Film, film roll, and method for producing film
A film with alternating convex and concave regions along its length addresses winding defects by controlling air gaps, ensuring film integrity and device performance in applications like displays and touch sensors.
Patent Information
- Application Number
- JP2022534916
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-07-06
- Filing Date
- 2021-04-19
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2041-04-19
AI Technical Summary
Winding defects occur when forming film rolls due to improper air management between films, leading to issues such as sticking and deformation, especially in thinner films used in devices like displays and touch sensors.
The film is designed with alternating convex and concave regions along its length, where the thickness of the ends is either smaller or larger than the central portion, allowing precise control of air gaps and preventing defects.
This design effectively suppresses winding defects, maintaining film integrity and enhancing device performance by preventing sticking and deformation, even in long film rolls.
Smart Images

Figure 0007552694000013 
Figure 0007552694000018 
Figure 0007552694000011
Abstract
Description
[Technical field]
[0001] The present invention relates to a film, a film roll, and a method for producing the film. [Background technology]
[0002] In recent years, with the trend toward lighter and more flexible devices, films used in the devices have been made thinner. For example, thin optical films are used in devices such as displays and touch sensors (for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2017-100372 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, when the film is made thinner, winding defects are more likely to occur when the film roll is formed, and the quality of the film may be impaired. For example, if the amount of air between the film is too small, winding defects such as sticking between the film layers occur.
[0005] Therefore, an object of the present invention is to provide a film, a film roll, and a method for producing a film that are capable of suppressing the occurrence of winding defects. [Means for solving the problem]
[0006] The above-mentioned object of the present invention can be achieved by the following means.
[0007] a film having a first end and a second end in a width direction intersecting with a longitudinal direction, a central portion between the first end and the second end, a convex position where a thickness Te1 of at least the first end of the first end and the second end is smaller than a thickness Tc of the central portion, and a concave position that is disposed at a position different from the convex position in the longitudinal direction and where the thickness Te1 of the first end is larger than the thickness Tc of the central portion. Effect of the Invention
[0008] According to the present invention, the film has a convex position where the thickness Te1 of the first end is smaller than the thickness Tc of the central portion, and a concave position where the thickness Te1 of the first end is larger than the thickness Tc of the central portion, so that it is easy to control the amount of air between the film when forming a film roll. Therefore, it is possible to prevent winding defects. [Brief description of the drawings]
[0009] [Figure 1] FIG. 2 is a schematic diagram illustrating an example of a configuration of a film roll according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a plan view illustrating an example of the configuration of the film illustrated in FIG. [Diagram 3] 3A is a diagram illustrating a cross-sectional configuration of a convex region shown in FIG. 2, and FIG. 3B is a diagram illustrating a cross-sectional configuration of a concave region shown in FIG. [Figure 4] FIG. 4 is a diagram illustrating another example of the cross-sectional configuration of the end portion of the film shown in FIGS. [Figure 5A] 3 is a diagram illustrating an example of the relationship between the position in the longitudinal direction of the film illustrated in FIG. 2 and the difference ratio D between the thicknesses of the end portions and the central portion. FIG. [Figure 5B] 5B is a diagram illustrating another example of the relationship between the position in the longitudinal direction of the film and the difference ratio D illustrated in FIG. 5A. FIG. [Figure 5C] 5B is a diagram illustrating another example of the relationship between the position in the longitudinal direction of the film and the difference ratio D illustrated in FIG. 5A. FIG. [Figure 6A]5B is a diagram illustrating another example of the relationship between the position in the longitudinal direction of the film and the difference ratio D illustrated in FIG. 5A. FIG. [Figure 6B] 5B is a diagram illustrating another example of the relationship between the position in the longitudinal direction of the film and the difference ratio D illustrated in FIG. 5A. FIG. [Figure 7] 1 is a flow chart illustrating an example of a method for producing a film. [Figure 8] FIG. 8 is a diagram illustrating a configuration of a clip tenter used in the process of step S102 shown in FIG. [Figure 9A] 13 is a diagram illustrating an example of the relationship between the longitudinal position of a film and a difference ratio D according to a comparative example. FIG. [Figure 9B] 9B is a diagram illustrating another example of the relationship between the position in the longitudinal direction of the film and the difference ratio D illustrated in FIG. 9A. FIG. [Figure 9C] 9B is a diagram illustrating another example of the relationship between the position in the longitudinal direction of the film and the difference ratio D illustrated in FIG. 9A. FIG. [Figure 10] 2 is a diagram illustrating an example of a configuration of an end surface of the film roll illustrated in FIG. 1. [Figure 11] FIG. 13 is a diagram illustrating an example of a cross-sectional configuration of a film according to a modified example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Preferred embodiments of the present invention will be described below. In this specification, the range "X to Y" means "X or more and Y or less." Unless otherwise specified, the operations and physical properties are measured under the conditions of room temperature (20 to 25°C) and relative humidity of 40 to 50% RH.
[0011] Furthermore, the dimensional proportions in the drawings have been exaggerated for the convenience of explanation and may differ from the actual proportions.
[0012] FIG. 1 shows a schematic configuration of a film roll 1 according to one embodiment. This film roll 1 is formed by winding an optical film 11 in a roll shape around a winding core 12. The optical film 11 has optical functions such as light transmission, reflection, diffusion, and absorption, and is used, for example, in displays, touch sensors, and the like. The winding core 12 has, for example, a cylindrical shape and a predetermined length (the size in the X direction in FIG. 1). The optical film 11 is wound in the circumferential direction of this winding core 12. The total winding length of the film roll 1 is, for example, 500 m to 20,000 m.
[0013] 2 shows an example of a planar configuration of the optical film 11. The optical film 11 is wound around a core 12 along its longitudinal direction. In the following description, the longitudinal direction of the optical film 11 may be referred to as the Y direction, the width direction intersecting the longitudinal direction as the X direction, and the thickness direction as the Z direction. Here, the width direction of the optical film 11 is substantially perpendicular to the longitudinal direction. The longitudinal size of the optical film 11 is, for example, 500 m to 20,000 m, and the width direction of the optical film 11 is, for example, 100 mm to 3,000 mm.
[0014] The optical film 11 has a pair of ends e1, e2 in the width direction, and a central portion c between the pair of ends e1, e2. The pair of ends e1, e2 and the central portion c each have, for example, about 10% of the overall size of the optical film 11 in the width direction, with the end e1 including one end of the optical film 11 in the width direction, the end e2 including the other end of the optical film 11 in the width direction, and the central portion c including the center of the optical film 11 in the width direction. Here, the end e1 corresponds to a specific example of a first end portion of the present invention, and the end e2 corresponds to a specific example of a second end portion of the present invention.
[0015] This optical film 11 has convex regions R1 and concave regions R2 aligned in the Y direction. For example, the optical film 11 is provided with a plurality of convex regions R1 and concave regions R2, and the convex regions R1 and concave regions R2 are alternately arranged in the Y direction.
[0016] Fig. 3(A) shows the XZ cross section of the convex region R1, and Fig. 3(B) shows the XZ cross section of the concave region R2. In the convex region R1, the thickness Te1 of the end e1 and the thickness Te2 of the end e2 are smaller than the thickness Tc of the central portion c, and in the concave region R2, the thickness Te1 of the end e1 and the thickness Te2 of the end e2 are larger than the thickness Tc of the central portion c. That is, in the convex region R1, the thicknesses Te1, Te2, and Tc preferably satisfy the following formulas (1) and (2), and in the concave region R2, the thicknesses Te1, Te2, and Tc preferably satisfy the following formulas (3) and (4).
[0017]
number
[0018]
number
[0019] In other words, it is preferable that at the convex position P1 provided in the convex region R1, the thicknesses Te1, Te2, and Tc satisfy the formulas (1) and (2), and at the concave position P2 provided in the concave region R2, the thicknesses Te1, Te2, and Tc satisfy the formulas (3) and (4). The convex position P1 may be any position within the convex region R1, and the concave position P2 may be any position within the concave region R2.
