Composition and elastomer
A composition of block copolymers with defined molecular weights and a specific wax formulation addresses moldability, film thickness uniformity, and ozone crack resistance issues in elastic bodies for sanitary products, enhancing their performance and properties.
Patent Information
- Application Number
- JP2023098442
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-08-28
- Filing Date
- 2023-06-15
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2039-08-28
AI Technical Summary
Existing compositions for elastic bodies used in sanitary products, such as disposable diapers, face challenges in achieving excellent moldability, uniform film thickness, low permanent elongation, and ozone crack resistance while maintaining low odor and desirable hue.
A composition comprising a specific combination of block copolymers with asymmetric and symmetrical structures, along with a wax containing linear and branched hydrocarbons, is developed. The block copolymers have defined weight average molecular weights and monomer unit contents, and the wax is added in a specific ratio to enhance moldability, film thickness uniformity, and ozone crack resistance.
The composition achieves an elastic body with excellent moldability, minimal film thickness variation, low permanent elongation, and improved ozone crack resistance, along with reduced odor and better color, making it suitable for sanitary materials.
Smart Images

Figure 0007552801000001 
Figure 0007552801000002 
Figure 0007552801000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a composition containing a block copolymer having an aromatic vinyl polymer block and a conjugated diene polymer block, and more specifically to a composition which can give an elastomer having excellent moldability, little film thickness variation, and small permanent elongation, and an elastomer obtained from said composition. [Background technology]
[0002] Among thermoplastic elastomers, aromatic vinyl-conjugated diene-aromatic vinyl block copolymers are particularly elastic and flexible, and one of their representative applications is as a material for stretchable films used in sanitary products such as disposable diapers and sanitary napkins.
[0003] Sanitary products such as paper diapers and sanitary napkins are required to have the ability to follow the wearer's movements and to fit well, and therefore elastic films are used in various parts. For example, sanitary products such as pants-type diapers, which are a type of paper diaper, need not slip even if the wearer moves vigorously or wears them for a long time, so the elastic films used are required to have both a high elastic modulus and a small permanent elongation.
[0004] Patent Document 1 proposes a block copolymer composition which, after being formed into a film, has both a high elastic modulus and a small permanent elongation at a high level and can be molded with good moldability. The block copolymer composition contains 25 to 150 parts by weight of an aromatic vinyl polymer and 0.2 to 10 parts by weight of a fatty acid amide relative to 100 parts by weight of a block copolymer having at least one aromatic vinyl polymer block and at least one conjugated diene polymer block. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2016-69565 A Summary of the Invention [Problem to be solved by the invention]
[0006] A first object of the present invention is to provide a composition which is capable of giving an elastic body which has excellent moldability, little film thickness variation, and small permanent set. A second object of the present invention is to provide a composition which is excellent in hue and low odor and which can give an elastomer having excellent ozone cracking resistance. [Means for solving the problem]
[0007] Means for Solving the Problems The present inventors have conducted intensive research in order to achieve the first object, and have found that by using a combination of three types of block copolymers having different structures and by appropriately adjusting the weight-average molecular weights of some of the blocks constituting each block copolymer and the content of aromatic vinyl monomer units in each block copolymer, a composition having excellent moldability can be obtained and an elastomer having little film thickness variation and small permanent set can be obtained, thereby completing the present invention.
[0008] That is, according to the present invention, General formula (A): Ar1 a -D a -Ar2 a (In the formula, Ar1 a is an aromatic vinyl polymer block having a weight average molecular weight of 5,000 to 20,000; D a is a conjugated diene polymer block, Ar2 a represents an aromatic vinyl polymer block having a weight average molecular weight of more than 20,000 to 400,000), General formula (B): Ar1 b -D b -Ar2 b (In the formula, Ar1 b and Ar2 bare aromatic vinyl polymer blocks having a weight average molecular weight of 5,000 to 20,000, respectively, D b represents a conjugated diene polymer block), and General formula (C):(Ar c -D c ) n -X (In the formula, Ar c is an aromatic vinyl polymer block, D c represents a conjugated diene polymer block, n is an integer of 2 or more, and X represents a residue of a coupling agent, the content of aromatic vinyl monomer units in the block copolymer A is 40 to 50% by weight based on the total monomer units constituting the block copolymer A; the content of aromatic vinyl monomer units in the block copolymer B is 20 to 30% by weight based on the total monomer units constituting the block copolymer B; The content of aromatic vinyl monomer units in the block copolymer C is less than 20% by weight based on the total monomer units constituting the block copolymer C. A composition (hereinafter sometimes referred to as a "first composition") is provided.
[0009] In the first composition of the present invention, the conjugated diene polymer block (D a ) has a vinyl bond content of 1 to 20 mol %, and the conjugated diene polymer block (D a ) preferably has a weight average molecular weight of 40,000 to 400,000. In the first composition of the present invention, the conjugated diene polymer block (D b ) has a vinyl bond content of 1 to 20 mol %, and the conjugated diene polymer block (D b ) preferably has a weight average molecular weight of 40,000 to 400,000. In the first composition of the present invention, it is preferable that the block copolymer A and the block copolymer B are obtained by a production method in which an aromatic vinyl monomer, a conjugated diene monomer, and then an aromatic vinyl monomer are sequentially polymerized in this order to form a polymer block. In the first composition of the present invention, n in general formula (C) is preferably an integer of 2 to 4. In the first composition of the present invention, the conjugated diene polymer block (D c ) has a vinyl bond content of 1 to 20 mol %, and the conjugated diene polymer block (D c ) preferably has a weight average molecular weight of 20,000 to 200,000. In the first composition of the present invention, it is preferable that the block copolymer C is obtained by a production method including polymerizing an aromatic vinyl monomer and a conjugated diene monomer to form a diblock chain, and reacting the diblock chain with a coupling agent to perform coupling. The first composition of the present invention is a compound represented by the general formula (D): Ar d -D d (In the formula, Ar d is an aromatic vinyl polymer block, D d represents a conjugated diene polymer block), and the content of aromatic vinyl monomer units in the block copolymer D is preferably less than 20% by weight based on the total monomer units constituting the block copolymer D. It is preferable that the first composition of the present invention further contains a wax, the wax contains linear hydrocarbons and branched hydrocarbons, the weight ratio (n-form) of the linear hydrocarbons (n-form) to the branched hydrocarbons (iso-form) (n-form / iso-form) is 30 / 70 to 99 / 1, the melting point of the wax is less than 80°C, and the content of the wax in the composition is 0.1 to 5 parts by weight based on 100 parts by weight of the total of the block copolymers in the composition.
[0010] Furthermore, as a result of extensive research conducted by the inventors in order to achieve the second object, they discovered that by adding a wax having a relatively low melting point that contains linear hydrocarbons and branched hydrocarbons in a specific weight ratio to a block copolymer, a composition excellent in hue and low odor can be obtained, and an elastomer excellent in ozone crack resistance can be obtained, thereby completing the present invention.
[0011] The present invention also provides a composition containing a block copolymer having at least one aromatic vinyl polymer block and at least one conjugated diene polymer block, and a wax, wherein the wax contains linear hydrocarbons and branched hydrocarbons, the weight ratio (n-form) of the linear hydrocarbons (n-form) to the branched hydrocarbons (iso-form) (n-form / iso-form) is 30 / 70 to 99 / 1, the melting point of the wax is less than 80°C, and the content of the wax in the composition is 0.1 to 5 parts by weight per 100 parts by weight of the block copolymer (hereinafter sometimes referred to as a "second composition").
[0012] The present invention also provides an elastomer obtained from the above first and second compositions.
[0013] The elastic body is preferably an elastic body for sanitary materials. The elastic body or the elastic body for sanitary materials is preferably a film or a thread. Effect of the Invention
[0014] According to the present invention, it is possible to provide a first composition which is capable of producing an elastic body which has excellent moldability, little film thickness variation, and small permanent set. Furthermore, according to the present invention, a second composition can be provided that is excellent in hue and low odor and is capable of producing an elastomer that is excellent in ozone crack resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The first composition of the present invention contains a block copolymer A, a block copolymer B and a block copolymer C.
[0016] (Block Copolymer A) The block copolymer A is a copolymer represented by the following general formula (A). General formula (A): Ar1 a -D a -Ar2a (In the formula, Ar1 a is an aromatic vinyl polymer block having a weight average molecular weight of 5,000 to 20,000; D a is a conjugated diene polymer block, Ar2 a represents an aromatic vinyl polymer block having a weight average molecular weight of more than 20,000 to 400,000.
[0017] Aromatic vinyl polymer block (Ar1 a ) and aromatic vinyl polymer block (Ar2 a ) is a polymer block composed mainly of repeating units which are aromatic vinyl monomer units obtained by polymerizing aromatic vinyl monomers.
[0018] Aromatic vinyl polymer block (Ar1 a ) and aromatic vinyl polymer block (Ar2 a The aromatic vinyl monomer used to constitute the aromatic vinyl monomer unit of (1) is not particularly limited as long as it is an aromatic vinyl compound, and examples thereof include styrene, α-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2-ethylstyrene, 3-ethylstyrene, 4-ethylstyrene, 2,4-diisopropylstyrene, 2,4-dimethylstyrene, 4-t-butylstyrene, 5-t-butyl-2-methylstyrene, 2-chlorostyrene, 3-chlorostyrene, 4-chlorostyrene, 4-bromostyrene, 2-methyl-4,6-dichlorostyrene, 2,4-dibromostyrene, and vinylnaphthalene. Among these, it is preferable to use styrene. These aromatic vinyl monomers can be used alone or in combination of two or more. In addition, the two aromatic vinyl polymer blocks may be constituted by the same aromatic vinyl monomer unit, or may be constituted by different aromatic vinyl monomer units.
[0019] In addition, the aromatic vinyl polymer block (Ar1 a ) and aromatic vinyl polymer block (Ar2 aThe aromatic vinyl polymer block (Ar1) may contain other monomer units as long as the aromatic vinyl monomer unit is the main repeating unit. a ) and aromatic vinyl polymer block (Ar2 a Examples of monomers constituting monomer units other than aromatic vinyl monomer units that may be contained in the aromatic vinyl polymer block (Ar1) include conjugated diene monomers such as 1,3-butadiene and isoprene (2-methyl-1,3-butadiene), α,β-unsaturated nitrile monomers, unsaturated carboxylic acid or acid anhydride monomers, unsaturated carboxylic acid ester monomers, and non-conjugated diene monomers. a ) and aromatic vinyl polymer block (Ar2 a The content of monomer units other than aromatic vinyl monomer units in the aromatic vinyl polymer block (Ar1) is preferably 20% by weight or less, more preferably 10% by weight or less, and particularly preferably substantially 0% by weight. a ) and aromatic vinyl polymer block (Ar2 a ) is preferably substantially composed of one or more aromatic vinyl monomer units, and particularly preferably composed of styrene units.
[0020] In the block copolymer A, the aromatic vinyl polymer block (Ar1 a ) and aromatic vinyl polymer block (Ar2 a ) has a weight average molecular weight different from that of the block copolymer A. Since the first composition of the present invention contains such an asymmetric block copolymer A, it is possible to obtain an elastic body having excellent moldability, little film thickness variation, and small permanent elongation.
[0021] Aromatic vinyl polymer block (Ar1 a The weight average molecular weight of the copolymer is 5,000 to 20,000, more preferably 6,000 to 18,000, and further preferably 7,000 to 16,000.
[0022] Aromatic vinyl polymer block (Ar2 aThe weight average molecular weight of the copolymer is more than 20,000 and not more than 400,000, more preferably 25,000 to 300,000, and even more preferably 30,000 to 200,000.
