it has "conductivity" is determined by the volume resistivity being 10 or less, as measured in accordance with JIS-H-0505 (1975). 7 The threshold value is Ω·cm. The material of the positive electrode substrate is a metal such as aluminum, titanium, tantalum, stainless steel, or an alloy thereof. Among these, aluminum or an aluminum alloy is preferred from the viewpoints of potential resistance, high conductivity, and cost. The positive electrode substrate may be a foil, a vapor deposition film, a mesh, a porous material, etc., and a foil is preferred from the viewpoint of cost. Therefore, aluminum foil or an aluminum alloy foil is preferred as the positive electrode substrate. Examples of aluminum or an aluminum alloy include A1085, A3003, A1N30, etc., as specified in JIS-H-4000 (2014) or JIS-H4160 (2006).
[0027] The average thickness of the positive electrode substrate is preferably 3 μm to 50 μm, more preferably 5 μm to 40 μm, even more preferably 8 μm to 30 μm, and particularly preferably 10 μm to 25 μm. By setting the average thickness of the positive electrode substrate within the above range, the strength of the positive electrode substrate can be increased while increasing the energy density per volume of the secondary battery. The "average thickness" of the positive electrode substrate and the negative electrode substrate described later refers to the value obtained by dividing the punched mass when a substrate of a predetermined area is punched out by the true density and punched area of the substrate.
[0028] The intermediate layer is a layer disposed between the positive electrode substrate and the positive electrode active material layer. The intermediate layer contains a conductive agent such as carbon particles to reduce the contact resistance between the positive electrode substrate and the positive electrode active material layer. The configuration of the intermediate layer is not particularly limited, and may contain, for example, a binder and a conductive agent.
[0029] The positive electrode active material layer contains a positive electrode active material and, as necessary, optional components such as a conductive agent, a binder, a thickener, and a filler.
[0030] The positive electrode active material can be appropriately selected from known positive electrode active materials. A material capable of absorbing and releasing lithium ions is usually used as the positive electrode active material for a lithium ion secondary battery. Examples of the positive electrode active material include lithium transition metal composite oxides having an α-NaFeO2 type crystal structure, lithium transition metal composite oxides having a spinel type crystal structure, polyanion compounds, chalcogen compounds, and sulfur. Examples of the lithium transition metal composite oxides having an α-NaFeO2 type crystal structure include Li[Li x Ni (1-x) ]O2(0≦x<0.5), Li[Li x Ni γ Co (1-x-γ) ]O2(0≦x<0.5, 0<γ<1), Li[Li x Co (1-x) ]O2(0≦x<0.5), Li[Li x Ni γ Mn (1-x-γ) ]O2(0≦x<0.5, 0<γ<1), Li[Li x Ni γ Mnβ Co (1-x-γ-β) ]O2(0≦x<0.5, 0<γ, 0<β, 0.5<γ+β<1), Li[Li x Ni γ Co β Al (1-x-γ-β) ]O2 (0≦x<0.5, 0<γ, 0<β, 0.5<γ+β<1), etc. Lithium transition metal composite oxides with spinel crystal structure include Li x Mn2O4, Li x Ni γ Mn (2-γ) O4, etc. Examples of polyanion compounds include LiFePO4, LiMnPO4, LiNiPO4, LiCoPO4, Li3V2(PO4)3, Li2MnSiO4, Li2CoPO4F, etc. Examples of chalcogen compounds include titanium disulfide, molybdenum disulfide, molybdenum dioxide, etc. Atoms or polyanions in these materials may be partially substituted with atoms or anion species of other elements. The surfaces of these materials may be coated with other materials. In the positive electrode active material layer, one of these materials may be used alone, or two or more may be mixed and used.
[0031] As the positive electrode active material, a lithium transition metal composite oxide is preferable, a lithium transition metal composite oxide containing nickel, cobalt, and manganese or aluminum is more preferable, and a lithium transition metal composite oxide containing nickel, cobalt, and manganese is even more preferable. This lithium transition metal composite oxide preferably has an α-NaFeO2 type crystal structure. By using such a lithium transition metal composite oxide, it is possible to increase the energy density. In addition, such a lithium transition metal composite oxide is an active material that tends to have a particularly large increase in resistance at low temperatures.
[0032] As the lithium transition metal composite oxide having an α-NaFeO2 type crystal structure, a compound represented by the following formula 2 is preferable. Li 1+α Me 1-α O2···2 In formula 2, Me is a metal (excluding Li) including Ni, Co, Mn, and Al, and 0≦α<1.
[0033] In formula 2, Me is preferably substantially composed of the three elements Ni, Co, and Mn, or the three elements Ni, Co, and Al, and more preferably composed of the three elements Ni, Co, and Mn. However, Me may contain other metals.
[0034] From the viewpoint of achieving a larger electric capacity, the preferred contents (composition ratios) of the constituent elements in the compound represented by formula 2 are as follows. Note that the molar ratio is equal to the atomic ratio.
[0035] In formula 2, the lower limit of the molar ratio of Ni to Me (Ni / Me) is preferably 0.1, and in some cases, 0.2, 0.3, or 0.4 is more preferable. On the other hand, the upper limit of this molar ratio (Ni / Me) is preferably 0.9, and in some cases, 0.8, 0.7, or 0.6 is more preferable.
[0036] In formula 2, the lower limit of the molar ratio of Co to Me (Co / Me) is preferably 0.01, and in some cases, 0.1 or 0.2 is more preferable, while the upper limit of this molar ratio (Co / Me) is preferably 0.5, and in some cases, 0.4 or 0.3 is more preferable.
[0037] In formula 2, the lower limit of the molar ratio of Mn to Me (Mn / Me) may be 0, and in some cases is preferably 0.05, and more preferably 0.1 or 0.2. On the other hand, the upper limit of this molar ratio (Mn / Me) is preferably 0.6, and in some cases is more preferably 0.4 or 0.3.
[0038] In formula 2, the lower limit of the molar ratio of Al to Me (Al / Me) may be 0, and in some cases is preferably 0.01, and more preferably 0.02 or 0.03. On the other hand, the upper limit of this molar ratio (Al / Me) is preferably 0.3, and in some cases is more preferably 0.2 or 0.1.