[0020] Although details will be described later, in this embodiment, the optical film 11 has such convex positions P1 and concave positions P2, more specifically, convex regions R1 and concave regions R2, so that it is easy to control the amount of air between overlapping optical films 11 when forming the film roll 1. This makes it possible to prevent winding defects from occurring.
[0021] At the convex position P1 and the convex region R1, the thickness Te1 of the end e1 may be smaller than the thickness Tc of the central portion c, and at this time, at the concave position P2 and the concave region R2, the thickness Te1 of the end e1 may be larger than the thickness Tc of the central portion c. That is, at the convex position P1 and the convex region R1, the thicknesses Te1 and Tc may at least satisfy formula (1), and at this time, at the concave position P2 and the concave region R2, the thicknesses Te1 and Tc may at least satisfy formula (3).
[0022] In the optical film 11, it is preferable that the thicknesses Te1, Te2, and Tc at the convex position P1 and the convex region R1 satisfy the formulas (1) and (2), and that the thicknesses Te1, Te2, and Tc at the concave position P2 and the concave region R2 satisfy the formulas (3) and (4). This can more effectively prevent the occurrence of winding defects. For example, at a predetermined position in the Y direction, the thickness Te1 of the end e1 and the thickness Te2 of the end e2 are almost the same. The average thickness of the entire optical film 11 is, for example, about 10 μm to 40 μm. The size in the Y direction of each of the convex region R1 and the concave region R2 is preferably 100 m to 500 m, and more preferably 250 m or more. This can more effectively prevent the occurrence of winding defects. The size in the Y direction of the convex region R1 and the concave region R2 is, for example, almost the same. The sizes of the convex region R1 and the concave region R2 in the Y direction are different from each other. It may be possible.
[0023] Fig. 4 shows another example of the cross-sectional configuration of the optical film 11 shown in Fig. 3. The optical film 11 may have an embossed portion E. The embossed portion E is a portion that has been embossed, and for example, has projections and recesses on its surface. The embossed portion E is provided, for example, on ends e1 and e2. In this case, the thicknesses Te1 and Te2 of the ends e1 and e2 are, for example, the thicknesses of the projections of the embossed portion E.
[0024] In the optical film 11, the difference between the thicknesses Te1, Te2 of the ends e1, e2 and the thickness Tc of the central portion c at a predetermined position in the Y direction (for example, the convex position P1, the concave position P2) can be expressed by the difference ratio D1 and the difference ratio D2. The difference ratio D1 and the difference ratio D2 are the difference between the thicknesses Te1, Te2 and the thickness Tc with respect to the average thickness Ta of the optical film 11, and can be expressed by the following formula (5) and formula (6). In the convex region R1, the difference ratio D1 and the difference ratio D2 are positive values, and in the concave region R2, the difference ratio D1 and the difference ratio D2 are negative values. The absolute values of the difference ratio D1 and the difference ratio D2 (hereinafter, represented as |D1|, |D2|) are, for example, 10% or less, and more preferably 5% or less. By setting |D1|, |D2| to 5% or less, the occurrence of winding defects can be more effectively suppressed.
[0025]
number
[0026] For example, the difference ratio D1 and the difference ratio D2 at a predetermined position in the Y direction are approximately the same. In the following description, when the difference ratio D1 and the difference ratio D2 at a predetermined position in the Y direction are approximately the same, the difference ratio D1 and the difference ratio D2 are collectively referred to as the difference ratio D. In Figures 5A to 6B and 8A to 8C described below, the difference ratio D1 and the difference ratio D2 at a predetermined position in the Y direction are approximately the same, and the difference ratio D is used.
[0027] 5A, 5B, and 5C show an example of the relationship between the position in the Y direction of the optical film 11 and the differential ratio D. The optical film 11 has, for example, constant portions C1 and C2 in the convex region R1 and the concave region R2, respectively, where the differential ratio D is constant. For example, in the convex region R1, the absolute value of the differential ratio D (hereinafter referred to as |D|) is the largest in the constant portion C1, and in the concave region R2, |D| is the largest in the constant portion C2. The |D| of the constant portions C1 and C2, i.e., the maximum value of |D| of the convex region R1 and the concave region R2, is preferably 10% or less, and more preferably 5% or less.
[0028] The optical film 11 preferably has a sloping portion S between the constant portion C1 and the constant portion C2 (FIGS. 5A and 5B). The sloping portion S is a portion where the difference ratio D (%) changes continuously along the longitudinal direction. In other words, in the sloping portion S, at least one of the thicknesses Te1, Te2 of the ends e1, e2 and the thickness Tc of the central portion c changes continuously along the longitudinal direction. By having such a sloping portion S, the optical film 11 can more effectively prevent the occurrence of winding defects compared to a case where the sloping portion S is not present (FIG. 5C). By making the size of the sloping portion S in the Y direction 5 m or more, the occurrence of winding defects can be more effectively prevented. In the sloping portion S, the amount of change in |D| per 100 m of size in the Y direction, i.e., the slope of the sloping portion S, is, for example, preferably 0.03% to 10.0%, more preferably 0.05% to 7.5%, and even more preferably 2.0% to 5.0%. This makes it possible to more effectively prevent winding defects from occurring.
[0029] 6A and 6B show other examples of the relationship between the position in the Y direction of the optical film 11 and the differential ratio D. In this way, the change in the differential ratio D in the Y direction may be nonlinear. The differential ratio D may have multiple maximum values in the convex region R1 or the concave region R2 (FIG. 6B). An inflection point of the differential ratio D may be provided in the convex region R1 or the concave region R2. The relationship between the position in the Y direction of the optical film 11 and the differential ratio D is not limited to the examples shown in FIGS. 5A to 6B.
[0030] Such an optical film 11 is made of, for example, a resin having a property of being transparent to a desired wavelength. Examples of such resins include polymers containing an alicyclic structure such as cycloolefin resin (COP). The optical film 11 may be made of an acrylic resin, a cellulose ester resin, a polycarbonate resin, a polyethersulfone resin, a polyethylene terephthalate (PET) resin, a polyimide resin, a polymethyl methacrylate resin, a polysulfone resin, a polyarylate resin, a polyethylene resin, a polyvinyl chloride resin, or the like.
[0031] Among the above resins, it is preferable to use a cycloolefin resin from the viewpoints of transparency, mechanical strength, etc. Examples of the cycloolefin resin include (co)polymers having structural units derived from the following structures.
[0032] [ka]
[0033] In the formula, R 1 ~R 4 are each independently a hydrogen atom, a hydrocarbon group, a halogen atom, a hydroxyl group, an ester group, an alkoxy group, a cyano group, an amide group, an imide group, a silyl group, or a hydrocarbon group substituted with a polar group (i.e., a halogen atom, a hydroxyl group, an ester group, an alkoxy group, a cyano group, an amide group, an imide group, or a silyl group). 1 ~R 4Two or more of R may be bonded to each other to form an unsaturated bond, a monocyclic ring, or a polycyclic ring, and the monocyclic ring or polycyclic ring may have a double bond or form an aromatic ring. 1 and R 2 With or R 3 and R 4 and m may form an alkylidene group. Each of p and m is independently an integer of 0 or more.
[0034] In the above general formula, R 1 and R 3 R is preferably a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms, more preferably a hydrocarbon group having 1 to 4 carbon atoms, and particularly preferably a hydrocarbon group having 1 to 2 carbon atoms. 2 and R 4 is a hydrogen atom or a monovalent organic group, R 2 and R 4 At least one of the above is preferably a polar group having polarity other than a hydrogen atom or a hydrocarbon group. m is preferably an integer of 0 to 3, and p is preferably an integer of 0 to 3, more preferably m+p=0 to 4, further preferably m+p=0 to 2, and particularly preferably m=1 and p=0. The specific monomer where m=1 and p=0 is preferred in that the resulting cycloolefin resin has a high glass transition temperature and excellent mechanical strength.
