Adhesive, adhesive sheet and optical adhesive sheet
The adhesive composition, composed of an acrylic copolymer, epoxy resin, and curing agent, addresses the issues of adhesion, heat resistance, and dent resistance in shatterproof films, ensuring effective performance in thin films for display devices.
Patent Information
- Application Number
- JP2020210966
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-21
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2040-12-21
AI Technical Summary
Conventional adhesives used in shatterproof films for display devices do not meet the requirements of high adhesion, heat resistance, and dent resistance, especially in thinner films, and are prone to protrusion after heat treatment.
An adhesive composition comprising an acrylic copolymer, a bisphenol-type epoxy resin, and a curing agent, with specific monomer ratios and molecular weights, enhancing adhesion, heat resistance, and scratch resistance.
The adhesive composition achieves high adhesion, heat resistance, and dent resistance, even in thin films, suitable for both cover glass and housing glass applications, with improved transparency and suitability for optical adhesive sheets.
Smart Images

Figure 0007552340000002 
Figure 0007552340000003 
Figure 0007552340000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a pressure-sensitive adhesive, a pressure-sensitive adhesive sheet, and an optical pressure-sensitive adhesive sheet, each of which contains an acrylic copolymer. [Background technology]
[0002] In recent years, display devices such as smart devices and car navigation systems that use a combination of an image display device such as a liquid crystal display or an organic electroluminescence display with a touch panel have become widespread. In these display devices with an integrated touch panel, a cover panel is provided on the front to protect the module. Furthermore, a shatterproof film with an adhesive layer (hereinafter also referred to as a "film for cover glass") is used to prevent glass from shattering when the cover glass is broken.
[0003] Smartphones and tablets are composed of a cover glass, a module, and a housing that acts as the support. Traditionally, aluminum was used for the housing material, and it was composed of cover glass, module, and aluminum housing, but in recent years, glass has come to be used for the housing material in order to improve communication speed and design. In display devices with glass housings, a shatterproof film with an adhesive layer (hereinafter referred to as "film for housing glass") is used not only on the cover glass but also on the inside surface of the glass housing (between the layers of the module and the glass housing).
[0004] Shatterproof films need to protect glass from external impacts, and the adhesives used in shatterproof films need to have high adhesion and impact resistance (e.g., adhesive strength to glass of 20N or more) so that they do not peel off from the cover glass or casing glass when subjected to impact, such as when a smartphone or tablet is dropped.
[0005] On the other hand, in recent years, the thickness of materials used inside display devices has been reduced due to further weight reduction. The adhesive layer used was previously about 25 μm, but is now mainly used in a thin film (e.g., 5 μm), and high adhesiveness is required in the thin film. Accordingly, a bonding method using heat treatment has begun to be adopted as a method for improving the adhesion of shatterproof films to cover glass and case glass. In the past, the bonding method was to bond the shatterproof film to the cover glass and case glass without heat treatment, but a method is used in which the film is bonded by heat treatment (e.g., 30 minutes in a 150°C atmosphere) to improve the adhesion to the cover glass and case glass. In the case of a bonding method using heat treatment, if the heat resistance of the adhesive is insufficient, the adhesive may protrude from the edge of the film, which can be a problem. The adhesive used in the shatterproof film is required to be heat resistant, and after heat treatment, it is required to have higher adhesiveness than before.
[0006] In addition, with the recent trend towards 5G, the volume of electronic components such as capacitors and coils installed inside smartphones and tablets is increasing. This can lead to problems with poor appearance due to indentations left on the glass housing film caused by the pressure of the electronic components. The adhesive used in the glass housing film needs to be resistant to dents to prevent indentations caused by the electronic components.
[0007] As a shatterproof film, Patent Document 1 discloses an adhesive that contains a polymer and a carbodiimide and has a gel fraction of 10% or more and an acid value of 50 mgKOH / g or less.
[0008] Patent Document 2 discloses a pressure-sensitive adhesive containing a crosslinking agent and a (meth)acrylic copolymer having a glass transition temperature of -35°C or more and -10°C or less and a weight average molecular weight of 450,000 or more and 900,000 or less, the (meth)acrylic copolymer being composed of a constituent unit derived from a (meth)acrylic acid alkyl ester monomer having an alkyl group with 1 to 4 carbon atoms and a constituent unit derived from a monomer having a carboxy group. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2020-70313 A [Patent Document 2] JP 2020-132788 A Summary of the Invention [Problem to be solved by the invention]
[0010] These adhesives have a practical level of adhesion for use as films for conventional cover glass, but they do not have sufficient high adhesion for thinner films or heat resistance to withstand application methods that involve heat treatment. In addition, when used as films for glass housings, they do not meet the requirement of resistance to dents to prevent indentations caused by electronic components.
[0011] In other words, the present invention aims to provide an adhesive that can produce an adhesive sheet that can satisfy the required qualities of high adhesion and heat resistance, which are necessary for shatterproof films, even when the film is thin, and also has excellent dent resistance, which is necessary for films for glass casings. [Means for solving the problem]
[0012] As a result of intensive research, the present inventors have found that the problems of the present invention can be solved in the following aspect, and have completed the present invention. That is, the pressure-sensitive adhesive composition according to the present invention comprises an acrylic copolymer (A), an epoxy resin (B), and a curing agent (C), the acrylic copolymer (A) being a copolymer of a monomer mixture containing the following monomers (a-1) to (a-3), wherein 100% by mass of the monomer mixture contains 10 to 50% by mass of monomer (a-1), 40 to 80% by mass of monomer (a-2), and 5 to 10% by mass of monomer (a-3), and the epoxy resin (B) is a bisphenol-type epoxy resin having a weight average molecular weight (Mw) of 200 to 1,000. (a-1) (Meth)acrylic acid alkyl ester monomer having an alkyl group having 8 to 12 carbon atoms (a-2) (Meth)acrylic acid ester monomers having a homopolymer glass transition temperature of 0 to 100°C (excluding monomers (a-1) and (a-3)) (a-3) (Meth)acrylic acid alkyl ester monomer having a carboxyl group Effect of the Invention
[0013] The present invention makes it possible to provide a pressure-sensitive adhesive sheet that can satisfy the required qualities of shatterproof films, namely high adhesion and heat resistance, even when thin, and also has excellent dent resistance, which is necessary for films for glass casings. In addition, because of its excellent transparency, it can be suitably used as a shatterproof film for optical members. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The terms used in this specification are defined. (Meth)acrylic acid ester includes acrylic acid ester and methacrylic acid ester. Monomer is an ethylenically unsaturated group-containing monomer. Adherend refers to a counterpart to which the pressure-sensitive adhesive sheet is attached. In the present invention, sheet, film, and tape are synonymous terms. In this specification, the acrylic copolymer (A), (a-1) (meth)acrylic acid alkyl ester monomer having an alkyl group with 8 to 12 carbon atoms, (a-2) (meth)acrylic acid ester monomer having a homopolymer glass transition temperature of 0 to 100°C, (a-3) (meth)acrylic acid alkyl ester monomer having a carboxyl group, and bisphenol-type epoxy resin (B) having a weight average molecular weight (Mw) of 300 to 1000 may be abbreviated as copolymer (A), monomer (a-1), monomer (a-2), monomer (a-3), and epoxy resin (B), respectively. Unless otherwise noted, the various components appearing in this specification may be used independently as a single type, or as a mixture of two or more types. The following describes in detail the embodiments of the present invention. However, the following description is an example (representative example) of an embodiment of the present invention, and the present invention is not limited to these contents as long as it does not deviate from the gist of the present invention.