[0039] In formula 2, the molar ratio of Li to Me (Li / Me), i.e., (1+α) / (1-α), may be 1, and in some cases may be preferably greater than 1.0 (α>0) or 1.1 or greater. On the other hand, the upper limit of this molar ratio (Li / Me) is preferably 1.6, and in some cases may be more preferably 1.4 or 1.2.
[0040] The composition ratio of the lithium transition metal composite oxide refers to the composition ratio when the battery is fully discharged by the following method. First, the energy storage element (secondary battery) is charged at a constant current of 0.05 C until it reaches the end-of-charge voltage in normal use, and then fully charged. After a 30-minute rest, it is discharged at a constant current of 0.05 C until it reaches the lower limit voltage in normal use. Then, the battery is disassembled, the positive electrode is removed and used as the working electrode, and a test battery is assembled with metallic Li as the counter electrode. Then, at a current of 10 mA per 1 g of positive electrode active material, the positive electrode potential is 3.0 V vs. Li / Li. + The positive electrode is adjusted to a fully discharged state by discharging at a constant current until the positive electrode reaches a fully discharged state. The device is disassembled again and the positive electrode is removed. Dimethyl carbonate is used to thoroughly wash away the electrolyte adhering to the removed positive electrode, and the device is dried under reduced pressure at room temperature for 24 hours, after which the lithium transition metal composite oxide, the positive electrode active material, is extracted. The extracted lithium transition metal composite oxide is subjected to measurement. The operations from disassembling the energy storage element to extracting the lithium transition metal composite oxide are carried out in an argon atmosphere with a dew point of -60°C or lower.
[0041] Suitable lithium transition metal composite oxides include, for example, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, LiNi 3 / 5 Co 1 / 5 Mn 1 / 5 O2, LiNi 1 / 2 Co 1 / 5 Mn 3 / 10 O2, LiNi 1 / 2 Co 3 / 10 Mn 1 / 5 O2, LiNi 8 / 10 Co 1 / 10 Mn 1 / 10 O2, LiNi 0.8 Co 0.15 Al 0.05 Examples include O2.
[0042] The positive electrode active material may be used alone or in combination of two or more. The content of the lithium transition metal composite oxide in all the positive electrode active materials used is preferably 50% by mass or more, more preferably 70% by mass or more and 100% by mass or less, and even more preferably 80% by mass or more and 100% by mass or less. It is particularly preferable to use a positive electrode active material substantially composed of only the lithium transition metal composite oxide.
[0043] The positive electrode active material is usually a particle (powder). The average particle size of the positive electrode active material is preferably, for example, 0.1 μm or more and 20 μm or less. By setting the average particle size of the positive electrode active material to the above lower limit or more, the positive electrode active material can be easily manufactured or handled. By setting the average particle size of the positive electrode active material to the above upper limit or less, the electronic conductivity of the positive electrode active material layer is improved. In addition, when a composite of the positive electrode active material and another material is used, the average particle size of the composite is taken as the average particle size of the positive electrode active material. The "average particle size" means a value at which the volume-based cumulative distribution calculated in accordance with JIS-Z-8819-2 (2001) is 50% based on the particle size distribution measured by a laser diffraction / scattering method for a diluted solution obtained by diluting particles with a solvent in accordance with JIS-Z-8825 (2013).
[0044] In order to obtain powder with a predetermined particle size, a pulverizer, a classifier, etc. are used. Examples of the pulverization method include a method using a mortar, a ball mill, a sand mill, a vibration ball mill, a planetary ball mill, a jet mill, a counter jet mill, a swirling airflow type jet mill, or a sieve. During pulverization, wet pulverization in the presence of water or an organic solvent such as hexane can also be used. As a classification method, a sieve, an air classifier, etc. are used as necessary for both the dry and wet methods.
[0045] The content of the positive electrode active material in the positive electrode active material layer is preferably 50% by mass to 99% by mass, more preferably 70% by mass to 98% by mass, and even more preferably 80% by mass to 95% by mass. By setting the content of the positive electrode active material in the above range, both high energy density and manufacturability of the positive electrode active material layer can be achieved.
[0046] The conductive agent is not particularly limited as long as it is a material having electrical conductivity. Examples of such conductive agents include carbonaceous materials, metals, conductive ceramics, and the like. Examples of carbonaceous materials include graphitized carbon, non-graphitized carbon, graphene-based carbon, and the like. Examples of non-graphitized carbon include carbon nanofibers, pitch-based carbon fibers, carbon black, and the like. Examples of carbon black include furnace black, acetylene black, ketjen black, and the like. Examples of graphene-based carbon include graphene, carbon nanotubes (CNT), fullerene, and the like. Examples of the shape of the conductive agent include powder and fiber. As the conductive agent, one of these materials may be used alone, or two or more of them may be mixed and used. In addition, these materials may be used in a composite form. For example, a material in which carbon black and CNT are composited may be used. Among these, carbon black is preferable from the viewpoint of electronic conductivity and coatability, and acetylene black is preferable among them.
[0047] The content of the conductive agent in the positive electrode active material layer is preferably from 1% by mass to 10% by mass, more preferably from 3% by mass to 9% by mass. By setting the content of the conductive agent in the above range, the energy density of the secondary battery can be increased.
[0048] Examples of binders include thermoplastic resins such as fluororesins (polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), etc.), polyethylene, polypropylene, polyacrylic, polyimide, etc.; elastomers such as ethylene-propylene-diene rubber (EPDM), sulfonated EPDM, styrene butadiene rubber (SBR), fluororubber, etc.; polysaccharide polymers, etc.
[0049] The content of the binder in the positive electrode active material layer is preferably from 1% by mass to 10% by mass, and more preferably from 3% by mass to 9% by mass. By setting the content of the binder in the above range, the active material can be stably held.
[0050] Examples of the thickener include polysaccharide polymers such as carboxymethyl cellulose (CMC) and methyl cellulose. When the thickener has a functional group that reacts with lithium or the like, the functional group may be deactivated in advance by methylation or the like. The technology disclosed herein can be preferably implemented in an embodiment in which the positive electrode active material layer does not contain the thickener.
