Method for producing SiC single crystal and method for suppressing dislocations in SiC single crystal
By employing a SiC crucible with a specific alloy impregnation to stabilize the Si-C solution, the method addresses the issue of dislocations in SiC single crystals, achieving high-quality, low-defect wafers suitable for larger diameters and improving production efficiency.
Patent Information
- Application Number
- JP2021147017
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-09-09
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2041-09-09
AI Technical Summary
Conventional methods for producing SiC single crystals face challenges in reducing dislocations, particularly during the initial stages of growth, leading to unstable crystal quality and increased dislocations as the diameter increases, which affects the yield and quality of larger-diameter wafers.
A method involving the use of a SiC crucible with a relative density of 50 to 90% impregnated with an alloy of Si and a metal element M that increases the solubility of C, forming a Si-C solution, which is then used to grow SiC single crystals, followed by bulk growth using a sublimation or gas method to stabilize the crystal quality.
This approach significantly reduces dislocations in SiC single crystals, allowing for high-quality, large-diameter wafers with low defects, suitable for use as seed crystals in vapor phase methods, and enables repeated use of the crucible and solution, enhancing production efficiency.
Smart Images

Figure 0007552540000019 
Figure 0007552540000020 
Figure 0007552540000012
Abstract
Description
[Technical field]
[0001] The present invention relates to a crystal growth technology for silicon carbide (SiC), and more particularly to a method for producing a SiC single crystal that enables stable production of a high-quality SiC single crystal with few dislocations, and a method for suppressing dislocations in the SiC single crystal. [Background technology]
[0002] SiC is a wide band gap semiconductor material that has excellent thermal conductivity and chemical stability, and also has excellent basic physical properties for use in power devices, including transistor characteristics such as dielectric breakdown characteristics and saturated drift velocity. For these reasons, there are high expectations for SiC as a material for next-generation power devices, and commercialization of SiC power devices has been reported.
[0003] However, SiC substrates are more expensive than Si substrates, and there is a problem that the single crystal substrates are not sufficiently low in dislocations and high in quality. The main reason why it is difficult to manufacture high-quality SiC single crystal substrates with low dislocations is that SiC does not melt under normal pressure. In the case of Si, which is widely used as a substrate for semiconductor devices, the melting point at normal pressure is 1,414°C, and large-diameter single crystals with low dislocations and high quality can be obtained from molten Si by the CZ method or FZ method.
[0004] In contrast, SiC sublimes at around 2,000°C when heated under normal pressure, so the crystal growth methods using the CZ method and FZ method cannot be used. Therefore, currently, SiC single crystals are mainly manufactured by sublimation methods, including the modified Lely process. The sublimation method is currently the only method for mass-producing SiC single crystals, and 4-inch SiC single crystal substrates manufactured by this method are widely available on the market, and 6-inch SiC single crystal substrates have also been mass-produced and are commercially available.
[0005] However, even if power devices are fabricated using SiC single crystals obtained by the sublimation method, their characteristics are not necessarily sufficient. The reason is that it is not easy to reduce the dislocations in SiC single crystals. Crystal growth by the sublimation method is a precipitation phenomenon from the gas phase, so the growth rate is slow and it is difficult to control the temperature in the reaction space. In recent years, as a result of vigorous improvements and improvements, the dislocation density of micropipes has been reduced, but lattice dislocations that affect the electrical characteristics of devices, such as threading screw dislocations (TSDs), threading edge dislocations (TEDs), and basal plane dislocations (BPDs), still exist at a high density.
[0006] In addition, the mainstream wafer size for semiconductor device substrates has recently shifted from 4 inches to 6 inches in diameter. With this increase in diameter, the number of dislocations in the crystals has increased, and the device yield is currently lower than that of 4 inches. It is expected that the problem of dislocations will become even more serious as the diameter increases (diameter 8 inches or more) in the future. In this case, the quality of the seed crystal is important because vapor phase growth using the sublimation method or gas method propagates dislocations in the seed crystal (substrate). Naturally, high-quality large-diameter seed crystals are required as the diameter increases, but the current situation is that high-quality seed crystals cannot be obtained because dislocations increase with the diameter. On the other hand, in crystal growth using the solution method, a growth rate of about 200 μm / h can be obtained by considering the solvent composition and the crucible material, which is the carbon supply source, and the obtained crystals have much lower dislocations and are of higher quality than commercially available products produced by the sublimation method.
[0007] Therefore, recently, a method for growing SiC crystals by a solution method has been attracting attention (for example, JP 2000-264790 A (Patent Document 1), JP 2004-002173 A (Patent Document 2), and JP 2006-143555 A (Patent Document 3)). As described above, SiC itself does not melt under normal pressure. Therefore, in a method for producing a SiC single crystal by a solution method, C is dissolved in a Si melt in a graphite crucible from a high-temperature part below the crucible, and a SiC seed crystal is brought into contact with this Si-C melt, and epitaxial growth is performed on the SiC seed crystal to obtain a SiC single crystal. In such a solution method, the crystal growth of SiC proceeds in a state very close to thermal equilibrium, and therefore a crystal with fewer dislocations is obtained compared to a SiC single crystal obtained by a sublimation method.
[0008] There are various solution methods for obtaining SiC single crystals, and in "Latest Technology of SiC Power Devices", Chapter 4, Section 1, 1.2 SiC Solution Growth Method, pp. 41-43, published by S&T Publishing Co., Ltd. on May 14, 2010 (Non-Patent Document 1), they are roughly classified into four types: Traveling Solvent Method (TSM), Slow Cooling Technique (SCT), Vapor Liquid Solid (VLS), and Top Seeded Solution Growth (TSSG). In the present invention, "solution method" means the Top Seeded Solution Growth (TSSG) unless otherwise specified.
[0009] In the method for producing a SiC single crystal by the solution method, a Si melt is first formed in a graphite crucible, and C is dissolved therein to form a Si-C solution. However, since the solubility of C in the Si-C solution is extremely low at about 1 atomic %, transition metals and the like are generally added to the Si-C solution to facilitate the dissolution of C (Patent Documents 1 to 3). As additive elements, transition metal elements such as Ti, Cr, Ni, and Fe, low melting point metal elements such as Al, Sn, and Ga, and various rare earth elements have been reported. The type and amount of such additive elements are determined in consideration of the following: promoting the dissolution of C; precipitating SiC as primary crystals from the Si-C solution and achieving good equilibrium with the remainder as a liquid phase; preventing the additive elements from precipitating carbides and other phases; precipitating the desired polymorph among the crystal polymorphs of SiC stably; and being able to obtain a solution composition that increases the growth rate of the single crystal as much as possible.
[0010] The growth of SiC single crystals by the conventional solution method is generally carried out according to the following procedure. First, the Si raw material is placed in a crucible made of carbon or graphite, which is heated and melted under an inert gas atmosphere. The C component is fed from the crucible into the Si melt to form a Si-C solution. In some cases, a carbon compound is placed in the crucible together with the Si raw material and melted. After the C component is sufficiently dissolved in the Si-C solution, a SiC seed crystal is brought into contact with the Si-C solution, and a single crystal is grown by utilizing the temperature gradient formed throughout the solution.
[0011] However, such conventional solution methods have the following problems. The first problem is that as the SiC single crystal grows, the Si component is gradually lost from the Si-C solution, and the solution composition gradually changes. If the solution composition changes during the growth of the SiC single crystal, the SiC precipitation environment naturally changes. As a result, it becomes difficult to stably continue the growth of the SiC single crystal for a long period of time. The second problem is the problem of excessive melting of C from the crucible. As the SiC single crystal grows, the Si component is gradually lost from the Si-C solution, while C is continuously supplied from the crucible. As a result, C is melted relatively excessively into the Si-C solution, and the Si / C composition ratio of the Si-C solution changes. The third problem is the precipitation of SiC polycrystals on the surface of the crucible (especially the inner wall surface) that comes into contact with the Si-C solution. As mentioned above, when an excessive amount of C is dissolved from the crucible into the Si-C solution, fine polycrystalline SiC is likely to be generated on the inner wall surface of the crucible. Such polycrystalline SiC (miscellaneous crystals) float in the SiC solution and reach the vicinity of the solid-liquid interface between the SiC single crystal and the Si-C solution during crystal growth, resulting in the inhibition of single crystal growth. [Prior art documents] [Patent documents]
[0012] [Patent Document 1] JP 2000-264790 A [Patent Document 2] JP 2004-002173 A [Patent Document 3] JP 2006-143555 A [Patent Document 4] JP 2015-110495 A [Patent Document 5] JP 2015-110496 A [Patent Document 6] JP 2015-110498 A [Patent Document 7] JP 2015-110499 A [Patent Document 8] JP 2015-110500 A [Patent Document 9] JP 2015-110501 A [Patent Document 10] JP 2017-031034 A [Patent Document 11] JP 2017-031036 A [Non-patent literature]
[0013] [Non-Patent Document 1] "Latest Technology of SiC Power Devices" Chapter 4, Section 1, 1.2 SiC Solution Growth Method, pp. 41-43, S&T Publishing Co., Ltd., published May 14, 2010 [Non-Patent Document 2] 5th Advanced Power Semiconductors Subcommittee (2018) Vol.05 Proceedings "Low TSD bulk growth by applying solution-based C-plane 4 degree off TSD conversion layer to sublimation method" pp.125-126 Summary of the Invention [Problem to be solved by the invention]
[0014] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a method for producing high-quality SiC single crystal with few dislocations even by a vapor phase method such as a sublimation method or a gas method, and a method for suppressing dislocations in SiC single crystal. [Means for solving the problem]
[0015] By the way, the solution method can produce SiC single crystals with fewer dislocations than those obtained by the sublimation method, but in the conventional solution method using a graphite crucible, voids are likely to occur due to the influence of gas components contained in the solvent and crucible in the early stages of growth, so after the bulk crystal is taken out, the crystal near the seed crystal is not used. Even in the case of crystal growth by the usual sublimation method, the growth is unstable in the early stages, so after bulk growth, the crystal part near the seed crystal is of poor quality and is therefore excluded from device applications. In addition, according to a previous report (5th Advanced Power Semiconductor Subcommittee (2018) Vol. 05 Proceedings "Low TSD Bulk Growth by Application of Solution Method C-Plane 4 Degree Off TSD Conversion Layer to Sublimation Method" pp. 125-126 (Non-Patent Document 2)), when a SiC single crystal is grown on the C-plane of 4H-SiC with an off-angle of 4 degrees by the solution method, a growth surface with a low density of threading screw dislocations (TSDs) is obtained, but when CMP polishing or the like is performed to remove adhesions and unevenness on the growth surface, there is a problem that dislocations are reconverted and increase in dislocations in the subsequent bulk growth by the vapor phase method. Furthermore, since the seed crystal for the sublimation method is solution grown on the C-plane with an off-angle of 4 degrees as reported previously, as the growth thickness increases, it becomes easier for the solvent to be trapped. In other words, the crystal quality at the initial stage of growth is important, and in order to achieve high quality by bulk growth by the vapor phase method after solution growth, it was necessary to remove gas components that cause voids and defects from the initial stage of growth and stabilize the carbon concentration in the solvent.