[0015] The pressure-sensitive adhesive composition of the present invention comprises an acrylic copolymer (A), an epoxy resin (B), and a curing agent (C), The acrylic copolymer (A) is a copolymer of a monomer mixture containing the following monomers (a-1) to (a-3): The monomer mixture contains 10 to 50 mass% of monomer (a-1), 40 to 80 mass% of monomer (a-2), and 5 to 10 mass% of monomer (a-3) based on 100 mass% of the monomer mixture, The epoxy resin (B) is a bisphenol type epoxy resin having a weight average molecular weight (Mw) of 200-1,000. (a-1) (Meth)acrylic acid alkyl ester monomer having an alkyl group having 8 to 12 carbon atoms (a-2) (Meth)acrylic acid ester monomers having a homopolymer glass transition temperature of 0 to 100°C (excluding monomers (a-1) and (a-3)) (a-3) (Meth)acrylic acid alkyl ester monomer having a carboxyl group
[0016] The pressure-sensitive adhesive composition of the present invention is preferably used as a pressure-sensitive adhesive sheet having a substrate by forming a pressure-sensitive adhesive layer by coating the pressure-sensitive adhesive composition. The pressure-sensitive adhesive sheet is preferably used as an optical pressure-sensitive adhesive sheet for use in optical members, for example.
[0017] Adhesive Composition The adhesive composition of the present invention uses specific amounts of each of the (meth)acrylic acid alkyl ester monomer (a-1) having an alkyl group with 8 to 12 carbon atoms, the (meth)acrylic acid ester monomer (a-2) having a homopolymer glass transition temperature of 0 to 100°C, and the (meth)acrylic acid alkyl ester monomer (a-3) having a carboxyl group as monomers constituting the acrylic copolymer (A), thereby obtaining a trade-off property of achieving both hardness and softness in the adhesive layer. Therefore, even if the adhesive layer is thin, it can achieve both high adhesion and heat resistance and also have excellent dent resistance.
[0018] The adhesive composition of the present invention is suitable as an adhesive sheet, and can also be very useful as a raw material for various plastic sheets, general labels and stickers, tackifiers, adhesives for laminated structures, and sealants, as well as various resin additives and their raw materials, etc.
[0019] <Acrylic copolymer (A)> The acrylic copolymer (A) in this specification is a copolymer of a monomer mixture containing (a-1) a (meth)acrylic acid alkyl ester monomer having an alkyl group with 8 to 12 carbon atoms, (a-2) a (meth)acrylic acid ester monomer having a homopolymer glass transition temperature of 0 to 100°C, and (a-3) a (meth)acrylic acid alkyl ester monomer having a carboxyl group. The monomer mixture contains 10 to 50 mass % of monomer (a-1), 40 to 80 mass % of monomer (a-2), and 5 to 10 mass % of monomer (a-3) based on 100 mass % of the monomer mixture. Other monomers may be used in combination as long as the effects of the present invention are not impaired.
[0020] [Monomer (a-1)] The monomer (a-1) is a (meth)acrylic acid alkyl ester monomer having an alkyl group having 8 to 12 carbon atoms, except for the monomer (a-3). By containing the monomer (a-1), it is possible to impart sufficient wettability and cohesiveness to the adhesive layer, and to improve the adhesion to the substrate. If the number of carbon atoms is less than 8, the flexibility of the adhesive layer decreases, and the adhesion to the substrate decreases. Also, if the number of carbon atoms exceeds 12, the rigidity of the adhesive layer decreases, and the durability decreases.
[0021] Examples of the monomer (a-1) include n-octyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, undecyl (meth)acrylate, and dodecyl (meth)acrylate.
[0022] Among the monomers (a-1), 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, and dodecyl (meth)acrylate are preferred in terms of achieving both flexibility and cohesiveness.
[0023] The content of monomer (a-1) is 10 to 50 mass%, and more preferably 20 to 40 mass%, in 100 mass% of the monomer mixture. When the content is 10 mass% or more, sufficient adhesiveness is obtained, and when the content is 50 mass% or less, adhesive strength, heat resistance, and dent resistance can be simultaneously achieved at high levels.
[0024] [Monomer (a-2)] The monomer (a-2) is a (meth)acrylic acid ester monomer having a homopolymer glass transition temperature (Tg) of 0 to 100° C., except for the monomers (a-1) and (a-3). By containing the monomer (a-2), it is possible to impart sufficient cohesiveness to the adhesive layer and improve adhesion to the substrate. If the glass transition temperature of the homopolymer is less than 0°C, the rigidity of the adhesive layer decreases and the heat resistance decreases. If the glass transition temperature of the homopolymer is more than 100°C, the flexibility of the adhesive layer decreases and the adhesiveness decreases. More preferably, it is a (meth)acrylic acid ester monomer having a Tg of 5 to 100°C, and even more preferably, it is a (meth)acrylic acid ester monomer having a Tg of 10 to 95°C. Here, a monomer having a homopolymer glass transition temperature of 0 to 100° C. means a monomer having a Tg of 0 to 100° C. when polymerized to form a homopolymer. The Tg of the homopolymer may be a published value such as a literature value or a catalog value.
[0025] Examples of the monomer (a-2) include (meth)acrylic acid alkyl ester monomers having a homopolymer glass transition temperature of 0 to 100°C, alicyclic (meth)acrylic acid ester monomers having a homopolymer glass transition temperature of 0 to 100°C, aromatic (meth)acrylic acid ester monomers having a homopolymer glass transition temperature of 0 to 100°C, and amino group-containing (meth)acrylic acid ester monomers having a homopolymer glass transition temperature of 0 to 100°C.
[0026] Examples of (meth)acrylic acid alkyl ester monomers having a homopolymer glass transition temperature of 0 to 100° C. include methyl (meth)acrylate, ethyl methacrylate, propyl methacrylate, isopropyl methacrylate, butyl methacrylate, isobutyl methacrylate, and t-butyl methacrylate.
