Resin composition, optical fiber, and method for producing optical fiber

A resin composition with urethane (meth)acrylate oligomer and hydrophobic inorganic oxide particles addresses the toughness issue in optical fiber secondary resin layers, improving durability by balancing Young's modulus and elongation.

JP7552594B2Active Publication Date: 2024-09-18SUMITOMO ELECTRIC INDUSTRIES LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021526073
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-06-11
Filing Date
2020-06-05
Publication Date
2024-09-18
Estimated Expiration
2040-06-05

AI Technical Summary

Technical Problem

Existing optical fiber coating resin layers, particularly the secondary resin layer, suffer from reduced toughness when filled with fillers, leading to potential cracking and inability to withstand long-term use under lateral pressure.

Method used

A resin composition comprising a urethane (meth)acrylate oligomer, monomer, photopolymerization initiator, and hydrophobic inorganic oxide particles is used to form a secondary resin layer with a balanced Young's modulus and elongation, enhancing toughness and lateral pressure characteristics.

Benefits of technology

The resin composition forms a resin layer with excellent toughness, improving the optical fiber's ability to withstand bending without cracking, thereby enhancing its long-term durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007552594000004
    Figure 0007552594000004
  • Figure 0007552594000003
    Figure 0007552594000003
  • Figure 0007552594000002
    Figure 0007552594000002
Patent Text Reader

Abstract

A resin composition for coating optical fibers includes a base resin, that contains an oligomer including a urethane (meth)acrylate oligomer, a monomer, and a photopolymerization initiator, and hydrophobic inorganic oxide particles. A resin film obtained by curing the resin composition at an integrated light intensity of from 900 mJ / cm2 to 1100 mJ / cm2 has a break elongation of from 2.5% to 50% at 23°C and a Young's modulus of from 1150 MPa to 2700 MPa at 23°C.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a resin composition, an optical fiber, and a method for producing an optical fiber. This application claims priority to Japanese Application No. 2019-108597, filed on June 11, 2019, and incorporates by reference all of the contents of said Japanese application. [Background technology]

[0002] In general, an optical fiber has a coating resin layer for protecting a glass fiber that is an optical transmission medium. The optical fiber is required to have excellent lateral pressure characteristics in order to reduce an increase in transmission loss induced by a minute bending that occurs when a lateral pressure is applied to the optical fiber.

[0003] The coating resin layer can be formed using an ultraviolet-curable resin composition containing an oligomer, a monomer, a photopolymerization initiator, etc. For example, Patent Document 1 discusses improving the lateral pressure characteristics of an optical fiber by forming a resin layer using an ultraviolet-curable resin composition containing a filler made of synthetic quartz. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2014-219550 A Summary of the Invention

[0005] The resin composition according to one embodiment of the present disclosure includes a base resin containing an oligomer including a urethane (meth)acrylate oligomer, a monomer, and a photopolymerization initiator, and hydrophobic inorganic oxide particles. 2 More than 1100mJ / cm 2 The resin film cured with the following integrated light amount has a breaking elongation of 2.5% or more and 50% or less at 23°C, and a Young's modulus of 1150 MPa or more and 2700 MPa or less at 23°C. [Brief description of the drawings]

[0006] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of an optical fiber according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] [Problem that this disclosure aims to solve] The coating resin layer generally includes a primary resin layer and a secondary resin layer. The resin composition forming the secondary resin layer is required to improve the lateral pressure characteristics of the optical fiber by increasing the Young's modulus. However, the resin layer formed from the resin composition containing a filler has reduced toughness, and when the optical fiber is bent, cracks may occur in the coating resin layer, and the optical fiber may not be able to withstand long-term use.

[0008] An object of the present disclosure is to provide a resin composition capable of forming a resin layer having excellent toughness, and an optical fiber including a secondary resin layer formed from the resin composition.

[0009] [Effects of this disclosure] According to the present disclosure, it is possible to provide a resin composition capable of forming a resin layer having excellent toughness, and an optical fiber including a secondary resin layer formed from the resin composition.