[0035] Examples of the polar group of the specific monomer include a carboxy group, a hydroxy group, an alkoxycarbonyl group, an allyloxycarbonyl group, an amino group, an amide group, and a cyano group. These polar groups may be bonded via a linking group such as a methylene group. Examples of the polar group include a hydrocarbon group to which a divalent organic group having polarity is bonded as a linking group, such as an ether group, a silyl ether group, a thioether group, or an imino group. Among these, a carboxy group, a hydroxy group, an alkoxycarbonyl group, or an aryloxycarbonyl group is preferred, and an alkoxycarbonyl group or an aryloxycarbonyl group is particularly preferred.
[0036] In addition, R 2 and R 4At least one of the formula -(CH2) n Monomers having a polar group represented by COOR are preferred in that the resulting cycloolefin resin has a high glass transition temperature, low moisture absorption, and excellent adhesion to various materials. In the formula for the specific polar group, R is preferably an alkyl group having 1 to 12 carbon atoms, more preferably an alkyl group having 1 to 4 carbon atoms, and particularly preferably an alkyl group having 1 to 2 carbon atoms. n is an integer of 0 or more.
[0037] When the above structural unit has a polar group, specific examples of other copolymerizable monomers include cycloolefins such as cyclobutene, cyclopentene, cycloheptene, cyclooctene, dicyclopentadiene, and norbornene.
[0038] The number of carbon atoms in the cycloolefin as a copolymerizable monomer is not particularly limited, but is preferably 4-20, and more preferably 5-12.
[0039] The cycloolefin resin contained in the optical film 11 may be one type, or two or more types.
[0040] The cycloolefin resin contained in the optical film 11 has an intrinsic viscosity [ηinh] of preferably 0.2 to 5 dL / g, more preferably 0.3 to 3 dL / g, and even more preferably 0.4 to 1.5 dL / g. The number average molecular weight (Mn) in terms of polystyrene measured by gel permeation chromatography (GPC) is preferably 8,000 to 100,000, more preferably 10,000 to 80,000, and even more preferably 12,000 to 50,000, and the weight average molecular weight (Mw) is preferably in the range of 20,000 to 300,000, more preferably 30,000 to 250,000, and even more preferably 40,000 to 200,000.
[0041] By having the intrinsic viscosity [ηinh], number average molecular weight, and weight average molecular weight within the above ranges, the cycloolefin resin has good heat resistance, water resistance, chemical resistance, mechanical properties, and moldability as a cycloolefin film. The intrinsic viscosity [ηinh] value is the viscosity of a solution in which the cycloolefin resin is dissolved in chloroform, measured at a temperature of 30°C. Viscosity measurements are performed on three or more solutions each having a different concentration of cycloolefin resin. An Ubbelohde viscometer is used for the measurements.
[0042] The glass transition temperature (Tg) of the cycloolefin resin contained in the optical film 11 is, for example, preferably 110°C or higher, more preferably 110 to 350°C, further preferably 120 to 250°C, and particularly preferably 120 to 220°C. If the Tg is 110°C or higher, deformation due to use under high temperature conditions or secondary processing such as coating and printing can be suppressed. On the other hand, if the Tg is 350°C or lower, molding processing becomes easy and deterioration of the resin due to heat during molding processing can be prevented. For the value of the glass transition temperature (Tg), a thermal analysis of the cycloolefin resin is performed at a heating rate of 20°C / min, and the midpoint glass transition temperature value obtained according to JIS K7121 (1987) is adopted. For the thermal analysis, a differential scanning calorimeter DSC220 manufactured by Seiko Instruments Inc. is used.
[0043] The optical film 11 preferably contains 50% by mass or more, more preferably 70 to 90% by mass or more. It contains the above cycloolefin resin.
[0044] The optical film 11 may contain known hydrocarbon resins, thermoplastic resins, thermoplastic elastomers, rubbery polymers, organic particles, or inorganic particles, as described in, for example, JP-A-9-221577 and JP-A-10-287732, within the scope of not impairing the effects of this embodiment. The optical film 11 may contain additives, such as a specific wavelength dispersion agent, a sugar ester compound (also simply called sugar ester), an antioxidant, a peeling promoter, rubber particles, or a plasticizer.
[0045] The cycloolefin resin contained in the optical film 11 may be a commercially available product or a synthetic product. Examples of commercially available products include SANUQI (registered trademark) from Konica Minolta, Inc., ARTON (registered trademark, the same applies below) G, ARTON F, ARTON R, and ARTON RX from JSR Corporation, and ZEONOR (registered trademark) ZF14, ZF16, ZEONEX (registered trademark, the same applies below) 250, and ZEONEX 280 from Zeon Corporation.
[0046] <Method of manufacturing optical film> Fig. 7 is a flow chart showing an example of a method for producing the optical film 11. The optical film 11 is preferably produced, for example, by preparing or forming an original film (for example, an original film 11f in Fig. 8 described later) and then forming the convex regions R1 and the concave regions R2 in this original film. More preferably, the optical film 11 is produced, for example, by forming an original film (step S101) and then forming the convex regions R1 and the concave regions R2 in this original film (step S102). The method for producing the optical film 11 will be described below.
[0047] In step S101, the raw film may be a preformed one or may be newly formed. In step S101, for example, a raw film having a width direction and a length direction is formed.
[0048] The method of forming the raw film is not particularly limited, and known methods can be used. Among these, from the viewpoint of productivity, it is preferable to manufacture by the solution casting method or the melt casting method, and from the viewpoint of transparency, transportability and flexibility, it is more preferable to manufacture by the solution casting method. Here, the solution casting method is generally a method in which a solution in which a resin and other components that may be optionally contained are dissolved is cast onto a support, dried on the support, and then a film-like material (web) is peeled off, and the web is further dried after peeling to form a film. On the other hand, the melt casting method is generally a method in which a resin and other components that may be optionally contained are melt-kneaded to manufacture a film, and the mixture is heated to a temperature at which it exhibits fluidity and melted, and then cast as a fluid molten material to form a film.
[0049] When the solution casting method is used, the raw film according to the present invention may be a film-like material (web) or a film obtained by peeling the web and then drying it.
[0050] The amount of residual solvent when peeling the web from the support is not particularly limited as long as the amount is sufficient to provide self-supporting properties that allow peeling, but from the viewpoint of providing good flatness to the raw film, the amount is preferably within the range of 10 to 50% by mass, more preferably within the range of 15 to 40% by mass, and even more preferably within the range of 20 to 30% by mass.
[0051] The residual solvent content of the web or film is defined by the following formula: Residual solvent amount (mass%) = {(MN) / N} x 100 Here, M is the mass of a sample taken at any time during or after the production of the web or film, and N is the mass of M after heating at 115° C. for 1 hour.
[0052] The residual solvent amount in the film obtained by further drying the web after peeling is preferably 1% by mass or less, more preferably 0.1% by mass or less, and particularly preferably within the range of 0 to 0.01% by mass.
[0053] For example, it is preferable to form a raw film as follows. In the solution casting method, first, a dope containing a resin and a solvent is prepared. Then, the dope is cast onto a support. The casting is performed while moving the support. Next, the cast film formed on the support is peeled off from the support. After that, the cast film is dried as necessary to form a raw film containing a resin. As described above, the raw film may be a so-called web.
[0054] The solvent used for the dope is not particularly limited, and examples thereof include chlorine-based solvents such as chloroform and dichloromethane (methylene chloride); aromatic solvents such as toluene, xylene, benzene, and mixtures thereof; alcohol-based solvents such as methanol, ethanol, isopropanol, n-butanol, and 2-butanol; methyl cellosolve, ethyl cellosolve, butyl cellosolve, ethylene glycol monomethyl ether, dimethylformamide, dimethyl sulfoxide, dioxane, cyclohexanone, tetrahydrofuran, acetone, methyl ethyl ketone (MEK), ethyl acetate, and diethyl ether.
[0055] The solid content of the dope is not particularly limited, but is preferably 10 to 35% by mass, and more preferably 15 to 35% by mass.