[0023] Conjugated diene polymer block (D a ) is a polymer block composed mainly of repeating units of conjugated diene monomer units obtained by polymerizing a conjugated diene monomer.
[0024] Conjugated diene polymer block (D a The conjugated diene monomer used to constitute the conjugated diene monomer unit of the conjugated diene polymer block (D) is not particularly limited as long as it is a conjugated diene compound, and examples thereof include 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 2-chloro-1,3-butadiene, 1,3-pentadiene, 1,3-hexadiene, myrcene, and farnesene. Among these, it is preferable to use 1,3-butadiene and / or isoprene, and it is particularly preferable to use isoprene. These conjugated diene monomers can be used alone or in combination of two or more kinds. Furthermore, the conjugated diene polymer block (D a ) may be subjected to a hydrogenation reaction on some of the unsaturated bonds.
[0025] Also, the conjugated diene polymer block (D a The conjugated diene polymer block (D) may contain other monomer units as long as the conjugated diene monomer unit is the main repeating unit. a Examples of monomers constituting monomer units other than the conjugated diene monomer units that may be contained in the conjugated diene polymer block (D) include aromatic vinyl monomers such as styrene and α-methylstyrene, α,β-unsaturated nitrile monomers, unsaturated carboxylic acid or acid anhydride monomers, unsaturated carboxylic acid ester monomers, and non-conjugated diene monomers. aThe content of monomer units other than the conjugated diene monomer units in the conjugated diene polymer block (D) is preferably 20% by weight or less, more preferably 10% by weight or less, and particularly preferably substantially 0% by weight. a ) is preferably substantially composed of one or more conjugated diene monomer units, and particularly preferably composed of isoprene units.
[0026] Conjugated diene polymer block (D a ) vinyl bond content (conjugated diene polymer block (D a The proportion of 1,2-vinyl bond units and 3,4-vinyl bond units in all conjugated diene monomer units in the copolymer (a) is not particularly limited, but is preferably 1 to 20 mol %, more preferably 2 to 15 mol %, and particularly preferably 3 to 10 mol %. If the vinyl bond content is too high, the flexibility of the resulting elastomer tends to be impaired.
[0027] Conjugated diene polymer block (D a The weight average molecular weight of the copolymer is preferably 40,000 to 400,000, more preferably 45,000 to 350,000, and even more preferably 50,000 to 300,000.
[0028] The weight average molecular weight of block copolymer A (that is, the weight average molecular weight of the entire block copolymer A) is preferably 65,000 to 800,000, more preferably 70,000 to 700,000, and further preferably 75,000 to 650,000.
[0029] In the present invention, the weight average molecular weight of each polymer block and the weight average molecular weight of the entire block polymer are determined as polystyrene-equivalent values measured by high performance liquid chromatography.
[0030] The weight average molecular weight of each polymer block and the weight average molecular weight of the entire block polymer can be adjusted by adjusting the amount of each monomer used to form each polymer block and the amount of polymerization initiator used when obtaining a block copolymer by polymerization reaction.
[0031] The content of aromatic vinyl monomer units in block copolymer A is 40 to 50% by weight based on the total monomer units constituting block copolymer A. Since the first composition of the present invention contains an asymmetric block copolymer A containing aromatic vinyl monomer units in the above content, it is possible to obtain an elastic body having excellent moldability, little film thickness variation, and small permanent elongation.
[0032] The block copolymer A is preferably obtained by a manufacturing method in which an aromatic vinyl monomer, a conjugated diene monomer, and then an aromatic vinyl monomer are sequentially polymerized in this order to form a polymer block. Therefore, the block copolymer A is preferably free of a residue of a coupling agent. The details of such a manufacturing method will be described later.
[0033] (Block copolymer B) The block copolymer B is a copolymer represented by the following general formula (B). General formula (B): Ar1 b -D b -Ar2 b (In the formula, Ar1 b and Ar2 b are aromatic vinyl polymer blocks having a weight average molecular weight of 5,000 to 20,000, respectively, D b represents a conjugated diene polymer block)
[0034] Aromatic vinyl polymer block (Ar1 b ) and aromatic vinyl polymer block (Ar2 b ) is a polymer block composed mainly of repeating units which are aromatic vinyl monomer units obtained by polymerizing aromatic vinyl monomers.
[0035] Aromatic vinyl polymer block (Ar1 b ) and aromatic vinyl polymer block (Ar2 b The aromatic vinyl monomer used to constitute the aromatic vinyl monomer unit of the aromatic vinyl polymer block (Ar1) is not particularly limited as long as it is an aromatic vinyl compound. For example, a ) and aromatic vinyl polymer block (Ar2 a ) are similar to those mentioned above.
[0036] Aromatic vinyl polymer block (Ar1 b ) and aromatic vinyl polymer block (Ar2 b As long as the aromatic vinyl monomer unit is the main repeating unit, it may contain other monomer units. Examples of monomers constituting monomer units other than aromatic vinyl monomer units include aromatic vinyl polymer blocks (Ar1 a ) and aromatic vinyl polymer block (Ar2 a The aromatic vinyl polymer block (Ar1) may be the same as the aromatic vinyl polymer block (Ar1), and the content of the aromatic vinyl polymer block (Ar1) may be the same as the aromatic vinyl polymer block (Ar1). b ) and aromatic vinyl polymer block (Ar2 b ) is also preferably composed substantially of one or more aromatic vinyl monomer units, and particularly preferably composed of styrene units.
[0037] In the block copolymer B, the aromatic vinyl polymer block (Ar1 b ) and aromatic vinyl polymer block (Ar2 b ) each have a weight average molecular weight in the range of 5,000 to 20,000. Since the first composition of the present invention contains such a symmetric block copolymer B, it is possible to obtain an elastic body having excellent moldability, little film thickness variation, and small permanent elongation.
[0038] Aromatic vinyl polymer block (Ar1 b ) and aromatic vinyl polymer block (Ar2 bThe weight average molecular weight of the copolymer is 5,000 to 20,000, more preferably 6,000 to 18,000, and further preferably 7,000 to 16,000.
[0039] Aromatic vinyl polymer block (Ar1 b ) and aromatic vinyl polymer block (Ar2 b The weight average molecular weights of the aromatic vinyl polymer block (Ar1) may be equal to or different from each other as long as they are within the above range, but it is preferable that they are substantially equal to each other. b ) and aromatic vinyl polymer block (Ar2 b The weight average molecular weight of the aromatic vinyl polymer block (Ar1) of the block copolymer A is relatively small. a ) is preferably substantially equal to the weight average molecular weight of
[0040] Conjugated diene polymer block (D b ) is a polymer block composed mainly of repeating units of conjugated diene monomer units obtained by polymerizing a conjugated diene monomer.
[0041] Conjugated diene polymer block (D b The conjugated diene monomer used to constitute the conjugated diene monomer unit of the conjugated diene polymer block (D a ) are similar to those mentioned above.
[0042] Also, the conjugated diene polymer block (D b ) may contain other monomer units as long as the conjugated diene monomer unit is the main repeating unit. Examples of the monomer constituting the monomer units other than the conjugated diene monomer unit include a conjugated diene polymer block (D a The conjugated diene polymer block (D b) is also preferably composed substantially of one or more conjugated diene monomer units, and particularly preferably composed of isoprene units.
[0043] Conjugated diene polymer block (D b The vinyl bond content of the conjugated diene polymer block (D a ) is preferably substantially equal to the vinyl bond content of
[0044] Conjugated diene polymer block (D b The weight average molecular weight of the copolymer is preferably 40,000 to 400,000, more preferably 45,000 to 350,000, and even more preferably 50,000 to 300,000.
[0045] Conjugated diene polymer block (D b The weight average molecular weight of the conjugated diene polymer block (D a ) is preferably substantially equal to the weight average molecular weight of
[0046] The weight average molecular weight of block copolymer B (that is, the weight average molecular weight of the entire block copolymer B) is preferably 65,000 to 800,000, more preferably 70,000 to 700,000, and further preferably 75,000 to 600,000.
[0047] The content of aromatic vinyl monomer units in block copolymer B is 20 to 30% by weight based on the total monomer units constituting block copolymer B. Since the first composition of the present invention contains a symmetric block copolymer B containing aromatic vinyl monomer units in the above content, it is possible to obtain an elastic body having excellent moldability, little film thickness variation, and small permanent elongation.
[0048] The block copolymer B is preferably obtained by a manufacturing method in which an aromatic vinyl monomer, a conjugated diene monomer, and then an aromatic vinyl monomer are sequentially polymerized in this order to form a polymer block. Therefore, the block copolymer B preferably does not contain a residue of a coupling agent. The details of such a manufacturing method will be described later.
[0049] (Block Copolymer C) The block copolymer C is a copolymer represented by the following general formula (C). General formula (C):(Ar c -D c ) n -X (In the formula, Ar c is an aromatic vinyl polymer block, D c represents a conjugated diene polymer block, n is an integer of 2 or more, and X represents a residue of a coupling agent.
[0050] The block copolymer C is a diblock copolymer having n units (Ar c -D c ) are bonded to each other. In the general formula (C), n represents the number of branches in the block copolymer C. The block copolymer C may be a mixture of two or more kinds of block copolymers in which diblock bodies are bonded in different numbers. n is an integer of 2 or more, preferably an integer of 2 to 8, and more preferably an integer of 2 to 4. The residue of the coupling agent (X) is not particularly limited as long as it is a residue of an n-valent coupling agent, but is preferably a residue of a silicon atom-containing coupling agent, and more preferably a residue of a halogenated silane or an alkoxysilane. Examples of coupling agents constituting the residue of the coupling agent include those described below.
[0051] Particularly preferred block copolymer C is a mixture of block copolymer C1 in which n is 2, block copolymer C2 in which n is 3, and block copolymer C3 in which n is 4. In this case, the weight ratio (C1 / C2 / C3) of block copolymers C1 to C3 is preferably 40-80 / 30-10 / 30-10.
[0052] Aromatic vinyl polymer block (Ar c ) is a polymer block composed mainly of repeating units which are aromatic vinyl monomer units obtained by polymerizing aromatic vinyl monomers.
[0053] Aromatic vinyl polymer block (Ar c The aromatic vinyl monomer used to constitute the aromatic vinyl monomer unit of the aromatic vinyl polymer block (Ar1) is not particularly limited as long as it is an aromatic vinyl compound. For example, a ) and aromatic vinyl polymer block (Ar2 a ) are similar to those mentioned above.
[0054] Aromatic vinyl polymer block (Ar c As long as the aromatic vinyl monomer unit is the main repeating unit, it may contain other monomer units. Examples of monomers constituting monomer units other than aromatic vinyl monomer units include aromatic vinyl polymer blocks (Ar1 a ) and aromatic vinyl polymer block (Ar2 a ) and the content thereof may be the same. In addition, each aromatic vinyl polymer block in the block copolymer C may be composed of the same aromatic vinyl monomer unit or different aromatic vinyl monomer units. In addition, the aromatic vinyl polymer block (Ar c ) is also preferably composed substantially of one or more aromatic vinyl monomer units, and particularly preferably composed of styrene units.
[0055] Aromatic vinyl polymer block (Arc The weight average molecular weight of the copolymer is preferably 4,000 to 18,000, more preferably 5,000 to 16,000, and further preferably 6,000 to 14,000.
[0056] Block copolymer C has multiple aromatic vinyl polymer blocks (Ar c ) may be equal to or different from each other so long as they are within the above range, but it is preferable that they are substantially equal to each other.
[0057] Conjugated diene polymer block (D c ) is a polymer block composed mainly of repeating units of conjugated diene monomer units obtained by polymerizing a conjugated diene monomer.
