All solid state battery
By integrating intermediate layers between electrode current collectors and active materials in all-solid-state batteries, the bonding issues are resolved, leading to improved cycle characteristics and reduced localized reactions, enhancing battery performance.
Patent Information
- Application Number
- JP2020509163
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-03-28
- Filing Date
- 2019-03-27
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2039-03-27
AI Technical Summary
Existing all-solid-state batteries face challenges in bonding the positive and negative electrode current collectors with their respective active materials, leading to localized electrochemical reactions and deteriorated cycle characteristics due to unbonded parts.
Incorporating intermediate layers between the electrode current collectors and active materials, specifically the first and second intermediate layers, to enhance bonding and reduce unbonded areas, thereby improving the uniformity of electrochemical reactions.
The introduction of intermediate layers improves the cycle characteristics of all-solid-state batteries by reducing localized reactions and enhancing the uniformity of material interactions, resulting in higher capacity retention rates.
Smart Images

Figure 0007553352000003 
Figure 0007553352000004 
Figure 0007553352000005
Abstract
Description
[Technical field]
[0001] The present invention relates to an all-solid-state battery. This application claims priority based on Japanese Patent Application No. 2018-62460, filed on March 28, 2018, the contents of which are incorporated herein by reference. [Background technology]
[0002] In recent years, lithium-ion secondary batteries have been widely used as power sources for mobile communication devices such as mobile phones and smartphones, as well as small portable devices such as notebook computers, tablet PCs, and game consoles. The lithium-ion secondary batteries used in such small portable devices are required to be smaller, thinner, and more reliable. In order to operate these electronic devices for long periods of time, research and development is being actively conducted to extend the life and increase the capacity of lithium-ion secondary batteries.
[0003] Known lithium ion secondary batteries include those that use an organic electrolyte solution as the electrolyte and those that use a solid electrolyte solution. Conventionally, lithium ion secondary batteries that use an organic electrolyte solution as the electrolyte have a positive electrode and a negative electrode, in which a positive electrode active material or a negative electrode active material that absorbs and releases lithium ions is applied to both sides of a sheet-like current collector made of aluminum, copper, or the like, and a separator is sandwiched between the positive electrode and the negative electrode, which is wound multiple times to form a wound body, which is then enclosed together with the electrolyte solution in an exterior body of a cylindrical, square, coin, or other shape. The electrolyte in such lithium-ion secondary batteries contains a flammable organic solvent, and an unexpected excessive impact can cause leakage or a short circuit, resulting in abnormal heat generation. For this reason, there has been a demand for batteries with greater safety.
[0004] Lithium-ion secondary batteries that use a solid electrolyte (all-solid-state batteries) have a higher degree of freedom in designing the battery shape and can be made smaller and thinner, compared to lithium-ion secondary batteries that use an organic electrolyte. In addition, because they do not contain electrolyte, they have the advantage of being highly reliable and free from leakage or abnormal heat generation.
[0005] Solid-state batteries are mainly classified into two types: thin-film and bulk. Thin-film types are produced using thin-film technologies such as the PVD method and the sol-gel method, while bulk types are produced by powder molding of electrode active materials and sulfide-based solid electrolytes. However, thin-film types have problems in that it is difficult to thicken the active material layer or to highly laminate the layers, resulting in small battery capacity and high manufacturing costs.
[0006] On the other hand, bulk-type batteries use sulfide-based solid electrolytes, which generate hydrogen sulfide when they react with water, so the batteries must be fabricated in a glove box with a controlled dew point. In addition, it is difficult to make sulfide solid electrolytes into sheets, so there are challenges in making the solid electrolyte layer thinner and increasing the number of layers in the battery.
[0007] In view of these problems, Patent Documents 1 and 2 propose a method for manufacturing an all-solid-state battery that can be mass-produced industrially by using an oxide-based solid electrolyte that is stable in air, forming each component into a sheet, stacking them, and then firing them at the same time. Furthermore, Patent Document 2 proposes a manufacturing method in which a first electrode layer and the second electrode layer are configured to contain the same active material, and are alternately stacked with an electrolyte region therebetween to realize a non-polar all-solid-state battery, which eliminates the need to distinguish between terminal electrodes, simplifies the battery manufacturing process and mounting process, and is effective in reducing manufacturing costs. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Special Publication No. 07-135790 [Patent Document 2] Patent No. 5512293 Summary of the Invention [Problem to be solved by the invention]
[0009] However, in the configurations shown in Patent Documents 1 and 2, although the manufacturing methods are applicable to mass production, the bonding between the positive electrode current collector and the positive electrode active material, or between the negative electrode current collector and the negative electrode active material, is insufficient, resulting in the existence of unbonded portions, which may cause localized electrochemical reactions and result in deterioration of cycle characteristics.
[0010] The present invention has been made in consideration of the above problems, and has an object to provide an all-solid-state battery having high cycle characteristics. [Means for solving the problem]
[0011] The all-solid-state battery according to the present invention includes a positive electrode current collector layer and a positive electrode active material layer, a negative electrode current collector layer and a negative electrode active material layer, a solid electrolyte layer disposed between the positive electrode active material layer and the negative electrode active material layer and made of a solid electrolyte, and at least one of a first intermediate layer formed between the positive electrode current collector layer and the positive electrode active material layer and a second intermediate layer formed between the negative electrode current collector layer and the negative electrode active material layer.
[0012] According to this configuration, by providing a first intermediate layer formed between the positive electrode collector layer and the positive electrode active material layer, and a second intermediate layer formed between the negative electrode collector layer and the negative electrode active material layer, it is possible to improve the bonding between the positive electrode collector and the positive electrode active material, or between the negative electrode collector and the negative electrode active material, and to reduce unbonded parts. This reduces localization of electrochemical reactions during charging or discharging, enables the reactions of the positive electrode active material and the negative electrode active material to occur uniformly, and improves cycle characteristics.
[0013] In the all-solid-state battery according to the present invention, it is preferable that a bonding rate of the first intermediate layer or the second intermediate layer to the positive electrode current collector layer or the negative electrode current collector layer is greater than 1%.
[0014] According to this configuration, by providing the first intermediate layer or the second intermediate layer such that the proportion of the positive electrode collector layer or the negative electrode collector layer bonded thereto is greater than 1%, it is possible to improve the bonding between the positive electrode collector layer and the first intermediate layer or between the negative electrode collector layer and the second intermediate layer, which further reduces unbonded portions between the positive electrode collector layer and the positive electrode active material layer or between the negative electrode collector layer and the negative electrode active material layer, thereby further reducing localization of electrochemical reactions during charging or discharging and enabling reactions between the positive electrode active material and the negative electrode active material to occur uniformly, thereby further improving cycle characteristics.
[0015] In the all-solid-state battery according to the present invention, the bonding rate is preferably greater than 30%.
[0016] According to this configuration, by providing the first intermediate layer or the second intermediate layer so that the proportion of the positive electrode current collector layer or the negative electrode current collector layer that is bonded thereto is greater than 1%, it is possible to improve the bonding between the positive electrode current collector layer and the first intermediate layer or between the negative electrode current collector layer and the second intermediate layer, which further reduces unbonded portions between the positive electrode current collector layer and the positive electrode active material layer or between the negative electrode current collector layer and the negative electrode active material layer, thereby further reducing localization of electrochemical reactions during charging or discharging, and enabling reactions between the positive electrode active material and the negative electrode active material to occur uniformly, thereby further improving cycle characteristics.
[0017] In the all-solid-state battery according to the present invention, the first intermediate layer 56 or the second intermediate layer 57 may be amorphous.
[0018] According to this configuration, since the first intermediate layer or the second intermediate layer is amorphous, it becomes possible to soften and form a better bond between the positive electrode current collector layer and the positive electrode active material layer or the negative electrode current collector layer and the negative electrode active material layer, and the number of unbonded parts can be further reduced, which further reduces localization of electrochemical reactions during charging or discharging and allows the reactions of the positive electrode active material and the negative electrode active material to occur uniformly, thereby further improving cycle characteristics.
[0019] In the all-solid-state battery according to the present invention, at least one of the first intermediate layer and the second intermediate layer may contain a constituent material that includes at least an anion.
[0020] According to this configuration, since the first intermediate layer and the second intermediate layer contain at least anions, the surfaces of the constituent materials constituting the positive electrode collector layer or the negative electrode collector layer, the positive electrode active material layer or the negative electrode active material layer, and the anions contained in the first intermediate layer and the second intermediate layer are easily bonded to each other, and it is possible to improve the bonding between the positive electrode collector layer and the first intermediate layer, the negative electrode collector layer and the second intermediate layer, the positive electrode active material layer and the first intermediate layer, or the negative electrode active material layer and the second intermediate layer. This makes it possible to form a better bond between the positive electrode collector layer and the positive electrode active material layer, or the negative electrode collector layer and the negative electrode active material layer, and further reduce unbonded parts, further reduce localization of electrochemical reactions during charging or discharging, and make it possible to uniformly cause reactions between the positive electrode active material and the negative electrode active material, thereby further improving cycle characteristics.