[0051] The filler is not particularly limited. Examples of the filler include polyolefins such as polypropylene and polyethylene, inorganic oxides such as silicon dioxide, alumina, titanium dioxide, calcium oxide, strontium oxide, barium oxide, magnesium oxide, and aluminosilicate, hydroxides such as magnesium hydroxide, calcium hydroxide, and aluminum hydroxide, carbonates such as calcium carbonate, poorly soluble ion crystals such as calcium fluoride, barium fluoride, and barium sulfate, nitrides such as aluminum nitride and silicon nitride, mineral resource-derived substances such as talc, montmorillonite, boehmite, zeolite, apatite, kaolin, mullite, spinel, olivine, sericite, bentonite, and mica, and artificial products thereof. When a filler is used, the content of the filler in the positive electrode active material layer can be 0.1% by mass or more and 8% by mass or less, and is usually preferably 5% by mass or less, and more preferably 2% by mass or less. The technology disclosed herein can be preferably implemented in an embodiment in which the positive electrode active material layer does not contain the filler.
[0052] The positive electrode active material layer may contain typical nonmetallic elements such as B, N, P, F, Cl, Br, and I, typical metallic elements such as Li, Na, Mg, Al, K, Ca, Zn, Ga, Ge, Sn, Sr, and Ba, and transition metallic elements such as Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Mo, Zr, Nb, and W as components other than the positive electrode active material, conductive agent, binder, thickener, and filler.
[0053] The positive electrode active material layer is a porous layer. The peak pore diameter X of the positive electrode active material layer (the maximum pore diameter in the range of pore diameters of 0.01 μm to 20 μm in the Log differential pore volume distribution) is preferably 0.04 μm to 0.4 μm, more preferably 0.06 μm to 0.2 μm, even more preferably 0.08 μm to 0.17 μm, and particularly preferably 0.10 μm to 0.14 μm. When the peak pore diameter X of the positive electrode active material layer is in the above range, the permeability of the electrolyte into the pores of the positive electrode active material layer is further increased, and the resistance increase rate at low temperatures after charge / discharge cycles is reduced. The peak pore diameter X of the positive electrode active material layer is usually a pore diameter derived from the positive electrode active material, and can be adjusted mainly by the type (particle size, shape, etc.) of the positive electrode active material. In addition, the peak pore diameter X of the positive electrode active material layer can be adjusted by the type and content of other components, whether or not the positive electrode active material layer is pressed during preparation of the positive electrode, and the strength of the pressing pressure.
[0054] The positive electrode can be produced, for example, by applying a positive electrode mixture paste directly or via an intermediate layer to a positive electrode substrate and drying it. After drying, pressing or the like may be performed as necessary. The positive electrode mixture paste contains each component constituting the positive electrode active material layer, including a positive electrode active material and optional components such as a conductive agent and a binder. The positive electrode mixture paste usually further contains a dispersion medium.
[0055] (Negative electrode) The negative electrode has a negative electrode substrate and a negative electrode active material layer disposed on the negative electrode substrate directly or via an intermediate layer. The configuration of the intermediate layer is not particularly limited and can be selected from the configurations exemplified for the positive electrode.
[0056] The negative electrode substrate has electrical conductivity. Metals such as copper, nickel, stainless steel, nickel-plated steel, and aluminum, or alloys thereof, carbonaceous materials, etc. are used as the material of the negative electrode substrate. Among these, copper or copper alloys are preferred. Examples of the negative electrode substrate include foils, vapor deposition films, meshes, and porous materials, and foils are preferred from the viewpoint of cost. Therefore, copper foil or copper alloy foil is preferred as the negative electrode substrate. Examples of copper foil include rolled copper foil and electrolytic copper foil.
[0057] The average thickness of the negative electrode substrate is preferably 2 μm to 35 μm, more preferably 3 μm to 30 μm, further preferably 4 μm to 25 μm, and particularly preferably 5 μm to 20 μm. By setting the average thickness of the negative electrode substrate within the above range, it is possible to increase the strength of the negative electrode substrate and to increase the energy density per volume of the secondary battery.
[0058] The negative electrode active material layer contains a negative electrode active material. The negative electrode active material layer contains optional components such as a conductive agent, a binder, a thickener, a filler, etc., as necessary. The optional components such as a conductive agent, a binder, a thickener, a filler, etc. can be selected from the materials exemplified for the positive electrode above.
[0059] The negative electrode active material layer may contain typical nonmetallic elements such as B, N, P, F, Cl, Br, and I, typical metallic elements such as Li, Na, Mg, Al, K, Ca, Zn, Ga, Ge, Sn, Sr, and Ba, and transition metallic elements such as Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Mo, Zr, Ta, Hf, Nb, and W as components other than the negative electrode active material, conductive agent, binder, thickener, and filler.
[0060] The negative electrode active material can be appropriately selected from known negative electrode active materials. A material capable of absorbing and releasing lithium ions is usually used as the negative electrode active material for lithium ion secondary batteries. Examples of the negative electrode active material include metal Li; metals or semimetals such as Si and Sn; metal oxides or semimetal oxides such as Si oxide, Ti oxide, and Sn oxide; Li4Ti5O 12 , LiTiO 2、 Examples of the material include titanium-containing oxides such as TiNb2O7, polyphosphate compounds, silicon carbide, and carbon materials such as graphite and non-graphitic carbon (easily graphitized carbon or non-graphitizable carbon). Among these materials, carbon materials are preferred, graphite and non-graphitic carbon are more preferred, and graphite is even more preferred. In the negative electrode active material layer, one of these materials may be used alone, or two or more of them may be used in combination.
[0061] "Graphite" refers to graphite that has an average lattice spacing (d 002 ) is 0.33 nm or more and less than 0.34 nm. Examples of graphite include natural graphite and artificial graphite. Artificial graphite is preferred from the viewpoint of availability of materials with stable physical properties.
[0062] "Non-graphitic carbon" refers to carbon that has an average lattice spacing (d 002 ) is 0.34 nm or more and 0.42 nm or less. Examples of non-graphitizable carbon include non-graphitizable carbon and graphitizable carbon. Examples of non-graphitizable carbon include resin-derived materials, petroleum pitch or petroleum pitch-derived materials, petroleum coke or petroleum coke-derived materials, plant-derived materials, and alcohol-derived materials.