[0058] Conjugated diene polymer block (D c The conjugated diene monomer used to constitute the conjugated diene monomer unit of the conjugated diene polymer block (D a In addition, each of the conjugated diene polymer blocks in the block copolymer C may be composed of the same conjugated diene monomer units, or may be composed of different conjugated diene monomer units.
[0059] Also, the conjugated diene polymer block (D c ) may contain other monomer units as long as the conjugated diene monomer unit is the main repeating unit. Examples of the monomer constituting the monomer units other than the conjugated diene monomer unit include a conjugated diene polymer block (D a The conjugated diene polymer block (D c ) is also preferably composed substantially of one or more conjugated diene monomer units, and particularly preferably composed of isoprene units.
[0060] Conjugated diene polymer block (D c The weight average molecular weight of the copolymer is preferably 20,000 to 200,000, more preferably 25,000 to 180,000, and further preferably 30,000 to 150,000.
[0061] The block copolymer C has a plurality of conjugated diene polymer blocks (D c ) may be equal to or different from each other so long as they are within the above range, but it is preferable that they are substantially equal to each other.
[0062] The weight average molecular weight of the block copolymer C (that is, the weight average molecular weight of the entire block copolymer C) is preferably 60,000 to 800,000, and more preferably 80,000 to 600,000.
[0063] The content of aromatic vinyl monomer units in block copolymer C is less than 20% by weight, more preferably less than 18% by weight, and even more preferably less than 16% by weight, and the lower limit is not particularly limited, but may be 5% by weight or more, based on the total monomer units constituting block copolymer C. Since the first composition of the present invention contains block copolymer C containing aromatic vinyl monomer units in the above content and also containing a residue of a coupling agent, it is possible to obtain an elastic body having excellent moldability, small film thickness variation, and small permanent elongation.
[0064] The block copolymer C is preferably obtained by a manufacturing method in which an aromatic vinyl monomer and a conjugated diene monomer are polymerized to form a diblock chain, and the diblock chain is reacted with a coupling agent to perform coupling. Therefore, the block copolymer C contains a residue of the coupling agent. The details of such a manufacturing method will be described later.
[0065] (Block Copolymer D) The first composition of the present invention may further contain a block copolymer D. The block copolymer D is a copolymer represented by the following general formula (D). General formula (D): Ard -D d (In the formula, Ar d is an aromatic vinyl polymer block, D d represents a conjugated diene polymer block)
[0066] Aromatic vinyl polymer block (Ar d ) is a polymer block composed mainly of repeating units which are aromatic vinyl monomer units obtained by polymerizing aromatic vinyl monomers.
[0067] Aromatic vinyl polymer block (Ar d The aromatic vinyl monomer used to constitute the aromatic vinyl monomer unit of the aromatic vinyl polymer block (Ar1) is not particularly limited as long as it is an aromatic vinyl compound. For example, a ) and aromatic vinyl polymer block (Ar2 a ) are similar to those mentioned above.
[0068] Aromatic vinyl polymer block (Ar d As long as the aromatic vinyl monomer unit is the main repeating unit, it may contain other monomer units. Examples of monomers constituting monomer units other than aromatic vinyl monomer units include aromatic vinyl polymer blocks (Ar1 a ) and aromatic vinyl polymer block (Ar2 a The aromatic vinyl polymer block (Ar d ) is also preferably composed substantially of one or more aromatic vinyl monomer units, and particularly preferably composed of styrene units.
[0069] Aromatic vinyl polymer block (Ar d The weight average molecular weight of the copolymer is preferably 4,000 to 18,000, more preferably 5,000 to 16,000, and further preferably 6,000 to 14,000.
[0070] Aromatic vinyl polymer block (Ar d The weight average molecular weight of the aromatic vinyl polymer block (Ar c ) is preferably substantially equal to the weight average molecular weight of
[0071] Conjugated diene polymer block (D d ) is a polymer block composed mainly of repeating units of conjugated diene monomer units obtained by polymerizing a conjugated diene monomer.
[0072] Conjugated diene polymer block (D d The conjugated diene monomer used to constitute the conjugated diene monomer unit of the conjugated diene polymer block (D a ) are similar to those mentioned above.
[0073] Also, the conjugated diene polymer block (D d ) may contain other monomer units as long as the conjugated diene monomer unit is the main repeating unit. Examples of the monomer constituting the monomer units other than the conjugated diene monomer unit include a conjugated diene polymer block (D a The conjugated diene polymer block (D d ) is also preferably composed substantially of one or more conjugated diene monomer units, and particularly preferably composed of isoprene units.
[0074] Conjugated diene polymer block (D d The vinyl bond content of the conjugated diene polymer block (D c ) is preferably substantially equal to the vinyl bond content of
[0075] Conjugated diene polymer block (D dThe weight average molecular weight of the copolymer is preferably 20,000 to 200,000, more preferably 25,000 to 180,000, and further preferably 30,000 to 150,000.
[0076] Conjugated diene polymer block (D d The weight average molecular weight of the conjugated diene polymer block (D c ) is preferably substantially equal to the weight average molecular weight of
[0077] The weight average molecular weight of block copolymer D (that is, the weight average molecular weight of the entire block copolymer D) is preferably 30,000 to 200,000, and more preferably 40,000 to 180,000.
[0078] The content of aromatic vinyl monomer units in block copolymer D is less than 20% by weight, preferably less than 18% by weight, more preferably less than 16% by weight, and the lower limit is not particularly limited, but may be 5% by weight or more, based on the total monomer units constituting block copolymer D. When the first composition of the present invention contains block copolymer D containing aromatic vinyl monomer units in the above content, it is possible to obtain an elastic body having better moldability, less film thickness variation, and less permanent set.
[0079] The first composition of the present invention contains the above-mentioned block copolymers A to C, and optionally further contains block copolymer D. The weight ratio (A / B / C) of block copolymers A to C in the first composition of the present invention is preferably 10-40 / 10-40 / 80-20, more preferably 15-40 / 15-40 / 70-25, and further preferably 20-35 / 20-35 / 60-30.
[0080] When the first composition of the present invention further contains block copolymer D, the content of block copolymer D in the first composition of the present invention including block copolymers A to C is preferably 1 to 20% by weight, more preferably 2 to 18% by weight, and even more preferably 3 to 16% by weight.
[0081] The block copolymers A to D can be produced according to a conventional method. The most common production method is a method in which an aromatic vinyl monomer and a conjugated diene monomer are sequentially polymerized by an anionic living polymerization method to form a polymer block, and if necessary, a coupling agent is reacted to perform coupling. A method in which an aromatic vinyl monomer, a conjugated diene monomer, and then an aromatic vinyl monomer are sequentially polymerized in this order to form a polymer block may also be used. In addition, each polymer may be produced separately according to a conventional polymerization method, and other polymer components may be blended as necessary, and then the polymers may be mixed according to a conventional method such as kneading or solution mixing to produce the block copolymers. In addition, as described below, it is also possible to simultaneously produce block copolymers A and B, or to simultaneously produce block copolymers C and D.
[0082] In addition, in the present invention, it is also possible to use commercially available block copolymers, such as "Quintac (registered trademark)" (manufactured by Zeon Corporation), "JSR-SIS (registered trademark)" (manufactured by JSR Corporation), "Vector (registered trademark)" (manufactured by DEXCO polymers), "Asaprene (registered trademark)", "Tufprene (registered trademark)", "Tuftec (registered trademark)" (manufactured by Asahi Kasei Chemicals Corporation), "Septon (registered trademark)" (manufactured by Kuraray Co., Ltd.), and "Kraton (registered trademark)" (manufactured by Kraton Corporation).
[0083] The block copolymers A and B are preferably produced by a method in which an aromatic vinyl monomer, a conjugated diene monomer and then an aromatic vinyl monomer are sequentially polymerized in this order to form a polymer block.
[0084] More specifically, the block copolymer A and the block copolymer B are preferably produced by the following production method: a first polymerization step of polymerizing a monomer including an aromatic vinyl monomer in a solvent in the presence of a polymerization initiator to obtain a solution containing an aromatic vinyl polymer block chain; a second polymerization step of adding a monomer including a conjugated diene monomer to the solution including the aromatic vinyl polymer block chain and polymerizing the monomer to obtain a solution including a diblock chain; a third polymerization step of adding a monomer including an aromatic vinyl monomer to the solution including the diblock chain and polymerizing the monomer to obtain a solution including a triblock chain; a terminating step of adding a polymerization terminator to the solution containing the triblock chain in an amount of less than 1 molar equivalent relative to the active terminals of the triblock chain to inactivate a portion of the active terminals, thereby obtaining a solution containing block copolymer B and the triblock chain; a fourth polymerization step of adding a monomer including an aromatic vinyl monomer to the solution including the triblock chain and the block copolymer B, and polymerizing the monomer to obtain a solution including the block copolymer A and the block copolymer B; A manufacturing method comprising the steps of:
[0085] In the above-mentioned production method, first, a monomer containing an aromatic vinyl monomer as a main component is polymerized in a solvent using a polymerization initiator (first polymerization step). As the polymerization initiator used, an organic alkali metal compound, an organic alkaline earth metal compound, an organic lanthanoid series rare earth metal compound, etc., which are generally known to have anionic polymerization activity for aromatic vinyl monomers and conjugated diene monomers, can be used. As the organic alkali metal compound, an organic lithium compound having one or more lithium atoms in the molecule is particularly preferably used, and specific examples thereof include organic monolithium compounds such as ethyl lithium, n-propyl lithium, isopropyl lithium, n-butyl lithium, sec-butyl lithium, t-butyl lithium, hexyl lithium, phenyl lithium, stilbene lithium, dialkylamino lithium, diphenylamino lithium, and ditrimethylsilylamino lithium, organic dilithium compounds such as methylene dilithium, tetramethylene dilithium, hexamethylene dilithium, isoprenyl dilithium, and 1,4-dilithio-ethylcyclohexane, and further, organic trilithium compounds such as 1,3,5-trilithiobenzene. Among these, organic monolithium compounds are particularly preferably used.
[0086] Examples of organic alkaline earth metal compounds used as polymerization initiators include n-butyl magnesium bromide, n-hexyl magnesium bromide, ethoxy calcium, calcium stearate, t-butoxy strontium, ethoxy barium, isopropoxy barium, ethyl mercapto barium, t-butoxy barium, phenoxy barium, diethylamino barium, barium stearate, and ethyl barium. Specific examples of other polymerization initiators include composite catalysts consisting of lanthanoid series rare earth metal compounds containing neodymium, samarinium, gadolinium, etc. / alkyl aluminum / alkyl aluminum halide / alkyl aluminum hydride, and metallocene catalysts containing titanium, vanadium, samarinium, gadolinium, etc., which are homogeneous in organic solvents and have living polymerizability. Note that these polymerization initiators may be used alone or in combination of two or more.
[0087] The amount of the polymerization initiator used may be determined depending on the target molecular weight and is not particularly limited, but is preferably 0.01 to 20 mmol, more preferably 0.05 to 15 mmol, and even more preferably 0.1 to 10 mmol, per 100 g of the total monomers used.
[0088] The solvent used in the polymerization is not particularly limited as long as it is inactive to the polymerization initiator, and for example, a chain hydrocarbon solvent, a cyclic hydrocarbon solvent, or a mixed solvent thereof is used. Examples of the chain hydrocarbon solvent include chain alkanes and alkenes having 4 to 6 carbon atoms, such as n-butane, isobutane, 1-butene, isobutylene, trans-2-butene, cis-2-butene, 1-pentene, trans-2-pentene, cis-2-pentene, n-pentane, isopentane, neo-pentane, and n-hexane. Specific examples of the cyclic hydrocarbon solvent include aromatic compounds such as benzene, toluene, and xylene; and alicyclic hydrocarbon compounds such as cyclopentane and cyclohexane. These solvents may be used alone or in combination of two or more.