[0027] Examples of alicyclic (meth)acrylic acid ester monomers having a homopolymer glass transition temperature of 0 to 100° C. include cyclohexyl (meth)acrylate and isobornyl acrylate.
[0028] Examples of aromatic (meth)acrylic acid ester monomers having a homopolymer glass transition temperature of 0 to 100° C. include benzyl (meth)acrylate and phenoxyethyl (meth)acrylate.
[0029] Examples of amino group-containing monomers having a homopolymer glass transition temperature of 0 to 100° C. include dimethylaminoethyl methacrylate and diethylaminoethyl methacrylate.
[0030] Among the (meth)acrylic acid ester monomers (a-2) having a homopolymer glass transition temperature of 0 to 100°C, methyl (meth)acrylate, isobornyl acrylate, benzyl (meth)acrylate, and dimethylaminoethyl methacrylate are preferred in terms of achieving both flexibility and cohesiveness, and methyl (meth)acrylate and isobornyl acrylate are more preferred in terms of heat resistance and dent resistance.
[0031] The content of monomer (a-2) is 40 to 80 mass% and more preferably 30 to 70 mass% in 100 mass% of the monomer mixture. When the content is 40 mass% or more, sufficient cohesive strength is obtained, thereby improving heat resistance, and when the content is 80 mass% or less, transparency, heat resistance, and adhesion can be simultaneously achieved at a high level.
[0032] [Monomer (a-3)] The monomer (a-3) is a (meth)acrylic acid alkyl ester monomer having a carboxyl group. Note that even if the monomer has an alkyl group having 8 to 12 carbon atoms, or the (meth)acrylic acid ester monomer has a homopolymer glass transition temperature (Tg) of 0 to 100° C., it falls under the category of monomer (a-3) if it has a carboxyl group. By including the monomer (a-3), it is possible to impart sufficient rigidity to the adhesive layer, improving heat resistance, and also increasing the polarity of the adhesive layer, improving adhesion to highly polar adherends.
[0033] Examples of the monomer (a-3) include (meth)acrylic acid, p-carboxybenzyl acrylate, β-carboxyethyl acrylate, maleic acid, monoethyl maleic acid, itaconic acid, citraconic acid, and fumaric acid. Among these, (meth)acrylic acid is preferred in terms of ensuring sufficient adhesiveness.
[0034] The content of monomer (a-3) is 5 to 15 mass% and more preferably 5 to 10 mass% in 100 mass% of the monomer mixture. When the content is 5 mass% or more, sufficient cohesive strength is obtained and heat resistance is improved, and when the content is 15 mass% or less, sufficient adhesion can be ensured and adhesiveness is improved.
[0035] [Other monomers] In addition to the monomers (a-1), (a-2) and (a-3), other monomers may be used in the copolymer (A). Examples of the other monomer include (meth)acrylic acid alkyl ester monomers other than the (meth)acrylic acid alkyl ester monomer (a-1) having an alkyl group having 8 to 12 carbon atoms, the homopolymer of which has a glass transition temperature of less than 0°C, (meth)acrylic acid alkyl ester monomers having a hydroxyl group, monomers having an amide bond, (meth)acrylic acid monomers having an epoxy group, and vinyl monomers.
[0036] Examples of (meth)acrylic acid alkyl ester monomers having a homopolymer glass transition temperature of less than 0°C other than the (meth)acrylic acid alkyl ester monomer (a-1) having an alkyl group having 8 to 12 carbon atoms include ethyl acrylate, propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, and t-butyl acrylate.
[0037] Examples of (meth)acrylic acid alkyl ester monomers having a hydroxyl group include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, (meth)acrylic acid, and 4-hydroxybutyl (meth)acrylate.
[0038] Examples of the monomer having an amide bond include (meth)acrylamide-based compounds such as (meth)acrylamide, N-methylacrylamide, N-isopropylacrylamide, N,N-dimethylacrylamide, N,N-diethylacrylamide, N,N-dimethylaminopropyl(meth)acrylamide, diacetoneacrylamide, and N-(butoxymethyl)acrylamide; Examples of the heterocyclic compound include compounds having a heterocycle such as N-vinylpyrrolidone, N-vinylcaprolactam, and acryloylmorpholine.
[0039] Examples of monomers having an epoxy group include glycidyl (meth)acrylate, methyl glycidyl (meth)acrylate, 3,4-epoxycyclohexylmethyl (meth)acrylate, and 6-methyl-3,4-epoxycyclohexylmethyl (meth)acrylate.
[0040] Examples of the vinyl monomer include vinyl acetate, vinyl crotonate, styrene, and acrylonitrile.
[0041] The content of the other monomer is preferably 5 to 30% by weight in 100% by mass of the monomer mixture. When the content is 5% by weight or more, the adhesion is further improved. Also, when the content is 30% by weight or less, it is easy to achieve both cohesive strength and adhesion.
[0042] [Method for producing copolymer (A)] The copolymer (A) can be synthesized by polymerizing a monomer mixture. The polymerization can be performed by a known polymerization method such as solution polymerization, bulk polymerization, emulsion polymerization, suspension polymerization, etc., but solution polymerization is preferred. The solvent used in the solution polymerization is preferably, for example, acetone, methyl acetate, ethyl acetate, toluene, xylene, anisole, methyl ethyl ketone, cyclohexanone, etc. The polymerization temperature is preferably a boiling point reaction at 60 to 120° C. The polymerization time is preferably about 5 to 12 hours.
[0043] The polymerization initiator used in the polymerization is preferably a radical polymerization initiator, and the radical polymerization initiator is generally a peroxide or an azo compound. Examples of peroxides include dialkyl peroxides such as di-t-butyl peroxide, dicumyl peroxide, t-butylcumyl peroxide, α,α'-bis(t-butylperoxy-m-isopropyl)benzene, and 2,5-di(t-butylperoxy)hexyne-3; Peroxyesters such as t-butyl peroxybenzoate, t-butyl peroxyacetate, and 2,5-dimethyl-2,5-di(benzoylperoxy)hexane; ketone peroxides such as cyclohexanone peroxide, 3,3,5-trimethylcyclohexanone peroxide, and methylcyclohexanone peroxide; Peroxyketals such as 2,2-bis(4,4-di-t-butylperoxycyclohexyl)propane, 1,1-bis(t-butylperoxy)3,3,5-trimethylcyclohexane, 1,1-bis(t-butylperoxy)cyclohexane, and n-butyl-4,4-bis(t-butylperoxy)valerate; Hydroperoxides such as cumene hydroperoxide, diisopropylbenzene hydroperoxide, and 2,5-dimethylcyclohexane-2,5-dihydroperoxide; diacyl peroxides such as benzoyl peroxide, decanoyl peroxide, lauroyl peroxide, and 2,4-dichlorobenzoyl peroxide; Examples include peroxydicarbonates such as bis(t-butylcyclohexyl) peroxydicarbonate.