[0063] Here, the "discharged state" of carbon materials (graphite and non-graphitic carbon) means a discharged state in which lithium ions capable of being absorbed and released during charging and discharging are sufficiently released from the carbon material, which is the negative electrode active material. For example, in a single-electrode battery using a negative electrode containing a carbon material as the negative electrode active material as a working electrode and metallic Li as a counter electrode, it is a state in which the open circuit voltage is 0.7 V or more.
[0064] "Non-graphitizable carbon" means the above d 002 This refers to carbon materials with a particle size of 0.36 nm or more and 0.42 nm or less.
[0065] "Graphitizable carbon" means the above d 002 This refers to carbon materials with a particle size of 0.34 nm or more and less than 0.36 nm.
[0066] The negative electrode active material is usually a particle (powder). The average particle size of the negative electrode active material can be, for example, 1 nm or more and 100 μm or less. When the negative electrode active material is a carbon material, a titanium-containing oxide, or a polyphosphate compound, the average particle size may be 1 μm or more and 100 μm or less. When the negative electrode active material is Si, Sn, Si oxide, Sn oxide, or the like, the average particle size may be 1 nm or more and 1 μm or less. By setting the average particle size of the negative electrode active material to the above lower limit or more, the negative electrode active material can be easily manufactured or handled. By setting the average particle size of the negative electrode active material to the above upper limit or less, the electronic conductivity of the active material layer is improved. In order to obtain powder with a predetermined particle size, a pulverizer, a classifier, or the like is used. The pulverizing method and the powder classification method can be selected, for example, from the methods exemplified for the positive electrode.
[0067] The BET specific surface area of the negative electrode active material layer is 2m 2 / g or more 12m 2 / g or less is preferable, and 3m 2 / g or more 10m 2 / g or less is more preferable, and 4m 2 / g or more 8m 2 / g or less is even more preferable. By setting the BET specific surface area of the negative electrode active material layer within the above range, it is possible to improve the output performance of the secondary battery. The "BET specific surface area" of the negative electrode active material layer is a value determined from an adsorption isotherm using a nitrogen gas adsorption method. Specifically, the BET specific surface area is measured by the following method. First, the energy storage element (secondary battery) is discharged at a constant current of 0.05 C to the lower limit voltage during normal use. The energy storage element is disassembled, the negative electrode is removed and used as the working electrode, and a test battery is assembled with metallic Li as the counter electrode. A current of 10 mA per 1 g of negative electrode active material is applied until the negative electrode potential reaches 2.0 V vs. Li / Li. +The test battery is disassembled again, and the negative electrode is removed. The electrolyte attached to the removed negative electrode is thoroughly washed using dimethyl carbonate, and the negative electrode is dried under reduced pressure for 24 hours at room temperature, and then the negative electrode active material layer is collected to be used as the sample to be measured. 1.00 g of the powder of the sample to be measured (negative electrode active material layer) is placed in a sample tube for measurement, and vacuum dried at 120°C for 12 hours to thoroughly remove moisture in the measurement sample. Next, an adsorption isotherm is measured within the relative pressure P / P0 (P0 = approximately 770 mmHg) range of 0 to 1 by a nitrogen gas adsorption method using liquid nitrogen. Five points are extracted from the region of P / P0 = 0.06 to 0.3 of the obtained adsorption isotherm, and a BET plot is performed, and the BET specific surface area is calculated from the y-intercept and slope of the straight line. The work from disassembling the storage element to collecting the negative electrode active material layer is performed in an argon atmosphere with a dew point of -60°C or less.
[0068] The content of the negative electrode active material in the negative electrode active material layer is preferably 60% by mass to 99% by mass, more preferably 90% by mass to 98% by mass. By setting the content of the negative electrode active material in the above range, both high energy density and manufacturability of the negative electrode active material layer can be achieved.
[0069] The negative electrode active material layer is a porous layer. The pore volume of the negative electrode active material layer in the pore diameter range of 0.01 μm to 20 μm is, for example, 0.1 cm 3 / g or more 1cm 3 / g or less is preferable, and 0.2 cm 3 / g or more 0.7cm 3 / g or less is more preferable, and 0.3 cm 3 / g or more 0.5cm 3 / g or less is more preferable. By having the pore volume of the negative electrode active material layer in the above range, sufficient output performance can be exhibited. The pore volume of the negative electrode active material layer can be adjusted, for example, by the type (particle size, shape, etc.) of the negative electrode active material, whether or not the negative electrode active material layer is pressed when preparing the negative electrode, and the strength of the pressing pressure.
[0070] The negative electrode can be produced, for example, by applying a negative electrode mixture paste directly or via an intermediate layer to a negative electrode substrate and drying it. After drying, pressing or the like may be performed as necessary. The negative electrode mixture paste contains each component constituting the negative electrode active material layer, including a negative electrode active material and optional components such as a conductive agent and a binder. The negative electrode mixture paste usually further contains a dispersion medium.
[0071] (Relationship between positive and negative electrodes) The secondary battery satisfies the following formula 1. A / B≦0.64 1 In formula 1, A is the pore volume of the negative electrode active material layer in the range of pore diameters of 0.01 μm or more and less than X μm. B is the pore volume in the negative electrode active material layer in the range of pore diameters of X μm or more and 20 μm or less. X is the maximum pore diameter in the pore diameter range of 0.01 μm or more and 20 μm or less in the Log differential pore volume distribution of the positive electrode active material layer.
[0072] In formula 1, A / B is preferably 0.62 or less, more preferably 0.60 or less, and even more preferably 0.59 or less. By setting A / B to the above upper limit or less, the permeability of the electrolyte into the pores of the positive electrode active material layer is increased, and the electrolyte in the positive electrode active material layer is less likely to run out, thereby reducing the rate of increase in resistance at low temperatures after charge / discharge cycles.
[0073] Moreover, it is preferable that the secondary battery satisfies the following formula 1'. 0.30≦A / B≦0.64...1' In formula 1′, A and B have the same meanings as A and B in formula 1.