[0016] Accordingly, the present invention provides the following method for producing a SiC single crystal, and a method for suppressing dislocations in a SiC single crystal. 1. A SiC sintered body having a relative density of 50 to 90% is impregnated with an alloy of Si and a metal element M that increases the solubility of C as a melt to form a SiC crucible, and then Si and the metal element M are placed in the SiC crucible. The Si and metal element M in the SiC crucible are melted by heating the SiC crucible to form a Si-C solution. Si and C originating from the components of the SiC crucible are dissolved into the Si-C solution from the surface of the SiC crucible that is in contact with the Si-C solution, and a SiC seed crystal is brought into contact with the upper part of the Si-C solution to grow a SiC single crystal on the SiC seed crystal. At a growth rate of 100μm / hr or moreand then subjecting the surface of the grown SiC single crystal to bulk growth by a sublimation method or a gas method. 2. 2. The method for producing a SiC single crystal according to 1, wherein the metal element M is a metal consisting of the metal element M alone or an alloy containing the metal element M (but not containing Si) in the SiC crucible. 3. 3. The method for producing a SiC single crystal according to 1 or 2, wherein the metal element M is at least one first metal element M1 selected from the group consisting of La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Y, and Lu, at least one second metal element M2 selected from the group consisting of Ti, V, Cr, Mn, Fe, Co, Ni, and Cu, and / or at least one third metal element M3 selected from the group consisting of Ga, Ge, Sn, Pb, and Zn. 4. 4. The method for producing a SiC single crystal according to 3, wherein the metal element M is a metal element consisting of the first metal element M1 and the second metal element M2. 5. 5. The method for producing a SiC single crystal according to 3 or 4, wherein the total content of the metal element M in the Si—C solution is 1 to 80 atomic % based on the total amount of Si and M. 6. 6. A method for producing a SiC single crystal according to any one of 3 to 5, wherein the content of the first metal element M1 in the Si-C solution is 1 atomic % or more relative to the total amount of Si and metal element M, and the contents of the second metal element M2 and the third metal element M3 in the Si-C solution are each 1 atomic % or more relative to the total amount of Si and metal element M. 7. 7. The method for producing a SiC single crystal according to any one of 1 to 6, wherein the SiC sintered body has an oxygen content of 100 ppm or less. 8. 8. The method for producing a SiC single crystal according to any one of 1 to 7, wherein the growth of the SiC single crystal by a solution method is carried out at a temperature of the Si-C solution of 1,300 to 2,300°C. 9. 9. The method for producing a SiC single crystal according to any one of 1 to 8, wherein the method is carried out in a state in which the SiC crucible is housed in a second crucible made of a heat-resistant carbon material. 10. 10. The method for producing a SiC single crystal according to any one of 1 to 9, wherein the SiC single crystal grown by the solution method has a thickness of 10 to 1,000 μm. 11. 11. The method for producing a SiC single crystal according to any one of 1 to 10, wherein the SiC crucible and the Si-C solution are repeatedly used. 12. A SiC sintered body having a relative density of 50 to 90% is impregnated with an alloy of Si and a metal element M that increases the solubility of C as a melt to form a SiC crucible, and then Si and the metal element M are placed in the SiC crucible. The Si and metal element M in the SiC crucible are melted by heating the SiC crucible to form a Si-C solution. Si and C originating from the components of the SiC crucible are dissolved into the Si-C solution from the surface of the SiC crucible that is in contact with the Si-C solution, and a SiC seed crystal is brought into contact with the upper part of the Si-C solution to grow a SiC single crystal on the SiC seed crystal by a solution method. At a growth rate of 100μm / hr or more A method for suppressing dislocations in a SiC single crystal, comprising: growing the SiC single crystal. 13. 13. The method for suppressing dislocations in a SiC single crystal according to 12, further comprising bulk growing a SiC single crystal on the surface of the SiC single crystal obtained by the solution method by a sublimation method or a gas method. 14. 14. The method for suppressing dislocations in a SiC single crystal according to 13, wherein a SiC single crystal wafer obtained from a SiC single crystal bulk-grown by the sublimation method or gas method is used as a SiC seed crystal, and a SiC single crystal is grown on the SiC seed crystal by the solution method. 15. 15. The method for suppressing dislocations in a SiC single crystal according to 14, further comprising bulk growing a SiC single crystal on the surface of the SiC single crystal obtained by the solution method by a sublimation method or a gas method. Effect of the Invention
[0017] According to the present invention, even if the SiC wafer is cut from a SiC ingot manufactured by a gas phase method such as sublimation, the SiC wafer can be grown by a specific solution method to reduce dislocations, and further, a high-quality SiC single crystal can be obtained by performing bulk growth on the growth surface of the SiC single crystal by a gas phase method such as sublimation or gas method. Specifically, dislocations can be significantly reduced by performing crystal growth of about 10 to 1,000 μm by a solution method on a SiC wafer manufactured by sublimation. Even if the SiC wafer has increased dislocations due to its large diameter, the dislocations can be reduced, so if it is used as a seed crystal (substrate), the bulk crystal obtained by the sublimation or gas method can be of high quality. [Brief description of the drawings]
[0018] [Figure 1] 1 is a cross-sectional view showing an example of a main part of a SiC single crystal manufacturing apparatus suitably used for growing a SiC single crystal. [Diagram 2] FIG. 1 is a conceptual diagram for explaining the dissolution of Si and C from a SiC crucible into a Si-C solution when growing a SiC single crystal using a SiC crucible formed from a SiC sintered body with a relative density of 50 to 90%. [Diagram 3] FIG. 1 is a conceptual diagram for explaining the dissolution of Si and C from a SiC crucible into a Si-C solution when growing a SiC single crystal using a conventional dense SiC crucible. [Figure 4] 1 is a diagram showing the appearance of the growth surface (C-plane) of the SiC single crystal obtained in Example 1. [Diagram 5] FIG. 2 is a diagram showing the results of observation of dislocations in a seed crystal portion of the SiC single crystal sample of Example 1. [Figure 6] FIG. 2 is a diagram showing the results of observation of dislocations in the solution growth portion (growth surface) of the SiC single crystal sample of Example 1. [Figure 7] FIG. 2 is a diagram showing the appearance of the growth surface (C-plane) of the SiC single crystal of Example 2. [Figure 8] 1 is a reflection X-ray topographic image of a seed crystal portion of a SiC single crystal sample of Example 2. [Figure 9] 1 is a reflection X-ray topographic image of a solution growth portion (growth surface) of a SiC single crystal sample of Example 2. [Figure 10] FIG. 1 is a diagram showing the appearance of the growth surface (C-plane) of the SiC single crystal of Example 3. [Figure 11] 1 is a laser microscope image of the growth surface (C-plane) of the SiC single crystal in Example 3. [Figure 12] FIG. 1 is a diagram showing a cross section of a SiC single crystal sample of Example 3. [Figure 13] 1 is a reflection X-ray topographic image of a seed crystal portion of a SiC single crystal sample of Example 3. [Figure 14] 1 is a reflection X-ray topographic image of a solution growth portion (growth surface) of a SiC single crystal sample of Example 3. [Figure 15] 1 is a diagram showing the appearance of the growth surface (C-plane) of the SiC single crystal of Comparative Example 1. FIG. [Figure 16] FIG. 2 is a diagram showing a cross section of a SiC single crystal sample of Comparative Example 1. [Figure 17] FIG. 4 is a diagram showing a cross section of a SiC single crystal sample of Example 2. [Figure 18] FIG. 11 is a diagram showing the appearance of the growth surface (C-plane) of the SiC single crystal of Example 5. [Figure 19] FIG. 1 is a schematic cross-sectional view of a reaction vessel for bulk growth by sublimation. [Figure 20] FIG. 1 is a schematic cross-sectional view of a reaction apparatus for bulk growth by sublimation. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] The present invention will now be described in further detail. The method for producing a SiC single crystal of the present invention utilizes a solution method (i.e., seeded solution growth method (TSSG)) in which a seed crystal is brought into contact with a Si-C solution (Si-C melt) contained in a crucible to grow a SiC single crystal. That is, the method for producing a SiC single crystal of the present invention is characterized in that an alloy of Si and a metal element M that increases the solubility of C is impregnated as a melt into a SiC sintered body having a relative density of 50 to 90% to form a SiC crucible, Si and the metal element M are then placed in the SiC crucible, and the Si and metal element M in the SiC crucible are melted by heating the SiC crucible to form a Si-C solution, and Si and C originating from the components of the SiC crucible are dissolved into the Si-C solution from the surface of the SiC crucible in contact with the Si-C solution, and a SiC seed crystal is brought into contact with the upper part of the Si-C solution to grow a SiC single crystal on the SiC seed crystal, and then a SiC single crystal is further bulk-grown on the surface of the grown SiC single crystal by a sublimation method or a gas method.