[0010] [Description of the embodiments of the present disclosure] First, the contents of the embodiment of the present disclosure will be listed and described. The resin composition according to one aspect of the present disclosure includes a base resin containing an oligomer including a urethane (meth)acrylate oligomer, a monomer, and a photopolymerization initiator, and hydrophobic inorganic oxide particles. The resin composition is applied to a substrate at a dose of 900 mJ / cm. 2 More than 1100mJ / cm 2 The resin film cured with the following integrated light amount has a breaking elongation of 2.5% or more and 50% or less at 23°C, and a Young's modulus of 1150 MPa or more and 2700 MPa or less at 23°C.

[0011] Such a resin composition can form a resin layer having excellent toughness. Moreover, by using the resin composition as an ultraviolet-curable resin composition for coating an optical fiber, an optical fiber having excellent lateral pressure characteristics can be produced.

[0012] Since the resin layer has an excellent balance between Young's modulus and elongation, the content of the urethane (meth)acrylate oligomer may be 15% by mass or more and 70% by mass or less based on the total amount of the oligomer and monomer.

[0013] The above monomers may include a monomer having a phenoxy group, since this makes it easier to form a tough resin layer.

[0014] The inorganic oxide particles may be particles containing at least one selected from the group consisting of silicon dioxide, zirconium dioxide, aluminum oxide, magnesium oxide, titanium oxide, tin oxide and zinc oxide, because they have excellent dispersibility in the resin composition and allow easy adjustment of the Young's modulus.The inorganic oxide particles may have an average primary particle size of 5 nm or more and 800 nm or less, because they form a resin layer with a high Young's modulus.

[0015] Since a tougher resin layer is easily formed, the resin film may have a breaking elongation of 5.0% or more and 45% or less at 23°C.

[0016] An optical fiber according to an embodiment of the present disclosure includes a glass fiber including a core and a cladding, a primary resin layer that contacts the glass fiber and coats the glass fiber, and a secondary resin layer that coats the primary resin layer, the secondary resin layer including a cured product of the resin composition, thereby improving the lateral pressure characteristics of the optical fiber.

[0017] The method for producing an optical fiber according to one aspect of the present disclosure includes a coating step of coating the resin composition on the outer periphery of a glass fiber composed of a core and a cladding, and a curing step of curing the resin composition by irradiating ultraviolet light after the coating step. This allows a resin layer with excellent toughness to be formed, thereby making it possible to produce an optical fiber that is prevented from being damaged during a rewinding operation.

[0018] [Details of the embodiment of the present disclosure] Specific examples of the resin composition and optical fiber according to the present embodiment will be described with reference to the drawings as necessary. Note that the present invention is not limited to these examples, but is indicated by the claims, and is intended to include all modifications within the meaning and scope equivalent to the claims. In the following description, the same elements in the description of the drawings will be given the same reference numerals, and duplicated descriptions will be omitted.

[0019] <Resin composition> The resin composition according to the present embodiment contains a base resin containing an oligomer including a urethane (meth)acrylate oligomer, a monomer, and a photopolymerization initiator, and hydrophobic inorganic oxide particles.

[0020] From the viewpoint of forming a resin layer having excellent toughness, the above resin composition is applied at a pressure of 900 mJ / cm 2 More than 1100mJ / cm 2 The breaking elongation of the resin film cured with the following integrated light amount is 2.5% or more and 50% or less at 23° C. The lower limit of the breaking elongation of the resin film may be 2.6% or more, 2.8% or more, 5.0% or more, or 7.0% or more, and the upper limit of the breaking elongation of the resin film may be 48% or less, 45% or less, or 40% or less. Since the effects of the present disclosure are easily exhibited, the breaking elongation of the resin film is preferably 5.0% or more and 45% or less at 23° C., and more preferably 7.0% or more and 45% or less.

[0021] The Young's modulus of the resin film is 1150 MPa or more and 2700 MPa or less at 23° C., preferably 1200 MPa or more and 2600 MPa or less, and more preferably 1200 MPa or more and 2500 MPa or less. When the Young's modulus of the resin film is 1150 MPa or more, the lateral pressure characteristics of the optical fiber are easily improved. When the Young's modulus of the resin film is 2700 MPa or less, appropriate toughness can be imparted to the secondary resin layer, making it difficult for cracks and the like to occur in the secondary resin layer.