[0074] Thus, A / B is preferably 0.30 or more, more preferably 0.35 or more, and even more preferably 0.40 or 0.50 or more. When A / B is equal to or less than the upper limit and equal to or more than the lower limit, the electrolyte is unlikely to run out in both the positive electrode active material layer and the negative electrode active material layer, and the resistance increase rate at low temperatures after charge / discharge cycles is further reduced.
[0075] The value of A / B can be adjusted by the materials constituting the positive electrode active material layer and the negative electrode active material layer, in particular the type of active material, whether or not the positive electrode active material layer and the negative electrode active material layer are pressed when producing the positive electrode and the negative electrode, the strength of the pressing pressure, and the like.
[0076] The pore volume A of the negative electrode active material layer (the pore volume of the negative electrode active material layer in the range of pore diameters of 0.01 μm or more and less than X μm) is, for example, 0.05 cm 3 / g or more 0.25cm 3 / g or less is preferable, and 0.10 cm 3 / g or more 0.20cm 3 / g or less is more preferable, and 0.12 cm 3 / g or more 0.15cm 3 In some cases, the pore volume B of the negative electrode active material layer (the pore volume of the negative electrode active material layer in the range of pore diameters of X μm or more and 20 μm or less) is, for example, 0.10 cm 3 / g or more 0.45cm 3 / g or less is preferable, and 0.15 cm 3 / g or more 0.35cm 3 / g or less is more preferable, and 0.20 cm 3 / g or more 0.25cm 3 / g or less may be even more preferable.
[0077] (Separator) The separator can be appropriately selected from known separators. For example, a separator consisting of only a substrate layer, a separator in which a heat-resistant layer containing heat-resistant particles and a binder is formed on one or both surfaces of the substrate layer, etc. can be used as the separator. Examples of the material of the substrate layer of the separator include woven fabric, nonwoven fabric, and porous resin film. Among these materials, a porous resin film is preferable from the viewpoint of strength, and a nonwoven fabric is preferable from the viewpoint of electrolyte retention. As the material of the substrate layer of the separator, polyolefins such as polyethylene and polypropylene are preferable from the viewpoint of shutdown function, and polyimide and aramid are preferable from the viewpoint of oxidation decomposition resistance. A material obtained by combining these resins may be used as the substrate layer of the separator.
[0078] The heat-resistant particles contained in the heat-resistant layer preferably have a mass loss of 5% or less when heated from room temperature to 500°C under an air atmosphere at 1 atmosphere, and more preferably have a mass loss of 5% or less when heated from room temperature to 800°C. Examples of materials with a mass loss of a predetermined amount or less include inorganic compounds. Examples of inorganic compounds include oxides such as iron oxide, silicon oxide, aluminum oxide, titanium oxide, barium titanate, zirconium oxide, calcium oxide, strontium oxide, barium oxide, magnesium oxide, and aluminosilicate; nitrides such as aluminum nitride and silicon nitride; carbonates such as calcium carbonate; sulfates such as barium sulfate; sparingly soluble ion crystals such as calcium fluoride and barium fluoride; covalent crystals such as silicon and diamond; mineral resource-derived substances such as talc, montmorillonite, boehmite, zeolite, apatite, kaolin, mullite, spinel, olivine, sericite, bentonite, and mica, or artificial products thereof. As the inorganic compound, these substances may be used alone or in the form of a complex, or two or more of them may be mixed and used. Among these inorganic compounds, silicon oxide, aluminum oxide, or aluminosilicate is preferred from the viewpoint of the safety of the energy storage element.
[0079] The porosity of the separator is preferably 80% by volume or less from the viewpoint of strength, and is preferably 20% by volume or more from the viewpoint of discharge performance. Here, "porosity" refers to a volume-based value measured with a mercury porosimeter.
[0080] (electrolyte) The electrolyte can be appropriately selected from known electrolytes. The electrolyte may be a non-aqueous electrolyte. The non-aqueous electrolyte contains a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent.
[0081] The non-aqueous solvent can be appropriately selected from known non-aqueous solvents. Examples of the non-aqueous solvent include cyclic carbonates, chain carbonates, carboxylates, phosphates, sulfonates, ethers, amides, and nitriles. As the non-aqueous solvent, those in which some of the hydrogen atoms contained in these compounds are substituted with halogens may be used.
[0082] Examples of cyclic carbonates include ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), vinylene carbonate (VC), vinylethylene carbonate (VEC), chloroethylene carbonate, fluoroethylene carbonate (FEC), difluoroethylene carbonate (DFEC), styrene carbonate, 1-phenylvinylene carbonate, 1,2-diphenylvinylene carbonate, etc. Among these, EC is preferred.
[0083] Examples of the chain carbonate include diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diphenyl carbonate, trifluoroethyl methyl carbonate, bis(trifluoroethyl) carbonate, etc. Among these, EMC is preferable.
[0084] As the non-aqueous solvent, it is preferable to use a cyclic carbonate or a chain carbonate, and it is more preferable to use a combination of a cyclic carbonate and a chain carbonate. By using a cyclic carbonate, it is possible to promote dissociation of the electrolyte salt and improve the ionic conductivity of the non-aqueous electrolyte. By using a chain carbonate, it is possible to keep the viscosity of the non-aqueous electrolyte low. When using a cyclic carbonate and a chain carbonate in combination, it is preferable that the volume ratio of the cyclic carbonate to the chain carbonate (cyclic carbonate:chain carbonate) is, for example, in the range of 5:95 to 50:50.
[0085] The electrolyte salt can be appropriately selected from known electrolyte salts. Examples of the electrolyte salt include lithium salts, sodium salts, potassium salts, magnesium salts, onium salts, etc. Among these, lithium salts are preferred.
[0086] Examples of the lithium salt include inorganic lithium salts such as LiPF6, LiPO2F2, LiBF4, LiClO4, and LiN(SO2F)2, lithium oxalate salts such as lithium bis(oxalate)borate (LiBOB), lithium difluorooxalateborate (LiFOB), and lithium bis(oxalate)difluorophosphate (LiFOP), and lithium salts having a halogenated hydrocarbon group such as LiSO3CF3, LiN(SO2CF3)2, LiN(SO2C2F5)2, LiN(SO2CF3)(SO2C4F9), LiC(SO2CF3)3, and LiC(SO2C2F5)3. Among these, inorganic lithium salts are preferred, and LiPF6 is more preferred.