[0044] Examples of the azo compound include 2,2'-azobisbutyronitrile such as 2,2'-azobisisobutyronitrile (ABN) and 2,2'-azobis(2-methylbutyronitrile); 2,2'-azobisvaleronitrile such as 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile) and 2,2'-azobis(2,4-dimethylvaleronitrile); 2,2'-azobispropionitriles, such as 2,2'-azobis(2-hydroxymethylpropionitrile); Examples include 1,1'-azobis-1-alkanenitriles such as 1,1'-azobis(cyclohexane-1-carbonitrile).
[0045] The polymerization initiator is preferably used in an amount of 0.01 to 10 parts by mass, more preferably 0.1 to 2 parts by mass, based on 100 parts by mass of the monomer mixture.
[0046] The weight average molecular weight of the copolymer (A) is preferably 300,000 to 1,800,000, more preferably 500,000 to 1,200,000. When it is in the range of 300,000 to 1,800,000, the cohesive force is improved, and the wet heat resistance and heat resistance are improved. The weight average molecular weight and the number average molecular weight are values measured by gel permeation chromatography (GPC) in terms of polystyrene. Details of the GPC measurement method are described in the Examples.
[0047] <Epoxy resin (B)> The epoxy resin (B) is a bisphenol type epoxy resin with a weight average molecular weight (Mw) of 200 to 1000. By including the epoxy resin (B), high adhesion to the adherend is exhibited. In particular, when used as an adhesive layer for a film for a glass housing, the adhesive hardness after heat treatment can be improved, and high heat resistance and dent resistance are exhibited.
[0048] Epoxy resin (B) is -O-Ph-CR 1 R 2 It is a compound that has a bisphenol skeleton in the molecule, as represented by -Ph-O-, and has an epoxy group as a functional group. Ph is an aromatic hydrocarbon group, and R 1 , R 2 are each independently a hydrogen atom or a methyl group. Examples of such bisphenol type epoxy resins (B) include JER825 (Mw=350), JER828 (Mw=370), JER806 (Mw=330), and JER1001 (Mw=900) (all manufactured by Mitsubishi Chemical Corporation).
[0049] The weight average molecular weight (Mw) of the epoxy resin (B) is 200 to 1000, and more preferably 300 to 900. When the weight average molecular weight (Mw) is 200 or more, sufficient cohesive force is obtained, and heat resistance and dent resistance are improved. When the weight average molecular weight (Mw) is 1000 or less, transparency and sufficient adhesion can be ensured, and adhesion is improved, as well as heat resistance and dent resistance.
[0050] The epoxy resin (B) is preferably contained in an amount of 5 to 45 parts by weight, more preferably 10 to 40 parts by weight, per 100 parts by weight of the acrylic copolymer (A). When the content is 5 parts by weight or more, sufficient cohesive strength is easily obtained, and when the content is 45 parts by weight or less, sufficient adhesion can be ensured, improving the adhesiveness.
[0051] <Hardening agent (C)> The curing agent (C) reacts with the carboxyl groups of the copolymer (A) to improve the cohesive strength of the adhesive layer, and further improve the adhesion, heat resistance, and dent resistance.
[0052] Examples of the curing agent (C) include an isocyanate compound, an epoxy compound, an aziridine compound, a carbodiimide compound, a metal chelate, etc. However, the epoxy resin (B) is excluded. Among these, isocyanate compounds are preferred from the viewpoint of achieving both high cohesive strength and adhesion. Use of an isocyanate compound can improve heat-resistant adhesiveness.
[0053] The isocyanate compound is an isocyanate having two or more isocyanate groups. The isocyanate compound is preferably, for example, an isocyanate monomer such as an aromatic polyisocyanate, an aliphatic polyisocyanate, an araliphatic polyisocyanate, or an alicyclic polyisocyanate, as well as a biuret, a nurate, or an adduct thereof.
[0054] Examples of aromatic polyisocyanates include 1,3-phenylene diisocyanate, 4,4'-diphenyl diisocyanate, 1,4-phenylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 4,4'-toluidine diisocyanate, 2,4,6-triisocyanate toluene, 1,3,5-triisocyanate benzene, dianisidine diisocyanate, 4,4'-diphenyl ether diisocyanate, and 4,4',4"-triphenylmethane triisocyanate.
[0055] Examples of aliphatic polyisocyanates include trimethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate (also known as HMDI), pentamethylene diisocyanate, 1,2-propylene diisocyanate, 2,3-butylene diisocyanate, 1,3-butylene diisocyanate, dodecamethylene diisocyanate, and 2,4,4-trimethylhexamethylene diisocyanate.
[0056] Examples of the aromatic aliphatic polyisocyanate include ω,ω'-diisocyanate-1,3-dimethylbenzene, ω,ω'-diisocyanate-1,4-dimethylbenzene, ω,ω'-diisocyanate-1,4-diethylbenzene, 1,4-tetramethylxylylene diisocyanate, and 1,3-tetramethylxylylene diisocyanate.
[0057] Examples of alicyclic polyisocyanates include 3-isocyanatemethyl-3,5,5-trimethylcyclohexyl isocyanate (also known as IPDI, isophorone diisocyanate), 1,3-cyclopentane diisocyanate, 1,3-cyclohexane diisocyanate, 1,4-cyclohexane diisocyanate, methyl-2,4-cyclohexane diisocyanate, methyl-2,6-cyclohexane diisocyanate, 4,4'-methylenebis(cyclohexyl isocyanate), and 1,4-bis(isocyanatemethyl)cyclohexane.
[0058] The biuret form is a self-condensation product having a biuret bond formed by self-condensation of an isocyanate monomer, for example, a biuret form of hexamethylene diisocyanate.
[0059] The nurate form is a trimer of an isocyanate monomer, such as a trimer of hexamethylene diisocyanate, a trimer of isophorone diisocyanate, or a trimer of tolylene diisocyanate.
[0060] The adduct is a bifunctional or higher isocyanate compound obtained by reacting an isocyanate monomer with a bifunctional or higher low-molecular active hydrogen-containing compound. Examples of the adduct include a compound obtained by reacting trimethylolpropane with hexamethylene diisocyanate, a compound obtained by reacting trimethylolpropane with tolylene diisocyanate, a compound obtained by reacting trimethylolpropane with xylylene diisocyanate, a compound obtained by reacting trimethylolpropane with isophorone diisocyanate, and a compound obtained by reacting 1,6-hexanediol with hexamethylene diisocyanate.