[0021] In the all-solid-state battery according to the present invention, at least one of the first intermediate layer and the second intermediate layer is preferably an amorphous material containing at least one element selected from the group consisting of Li, V, Si, Al, Ge, Sb, Sn, Ga, In, Fe, Co, Ni, Ti, Mn, Ca, Ba, La, Zr, Ce, Cu, Mg, Sr, Cr, Mo, Nb, Zn, and P.
[0022] According to this configuration, at least one of the first intermediate layer and the second intermediate layer is an amorphous material containing at least one element selected from the group consisting of Li, V, Si, Al, Ge, Sb, Sn, Ga, In, Fe, Co, Ni, Ti, Mn, Ca, Ba, La, Zr, Ce, Cu, Mg, Sr, Cr, Mo, Nb, Zn, and P. Therefore, the first intermediate layer, which is a good bond between the positive electrode current collector layer and the positive electrode active material layer, or the second intermediate layer, which is a good bond between the negative electrode current collector layer and the negative electrode active material layer, can have an electronic conduction function, and a more uniform electrochemical reaction can be achieved. This can further improve the cycle characteristics.
[0023] The thickness of the first intermediate layer or the second intermediate layer is preferably 0.1 μm or more and 10 μm or less.
[0024] According to this configuration, by setting the thickness of the first intermediate layer or the second intermediate layer to 0.1 μm or more and 10 μm or less, it is possible to suppress an increase in resistance due to the provision of the first intermediate layer which satisfactorily bonds the positive electrode current collector layer and the positive electrode active material layer, or the second intermediate layer which satisfactorily bonds the negative electrode current collector layer and the negative electrode active material layer, and it is possible to achieve a more uniform electrochemical reaction, thereby further improving the cycle characteristics. Effect of the Invention
[0025] According to the present invention, by adopting a structure including at least one of a first intermediate layer formed between a positive electrode current collector layer and a positive electrode active material layer, and a second intermediate layer formed between a negative electrode current collector layer and a negative electrode active material layer, it is possible to provide an all-solid-state battery having excellent cycle characteristics. [Brief description of the drawings]
[0026] [Figure 1] FIG. 1 is a cross-sectional view illustrating an all-solid-state battery according to an embodiment of the present invention. [Diagram 2] 4 is a cross-sectional SEM image of the vicinity of a positive electrode current collector layer illustrating the all-solid-state battery of this embodiment. [Diagram 3]FIG. 2 is a cross-sectional view illustrating a power storage section of the all-solid-state battery of the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0027] The present invention will be described in detail below with reference to the drawings as appropriate. The drawings used in the following description may show characteristic parts in an enlarged scale for the sake of convenience in order to make the features of the present invention easier to understand, and the dimensional ratios of each component may differ from the actual ones. The materials, dimensions, etc. exemplified in the following description are merely examples, and the present invention is not limited thereto, and may be appropriately modified and implemented within the scope of the present invention.
[0028] Fig. 1 shows a cross-sectional view of an all-solid-state battery according to an embodiment of the present invention. As shown in Fig. 1, an all-solid-state battery 50 is composed of a positive electrode current collector layer 51, a positive electrode active material layer 52, a negative electrode current collector layer 53, a negative electrode active material layer 54, a solid electrolyte layer 55, a first intermediate layer 56, a second intermediate layer 57, and a terminal electrode 58, each of which has a laminated structure and has one or more power storage units.
[0029] Specifically, the all-solid-state battery 50 includes a positive electrode current collector layer 51, a positive electrode active material layer 52 provided on the positive electrode current collector layer 51, a negative electrode current collector layer 53, a negative electrode active material layer 54 provided on the negative electrode current collector layer 53, a solid electrolyte layer 55 made of a solid electrolyte and disposed between the positive electrode active material layer 52 and the negative electrode active material layer 54, and at least one of a first intermediate layer 56 formed between the positive electrode current collector layer 51 and the positive electrode active material layer 52 and a second intermediate layer 57 formed between the negative electrode current collector layer 53 and the negative electrode active material layer 54.
[0030] According to this configuration, by providing the first intermediate layer 56 formed between the positive electrode collector layer 51 and the positive electrode active material layer 52, and the second intermediate layer 57 formed between the negative electrode collector layer 53 and the negative electrode active material layer 54, it is possible to improve the bonding between the positive electrode collector and the positive electrode active material, or between the negative electrode collector and the negative electrode active material, and to reduce unbonded parts. This reduces localization of electrochemical reactions during charging or discharging, and enables the reactions of the positive electrode active material and the negative electrode active material to occur uniformly, thereby improving cycle characteristics.
[0031] Furthermore, an intermediate layer for reducing the thermal expansion coefficient may be provided at least one between the positive electrode active material layer 52 and the solid electrolyte layer 55, or between the negative electrode active material layer 54 and the solid electrolyte layer 55.
[0032] The positive electrode active material layer 52 is provided on at least one or both sides of the positive electrode current collector layer 51 .
[0033] The first intermediate layer 56 is provided between the positive electrode active material layer 52 and the positive electrode current collector layer 51 continuously or discontinuously.
[0034] The negative electrode active material layer 54 is provided on at least one or both sides of the negative electrode current collector layer 53 .
[0035] The second intermediate layer 57 is provided between the negative electrode active material layer 54 and the negative electrode current collector layer 53 continuously or discontinuously.
[0036] Each positive electrode collector layer 51 and each negative electrode collector layer 53 are connected to a different terminal electrode 58, respectively, in order to electrically connect them to the outside.
[0037] In addition, Fig. 2 shows a cross-sectional SEM image of the positive electrode current collector layer of the all-solid-state battery according to the present embodiment as a representative image for explaining the intermediate layer. As shown in Fig. 2, it can be seen that the first intermediate layer is present between the positive electrode current collector layer and the positive electrode active material layer.
[0038] Fig. 3 is a cross-sectional view showing the electricity storage unit according to the present embodiment. As shown in Fig. 3, the electricity storage unit 10 is composed of a positive electrode current collector layer 11, a positive electrode active material layer 12, a negative electrode current collector layer 13, a negative electrode active material layer 14, a solid electrolyte layer 15, a first intermediate layer 16, and a second intermediate layer 17, and each of these is laminated.
[0039] Specifically, the power storage unit 10 includes a positive electrode current collector layer 11, a positive electrode active material layer 12 provided on the positive electrode current collector layer 11, a negative electrode current collector layer 13, a negative electrode active material layer 14 provided on the negative electrode current collector layer 13, a solid electrolyte layer 15 made of a solid electrolyte and disposed between the positive electrode active material layer 12 and the negative electrode active material layer 14, and at least one of a first intermediate layer 16 formed between the positive electrode current collector layer 11 and the positive electrode active material layer 12 and a second intermediate layer 17 formed between the negative electrode current collector layer 13 and the negative electrode active material layer 14.
[0040] According to this configuration, by providing the first intermediate layer 16 formed between the positive electrode collector layer 11 and the positive electrode active material layer 12, and the second intermediate layer 17 formed between the negative electrode collector layer 13 and the negative electrode active material layer 14, it is possible to improve the bonding between the positive electrode collector and the positive electrode active material, or between the negative electrode collector and the negative electrode active material, and to reduce unbonded parts. This reduces localization of electrochemical reactions during charging or discharging, and enables the reactions of the positive electrode active material and the negative electrode active material to occur uniformly, thereby improving cycle characteristics.
[0041] In the all-solid-state battery 50 of this embodiment, the bonding rate of the first intermediate layer 56, 16 or the second intermediate layer 57, 17 to the positive electrode current collector layer 51, 11 or the negative electrode current collector layer 53, 13 is preferably greater than 1%.
[0042] According to this configuration, the first intermediate layer 56, 16 or the second intermediate layer 57, 17 is provided so that the proportion of the positive electrode collector layer 51, 11 or the negative electrode collector layer 53, 13 bonded to the first intermediate layer 56, 16 can be increased to be greater than 1%, thereby improving the bonding between the positive electrode collector layer 51, 11 and the first intermediate layer 56, 16, or between the negative electrode collector layer 53, 13 and the second intermediate layer 57, 17. This can further reduce unbonded portions between the positive electrode collector layer 51, 11 and the positive electrode active material layer 52, 12, or between the negative electrode collector layer 53, 13 and the negative electrode active material layer 54, 14, thereby further reducing localization of electrochemical reactions during charging or discharging, and allowing the reactions of the positive electrode active material and the negative electrode active material to occur uniformly, thereby improving cycle characteristics.
[0043] In the all-solid-state battery 50 of this embodiment, the bonding rate of the all-solid-state battery according to the present invention is preferably greater than 30%.
[0044] According to this configuration, the bonding ratio of the first intermediate layer 56, 16 or the second intermediate layer 57, 17 to the positive electrode collector layer 51, 11 or the negative electrode collector layer 53, 13 is set to be greater than 1%, which can improve bonding between the positive electrode collector layer 51, 11 and the first intermediate layer 56, 16 or between the negative electrode collector layer 53, 13 and the second intermediate layer 57, 17. This can further reduce unbonded portions between the positive electrode collector layer 51, 11 and the positive electrode active material layer 52, 12 or between the negative electrode collector layer 53, 13 and the negative electrode active material layer 54, 14, further reducing localization of electrochemical reactions during charging or discharging, allowing the reactions of the positive electrode active material and the negative electrode active material to occur uniformly, and further improving cycle characteristics.