[0087] The electrolyte salt content in the non-aqueous electrolyte is 0.1 mol / dm at 20°C and 1 atmosphere. 3 More than 2.5mol / dm 3 It is preferable that the value is 0.3 mol / dm or less. 3 More than 2.0mol / dm 3 More preferably, it is 0.5 mol / dm or less. 3 More than 1.7mol / dm 3 More preferably, it is 0.7 mol / dm or less. 3More than 1.5mol / dm 3 By setting the content of the electrolyte salt within the above range, the ionic conductivity of the nonaqueous electrolyte can be increased.
[0088] The non-aqueous electrolyte may contain additives in addition to the non-aqueous solvent and the electrolyte salt. Examples of the additives include aromatic compounds such as biphenyl, alkylbiphenyl, terphenyl, partially hydrogenated terphenyl, cyclohexylbenzene, t-butylbenzene, t-amylbenzene, diphenyl ether, and dibenzofuran; partial halides of the aromatic compounds such as 2-fluorobiphenyl, o-cyclohexylfluorobenzene, and p-cyclohexylfluorobenzene; halogenated anisole compounds such as 2,4-difluoroanisole, 2,5-difluoroanisole, 2,6-difluoroanisole, and 3,5-difluoroanisole; vinylene carbonate, methylvinylene carbonate, ethylvinylene carbonate, succinic anhydride, glutaric anhydride, maleic anhydride, citraconic anhydride, glutaconic anhydride, itaconic anhydride, and cyclohexanedicarboxylic anhydride; ethylene sulfite, propylene sulfite, dimethyl sulfite, and propane sulfite. sultone, propene sultone, butane sultone, methyl methanesulfonate, busulfan, methyl toluenesulfonate, dimethyl sulfate, ethylene sulfate, sulfolane, dimethyl sulfone, diethyl sulfone, dimethyl sulfoxide, diethyl sulfoxide, tetramethylene sulfoxide, diphenyl sulfide, 4,4'-bis(2,2-dioxo-1,3,2-dioxathiolane), 4-methylsulfonyloxymethyl-2,2-dioxo-1,3,2-dioxathiolane, thioanisole, diphenyl disulfide, dipyridinium disulfide, 1,3-propene sultone, 1,3-propane sultone, 1,4-butane sultone, 1,4-butene sultone, perfluorooctane, tristrimethylsilyl borate, tristrimethylsilyl phosphate, tetrakistrimethylsilyl titanate, lithium monofluorophosphate, lithium difluorophosphate, and the like. These additives may be used alone or in combination of two or more.
[0089] The content of the additive contained in the non-aqueous electrolyte is preferably 0.01% by mass to 10% by mass, more preferably 0.1% by mass to 7% by mass, even more preferably 0.2% by mass to 5% by mass, and particularly preferably 0.3% by mass to 3% by mass. By setting the content of the additive within the above range, it is possible to improve the capacity retention performance or cycle performance after high-temperature storage, and to further improve safety.
[0090] (Pressing against the electrode body) At least a part of the electrode body is pressed in a discharged state. The lower limit of the pressure applied to at least a part of the electrode body in a discharged state is preferably 0.24 MPa, more preferably 0.3 MPa. This allows the secondary battery to exhibit good charge-discharge cycle performance by maintaining a uniform distance between the positive electrode and the negative electrode.
[0091] Usually, the electrode body stored in the container is pressed from the outside of the container, that is, through the container. Also, usually, the electrode body is pressed in the direction in which the positive electrode, the negative electrode, and the separator are stacked (thickness direction of each layer). That is, the positive electrode active material layer and the negative electrode active material layer are pressed in the direction in which they are crushed in the thickness direction. However, a part of the electrode body (for example, a pair of curved surface parts in a flat wound electrode body, etc.) may not be pressed. Also, a part of the flat part of the laminated electrode body and the flat wound electrode body, for example, only the central part, may be pressed. The upper limit of the pressure in the discharged state is, for example, preferably 2.4 MPa, more preferably 1.0 MPa, and even more preferably 0.5 MPa. When the pressure in the discharged state is equal to or less than the upper limit, the electrolyte is sufficiently flowed into the pores of the active material layer, and the resistance increase rate at low temperatures after the charge and discharge cycles of the secondary battery can be further reduced. The pressure in the discharged state may be equal to or greater than any of the lower limits and equal to or less than any of the upper limits.
[0092] The pressing (application of a load) to at least a part of the electrode body can be performed, for example, by a pressing member that presses the container from the outside. The pressing member may be a restraining member that restrains the shape of the container. The pressing member (restraining member) is provided so as to sandwich and press the electrode body from both sides in the thickness direction via the container, for example. The pressed surface of the electrode body is in contact with the inner surface of the container directly or via another member. Therefore, the electrode body is pressed by pressing the container. Examples of the pressing member include a restraining band and a metal frame. For example, the metal frame may be configured so that the load can be adjusted by a bolt or the like. In addition, a plurality of secondary batteries (electricity storage elements) may be arranged in the thickness direction of the electrode body, and fixed using a frame or the like in a state in which the plurality of secondary batteries are pressed from both ends in the thickness direction.
[0093] The electric storage element of this embodiment has a reduced resistance increase rate at low temperatures after charge and discharge cycles. In general electric storage elements, when charge and discharge are performed at a high rate (high current density), the resistance increase at low temperatures after charge and discharge cycles is usually significant. This is thought to be because the movement of the electrolyte cannot keep up with the high rate of charge and discharge, and the electrolyte is particularly likely to be depleted in the pores of the active material layer. For this reason, the electric storage element of this embodiment, which is configured so that the electrolyte can sufficiently flow into the pores of the active material layer, may be used at low temperatures and is suitable for applications in which charge and discharge are performed at a high rate, such as automotive power sources for electric vehicles (EVs), hybrid vehicles (HEVs), plug-in hybrid vehicles (PHEVs), etc.
[0094] The shape of the energy storage element (secondary battery) of this embodiment is not particularly limited, and examples thereof include a cylindrical battery, a square battery, a flat battery, a coin battery, and a button battery.