[0061] The isocyanate compound is preferably a trifunctional isocyanate compound from the viewpoint of forming a sufficient crosslinked structure. The isocyanate compound is more preferably an adduct or nurate, which is a reaction product between an isocyanate monomer and a trifunctional low molecular weight active hydrogen-containing compound. The isocyanate compound is preferably a trimethylolpropane adduct of hexamethylene diisocyanate, a nurate of hexamethylene diisocyanate, a trimethylolpropane adduct of tolylene diisocyanate, a nurate of tolylene diisocyanate, a trimethylolpropane adduct of isophorone diisocyanate, or a nurate of isophorone diisocyanate, and more preferably a trimethylolpropane adduct of hexamethylene diisocyanate, a trimethylolpropane adduct of tolylene diisocyanate, or a trimethylolpropane adduct of isophorone diisocyanate.
[0062] Examples of epoxy compounds include glycerin diglycidyl ether, 1,6-hexanediol diglycidyl ether, N,N,N',N'-tetraglycidyl-m-xylylenediamine, 1,3-bis(N,N'-diglycidylaminomethyl)cyclohexane, and N,N,N',N'-tetraglycidylaminophenylmethane.
[0063] Examples of the aziridine compound include N,N'-diphenylmethane-4,4'-bis(1-aziridinecarboxite), tris-2,4,6-(1-aziridinyl)-1,3,5-triazine, and 4,4'-bis(ethyleneiminocarbonylamino)diphenylmethane.
[0064] The carbodiimide compound is preferably a high molecular weight polycarbodiimide produced by decarboxylation condensation of a diisocyanate compound in the presence of a carbodiimide catalyst. The commercially available high molecular weight polycarbodiimide is preferably the Carbodilite series from Nisshinbo Industries, Ltd. Among them, Carbodilite V-03, 07, and 09 are preferred because of their excellent compatibility with organic solvents.
[0065] The metal chelate is preferably a coordination compound of a polyvalent metal such as aluminum, iron, copper, zinc, tin, titanium, nickel, antimony, magnesium, vanadium, chromium, or zirconium with acetylacetone or ethyl acetoacetate. Examples of the metal chelate include aluminum ethyl acetoacetate diisopropylate, aluminum trisacetylacetonate, aluminum bisethyl acetoacetate monoacetylacetonate, and aluminum alkyl acetoacetate diisopropylate.
[0066] The curing agent (B) is preferably contained in an amount of 0.01 to 5 parts by mass, more preferably 0.01 to 2 parts by mass, based on 100 parts by mass of the copolymer (A). When the content is 0.01 part by mass or more, the cohesive strength is further improved, and when the content is 5 parts by mass or less, it is preferable that the cohesive strength and flexibility are both easily achieved.
[0067] <Silane coupling agent (D)> The pressure-sensitive adhesive composition of the present invention can contain a silane coupling agent (D) as long as the problem can be solved. By containing the silane coupling agent (D), adhesion to glass is improved, and in particular, heat-resistant adhesion after heat treatment is dramatically improved.
[0068] Examples of the silane coupling agent (D) include alkoxysilane compounds having a (meth)acryloxy group, such as 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropyltriethoxysilane, 3-(meth)acryloxypropyltripropoxysilane, 3-(meth)acryloxypropyltributoxysilane, 3-(meth)acryloxypropylmethyldimethoxysilane, and 3-(meth)acryloxypropylmethyldiethoxysilane; Alkoxysilane compounds having a vinyl group, such as vinyltrimethoxysilane, vinyltriethoxysilane, vinyltriisopropoxysilane, vinyltributoxysilane, vinylmethyldimethoxysilane, and vinylmethyldiethoxysilane; alkoxysilane compounds having an amino group, such as 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropyltripropoxysilane, 3-aminopropylmethyldimethoxysilane, 3-aminopropylmethyldiethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldiethoxysilane, and N-phenyl-3-aminopropyltrimethoxysilane; alkoxysilane compounds having a mercapto group, such as 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 3-mercaptopropyltripropoxysilane, 3-mercaptopropylmethyldimethoxysilane, and 3-mercaptopropylmethyldiethoxysilane; alkoxysilane compounds having an epoxy group, such as 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropyltripropoxysilane, 3-glycidoxypropyltributoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; tetraalkoxysilane compounds such as tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, and tetrabutoxysilane; Examples of the silane include 3-chloropropyltrimethoxysilane, n-hexyltrimethoxysilane, n-hexyltriethoxysilane, n-decyltrimethoxysilane, n-decyltriethoxysilane, styryltrimethoxysilane, phenyltrimethoxysilane, diphenyldimethoxysilane, 3-triethoxysilyl-N-(1,3-dimethylbutylidene)propylamine, 1,3,5-tris(3-trimethoxysilylpropyl)isocyanurate, 3-isocyanatepropyltrimethoxysilane, 3-isocyanatepropyltriethoxysilane, hexamethyldisilazane, and silicone resins having alkoxysilyl groups in the molecule.
[0069] The silane coupling agent (D) is preferably used in an amount of 0.01 to 2 parts by mass, more preferably 0.05 to 1 part by mass, based on 100 parts by mass of the copolymer (A).
[0070] <Optional ingredients> The pressure-sensitive adhesive composition of the present invention may contain various resins, oils, softeners, dyes, pigments, antioxidants, UV absorbers, weather stabilizers, plasticizers, fillers, antioxidants, antistatic agents, and the like as optional components, so long as the problem can be solved.
[0071] Adhesive sheet The pressure-sensitive adhesive sheet of the present invention comprises an adhesive layer which is a cured product of the pressure-sensitive adhesive composition, and preferably comprises a substrate and an adhesive layer which is a cured product of the pressure-sensitive adhesive composition. The adhesive sheet is produced, for example, by coating an adhesive composition on a substrate and drying to form an adhesive layer. Alternatively, the adhesive sheet can be produced by coating an adhesive composition on a release sheet and drying to form an adhesive layer, and then laminating the substrate. Furthermore, the surface of the adhesive layer that is not in contact with the substrate is usually used with a release sheet laminated thereon until immediately before use in order to prevent adhesion of foreign matter. The drying temperature is usually about 60 to 150°C. The thickness of the adhesive layer is usually about 0.1 to 200 μm. The pressure-sensitive adhesive composition of the present invention can be used in a thickness range that is normally used, and has the excellent effect of being able to achieve sufficient adhesion and heat resistance even in a thin film of 0.1 to 30 μm, or even 0.1 to 10 μm.
[0072] Examples of the coating method include known methods such as a roll coater method, a comma coater method, a die coater method, a reverse coater method, a silk screen method, and a gravure coater method.