[0089] The amount of the solvent used in the polymerization is not particularly limited, but it is preferable to set the concentration of the block copolymer in the finally obtained block copolymer solution to be preferably in the range of 5 to 60% by weight, more preferably in the range of 10 to 55% by weight, and particularly preferably in the range of 20 to 50% by weight.
[0090] In addition, in order to control the structure of each polymer block, a Lewis base compound may be added to the reactor used for polymerization. Examples of the Lewis base compound include ethers such as tetrahydrofuran, diethyl ether, dioxane, ethylene glycol dimethyl ether, ethylene glycol dibutyl ether, diethylene glycol dimethyl ether, and diethylene glycol dibutyl ether; tertiary amines such as tetramethylethylenediamine, trimethylamine, triethylamine, pyridine, and quinuclidine; alkali metal alkoxides such as potassium t-amyl oxide and potassium t-butyl oxide; and phosphines such as triphenylphosphine. These Lewis base compounds may be used alone or in combination of two or more, and are appropriately selected within a range that does not impair the object of the present invention.
[0091] The timing of adding the Lewis base compound during the polymerization reaction is not particularly limited, and may be appropriately determined depending on the structure of each target block copolymer. For example, the Lewis base compound may be added in advance before the start of polymerization, or after some of the polymer blocks have been polymerized, or the Lewis base compound may be added in advance before the start of polymerization and then further added after some of the polymer blocks have been polymerized.
[0092] The polymerization reaction temperature is preferably 10 to 150° C., more preferably 30 to 130° C., and further preferably 40 to 90° C. The time required for polymerization varies depending on the conditions, but is usually within 48 hours, preferably 0.5 to 10 hours. The polymerization pressure is not particularly limited as long as it is within a pressure range sufficient to maintain the monomer and the solvent in a liquid phase at the above polymerization temperature range.
[0093] Under the above-mentioned conditions, a solution containing an aromatic vinyl polymer block chain can be obtained by polymerizing a monomer containing an aromatic vinyl monomer as a main component in a solvent using a polymerization initiator. The aromatic vinyl polymer block chain obtained by polymerization usually has an active terminal. The aromatic vinyl polymer block chain obtained has an aromatic vinyl polymer block (Ar1 a ) or aromatic vinyl polymer block (Ar1 b ), the amount of the monomer used in this first polymerization step is set to be 100%. a ) and aromatic vinyl polymer block (Ar1 b ) may be determined depending on the weight average molecular weight of the copolymer.
[0094] Next, a monomer containing a conjugated diene monomer as a main component is added to the solution containing the aromatic vinyl polymer block chain obtained in the first polymerization step, and polymerization is carried out (second polymerization step). This makes it possible to obtain a solution containing a diblock chain. The diblock chain obtained by polymerization usually has an active terminal. The diblock chain obtained in the second polymerization step is also a diblock chain obtained by adding the aromatic vinyl polymer block (Ar1) obtained in the first polymerization step. a ) or aromatic vinyl polymer block (Ar1 b ) is formed in the polymer chain, a conjugated diene polymer block (D a ) or conjugated diene polymer block (D b Since the polymer chains that will form the conjugated diene polymer block (D a ) and conjugated diene polymer block (D b The polymerization reaction temperature, polymerization time, and polymerization pressure may be controlled within the same ranges as in the first polymerization step.
[0095] Next, a monomer containing an aromatic vinyl monomer as a main component is added to the solution containing the diblock chain obtained in the second polymerization step, and polymerization is carried out (third polymerization step). This makes it possible to obtain a solution containing a triblock chain. The triblock chain obtained by polymerization usually has an active terminal. The triblock chain obtained in the third polymerization step is also a solution containing the aromatic vinyl polymer block (Ar1) obtained in the second polymerization step. a ) or aromatic vinyl polymer block (Ar1 b ) and conjugated diene polymer block (D a ) or conjugated diene polymer block (D b ) is formed in the polymer chain, an aromatic vinyl polymer block (Ar2 a ) or an aromatic vinyl polymer block (Ar2 b Since the polymer chains that will form the aromatic vinyl polymer block (Ar2) are further bonded, the amount of monomer used in this third polymerization step is b The polymerization reaction temperature, polymerization time, and polymerization pressure may be controlled within the same ranges as in the first polymerization step.
[0096] Next, a polymerization terminator is added to the solution containing the triblock chain obtained in the third polymerization step in an amount of less than 1 molar equivalent relative to the active terminals of the triblock chain (termination step). As a result, a part of the active terminals of the triblock chain is deactivated, and a block copolymer with deactivated active terminals is obtained. This block copolymer has the general formula (B): Ar1 b -D b -Ar2 b The block copolymer B is represented by the following formula:
[0097] The polymerization terminator is not particularly limited as long as it can react with an active terminal to deactivate the active terminal and does not react with another active terminal after reacting with one active terminal, but from the viewpoint of suppressing moisture absorption of the obtained composition, it is preferable that the polymerization terminator is a compound that does not contain a halogen atom, and among them, a polymerization terminator that generates a metal alkoxide, a metal aryloxide, or a metal hydroxide when reacting with an active terminal is particularly preferable. Examples of compounds that are particularly preferably used as the polymerization terminator include water, monohydric alcohols such as methanol and ethanol, and monohydric phenols such as phenol and cresol.
[0098] The amount of the polymerization terminator used is determined according to the weight ratio of the block copolymer A and the block copolymer B constituting the first composition, and is not particularly limited as long as it is an amount less than 1 molar equivalent relative to the active terminal of the triblock chain. Generally, the amount of the polymerization terminator is in the range of 0.18 to 0.91 molar equivalents relative to the active terminal, and preferably in the range of 0.35 to 0.80 molar equivalents.
[0099] As described above, when a polymerization terminator is added to a solution containing a triblock chain having an active end in an amount less than 1 molar equivalent relative to the active end, some of the active ends of the triblock chain having an active end are deactivated, and the polymer with the deactivated active ends becomes block copolymer B. The remaining part of the triblock chain having an active end that has not reacted with the polymerization terminator remains unreacted in the solution.
[0100] Next, a monomer containing an aromatic vinyl monomer as a main component is added to the solution containing the triblock chain and the block copolymer B obtained in the termination step, and polymerization is carried out (fourth polymerization step). a -D a -Ar2 aIn the fourth polymerization step, a solution containing a block copolymer A represented by the formula: and a block copolymer B represented by the formula: a Since the polymer chains which will form part of the aromatic vinyl polymer block (Ar2) are further joined, the amount of monomer used in this fourth polymerization step is a The polymerization reaction temperature, polymerization time, and polymerization pressure may be controlled within the same ranges as in the first polymerization step.
[0101] After the fourth polymerization step, the polymer component may be recovered from the solution containing the block copolymer A and the block copolymer B (recovery step). The recovery method may be any conventional method and is not particularly limited. For example, after the reaction is completed, if necessary, a polymerization terminator such as water, methanol, ethanol, propanol, hydrochloric acid, or citric acid may be added, and if necessary, an additive such as an antioxidant may be added, and then the solution may be directly subjected to a known method such as drying or steam stripping to recover the polymer component. When the polymer component is recovered as a slurry by applying steam stripping or the like, the polymer component may be dehydrated using any dehydrator such as an extruder-type squeezer to obtain crumbs having a water content of a predetermined value or less, and the crumbs may be further dried using any dryer such as a band dryer or an expansion extrusion dryer. The block copolymer obtained as described above may be processed into a pellet shape or the like according to a conventional method and then used. In this manner, block copolymer A and block copolymer B can be produced.
[0102] The block copolymer C is preferably produced by a method in which an aromatic vinyl monomer and a conjugated diene monomer are polymerized to form a diblock chain, and then the diblock chain is reacted with a coupling agent to perform coupling.
[0103] More specifically, the block copolymer C is preferably produced by the following production method: a first polymerization step of polymerizing a monomer including an aromatic vinyl monomer in a solvent in the presence of a polymerization initiator to obtain a solution containing an aromatic vinyl polymer block chain; a second polymerization step of adding a monomer including a conjugated diene monomer to the solution including the aromatic vinyl polymer block chain and polymerizing the monomer to obtain a solution including a diblock chain; a reaction step of adding a coupling agent to the solution containing the diblock chain to obtain a block copolymer C; A manufacturing method comprising the steps of:
[0104] In the above-mentioned production method, first, a monomer containing an aromatic vinyl monomer as a main component is polymerized in a solvent using a polymerization initiator (first polymerization step). The solvent and its amount used, and the polymerization initiator and its amount used in the first polymerization step may be the same as those in the first polymerization step in the above-mentioned preferred production method of block copolymer A and block copolymer B. Also, a Lewis base compound may be added as in the first polymerization step in the above-mentioned preferred production method of block copolymer A and block copolymer B. Also, the same polymerization reaction temperature, polymerization time, and polymerization pressure as those in the first polymerization step in the above-mentioned preferred production method of block copolymer A and block copolymer B can be adopted.
[0105] Under the above-mentioned conditions, a solution containing an aromatic vinyl polymer block chain can be obtained by polymerizing a monomer containing an aromatic vinyl monomer as a main component in a solvent using a polymerization initiator. The aromatic vinyl polymer block chain obtained by polymerization usually has an active terminal. The aromatic vinyl polymer block chain obtained has an aromatic vinyl polymer block (Ar c ), the amount of monomer used in this first polymerization step is c ) may be determined depending on the weight average molecular weight of the copolymer.
[0106] Next, a monomer containing a conjugated diene monomer as a main component is added to the solution containing the aromatic vinyl polymer block chain obtained in the first polymerization step, and polymerization is carried out (second polymerization step). This makes it possible to obtain a solution containing a diblock chain. The diblock chain obtained by polymerization usually has an active terminal. The diblock chain obtained in the second polymerization step is also a solution containing the aromatic vinyl polymer block (Ar c ) is formed in the polymer chain, a conjugated diene polymer block (D c Since the polymer chains that will form the conjugated diene polymer block (D c The polymerization reaction temperature, polymerization time, and polymerization pressure may be controlled within the same ranges as in the first polymerization step.
[0107] Next, a coupling agent is added to the solution containing the diblock chains (reaction step), whereby the active terminals of the diblock chains react with the coupling agent, and two or more diblock chains are bonded together via the residues of the coupling agent to form a block copolymer C.
[0108] The coupling agent is not particularly limited as long as it has two or more functional groups in one molecule that can react with the active terminals of the diblock chain, but a coupling agent having 2 to 8 functional groups in one molecule that can react with the active terminals of the diblock chain is preferred, and a coupling agent having 2 to 4 functional groups in one molecule that can react with the active terminals of the diblock chain is more preferred. The coupling agent preferably contains a silicon atom, and halogenated silanes and alkoxysilanes are more preferred.
[0109] Examples of coupling agents having two functional groups in one molecule that can react with the active terminal of the diblock chain (bifunctional coupling agents) include bifunctional halogenated silanes such as dichlorosilane, monomethyldichlorosilane, and dimethyldichlorosilane; bifunctional alkoxysilanes such as diphenyldimethoxysilane and diphenyldiethoxysilane; bifunctional halogenated alkanes such as dichloroethane, dibromoethane, methylene chloride, and dibromomethane; bifunctional tin halides such as dichlorotin, monomethyldichlorotin, dimethyldichlorotin, monoethyldichlorotin, diethyldichlorotin, monobutyldichlorotin, and dibutyldichlorotin; dibromobenzene, benzoic acid, CO, and 2-chloropropene. Among these, bifunctional halogenated silanes or bifunctional alkoxysilanes are particularly preferably used. These bifunctional coupling agents may be used alone or in combination of two or more.