[0020] Fig. 1 is a cross-sectional view showing an example of a SiC single crystal manufacturing apparatus (heating furnace) suitable for use in growing a SiC single crystal by the solution method in the present invention. In the figure, 1 is a SiC crucible that contains a Si-C solution, 2 is a second crucible made of a heat-resistant carbon material that contains the SiC crucible 1, 3 is a SiC single crystal (seed crystal), 4 is a Si-C solution contained in the SiC crucible 1, 5 is a rotating shaft for rotating the SiC crucible 1 and the second crucible 2 during the crystal growth of the SiC single crystal, 6 is a rotating shaft for holding the SiC single crystal 3 and rotating it during the crystal growth of the SiC single crystal, 7 is a susceptor made of a graphite material or the like, 8 is a heat insulating material made of a graphite material or the like, 9 is an upper lid for suppressing the evaporation of the Si-C solution, and 10 is a high-frequency coil for heating the inside of the furnace to set the Si-C solution to a predetermined temperature and temperature distribution. Although not shown, an exhaust port and an exhaust valve for creating a vacuum in the atmosphere inside the heating furnace, and a gas inlet and a gas inlet valve for introducing gas are provided.
[0021] The crucible before heating is usually filled with Si, but may be filled with a C source as well. When the inside of the crucible is heated, the components Si and C are dissolved from the surface of the SiC crucible that is in contact with the Si melt immediately after heating, and with the Si-C solution after the C has dissolved, into the Si melt or the Si-C solution. Note that the crucible before heating can also be filled with SiC together with Si or Si and C.
[0022] In the present invention, the SiC crucible 1 is made of a SiC sintered body, and the relative density of this SiC sintered body is 50% or more, preferably 70% or more, and 90% or less, preferably 88% or less, and more preferably 85% or less. Here, the relative density refers to the true density of SiC, 3.22 g / cm 3 The ratio (%) of the measured density or calculated density of the SiC sintered body to the true density of SiC, that is, the percentage of the measured density or calculated density of the SiC sintered body divided by the true density of SiC. The measured density is, for example, a value (density) measured by the Archimedes method for the SiC sintered body. The calculated density is a value (density) obtained by dividing the mass of the SiC sintered body by the volume of the SiC sintered body calculated from the measured dimensions of the SiC sintered body (i.e., in the case of a cylindrical crucible, the outer diameter, height, inner diameter (diameter of the housing part), and height of the housing part).
[0023] A SiC crucible formed of a SiC sintered body having a relative density within the above range can be obtained by a dry pressing method, a slip casting method or the like, but the manufacturing method is not limited to these.
[0024] The Si-C solution 4 contained in the SiC crucible 1 is doped with a metal element M that increases the solubility of C in the Si-C solution. When the Si-C solution is used with the metal element M that increases the solubility of C added, the use of a SiC crucible is advantageous because it suppresses the formation of metal carbides formed by the combination of the added metal element M and carbon C. When a C crucible (graphite crucible) is used, if the Si composition ratio in the Si-C solution decreases or C is dissolved excessively, and the Si / C composition ratio decreases, the metal element M that is added to facilitate the dissolution of C tends to easily combine with C, and metal carbides tend to be formed. Such metal carbides have a high melting point, and if they float in the Si-C solution and reach and adhere to the vicinity of the seed crystal surface, SiC single crystals cannot be formed. In contrast, when a SiC crucible is used, carbon (C) does not dissolve excessively in the Si-C solution, and as a result, the formation of metal carbides is suppressed, so the growth of the SiC single crystal is less likely to be hindered.
[0025] When a metal element M that increases the solubility of Si and C is placed in an SiC crucible 1 formed of a SiC sintered body with a relative density of 50 to 90%, whose cavity is not filled with a molten liquid (solid at room temperature) such as a Si-C solution, for example, in the state of an SiC crucible before use, and Si and the metal element M are melted to form a Si-C solution, if the metal element M is placed alone or as an alloy that does not contain Si, a metal or alloy with a low melting point will preferentially penetrate the SiC sintered body, causing a reaction between the metal element M and the SiC crucible, and problems will arise such as the composition of the Si-C solution in the SiC crucible deviating from the desired composition. Therefore, in the present invention, before the metal element M that increases the solubility of Si and C is placed in the SiC crucible, an alloy of Si and the metal element M, preferably an alloy having a composition ratio substantially the same as that of the Si-C solution used for growing the SiC single crystal, is melted and impregnated in advance into the pores of the SiC sintered body, that is, the SiC sintered body, to form the SiC crucible 1. Specifically, the alloy is placed in the SiC crucible, and heat-treated at a temperature of 1,300°C or higher, particularly 1,500°C or higher, and 2,300°C or lower, particularly 2,000°C or lower. The heat treatment time is usually 1 to 10 hours. The impregnation atmosphere may be an inert gas atmosphere such as argon or nitrogen, a vacuum (reduced pressure) atmosphere, or a combination of these (i.e., an atmosphere reduced pressure after an inert gas atmosphere).
[0026] Examples of the metal element M include at least one first metal element M1 selected from the group of La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Y, and Lu, at least one second metal element M2 selected from the group of Ti, V, Cr, Mn, Fe, Co, Ni, and Cu, and at least one third metal element M3 selected from the group of Ga, Ge, Sn, Pb, and Zn. The total content of the metal element M in the Si-C solution is preferably 1 atomic % or more, particularly 20 atomic % or more, and 80 atomic % or less, particularly 50 atomic % or less, based on the total amount of Si and M. In the present invention, it is preferable to store, in the crucible before heating, a metal consisting of the metal element M alone, or an alloy containing the metal element M (but not containing Si), particularly an alloy consisting of a plurality of the metal elements M, together with Si and optionally added C and / or SiC.
[0027] The metal element M may be composed of the first to third metal elements M1, M2 and M3, or may be composed of an appropriate combination of these, but is preferably composed of the first metal element M1 and the second metal element M2 and / or the third metal element M3, and is preferably composed of a combination of the metal element M1 and the metal element M2. In this case, the content of the first metal element M1 in the Si-C solution is preferably 1 atomic % or more, particularly 5 atomic % or more, based on the total amount of Si and M, and is preferably 50 atomic % or less, particularly 40 atomic % or less. In addition, the content of the second metal element M2 and the third metal element M3 in the Si-C solution is preferably 1 atomic % or more, particularly 2 atomic % or more, based on the total amount of Si and M, and is preferably 30 atomic % or less, particularly 20 atomic % or less.
[0028] In the present invention, the above-mentioned device is used, and the Si-C solution 4 is inductively heated from the high-frequency coil 10 to the SiC crucible 1, thereby forming a temperature distribution suitable for crystal growth, and Si and C originating from the SiC, which is a component of the SiC, are dissolved into the Si-C solution 4 from the SiC crucible 1 in contact with the Si-C solution 4. Then, the SiC seed crystal 3 is brought into contact with the Si-C solution 4 in the upper part of the SiC crucible 1, and a SiC single crystal is grown on the SiC seed crystal 3. Therefore, the temperature of the inner surface of the SiC crucible in contact with the Si-C solution is set to a temperature high enough to dissolve Si and C, which are the constituent elements of the SiC, into the Si-C solution 4. The temperature in the vicinity of the solid-liquid interface between the SiC seed crystal 3 and the Si-C solution 4 is set to a temperature sufficient for SiC to grow as a single crystal on the SiC seed crystal 3.