[0073] When applying the pressure-sensitive adhesive composition, the viscosity can be adjusted by using a solvent. Examples of the solvent include hydrocarbon solvents such as toluene, xylene, hexane, and heptane; ester solvents such as ethyl acetate and butyl acetate; ketone solvents such as acetone and methyl ethyl ketone; halogenated hydrocarbon solvents such as dichloromethane and chloroform; and ether solvents such as diethyl ether, methoxytoluene, and dioxane.
[0074] The substrate may be any flexible sheet or plate material without limitation, and examples of the substrate include plastic, paper, metal foil, and laminates thereof. In order to improve adhesion, the surface of the substrate that comes into contact with the adhesive layer may be previously subjected to an adhesion enhancing treatment, for example, a dry treatment such as a corona discharge treatment or a wet treatment such as application of an anchor coating agent. The substrate may be a single optical film or a laminate of a plurality of optical films. The thickness of the substrate is usually about 10 to 250 μm.
[0075] The release sheet may be a known release sheet having a surface of plastic or paper that has been subjected to a known release treatment using a silicone-based release agent or the like. The thickness of the release sheet is usually about 10 to 250 μm.
[0076] The adherend can be any one of various types without any particular limitations. Examples of the adherend include general-purpose glass, building materials, plastics such as polyolefin, ABS, polystyrene, and acrylic, cardboard, wood, plywood, stainless steel, and metals such as aluminum, as well as optical members such as non-alkali glass, polarizing plates, elliptically polarizing films, transparent conductive films, retardation films, anti-reflection films, brightness enhancing films, and super-water-repellent glass. The pressure-sensitive adhesive sheet of the present invention can be suitably used as an optical pressure-sensitive adhesive sheet for use in optical members as adherends.
[0077] <Optical adhesive sheet> The adhesive layer, which is the cured product of the adhesive composition of the present invention, has excellent transparency and can be suitably used as an optical adhesive sheet. The optical adhesive sheet is an adhesive sheet that is attached to an optical member and is suitable as a surface protection sheet for a display device, etc. In addition, since it has high adhesion and excellent heat resistance in a thin film, good shatterproof properties, and excellent resistance to dents to prevent indentations caused by electronic components, it can be suitably used not only as a film for cover glass but also as a film for housing glass.
[0078] When the optical pressure-sensitive adhesive sheet has a substrate, it preferably has an optical film as the substrate and a pressure-sensitive adhesive layer which is a cured product of a pressure-sensitive adhesive composition. The optical adhesive sheet is produced, for example, by coating an adhesive composition on an optical film and drying the same to form an adhesive layer. Alternatively, the optical adhesive sheet can be produced by coating an adhesive composition on a release sheet and drying the same to form an adhesive layer, and then laminating the optical film. Furthermore, the surface of the adhesive layer that is not in contact with the optical film is usually used with a release sheet laminated thereon until immediately before use in order to prevent adhesion of foreign matter. The drying temperature is usually about 60 to 150° C. The thickness of the adhesive layer is usually about 0.1 to 200 μm.
[0079] The optical film is a transparent film that can transmit light, and examples of the optical film include polyester resins such as polyvinyl alcohol, triacetyl cellulose, polyolefins (polypropylene, polyethylene), polycycloolefins, ethylene-vinyl acetate copolymers, polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate, polyacrylic resins such as polymethyl methacrylate and polybutyl methacrylate, polycarbonate resins, polynorbornene resins, polyarylate resins, polyacrylic resins, polyphenylene sulfide resins, polystyrene resins, polyamide resins, polyimide resins, and epoxy resins.
[0080] The optical pressure-sensitive adhesive sheet of the present invention can be suitably used as a shatterproof film for optical members, such as optical glass, water-repellent glass, decorative printed glass, polarizing plates, elliptically polarizing films, transparent conductive films, retardation films, anti-reflection films, and brightness-enhancing films.
[0081] Here, super-water-repellent glass is a surface-treated glass in which hydrophobic substances such as fluorine or silicon are coated or vapor-deposited on the glass surface, and then fine irregularities of 10 to 500 nm are formed on the surface, making it a material that has both oil-repellent and water-repellent properties.This allows for a high degree of prevention of surface contamination caused by moisture, sweat, and sebum.
[0082] Furthermore, the uses of the optical adhesive sheet of the present invention are not particularly limited, but it can also be used as a shatterproof film for various electronics-related components such as liquid crystal displays, organic EL displays, plasma displays, touch screen panels, car navigation systems, in-vehicle interior display devices, and electrode peripheral components.
[0083] Furthermore, in recent years, shatterproof films for display devices such as smartphones and tablets require properties that were not previously required, such as heat resistance during heat treatment processes and resistance to dents caused by the pressure of electronic components such as capacitors and coils that are installed inside.
[0084] As described above, the adhesive composition of the present invention, which is composed of the copolymer (A), the epoxy resin (B), and the curing agent (C), has a specific content of both the long-chain (meth)acrylic acid alkyl ester monomer-derived structural unit and the high Tg (meth)acrylic acid ester monomer-derived structural unit, and thus the adhesiveness to glass is dramatically improved, and both adhesiveness and heat resistance can be achieved. In addition, by containing the epoxy resin (B), high dent resistance can be achieved without impairing adhesiveness, and the adhesive composition can be applied as a shatterproof film. Furthermore, by containing the curing agent (C), the cohesive force of the adhesive layer is improved, and the adhesiveness, heat resistance, and dent resistance are excellent. In addition, the pressure-sensitive adhesive composition of the present invention not only can be used in a thickness range that is normally used, but also has the excellent effect of being able to achieve sufficient adhesion and heat resistance even in a thinner thickness than before. EXAMPLES
[0085] Next, the present invention will be described in more detail with reference to examples, but the present invention is not limited thereto. In the examples, unless otherwise specified, "parts" means "parts by mass" and "%" means "% by mass". The blend amounts in the tables are parts by mass, and values other than the solvent are calculated as non-volatile contents. Note that blanks in the tables indicate that no blend was made. The Tg of the monomers used in the following examples indicates the Tg of the homopolymer. Published values such as literature values and catalog values were used for the Tg of the homopolymer. The weight average molecular weight of the copolymer is measured by the following method.