[0110] Examples of coupling agents having three functional groups in one molecule that can react with the active terminal of the diblock chain (trifunctional coupling agents) include trifunctional halogenated alkanes such as trichloroethane and trichloropropane, trifunctional halogenated silanes such as methyltrichlorosilane and ethyltrichlorosilane, and trifunctional alkoxysilanes such as methyltrimethoxysilane, phenyltrimethoxysilane, and phenyltriethoxysilane. These trifunctional coupling agents may be used alone or in combination of two or more.
[0111] Examples of coupling agents having four functional groups in one molecule that can react with the active terminals of the diblock chain (tetrafunctional coupling agents) include tetrafunctional halogenated alkanes such as carbon tetrachloride, carbon tetrabromide, and tetrachloroethane; tetrafunctional halogenated silanes such as tetrachlorosilane and tetrabromosilane; tetrafunctional alkoxysilanes such as tetramethoxysilane and tetraethoxysilane; and tetrafunctional tin halides such as tetrachlorotin and tetrabromotin. These tetrafunctional coupling agents may be used alone or in combination of two or more.
[0112] The number n of the block copolymer C, i.e., the number of branches of the block copolymer C, can be adjusted by adjusting the type, amount used, timing of addition of the coupling agent, the amount used of the Lewis base compound, etc. Also, the number of branches of the block copolymer C can be adjusted by adjusting the coupling rate using a reaction terminator such as methanol. Also, the number of branches of the block copolymer C can be adjusted by combining two or more coupling agents having different numbers of functional groups that can react with the active terminals of the diblock chain. Furthermore, by these means, the diblock chain obtained in the second polymerization step may be left unreacted and finally recovered as the block copolymer D.
[0113] The amount of the coupling agent used is adjusted to an appropriate amount depending on the number of branches of the target block copolymer C. The amount of the coupling agent used is preferably 0.05 to 0.9 molar equivalents, more preferably 0.20 to 0.70 molar equivalents, based on the active terminal of the diblock chain.
[0114] The reaction temperature is preferably 10 to 150° C., more preferably 30 to 130° C., and further preferably 40 to 90° C. The time required for the reaction varies depending on the conditions, but is usually within 48 hours, preferably 0.5 to 10 hours.
[0115] After the reaction step, the polymer component may be recovered from the solution containing the block copolymer C and, optionally, the block copolymer D (recovery step). The recovery method may be any conventional method and is not particularly limited. For example, after the reaction is completed, if necessary, a polymerization terminator such as water, methanol, ethanol, propanol, hydrochloric acid, or citric acid may be added, and if necessary, an additive such as an antioxidant may be added, and then the solution may be directly subjected to a known method such as drying or steam stripping to recover the polymer component. When the polymer component is recovered as a slurry by applying steam stripping or the like, the polymer component may be dehydrated using any dehydrator such as an extruder-type squeezer to obtain crumbs having a water content of a predetermined value or less, and the crumbs may be further dried using any dryer such as a band dryer or an expansion extrusion dryer. The block copolymer obtained as described above may be processed into a pellet shape or the like according to a conventional method and then used. In this manner, block copolymer C and, optionally, block copolymer D can be produced.
[0116] The first composition of the present invention may contain a polyolefin-based thermoplastic resin in addition to the block copolymers A to C. A stretchable film can be easily obtained from the first composition containing the block copolymers A to C and the polyolefin-based thermoplastic resin. The resulting stretchable film and a nonwoven fabric may be laminated to obtain a stretchable laminate, in which case the stretchable film and the nonwoven fabric are firmly bonded. The stretchable laminate can be produced, for example, by extruding the composition onto a nonwoven fabric by extrusion molding. The polyolefin-based thermoplastic resin used in the present invention is not particularly limited as long as it is a resin having thermoplasticity with olefin as the main repeating unit, and may be any of a homopolymer of α-olefin, a copolymer of two or more kinds of α-olefin, and a copolymer of α-olefin and a monomer other than α-olefin, or may be a modified (co)polymer of these.
[0117] Specific examples of polyolefin-based thermoplastic resins include homopolymers or copolymers of α-olefins such as ethylene and propylene, such as polyethylenes such as linear low-density polyethylene (LLDPE), low-density polyethylene (LDPE), medium-density polyethylene (MDPE), high-density polyethylene (HDPE), and metallocene polyethylene, polypropylene, metallocene polypropylene, polymethylpentene, and polybutene; copolymers of ethylene and other α-olefins, such as ethylene-propylene random copolymers, ethylene-propylene block copolymers, ethylene-butene-1 copolymers, ethylene-propylene-butene-1 copolymers, and ethylene-cyclic olefin copolymers; copolymers of α-olefins and carboxylic acid unsaturated alcohols, mainly composed of α-olefins, and saponified products thereof, such as ethylene-vinyl acetate. copolymers, ethylene-vinyl alcohol copolymers; copolymers of α-olefins and α,β-unsaturated carboxylic esters or α,β-unsaturated carboxylic acids, etc., mainly composed of α-olefins, such as ethylene-α,β-unsaturated carboxylic ester copolymers (ethylene-ethyl acrylate copolymers, ethylene-methyl methacrylate copolymers, etc.), ethylene-α,β-unsaturated carboxylic acid copolymers (ethylene-acrylic acid copolymers, ethylene-methacrylic acid copolymers, etc.); acid-modified olefin resins obtained by modifying α-olefin (co)polymers such as polyethylene and polypropylene with unsaturated carboxylic acids and / or anhydrides thereof, such as acrylic acid, methacrylic acid, maleic acid, maleic anhydride, fumaric acid, itaconic acid, etc.; ionomer resins obtained by reacting Na ions, Zn ions, etc. with copolymers of ethylene and methacrylic acid; and mixtures thereof. Among these, copolymers of polyethylene or ethylene and other α-olefins are preferred, and among these, copolymers of polyethylene or ethylene and other α-olefins produced using a metallocene catalyst are particularly preferred.
[0118] The weight average molecular weight of the polyolefin thermoplastic resin is not particularly limited, but is usually selected in the range of 10,000 to 5,000,000, and preferably in the range of 50,000 to 800,000. The specific gravity and melt index of the polyolefin thermoplastic resin are also not particularly limited, but the specific gravity is usually 0.80 to 0.95 g / cm. 3 is selected in the range of 0.85 to 0.94 g / cm 3 The melt index, as a value measured in accordance with ASTM D-1238 (G condition, 200°C, 5 kg), is usually selected in the range of 1 to 1000 g / 10 min, and preferably selected in the range of 3 to 500 g / 10 min.
[0119] The content of the polyolefin thermoplastic resin is preferably 3 to 50 parts by weight, more preferably 5 to 40 parts by weight, and further preferably 8 to 30 parts by weight, based on 100 parts by weight in total of the block copolymers A to C. The polyolefin thermoplastic resin may be used alone or in combination of two or more kinds.
[0120] The first composition of the present invention may further contain, as necessary, fatty acid amides, polyethylene wax, antioxidants, tackifier resins, softeners, antibacterial agents, light stabilizers, ultraviolet absorbers, dyes, lubricants, and the like.
[0121] The fatty acid amide may be an aliphatic monoamide or an aliphatic bisamide. The aliphatic monoamide is not particularly limited as long as it is a compound in which a hydrocarbon group and one amide group (-NHCO) are bonded, but a monoamide of a higher saturated fatty acid having 12 or more carbon atoms (i.e., a compound in which a chain alkyl group having 12 or more carbon atoms and one amide group (-NHCO) are bonded) is preferably used.
[0122] Specific examples of fatty acid monoamides include saturated fatty acid monoamides such as lauric acid amide, myristic acid amide, palmitic acid amide, stearic acid amide, behenic acid amide, and hydroxystearic acid amide; and unsaturated fatty acid monoamides such as oleic acid amide and erucic acid amide.
[0123] The content of the fatty acid amide is preferably 0.2 to 10 parts by weight, more preferably 0.3 to 8 parts by weight, and further preferably 0.5 to 6 parts by weight, based on 100 parts by weight in total of the block copolymers A to C.
[0124] The polyethylene wax is a wax whose main constituent unit is an ethylene monomer unit. The polyethylene wax used in the present invention is not particularly limited, but one having a viscosity at 140°C of 20 to 6,000 mPa·s is preferably used.
[0125] Polyethylene wax is generally produced by polymerization of ethylene or decomposition of polyethylene, and either type of polyethylene wax may be used in the present invention. In addition, polyethylene wax is commercially available, and specific examples thereof include "AC Polyethylene" (manufactured by Honeywell), "Mitsui Hiwax" (manufactured by Mitsui Chemicals, Inc.), "Sunwax" (manufactured by Sanyo Chemical Industries, Ltd.), and "Epolene" (manufactured by Eastman Chemical Co.).
[0126] The antioxidant is not particularly limited, and examples of the antioxidant that can be used include hindered phenol compounds such as pentaerythritol tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 2,6-di-t-butyl-p-cresol, and di-t-butyl-4-methylphenol; thiodicarboxylate esters such as dilauryl thiopropionate; and phosphites such as tris(nonylphenyl)phosphite.
[0127] The content of the antioxidant is preferably 10 parts by weight or less, and more preferably 0.05 to 5 parts by weight, based on 100 parts by weight in total of the block copolymers A to C.
[0128] The first composition of the present invention preferably further contains a wax containing linear and branched chain hydrocarbons. By containing the wax containing linear and branched chain hydrocarbons, the first composition of the present invention can obtain an elastomer having excellent moldability, small thickness variation, and small permanent elongation, as well as excellent color, low odor, and excellent ozone crack resistance.
[0129] The wax used in the present invention may be a natural wax or a synthetic wax, but is preferably a natural wax, and more preferably a petroleum wax. A blended wax containing petroleum wax as the main component and other natural waxes or synthetic waxes may be used. In addition, a small amount of resin or the like may be further blended with the wax in order to improve the function or processability of the wax. The first composition of the present invention may contain waxes other than the wax containing linear and branched hydrocarbons, but from the viewpoint of obtaining an elastic body having excellent hue and low odor and excellent ozone crack resistance, it is preferable that the composition does not contain other waxes.
[0130] The linear hydrocarbon is preferably a linear aliphatic saturated hydrocarbon. The linear hydrocarbon may be called normal paraffin. The branched hydrocarbon is preferably a branched aliphatic saturated hydrocarbon. The branched hydrocarbon may be called isoparaffin. As the linear hydrocarbon and the branched hydrocarbon, the linear hydrocarbon and the branched hydrocarbon contained in petroleum wax are preferable.
[0131] The wax used in the present invention may contain cyclic hydrocarbons in addition to linear and branched hydrocarbons, but the total amount of linear and branched hydrocarbons in the wax is preferably 50 mass % or more, more preferably 70 mass % or more, even more preferably 80 mass % or more, and most preferably 90 mass % or more.
[0132] The weight ratio (n- / iso-) of linear hydrocarbons (n-form) to branched hydrocarbons (iso-form) in the wax is 30 / 70 to 99 / 1, preferably 50 / 50 to 97 / 3, more preferably 70 / 30 to 95 / 5, and most preferably 75 / 25 to 90 / 10. By keeping the weight ratio (n- / iso-form) within the above range, an elastic body having excellent ozone crack resistance can be obtained.