[0045] In the all-solid-state battery 50 of this embodiment, it is preferable that the first intermediate layer 56, 16 or the second intermediate layer 57, 17 is amorphous.
[0046] According to this configuration, the first intermediate layer 56, 16 or the second intermediate layer 57, 17 is amorphous, and thus softens to better form a bond between the positive electrode collector layer 51, 11 and the positive electrode active material layer 52, 12 or between the negative electrode collector layer 53, 13 and the negative electrode active material layer 54, 14, and the number of unjoined parts can be further reduced. This further reduces localization of the electrochemical reaction during charging or discharging, and allows the reaction of the positive electrode active material and the negative electrode active material to occur uniformly, thereby further improving the cycle characteristics.
[0047] In the present application, amorphous refers to a powder in which no clear diffraction phenomenon is observed when the same amount of powder is analyzed by an X-ray diffraction apparatus.
[0048] In the all-solid-state battery 50 according to this embodiment, at least one of the first intermediate layer 56, 16 and the second intermediate layer 57, 17 preferably contains a constituent material that includes at least an anion.
[0049] According to this configuration, at least one of the first intermediate layer 56, 16 and the second intermediate layer 57, 17 contains at least anions, which makes it easier for the surfaces of the constituent materials of the positive electrode collector layer 51, 11 or the negative electrode collector layer 53, 13, the positive electrode active material layer 52, 12 or the negative electrode active material layer 54, 14 to bond with the anions contained in the first intermediate layer 56, 16 and the second intermediate layer 57, 17, thereby making it possible to improve the bonding between the positive electrode collector layer 51, 11 and the first intermediate layer 56, 16, or between the negative electrode collector layer 53, 13 and the second intermediate layer 57, 17, or between the positive electrode active material layer 52, 12 and the first intermediate layer 56, 16, or between the negative electrode active material layer 54, 14 and the second intermediate layer 57, 17. This makes it possible to form better bonds between the positive electrode collector layers 51, 11 and the positive electrode active material layers 52, 12, or between the negative electrode collector layers 53, 13 and the negative electrode active material layers 54, 14, further reducing unjoined areas, and further reducing localization of electrochemical reactions during charging or discharging. This makes it possible to uniformly cause reactions between the positive electrode active material and the negative electrode active material, thereby further improving cycle characteristics.
[0050] In the all-solid-state battery 50 in this embodiment, the first intermediate layers 56, 16 preferably contain at least one of the constituent materials of the positive electrode current collector layers 51, 11 and the constituent materials of the positive electrode active material layers 52, 12.
[0051] According to this configuration, the first intermediate layers 56, 16 contain at least one of the constituent materials of the positive electrode collector layers 51, 11 and the positive electrode active material layers 52, 12, which makes it possible to form a better bond between the positive electrode collector layers 51, 11 and the positive electrode active material layers 52, 12 and further reduce unbonded portions. This further reduces localization of the electrochemical reaction during charging or discharging and allows the reaction of the positive electrode active material to occur uniformly, which is preferable from the viewpoint of obtaining an all-solid-state battery with a long cycle life.
[0052] In the all-solid-state battery 50 of this embodiment, the second intermediate layers 57, 17 preferably contain at least one of the constituent materials of the negative electrode current collector layers 53, 13 and the constituent materials of the negative electrode active material layers 54, 14.
[0053] According to this configuration, the second intermediate layers 57, 17 contain at least one of the constituent materials of the negative electrode current collector layers 53, 13 and the negative electrode active material layers 54, 14, so that it is possible to form a better bond between the negative electrode current collector layers 53, 13 and the negative electrode active material layers 54, 14, and it is possible to further reduce unbonded portions. This further reduces localization of the electrochemical reaction during charging or discharging, and enables the reaction of the negative electrode active material to occur uniformly, which is preferable from the viewpoint of obtaining an all-solid-state battery with a long cycle life.
[0054] In this embodiment, the all-solid-state battery 50 desirably has a relative density of 80% or more.
[0055] According to this configuration, by making the all-solid-state battery have a relative density of 80% or more, it is possible to reduce unjoined portions of each layer, such as the positive electrode collector layers 51, 11, the first intermediate layers 56, 16, the positive electrode active material layers 52, 12, the solid electrolyte layers 55, 15, the negative electrode active material layers 54, 14, the second intermediate layers 57, 17, and the negative electrode collector layers 53, 13. This reduces localization of electrochemical reactions during charging or discharging, and enables reactions of the positive electrode active material and the negative electrode active material to occur uniformly, which is preferable from the viewpoint of obtaining an all-solid-state battery with a long cycle life.
[0056] The compositions of the positive electrode current collector layers 51, 11 and the negative electrode current collector layers 53, 13 are not particularly limited, but may contain, for example, a positive electrode active material, a negative electrode active material, a solid electrolyte, and a sintering aid in addition to the current collector material.
[0057] The compositions of the positive electrode active material layers 52, 12 and the negative electrode active material layers 54, 14 are not particularly limited, but may contain, for example, a lithium ion conductive assistant, a sintering assistant, or a conductive assistant in addition to the positive electrode active material or the negative electrode active material.
[0058] The composition of the solid electrolyte layers 55, 15 is not particularly limited, but may contain, for example, a sintering aid in addition to the solid electrolyte.
[0059] The positive electrode active material or negative electrode active material constituting the positive electrode active material layers 52, 12 or the negative electrode active material layers 54, 14 may be formed by comparing the potentials of the respective compounds, and a compound exhibiting a more noble potential may be used as the positive electrode active material for the positive electrode active material layers 52, 12, and a compound exhibiting a more base potential may be used as the negative electrode active material for the negative electrode active material layers 54, 14. The positive electrode active material layers 52, 12 and the negative electrode active material layers 54, 14 may be formed of one type of compound.
[0060] (solid electrolyte) As the solid electrolyte constituting the solid electrolyte layers 55 and 15 of the all-solid-state battery of this embodiment, it is preferable to use a material having low electronic conductivity and high lithium ion conductivity. For example, La 0.5 Li 0.5 Perovskite compounds such as TiO3 and Li 14Lithium-ion type compounds such as Zn(GeO4)4, Li7La3Zr2O 12 Garnet-type compounds such as LiTi2(PO4)3, LiGe2(PO4)3, LiZr2(PO4)3 (monoclinic), LiZr2(PO4)3 (rhombohedral), Li 1.5 Ca 0.5 Zr 1.5 (PO4)3, Li 1.3 Al 0.3 Ti 1.7 (PO4)3 and Li 1.5 Al 0.5 Ge 1.5 (PO4)3, Li3PO4 and Li 3.5 S 0.5 P 0.5 O4 and Li 2.9 PO 3.3 N 0.46 Phosphate compounds such as Li 3.25 Ge 0.25 P 0.75 It is preferable that the material is at least one selected from the group consisting of thiolithium type compounds such as S4 and Li3PS4, and glass compounds such as Li2S-P2S5 and Li2O-V2O5-SiO2.
[0061] The particle size of the solid electrolyte constituting the solid electrolyte layer of the all-solid-state battery of this embodiment is desirably 0.05 μm or more and 5 μm or less in order to form a thin and dense layer.
[0062] The thickness of the solid electrolyte layer is not particularly limited, but from the viewpoint of realizing high rate characteristics, it is preferably 0.1 μm or more and 100 μm or less, and more preferably 0.3 μm or more and 20 μm or less.
[0063] By setting the thickness of the solid electrolyte layer to 0.1 μm or more and 100 μm or less, it is possible to shorten the migration distance of lithium ions during charging and discharging while maintaining the insulating properties of the solid electrolyte layer, and to reduce the internal resistance.
[0064] (Cathode active material) As the positive electrode active material contained in the positive electrode active material layers 52, 12 and the positive electrode current collector layers 51, 11 according to this embodiment, for example, lithium oxide, lithium sulfide, or a lithium-containing compound such as an intercalation compound containing lithium is suitable, and two or more of these may be mixed and used. In particular, in order to increase the energy density, a compound represented by the general formula Li x A lithium composite oxide represented by MO2 or an intercalation compound containing lithium is preferable. M is preferably one or more transition metals, specifically, at least one of Co, Ni, Mn, Fe, Al, V, and Ti is preferable. x varies depending on the charge / discharge state of the battery, and is usually a value within the range of 0.05≦x≦1.10. In addition, manganese spinel (LiMn2O4) having a spinel crystal structure, lithium iron phosphate (LiFePO4) having an olivine crystal structure, LiCoPO4, LiNiPO4, and the like are also preferable because they can obtain high energy density.
[0065] Specifically, it is preferable to use a material that efficiently releases and adsorbs lithium ions as the positive electrode active material constituting the all-solid-state battery 50, the positive electrode active material layers 52 and 12 of the power storage unit 10, and the positive electrode current collector layers 51 and 11. For example, it is preferable to use a transition metal oxide or a transition metal composite oxide. Specifically, a lithium manganese composite oxide Li2Mn x3 Ma 1-x3 O3 (0.8≦x3≦1, Ma=Co, Ni), lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese spinel (LiMn2O4), and the general formula: LiNi x4 Co y4 Mn z4 O2 (x4+y4+z4=1, 0≦x4≦1, 0≦y4≦1, 0≦z4≦1), lithium vanadium compound (LiV2O5), olivine type LiMbPO4 (where Mb is one or more elements selected from Co, Ni, Mn, Fe, Mg, Nb, Ti, Al, and Zr), lithium vanadium phosphate (Li3V2(PO4)3 or LiVOPO4), Li-rich solid solution positive electrode Li2MnO3-LiMcO2 (Mc=Mn, Co, Ni), lithium titanate (Li4Ti5O 12)、LiaNi x5 Co y5 Al z5 O2 (0.9 < a < 1.3, 0.9 < x5 + y5 + z5 < 1.1), and it is preferably any one of composite metal oxides represented by the formula. Also, it is not limited to these materials, and other cathode active material materials that can electrochemically insert and desorb lithium ions are not particularly limited.