[0029] In the growth process of the SiC single crystal, a desired temperature distribution can be formed in the Si-C solution by appropriately controlling the induction heating conditions from the high-frequency coil, appropriately setting the positional relationship between the crucible and the high-frequency coil (especially the vertical positional relationship), and appropriately rotating the crucible and the SiC single crystal (seed crystal), thereby making it possible to appropriately control the growth rate of the SiC single crystal and the dissolution rate of the SiC crucible components into the Si-C solution.
[0030] The temperature of the Si-C solution during crystal growth is preferably controlled within a range of 1,300°C or higher, particularly 1,500°C or higher, and 2,300°C or lower, particularly 2,000°C or lower. A seed crystal is brought into contact with the Si-C solution in the upper part of the SiC crucible to grow a SiC single crystal on the seed crystal. Therefore, at least a part of the contact area between the SiC crucible and the Si-C solution is a high-temperature area that can dissolve the components from the SiC crucible into the Si-C solution, while the contact area between the seed crystal or the growth surface of the SiC single crystal grown on the seed crystal and the Si-C solution is a low-temperature area that can grow SiC as a single crystal on the seed crystal or on the SiC single crystal grown on the seed crystal. The temperature distribution of the Si-C solution is preferably such that the temperature gradually increases from the vicinity of the seed crystal to the vicinity of the inner surface of the SiC crucible (i.e., the contact surface with the Si-C solution), preferably from the vicinity of the seed crystal to the vicinity of the inner surface of the SiC crucible (i.e., the contact surface with the Si-C solution) in the entire Si-C solution, and is preferably such that the temperature gradually increases from the upper part of the Si-C solution to the lower part, preferably from the upper part of the Si-C solution to the lower part in the entire Si-C solution. In this case, it is effective to set the temperature difference between the high temperature region and the low temperature region to, for example, 5°C or more, particularly 10°C or more, and 200°C or less, particularly 100°C or less. The gradient of the temperature distribution of the Si-C solution is preferably 1°C / cm or more, particularly 5°C / cm or more, and 50°C / cm or less, particularly 30°C / cm or less. The growth of the SiC single crystal is usually carried out in an inert gas atmosphere such as helium gas or argon gas.
[0031] Although FIG. 1 shows an embodiment in which the crucible is heated by high frequency, the heating method is not limited to high frequency, and other methods such as resistance heating may be used depending on the controlled temperature of the Si-C solution, etc.
[0032] FIG. 2 is a diagram for conceptually explaining the state in which Si and C are dissolved from a SiC crucible into a Si-C solution when crystals of SiC are grown using a SiC crucible formed of a SiC sintered body with a relative density of 50 to 90%. When a temperature distribution suitable for crystal growth is formed in the Si-C solution 4, Si and C originating from SiC, which is a component of the SiC crucible 1, are dissolved into the Si-C solution 4 from the surface (particularly the high-temperature region) of the SiC crucible 1 that contacts the Si-C solution 4. The dissolved Si and C become new Si and C components of the Si-C solution 4, and become the source of a single crystal that grows on the SiC seed crystal 3. In the figure, 2 is a second crucible, 6 is a rotation axis, and 9 is a top cover, each of which corresponds to FIG. 1.
[0033] In such an environment where elution of Si and C from the SiC crucible 1 into the Si-C solution 4 occurs, the problem of precipitation of SiC polycrystals on the crucible surface in contact with the Si-C solution does not occur. This is because, under conditions where SiC, a component of the SiC crucible 1, is eluted as Si and C into the Si-C solution 4, there is no room for Si and C to precipitate as SiC. In other words, by using a crucible containing SiC as a container for the Si-C solution, precipitation of SiC polycrystals on the crucible surface in contact with the Si-C solution is suppressed.
[0034] Furthermore, by using a SiC crucible formed of a SiC sintered body with a relative density of 50 to 90%, the Si-C solution not only contacts the surface of the SiC crucible, but also penetrates into the inside of the sintered body (pores), and as shown by the arrows in Figure 2, SiC is efficiently dissolved and supplied from the inside of the SiC crucible, improving the crystal growth rate and suppressing SiC polycrystals. As a result, it is considered that the state in the solution shown in Figure 2 is realized. If the relative density of the SiC sintered body constituting the SiC crucible is less than 50%, when the SiC crucible melts, SiC disintegrates into SiC particles, and the state in which the SiC particles float in the Si-C solution occurs significantly. Also, if the relative density exceeds 90%, the SiC solution hardly penetrates into the inside of the sintered body (pores), and efficient dissolution of SiC into the SiC solution cannot be achieved.
[0035] In contrast, Figure 3 is a diagram for conceptually explaining the dissolution of Si and C from a SiC crucible into a Si-C solution when growing SiC crystals using a conventional dense SiC crucible (for example, a SiC crucible formed of a SiC sintered body with a relative density of more than 90%). In this case, however, the Si-C solution 4 only comes into contact with the surface of the SiC crucible 1, and dissolution of Si and C into the Si-C solution 4 is insufficient, so that the supply of SiC from the SiC crucible 1 (dissolution into the Si-C solution) is not uniform at the contact point between the SiC crucible and the Si-C solution, and dissolution of SiC proceeds predominantly in the high-temperature parts of the SiC crucible, particularly in the bottom corners as shown by the arrows in Figure 3, making it difficult to grow SiC single crystals for a long period of time. In the figure, 2 is a second crucible, 3 is a SiC seed crystal, 6 is a rotation shaft, and 9 is an upper lid, each of which corresponds to FIG.
[0036] Furthermore, in the present invention, an alloy of Si and metal element M, preferably an alloy having a composition ratio approximately the same as that of the Si-C solution used to grow a SiC single crystal, is used as a molten liquid in the SiC crucible 1 and is pre-impregnated into the SiC sintered body (in the pores of the SiC sintered body).Therefore, when Si and the metal element M are melted to form a Si-C solution, the metal element M does not react preferentially with the SiC crucible, and the composition of the Si-C solution in the SiC crucible is maintained at the desired composition.
[0037] Si and C are continuously dissolved from the SiC crucible, but if the single crystal is grown while rotating the crucible and seed crystal, the stirring effect of the Si-C solution makes it possible to homogenize the composition of the Si-C solution.
[0038] In FIG. 1, a second crucible 2 made of a heat-resistant carbon material is used to accommodate the SiC crucible 1, and the SiC crucible 1 is accommodated in the second crucible 2 made of a heat-resistant carbon material. In the present invention, a SiC crucible made of a SiC sintered body with a relative density of 50 to 90% is used, but since the Si-C solution may leak from the outer surface of the SiC crucible through the pores of the SiC sintered body, it is preferable to accommodate the SiC crucible in the second crucible. In this case, it is preferable that the second crucible 2 is formed of a material dense enough that the Si-C solution does not leak out. In addition, the use of the second crucible has the advantage that the temperature distribution in the Si-C solution can be easily controlled.
[0039] In addition, the SiC sintered body that constitutes the SiC crucible usually contains oxygen as an impurity. The oxygen contained in the SiC sintered body forms an oxide (SiO), and since the boiling point of SiO is about 1,880°C, if the temperature of the Si-C solution is equal to or higher than this boiling point, SiO gasifies in the Si-C solution as SiC dissolves, and when this gas reaches the interface (solid-liquid interface) between the Si-C solution and the growing SiC single crystal, it may be taken in at the crystal growth surface and cause voids in the SiC single crystal. In addition, if the oxygen contained in the SiC sintered body dissolves into the Si-C solution as SiC dissolves, and when the temperature of the Si-C solution is lower than the boiling point of SiO, it reacts with Si in the Si-C solution to form SiO, and when this gas reaches the interface (solid-liquid interface) between the Si-C solution and the growing SiC single crystal, it may be taken in at the crystal growth surface and cause voids in the SiC single crystal. Therefore, it is preferable that the SiC sintered body has an oxygen content of 100 ppm or less.
[0040] In the solution method, a SiC single crystal is prepared as a seed crystal, and this seed crystal can be either a SiC single crystal obtained by a sublimation method or a SiC single crystal obtained by a solution method (here, this means a solution method in a broad sense including the above-mentioned solvent transfer crystal growth method, slow cooling method, vapor liquid-solid method, seeded solution growth method, etc.).
[0041] According to the method for producing a SiC single crystal of the present invention, a SiC crucible is used, which is made of a SiC sintered body with a relative density of 50 to 90%, and the SiC sintered body is impregnated with an alloy with a metal element M that increases the solubility of Si and C. By heating the SiC crucible, SiC, which is a component of the SiC sintered body, is dissolved from the inside of the sintered body into the Si-C solution as a source of Si and C, and Si and C are efficiently supplied to the Si-C solution. As a result, Si and C are supplied evenly and without excess or deficiency from the entire contact part of the SiC crucible with the Si-C solution, and high-quality SiC single crystals can be stably produced at a high growth rate for a long period of time.
[0042] The thickness of the SiC single crystal grown by the above-mentioned solution method is preferably 10 μm or more, and more preferably 50 μm or more. There is no particular upper limit to the thickness of the SiC single crystal grown by the solution method, and when it is necessary to use a single crystal with higher crystallinity as a seed crystal (substrate) for the vapor phase epitaxy method described later, the thickness may be more than 1,000 μm, but usually 1,000 μm or less is preferable, and 150 μm or less is more preferable in terms of productivity.