[0022] (Base resin) The oligomer according to the present embodiment includes a urethane (meth)acrylate oligomer. As the urethane (meth)acrylate oligomer, an oligomer obtained by reacting a polyol compound, a polyisocyanate compound, and a hydroxyl group-containing (meth)acrylate compound can be used. Here, the (meth)acrylate means an acrylate or a methacrylate corresponding thereto. The same applies to (meth)acrylic acid.

[0023] Examples of polyol compounds include polytetramethylene glycol, polypropylene glycol, and bisphenol A-ethylene oxide addition diol. Examples of polyisocyanate compounds include 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, isophorone diisocyanate, and dicyclohexylmethane 4,4'-diisocyanate. Examples of hydroxyl group-containing (meth)acrylate compounds include 2-hydroxyethyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 1,6-hexanediol mono(meth)acrylate, pentaerythritol tri(meth)acrylate, 2-hydroxypropyl (meth)acrylate, and tripropylene glycol mono(meth)acrylate.

[0024] From the viewpoint of adjusting the Young's modulus and elongation of the resin film, the number average molecular weight (Mn) of the polyol compound is preferably 300 or more and 3,000 or less, more preferably 400 or more and 2,500 or less, and even more preferably 500 or more and 2,000 or less.

[0025] In general, an organic tin compound is used as a catalyst when synthesizing urethane (meth)acrylate oligomer. Examples of the organic tin compound include dibutyltin dilaurate, dibutyltin diacetate, dibutyltin maleate, dibutyltin bis(2-ethylhexyl mercaptoacetate), dibutyltin bis(isooctyl mercaptoacetate), and dibutyltin oxide. In terms of easy availability or catalytic performance, it is preferable to use dibutyltin dilaurate or dibutyltin diacetate as a catalyst.

[0026] A lower alcohol having 5 or less carbon atoms may be used during synthesis of the urethane (meth)acrylate oligomer. Examples of the lower alcohol include methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, 2-methyl-2-propanol, 1-pentanol, 2-pentanol, 3-pentanol, 2-methyl-1-butanol, 3-methyl-1-butanol, 2-methyl-2-butanol, 3-methyl-2-butanol, and 2,2-dimethyl-1-propanol.

[0027] From the viewpoint of further increasing the toughness of the resin layer, the content of the urethane (meth)acrylate oligomer is preferably from 15% by mass to 70% by mass, more preferably from 16% by mass to 65% by mass, and even more preferably from 17% by mass to 60% by mass, based on the total amount of the oligomer and monomer.

[0028] From the viewpoint of increasing the Young's modulus of the resin film, the oligomer may further contain an epoxy (meth)acrylate oligomer. As the epoxy (meth)acrylate oligomer, an oligomer obtained by reacting an epoxy resin having two or more glycidyl groups with a compound having a (meth)acryloyl group can be used.

[0029] The monomer may be a monofunctional monomer having one polymerizable group or a polyfunctional monomer having two or more polymerizable groups. Two or more kinds of monomers may be mixed and used.

[0030] A monomer having a phenoxy group may be used as the monomer since it is easy to form a tough resin layer.

[0031] As the monomer having a phenoxy group, a (meth)acrylate compound having a phenoxy group can be used. As the (meth)acrylate compound having a phenoxy group, for example, phenol EO modified (meth)acrylate, nonylphenol EO modified (meth)acrylate, phenol PO modified (meth)acrylate, nonylphenol PO modified (meth)acrylate, phenoxyethyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, and 3-phenoxybenzyl (meth)acrylate can be mentioned. Here, EO modified means having an ethylene oxide group represented by (C2H4O)n, and PO modified means having a propylene oxide group represented by (C3H6O)n. n is an integer of 1 or more.

[0032] From the viewpoint of adjusting the Young's modulus of the resin film, the monomer having a phenoxy group may be at least one selected from the group consisting of phenol EO modified acrylate, nonylphenol EO modified acrylate, phenoxyethyl acrylate, 2-hydroxy-3-phenoxypropyl acrylate, and 3-phenoxybenzyl acrylate. Two or more types of monomers having a phenoxy group may be mixed and used.