[0066] From the viewpoint of forming the cathode active material layers 52 and 12 of the present embodiment densely and thinly, the particle size of the cathode active material constituting the cathode active material layers 52 and 12 is preferably 0.05 μm or more and 5 μm or less.
[0067] The thickness of the cathode active material layers 52 and 12 is not particularly limited, but from the viewpoint of obtaining a high-capacity and high-output all-solid-state battery, it is preferably 0.1 μm or more and 100 μm or less, and more preferably 0.3 μm or more and 10 μm or less.
[0068] (Anode active material) As the anode active material contained in the anode active material layers 54 and 14 and the anode current collector layers 53 and 13 according to the present embodiment, from the viewpoint of obtaining an all-solid-state battery with a high weight energy density and a high volume energy density, it is preferable to use one with a low potential with respect to lithium and a large capacity per unit weight. For example, at least one metal selected from the group consisting of Li, Sn, Si, Al, Ge, Sb, Ag, Ga, In, Fe, Co, Ni, Ti, Mn, Ca, Ba, La, Zr, Ce, Cu, Mg, Sr, Cr, Mo, Nb, V, and Zn, an alloy composed of two or more of these metals, an oxide of the above metal, a phosphide, and at least one of an oxide and a phosphide of the above alloy, or a material containing a carbon material is preferable.
[0069] From the viewpoint of forming the anode active material layers 54 and 14 of the present embodiment densely and thinly, the particle size of the anode active material constituting the anode active material layers 54 and 14 is preferably 0.05 μm or more and 5 μm or less.
[0070] The thicknesses of the negative electrode active material layers 54 and 14 are not particularly limited, but from the viewpoint of obtaining a high-capacity and high-cycle-life all-solid-state battery, it is preferably 0.1 μm or more and 100 μm or less, and more preferably 0.5 μm or more and 10 μm or less.
[0071] (First intermediate layer or second intermediate layer) As the material constituting the first intermediate layer 56, 16 or the second intermediate layer 57, 17 according to this embodiment, a material having electronic conductivity, not electrochemically decomposed at the operating potential of the positive electrode active material or the negative electrode active material, and capable of joining the positive electrode current collector material and the positive electrode active material, and the negative electrode current collector material and the negative electrode active material is preferable. Specifically, at least one of the first intermediate layer 56, 16 or the second intermediate layer 57, 17 is preferably a material containing at least one element selected from the group consisting of Li, V, Si, Al, Ge, Sb, Sn, Ga, In, Fe, Co, Ni, Ti, Mn, Ca, Ba, La, Zr, Ce, Cu, Mg, Sr, Cr, Mo, Nb, Zn and P, or an amorphous material thereof. For example, lithium vanadium phosphate (Li3V2(PO4)3 or LiVOPO4), olivine-type LiMbPO4 (where Mb is one or more elements selected from Co, Ni, Mn, Fe, Mg, Nb, Ti, Al, Zr), lithium cobalt oxide (LiCoO2), lithium manganese composite oxide Li2Mn x3 Ma 1-x3 O3 (0.8 ≦ x3 ≦ 1, Ma = Co, Ni), lithium nickel oxide (LiNiO2), lithium manganese spinel (LiMn2O4), and the general formula: LiNi x4 Co y4 Mn z4 O2 (x4 + y4 + z4 = 1, 0 ≦ x4 ≦ 1, 0 ≦ y4 ≦ 1, 0 ≦ z4 ≦ 1) represented by a composite metal oxide, lithium vanadium compound (LiV2O5), Li-excess solid solution Li2MnO3-LiMcO2 (Mc = Mn, Co, Ni), lithium titanate (Li4Ti5O 12 ), LiaNi x5 Co y5 Al z5 O2 (0.9 < a < 1.3, 0.9 < x5 + y5 + z5 < 1.1), any of the composite metal oxides represented by La0.5 Li 0.5 Perovskite compounds such as TiO3 and Li 14 Lithium-ion type compounds such as Zn(GeO4)4, Li7La3Zr2O 12 Garnet-type compounds such as LiTi2(PO4)3, LiGe2(PO4)3, LiZr2(PO4)3 (monoclinic), LiZr2(PO4)3 (rhombohedral), Li 1.5 Ca 0.5 Zr 1.5 (PO4)3, Li 1.3 Al 0.3 Ti 1.7 (PO4)3 and Li 1.5 Al 0.5 Ge 1.5 (PO4)3, Li3PO4 and Li 3.5 S 0.5 P 0.5 O4 and Li 2.9 PO 3.3 N 0.46 Phosphate compounds such as Li 3.25 Ge 0.25 P 0.75 Examples of the material include thiolithium-type compounds such as S4 and Li3PS4, glass compounds such as Li2S-P2S5 and Li2O-V2O5-SiO2, amorphous materials thereof, and conductive glass (transition element glass containing elements such as iron, molybdenum, vanadium, tungsten, and titanium). In addition, the material is not limited to these materials, and is not particularly limited as long as it has electronic conductivity and can be bonded to the positive electrode current collector material and the positive electrode active material.
[0072] The particle size of the material constituting the first intermediate layer 56, 16 or the second intermediate layer 57, 17 of the all-solid-state battery of this embodiment is desirably 0.05 μm or more and 5 μm or less, from the viewpoint of forming a dense layer.
[0073] The thickness of the first intermediate layer 56, 16 or the second intermediate layer 57, 17 in the all-solid-state battery of this embodiment is preferably 0.1 μm or more and 1000 μm or less, and more preferably 0.1 μm or more and 500 μm or less, from the viewpoint of obtaining a highly efficient all-solid-state battery while improving the bonding between the positive electrode collector layer 51, 11 and the positive electrode active material layer 52, 12, or between the negative electrode collector layer 53, 13 and the negative electrode active material layer 54, 14.
[0074] Moreover, the thickness of the first intermediate layer 56, 16 or the second intermediate layer 57, 17 is more preferably 0.1 μm or more and 10 μm or less.
[0075] According to this configuration, by setting the thickness of the first intermediate layer 56, 16 or the second intermediate layer 57, 17 to be 0.1 μm or more and 10 μm or less, it is possible to suppress an increase in resistance caused by providing the first intermediate layer 56, 16 which satisfactorily bonds the positive electrode current collector layer 51, 11 and the positive electrode active material layer 52, 12, or the second intermediate layer 57, 17 which satisfactorily bonds the negative electrode current collector layer 53, 13 and the negative electrode active material layer 54, 14, and to enable a more uniform electrochemical reaction, thereby enabling a further improvement in cycle characteristics.
[0076] (Conductive assistant) In the positive electrode active material layer 52, 12, the negative electrode active material layer 54, 14, the first intermediate layer 56, 16, or the second intermediate layer 57, 17 according to this embodiment, a conductive assistant may be added to improve the conductivity. The conductive assistant used in this embodiment is not particularly limited, and a well-known material may be used. The conductive assistants added to the positive electrode active material layer 52, 12, the negative electrode active material layer 54, 14, the first intermediate layer 56, 16, or the second intermediate layer 57, 17 may be the same or different.
[0077] The conductive assistant preferably has high conductivity. Therefore, for the positive electrode active material layers 52 and 12, the negative electrode active material layers 54 and 14, the first intermediate layers 56 and 16, or the second intermediate layers 57 and 17, it is preferable to use, for example, silver, palladium, a silver-palladium alloy, gold, platinum, aluminum, copper, nickel, carbon, or the like.
[0078] The particle size of the conductive additive is desirably 0.02 μm or more and 2 μm or less from the viewpoint of improving the electronic connection between the positive electrode active material, the first intermediate layer 56, 16, and the positive electrode collector layer 52, 12, or between the negative electrode active material, the second intermediate layer 57, 17, and the negative electrode collector layer 54, 14, thereby enabling high-output charging and discharging.
[0079] The ratio of the conductive assistant to be added is not particularly limited as long as the positive electrode active material or negative electrode active material contained in each of the positive electrode active material layers 52, 12 or the negative electrode active material layers 54, 14 functions electrochemically. For example, in order to obtain a higher capacity, higher output all-solid-state battery while improving the self-discharge characteristics, from the viewpoint of lowering electrical resistance, the ratio of the positive electrode active material / conductive assistant or the negative electrode active material / conductive assistant is preferably in the range of 100 / 0 to 60 / 40 by volume.