[0043] Moreover, the growth surface of the SiC single crystal obtained by the solution method is a high-quality surface with few defects such as dislocations. In this case, the obtained SiC single crystal can be directly subjected to the next process, that is, the bulk growth process of the SiC single crystal by the sublimation method or the gas method, without any other processing such as grinding, except for removing the adhering solvent by surface treatment such as fluoronitric acid treatment. In addition, in order to eliminate distortions and defects caused by processing of the SiC single crystal obtained by the solution method, these surface deteriorations may be improved by performing heat treatment in an atmosphere.
[0044] In the present invention, in the production of SiC single crystals by the above-mentioned solution method, the SiC crucible and the Si-C solution can be used repeatedly.
[0045] In the present invention, a SiC single crystal is then further bulk-grown by a sublimation method or a gas method on the surface of the SiC single crystal grown by the solution method as described above. This makes it possible to grow a SiC bulk while maintaining the low dislocation state of the SiC single crystal formed by the solution method described above by direct vapor phase growth.
[0046] Here, the bulk growth of SiC single crystals by the sublimation method is a method in which a solid SiC raw material (usually powder) is placed at the bottom of a graphite crucible placed in an apparatus, the bottom is heated at a high temperature (2,000°C or higher, for example, 2,200 to 2,600°C) to sublimate the SiC, which is then transported through an inert gas atmosphere in the apparatus and recrystallized on a SiC seed crystal placed in the low-temperature section to grow a bulk single crystal.
[0047] In addition, bulk growth of SiC single crystals by the gas method involves introducing silane (SiH4) and hydrocarbon gases (e.g., C2H4) from the outside onto a SiC seed crystal heated to approximately 2,100 to 2,300°C, in the same manner as in the thin-film CVD method, to carry out crystal growth; the introduced gas first reacts in the gas phase, forming clusters which are then introduced into the growth zone, where it is decomposed again, and ultimately becomes reaction precursors such as Si, SiC2, and Si2C, similar to those in the sublimation recrystallization method, and is then grown on the SiC seed crystal to grow a bulk single crystal.
[0048] [Method to suppress dislocations in SiC single crystals] The method for suppressing dislocation of SiC single crystal of the present invention is characterized in that the alloy of Si and metal element M that increases the solubility of C is impregnated as a melt into a SiC sintered body with a relative density of 50-90% to form a SiC crucible, then Si and the metal element M are placed in the SiC crucible, and the Si and metal element M in the SiC crucible are melted by heating the SiC crucible to form a Si-C solution, and Si and C originating from the components of the SiC crucible are dissolved into the Si-C solution from the surface of the SiC crucible that contacts with the Si-C solution, and a SiC seed crystal is contacted with the top of the Si-C solution to grow a SiC single crystal on the SiC seed crystal by a solution method.The solution method referred to here is the same as that described above. This makes it possible to suppress defects such as dislocations (reducing dislocations) on the growth surface of the SiC single crystal.
[0049] Note that "dislocations" here refer to threading dislocations (threading screw dislocations (TSDs) and threading edge dislocations (TEDs)) and basal plane dislocations (BPDs). The degree of dislocation suppression (reduced dislocation density) is determined by observing these dislocations using the alkali etching method or reflective X-ray topography method described below, and then determining the number of dislocations (dislocation density). <Alkaline etching method> A SiC crystal with a mirror-polished Si surface with an arithmetic mean roughness Ra (JIS B0601 (2001)) of 10 nm or less is immersed in molten KOH at 500°C for about 10 minutes, and threading dislocations (threading screw dislocations (TSDs) and threading edge dislocations (TEDs)) and basal plane dislocations (BPDs) that appear on the Si surface are observed as etch pits of different shapes. Specifically, the above-mentioned dislocations observed in multiple fields of view under an optical microscope at 100x magnification on the observation target surface after molten KOH treatment are counted, and the number of dislocations (dislocation density (pieces / cm)) is calculated. 2 )) is required. <Reflection X-ray topography> Using an X-ray topography device, dislocations inside the crystal are observed non-destructively from the intensity of the diffracted X-rays irradiated onto the surface of the sample at an acute angle. In this case, black dots in the X-ray topography image are identified as threading screw dislocations (TSDs) and wire-shaped ones as basal plane dislocations (BPDs). Specifically, the above-mentioned dislocations observed within a certain area of observation field are counted, and the number of dislocations (dislocation density (number / cm)) is calculated. 2 )) is required.
[0050] Here, it is preferable to further grow a SiC single crystal in bulk on the surface of the SiC single crystal obtained by the solution method by a sublimation method or a gas method, where the sublimation method and the gas method are the same as those described above. This maintains a low dislocation state in the bulk-grown SiC single crystal.
[0051] It is also more preferable to use a SiC single crystal wafer obtained from a SiC single crystal bulk-grown by the sublimation method or gas method as a SiC seed crystal, and grow a SiC single crystal on the SiC seed crystal by the solution method. This makes it possible to further suppress defects such as dislocations on the growth surface of the SiC single crystal.
[0052] Furthermore, it is particularly preferable to bulk grow a SiC single crystal on the surface of the SiC single crystal obtained by the solution method using a sublimation method or a gas method. This maintains a lower dislocation density for the bulk-grown SiC single crystal. EXAMPLES
[0053] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to the following examples.
[0054] In this example, the sample treatment and the observation and evaluation including observation of dislocations in the sample were carried out under the following conditions. <Alkaline etching method> A SiC crystal with a mirror-polished Si surface with an arithmetic mean roughness Ra (JIS B0601 (2001)) of 10 nm or less was immersed in molten KOH at 500 °C for about 10 minutes to observe threading dislocations (threading screw dislocations (TSDs) and threading edge dislocations (TEDs)) and basal plane dislocations (BPDs) that appeared on the Si surface as etch pits of different shapes. Specifically, the seed crystal side (Si surface) was ground against the growth side (C surface), and dislocations were observed in the thickness direction. To distinguish the etch pits, relatively large hexagons were distinguished as threading screw dislocations (TSDs), small hexagons as threading edge dislocations (TEDs), and ellipses (teardrop shapes) as basal plane dislocations (BPDs). In addition, the above dislocations observed in multiple fields of view of a 100x optical microscope were counted for the observation surface after molten KOH treatment to determine the number of dislocations (dislocation density). Incidentally, these etch pits only appear on the Si surface, and do not appear on the C surface. Also, the reason why a mirror finish (Ra: 10 nm or less) is essential on the Si surface is that if grinding marks remain, they will be enhanced by etching, making the observation of the etch pits unclear. <Reflection X-ray topography> In the reflection X-ray topography method, X-rays were irradiated at an acute angle to the sample, and dislocations inside the crystal were observed from the intensity of the diffracted X-rays. A feature of this method is that dislocations from the surface to a depth of 10 μm are reflected, making it possible to compare samples of different thin films and thicknesses. In addition, the reflection X-ray topography method allows non-destructive observation regardless of the Si surface or C surface, making it possible to observe the growth surface of the C surface. As a method for identifying dislocations in the X-ray topography image, black spots were identified as threading screw dislocations (TSDs) and wire-shaped ones as basal plane dislocations (BPDs). In this example, an X-ray topography device (device name: XRT-micron) manufactured by Rigaku Corporation was used. <Raman spectroscopy> When a material is irradiated with light, the interaction between the light and the material causes a phenomenon called scattering in addition to reflection, refraction, and absorption. This phenomenon includes Raman scattering (inelastic scattering), in which the light is scattered to a wavelength different from that of the incident light due to molecular vibration. Raman spectroscopy is a spectroscopic method that measures the wavelength and scattering intensity of this Raman line to identify and quantify the energy level and the material. In this example, the polytype of SiC was identified by analyzing the Raman shift of the Raman spectrum obtained by irradiating laser light. <Fluoro-nitric acid treatment> For the hydrofluoric and nitric acid treatment, the sample was immersed in a hydrofluoric acid:nitric acid:water = 1:1:2 mixture at 250°C or higher for 6 hours to remove solvents and foreign matter adhering to the SiC crystal. After treatment, the sample was ultrasonically cleaned with pure water and then dried. <Appearance Observation> The appearance of the samples was observed visually and photographed with a single-lens reflex camera (Canon EOS-X7) equipped with a close-up lens (EFS60 mm) by shining an LED light from above the crystal samples. <Transmission observation> For transmission observation of the sample, a transmission image was taken by shining an LED light from below the crystal sample using a single-lens reflex camera (Canon EOS-X7) equipped with a close-up lens (EFS 60 mm) in the same manner as for the external observation.