[0033] The content of the monomer having a phenoxy group is preferably 1% by mass or more and 30% by mass or less, more preferably 2% by mass or more and 25% by mass or less, and even more preferably 4% by mass or more and 20% by mass or less, based on the total amount of the oligomer and the monomer. By including the monomer having a phenoxy group in such a range in the resin composition, a resin layer having a Young's modulus more suitable as a secondary coating material for an optical fiber can be formed.

[0034] As the monomer, a monomer not having a phenoxy group may be used. The monomer not having a phenoxy group may be a monofunctional monomer or a polyfunctional monomer.

[0035] Examples of monofunctional monomers not having a phenoxy group include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, s-butyl (meth)acrylate, tert-butyl (meth)acrylate, isobutyl (meth)acrylate, n-pentyl (meth)acrylate, isopentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, isoamyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and n-octyl (Meth)acrylate, isooctyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, 4-tert-butylcyclohexanol (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, benzyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, dicyclopentanyl (meth)acrylate, nonylphenol polyethylene glycol (meth)acrylate, isobornyl (meth)acrylate, and other (meth)acrylates. Acrylate monomers; carboxyl group-containing monomers such as (meth)acrylic acid, (meth)acrylic acid dimer, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, and ω-carboxy-polycaprolactone (meth)acrylate; N-acryloylmorpholine, N-vinylpyrrolidone, N-vinylcaprolactam, N-acryloylpiperidine, N-methacryloylpiperidine, N-acryloylpyrrolidine, 3-(3-pyridine)propyl (meth)acrylate, and cyclic trimethylolpropane formal acrylate. heterocycle-containing (meth)acrylates such as acrylates; maleimide monomers such as maleimide, N-cyclohexylmaleimide, and N-phenylmaleimide; N-substituted amide monomers such as (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N-hexyl(meth)acrylamide, N-methyl(meth)acrylamide, N-butyl(meth)acrylamide, N-butyl(meth)acrylamide, N-methylol(meth)acrylamide, and N-methylolpropane(meth)acrylamide;Examples of such monomers include aminoalkyl (meth)acrylate monomers such as aminoethyl (meth)acrylate, aminopropyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, and tert-butylaminoethyl (meth)acrylate; and succinimide monomers such as N-(meth)acryloyloxymethylene succinimide, N-(meth)acryloyl-6-oxyhexamethylene succinimide, and N-(meth)acryloyl-8-oxyoctamethylene succinimide.

[0036] Examples of polyfunctional monomers not having a phenoxy group include ethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, di(meth)acrylate of an alkylene oxide adduct of bisphenol A, tetraethylene glycol di(meth)acrylate, and neopentyl glycol di(meth)acrylate of hydroxypivalic acid. acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,12-dodecanediol di(meth)acrylate, 1,14-tetradecanediol di(meth)acrylate, 1,16-hexadecanediol di(meth)acrylate, 1,20-eicosanediol di(meth)acrylate, isopentyldiol di(meth)acrylate, 3-ethyl-1,8-octanediol di(meth)acrylate , EO adduct di(meth)acrylate of bisphenol A, trimethylolpropane tri(meth)acrylate, trimethyloloctane tri(meth)acrylate, trimethylolpropane polyethoxy tri(meth)acrylate, trimethylolpropane polypropoxy tri(meth)acrylate, trimethylolpropane polyethoxy polypropoxy tri(meth)acrylate, tris[(meth)acryloyloxyethyl]isocyanurate, pentaerythritol tri(meth)acrylate, penta Examples of the polyether acrylate include erythritol polyethoxy tetra(meth)acrylate, pentaerythritol polypropoxy tetra(meth)acrylate, pentaerythritol tetra(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and caprolactone-modified tris[(meth)acryloyloxyethyl]isocyanurate.

[0037] The photopolymerization initiator can be appropriately selected from known radical photopolymerization initiators. Examples of the photopolymerization initiator include 1-hydroxycyclohexyl phenyl ketone (Omnirad 184, manufactured by IGM Resins), 2,2-dimethoxy-2-phenylacetophenone, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropan-1-one, bis(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-propan-1-one (Omnirad 907, manufactured by IGM Resins), 2,4,6-trimethylbenzoyldiphenylphosphine oxide (Omnirad TPO, manufactured by IGM Resins), and bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide (Omnirad 819, manufactured by IGM Resins).