[0080] (Lithium ion conductive agent) In the positive electrode active material layer 52, 12, the negative electrode active material layer 54, 14, the first intermediate layer 56, 16, or the second intermediate layer 57, 17 according to this embodiment, a lithium ion conductive assistant may be added for the purpose of improving lithium ion conductivity. The lithium ion conductive assistant used in this embodiment is not particularly limited, and a well-known material may be used. The lithium ion conductive assistant added to the positive electrode active material layer 52, 12, the negative electrode active material layer 54, 14, the first intermediate layer 56, 16, or the second intermediate layer 57, 17 may be the same or different.
[0081] It is preferable to use a material having high lithium ion conductivity as the lithium ion conductive assistant. For example, La 0.5 Li 0.5 Perovskite compounds such as TiO3 and Li 14 Lithium-ion type compounds such as Zn(GeO4)4, Li7La3Zr2O 12 Garnet-type compounds such as LiTi2(PO4)3, LiGe2(PO4)3, LiZr2(PO4)3 (monoclinic), LiZr2(PO4)3 (rhombohedral), Li 1.5 Ca 0.5 Zr 1.5 (PO4)3, Li1.3 Al 0.3 Ti 1.7 (PO4)3 and Li 1.5 Al 0.5 Ge 1.5 (PO4)3, Li3PO4 and Li 3.5 S 0.5 P 0.5 O4 and Li 2.9 PO 3.3 N 0.46 , phosphate compounds such as lithium phosphate, Li 3.25 Ge 0.25 P 0.75 It is desirable to use at least one selected from the group consisting of thiolithium type compounds such as S4 and Li3PS4, oxides such as LiPON, lithium niobate, lithium silicate, and lithium borate, and glass compounds such as Li2S-P2S5 and Li2O-V2O5-SiO2.
[0082] From the viewpoint of improving the movement of lithium ions between the positive electrode active material and the solid electrolyte layer 55, 15 or between the negative electrode active material and the solid electrolyte layer 55, 15, the particle size of the lithium ion conductive assistant is desirably 0.02 μm or more and 2 μm or less.
[0083] The ratio of the lithium ion conductive assistant to be added is not particularly limited as long as the positive electrode active material or negative electrode active material contained in each of the positive electrode active material layers 52, 12 or the negative electrode active material layers 54, 14 functions electrochemically. For example, in order to obtain a higher capacity and higher output all-solid-state battery while improving the self-discharge characteristics, the ratio of the positive electrode active material / lithium ion conductive assistant or the negative electrode active material / lithium ion conductive assistant is preferably in the range of 100 / 0 to 60 / 40 by volume from the viewpoint of reducing internal resistance.
[0084] (Collector material) Preferred specific examples of the collector material constituting the positive electrode collector layers 51, 11 and the negative electrode collector layers 53, 13 include gold (Au), platinum (Pt), platinum (Pt)-palladium (Pd), silver (Ag), silver (Ag)-palladium (Pd), aluminum (Al), copper (Cu), nickel (Ni), and indium tin oxide (ITO).
[0085] The positive electrode collector layers 51 and 11 and the negative electrode collector layers 53 and 13 may each contain a positive electrode active material and a negative electrode active material. The content ratio of the active materials contained in each collector is not particularly limited as long as it functions as a collector. For example, the volume ratio of the positive electrode collector material / positive electrode active material or the negative electrode collector material / negative electrode active material is preferably in the range of 95 / 5 to 70 / 30.
[0086] It is preferable that the positive electrode collector layers 51, 11 and the negative electrode collector layers 53, 13 contain a positive electrode active material and a negative electrode active material, respectively, in that the adhesion between the positive electrode collector layers 51, 11 and the positive electrode active material layers 52, 12, and between the negative electrode collector layers 53, 13 and the negative electrode active material layers 54, 14 is improved and cracks are suppressed.
[0087] (Sintering aid) The type of sintering aid added to the positive electrode current collector layers 51, 11, the positive electrode active material layers 52, 12, the negative electrode current collector layers 53, 13, the negative electrode active material layers 54, 14, the solid electrolyte layers 55, 15, the first intermediate layers 56, 16, and the second intermediate layers 57, 17 constituting the all-solid-state battery 50 is not particularly limited as long as it is possible to lower the sintering temperature of each of the constituent materials, but it is preferable to use lithium compounds such as lithium carbonate, lithium hydroxide, and lithium phosphate, boron compounds such as H3BO3, and compounds consisting of lithium and boron. These materials are preferable because their compound form is unlikely to change due to water or carbon dioxide, so they can be weighed in air, and lithium and boron can be added simply and accurately.
[0088] (terminal electrode) It is preferable to use a material with high electrical conductivity for the terminal electrodes 58 of the all-solid-state battery 50. For example, silver, gold, platinum, aluminum, copper, tin, and nickel can be used. The terminal electrodes may be single-layered or multi-layered.
[0089] (Manufacturing method of all-solid-state batteries) The manufacturing method of the all-solid-state battery 50 may use a co-firing method or a sequential firing method. The co-firing method is a method of stacking materials forming each layer and baking them all at once to produce a laminate. The sequential firing method is a method of producing each layer in order, and a firing process is inserted after each layer is produced. The co-firing method can reduce the number of work steps for the all-solid-state battery 50. Below, the manufacturing method of the all-solid-state battery 50 will be described using the co-firing method as an example.
[0090] The materials constituting the all-solid-state battery 50 of this embodiment, that is, the positive electrode current collector layer 51, the positive electrode active material layer 52, the solid electrolyte layer 55, the negative electrode current collector layer 53, the negative electrode active material layer 54, the first intermediate layer 56, and the second intermediate layer 57, are made into a paste.
[0091] The method of making the paste is not particularly limited. For example, the powder of each material is mixed with a vehicle to obtain a paste. Here, the vehicle is a general term for a medium in a liquid phase. The vehicle generally includes a solvent, a dispersant, and a binder. By this method, a paste for an exterior part, a paste for a positive electrode current collector layer, a paste for a positive electrode active material layer, a paste for a solid electrolyte layer, a paste for a negative electrode current collector layer, a paste for a negative electrode active material layer, a paste for a first intermediate layer, and a paste for a second intermediate layer are prepared.
[0092] The compositions of the paste for the positive electrode current collector layer and the paste for the negative electrode current collector layer are not particularly limited, but may contain, for example, a positive electrode active material, a negative electrode active material, a solid electrolyte, and a sintering aid in addition to the current collector material.
[0093] The compositions of the paste for the positive electrode active material layer and the paste for the negative electrode active material layer are not particularly limited, but may contain, for example, a solid electrolyte, a sintering aid, a conductive aid, or a lithium ion conductive aid in addition to the positive electrode active material or the negative electrode active material.
[0094] The composition of the paste for the solid electrolyte layer is not particularly limited, but may contain, for example, a sintering aid in addition to the solid electrolyte.
[0095] The composition of the first intermediate layer paste is not particularly limited, but may contain, for example, a sintering aid, a conductive aid, and a lithium ion conductive aid in addition to the first intermediate layer material.
[0096] The composition of the second intermediate layer paste is not particularly limited, but may contain, for example, a sintering aid, a conductive aid, and a lithium ion conductive aid in addition to the second intermediate layer material.
[0097] The prepared paste for solid electrolyte layer is applied to a substrate such as PET (polyethylene terephthalate) in a desired order, and dried as necessary to obtain a green sheet for solid electrolyte layer. The method for applying the paste is not particularly limited, and known methods such as screen printing, application, transfer, doctor blade, etc. can be used.
[0098] The cathode active material layer paste, the first intermediate layer paste, and the cathode current collector layer paste are screen-printed in a predetermined order on the prepared solid electrolyte layer green sheet or exterior green sheet to form the cathode active material layer, the first intermediate layer, and the cathode current collector layer, thereby preparing the cathode layer green sheet. In some cases, the screen may be changed to one with a pattern that is not printed on the printed cathode active material layer, the first intermediate layer, and the cathode current collector layer, and the solid electrolyte layer paste may be printed on the unprinted portion of the cathode layer green sheet.
[0099] Similarly, for the negative electrode, the negative electrode active material layer paste, the second intermediate layer paste, and the negative electrode current collector layer paste are screen-printed in a predetermined order on the prepared solid electrolyte layer green sheet or exterior green sheet to form the negative electrode active material layer, the second intermediate layer, and the negative electrode current collector layer, and the negative electrode layer green sheet is prepared. In some cases, the screen may be changed to one with a pattern that is not printed on the printed negative electrode active material layer, the second intermediate layer, and the negative electrode current collector layer, and the solid electrolyte layer paste may be printed on the unprinted parts of the negative electrode layer green sheet.
[0100] After stacking the desired number of green sheets for the solid electrolyte layer, the prepared positive electrode layer green sheet and negative electrode layer green sheet are stacked in a desired order with a shift so that the positive electrode current collector layer of the positive electrode layer green sheet extends only on one end surface and the negative electrode current collector layer of the negative electrode layer green sheet extends only on the other surface, and then the desired number of green sheets for the solid electrolyte layer are stacked again to obtain a temporary laminate.
[0101] When preparing a parallel or series-parallel battery, it is preferable to stack the layers with alignment so that the end faces of the positive electrode active material layer and the negative electrode active material layer do not coincide with each other. The stacked structure is not limited to this.
[0102] The prepared temporary laminates are pressed together to prepare a laminate. The pressing is performed while heating, and the heating temperature is, for example, 40 to 90°C.