[0055] [Example 1] A crucible-shaped SiC sintered body (outer diameter φ60 mm, height 70 mm, inner diameter (diameter of the container) φ50 mm, container height 60 mm, relative density 80%, oxygen content 80 ppm sintered body) was used to manufacture SiC single crystals (crystal growth) in the manufacturing device shown in Figure 1. Crucible-shaped SiC sintered body To, A Pr-Fe-Si alloy with a composition of 20 atomic % Pr, 20 atomic % Fe, and 60 atomic % Si was charged and heat-treated at 1,500°C for 10 hours in an argon atmosphere to fill the pores of the SiC sintered body. The total volume of the holeThe alloy was impregnated to form a SiC crucible 1. Then, Pr, Fe, and Si were charged as single metals with a composition of Pr: 20 atomic %, Fe: 20 atomic %, and Si: 60 atomic %, and the amount was adjusted so that the depth of the Si-C solution was 27 mm based on density calculations. The seed crystal 3 was a single crystal (polytype: 4H, On-axis high grade) produced by sublimation method with a diameter of 21 mm and a thickness of 0.3 mm, which was bonded to a graphite seed shaft (rotating shaft 6) with a diameter of 19 mm so that the growth surface was the C-face. The SiC crucible 1 and the seed shaft (rotating shaft 6) were rotated at 20 rpm in different rotation directions (i.e., one clockwise and the other counterclockwise), and crystal growth was performed for 5 hours at 2,000 ° C. in an argon atmosphere with a pulling speed of 0.1 mm / hr.
[0056] Figure 4 shows the appearance of the growth surface (C-plane), which is a surface perpendicular (orthogonal) to the seed axis direction of the obtained SiC single crystal sample. The actual size of the photograph in Figure 4 is 27 mm in length and 23 mm in width. When the appearance of the SiC single crystal was evaluated, it was found that the growth surface of the SiC single crystal shown in Figure 4 was a crystal with no polycrystals attached. In addition, the growth rate of the SiC single crystal was 180 μm / hr.
[0057] The obtained SiC single crystal sample was ground and polished to provide a slope in the thickness direction from the crystal face (Si face) side to the growth part, resulting in a mirror-finished slope (Si face) with a slope angle of 2.6°. Next, the slope (Si face) was subjected to an alkaline etching method to create etch pits, and the type and number of dislocations were observed (Figs. 5 and 6). The dislocations can be classified into threading screw dislocations (TSDs), threading edge dislocations (TEDs), and basal plane dislocations (BPDs) based on their shape and size. The respective dislocations in Figs. 5 and 6 are indicated as "TSDs," "TEDs," and "BPDs." When all three types of dislocations were counted in all observable areas of the slope of the SiC single crystal sample, the number of dislocations in the seed crystal part (Fig. 5) was 5,152 / cm. 2 The number of dislocations in the solution-grown area (Fig. 6) was 952 / cm 2This confirmed the low dislocation count achieved by the solution method. Furthermore, the number of basal plane dislocations (BPDs), which are killer dislocations that cause yield reductions during device manufacturing, was 0 / cm in the solution-grown area (Figure 6). 2 It was as follows.
[0058] [Example 2] A crucible-shaped SiC sintered body (outer diameter φ90 mm, height 70 mm, inner diameter (diameter of the container) φ80 mm, container height 60 mm, relative density 80%, oxygen content 50 ppm sintered body) was used to manufacture SiC single crystals (crystal growth) in the manufacturing equipment shown in Figure 1. Crucible To, An Nd-Fe-Si alloy with a composition of Nd: 20 atomic %, Fe: 20 atomic %, and Si: 60 atomic % was charged and heat-treated at 1,500°C for 10 hours in an argon atmosphere to fill the pores of the SiC sintered body. The total volume of the hole The alloy was impregnated to form a SiC crucible 1. Nd, Fe, and Si were then charged as single metals with a composition of Nd: 20 atomic %, Fe: 20 atomic %, and Si: 60 atomic %, and the amount was adjusted so that the depth of the Si-C solution was 27 mm based on density calculations. The seed crystal 3 was a single crystal (polytype: 4H, On-axis, dummy grade) produced by sublimation method with a diameter of 50 mm and a thickness of 0.3 mm, which was bonded to a graphite seed shaft (rotating shaft 6) with a diameter of 49 mm so that the growth surface was the C-face. The SiC crucible 1 and the seed shaft (rotating shaft 6) were rotated at 5 rpm in different rotation directions (i.e., one clockwise and the other counterclockwise), and crystal growth was performed for 2 hours at 2,000 ° C. in an argon atmosphere with a pulling speed of 0.1 mm / hr.
[0059] Figure 7 shows the appearance of the growth surface (C-plane) of the obtained SiC single crystal sample. The actual size of the photograph in Figure 7 is 51 mm long and 51 mm wide. When the appearance of the obtained SiC single crystal was evaluated, the growth surface of the SiC single crystal shown in Figure 7 was flat and no polycrystals were attached. In addition, in Figure 7, the circular black part is a part where the Si-C solution adhered to the growth surface when the seed crystal grown by crystallization was separated from the Si-C solution after the crystal growth was completed and became a droplet (convex shape), and is not subject to evaluation (the same applies to the black parts in Figures 10 and 15 below). In addition, the growth thickness of the SiC single crystal was 300 μm in 2 hours, and the growth rate was 150 μm / hr.
[0060] The crystal face (Si face) of the seed crystal part of the obtained SiC single crystal sample and the crystal face of the solution growth part (i.e., the growth face (C face)) were each ground to a thickness of 100 μm, and then polished to a mirror finish. Next, dislocations were observed on this polished surface by reflection X-ray topography (Figures 8 and 9). As a result, there were fewer dislocations in the solution growth part (Figure 9) than in the seed crystal part (Figure 8), confirming the reduction in dislocations by the solution method. The dislocations observed in Figures 8 and 9 are threading dislocations (TSD, TED) as black dots and basal plane dislocations (BPD) as wire-like ones. The SiC wafer used as the seed crystal here was a dummy grade that had many dislocations and could not be used for devices, but the SiC single crystal was reduced in dislocations by growing it in the solution using the solution method. Threading screw dislocations (TSDs), threading edge dislocations (TEDs), and basal plane dislocations (BPDs) were all counted in the entire observation field area (area of 2.1 mm × 1.6 mm) of the polished surface of the SiC single crystal sample. As a result, the number of basal plane dislocations (BPDs), which have a large effect on the yield in device manufacturing, was 0 / cm in the solution growth area (Figure 9). 2 The number of dislocations in the seed crystal (Figure 8) was 50,115 / cm. 2 The number of dislocations in the solution-grown portion (Fig. 9) was 1,144 / cm 2The dislocations were reduced by approximately 98%. Furthermore, these results showed that even SiC wafers that contain many dislocations and cannot be used for devices can be regenerated into high-quality SiC single crystal wafers by using them as seed crystals for crystal growth by the solution method, which can be used as is for devices or as seed crystals (substrates) for vapor phase growth methods such as the sublimation method or gas method.
[0061] [Example 3] Next, solution growth was carried out for the case where the SiC single crystal seed crystal was off-axis (the (0001) Si face was slightly tilted in a specific direction ([11-20] direction) from the surface normal axis). That is, a SiC single crystal (polytype: 4H, off-axis 4°, dummy grade) with a diameter of 50 mm and a thickness of 0.3 mm was used as the seed crystal 3, which was attached to a graphite seed shaft with a diameter of 49 mm so that the growth surface was the C-plane, and the rest (SiC crucible 1 and metal components (composition) contained in the SiC crucible 1) were the same as in Example 2, and the SiC single crystal was manufactured (crystal growth) using a manufacturing apparatus as shown in Figure 1. At this time, the SiC crucible 1 and the seed shaft (rotating shaft 6) were rotated at 5 rpm each in different rotation directions (i.e., one clockwise and the other counterclockwise), and the crystal growth was performed at 2,000 °C for 2 hours in an argon atmosphere with a pulling speed of 0.1 mm / hr.
[0062] Figure 10 shows the appearance of the growth surface (C-plane) of the obtained SiC single crystal sample. The actual size of the photograph in Figure 10 is 51 mm in length and 51 mm in width. When the appearance of the obtained SiC single crystal was evaluated, it was found that the growth surface of the SiC single crystal was flat and free of polycrystal adhesion.
[0063] When the growth surface of the SiC single crystal was observed with a laser microscope (magnification: 5x), it was confirmed that macrosteps had formed on the C-face (000-1) toward the off-axis direction [11-20] (Figure 11). Next, to observe the cross-section of the SiC single crystal sample, the sample was sliced parallel to the off-axis direction [11-20] and perpendicular to the C-plane (000-1), and the cross-section was observed. As a result, the Si-C solution components (hereinafter simply referred to as solvent) were found to be trapped (Si-C solution components were included in the solution growth part) in the solution growth part with a thickness of 150 μm or more on the surface side out of the total thickness of 300 μm (Figure 12). This is thought to be because the growth on the SiC single crystal (off-axis substrate) with an off-axis angle formed macro steps, making it easier for the solvent to be trapped. The crystal cross-section shown in Figure 12 is a transmission image taken with a single-lens reflex camera (Canon EOS-X7) equipped with a close-up lens (EFS 60 mm) by illuminating the bottom of the crystal sample with an LED white light.