[0133] The melting point of the wax is less than 80°C, preferably 76°C or less, more preferably 73°C or less, preferably 30°C or more, more preferably 40°C or more, and even more preferably 45°C or more. The melting point of the wax can be measured using a differential scanning calorimeter or the like. If the melting point of the wax is too high, it becomes difficult to obtain an elastic body having excellent ozone crack resistance. If the melting point of the wax is too low, blocking is likely to occur during transportation and storage, and it is likely to melt during processing, resulting in poor handling properties.
[0134] The content of the wax in the first composition of the present invention is preferably 0.1 to 5 parts by weight, more preferably 0.3 to 3.5 parts by weight, and even more preferably 0.5 to 2 parts by weight, based on 100 parts by weight of the total of the block copolymers in the composition. If the wax content is too high, it may be difficult to obtain an elastic body with a small permanent elongation, and if the wax content is too low, it may be difficult to obtain an elastic body with excellent ozone crack resistance. The weight of the block copolymer in the composition means, for example, the total weight of the block copolymers A to C when the first composition of the present invention contains block copolymers A to C, and the total weight of the block copolymers A to D when the first composition of the present invention contains block copolymers A to D.
[0135] In obtaining the first composition of the present invention, the method of mixing the block copolymers A to C with the other components is not particularly limited. For example, the components are dissolved in a solvent and mixed uniformly, and then the solvent is removed by heating or the like, or the components are melt-mixed in a screw extruder, kneader, or the like. Among these, melt mixing is preferred from the viewpoint of more efficient mixing. The temperature at which melt mixing is performed is not particularly limited, but is usually in the range of 100 to 250°C.
[0136] When the block copolymers A to C are melt-mixed with the other components, in order to mix the other components with the block copolymers A to C more uniformly, it is preferable to prepare master batch pellets in advance by kneading all or a part of one or more of the block copolymers A to C with the other components using a single screw extruder, a twin screw extruder, a Banbury mixer, etc. Among the above, it is particularly preferable to use a twin screw extruder from the viewpoints of kneading ability, cleaning ability, and cost.
[0137] When producing an elastomer, by simultaneously supplying block copolymers A to C and supplying the master batch pellets and uniformly mixing them, an elastomer can be obtained with good productivity in which the other components are highly uniformly dispersed in the block copolymers A to C.
[0138] One or more of the block copolymers A to C used to produce the master batch pellets may be allocated to the production of the master batch pellets in an amount necessary for the production of the master batch pellets, and the composition ratio of the block copolymers A to C described above can be achieved by adjusting the supply amounts of the block copolymers A to C and the supply amount of the master batch pellets when producing the elastomer.
[0139] The second composition of the present invention contains a block copolymer having at least one aromatic vinyl polymer block and at least one conjugated diene polymer block, and a wax.
[0140] (Block Copolymer) The block copolymer used in the second composition of the present invention has at least one aromatic vinyl polymer block and at least one conjugated diene polymer block. The aromatic vinyl polymer block contains aromatic vinyl monomer units formed from an aromatic vinyl monomer, and the conjugated diene polymer block contains conjugated diene monomer units formed from a conjugated diene monomer.
[0141] The aromatic vinyl monomer forming the aromatic vinyl monomer unit is not particularly limited as long as it is an aromatic vinyl compound, and examples thereof include styrene, α-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2-ethylstyrene, 3-ethylstyrene, 4-ethylstyrene, 2,4-diisopropylstyrene, 2,4-dimethylstyrene, 4-t-butylstyrene, 5-t-butyl-2-methylstyrene, 2-chlorostyrene, 3-chlorostyrene, 4-chlorostyrene, 4-bromostyrene, 2-methyl-4,6-dichlorostyrene, 2,4-dibromostyrene, and vinylnaphthalene. Among these, it is preferable to use styrene. These aromatic vinyl monomers can be used alone or in combination of two or more. In addition, when the block copolymer has a plurality of aromatic vinyl polymer blocks, each aromatic vinyl polymer block may be composed of the same aromatic vinyl monomer unit or may be composed of different aromatic vinyl monomer units.
[0142] In addition, the aromatic vinyl polymer block may contain other monomer units as long as the aromatic vinyl monomer unit is the main repeating unit. Examples of monomers constituting the monomer units other than the aromatic vinyl monomer units that can be contained in the aromatic vinyl polymer block include conjugated diene monomers such as 1,3-butadiene and isoprene (2-methyl-1,3-butadiene), α,β-unsaturated nitrile monomers, unsaturated carboxylic acid or acid anhydride monomers, unsaturated carboxylate monomers, and non-conjugated diene monomers. The content of monomer units other than the aromatic vinyl monomer units in the aromatic vinyl polymer block is preferably 20% by mass or less, more preferably 10% by mass or less, and particularly preferably substantially 0% by mass.
[0143] The conjugated diene monomer forming the conjugated diene monomer unit is not particularly limited as long as it is a conjugated diene compound, and examples thereof include 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 2-chloro-1,3-butadiene, 1,3-pentadiene, and 1,3-hexadiene. Among these, it is preferable to use 1,3-butadiene and / or isoprene, and it is particularly preferable to use isoprene. These conjugated diene monomers can be used alone or in combination of two or more. In addition, when the block copolymer has a plurality of conjugated diene polymer blocks, each conjugated diene polymer block may be composed of the same conjugated diene monomer unit or may be composed of different conjugated diene monomer units. Furthermore, a hydrogenation reaction may be performed on a part of the unsaturated bonds of the conjugated diene polymer block.
[0144] In addition, the conjugated diene polymer block may contain other monomer units as long as the conjugated diene monomer unit is the main repeating unit. Examples of monomers constituting the monomer units other than the conjugated diene monomer units that can be contained in the conjugated diene polymer block include aromatic vinyl monomers such as styrene and α-methylstyrene, α,β-unsaturated nitrile monomers, unsaturated carboxylic acid or acid anhydride monomers, unsaturated carboxylic acid ester monomers, and non-conjugated diene monomers. The content of monomer units other than the conjugated diene monomer units in the conjugated diene polymer block is preferably 20% by mass or less, more preferably 10% by mass or less, and particularly preferably substantially 0% by mass.
[0145] The vinyl bond content of the conjugated diene polymer block (the ratio of 1,2-vinyl bond units and 3,4-vinyl bond units to all conjugated diene monomer units in the conjugated diene polymer block) is not particularly limited, but is preferably in the range of 1 to 20 mol%, more preferably in the range of 2 to 15 mol%, and particularly preferably in the range of 3 to 10 mol%.
[0146] The block copolymer used in the second composition of the present invention is not particularly limited in the number of each polymer block and the bond form thereof, as long as it has at least one aromatic vinyl polymer block and at least one conjugated diene polymer block. Specific examples of the form of the block copolymer used in the second composition of the present invention include, but are not limited to, aromatic vinyl-conjugated diene block copolymers represented as Ar-D, aromatic vinyl-conjugated diene-aromatic vinyl block copolymers represented as Ar-D-Ar or (Ar-D)nX, conjugated diene-aromatic vinyl-conjugated diene block copolymers represented as D-Ar-D or (D-Ar)nX, aromatic vinyl-conjugated diene-aromatic vinyl-conjugated diene block copolymers represented as Ar-D-Ar-D, and mixtures of block copolymers obtained by mixing two or more of these in any combination, where Ar represents an aromatic vinyl polymer block, D represents a conjugated diene polymer block, X represents a residue of a coupling agent, and n represents an integer of 2 or more. In the second composition of the present invention, examples of block copolymers that are particularly preferably used include block copolymers selected from aromatic vinyl-conjugated diene block copolymers represented as Ar-D, aromatic vinyl-conjugated diene-aromatic vinyl block copolymers represented as Ar-D-Ar or (Ar-D)nX, and mixtures thereof. In the aromatic vinyl-conjugated diene-aromatic vinyl block copolymer represented by Ar-D-Ar or (Ar-D)X, the molecular chain length of each aromatic vinyl block (Ar) may be the same, or the aromatic vinyl blocks (Ar) may have different molecular chain lengths.
[0147] The weight average molecular weight of the block copolymer used in the second composition of the present invention is not particularly limited, but is usually selected in the range of 40,000 to 500,000, and preferably in the range of 50,000 to 400,000.
[0148] The content of aromatic vinyl monomer units in the block copolymer used in the second composition of the present invention is not particularly limited, but is preferably in the range of 5 to 60 mass%, more preferably in the range of 7 to 55 mass%, and even more preferably in the range of 10 to 50 mass%. If the block copolymer is substantially composed of only aromatic vinyl monomer units and conjugated diene monomer units, the block copolymer can be decomposed by ozonolysis according to the method described in Rubber Chem. Technol., 45, 1295 (1972), and then reduced with lithium aluminum hydride, whereby the conjugated diene monomer unit portion can be decomposed and the aromatic monovinyl monomer unit portion can be extracted, and the aromatic vinyl monomer unit content can be measured by such a method.
[0149] The block copolymer having an aromatic vinyl polymer block and a conjugated diene polymer block as described above can be produced according to a conventional method, and the most common production method is a method in which an aromatic vinyl monomer and a conjugated diene monomer are sequentially polymerized by an anionic living polymerization method to form a polymer block, and if necessary, a coupling agent is reacted to perform coupling. Alternatively, a method in which an aromatic vinyl monomer, a conjugated diene monomer, and then an aromatic vinyl monomer are sequentially polymerized in this order to form a polymer block may be used.
[0150] In addition, as the block copolymer used in the second composition of the present invention, it is also possible to use commercially available block copolymers, such as "Quintac (registered trademark)" (manufactured by Zeon Corporation), "JSR-SIS (registered trademark)" (manufactured by JSR Corporation), "Vector (registered trademark)" (manufactured by DEXCO polymers), "Asaprene (registered trademark)", "Tufprene (registered trademark)", "Tuftec (registered trademark)" (manufactured by Asahi Kasei Chemicals Corporation), and "Septon (registered trademark)" (manufactured by Kuraray Co., Ltd.).
[0151] As the block copolymer used in the second composition of the present invention, a composition containing the block copolymers A to D described above as the first composition of the present invention is particularly preferred. By containing a composition containing the block copolymers A to D as the block copolymer, the second composition of the present invention can obtain an elastomer having excellent hue and low odor and excellent ozone crack resistance, as well as excellent moldability, small film thickness variation, and small permanent set.
[0152] (wax) The wax used in the second composition of the present invention contains linear and branched chain hydrocarbons. By containing the wax containing linear and branched chain hydrocarbons, the second composition of the present invention has excellent color and low odor, and can provide an elastomer having excellent ozone crack resistance.
[0153] As the wax used in the second composition of the present invention, those waxes described in detail as the wax used in the first composition of the present invention can be used.
[0154] The wax content in the second composition of the present invention is preferably 0.1 to 5 parts by weight, more preferably 0.3 to 3.5 parts by weight, and even more preferably 0.5 to 2 parts by weight, based on 100 parts by weight of the block copolymer. If the wax content is too high, it may be difficult to obtain an elastomer with a small permanent elongation, and if the wax content is too low, it may be difficult to obtain an elastomer with excellent ozone crack resistance.
[0155] In obtaining the second composition of the present invention, the method of mixing the block copolymer with other components such as wax is not particularly limited. For example, the method of dissolving each component in a solvent and mixing them uniformly, and then removing the solvent by heating, etc., and the method of melt-mixing each component with a screw extruder, kneader, etc. are exemplified. Among these, melt mixing is preferable from the viewpoint of more efficient mixing. The temperature when melt mixing is not particularly limited, but is usually in the range of 100 to 250°C.