[0095] FIG. 1 shows an energy storage element 1 as an example of a prismatic battery. Note that this figure is a see-through view of the inside of the case. An electrode body 2 having a positive electrode and a negative electrode wound with a separator sandwiched therebetween is housed in a prismatic container 3. The positive electrode is electrically connected to a positive electrode terminal 4 via a positive electrode lead 41. The negative electrode is electrically connected to a negative electrode terminal 5 via a negative electrode lead 51. In addition, in the energy storage element 1 of FIG. 1, a pressing member (not shown) or the like may be provided to pressurize the container 3 and the electrode body 2 housed in the container 3, for example, by sandwiching both sides of the container 3 (usually the front side and the back side in FIG. 1).
[0096] <Electricity storage device> The energy storage element of this embodiment can be mounted as an energy storage unit (battery module) formed by assembling a plurality of energy storage elements 1 in a power source for an automobile such as an EV, HEV, or PHEV, a power source for electronic devices such as a personal computer or a communication terminal, or a power storage power source, etc. In this case, the technology of the present invention may be applied to at least one energy storage element included in the energy storage device.
[0097] 2 shows an example of an energy storage device 30 in which energy storage units 20, each of which is an assembly of two or more electrically connected energy storage elements 1, are further assembled. The energy storage units 20 or the energy storage device 30 may include a pressure member (not shown) that presses the multiple energy storage elements 1, for example, from the left and right directions in FIG. 2. The energy storage device 30 may include a bus bar (not shown) that electrically connects two or more energy storage elements 1, a bus bar (not shown) that electrically connects two or more energy storage units 20, and the like. The energy storage unit 20 or the energy storage device 30 may include a status monitoring device (not shown) that monitors the status of one or more energy storage elements.
[0098] <Method of manufacturing the energy storage element> The manufacturing method of the energy storage element of this embodiment can be appropriately selected from known methods. The manufacturing method includes, for example, preparing an electrode body, preparing an electrolyte, and housing the electrode body and the electrolyte in a container. Preparing the electrode body includes preparing a positive electrode and a negative electrode, and forming the electrode body by stacking or rolling the positive electrode and the negative electrode with a separator interposed therebetween. The manufacturing method may further include attaching a pressure member or the like.
[0099] <Other embodiments> The energy storage element of the present invention is not limited to the above-described embodiment, and various modifications may be made without departing from the scope of the present invention. For example, the configuration of one embodiment may be added to the configuration of another embodiment, and a part of the configuration of one embodiment may be replaced with the configuration of another embodiment or a well-known technique. Furthermore, a part of the configuration of one embodiment may be deleted. Also, a well-known technique may be added to the configuration of one embodiment.
[0100] In the above embodiment, the case where the storage element is used as a chargeable and dischargeable nonaqueous electrolyte secondary battery (e.g., a lithium ion secondary battery) has been mainly described, but the type, shape, size, capacity, etc. of the storage element are arbitrary. The present invention can also be applied to various secondary batteries, electric double layer capacitors, lithium ion capacitors, and other capacitors.
[0101] In the above embodiment, the electrode body in which the positive electrode and the negative electrode are stacked with a separator interposed therebetween has been described, but the electrode body may not include a separator. For example, the positive electrode and the negative electrode may be in direct contact with each other in a state in which a non-conductive layer is formed on the active material layer of the positive electrode or the negative electrode. In addition, the electric storage element of the present invention can also be applied to an electric storage element in which the electrolyte is an electrolyte other than a non-aqueous electrolyte. EXAMPLES
[0102] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.
[0103] [Example 1] (Preparation of positive electrode) Positive electrode active material LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 A positive electrode mixture paste was prepared using O2, acetylene black (AB) as a conductive agent, polyvinylidene fluoride (PVDF) as a binder, and N-methylpyrrolidone (NMP) as a dispersion medium. The mass ratio of the positive electrode active material, AB, and PVDF was 93:3.5:3.5 (solid content conversion). The positive electrode mixture paste was applied to both sides of an aluminum foil as a positive electrode substrate and dried. Then, roll pressing was performed to obtain a positive electrode a. The peak pore diameter X of the positive electrode active material layer was 0.117 μm.
[0104] (Preparation of negative electrode) A negative electrode mixture paste was prepared by mixing graphite a (average particle size 9.0 μm) as a negative electrode active material, styrene-butadiene rubber (SBR) as a binder, carboxymethyl cellulose (CMC) as a thickener, and water as a dispersion medium. The mass ratio of the negative electrode active material, SBR, and CMC was 97.5:1.5:1 (solid content conversion). The negative electrode mixture paste was applied to both sides of copper foil as a negative electrode substrate and dried. Then, roll pressing was performed to obtain negative electrode a. The pore volume A of the negative electrode active material layer was 0.133 cm 3 / g, pore volume B is 0.224 cm 3 The BET specific surface area of the negative electrode active material layer was 5.2 m 2 / g.
[0105] (Non-aqueous electrolyte) A mixture of ethylene carbonate and ethyl methyl carbonate in a volume ratio of 30:70 was added to a solvent with a salt concentration of 1.2 mol / dm 3 LiPF6 was dissolved so as to obtain a non-aqueous electrolyte solution.
[0106] (Separator) The separator used was a microporous polyolefin film.
[0107] (Battery Assembly) A wound type electrode body was obtained using the positive electrode a, the negative electrode a, and a separator. The electrode body was housed in a square container, and a non-aqueous electrolyte was poured in and sealed. A pressure member was attached, and the electrode body was pressed at 0.48 MPa in a discharged state from both sides of the container by this pressure member, to obtain a secondary battery (electricity storage element) of Example 1. The capacity of the secondary battery of Example 1 was designed to be 5.2 Ah.
[0108] [Example 2] Negative electrode b' was obtained in the same manner as negative electrode a in Example 1, except that the negative electrode active material was changed to graphite b (average particle size 10 μm) and the pressure applied during roll pressing was reduced. A secondary battery of Example 2 was obtained in the same manner as in Example 1, except that negative electrode b' was used as the negative electrode. The pore volume A of the negative electrode active material layer in the secondary battery of Example 2 was 0.115 cm 3 / g, pore volume B is 0.301 cm 3 The BET specific surface area of the negative electrode active material layer was 5.7 m 2 / g.