[0064] By the way, although the obtained SiC single crystal sample had some solvent inclusions, the growth thickness of the SiC single crystal was 300 μm in 2 hours, and the growth rate was 150 μm / hr. Since normal crystals were obtained up to 150 μm thick on the seed crystal side of the solution growth part, the crystal surface of the solution growth part was ground to remove a thickness of 200 μm, and the crystal surface of the seed crystal part was ground to remove a thickness of 100 μm, and then polished to a mirror finish (arithmetic mean roughness Ra: 10 nm or less). Next, dislocations were observed on these polished surfaces by reflection X-ray topography (Figures 13 and 14). As a result, there were fewer dislocations in the solution growth part (Figure 14) compared to the seed crystal part (Figure 13), and it was confirmed that the solution method reduced dislocations. The SiC wafer used as the seed crystal here was a dummy grade that had many dislocations and could not be used for devices, but dislocations were reduced by growing it in the solution using the solution method. When threading screw dislocations (TSDs), threading edge dislocations (TEDs), and basal plane dislocations (BPDs) were all counted in the entire observation field area (area of 2.1 mm × 1.6 mm) of the polished surface of the SiC single crystal sample, the number of basal plane dislocations (BPDs), which are killer dislocations that have a large impact on the yield in device manufacturing, in the solution growth area (Figure 14) was 0 / cm 2The number of dislocations in the seed crystal (Figure 13) was 29,762 / cm. 2 The number of dislocations in the solution-grown portion (Fig. 14) was 4,062 / cm 2 The dislocations were reduced by approximately 86%.
[0065] [Comparative Example 1] A graphite crucible (outer diameter φ90 mm, inner diameter φ80 mm, outer height 90 mm, inner height 90 mm) was used, and SiC single crystals were produced (crystal growth) using the production equipment shown in Figure 1. Nd, Fe, and Si were charged into the graphite crucible as single metals with compositions of Nd: 16 atomic %, Fe: 20 atomic %, and Si: 64 atomic %, and the amount was adjusted so that the depth of the Si-C solution was 27 mm based on density calculations. The seed crystal used was a single crystal (polytype: 4H, On-axis, dummy grade) with a diameter of 50 mm and a thickness of 0.3 mm, attached to a graphite seed axis with a diameter of 49 mm so that the growth surface was the C-plane. The crucible and the seed shaft were rotated in different directions (i.e., one clockwise and the other counterclockwise) at 5 rpm each, and the crystal was grown at a pulling rate of 0.1 mm / hr in an argon atmosphere at 2,000° C. for 2 hr.
[0066] As a result, the grown thickness of the obtained SiC single crystal sample was 300 μm in 5 hours, and the growth rate was 60 μm / hr, which was lower than that of Example 2 (growth rate 150 μm / hr).
[0067] Figure 15 shows the appearance of the growth surface (C-plane) of the obtained SiC single crystal sample. The actual size of the photograph in Figure 15 is 51 mm in length and 51 mm in width. When the appearance of the obtained SiC single crystal was compared with that of the SiC single crystal sample of Example 2 (Figure 7), no abnormalities were found on the growth surface of either.
[0068] Next, in order to observe the crystal cross section of the SiC single crystal sample, the sample was sliced perpendicular to the growth surface (C surface), polished, and then the cross section was observed. The SiC single crystal sample of Example 2 was also observed in the same manner. As a result, a large number of voids were observed near the seed crystal in the solution growth portion in Comparative Example 1 (FIG. 16), whereas no voids were observed in the solution growth portion in Example 2 (FIG. 17). This is believed to be because gas components (oxygen, nitrogen, etc.) contained in the graphite crucible used were generated in the early growth stage and inhibited normal solution growth. In contrast, since the present invention uses a SiC sintered body in a crucible shape with a low oxygen content (oxygen content rate of 50 ppm), it is believed that stable crystal growth is performed from the early growth stage without gas generation from the crucible. From this result, when a graphite crucible is used, it is necessary to grow the layer thicker than 200 to 300 μm to obtain a normal crystal growth surface, which is disadvantageous in terms of mass production. Furthermore, it is expected that growth will be even more difficult when using a SiC single crystal (off-axis substrate) as a seed crystal, which has an off-axis that makes it easy for the solvent to get caught in the solution growth area. Currently, the SiC seed crystals used in the gas phase method are mainly 4° off-axis, so the occurrence of voids in the early stages of growth can be said to be a fatal problem.
[0069] [Example 4] The SiC crucible used in the present invention (i.e., a SiC crucible in which an alloy of Si and a metal element M that increases the solubility of C is impregnated as a melt into a SiC sintered compact with a relative density of 50 to 90%) is suitable for long-term growth because there is no compositional variation in the Si-C solution (solvent). On the other hand, the growth time required for low-dislocation SiC crystal growth using the SiC crucible of the present invention is about 1 to 2 hours. Therefore, considering mass production, we investigated whether the SiC crucible and Si-C solution (solvent) used in the present invention can be used repeatedly.
[0070] As a method of investigation, the crystal growth (cultivation) of SiC single crystals was repeatedly performed under the same conditions as in Example 2 without replacing the SiC crucible and the Si-C solution (solvent), and the effect on the crystal quality of the obtained SiC single crystal sample was confirmed. That is, the crystal growth of the SiC single crystal was repeated five times, and the crystal quality of the obtained SiC single crystal sample was evaluated after each crystal growth. The evaluation methods were the same as those of Example 2, including appearance observation (presence or absence of polycrystal adhesion or abnormal growth (e.g., two-dimensional nucleation growth)) and growth rate, as well as the solvent entrapment observation (cross-sectional observation) and appearance observation of the crucible as in Comparative Example 1. The results are shown in Table 1.
[0071] [Table 1]
[0072] As a result, although a decrease in the growth rate was observed with the number of repeated crystal growth cycles, there were no problems with the appearance or end faces of the SiC single crystal sample, and no abnormalities were found in the crucible, confirming that crystal growth was possible about five times. The reason for the decrease in growth rate is thought to be that the SiC polycrystals formed in the crucible after crystal growth consumed the carbon supplied to the seed crystal (SiC single crystal). From the perspective of efficiency, if a continuous growth system could be constructed that could perform the next crystal growth without cooling the Si-C solution in the crucible after crystal growth, an increase in the number of repeated crystal growth cycles and stable crystal growth could be expected.
[0073] [Comparative Example 2] Under the same conditions as in Comparative Example 1, the graphite crucible and the Si-C solution (solvent) were used without being replaced to repeatedly grow a SiC single crystal, and the same evaluations were performed as in Example 4. The results are shown in Table 2.
[0074] [Table 2]
[0075] As a result, no polycrystals were found to adhere to the SiC single crystal sample in the first crystal growth, but polycrystals were found to adhere in the second crystal growth. In addition, a crack occurred in the graphite crucible in the second crystal growth, so the repeated crystal growth was stopped. It is considered difficult to repeatedly use the Si-C solution (solvent) in the graphite crucible. In addition, in Comparative Example 2, the growth rate in the second crystal growth was reduced to 57% of the growth rate in the first crystal growth. This is considered to be because the Si-C solution (solvent) was cooled after the first crystal growth, causing SiC to precipitate in a form that covered the graphite crucible wall, preventing carbon from dissolving out of the crucible during the second crystal growth. In contrast, in Example 4, the Si-C solution (solvent) composition was adjusted on the assumption that SiC would dissolve out, so the decrease in growth rate was small. As described above, by repeatedly using the SiC crucible used in the present invention (i.e., a SiC crucible in which a SiC sintered compact having a relative density of 50 to 90% is impregnated with an alloy of Si and a metal element M that increases the solubility of C as a molten liquid) and the Si-C solution (solvent), it is possible to efficiently produce high-quality SiC single crystals in a stable manner.
[0076] [Example 5] (i) Crystal growth by solution method A crucible-shaped SiC sintered body (outer diameter φ180 mm, height 60 mm, inner diameter (diameter of the container) φ150 mm, container height 40 mm, relative density 80%, oxygen content 40 ppm sintered body) was used to manufacture SiC single crystals (crystal growth) in the manufacturing device shown in Figure 1. Crucible To, An Nd-Fe-Si alloy with a composition of Nd: 20 atomic %, Fe: 20 atomic %, and Si: 60 atomic % was charged and heat-treated at 1,500°C for 10 hours in an argon atmosphere to fill the pores of the SiC sintered body. The total volume of the holeThe alloy was impregnated to form a SiC crucible 1. Nd, Fe, and Si were then charged as single metals with a composition of Nd: 20 atomic %, Fe: 20 atomic %, and Si: 60 atomic %, and the amount was adjusted so that the depth of the Si-C solution was 27 mm based on density calculations. The seed crystal 3 was a single crystal (polytype: 4H, off-axis 4°, dummy grade) with a diameter of 100 mm and a thickness of 1 mm, which was bonded to a graphite seed shaft (rotating shaft 6) with a diameter of 99 mm so that the growth surface was the C-plane. The SiC crucible 1 and the seed shaft (rotating shaft 6) were rotated at 5 rpm in different rotation directions (i.e., one clockwise and the other counterclockwise), and crystal growth was performed at 2,000 ° C. for 1 hour in an argon atmosphere with a pulling speed of 0.1 mm / hr. The C-plane of the seed crystal used was previously observed for dislocations by reflection X-ray topography.
[0077] When the obtained SiC single crystal sample (1) was evaluated, the crystal surface (growth surface (C-plane)) of the solution growth portion of the SiC single crystal sample shown in FIG. 18 had a mirror-like appearance with macrosteps uniformly formed on the C-plane (000-1) toward the [11-20] direction, similar to Example 3. Furthermore, when the polytype of the obtained SiC single crystal sample was identified by Raman observation (Raman spectroscopy), it was confirmed that the entire surface was 4H-SiC. In addition, the growth thickness of the solution-grown portion of the SiC single crystal sample reached 100 μm in 1 hour, and the growth rate was 100 μm / hr.