[0103] The obtained laminate is aligned as necessary and cut to produce laminates separated into pieces of desired dimensions. The cutting method is not limited, but may be dicing or knife cutting.
[0104] Before firing the individual laminated body, the corners may be rounded off using a dry green barrel or a wet green barrel.
[0105] When dry green barreling, it is a good idea to use abrasives such as alumina, zirconia, or resin beads.
[0106] In the case of wet green barrel, a solvent is used in addition to abrasives such as alumina, zirconia, resin beads, etc. The solvent may be, for example, ion-exchanged water, pure water, or a fluorine-based solvent.
[0107] The individual laminated body is heated and sintered, for example, under a nitrogen atmosphere, to obtain a sintered body. In the manufacture of the all-solid-state battery 50 of this embodiment, the sintering temperature is preferably in the range of 600 to 1200°C. If the temperature is less than 600°C, the sintering does not proceed sufficiently, and if the temperature exceeds 1200°C, problems such as dissolution of the collector material and changes in the structure of the positive electrode active material and the negative electrode active material occur. Furthermore, the range of 700 to 1000°C is more preferable. By setting the temperature in the range of 700 to 1000°C, it is more suitable for accelerating the sintering and reducing the manufacturing cost. The sintering time is, for example, 10 minutes to 3 hours.
[0108] The obtained sintered body may be placed in a cylindrical container together with an abrasive such as alumina or resin beads and barrel polished. This allows the corners of the sintered body to be chamfered. Alternatively, the sintered body may be polished by sandblasting. This method is preferable because it allows only specific parts to be polished.
[0109] When the terminal electrodes 58 are not formed before firing, they can be formed on the obtained sintered body by using a known method such as a sputtering method, a dipping method, a spray coating method, etc. When they are formed only on predetermined parts, they are formed by applying masking with tape, for example.
[0110] There is no limitation on the method for forming the terminal electrode 58, but specific examples of materials that can be used for the terminal electrode include gold (Au), platinum (Pt), platinum (Pt)-palladium (Pd), silver (Ag), silver (Ag)-palladium (Pd), aluminum (Al), copper (Cu), indium, and indium-tin oxide (ITO).
[0111] Also, the terminal electrodes may be formed from a thermosetting conductive paste prepared by mixing particles of the conductive material with a thermosetting resin to form a paste.
[0112] A plating film may be applied to the terminal electrode 58. The plating method and the type of film are not particularly limited, but for example, a Ni-Sn film may be formed by forming a Ni film by electroless Ni plating or electrolytic Ni plating, and then forming a Sn film by electrolytic tin plating.
[0113] Also, a coating of at least one metal such as Pt, Au, Cu, Ti, Ni, Sn, or an alloy thereof may be formed on the terminal electrodes by sputtering.
[0114] The surface of the all-solid-state battery 50 of this embodiment may be subjected to a water-repellent treatment. The method of the water-repellent treatment is not particularly limited, but for example, the surface may be formed by immersing the battery in a solution made of fluorine resin, silane resin, or the like.
[0115] A glass layer may be formed on the surface of the all-solid-state battery 50 of this embodiment. The method for forming the glass layer is not particularly limited, but the glass layer can be formed by applying a low-melting glass and performing a heat treatment at a desired temperature.
[0116] The all-solid-state battery 50 of this embodiment may be housed in a highly sealed case. The shape of the case to house the all-solid-state battery 50 is not limited, and may be a square, cylindrical, coin, card, or other shape.
[0117] The all-solid-state battery 50 of this embodiment may be coated with a resin. From the viewpoint of improving the heat resistance and moisture resistance of the coating, it is preferable to use a fluorine-based resin.
[0118] In the all-solid-state battery 50 of this embodiment, a lead may be provided on the terminal electrode. After the lead is attached, the terminal electrode may be coated with resin. This is preferable from the viewpoint of improving electrical connection with an external circuit.
[0119] The all-solid-state battery 50 of this embodiment may be resin-coated after providing leads to the terminal electrodes. This is preferable from the viewpoints of improving electrical connection with an external circuit and improving cycle characteristics by improving moisture resistance.
[0120] The all-solid-state battery 50 of this embodiment may be used in combination with other lithium ion secondary batteries, solar power generation units, wind power generation units, geothermal power generation units, piezoelectric elements, thermoelectric elements, and the like.
[0121] The above describes the embodiments of the present invention in detail with reference to the drawings. However, each configuration and combination thereof in each embodiment is merely an example, and addition, omission, substitution, and other modifications of the configuration are possible without departing from the spirit of the present invention. EXAMPLES
[0122] The present invention will be described in detail below using examples, but the present invention is not limited to these examples. Note that parts are by weight unless otherwise specified.
[0123] Example 1 (Preparation of Positive and Negative Electrode Active Materials) The positive and negative active materials were Li3V2(PO4)3 prepared by the following method. Li2CO3, V2O5, and NH4H2PO4 were used as starting materials, and were weighed out to a molar ratio of 3:2:6. They were wet-mixed in a ball mill using water as a solvent for 16 hours, and then dehydrated and dried. The obtained powder was calcined in a nitrogen-hydrogen mixed gas at 850°C for 2 hours. The calcined product was coarsely crushed, wet-pulverized in a ball mill using ethanol as a solvent for 24 hours, and then dried to obtain positive and negative active material powders. The average particle size of this powder was 0.3 μm. It was confirmed that the powder prepared was Li3V2(PO4)3 using an X-ray diffraction device.
[0124] (Preparation of Positive Electrode Active Material Paste and Negative Electrode Active Material Paste) The positive electrode active material paste and the negative electrode active material paste were prepared by adding 15 parts of ethyl cellulose as a binder and 65 parts of dihydroterpineol as a solvent to 100 parts of the prepared Li3V2(PO4)3 active material powder, and kneading and dispersing them in a hybrid mixer.
[0125] (Preparation of solid electrolyte) The solid electrolyte used was LiZr2(PO4)3 rhombohedral crystals prepared by the following method. First, LiOH·H2O, ZrO(NO3)2, and NH4(H2PO4) were weighed out in stoichiometric ratios and dissolved in water. The solutions were mixed, the pH was adjusted, and the mixture was heated to 80°C and then slowly cooled. X-ray diffraction was used to confirm that the powder produced was LiZr2(PO4)3 rhombohedral crystals. The particle size (D50) was 0.5 μm.
[0126] (Preparation of solid electrolyte layer sheet) The solid electrolyte layer sheet was prepared by adding 100 parts of the LiZr2(PO4)3 rhombohedral powder prepared above with 100 parts of ethanol and 200 parts of toluene as solvents in a ball mill and wet mixing. Then, 16 parts of polyvinyl butyral binder and 4.8 parts of benzyl butyl phthalate were further added and mixed to prepare a solid electrolyte slurry. This solid electrolyte slurry was formed into a sheet using a doctor blade method with a PET film as a substrate to obtain a solid electrolyte layer sheet with a thickness of 15 μm.
[0127] (Preparation of solid electrolyte paste) The solid electrolyte paste was prepared by adding 15 parts of ethyl cellulose as a binder and 65 parts of dihydroterpineol as a solvent to 100 parts of the LiZr2(PO4)3 rhombohedral powder prepared above, and kneading and dispersing the mixture in a hybrid mixer to prepare a positive electrode active material paste.
[0128] (Preparation of the first and second intermediate layer materials) Amorphous Li3V2(PO4)3 prepared by the following method was used as the first intermediate layer material and the second intermediate layer material. Li2CO3, V2O5, and NH4H2PO4 were used as starting materials, and were weighed out to a molar ratio of 3:2:6. They were wet-mixed in a ball mill using water as a solvent for 16 hours, and then dehydrated and dried. The obtained powder was calcined in a nitrogen-hydrogen mixed gas at 850°C for 2 hours. The calcined product was coarsely crushed, wet-pulverized in a ball mill using ethanol as a solvent for 24 hours, and then dried to obtain a positive electrode active material powder. The average particle size of this powder was 0.3 μm. It was confirmed that the prepared powder was Li3V2(PO4)3 using an X-ray diffraction device. The Li3V2(PO4)3 powder obtained was then placed in an alumina crucible and calcined in air gas at 700°C for 1 hour. The calcined product was coarsely crushed and wet-milled in a ball mill using ethanol as a solvent for 24 hours, then passed through a mesh and dried in an explosion-proof dryer. The dried powder was crushed and passed through a mesh to obtain the first and second intermediate layer materials. The average particle size of this powder was 0.1 μm. The peak of the original Li3V2(PO4)3 had disappeared from the powder produced, and no clear diffraction phenomenon was observed. It was confirmed by an X-ray diffraction device that it was amorphous Li3V2(PO4)3 powder. The composition was also confirmed by ICP emission spectroscopy.
[0129] (Preparation of first and second intermediate layer pastes) The first and second intermediate layer pastes were prepared by adding 10 parts of ethyl cellulose as a binder and 60 parts of dihydroterpineol as a solvent to 100 parts of the amorphous Li3V2(PO4)3 prepared above, and kneading and dispersing the mixture in a hybrid mixer.