[0056] The support is not particularly limited, but is preferably one with a mirror-finished surface, and a stainless steel belt (stainless steel belt) or a cast drum with a plated surface is preferably used.
[0057] In step S102, for example, the original film is stretched in the width direction while the end portions of the original film in the width direction are heated to form the convex regions R1 and the concave regions R2 in the original film. The thickness of the original film is generally reduced by stretching compared to before stretching, but the thickness is less likely to be reduced near the ends held by clips or the like compared to the central portion. By heating the ends of this original film, the thicknesses Te1 and Te2 of the ends e1 and e2 of the film 11 are adjusted.
[0058] It is possible to control the thicknesses Te1, Te2 of the ends e1, e2 by adjusting the temperature, conveying speed, and equipment when stretching the raw film (see, for example, SEN-I GAKKAISHI (Textiles and Industry), Vol. 41, No. 9, pp. 290-301, 1985), and any method may be used for the stretching technique.
[0059] 8 shows an example of the configuration of a clip tenter 50 used for stretching the original film (original film 11f) in the width direction. In the clip tenter 50, the original film 11f is stretched in the width direction while being transported along the longitudinal direction. In the clip tenter 50, a first relaxation area 50A before stretching, a stretching area 50B, a second relaxation area 50C after stretching, and a cooling area 50D are arranged in this order. The original film 11f is transported by passing through the first relaxation area 50A, the stretching area 50B, the second relaxation area 50C, and the cooling area 50D in this order.
[0060] For example, the first relaxation area 50A, the stretching area 50B, and the second relaxation area 50C of the clip tenter 50 each include a heating member for heating both ends of the raw film 11f. 51 is arranged (see, for example, JP 2011-115985 A). For example, the heating members 51 are arranged in each of the first relaxation area 50A, the stretching area 50B, and the second relaxation area 50C. The heating members 51 may be arranged in at least one of the first relaxation area 50A, the stretching area 50B, and the second relaxation area 50C. The heating members 51 may be capable of adjusting the temperature depending on the position in the X direction. For example, a plurality of heating members 51 may be arranged in the X direction, and the temperature of the heating members 51 may be changed in the X direction. The temperature of the heating members 51 is controlled by a control unit 52.
[0061] The heating member 51 is, for example, an infrared ray irradiating member that irradiates infrared rays toward the end of the original film 11f in the width direction. The heating member 51 may be a blowing member that blows high-temperature air or inert gas toward the end of the original film 11f in the width direction, or may be a heating wire and a heating roll. The heating member 51 is, for example, disposed at the front, rear, top, or bottom of the original film 11f, or at a plurality of these locations. The position of the heating member 51 in the X direction is preferably 10 mm to 500 mm away from the portion where both ends of the film 11 in the width direction are to be formed, and more preferably 20 mm to 400 mm away. This makes it easier to control the thicknesses Te1 and Te2 of the ends e1 and e2. The both ends of the film 11 in the width direction are formed, for example, by slitting the portion (ends in the width direction) held by the clip from the original film 11f after stretching.
[0062] Using a clip tenter 50 provided with heating members 51 in each of the first relaxation area 50A, the stretching area 50B, and the second relaxation area 50C, convex areas R1 and concave areas R2 are formed in the raw film 11f, for example, as follows.
[0063] First, both ends of the original film 11f in the width direction are held by clips or the like. Then, the conveyance of the original film 11f is started. As a result, the original film 11f passes through the first relaxation area 50A, the stretching area 50B, the second relaxation area 50C, and the cooling area 50D in order, and is stretched in the width direction. The conveyance speed of the original film 11f is not particularly limited, but is preferably 3 m / min to 100 m / min, and more preferably 5 m / min to 50 m / min. By setting the conveyance speed to 3 m / min or more, more preferably 5 m / min or more, it becomes easy to adjust the amount of air between the films 11, and it becomes possible to reduce the conveyance time and reduce costs. By setting the conveyance speed to 100 m / min or less, more preferably 50 m / min or less, it is possible to prevent the heating member 51 for applying a sufficient amount of heat to the target area from becoming large, and to reduce equipment costs.
[0064] In the first relaxation area 50A, the stretching area 50B, and the second relaxation area 50C, the temperatures of both ends in the width direction of the original film 11f are preferably about 0°C to 50°C higher than the temperature of the center. Here, the temperature of the heating member 51 is changed over time by the control unit 52, so that the temperature difference between both ends and the center of the part forming the convex region R1 in the original film 11f is made larger than the temperature difference between both ends and the center of the part forming the concave region R2. As a result, the thicknesses Te1 and Te2 of the ends e1 and e2 of the convex region R1 become smaller than the thicknesses Te1 and Te2 of the ends e1 and e2 of the concave region R2, and the convex region R1 and the concave region R2 are formed in the original film 11f. For example, in the portion where the convex region R1 is formed, the temperature difference between both ends and the center of the original film 11f is set to 20°C to 30°C, and in the portion where the concave region R2 is formed, the temperature difference between both ends and the center of the original film 11f is set to 0°C to 10°C.
[0065] For example, the magnitude of |D| can be controlled by adjusting the temperature difference between both ends and the center of the original film 11f. In the portion forming the convex region R1, the greater the temperature difference between the ends and the center, the greater the |D| becomes. In the portion forming the concave region R2, the greater the temperature difference between the ends and the center, the greater the |D| becomes. The smaller the temperature difference between the bottom and center, the larger |D| becomes.
[0066] For example, the rate of change in |D| per 100 m in the Y direction can be controlled by adjusting the rate of increase and decrease in temperature at both ends of the original film 11f (or the heating member 51). The faster the rate of increase or decrease in temperature at both ends, the greater the rate of change in |D| per 100 m in the Y direction.
[0067] The difference in temperature between both ends and the center of the original film 11f is preferably 50°C or less. This prevents the ends e1 and e2 of the film 11 from softening, and allows the thicknesses Te1 and Te2 of the ends e1 and e2 to be adjusted with high accuracy. In the portion forming the convex region R1, the temperature difference between both ends and the center of the original film 11f is preferably 3°C or more. This allows the thicknesses Te1 and Te2 of the ends e1 and e2 to be sufficiently small in a relatively short time without enlarging the equipment. In addition, the temperatures of both ends of the original film 11f may be different from each other, but are preferably approximately the same.
[0068] The temperatures of both ends and the center of the original film 11f are measured from below the direction of gravity using, for example, a thermal non-contact temperature sensor (MT150 manufactured by Raytec Corporation). The temperatures of both ends of the original film 11f are measured, for example, at positions overlapping near the center of the heating member 51, and the average value over a range of 50 mm in the width direction is used. The temperature of the center of the original film 11f is measured, for example, at a position midway between both ends, and the average value over 100 mm in the width direction is used.
[0069] The stretching ratio in the width direction is not particularly limited, but is preferably 5% or more, more preferably 10% or more, and even more preferably 15% or more. This allows the thicknesses Te1 and Te2 of the ends e1 and e2 to be effectively adjusted by heating the ends e1 and e2. In addition, the stretching ratio in the width direction is preferably 1000% or less. This allows stretching to be performed without enlarging the stretching equipment, making it possible to reduce equipment costs. The stretching ratio in the width direction can be adjusted by the distance between the clips of the clip tenter 50. The stretching ratio in the width direction can be evaluated by comparing the width of the film before and after stretching. The above-mentioned stretching ratio and temperature are examples, and are appropriately adjusted to obtain the desired orientation, physical properties, and surface state of the film 11. For stretching in the width direction, any method can be used, not limited to the clip tenter 50, but for example, a pin tenter or the like may be used.
[0070] The stretching ratio in the conveying direction is not particularly limited. Any method can be used for stretching in the conveying direction, and for example, a pantograph method, a draw method between rolls, a float method, or the like can be used.