[0078] Next, the obtained SiC single crystal sample (1) was treated with fluoronitric acid, ultrasonically cleaned, and dried to remove the solvent components adhering to the growth surface, and then dislocations were observed on the solution growth surface (C surface) by reflection X-ray topography. That is, when threading screw dislocations (TSDs), threading edge dislocations (TEDs), and basal plane dislocations (BPDs) were all counted in the entire observation field area (area of 2.1 mm x 1.6 mm), the number of basal plane dislocations (BPDs), which are killer dislocations that have a large impact on the yield in device manufacturing, in the solution growth area was 0 / cm. 2The number of dislocations in the seed crystal was 32,506 / cm. 2 The number of dislocations in the solution-grown region was 4,020 / cm 2 From this result, it was demonstrated that the present invention enables uniform crystal growth even in a large-diameter solution growth.
[0079] (ii) Bulk growth by sublimation Next, the number of dislocations is 4,020 / cm 2 Using the reduced SiC single crystal sample (1) as a seed crystal, bulk growth was carried out by sublimation method using the following procedure. The above-mentioned SiC single crystal sample (seed crystal) 11 was set on the top (inner wall of the upper lid 12a) of the reaction vessel 12 shown in Figure 19 with the solution growth portion 11b facing downward, and the raw material SiC powder 13 was placed directly below it, and this reaction vessel 12 was then placed in a sublimation reaction apparatus 20 shown in Figure 20. The SiC growth in the sublimation reaction apparatus 20 of FIG. 20 was performed under typical conditions, with the source temperature being 2,200 to 2,500° C., the seed crystal temperature being 2,100 to 2,400° C., the temperature gradient being 1 to 50° C. / cm, the pressure being 100 to 5,000 Pa (argon atmosphere), and the growth rate being 0.05 to 0.2 mm / hr.
[0080] The resulting SiC single crystal (SiC ingot) sample (2) had a growth thickness of 5 mm, which was sliced, ground and polished to obtain four wafers with a thickness of 1 mm. Dislocation observation was performed on these wafers using the reflection X-ray topography method in the same manner as above, and the number of dislocations was found to be 4,210 to 4,400 / cm. 2 It was.
[0081] Furthermore, this wafer (dislocation count 4,210 / cm 2 ) was again subjected to solution growth under the conditions in (i) above to obtain a SiC single crystal sample (3). The crystal faces of the obtained SiC single crystal sample (3) were counted for threading screw dislocations (TSDs), threading edge dislocations (TEDs), and basal plane dislocations (BPDs) by reflection X-ray topography in the same manner as described above. The number of basal plane dislocations (BPDs), which are killer dislocations that have a large impact on the yield in device manufacturing in the solution growth area, was 0 / cm. 2 Other dislocations were also significantly reduced, with the number of dislocations being 590 / cm 2 It was. Next, this SiC single crystal sample (4) was used as a seed crystal and bulk grown again by sublimation under the conditions in (ii) above to obtain a SiC single crystal sample (5). The obtained SiC single crystal sample (5) was subjected to dislocation observation by reflection X-ray topography in the same manner as described above. As a result, the number of dislocations was 625 to 643 / cm. 2 The increase in the number of dislocations compared to the above-mentioned SiC single crystal sample (4) is believed to be due to reconversion or new generation of dislocations during bulk growth by the sublimation method.
[0082] From the above results, it was found that dislocations can be reduced by performing solution growth to a thickness of about 100 μm on a seed crystal (SiC wafer) produced by sublimation using the solution method of the present invention, and that the low dislocation state can be maintained even if this is used as a seed crystal (substrate) for bulk growth by sublimation. It was also demonstrated that bulk-grown SiC single crystal with low dislocations can be further solution-grown by the solution method of the present invention to further reduce dislocations, and that by using this as a seed crystal, bulk growth maintaining an even lower dislocation state is possible. [Explanation of symbols]
[0083] 1 SiC crucible 2. The Second Crucible 3. SiC single crystal (seed crystal) 4 Si-C solution 5th and 6th rotation axes 7 Susceptor 8. Insulation 9 Top lid 10 High frequency coil 11 Seed Crystal 11a Seed crystal part 11b Solution growth section 11c Growing SiC single crystal 12 Reaction vessel 12a Top lid 12b Carbon container 13 SiC powder 20 Sublimation reactor 21 High frequency coil 1 22 High frequency coil 2 23 Insulation 24 Insulator 25 Lifting Stage
Claims
1. A method for producing a SiC single crystal, comprising the steps of: impregnating a SiC sintered body having a relative density of 50 to 90% with a molten alloy of Si and a metal element M that increases the solubility of C to form a SiC crucible; then, placing Si and the metal element M in the SiC crucible; heating the SiC crucible to melt the Si and the metal element M in the SiC crucible and form a Si-C solution; dissolving Si and C originating from the components of the SiC crucible into the Si-C solution from the surface of the SiC crucible in contact with the Si-C solution; contacting a SiC seed crystal with an upper portion of the Si-C solution; growing a SiC single crystal on the SiC seed crystal at a growth rate of 100 μm / hr or more; and then bulk-growing a SiC single crystal on the surface of the grown SiC single crystal by a sublimation method or a gas method.
2. 2. The method for producing a SiC single crystal according to claim 1, wherein the metal element M is a metal consisting of the metal element M alone or an alloy containing the metal element M (but not containing Si) contained in the SiC crucible.
3. 3. The method for producing a SiC single crystal according to claim 1 or 2, wherein the metal element M is at least one first metal element M1 selected from the group consisting of La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Y, and Lu, at least one second metal element M2 selected from the group consisting of Ti, V, Cr, Mn, Fe, Co, Ni, and Cu, and / or at least one third metal element M3 selected from the group consisting of Ga, Ge, Sn, Pb, and Zn.
4. The method for producing a SiC single crystal according to claim 3, wherein the metal element M is a metal element consisting of the first metal element M1 and the second metal element M2.
5. 5. The method for producing a SiC single crystal according to claim 3, wherein the total content of the metal element M in the Si-C solution is 1 to 80 atomic % with respect to the total amount of Si and M.
6. The method for producing a SiC single crystal according to any one of claims 3 to 5, wherein the content of the first metal element M1 in the Si-C solution is 1 atomic % or more with respect to the total amount of Si and metal element M, and the contents of the second metal element M2 and the third metal element M3 in the Si-C solution are each 1 atomic % or more with respect to the total amount of Si and metal element M.
7. The method for producing a SiC single crystal according to any one of claims 1 to 6, wherein the SiC sintered body has an oxygen content of 100 ppm or less.
8. The method for producing a SiC single crystal according to any one of claims 1 to 7, wherein the growth of the SiC single crystal by the solution method is carried out at a temperature of the Si-C solution of 1,300 to 2,300°C.
9. The method for producing a SiC single crystal according to any one of claims 1 to 8, wherein the method is carried out in a state in which the SiC crucible is contained in a second crucible made of a heat-resistant carbon material.
10. The method for producing a SiC single crystal according to any one of claims 1 to 9, wherein the thickness of the SiC single crystal grown by the solution method is 10 to 1,000 µm.
11. The method for producing a SiC single crystal according to any one of claims 1 to 10, wherein the SiC crucible and the Si-C solution are repeatedly used.
12. A method for suppressing dislocations in a SiC single crystal, comprising: impregnating a SiC sintered body having a relative density of 50 to 90% with a molten alloy of Si and a metal element M that increases the solubility of C to form a SiC crucible; then, placing Si and the metal element M in the SiC crucible; heating the SiC crucible to melt the Si and the metal element M in the SiC crucible and form a Si-C solution; dissolving Si and C originating from components of the SiC crucible into the Si-C solution from the surface of the SiC crucible in contact with the Si-C solution; and contacting a SiC seed crystal with an upper portion of the Si-C solution to grow a SiC single crystal on the SiC seed crystal by a solution method at a growth rate of 100 μm / hr or more.
13. 13. The method for suppressing dislocations in a SiC single crystal according to claim 12, further comprising the step of bulk growing a SiC single crystal on a surface of the SiC single crystal obtained by the solution method by a sublimation method or a gas method.
14. 14. The method for suppressing dislocations in a SiC single crystal according to claim 13, wherein a SiC single crystal wafer obtained from a SiC single crystal bulk-grown by the sublimation method or the gas method is used as a SiC seed crystal, and a SiC single crystal is grown on the SiC seed crystal by the solution method.
15. 15. The method for suppressing dislocations in a SiC single crystal according to claim 14, further comprising the step of bulk growing a SiC single crystal on a surface of the SiC single crystal obtained by the solution method by a sublimation method or a gas method.
Citation Information
Patent Citations
Production of silicon carbide single crystal
JP2000264790A
Silicon carbide single crystal and its manufacturing method
JP2004002173A
Method for manufacturing silicon carbide single crystal
JP2006143555A
Silicon carbide crystal growth method
JP2015110495A
Silicon carbide crystal growth method
JP2015110496A