[0038] The resin composition may further contain a silane coupling agent, a leveling agent, a defoaming agent, an antioxidant, a sensitizer, and the like.

[0039] Silane coupling agents are not particularly limited as long as they do not interfere with the curing of the resin composition. Examples of silane coupling agents include tetramethyl silicate, tetraethyl silicate, mercaptopropyl trimethoxysilane, vinyl trichlorosilane, vinyl triethoxysilane, vinyl tris(β-methoxy-ethoxy)silane, β-(3,4-epoxycyclohexyl)-ethyl trimethoxysilane, dimethoxydimethylsilane, diethoxydimethylsilane, 3-acryloxypropyl trimethoxysilane, γ-glycidoxypropyl trimethoxysilane, γ-glycidoxypropyl methyl diethoxysilane, γ-methacryloxypropyl trimethoxysilane, N-(β-aminoethyl)-γ -aminopropyltrimethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethyldimethoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, γ-chloropropyltrimethoxysilane, γ-mercaptopropyltrimethoxysilane, γ-aminopropyltrimethoxysilane, bis-[3-(triethoxysilyl)propyl]tetrasulfide, bis-[3-(triethoxysilyl)propyl]disulfide, γ-trimethoxysilylpropyldimethylthiocarbamyltetrasulfide, and γ-trimethoxysilylpropylbenzothiazyltetrasulfide.

[0040] (Inorganic oxide particles) The inorganic oxide particles according to the present embodiment have their surfaces hydrophobically treated. The hydrophobic treatment according to the present embodiment refers to the introduction of a hydrophobic group to the surface of the inorganic oxide particles. The inorganic oxide particles having the hydrophobic group introduced thereto have excellent dispersibility in the resin composition. The hydrophobic group may be a reactive group such as a (meth)acryloyl group or a vinyl group, or a non-reactive group such as an aliphatic hydrocarbon group (e.g., an alkyl group) or an aromatic hydrocarbon group (e.g., a phenyl group). When the inorganic oxide particles have a reactive group, it becomes easier to form a resin layer having a high Young's modulus.

[0041] The inorganic oxide particles according to the present embodiment are dispersed in a dispersion medium. By using the inorganic oxide particles dispersed in a dispersion medium, the inorganic oxide particles can be uniformly dispersed in the resin composition, and the storage stability of the resin composition can be improved. The dispersion medium is not particularly limited as long as it does not inhibit the curing of the resin composition. The dispersion medium may be reactive or non-reactive.

[0042] As the reactive dispersion medium, monomers such as (meth)acryloyl compounds and epoxy compounds may be used. As the (meth)acryloyl compounds, for example, 1,6-hexanediol di(meth)acrylate, EO modified bisphenol A di(meth)acrylate, polyethylene glycol di(meth)acrylate, PO modified bisphenol A di(meth)acrylate, polypropylene glycol di(meth)acrylate, and polytetramethylene glycol di(meth)acrylate may be used. As the (meth)acryloyl compounds, compounds exemplified as the monomers described above may be used.

[0043] As the non-reactive dispersion medium, a ketone solvent such as methyl ethyl ketone (MEK), an alcohol solvent such as methanol (MeOH), or an ester solvent such as propylene glycol monomethyl ether acetate (PGMEA) may be used. In the case of a non-reactive dispersion medium, a resin composition may be prepared by mixing a base resin and inorganic oxide particles dispersed in the dispersion medium, and then removing a part of the dispersion medium.

[0044] The inorganic oxide particles dispersed in the dispersion medium remain dispersed in the resin layer even after the resin composition is cured. When a reactive dispersion medium is used, the inorganic oxide particles are mixed into the resin composition together with the dispersion medium, and are incorporated into the resin layer while maintaining the dispersed state. When a non-reactive dispersion medium is used, at least a part of the dispersion medium is evaporated from the resin composition, but the inorganic oxide particles remain dispersed in the resin composition and remain dispersed in the resin layer after curing. When the inorganic oxide particles present in the resin layer are observed with an electron microscope, the primary particles are observed to be dispersed.