[0071] The convex region R1 and the concave region R2 may be formed by using other methods. For example, the convex region R1 and the concave region R2 may be formed by controlling the amount of dope cast when casting. For example, the amount of dope cast may be adjusted by using a choke bar (also called a die bolt) or the like (see, for example, JP 2016-190344 A) to form the convex region R1 and the concave region R2. The amount of dope cast may be adjusted by independently controlling and supplying the dope for forming the central portion c and the ends e1 and e2 (see, for example, JP 2009-78371 A) to form the convex region R1 and the concave region R2. For example, when the thicknesses Te1 and Te2 of the ends e1 and e2 are to be increased, the flow rate of the dope for forming the ends e1 and e2 may be increased, and when the thicknesses Te1 and Te2 of the ends e1 and e2 are to be decreased, the flow rate of the dope for forming the ends e1 and e2 may be decreased.
[0072] Alternatively, the convex regions R1 and the concave regions R2 may be formed by controlling the presence or absence and size of an embossed portion (for example, embossed portion E in FIG. 4) (for example, see JP 2009-73154 A). The convex regions R1 and the concave regions R2 may be formed by combining a plurality of these methods.
[0073] For example, an optical film 11 having convex regions R1 and concave regions R2 can be produced in this manner. The optical film 11 is wound around a core 12 using a winding machine, for example, to form a film roll 1.
[0074] <Functions and Effects of Optical Films and Film Rolls> The optical film 11 of this embodiment has a convex region R1 (or convex position P1) where the thicknesses Te1, Te2 of the ends e1, e2 are smaller than the thickness Tc of the central portion c, and a concave region R2 (or concave position P2) where the thicknesses Te1, Te2 of the ends e1, e2 are larger than the thickness Tc of the central portion c, so that when forming the film roll 1, it becomes easy to control the amount of air between the optical films 11. Therefore, it becomes possible to suppress the occurrence of winding defects. The effect of this will be described in detail below.
[0075] 9A, 9B, and 9C each show the relationship between the position in the Y direction (longitudinal direction) of the optical film according to the comparative example and the difference ratio D. Each of these optical films according to the comparative examples has only one of the convex region R1 and the concave region R2. The optical film shown in FIG. 9A and the optical film shown in FIG. 9C have only the convex region R1, and the thickness of the end portion is smaller than the thickness of the central portion at all positions in the longitudinal direction (difference ratio D>0). The optical film shown in FIG. 9B has only the concave region R2, and the thickness of the end portion is larger than the thickness of the central portion at all positions in the longitudinal direction (difference ratio D<0). In such an optical film according to the comparative example, when forming a film roll, it is difficult to control the amount of air between the overlapping optical films, and winding defects are likely to occur.
[0076] For example, in the optical film shown in FIG. 9A and the optical film shown in FIG. 9C, the amount of air between the overlapping optical films is relatively small, and strong sticking is likely to occur in the thicker central portion. This sticking between the optical films may cause black bands in the film roll. In black bands, expansion and contraction occurs between the central portion where the sticking is strong and the end portions where the sticking is weak, causing deformation of the optical film. In addition, minute air particles caught between the films may grow as the film is wound up, forming dents (dents).
[0077] On the other hand, in the optical film shown in Fig. 9B, the amount of air between the overlapping optical films is relatively large, making it possible to suppress winding defects caused by sticking between the optical films. However, with this optical film, after the film roll is formed, the air between the optical films escapes over time, making it difficult to maintain the shape. There is a risk of the optical film being deformed due to this air escape.
[0078] Deterioration of the optical film caused by such poor winding also affects devices using the optical film, such as displays and touch sensors. For example, in displays, image visibility decreases, and in touch sensors, resistance fluctuates, reducing the sensor function.
[0079] In contrast to these comparative optical films, the optical film 11 of this embodiment has both the convex regions R1 and the concave regions R2, and therefore the amount of air between the overlapping optical films 11 can be controlled.
[0080] 10 shows an example of the configuration of the end face of the film roll 1. In the film roll 1, for example, convex regions R1 and concave regions R2 overlap each other alternately, which prevents the optical films 11 from sticking together and maintains their shape. That is, it is possible to prevent the occurrence of black bands and dents, and to prevent the optical films 11 from deforming over time.
[0081] As described above, in the optical film 11 and film roll 1 of this embodiment, the optical film 11 has a convex position P1 where the thicknesses Te1, Te2 of the ends e1, e2 are smaller than the thickness Tc of the central portion c, and a concave position P2 where the thicknesses Te1, Te2 of the ends e1, e2 are larger than the thickness Tc of the central portion c, so that it is easy to control the amount of air between the optical films 11 when forming the film roll 1. This makes it possible to prevent winding defects from occurring.
[0082] When such an optical film 11 is used in devices such as displays and touch sensors, the performance of the devices can be improved.
[0083] Furthermore, this optical film 11 can be made thinner because occurrence of winding defects is suppressed. Furthermore, a low-elasticity material can be suitably used for the optical film 11. In addition, even when a long optical film 11 is manufactured, a decrease in productivity can be suppressed. When the total winding length of the film roll 1 is 1000 m or more, preferably 4000 m or more, occurrence of winding defects can be more effectively suppressed.
[0084] <Modification> The film roll 1 may be formed by winding up a laminate of multiple films. This laminate may have, for example, an optical film 11 and a protective film (protective film 21 in FIG. 11 described below). Here, the optical film 11 corresponds to one specific example of the functional film of the present invention.
[0085] 11 shows an example of a cross-sectional configuration of a laminate of an optical film 11 and a protective film 21. The protective film 21 is for protecting the optical film 11, and is configured to be peelable from the optical film 11. The protective film 21 contains, for example, a polyester resin such as polyethylene terephthalate or polyethylene naphthalate, a polyethersulfone resin, a polysulfone resin, a polycarbonate resin, a polyamide resin, a polyimide resin, a polyolefin resin, a (meth)acrylic resin such as polymethyl methacrylate, a polyarylate resin, a polystyrene resin, a polyvinyl alcohol resin, an epoxy resin, or a mixture thereof.
[0086] For example, the film roll 1 is formed by laminating the protective film 21 on the optical film 11 and then winding up this laminate.
[0087] <Other Modifications> A transparent conductive film may be laminated on the optical film 11. Examples of materials used to form the transparent conductive film include metals such as Sn, In, Ti, Pb, Au, Pt, and Ag, and oxides thereof. Examples of the oxides include indium tin oxide (ITO), aluminum oxide, silicon oxide, titanium oxide, zinc oxide, and tungsten oxide. The transparent conductive film may be formed using aluminum nitride, silicon nitride, titanium nitride, cadmium sulfide, zinc sulfide, zinc selenide, or the like.
[0088] An adhesive layer and an anchor coat layer may be provided between the optical film 11 and the transparent conductive film. The adhesive layer may be made of, for example, an epoxy resin, a polyimide, a polybutadiene, a phenylene, or the like. The anchor coat layer can be formed by using a heat-resistant resin such as a nol resin and polyether ether ketone. The anchor coat layer can be formed by using an anchor coat agent containing an acrylic prepolymer such as epoxy diacrylate, urethane diacrylate, or polyester diacrylate, and curing it by a known curing method such as UV curing or heat curing.
[0089] An adhesive layer for the purpose of improving the smoothness of the film and the adhesion to the transparent conductive film may be provided between the optical film 11 and the transparent conductive film. This adhesive layer can be obtained, for example, by applying a resin varnish and removing the solvent by drying.
[0090] The laminate including the optical film 11 and the transparent conductive film may have a gas barrier layer on the side opposite to the transparent conductive film. The gas barrier layer may be formed of an inorganic material or an organic material. Usable inorganic materials include silicon oxide, aluminum oxide, indium oxide, etc., and usable organic materials include polyvinyl alcohol, ethylene-vinyl alcohol copolymer, polyamide, etc. Furthermore, a protective coating layer for protecting the gas barrier layer may be laminated on the gas barrier layer.