[0130] (Preparation of positive and negative electrode collector pastes) To prepare the positive and negative current collector pastes, copper powder and Li3V2(PO4)3 powder were mixed in a volume ratio of 80 / 20. After mixing, 10 parts of ethyl cellulose as a binder and 50 parts of dihydroterpineol as a solvent were added, and the mixture was kneaded and dispersed using a three-roll mill to prepare the positive and negative current collector pastes.
[0131] Using these pastes, all-solid-state batteries were fabricated as follows.
[0132] (Preparation of positive electrode active material unit) On the solid electrolyte layer sheet, the positive electrode active material paste, the first intermediate layer paste, the positive electrode current collector paste, the first intermediate layer paste, and the positive electrode active material paste were printed in this order by screen printing. After printing each paste, it was dried at 80 to 100°C for 5 to 10 minutes, and then the next paste was printed. Next, the screen was changed, and the solid electrolyte paste was printed on the areas where the positive electrode active material paste, the first intermediate layer paste, and the positive electrode current collector paste were not printed, and dried at 80 to 100°C for 5 to 10 minutes. After all printing was completed, the PET film was peeled off. In this way, a positive electrode active material unit was obtained in which the positive electrode active material paste, the first intermediate layer paste, the positive electrode current collector paste, the first intermediate layer paste, the positive electrode active material paste, and the solid electrolyte paste were printed and dried on the solid electrolyte layer sheet.
[0133] (Preparation of negative electrode active material unit) On the solid electrolyte layer sheet, the negative electrode active material paste, the second intermediate layer paste, the negative electrode current collector paste, the second intermediate layer paste, and the negative electrode active material paste were printed in this order by screen printing. After printing each paste, it was dried at 80 to 100°C for 5 to 10 minutes, and then the next paste was printed. Next, the screen was changed, and the solid electrolyte paste was printed on the parts where the negative electrode active material paste, the second intermediate layer paste, and the negative electrode current collector paste were not printed, and dried at 80 to 100 ° C for 5 to 10 minutes. After all printing was completed, the PET film was peeled off. In this way, a negative electrode active material unit was obtained in which the negative electrode active material paste, the second intermediate layer paste, the negative electrode current collector paste, the first intermediate layer paste, the negative electrode active material paste, and the solid electrolyte paste were printed and dried on the solid electrolyte layer sheet.
[0134] (Preparation of Laminate) Ten solid electrolyte sheets were stacked, and 13 positive electrode active material units and 13 negative electrode active material units were stacked with the paste printed surface facing down, in the order of the positive electrode active material units and the negative electrode active material units, to form a laminate. At this time, each unit was stacked with a shift so that the positive electrode current collector paste layer of the positive electrode active material unit extended only to one end surface, and the negative electrode current collector paste layer of the negative electrode active material unit extended to the other surface. Then, ten solid electrolyte sheets were stacked. This was then subjected to a temperature of 80°C and a pressure of 1000 kgf / cm. 2 (98MPa), and then cut to produce a laminated block. The laminated block was then co-fired to obtain a sintered body. The co-fired body was heated to a firing temperature of 900°C at a rate of 200°C / hour in nitrogen, and held at that temperature for 0.5 hours. After firing, the battery was naturally cooled. The external dimensions of the battery after co-fired were 3.2mm x 2.5mm x 1.0mm.
[0135] (terminal electrode formation) Then, an InGa electrode paste was applied to each of the positive electrode collector layer and the negative electrode collector layer of the obtained sintered body, and dried. Terminal electrodes were then attached to the positive electrode collector layer and the negative electrode collector layer to produce an all-solid-state battery.
[0136] (evaluation) The chemical composition and crystal structure of the prepared solid electrolyte and exterior material were measured by the following methods.
[0137] (chemical composition) The compositions of the positive electrode active material, the negative electrode active material, the solid electrolyte, the first intermediate layer material, and the second intermediate layer material were analyzed by ICP-AES.
[0138] (Crystal structure) The crystal structures of the positive electrode active material, negative electrode active material, solid electrolyte, first intermediate layer material, and second intermediate layer material were measured and identified by powder X-ray diffraction.
[0139] (Cross-section observation) The fabricated all-solid-state battery was carefully dry-polished to the very center with abrasive paper, the abrasive debris was removed by air blowing, and then the polished surface was subjected to ion milling with Ar gas. Thereafter, the vicinity of the positive electrode current collector and the vicinity of the negative electrode current collector of the all-solid-state battery were observed using an electron microscope, with the positive electrode current collector layer, the first intermediate layer, and the positive electrode active material layer, and the negative electrode current collector layer, the second intermediate layer, and the negative electrode active material layer being in the field of view.
[0140] In the present embodiment, the bonding ratio is determined by first measuring the length of the positive electrode current collector layer and the length of the first intermediate layer in a field of view observed with an electron microscope, and then dividing the measured length of the first intermediate layer by the length of the positive electrode current collector layer. Alternatively, the length of the negative electrode current collector layer and the length of the second intermediate layer are measured, and then dividing the measured length of the second intermediate layer by the length of the negative electrode current collector layer. The bonding rate of the first intermediate layer and the bonding rate of the second intermediate layer are shown in Tables 1 and 2.
[0141] Example 2 An all-solid-state battery was produced in the same manner as in Example 1, except that the second intermediate layer was not provided.
[0142] Example 3 An all-solid-state battery was produced in the same manner as in Example 1, except that the first intermediate layer was not provided.
[0143] Example 4 An all-solid-state battery was produced in the same manner as in Example 1, except that the first intermediate layer paste and the second intermediate layer paste were prepared by adding 10 parts of ethyl cellulose as a binder and 50 parts of dihydroterpineol as a solvent to 100 parts of the amorphous Li3V2(PO4) prepared above, and kneading and dispersing the mixture in a hybrid mixer to prepare the first intermediate layer paste and the second intermediate layer paste.
[0144] Example 5 An all-solid-state battery was produced in the same manner as in Example 1, except that the first intermediate layer paste and the second intermediate layer paste were prepared by adding 15 parts of ethyl cellulose as a binder and 60 parts of dihydroterpineol as a solvent to 3,100 parts of the amorphous Li3V2(PO4) prepared above, and kneading and dispersing the mixture in a hybrid mixer to prepare the first intermediate layer paste and the second intermediate layer paste.
[0145] Example 6 An all-solid-state battery was produced in the same manner as in Example 1, except that the first intermediate layer paste and the second intermediate layer paste were prepared by adding 15 parts of ethyl cellulose as a binder and 75 parts of dihydroterpineol as a solvent to 3,100 parts of the amorphous Li3V2(PO4) prepared above, and kneading and dispersing the mixture in a hybrid mixer to prepare the first intermediate layer paste and the second intermediate layer paste.
[0146] Example 7 An all-solid-state battery was produced in the same manner as in Example 1, except that the first intermediate layer paste and the second intermediate layer paste were prepared by adding 20 parts of ethyl cellulose as a binder and 100 parts of dihydroterpineol as a solvent to 100 parts of the amorphous Li3V2(PO4)3 prepared above, and kneading and dispersing the mixture in a hybrid mixer to prepare the first intermediate layer paste and the second intermediate layer paste.
[0147] Example 8 An all-solid-state battery was produced in the same manner as in Example 1, except that the first intermediate layer paste and the second intermediate layer paste were prepared by adding 25 parts of ethyl cellulose as a binder and 150 parts of dihydroterpineol as a solvent to 3,100 parts of the amorphous Li3V2(PO4) prepared above, and kneading and dispersing the mixture in a hybrid mixer to prepare the first intermediate layer paste and the second intermediate layer paste.
[0148] Example 9 An all-solid-state battery was produced in the same manner as in Example 1, except that the first intermediate layer paste and the second intermediate layer paste were prepared by adding 30 parts of ethyl cellulose as a binder and 200 parts of dihydroterpineol as a solvent to 3,100 parts of the amorphous Li3V2(PO4) prepared above, and kneading and dispersing the mixture in a hybrid mixer to prepare the first intermediate layer paste and the second intermediate layer paste.
[0149] Example 10 An all-solid-state battery was produced in the same manner as in Example 1, except that the first intermediate layer paste and the second intermediate layer paste were prepared by adding 50 parts of ethyl cellulose as a binder and 300 parts of dihydroterpineol as a solvent to 3,100 parts of the amorphous Li3V2(PO4) prepared above, and kneading and dispersing the mixture in a hybrid mixer to prepare the first intermediate layer paste and the second intermediate layer paste.
[0150] Example 11 An all-solid-state battery was produced in the same manner as in Example 1, except that the first intermediate layer paste and the second intermediate layer paste were prepared by adding 70 parts of ethyl cellulose as a binder and 500 parts of dihydroterpineol as a solvent to 3,100 parts of the amorphous Li3V2(PO4) prepared above, and kneading and dispersing the mixture in a hybrid mixer to prepare the first intermediate layer paste and the second intermediate layer paste.
[0151] Example 12 An all-solid-state battery was produced in the same manner as in Example 1, except that the first intermediate layer paste and the second intermediate layer paste were prepared by adding 90 parts of ethyl cellulose as a binder and 700 parts of dihydroterpineol as a solvent to 3,100 parts of the amorphous Li3V2(PO4) prepared above, and kneading and dispersing the mixture in a hybrid mixer to prepare the first intermediate layer paste and the second intermediate layer paste.