[0045] The inorganic oxide particles are preferably at least one selected from the group consisting of silicon dioxide (silica), zirconium dioxide (zirconia), aluminum oxide (alumina), magnesium oxide (magnesia), titanium oxide (titania), tin oxide, and zinc oxide, because they have excellent dispersibility in the resin composition and are easy to form a tough resin layer. From the viewpoints of low cost, ease of surface treatment, ultraviolet transmittance, and ease of imparting appropriate hardness to the resin layer, it is more preferable to use hydrophobic silica particles as the inorganic oxide particles according to this embodiment.

[0046] From the viewpoint of increasing the Young's modulus of the resin film, the average primary particle size of the inorganic oxide particles is preferably 5 nm to 800 nm, more preferably 10 nm to 700 nm, and even more preferably 10 nm to 650 nm. The average primary particle size can be measured, for example, by image analysis of an electron microscope photograph, a light scattering method, a BET method, or the like. The dispersion medium in which the primary particles of the inorganic oxide are dispersed appears transparent to the naked eye when the particle size of the primary particles is small. When the particle size of the primary particles is relatively large (40 nm or more), the dispersion medium in which the primary particles are dispersed appears cloudy, but no sediment is observed.

[0047] The content of inorganic oxide particles is preferably 1% by mass or more and 60% by mass or less, more preferably 10% by mass or more and 50% by mass or less, and even more preferably 15% by mass or more and 40% by mass or less, based on the total amount of oligomer, monomer and inorganic oxide particles. When the content of inorganic oxide particles is 1% by mass or more, it is easy to form a resin layer having excellent lateral pressure characteristics. When the content of inorganic oxide particles is 60% by mass or less, it is easy to improve the coatability of the resin composition.

[0048] The resin composition according to the present embodiment can be suitably used as a secondary coating material for an optical fiber. By using the resin composition according to the present embodiment for the secondary resin layer, a coating resin layer having excellent toughness can be formed, and the lateral pressure characteristics of the optical fiber can be improved.

[0049] <Optical fiber> 1 is a schematic cross-sectional view showing an example of an optical fiber according to the present embodiment. The optical fiber 10 includes a glass fiber 13 including a core 11 and a cladding 12, and a coating resin layer 16 including a primary resin layer 14 and a secondary resin layer 15 provided on the outer periphery of the glass fiber 13.

[0050] The cladding 12 surrounds the core 11. The core 11 and the cladding 12 mainly contain glass such as silica glass, and for example, the core 11 can be made of silica glass doped with germanium or pure silica glass, and the cladding 12 can be made of pure silica glass or silica glass doped with fluorine.

[0051] 1, for example, the outer diameter (D2) of the glass fiber 13 is about 100 μm to 125 μm, and the diameter (D1) of the core 11 constituting the glass fiber 13 is about 7 μm to 15 μm. The thickness of the coating resin layer 16 is usually about 22 μm to 70 μm. The thickness of each of the primary resin layer 14 and the secondary resin layer 15 may be about 5 μm to 50 μm.

[0052] When the outer diameter (D2) of the glass fiber 13 is about 125 μm and the thickness of the coating resin layer 16 is 60 μm to 70 μm, the thickness of each of the primary resin layer 14 and the secondary resin layer 15 may be about 10 μm to 50 μm, for example, the thickness of the primary resin layer 14 may be 35 μm and the thickness of the secondary resin layer 15 may be 25 μm. The outer diameter of the optical fiber 10 may be about 245 μm to 265 μm.

[0053] When the outer diameter (D2) of the glass fiber 13 is about 125 μm and the thickness of the coating resin layer 16 is 27 μm to 48 μm, the thickness of each of the primary resin layer 14 and the secondary resin layer 15 may be about 10 μm to 38 μm, for example, the thickness of the primary resin layer 14 may be 25 μm and the thickness of the secondary resin layer 15 may be 10 μm. The outer diameter of the optical fiber 10 may be about 179 μm to 221 μm.

[0054] When the outer diameter (D2) of the glass fiber 13 is about 100 μm and the thickness of the coating resin layer 16 is 22 μm to 37 μm, the thickness of each of the primary resin layer 14 and the secondary resin layer 15 may be about 5 μm to 32 μm, for example, the thickness of the primary resin layer 14 may be 25 μm and the thickness of the secondary resin layer 15 may be 10 μm. The outer diameter of the optical fiber 10 may be about 144 μm to 174 μm.