[0091] <Application Examples> The optical film 11 is used, for example, as a substrate for a color filter, a light guide plate, a protective film, a polarizing film, a retardation film, a touch panel, a transparent electrode substrate, a compact disc (CD), a mini disc (MD), a digital versatile disc (DVD), etc. The film can be suitably used as an optical recording substrate such as a disc (optical disk), a substrate for a thin film transistor (TFT), a liquid crystal display substrate, an organic electroluminescence (EL) display substrate, or an optical component such as a light transmission waveguide and an optical element sealant. In particular, the film can be suitably used as a member for a display element, specifically, a substrate for a color filter, a light guide plate, a protective film, a polarizing film, a retardation film, a touch sensor, a transparent electrode substrate, a substrate for a TFT, a liquid crystal display substrate, an organic EL display substrate, etc.
[0092] For example, a color filter can be obtained by laminating a color filter layer on a color filter substrate including the optical film 11. As the lamination method, a known pigment dispersion method, dyeing method, electrodeposition method, printing method, transfer method, etc. can be used. This color filter can be used as a color filter for a liquid crystal display device, and can also be used as a part of a color display, liquid crystal display device, etc.
[0093] The optical film 11 can be used not only for optical components, but also for electrical insulation components, electrical and electronic components, electronic component sealants, medical equipment, and packaging materials. In particular, the optical film 11 containing a cycloolefin resin is excellent in heat resistance and electrical properties, and has small dimensional changes even when subjected to high-temperature treatment or chemical treatment, making it ideal as an electrical insulation component. Examples of electrical insulation components include coating materials for electric wires and cables, insulating materials for office automation equipment such as computers, printers, and copiers, and insulating components for flexible printed circuit boards, and is particularly suitable for use as a flexible printed circuit board.
[0094] The optical film 11 can also be suitably used, for example, in a touch sensor (claim 12). A touch sensor is, for example, a device that is attached to the surface of a display device and converts physical contact with a user's finger, a touch pen, etc. into an electrical signal and outputs it. Examples of such display devices include liquid crystal display devices, plasma display devices, and EL display devices.
[0095] The touch sensor including the optical film 11 is, for example, a transparent electrode type touch sensor. In the transparent electrode type touch sensor, for example, the optical film 11 is coated with a metal oxide. By covering the metal film 11, a transparent electrode is formed, and the position is sensed by contacting the transparent electrode. The metal oxide may be, for example, indium tin oxide (ITO). The metal oxide is coated on the optical film 11 by, for example, vacuum deposition or sputtering.
[0096] The optical film 11 used in such a touch sensor preferably has high heat resistance. The heat resistance can be evaluated, for example, by the glass transition temperature, and the optical film 11 preferably has, for example, a high glass transition temperature equal to or higher than the sputtering temperature and high mechanical strength.
[0097] Furthermore, the optical film 11 used in the touch sensor preferably has transparency in the visible light region, and preferably has a light transmittance of, for example, 90% or more for visible light.
[0098] The optical film 11 containing a cycloolefin resin has a high glass transition temperature, high heat resistance, and high optical transparency to visible light, and therefore can be suitably used for a touch sensor. EXAMPLES
[0099] The effects of the present invention will be described using the following examples and comparative examples, although the technical scope of the present invention is not limited to the following examples.
[0100] <Example 1> First, a raw film was prepared as follows.
[0101] (Preparation of dope) PET resin (Toyobo Ester Film E7002, manufactured by Toyobo Co., Ltd.) 100 parts by weight Dichloromethane 200 parts by mass Ethanol 10 parts by weight First, the above components were charged into a sealed container, and the PET resin was dissolved under stirring to prepare a dope.
[0102] (Film forming) Next, the dope was uniformly cast (cast) on a stainless steel belt support at a temperature of 31°C and a width of 1800 mm using an endless belt casting apparatus to form a casting film. The temperature of the stainless steel belt was controlled at 28°C. Next, the solvent was evaporated on the stainless steel belt support until the amount of residual solvent in the casting film was 30%. Next, the casting film was peeled off from the stainless steel belt support at a peeling tension of 128 N / m, and then the casting film was stretched 1.15 times in the width direction under the condition of 160°C. The residual solvent at the start of the stretching was 5 mass%. Next, the casting film was dried while being conveyed by a number of rollers. Next, the parts of the casting film that were clamped by the tenter clips (both ends) were slit by a laser cutter, and then the casting film was wound up. As a result, a raw film having a thickness of 33 μm was produced.
[0103] Next, while holding both ends in the width direction of this raw film with clips, the raw film was stretched in the width direction using a clip tenter. At this time, both ends in the width direction of the raw film were heated in the stretching area (stretching area 50B in Figure 8) to form convex regions R1 and concave regions R2. An infrared irradiation member was used as the heating member. The heating member was positioned within a distance of 150 mm from the position where both ends in the width direction of the film roll were to be formed. The central part of the raw film was heated to 130°C and both ends to 160°C to form convex regions, and the raw film was heated to 130°C. The central portion and both ends of the film were both heated to 130° C. to form recessed regions. The stretching ratio in the width direction of both the raised region R1 and the recessed region R2 was 30%.
[0104] Using an in-line thickness gauge, the average thickness of the film prepared above, the difference ratio D of each of the convex region R1 and the concave region R2 where |D| is maximum, and the longitudinal size of each of the convex region R1 and the concave region R2 were measured. In addition, using an in-line thickness gauge and an encoder (length measuring device), the change in the difference ratio D of the inclined portion per 100 m of longitudinal size was measured (see Figures 5A and 5B). The average thickness of the prepared film was 25 μm, and the difference ratio D of each of the convex region and the concave region where |D| is maximum was 7.5% and -7.5%. The longitudinal size of the convex region R1 and the longitudinal size of the concave region R2 were the same, 250 m. The change in the difference ratio D per 100 m at the inclined portion was 7.5%. In addition, the glass transition temperature of this film was 80 ° C. Thereafter, the prepared film was wound around a core to prepare a film roll. The total length of the roll was 4000m.
[0105] <Example 2> First, a raw film was prepared as follows.
[0106] (Preparation of Rubber Particle Dispersion) A solution containing 10 parts by mass of rubber particles (Kane Ace (registered trademark) M210, average primary particle diameter R: 200 nm, manufactured by Kaneka Corporation) and 90 parts by mass of ME16 (a mixed solvent of methylene chloride and ethanol in a mass ratio of 84:16) was stirred and mixed with a dissolver for 50 minutes. After that, the solution was dispersed using a Milder disperser (manufactured by Pacific Machinery Works, Ltd.) under a condition of 1500 rpm to obtain a rubber particle dispersion.
[0107] (Preparation of Silica Particle Dispersion) 20 parts by mass of silica particles (Aerosil (registered trademark) R812, manufactured by Nippon Aerosil Co., Ltd., hydrophobic fumed silica, average primary particle diameter Rs1: 7 nm, specific surface area: 260 ± 30 m 2 A mixture of 80 parts by mass of 100 parts by mass of 100% ethanol (100% by mass / g) and 80 parts by mass of ME50 (a mixed solvent of methylene chloride and ethanol in a mass ratio of 50:50) was stirred and mixed in a dissolver for 50 minutes. After that, the mixture was dispersed in a Manton-Gaulin to obtain an additive solution.
[0108] Next, 10 parts by mass of the additive solution was slowly added to 90 parts by mass of ME16 that was being thoroughly stirred in a dissolution tank. The additive solution added to ME16 was then dispersed using an attritor. The dispersion was filtered using Finemet NF manufactured by Nippon Seisen Co., Ltd. to obtain a silica particle dispersion.
[0109] (Preparation of dope) Next, a dope having the following composition was prepared. First, 90 parts by mass of methylene chloride and 10 parts by mass of ethanol were added to a pressure dissolving tank. Next, 80 parts by mass of acrylic resin (MR1000, manufactured by Nippon Shokubai Co., Ltd., lactone acrylic resin) was added to the pressure dissolving tank while stirring. Next, the rubber particle dispersion liquid prepared above was added to the pressure dissolving tank, and then stirring was performed to dissolve the acrylic resin. This acrylic resin solution was filtered using SHP150 (manufactured by Roki Techno Co., Ltd.) to obtain a dope.