[0086] <Measurement of weight average molecular weight (Mw)> The weight average molecular weight (Mw) was measured using a GPC "LC-GPC system" manufactured by Shimadzu Corporation. The weight average molecular weight (Mw) was determined by conversion using polystyrene with a known molecular weight as the standard substance. Device name: Shimadzu Corporation, LC-GPC system "Prominence" Column: Four GMHXL columns manufactured by Tosoh Corporation and one HXL-H column manufactured by Tosoh Corporation were connected together. Mobile phase solvent: Tetrahydrofuran Flow rate: 1.0ml / min Column temperature: 40℃
[0087] <Production of Acrylic Copolymer> (Synthesis example 1: Copolymer (A)) A reaction vessel (hereinafter simply referred to as "reaction vessel") equipped with a stirrer, a thermometer, a reflux condenser, a dropping device, and a nitrogen inlet tube was charged with 10 parts of 2-ethylhexyl acrylate (EHA), 80 parts of methyl acrylate (MA), 10 parts of acrylic acid, 100 parts of ethyl acetate, and 0.2 parts of 2,2'-azobisisobutyronitrile (hereinafter referred to as AIBN), and the atmosphere in the reaction vessel was replaced with nitrogen gas. Then, the mixture was heated to 65°C while stirring under a nitrogen atmosphere to start the reaction. The reaction solution was then reacted at 65°C for 4 hours. After the reaction was completed, the mixture was cooled and diluted with ethyl acetate to obtain a copolymer (A-1) solution with a non-volatile content of 30%. The weight average molecular weight of the obtained copolymer (A-1) was 1.8 million.
[0088] (Synthesis Examples 2 to 18) An acrylic copolymer was produced in the same manner as in Synthesis Example 1, except that the raw materials and the amounts used were changed according to the mass ratios in Table 1. The weight average molecular weight (Mw) of the obtained copolymer is shown in Table 1.
[0089] [Table 1]
[0090] [Monomer (a-1)] EHA: 2-Ethylhexyl acrylate OTA: n-octyl acrylate DCA: Dodecyl acrylate [Monomer (a-2)] MA: Methyl acrylate (Tg: 6℃) IBXA: Isobornyl acrylate (Tg: 97℃) BzA: Benzyl acrylate (Tg: 6℃) DMAEMA: Dimethylaminoethyl methacrylate (Tg: 18℃) [Monomer (a-3)] AA: Acrylic acid MAA: Methacrylic acid [Other monomers] BA: n-Butyl acrylate EA: Ethyl acrylate
[0091] Example 1 <Preparation of Adhesive> In the obtained copolymer (A-1) solution, 100 parts by weight of copolymer (A-1) was mixed with 5 parts by weight of epoxy resin (B-1) "JER825" (bisphenol type epoxy resin, Mw=350, manufactured by Mitsubishi Chemical Corporation) as epoxy resin (B), 0.01 parts by weight of curing agent (C-1) "adduct of hexamethylene diisocyanate and trimethylolpropane" as curing agent (C), and ethyl acetate was added so that the non-volatile content was 20%, and the mixture was stirred to obtain an adhesive solution.
[0092] <Preparation of adhesive sheet> The obtained adhesive solution was applied onto a 50 μm-thick release sheet (polyethylene terephthalate (PET), "E7004", silicone-based release layer, manufactured by Toyobo Co., Ltd.) so that the thickness after drying was 5 μm, and the coating was dried at 120° C. for 3 minutes to form an adhesive layer. Next, one side of a 38 μm-thick release sheet (polyethylene terephthalate, "SP-PET3811", silicone-based release layer, manufactured by Lintec Co., Ltd.) was attached to this adhesive layer to prepare a "release sheet / adhesive layer / release sheet" laminate. Next, the obtained laminate was aged for 1 week under conditions of a temperature of 25° C. and a relative humidity of 55%, to obtain an adhesive sheet.
[0093] (Examples 2 to 12, Comparative Examples 1 to 8) As shown in Table 2, pressure-sensitive adhesive sheets were obtained in the same manner as in Example 1, except that the types and amounts of copolymer, epoxy resin, and curing agent were changed.
[0094] (Example 13) <Preparation of Adhesive> In the copolymer (A-2) solution, 100 parts by weight of the copolymer (A-2) was mixed with 5 parts by weight of JER825 (bisphenol type epoxy resin, Mw=350, manufactured by Mitsubishi Chemical Corporation) as the epoxy resin (B), 1.0 part by weight of an adduct of tolylene diisocyanate and trimethylolpropane (I-1) as the curing agent (C), 0.1 part by weight of 3-glycidoxypropyltriethoxysilane as the silane coupling agent (D), and ethyl acetate was added to obtain a non-volatile content of 20%, and the mixture was stirred to obtain an adhesive solution.
[0095] <Preparation of adhesive sheet> An adhesive sheet was obtained according to the procedure for producing the adhesive sheet in Example 1 described above.
[0096] (Examples 14 to 18) As shown in Table 2, pressure-sensitive adhesive sheets were obtained in the same manner as in Example 13, except that the types and amounts of copolymer, epoxy resin, and curing agent were changed.
[0097] [Table 2]
[0098] [Epoxy resin (B)] B-1: JER825 (Bisphenol type epoxy resin, Mw=350, manufactured by Mitsubishi Chemical Corporation) B-2: JER828 (Bisphenol type epoxy resin, Mw=370, manufactured by Mitsubishi Chemical Corporation) B-3: JER806 (Bisphenol type epoxy resin, Mw=330, manufactured by Mitsubishi Chemical Corporation) B-4: JER1001 (Bisphenol type epoxy resin, Mw=900, manufactured by Mitsubishi Chemical Corporation) [Hardening agent (C)] C-1: Hexamethylene diisocyanate trimethylolpropane adduct C-2: Trimethylolpropane adduct of tolylene diisocyanate C-3: Trimethylolpropane adduct of isophorone diisocyanate C-4: N,N,N',N'-tetraglycidyl-m-xylylenediamine [Silane coupling agent (D)] D-1: 3-glycidoxypropyltriethoxysilane
[0099] The obtained adhesive sheet was used to evaluate transparency, adhesion, heat-resistant adhesion, heat resistance, shatterproofness, and impact resistance as tests for films for cover glass and films for housing glass, and dent resistance as a test for films for housing glass.
[0100] Preparation of Test Laminates [Test laminate 1: PET film / adhesive layer / glass] The obtained adhesive sheet was cut into a size of 25 mm width x 100 mm length to prepare a test adhesive sheet 1 consisting of PET film / adhesive layer / peelable sheet. The release sheet was peeled off from this test adhesive sheet 1, and the exposed adhesive layer was attached to an alkali-free glass plate (EN-A1: manufactured by Asahi Glass Co., Ltd.) using a laminator at 25°C and a relative humidity of 50%, resulting in a test laminate 1 consisting of PET film / adhesive layer / glass.
[0101] [Test laminate 2: PET film / adhesive layer / display] The obtained adhesive sheet was cut into a size of 75 mm width x 150 mm length (equivalent to 6.1 inches) to prepare a test adhesive sheet 2 consisting of PET film / adhesive layer / peelable sheet. The release sheet was peeled off from this test adhesive sheet 2, and the exposed adhesive layer was attached to the display of a smartphone (iPhone (registered trademark) 11: manufactured by Apple Inc.) in an atmosphere of 25°C and relative humidity of 50%, to obtain test laminate 2.