[0055] The resin composition according to the present embodiment can be applied to the secondary resin layer. The secondary resin layer can be formed by curing the resin composition containing the above-mentioned base resin and inorganic oxide particles. This makes it possible to form a resin layer having excellent toughness.

[0056] The manufacturing method of the optical fiber according to this embodiment includes a coating step of coating the above-mentioned resin composition on the outer circumference of a glass fiber composed of a core and a cladding, and a curing step of curing the resin composition by irradiating it with ultraviolet light after the coating step.

[0057] The primary resin layer 14 can be formed, for example, by curing a resin composition containing a urethane (meth)acrylate oligomer, a monomer, a photopolymerization initiator, and a silane coupling agent. The resin composition for the primary resin layer can be formed using a conventionally known technique. The urethane (meth)acrylate oligomer, the monomer, the photopolymerization initiator, and the silane coupling agent may be appropriately selected from the compounds exemplified for the base resin above. However, the resin composition forming the primary resin layer has a different composition from the base resin forming the secondary resin layer. EXAMPLES

[0058] The present disclosure will be described in more detail below by showing the results of evaluation tests using examples and comparative examples according to the present disclosure. Note that the present disclosure is not limited to these examples.

[0059] [Resin composition for secondary resin layer] (Oligomer) The oligomers prepared were a urethane acrylate oligomer (UA-1) obtained by reacting polypropylene glycol having a molecular weight of 2000, 2,4-tolylene diisocyanate, and hydroxyethyl acrylate, a urethane acrylate oligomer (UA-2) obtained by reacting polypropylene glycol having a molecular weight of 600, 2,4-tolylene diisocyanate, and hydroxyethyl acrylate, and an epoxy acrylate oligomer (EA).

[0060] (monomer) As monomers, 2-phenoxyethyl acrylate (POA, trade name "Light Acrylate PO-A" manufactured by Kyoeisha Chemical Co., Ltd.) and tripropylene glycol diacrylate (TPGDA, trade name "Viscoat #310HP" manufactured by Osaka Organic Chemical Industry Ltd.) were prepared.

[0061] (Photopolymerization initiator) As photopolymerization initiators, 1-hydroxycyclohexyl phenyl ketone and 2,4,6-trimethylbenzoyldiphenylphosphine oxide were prepared.

[0062] (Inorganic oxide particles) As inorganic oxide particles, a silica sol containing silica particles (Si-1 to Si-6) having the surface conditions and average primary particle sizes shown in Table 1 was prepared.

[0063] [Table 1]

[0064] (Resin composition) First, the oligomer, monomer, and photopolymerization initiator were mixed to prepare a base resin. Next, silica sol was mixed with the base resin so as to obtain the content of silica particles shown in Table 2 or Table 3, and then most of MEK (methyl ethyl ketone) as a dispersion medium was removed under reduced pressure to prepare the resin compositions of the examples and comparative examples. The content of MEK remaining in the resin composition was 5 mass% or less.

[0065] In Tables 2 and 3, the numerical values ​​for oligomer and monomer are the contents based on the total amount of oligomer and monomer, and the numerical value for silica particles is the content based on the total amount of monomer, oligomer and silica particles.

[0066] (Young's Modulus) The resin composition was applied onto a polyethylene terephthalate (PET) film using a spin coater, and then 900 mJ / cm was applied using an electrodeless UV lamp system (Heraeus's "VPS600 (D bulb)"). 2 More than 1100mJ / cm 2 The resin was cured with the following accumulated light amount to form a resin layer with a thickness of 200±20 μm on the PET film. The resin layer was peeled off from the PET film to obtain a resin film. The resin film was punched into a dumbbell shape according to JIS K 7127 Type 5 to prepare a test piece for measuring Young's modulus. The test piece was pulled using a tensile tester at 23±2°C, 50±10% RH, a pulling speed of 1 mm / min, and a gauge distance of 25 mm to obtain a stress-strain curve. Young's modulus was calculated using the 2.5% secant line.