[0110] (Film forming) Next, the above dope was used to form a membrane. Specifically, the dope was uniformly cast on a stainless steel belt supporter at a temperature of 30°C and a width of 1800 mm using an endless belt casting apparatus to form a cast membrane. The temperature of the stainless steel belt was controlled at 28°C.
[0111] The solvent was evaporated on the stainless steel belt support until the residual solvent content in the cast film reached 30% by mass. Then, the cast film was peeled off from the stainless steel belt support at a peeling tension of 128 N / m. The residual solvent content of the cast film after peeling was 30% by mass.
[0112] Next, the cast film after peeling was stretched 50% in the width direction under the condition of 140°C in a tenter while being transported by many rollers. Next, the cast film was dried at 105°C while being transported by rolls. Next, the part of the cast film that was clamped by the tenter clips (both ends) was slit, and then the cast film was wound up. As a result, a raw film having a thickness of 33 μm was obtained.
[0113] Next, the raw film was stretched in the width direction using a clip tenter while holding both ends in the width direction of the raw film with clips. A film roll was produced in the same manner as the stretching of the raw film described in Example 1 above, except that the temperatures of the center and both ends of the raw film were changed. Specifically, the center of the raw film was heated to 140°C and both ends were heated to 170°C to form a convex region, and both the center and both ends of the raw film were heated to 140°C to form a concave region. The stretch ratio in the width direction was 30% for both the convex region R1 and the concave region R2.
[0114] <Example 3> First, a raw film was prepared as follows.
[0115] (Preparation of Microparticle Dispersion) 11.3 parts by mass of fine particles (Aerosil (registered trademark) R812, manufactured by Nippon Aerosil Co., Ltd.) and 84 parts by mass of ethanol were mixed and stirred for 50 minutes using a dissolver, and then the mixture was dispersed using a Manton-Gaulin mixer to obtain a fine particle dispersion.
[0116] Five parts by mass of the microparticle dispersion liquid was slowly added to methylene chloride (100 parts by mass) that was being thoroughly stirred in a dissolution tank. The microparticle dispersion liquid added to the methylene chloride was then dispersed in an attritor so that the secondary particles had a predetermined particle size. The resulting solution was filtered through Finemet NF manufactured by Nippon Seisen Co., Ltd. to prepare a microparticle-added liquid.
[0117] (Preparation of dope) A dope having the following composition was prepared. First, 200 parts by mass of dichloromethane and 10 parts by mass of ethanol were added to a pressurized dissolution tank. Next, 100 parts by mass of cycloolefin resin (ARTON (registered trademark) F4520, manufactured by JSR Corporation), 5 parts by mass of ultraviolet absorber (Tinuvin (registered trademark) 477, manufactured by BASF Japan Ltd.), and 3 parts by mass of the above-mentioned fine particle additive solution were added to the pressurized dissolution tank containing the mixed solution of dichloromethane and ethanol while stirring. Next, the mixture was heated and the cycloolefin resin was dissolved while stirring. Next, the cycloolefin resin solution was filtered using Azumi filter paper No. 244 manufactured by Azumi Filter Paper Co., Ltd. to prepare a dope.
[0118] Incidentally, ARTON (registered trademark) F4520 is a polymer having a structural unit of the following structure.
[0119] [ka]
[0120] (Film forming) Next, the dope was uniformly cast on a stainless steel belt support at a temperature of 31°C and a width of 1800 mm using an endless belt casting apparatus to form a cast film. The temperature of the stainless steel belt was controlled at 28°C. Next, the solvent was evaporated on the stainless steel belt support until the residual solvent amount in the cast film was 30% by mass. Next, the cast film was peeled off from the stainless steel belt support at a peeling tension of 128 N / m. Next, the peeled cast film was stretched 1.15 times in the width direction under the condition of 160°C. The residual solvent amount in the cast film at the start of stretching was 5% by mass. Next, the cast film was dried while being conveyed by a number of rollers. Next, the parts of the cast film that were clamped by the tenter clips (both ends) were slit by a laser cutter, and then the cast film was wound up. As a result, a raw film having a thickness of 33 μm was obtained.
[0121] Next, the raw film was stretched in the width direction using a clip tenter while holding both ends in the width direction of the raw film with clips. A film roll was produced in the same manner as the stretching of the raw film described in Example 1 above, except that the temperatures of the center and both ends of the raw film were changed. Specifically, the center of the raw film was heated to 180°C and both ends were heated to 210°C to form a convex region, and both the center and both ends of the raw film were heated to 180°C to form a concave region. The stretch ratio in the width direction was 30% for both the convex region R1 and the concave region R2.
[0122] <Example 4> A film roll was produced in the same manner as in the production of the film roll of Example 3, except that the temperatures of the center and both ends of the original film when stretching the original film in the width direction were changed. Specifically, the center of the original film was heated to 180°C and both ends to 200°C to form a convex region, and the center of the original film was heated to 180°C and both ends to 190°C to form a concave region. As a result, the maximum values of |D| in the convex region R1 and the concave region R2 were changed from those of the film roll of Example 3.
[0123] <Example 5> A film roll was produced in the same manner as in the production of the film roll of Example 3, except that the temperature increase and decrease rates at both ends of the original film were changed. Specifically, the temperature increase and decrease rates at both ends of the original film were slowed down by 2.1 times compared to Example 3. As a result, the change in the difference ratio D per 100 m at the inclined portion was changed from that of the film roll of Example 3.
[0124] <Example 6> A film roll was produced in the same manner as in Example 4, except that the temperature increase and decrease rates at both ends of the raw film were changed. Specifically, compared to Example 4, the temperature increase and decrease rates at both ends of the raw film were changed to 2. As a result, the amount of change in the difference ratio D per 100 m in the inclined portion was changed from that of the film roll in Example 4.
[0125] <Example 7> A film roll was produced in the same manner as in Example 6 above, except that the total wound length was changed.
[0126] <Example 8> A film roll was produced in the same manner as in the production of the film roll of Example 4, except that the period of temperature change at both ends of the original film was changed. Specifically, the period of temperature change of the heating member was made shorter than that in the production of the film roll of Example 4. As a result, the longitudinal sizes of the convex regions R1 and the concave regions R2 were changed from those of the film roll of Example 4.
[0127] <Example 9> A film roll was produced in the same manner as in the production of the film roll of Example 6, except that the method of forming the convex regions R1 and the concave regions R2 was changed. Specifically, a plurality of heat bolts were arranged in the width direction of the casting die, and the value of the voltage applied to the heat bolts was changed according to the position in the width direction. As a result, the dope casting amount at both ends of the casting die and the dope casting amount at the center of the casting die were adjusted, respectively, to form the convex regions R1 and the concave regions R2. Specifically, the casting gap at both ends in the width direction was changed between -2.5% and 2.5% with respect to the casting gap at the center in the width direction.
[0128] <Example 10> A film roll was produced in the same manner as in the production of the film roll of Example 6, except that the method of forming the convex regions R1 and the concave regions R2 was changed. Specifically, the temperature of the embossing ring was changed from 180°C to 200°C under a constant pressure. This adjusted the height of the embossed portions, and formed the convex regions R1 and the concave regions R2.
[0129] <Example 11> In the preparation of the film roll of Example 1, the temperatures of the center and both ends of the original film when stretching the original film in the width direction, and the temperature increase and decrease rates of the temperature of both ends of the original film were changed. Except for this, the film roll was prepared in the same manner as in Example 1. As a result, the maximum values of |D| in the convex region R1 and the concave region R2, and the change in the difference ratio D per 100 m in the inclined portion were changed from those of the film roll of Example 1.
[0130] <Example 12> A film roll was produced in the same manner as in Example 6, except that the temperatures at both ends of the original film were changed nonlinearly, causing the difference ratio D to change sinusoidally along the longitudinal direction.