[0156] When the block copolymer and other components such as wax are melt-mixed, in order to mix the other components and the block copolymer more uniformly, it is preferable to prepare master batch pellets by previously kneading a part of the block copolymer with the other components using a single screw extruder, a twin screw extruder, a Banbury mixer, etc. Among the above, it is particularly preferable to use a twin screw extruder from the viewpoints of kneading properties, cleaning properties, and costs.
[0157] When producing an elastomer, by simultaneously supplying the block copolymer and supplying the master batch pellets and uniformly mixing them, an elastomer can be obtained with good productivity in which the other components are highly uniformly dispersed in the block copolymer.
[0158] The second composition of the present invention may further contain the above-mentioned polyolefin-based thermoplastic resin. In addition, the second composition of the present invention may contain, as necessary, fatty acid amide, antioxidant, tackifier resin, softener, antibacterial agent, light stabilizer, ultraviolet absorber, dye, lubricant, etc.
[0159] The first composition of the present invention has excellent moldability, and can produce an elastomer with little film thickness variation and small permanent elongation. Therefore, the first composition of the present invention can be suitably used for elastomers, particularly for elastomers for sanitary materials. In addition, the first composition of the present invention can be suitably used for the following applications:
[0160] The second composition of the present invention is excellent in hue and low odor, and can provide an elastomer having excellent ozone crack resistance. Therefore, the second composition of the present invention can be suitably used for elastomers, particularly for elastomers for sanitary materials. In addition, the second composition of the present invention can be suitably used for the following applications.
[0161] The first and second compositions and elastomers of the present invention can be used in applications such as films, threads (elastic strands), gloves, elastic bands, condoms, various rolls for office equipment and office use, vibration-proof sheets for electric and electronic devices, vibration-proof rubber, impact absorbing sheets, impact cushioning films and sheets, vibration-proof sheets for homes, vibration-proof damper materials, and the like; adhesives used in adhesive tapes, adhesive sheets, adhesive labels, dust removal rollers, and the like; adhesives used in sanitary products and bookbinding; and elastic fibers used in clothing, sporting goods, and the like.
[0162] The first and second compositions and elastic bodies of the present invention can be suitably used for films, particularly elastic films for sanitary materials. The elastic bodies and films of the present invention are obtained from the first and second compositions of the present invention, and therefore are strong and highly elastic, have little thickness variation, and have small permanent set. The first and second compositions and elastic bodies of the present invention can also be suitably used as threads (elastic strands).
[0163] The thickness of the film of the present invention is not particularly limited and is adjusted depending on the application, but when it is used as a film for sanitary products such as disposable diapers and sanitary products, it is usually 0.01 to 5 mm, preferably 0.01 to 1 mm, and more preferably 0.02 to 0.2 mm.
[0164] The method for molding the first and second compositions of the present invention into a film is not particularly limited, and any conventionally known film molding method can be applied. From the viewpoint of obtaining a smooth film with good productivity, however, extrusion molding is preferred, and among them, extrusion molding using a T-die is particularly preferred.
[0165] A specific example of extrusion molding using a T-die is a method in which a molten composition is extruded at 150 to 250°C from a T-die attached to a single-screw extruder or a twin-screw extruder, and then wound up while being cooled with a take-up roll. When cooling with a take-up roll, the film may be stretched. When winding the film, the melt of the composition may be coated on a substrate made of polyethylene terephthalate, polyethylene, polypropylene, nonwoven fabric, or release paper to form a film, or the melt of the composition may be sandwiched between these substrates to form a film. The film thus obtained may be used in a form integral with the substrate, or may be peeled off from the substrate.
[0166] The elastic body and film of the present invention are excellent in uniformity of film thickness. The excellent uniformity of thickness of the elastic body and film of the present invention can be confirmed, for example, by cutting a sample film to a length of 30 cm along the melt flow direction during molding, measuring the thickness of the film at 15 points at 2 cm intervals along the melt flow direction in the center of the film using a digital thickness gauge (manufactured by Toyo Seiki Co., Ltd., measurement accuracy: 0.001 mm units), and finding that the ratio of the standard deviation of the film thickness to the average film thickness (standard deviation / average value) calculated from these measurements is usually 30% or less, preferably 20% or less.
[0167] The permanent elongation of the elastic body and film of the present invention is usually 5% or less, and preferably 2% or less. The permanent elongation of the film can be determined by the method described in the Examples.
[0168] The elastic body and film of the present invention can be used as a single layer or can be laminated with other members to be used as a multilayer body depending on the application. Specific examples of the use of the elastic body and film as a single layer include an elastic film used in sanitary products such as paper diapers and sanitary products, a protective film for protecting optical films, and a heat-shrinkable film used for shrink packaging of containers or heat-shrinkable labels. Specific examples of the use of the elastic body and film as a multilayer body include a case in which the film of the present invention is slit and then coated with a hot melt adhesive or the like to form a tape, and the tape is attached in a shrunk state to a nonwoven fabric, a woven fabric, a plastic film, or a laminate of these, and the shrinkage of the tape is relaxed to form an elastic gather member. Furthermore, the elastic body and film can be appropriately processed according to a known method depending on other applications, and can be used as an elastic member such as a base material for elastic patches, gloves, surgical gloves, finger cots, tourniquets, contraceptives, headbands, goggle bands, and rubber bands. EXAMPLES
[0169] The present invention will be described in detail below with reference to examples and comparative examples. In the following, "parts" are by weight unless otherwise specified. Tests and evaluations were performed according to the following methods.
[0170] [Weight average molecular weight of each block copolymer] The weight average molecular weight was determined as a polystyrene-equivalent molecular weight by high performance liquid chromatography using tetrahydrofuran as a carrier at a flow rate of 0.35 ml / min. The apparatus used was a Tosoh HLC8320, the column consisted of three connected Shodex KF-404HQ columns (column temperature 40°C) manufactured by Showa Denko, and the detectors were a differential refractometer and an ultraviolet detector. The molecular weight was calibrated at 12 points using standard polystyrene (5 to 3 million) manufactured by Tosoh.
[0171] [Weight ratio of each block copolymer in the block copolymer mixture] The ratio was determined from the area ratio of the peaks corresponding to each block copolymer in the chart obtained by the above-mentioned high performance liquid chromatography.
[0172] [Weight average molecular weight of styrene polymer block of each block copolymer] According to the method described in Rubber Chem. Technol., 45, 1295 (1972), the block copolymer was reacted with ozone and reduced with lithium aluminum hydride to decompose the isoprene polymer block of the block copolymer. Specifically, the following procedure was followed. That is, 300 mg of the sample was dissolved in a reaction vessel containing 100 ml of dichloromethane treated with molecular sieves. After placing this reaction vessel in a cooling bath and lowering the temperature to -25°C, ozone generated by an ozone generator was introduced into the reaction vessel while oxygen was flowing at a flow rate of 170 ml / min. After 30 minutes had passed since the start of the reaction, the completion of the reaction was confirmed by introducing the gas flowing out of the reaction vessel into the potassium iodide aqueous solution. Next, 50 ml of diethyl ether and 470 mg of lithium aluminum hydride were charged into another reaction vessel substituted with nitrogen, and the solution reacted with ozone was slowly dropped into the reaction vessel while cooling the reaction vessel with ice water. The reaction vessel was then placed in a water bath, gradually heated, and refluxed at 40°C for 30 minutes. After that, while stirring the solution, dilute hydrochloric acid was dripped into the reaction vessel in small amounts until hydrogen generation was almost no longer observed. After this reaction, the solid product generated in the solution was filtered, and the solid product was extracted with 100 ml of diethyl ether for 10 minutes. This extract was combined with the filtrate obtained by filtration, and the solvent was distilled off to obtain a solid sample. The weight average molecular weight of the sample thus obtained was measured according to the above-mentioned method for measuring weight average molecular weight, and the value was taken as the weight average molecular weight of the styrene polymer block.
[0173] [Weight average molecular weight of isoprene polymer block of each block copolymer] The weight average molecular weight of the corresponding styrene polymer block was subtracted from the weight average molecular weight of the block copolymer obtained as described above, and the weight average molecular weight of the isoprene polymer block was calculated based on the calculated value.
[0174] [Vinyl bond content of isoprene polymer block of each block copolymer] It was determined based on proton NMR measurement.
[0175] [Styrene unit content of each block copolymer] The value was determined based on the ratio of the detection intensities of the differential refractometer and the ultraviolet detector in the measurement by high performance liquid chromatography. Note that copolymers having different styrene unit contents were prepared in advance, and a calibration curve was prepared using them.
[0176] [Thickness uniformity (film thickness variation)] The film was cut to a length of 30 cm along the melt flow direction during molding, and the thickness of the film was measured at 15 points at 2 cm intervals along the melt flow direction in the center of the film using a digital thickness gauge (manufactured by Toyo Seiki Co., Ltd., measurement accuracy: 0.001 mm units), the average and standard deviation of these measurements were obtained, and the ratio of the standard deviation of the film thickness to the average film thickness (standard deviation / average value) was calculated and evaluated according to the following criteria. The smaller the ratio, the higher the uniformity of the film thickness and the better the moldability of the composition used for molding. ○: 20% or less △: More than 20% but less than 30% ×: More than 30%
[0177] [Permanent elongation of film] The measurements were made using a Tensilon universal testing machine RTC-1210 manufactured by ORIENTEC in accordance with ASTM 412. Specifically, a DieA sample shape was used, the gauge length before stretching was set to 40 mm, the film was stretched at an elongation rate of 200%, and then held in this state for 10 minutes, after which it was suddenly shrunk without rebounding, and after leaving it for 10 minutes, the gauge length was measured, and the permanent elongation was calculated based on the following formula. Permanent elongation (%) = (L1-L0) / L0 x 100 L0: Gauge length before stretching (mm) L1: Gauge distance after shrinking and leaving for 10 minutes (mm) In this measurement, two films were used, one was measured along the melt flow direction (MD) during molding, and the other was measured along the direction perpendicular to the melt flow (CD) during molding, and the evaluation was based on the following criteria. Permanent elongation in melt flow direction (MD) ○: 2% or less △: More than 2% but less than 5% ×: More than 5% Permanent elongation in the direction perpendicular to melt flow (CD) ○: 2% or less △: More than 2% but less than 5% ×: More than 5%
[0178] [Ozone crack resistance of film] The film was fixed to a tension holder with a chuck distance of 4.0 cm. The chuck distance was then extended to 5.0 cm, and the film was fixed in a 25% stretched state. The fixed film was left in a thermostatic chamber at 30°C, 50% RH, and an ozone concentration of 5 pphm, and the time until cracks were visible to the naked eye was measured and evaluated according to the following criteria. No cracks occurred even after more than 2 hours. ×: Cracks occurred within 2 hours.