[0109] [Example 3] The positive electrode active material is LiNi 1 / 2 Co 3 / 10 Mn 1 / 5 A positive electrode b was obtained in the same manner as the positive electrode a in Example 1, except that O2 was changed. The peak pore diameter X of the positive electrode active material layer of the positive electrode b was 0.118 μm. A secondary battery of Example 3 was obtained in the same manner as in Example 1, except that the positive electrode b was used as the positive electrode. The pore volume A of the negative electrode active material layer in the secondary battery of Example 3 was 0.133 cm 3 / g, pore volume B is 0.224 cm 3 / g, and the ratio A / B thereof was 0.59.
[0110] [Comparative Example 1] A negative electrode b was obtained in the same manner as the negative electrode a in Example 1, except that the negative electrode active material was changed to graphite b (average particle diameter: 10 μm). A secondary battery of Comparative Example 1 was obtained in the same manner as in Example 1, except that negative electrode b was used as the negative electrode. The pore volume A of the negative electrode active material layer in the secondary battery of Comparative Example 1 was 0.144 cm 3 / g, pore volume B is 0.211 cm 3 The BET specific surface area of the negative electrode active material layer was 4.9 m 2 / g.
[0111] [Comparative Example 2] The positive electrode active material is LiNi 1 / 2 Co 3 / 10 Mn 1 / 5 A positive electrode b' was obtained in the same manner as the positive electrode a in Example 1, except that the oxygen gas was changed to O2 and the conductive agent was changed to furnace black. The peak pore diameter X of the positive electrode active material layer of the positive electrode b' was 0.179 μm. A secondary battery of Comparative Example 2 was obtained in the same manner as in Example 1, except that positive electrode b' was used as the positive electrode. The pore volume A of the negative electrode active material layer in the secondary battery of Comparative Example 2 was 0.153 cm 3 / g, pore volume B is 0.203 cm 3 / g, and the ratio A / B thereof was 0.76.
[0112] [Comparative Example 3] A secondary battery of Comparative Example 3 was obtained in the same manner as in Example 1, except that a positive electrode b' similar to that in Comparative Example 2 was used as the positive electrode, and a negative electrode b similar to that in Comparative Example 1 was used as the negative electrode. The pore volume A of the negative electrode active material layer in the secondary battery of Comparative Example 3 was 0.144 cm 3 / g, pore volume B is 0.211 cm 3 / g, and the ratio A / B thereof was 0.68.
[0113] [evaluation] (Initial Resistance) Each secondary battery obtained was charged at a constant current of 1.0 C in a thermostatic chamber at 25° C. to a voltage equivalent to a SOC (State of Charge) of 50%, and the SOC was adjusted to 50%. After storing in a thermostatic chamber at −30° C. for 3 hours, the battery was discharged at a current of 0.2 C, 0.5 C, or 1.0 C for 30 seconds. After each discharge, the battery was charged at a constant current of 1.0 C to adjust the SOC to 50%. The relationship between the current and the voltage 10 seconds after the start of discharge in each discharge was plotted, and the DC resistance (initial resistance) was calculated from the slope of the straight line obtained by plotting the three points.
[0114] (Charge-discharge cycle test) Next, the following charge-discharge cycle test was carried out. At 60° C., the battery was charged at a constant current of 8 C up to 4.10 V. Thereafter, without a rest period, the battery was discharged at a constant current of 8 C up to 2.50 V. These charging and discharging steps were counted as one cycle, and 1000 cycles were carried out.
[0115] (Rate of increase in resistance) After the charge-discharge cycle test, the DC resistance (resistance after the charge-discharge cycle test) of each secondary battery was determined in the same manner as in the above "initial resistance". The resistance increase rate after the charge-discharge cycle test was calculated by subtracting the initial resistance from the resistance after the charge-discharge cycle test and dividing the result by the initial resistance. The results are shown in Table 1.
[0116] [Table 1]
[0117] As shown in Table 1, in each of the secondary batteries of Examples 1 to 3 in which the ratio (A / B) of the pore volume A to the pore volume B of the negative electrode active material layer was 0.64 or less, the resistance increase rate at low temperature (-30°C) after charge-discharge cycles was reduced. [Industrial Applicability]
[0118] The present invention can be applied to electronic devices such as personal computers and communication terminals, and to energy storage elements used as power sources for automobiles and the like. [Explanation of symbols]
[0119] 1 Energy storage element 2 Electrode body 3 containers 4 Positive terminal 41 Positive lead 5 Negative terminal 51 Negative lead 20 Energy Storage Unit 30 Energy storage device
Claims
1. The battery includes an electrode assembly having a positive electrode including a positive electrode active material layer and a negative electrode including a negative electrode active material layer, and an electrolyte solution; In a discharge state, at least a part of the electrode body is pressed, An energy storage element that satisfies the following formula 1. 0.30≦A / B≦0.64 . . . 1' In formula 1', The A is the pore volume of the negative electrode active material layer having a pore diameter in the range of 0.01 μm or more and less than X μm, The B is a pore volume of the negative electrode active material layer having a pore diameter in the range of X μm or more and 20 μm or less, The above X is a pore diameter that shows the maximum value in the pore diameter range of 0.06 μm or more and 0.2 μm or less in the log differential pore volume distribution of the above positive electrode active material layer.
2. 2. The energy storage element according to claim 1, wherein a pressure of 0.24 MPa or more is applied to at least a portion of the electrode body in a discharged state.
3. the positive electrode active material layer contains a transition metal composite oxide containing nickel, cobalt, and manganese or aluminum, 3. The electric storage element according to claim 1, wherein the negative electrode active material layer contains a carbon material.
4. 4. The energy storage element according to claim 1, having a rated capacity of 4 Ah or more.
Citation Information
Patent Citations
Secondary battery and battery assembly of the same, and vehicle and battery-mounting device equipped with the secondary battery
JP2010146759A
Active material particles, and use of same
JP2011119092A
Power storage element
JP2013073761A
Power storage device
JP2017069002A
Power storage element
JP2018055801A