[0131] <Example 13> A film roll was produced in the same manner as in Example 6 above, except that the total wound length was changed.
[0132] <Example 14> A film roll was produced in the same manner as in Example 6 above, except that the total wound length was changed.
[0133] <Example 15> A film roll was produced in the same manner as in the production of the film roll of Example 4, except that the temperature change period of both ends of the original film was changed. Specifically, the temperature change period of the heating member was made longer than that in the production of the film roll of Example 4. As a result, the longitudinal sizes of the convex regions R1 and the concave regions R2 were changed from those of the film roll of Example 4.
[0134] <Comparative Example 1> A film roll was produced in the same manner as in the production of the film roll of Example 3, except that the temperatures of the center and both ends of the original film when stretching the original film in the width direction were changed. Specifically, the original film was stretched in the width direction while maintaining the center of the original film at 180°C and both ends at 210°C. As a result, only convex regions were formed in the film roll.
[0135] <Comparative Example 2> A film roll was produced in the same manner as in the production of the film roll of Example 3, except that the temperatures of the center and both ends of the original film when stretching the original film in the width direction were changed. Specifically, the original film was stretched in the width direction while maintaining the center of the original film at 180°C and both ends at 190°C. As a result, only concave regions were formed in the film roll.
[0136] <Comparative Example 3> A film roll was produced in the same manner as in the production of the film roll of Comparative Example 1, except that the temperatures of the center and both ends of the original film when stretching the original film in the width direction were changed. Specifically, the center of the original film was heated to 180°C and both ends to 210°C to form a first convex region, and the center of the original film was heated to 180°C and both ends to 200°C to form a second convex region. This resulted in the formation of two convex regions (first convex region and second convex region) having different values of the difference ratio D.
[0137] The properties of the film rolls thus produced according to Examples 1 to 15 and Comparative Examples 1 to 3 are summarized in Table 1 below.
[0138] <Film roll evaluation> (Black Band Rating) Immediately after the film roll was produced, the color of the film surface was observed by visually observing the film roll surface in the direction of the core under white fluorescent light. The observation was performed over the entire width of the film roll, covering one revolution of the film roll. At this time, the presence or absence of a part where the color of the core was visible and the color looked different from the surroundings was confirmed. A specified limit sample was used for this color confirmation. If there was a part where the color looked different, the presence or absence of deformation of the film was confirmed for this part. Specifically, the film was placed on a table set approximately horizontally to black rag paper, and the presence or absence of deformation of the film was confirmed by the reflected light of the light irradiated to the film. The light was irradiated to the film using a fluorescent lamp of 2500 lux or more, and the fluorescent lamp was placed within 2 m from the film. In this way, the black band of the film roll was evaluated according to the following evaluation criteria. The results are shown in Table 1 below; Evaluation Criteria A: There are no areas on the film roll that look different in color. B: There are some areas on the film roll that appear to be different colors, but no deformation of the film is observed. C: Deformation of the film was observed.
[0139] (Evaluation of changes over time) Immediately after the film roll was produced, the surface of the black core was visually observed from the outside to confirm whether or not there were any areas that looked different in color. Next, the film roll was left for 500 hours under conditions of 23°C and 90% RH, and the surface of the black core was visually observed from the outside again to confirm whether or not there were any areas that looked different in color. If there were any areas that looked different in color immediately after the film roll was produced and after 500 hours had passed, the presence or absence of film deformation in these areas was confirmed. In this way, the change over time of the film roll was evaluated according to the following evaluation criteria. The results are shown in Table 1 below; Evaluation Criteria A: Even after 500 hours, there are no more areas of the film roll that look different in color. B: After 500 hours, there are more and more areas of the film roll that look different in color, but no deformation of the film is observed in these areas. C: After 500 hours, new deformation of the film was observed.
[0140] [Table 1]
[0141] The film and film roll according to the present invention have convex positions (or convex regions) where the thickness of the ends in the width direction is smaller than the thickness of the center, and concave positions (or concave regions) where the thickness of the ends is larger than the thickness of the center. From the results in Table 1, it was confirmed that the films according to the examples of the present invention are superior in terms of black bands and changes over time, and suppress the occurrence of winding defects, compared to films having only either convex positions or concave positions.
[0142] This application is based on a Japanese patent application (Patent Application No. 2020-116621) filed on July 6, 2020, the disclosure of which is hereby incorporated by reference in its entirety.
Claims
1. a first end portion and a second end portion in a width direction intersecting with the longitudinal direction; a central portion between the first end and the second end; a convex position in which a thickness Te1 of at least the first end of the first end and the second end is smaller than a thickness Tc of the central portion; a concave position that is disposed at a position different from the convex position in the longitudinal direction, and a thickness Te1 of the first end portion is greater than a thickness Tc of the central portion; A film comprising:
2. At the convex position, the thickness Te2 of the second end portion is smaller than the thickness Tc of the central portion, The film of claim 1 , wherein at the concave position, the thickness Te2 of the second end is greater than the thickness Tc of the central portion.
3. a convex region in which the convex position is provided and a thickness Te1 of at least the first end of the first end and the second end is smaller than a thickness Tc of the central portion; The film of claim 1 or 2, further comprising a recessed region in which the recessed position is provided and the thickness Te1 of the first end is greater than the thickness Tc of the central portion.
4. The film of claim 3 having a plurality of alternating raised and recessed regions along the longitudinal direction.
5. 5. The film according to claim 3, wherein the length of the convex regions and the concave regions in the longitudinal direction is from 100 m to 500 m.
6. a difference between a thickness Te1 of the first end portion at the convex position and a thickness Tc of the central portion is 10% or less of an average thickness of the film at the convex position; The film according to any one of claims 1 to 5, wherein the difference between the thickness Te1 of the first end portion at the concave position and the thickness Tc of the central portion is 10% or less of the average thickness of the film at the concave position.
7. a difference between a thickness Te1 of the first end portion at the convex position and a thickness Tc of the central portion is 5% or less of an average thickness of the film at the convex position; The film according to any one of claims 1 to 6, wherein the difference between the thickness Te1 of the first end portion at the concave position and the thickness Tc of the central portion is 5% or less of the average thickness of the film at the concave position.
8. The film according to any one of claims 1 to 7, further comprising an inclined portion between the convex position and the concave position, in which at least one of the thickness Te1 of the first end portion and the thickness Tc of the central portion changes continuously.
9. The film of claim 8 , wherein the longitudinal extent of the inclined portion is 5 m or more.
10. The film according to any one of claims 1 to 9, comprising an alicyclic structure-containing polymer.
11. The film according to any one of claims 1 to 10, which has an optical function.
12. The film according to any one of claims 1 to 11, which is used in a touch sensor.
13. A film according to any one of claims 1 to 12, A laminate having a protective film laminated on the film.
14. A core; The film according to any one of claims 1 to 12 or the laminate according to claim 13 wound around the core; A film roll comprising:
15. Providing or forming a web of film; forming a convex position and a concave position at different positions in a longitudinal direction of the raw film; Including, The convex position is formed by making a thickness Te1 of at least the first end of the first end and a second end of the original film in a width direction intersecting the longitudinal direction smaller than a thickness Tc of a central portion between the first end and the second end, The method for manufacturing a film, wherein the recessed position is formed by making a thickness Te1 of the first end portion greater than a thickness Tc of the central portion.
16. In forming the convex portion and the concave portion, at least the first end portion of the first end portion and the second end portion is heated while the raw film is stretched in the width direction; The method for manufacturing a film according to claim 15 , wherein the temperature difference between the first end and the central portion when the convex position is formed is made larger than the temperature difference between the first end and the central portion when the concave position is formed.
Citation Information
Patent Citations
Method for manufacturing film having uneven structure and method for measuring film having uneven structure
JP2016144896A
Manufacturing method of film roll
JP2017100372A
Film roll and manufacturing method thereof
JP2017202644A
Method for producing optical film
WO2012108208A1
Stretched cellulose ester film and method for producing same
WO2012153612A1