[0179] [Film hue] The Gardner color index of the film was measured in accordance with JIS K0071-2 and evaluated according to the following criteria. ○: Gardner color count is less than 2 ×: Number of Gardner colors is 2 or more
[0180] [Film odor] The film was subjected to a sensory test in accordance with the odor intensity indication method in the olfactory measurement method for odors published by the Odor Countermeasure Research Association. Specifically, a film measuring 100mm x 300mm was placed in a 120mL heat-resistant container and covered with aluminum foil. The heat-resistant container containing the film was then placed in an oven and heated at 140°C for 20 minutes, after which the odor was checked. The odor was checked by a panel of six people. In this test, in order to prevent olfactory fatigue, the six-person panel was divided into two groups of three people, and each group was given a chance to smell the odor. The order in which the samples were smelled was random. 0: Odorless 1: Smell that can just be detected (detection threshold concentration) 2: Weak odor that can be identified (recognition threshold concentration) 3. Easily detectable odors 4: Strong odor 5: Strong odor The results of the sensory test were calculated by excluding the maximum and minimum values from the scores judged by the six panelists and averaging the scores judged by the remaining four panelists, and were evaluated according to the following criteria. ○: Sensory test score is less than 3 points ×: Sensory test score is 3 points or more
[0181] [Production Example 1] In a pressure-resistant reactor, 23.3 kg of cyclohexane, 1.4 mmol of N,N,N',N'-tetramethylethylenediamine (hereinafter referred to as "TMEDA"), and 1.04 kg of styrene were added, and while stirring at 40°C, 92.9 mmol of n-butyllithium was added, and polymerization was carried out for 1 hour while raising the temperature to 50°C. The polymerization conversion rate of styrene was 100%. Subsequently, 5.66 kg of isoprene was continuously added to the reactor over 1 hour while controlling the temperature to maintain 50-60°C. After the addition of isoprene was completed, polymerization was carried out for another 1 hour. The polymerization conversion rate of isoprene was 100%. Next, 1.04 kg of styrene was continuously added over 1 hour while controlling the temperature to maintain 50-60°C. After the addition of styrene was completed, polymerization was carried out for another 1 hour to form a triblock chain having an active end. The polymerization conversion rate of styrene was 100%. Next, 63.4 mmol of methanol was added as a polymerization terminator and mixed to deactivate some of the active ends of the triblock chain having an active end, forming a styrene-isoprene-styrene triblock copolymer B1. After this, 0.98 kg of styrene was continuously added over 1 hour while controlling the temperature to maintain 50 to 60°C. After the addition of styrene was completed, polymerization was continued for another 1 hour to form a triblock chain having an active end. The polymerization conversion rate of styrene was 100%. Finally, 63.4 mmol of methanol was added as a polymerization terminator and mixed to deactivate all of the active ends of the triblock chain, forming a styrene-isoprene-styrene triblock copolymer A1. A part of the obtained reaction solution was taken out and the block copolymer was evaluated according to the above measurement method. The results are shown in Table 2.
[0182] 0.3 parts of 2,6-di-tert-butyl-p-cresol was added as an antioxidant to 100 parts of the reaction liquid obtained as described above (containing 30 parts of the polymer component), and the mixed solution was dropped in small amounts into warm water heated to 85 to 95°C to volatilize the solvent and obtain a precipitate. The precipitate was pulverized and dried with hot air at 85°C to recover a mixture containing block copolymer A1 and block copolymer B1.
[0183] The weight ratio of block copolymer A1 to block copolymer B1 (block copolymer A1 / block copolymer B1) in the above mixture was 40 / 60.
[0184] [Production Examples 2 to 4] A reaction solution and a mixture were obtained in the same manner as in Production Example 1, except that the amounts of raw materials such as styrene and isoprene were changed as shown in Table 1. The evaluation results are shown in Table 2.
[0185] [Table 1]
[0186] [Table 2]
[0187] [Production Example 5] In a pressure-resistant reactor, 23.2 kg of cyclohexane, 1.5 mmol of N,N,N',N'-tetramethylethylenediamine (hereinafter referred to as TMEDA), and 1.20 kg of styrene were added, and while stirring at 40°C, 101.7 mmol of n-butyllithium was added, and polymerization was carried out for 1 hour while raising the temperature to 50°C. The polymerization conversion rate of styrene was 100%. Subsequently, 6.53 kg of isoprene was continuously added to the reactor over 1 hour while controlling the temperature to maintain 50-60°C. After the addition of isoprene was completed, polymerization was carried out for another 1 hour to form a diblock chain having an active terminal. The polymerization conversion rate of isoprene was 100%. Next, 25.4 mmol of dimethyldichlorosilane and 9.7 mmol of tetramethoxysilane were added as coupling agents, and a coupling reaction was carried out for 2 hours to form a styrene-isoprene coupling block copolymer C1. Then, 203 mmol of methanol was added as a polymerization terminator and mixed to inactivate all the active ends of the diblock chain to form styrene-isoprene diblock copolymer D1. A portion of the resulting reaction solution was taken out and the block copolymer was evaluated according to the above-mentioned measurement method. The results are shown in Table 4.
[0188] To 100 parts of the reaction liquid obtained as described above, 0.3 parts of 2,6-di-tert-butyl-p-cresol was added as an antioxidant and mixed, and the mixed solution was dropped in small amounts into warm water heated to 85 to 95°C to volatilize the solvent and obtain a precipitate. The precipitate was pulverized and dried with hot air at 85°C to recover a mixture containing block copolymers C1 and D1.
[0189] The weight ratio of block copolymer C1 to block copolymer D1 (block copolymer C1 / block copolymer D1) in the above mixture was 90 / 10.
[0190] [Production Examples 6 to 7] A reaction solution and a mixture were obtained in the same manner as in Production Example 4, except that the amounts of raw materials such as styrene and isoprene used were changed as shown in Table 3. The evaluation results are shown in Table 4.
[0191] [Table 3]
[0192] [Table 4]
[0193] Example 1 The mixture obtained in Production Example 1 and the mixture obtained in Production Example 5 were mixed so as to obtain the weight ratio of each block copolymer shown in Table 5 to prepare a composition. The obtained composition was put into a twin-screw extruder equipped with a T-die. Then, in this twin-screw extruder, these were heated and melted at 200°C, kneaded, and extruded continuously for 20 minutes while being sandwiched between PET release films, thereby forming into a film having an average thickness of 0.05 mm. The film thickness variation and permanent set of the film of Example 1 obtained in this manner were measured. The results are shown in Table 5. The details of the film forming conditions are as follows.
[0194] (Film forming conditions) Compound processing speed: 5kg / hour Film take-up speed: 4m / min Extruder temperature: Adjust to 100℃ at the inlet and 200℃ at the T-die Screw: Full flight Extruder L / D: 30 T-die: width 200mm, lip 0.5mm
[0195] [Examples 2 to 3, Comparative Examples 1 to 4] A composition and a film were obtained and evaluated in the same manner as in Example 1, except that the weight ratio of each block copolymer was changed to that shown in Table 5. The results are shown in Table 5.
[0196] [Table 5]
[0197] As the results in Table 5 show, when three types of block copolymers with different structures were used in combination and the weight average molecular weight of each block constituting each block copolymer and the content of aromatic vinyl monomer units in each block copolymer were appropriately adjusted, a composition having excellent moldability was obtained, and a film with little film thickness variation and small permanent set was obtained (Examples 1 to 3).
[0198] On the other hand, even when three types of block copolymers with different structures were used in combination, if a block copolymer with an excessively high content of aromatic vinyl monomer units was included, the moldability of the composition was insufficient, and the film thickness of the obtained film varied greatly and the permanent set was also large (Comparative Examples 1 to 4).
[0199] Example 4 100 parts of the composition prepared in Example 1 and 3 parts of additives having the composition shown in Table 7 were put into a twin-screw extruder equipped with a T-die. In the twin-screw extruder, these were heated, melted and kneaded at 200°C, and extruded continuously for 20 minutes while sandwiched between PET release films, to form a film having an average thickness of 0.05 mm. The film thickness variation and permanent elongation of the film of Example 4 thus obtained were measured. The results are shown in Table 8. The details of the film forming conditions are as follows. The weight ratio (n-form / iso-form) and melting point of the additives shown in Table 7 are also shown in Table 6.
[0200] (Film forming conditions) Compound processing speed: 5kg / hour Film take-up speed: 4m / min Extruder temperature: Adjust to 100℃ at the inlet and 200℃ at the T-die Screw: Full flight Extruder L / D: 30 T-die: width 200mm, lip 0.5mm
[0201] [Examples 5 to 14] Films were obtained and evaluated in the same manner as in Example 4, except that the types and amounts of additives were changed as shown in Table 8. The results are shown in Table 8.
[0202] [Reference examples 5 to 11] Films were obtained and evaluated in the same manner as in Example 4, except that the types and amounts of additives were changed as shown in Table 9. The results are shown in Table 9.
[0203] [Table 6]
[0204] [Table 7]
[0205] [Table 8]
[0206] [Table 9]
[0207] As the results in Table 8 show, when a wax having a relatively low melting point containing linear hydrocarbons and branched hydrocarbons in a specific weight ratio was added to the block copolymer, a composition excellent in hue and low odor was obtained, and an elastomer excellent in ozone crack resistance was obtained (Examples 4 to 14).
[0208] On the other hand, as shown by the results in Table 9, when a wax having a relatively high melting point was added, an elastic body having excellent ozone crack resistance could not be obtained (Reference Example 5). Furthermore, as shown in the results in Table 9, when a wax having a relatively high melting point and not containing linear and branched hydrocarbons in an appropriate weight ratio was used, an elastomer having excellent ozone crack resistance could not be obtained (Reference Examples 6 to 8). Furthermore, as shown in the results in Table 9, when a wax that did not contain an appropriate weight ratio of linear hydrocarbons and branched hydrocarbons was used, an elastomer with excellent ozone crack resistance could not be obtained (Reference Example 11). Furthermore, as shown by the results in Table 9, when additives other than wax were used, the color of the resulting composition was poor and the odor of the resulting composition was also strong (Reference Examples 9 to 10).
Claims
1. A composition comprising a block copolymer having at least one aromatic vinyl polymer block and at least one conjugated diene polymer block, and a wax, comprising: The content of aromatic vinyl monomer units in the block copolymer is 5 to 55% by mass, the wax contains linear hydrocarbons and branched hydrocarbons, and the weight ratio of the linear hydrocarbons to the branched hydrocarbons, expressed as linear hydrocarbons / branched hydrocarbons, is 75 / 25 to 99 / 1; The melting point of the wax is less than 80° C. the total amount of the linear hydrocarbons and the branched hydrocarbons in the wax is 90 mass% or more, The content of the wax in the composition is 0.1 to 5 parts by weight based on 100 parts by weight of the block copolymer.
2. The composition described in claim 1, wherein the content of monomer units other than conjugated diene monomer units in the conjugated diene polymer block is 20 mass% or less.
3. 3. The composition according to claim 1, wherein the vinyl bond content of the conjugated diene polymer block is in the range of 1 to 20 mol %.
4. 4. The composition according to claim 1, wherein the block copolymer has a weight average molecular weight of 40,000 to 500,000.
5. In the case where Ar represents an aromatic vinyl polymer block, D represents a conjugated diene polymer block, X represents a residue of a coupling agent, and n represents an integer of 2 or more, The composition according to any one of claims 1 to 4, wherein the block copolymer is a block copolymer selected from an aromatic vinyl-conjugated diene block copolymer represented as Ar-D, an aromatic vinyl-conjugated diene-aromatic vinyl block copolymer represented as Ar-D-Ar or (Ar-D)n-X, and a mixture thereof.
6. 6. The composition of claim 5, wherein the block copolymer comprises a vinyl aromatic-conjugated diene-vinyl aromatic block copolymer represented as Ar-D-Ar or (Ar-D)n-X.
7. 7. The composition of claim 6, wherein the block copolymer further comprises an aromatic vinyl-conjugated diene block copolymer designated as Ar-D.
8. The composition of claim 1, wherein the block copolymer has an isoprene polymer block.
9. An elastomer obtained from the composition according to any one of claims 1 to 8.
10. 10. The elastic body according to claim 9, which is an elastic body for use in sanitary materials.
11. 11. The elastic body according to claim 9 or 10, which is a film or a thread.
Citation Information
Patent Citations
Rubbery composition
JP1976122153A
Thermoplastic elastomer composition excellent in durability
JP2001316594A
s-eb-s block copolymer / oil-aqueous dispersion and its use in molding articles
JP2002514232A
Block copolymer composition
JP2005139326A
Block copolymer composition and film
JP2016069565A