[0102] Evaluation Method <Transparency> The test laminate 1 was left to stand for one week at 23° C. and a relative humidity of 50%, and then the haze was measured using a Turbidimeter NDH5000W manufactured by Nippon Denshoku Industries Co., Ltd. [Evaluation Criteria] ○: Haze is less than 1.0 (good). ×: Haze is 1.0 or more (poor).
[0103] <Adhesiveness> After leaving the test laminate 1 at 23°C and 50% relative humidity for 24 hours, a 180° peel test was carried out in which the laminate was peeled off in a 180° direction at a speed of 300 mm / min. The peel strength at the time of peeling was measured, and the adhesion was evaluated on a two-level scale. [Evaluation Criteria] ○: "The peel strength is 20N or more, and there is no problem in practical use." △: "The peel strength is between 10N and 20N, but still usable" ×: "The peel strength is less than 10N, and it is not practical"
[0104] <Heat-resistant adhesiveness> Test laminate 1 was left for 30 minutes in an atmosphere at 150°C, then left to stand for 30 minutes in an atmosphere at 25°C and 50% relative humidity, after which a 180° peel test was performed in which the laminate was peeled off in a 180° direction at a speed of 300 mm / min. The peel strength at the time of peeling was measured, and the adhesion was evaluated on a three-point scale. [Evaluation Criteria] ○: "The peel strength is 30N or more, and there is no problem in practical use." △: "Peel strength is between 20N and 30N, making it practical." ×: "The peel strength is less than 20N, and it is not practical"
[0105] <Heat resistance> The test laminate 1 was left to stand in an atmosphere of 150°C for 30 minutes, and then left to stand in an atmosphere of 25°C and 50% relative humidity for 30 minutes, after which the edge of the test pressure-sensitive adhesive sheet was visually observed. The length of the pressure-sensitive adhesive protruding from the test pressure-sensitive adhesive sheet was measured, and the heat resistance was evaluated on a three-point scale. [Evaluation Criteria] ○: "No protrusion, no practical problems at all" △: "The protrusion length is within 0.2 mm, so it is usable." ×: "The protruding length is greater than 0.2 mm, and is not practical"
[0106] <Impact resistance> The test laminate 2 was dropped onto a concrete surface from a height of 1 m, and it was visually confirmed whether the test adhesive sheet 2 had peeled off from the information display surface of the display, and the impact resistance was evaluated on a two-level scale. [Evaluation Criteria] ○: "No peeling, no practical problems" ×: "Peeling was observed, not usable"
[0107] <Shatterproof> The test laminate 2 was placed with the display surface to which the test adhesive sheet 2 was attached facing up, and a 50g stainless steel ball was dropped from a height of 1.5m onto the display surface to which the test adhesive sheet 2 was attached. It was visually confirmed whether the display glass shattered or not, and the shatterproofness was evaluated on a two-level scale. [Evaluation Criteria] ○: "The glass broke, but the pieces did not scatter around and there was no problem in practical use." ×: "Glass was broken and fragments were scattered around, making it unusable."
[0108] <Mark resistance> The test laminate 2 was left for 30 minutes in an atmosphere at 150°C, and then left to stand for 30 minutes in an atmosphere at 25°C and 50% relative humidity. 20 stainless steel beads with a diameter of 1 mm were placed on the test pressure-sensitive adhesive sheet 1, and an alkali-free glass plate (EN-A1: manufactured by Asahi Glass Co., Ltd.) was placed on the stainless steel beads. A weight of 500 g was placed on the topmost alkali-free glass plate, and the plate was left for 24 hours in an atmosphere at 25°C and 50% relative humidity. The weight, alkali-free glass, and stainless steel beads were then removed, and the presence or absence of indentations caused by the pressing of the stainless steel beads was visually confirmed, and the impact resistance was evaluated on a three-point scale. [Evaluation Criteria] ○: "No indentations, no practical problems at all" △: "There are 5 or fewer dents, and the product is still in use." ×: "More than 5 indentations, not usable"
[0109] [Table 3]
[0110] From the results in Table 3, it was confirmed that the pressure-sensitive adhesive composition of the present invention has excellent transparency and good shatterproof properties, and therefore can be suitably used as a shatterproof film for optical members. Furthermore, it was confirmed that even at a film thickness of 5 μm, which is thinner than conventional films, it has high adhesion and heat resistance, and also has good dent resistance, which is necessary for films for glass casings. On the other hand, the pressure-sensitive adhesive compositions of Comparative Examples 1 to 8 could not satisfy all of the above characteristics.
Claims
1. The composition comprises an acrylic copolymer (A), an epoxy resin (B), and a curing agent (C) which is a curing agent for the acrylic copolymer (A) (excluding the epoxy resin (B)), The acrylic copolymer (A) is a copolymer of a monomer mixture containing the following monomers (a-1) to (a-3): The monomer mixture contains 10 to 50 mass% of monomer (a-1), 40 to 80 mass% of monomer (a-2), and 5 to 10 mass% of monomer (a-3), based on 100 mass% of the monomer mixture; The epoxy resin (B) is a bisphenol type epoxy resin having a weight average molecular weight (Mw) of 200 to 1,000. (a-1) (Meth)acrylic acid alkyl ester monomer having an alkyl group having 8 to 12 carbon atoms (a-2) (meth)acrylic acid ester monomers having a homopolymer glass transition temperature of 0 to 100°C (excluding monomers (a-1) and (a-3)). (a-3) (Meth)acrylic acid alkyl ester monomer having a carboxyl group
2. The pressure-sensitive adhesive composition according to claim 1, wherein the content of the epoxy resin (B) is 5 to 45 parts by mass based on 100 parts by mass of the acrylic copolymer (A).
3. The pressure-sensitive adhesive composition according to claim 1 or 2, wherein the curing agent (C) comprises an isocyanate compound.
4. The pressure-sensitive adhesive composition according to any one of claims 1 to 3, further comprising a silane coupling agent (D).
5. A pressure-sensitive adhesive sheet comprising a pressure-sensitive adhesive layer which is a cured product of the pressure-sensitive adhesive composition according to any one of claims 1 to 4.
6. An optical adhesive sheet comprising an adhesive layer which is a cured product of the adhesive composition according to any one of claims 1 to 4.
Citation Information
Patent Citations
Adhesive composition for polarizing plate
JP2011128439A
Adhesive composition and adhesive film using the same
JP2015025118A
Adhesive for glass attached decorative sheet and decorative sheet using the same
JP2016050285A
Scattering prevention adhesive sheet
JP2020070313A
Adhesive for optical film, adhesive layer, optical member and image display device
JP2020090586A