[0067] (Elongation at break) A resin layer having a thickness of 50±5 μm was formed on a PET film in the same manner as in the preparation of the resin film. The resin layer was peeled off from the PET film to obtain a resin film. The resin film was punched into a dumbbell shape conforming to JIS Z6251 No. 3 to prepare a test piece for measuring the breaking elongation. The test piece was pulled at a speed of 1 mm / min using an INSTRON material testing machine Model 5985 under conditions of 23±2°C and 50±10% RH, and the elongation was measured using an INSTRON high-precision video extensometer AVE.

[0068] [Fabrication of optical fiber] A urethane acrylate oligomer was prepared by reacting polypropylene glycol having a molecular weight of 4000, isophorone diisocyanate, hydroxyethyl acrylate, and methanol. 75 parts by mass of this urethane acrylate oligomer, 12 parts by mass of nonylphenol EO-modified acrylate, 6 parts by mass of N-vinyl caprolactam, 2 parts by mass of 1,6-hexanediol diacrylate, 1 part by mass of 2,4,6-trimethylbenzoyldiphenylphosphine oxide, and 1 part by mass of 3-mercaptopropyltrimethoxysilane were mixed to obtain a resin composition for the primary resin layer.

[0069] The resin composition for the primary resin layer and the resin composition for the example or comparative example were applied to the outer circumference of a glass fiber having a diameter of 125 μm, which is composed of a core and a clad, and then the resin composition was cured by irradiating with ultraviolet light to form a primary resin layer having a thickness of 35 μm and a secondary resin layer having a thickness of 25 μm on the outer circumference of the primary resin layer, thereby producing an optical fiber. The drawing speed was 1500 m / min.

[0070] (Bending test) An optical fiber with a length of 1 m was wound once around a mandrel with a diameter of 3 mm, both ends were fixed, and the mandrel was moved back and forth three times in the longitudinal direction to check for the presence or absence of breakage.

[0071] [Table 2]

[0072] [Table 3] [Explanation of symbols]

[0073] 10 Optical Fiber 11 cores 12 Clad 13 Glass Fiber 14 Primary resin layer 15 Secondary resin layer 16 Resin coating layer

Claims

1. The present invention relates to a resin composition comprising a base resin containing an oligomer including a urethane (meth)acrylate oligomer, a monomer including a monomer having a phenoxy group, and a photopolymerization initiator, and hydrophobic inorganic oxide particles having a hydrophobic surface, the content of the urethane (meth)acrylate oligomer is 15% by mass or more and 70% by mass or less based on the total amount of the oligomer and the monomer, The resin composition is applied at 900 mJ / cm 2 More than 1100mJ / cm 2 A resin composition for coating an optical fiber, the resin film cured with the following integrated light amount has a breaking elongation of 2.5% or more and 50% or less at 23°C and a Young's modulus of 1150 MPa or more and 2700 MPa or less at 23°C.

2. 2. The resin composition according to claim 1, wherein the inorganic oxide particles are at least one selected from the group consisting of silicon dioxide, zirconium dioxide, aluminum oxide, magnesium oxide, titanium oxide, tin oxide, and zinc oxide.

3. The resin composition according to claim 1 or 2, wherein the inorganic oxide particles have an average primary particle size of 5 nm or more and 800 nm or less.

4. The resin composition according to claim 1 , wherein the resin film has a breaking elongation of 5.0% or more and 45% or less at 23° C.

5. a glass fiber including a core and a cladding; a primary resin layer that is in contact with and covers the glass fiber; A secondary resin layer that covers the primary resin layer, An optical fiber, wherein the secondary resin layer comprises a cured product of the resin composition according to claim 1 .

6. A coating step of coating the resin composition according to any one of claims 1 to 4 on an outer periphery of a glass fiber including a core and a clad; a curing step of curing the resin composition by irradiating the resin composition with ultraviolet light after the coating step; A method for manufacturing an optical fiber, comprising:

Citation Information

Patent Citations

  • Coated optical fiber

    JP1990069706A

  • Ultraviolet-curing resin composition

    JP2000007717A

  • Photocurable composition and its manufacturing method, as well as cured product

    JP2004204206A

  • Radiation-curable coating composition

    JP2010511770A

  • Coated optical fiber

    JP2014219550A