[0152] Example 13 The negative electrode active material was Li4Ti5O prepared by the following method. 12 An all-solid-state battery was produced in the same manner as in Example 1, except that the above was used. Starting materials were Li2CO3 and TiO2, which were weighed out to a molar ratio of 2:5 and wet-mixed in a ball mill using water as a solvent for 16 hours, then dehydrated and dried. The resulting powder was calcined in air at 950°C for 4 hours. The calcined product was coarsely pulverized and wet-pulverized in a ball mill using ethanol as a solvent for 16 hours, then dehydrated and dried to obtain a negative electrode active material powder. The average particle size of this powder was 0.4 um. The powder produced was Li4Ti5O 12 This was confirmed using an X-ray diffraction apparatus.
[0153] Example 14 An all-solid-state battery was produced in the same manner as in Example 13, except that the second intermediate layer was not provided.
[0154] Example 15 An all-solid-state battery was produced in the same manner as in Example 13, except that the first intermediate layer was not provided.
[0155] (Example 16) An all-solid-state battery was produced in the same manner as in Example 1, except that lithium cobalt oxide manufactured by Sigma-Aldrich was used as the positive electrode active material.
[0156] (Example 17) An all-solid-state battery was produced in the same manner as in Example 16, except that the second intermediate layer was not provided.
[0157] (Example 18) An all-solid-state battery was produced in the same manner as in Example 16, except that the first intermediate layer was not provided.
[0158] (Example 19) An all-solid-state battery was produced in the same manner as in Example 1, except that LiCoPO4 produced by the following method was used as the positive electrode active material. Starting materials were Li2CO3, CoO2, and NH4H2PO4, which were weighed according to the stoichiometric ratio and wet-mixed in a ball mill using ethanol as a solvent for 16 hours, then dehydrated and dried. The resulting powder was calcined in air at 700°C for 4 hours. The calcined product was coarsely crushed and wet-pulverized in a ball mill using ethanol as a solvent for 16 hours, then dehydrated and dried to obtain a powder of the positive electrode active material. The average particle size of this powder was 0.5um. The powder produced was confirmed to be LiCoPO4 using an X-ray diffraction device.
[0159] (Example 20) An all-solid-state battery was produced in the same manner as in Example 19, except that the second intermediate layer was not provided.
[0160] Example 21 An all-solid-state battery was produced in the same manner as in Example 19, except that the first intermediate layer was not provided.
[0161] Example 22 (Preparation of the first and second intermediate layer materials) Amorphous Li3V2(PO4)3 prepared by the following method was used as the first intermediate layer material and the second intermediate layer material. Li2CO3, V2O5, and NH4H2PO4 were used as starting materials, and were weighed out to a molar ratio of 3:2:6. They were wet-mixed in a ball mill using water as a solvent for 16 hours, and then dehydrated and dried. The obtained powder was calcined in a nitrogen-hydrogen mixed gas at 850°C for 2 hours. The calcined product was coarsely crushed, wet-pulverized in a ball mill using ethanol as a solvent for 24 hours, and then dried to obtain a positive electrode active material powder. The average particle size of this powder was 0.3 μm. It was confirmed that the prepared powder was Li3V2(PO4)3 using an X-ray diffraction device. The obtained Li3V2(PO4)3 powder was then placed in an alumina crucible and calcined in air gas at 700°C for 1 hour. The calcined product was coarsely crushed and wet-pulverized in a planetary ball mill for 24 hours using ethanol as a solvent, then mesh-passed and dried in an explosion-proof dryer. The dried powder was crushed and mesh-passed to obtain a first intermediate layer material and a second intermediate layer material. The average particle size of this powder was 0.03 μm. The peak of the original Li3V2(PO4)3 had disappeared from the produced powder, and no clear diffraction phenomenon was confirmed, and it was confirmed by an X-ray diffraction device that it was amorphous Li3V2(PO4)3 powder. In addition, the composition was confirmed by ICP emission spectroscopy. A solid-state battery was produced in the same manner as in Example 1, except that the first intermediate layer material and the second intermediate layer material produced in this way were used.
[0162] (Examples 23, 24, 33, 37, and 41) (Preparation of the first and second intermediate layer materials) Amorphous Li3V2(PO4)3 prepared by the following method was used as the first intermediate layer material and the second intermediate layer material. Li2CO3, V2O5, and NH4H2PO4 were used as starting materials, and were weighed out to a molar ratio of 3:2:6. They were wet-mixed in a ball mill using water as a solvent for 16 hours, and then dehydrated and dried. The obtained powder was calcined in a nitrogen-hydrogen mixed gas at 850°C for 2 hours. The calcined product was coarsely crushed, wet-pulverized in a ball mill using ethanol as a solvent for 24 hours, and then dried to obtain a positive electrode active material powder. The average particle size of this powder was 0.3 μm. It was confirmed that the prepared powder was Li3V2(PO4)3 using an X-ray diffraction device. The obtained Li3V2(PO4)3 powder was then placed in an alumina crucible and calcined in air gas at 700°C for 1 hour. The calcined product was coarsely crushed and wet-pulverized in a planetary ball mill for 16 hours using ethanol as a solvent, then mesh-passed and dried in an explosion-proof dryer. The dried powder was crushed and mesh-passed to obtain the first intermediate layer material and the second intermediate layer material. The average particle size of this powder was 0.05 μm. The peak of the original Li3V2(PO4)3 had disappeared from the produced powder, and no clear diffraction phenomenon was confirmed, and it was confirmed by an X-ray diffraction device that it was amorphous Li3V2(PO4)3 powder. In addition, the composition was confirmed by ICP emission spectroscopy. Except for using the first intermediate layer material and the second intermediate layer material produced in this way, all-solid-state batteries were produced in the same manner as in Example 1, Example 3, Example 13, Example 16, and Example 19.
[0163] (Examples 25, 26, 34, 38, and 42) (Preparation of the first and second intermediate layer materials) Amorphous Li3V2(PO4)3 prepared by the following method was used as the first intermediate layer material and the second intermediate layer material. Li2CO3, V2O5, and NH4H2PO4 were used as starting materials, and were weighed out to a molar ratio of 3:2:6. They were wet-mixed in a ball mill using water as a solvent for 16 hours, and then dehydrated and dried. The obtained powder was calcined in a nitrogen-hydrogen mixed gas at 850°C for 2 hours. The calcined product was coarsely crushed, wet-pulverized in a ball mill using ethanol as a solvent for 24 hours, and then dried to obtain a positive electrode active material powder. The average particle size of this powder was 0.3 μm. It was confirmed that the prepared powder was Li3V2(PO4)3 using an X-ray diffraction device. The Li3V2(PO4)3 powder obtained was then placed in an alumina crucible and calcined in air gas at 700°C for 1 hour. The calcined product was coarsely crushed, and wet-milled in a ball mill using ethanol as a solvent for 18 hours, then passed through a mesh, dried in an explosion-proof dryer, and the dried powder was crushed and passed through a mesh to obtain a first intermediate layer material and a second intermediate layer material. The average particle size of this powder was 0.3 μm. The peak of the original Li3V2(PO4)3 had disappeared from the powder produced, and no clear diffraction phenomenon was confirmed, and it was confirmed by an X-ray diffraction device that it was amorphous Li3V2(PO4)3 powder. In addition, the composition was confirmed by ICP emission spectroscopy. Except for using the first intermediate layer material and the second intermediate layer material produced in this way, all-solid-state batteries were produced in the same manner as in Example 1, Example 2, Example 13, Example 16, and Example 19.
[0164] (Examples 27 and 28) (Preparation of the first and second intermediate layer materials) Amorphous Li3V2(PO4)3 prepared by the following method was used as the first intermediate layer material and the second intermediate layer material. Li2CO3, V2O5, and NH4H2PO4 were used as starting materials, and were weighed out to a molar ratio of 3:2:6. They were wet-mixed in a ball mill using water as a solvent for 16 hours, and then dehydrated and dried. The obtained powder was calcined in a nitrogen-hydrogen mixed gas at 850°C for 2 hours. The calcined product was coarsely crushed, wet-pulverized in a ball mill using ethanol as a solvent for 24 hours, and then dried to obtain a positive electrode active material powder. The average particle size of this powder was 0.3 μm. It was confirmed that the prepared powder was Li3V2(PO4)3 using an X-ray diffraction device. The Li3V2(PO4)3 powder obtained was then placed in an alumina crucible and calcined in air gas at 700°C for 1 hour. The calcined product was coarsely crushed, and wet-milled in a ball mill using ethanol as a solvent for 16 hours, then passed through a mesh, dried in an explosion-proof dryer, and the dried powder was crushed and passed through a mesh to obtain a first intermediate layer material and a second intermediate layer material. The average particle size of this powder was 0.5 μm. The peak of the original Li3V2(PO4)3 had disappeared from the powder produced, and no clear diffraction phenomenon was confirmed, and it was confirmed by an X-ray diffraction device that it was amorphous Li3V2(PO4)3 powder. In addition, the composition was confirmed by ICP emission spectroscopy. Except for using the first intermediate layer material and the second intermediate layer material produced in this way, an all-solid-state battery was produced in the same manner as in Example 1 and Example 3.
[0165] (Examples 29, 35, 39, and 43) (Preparation of the first and second intermediate layer materials) Amorphous Li3V2(PO4)3 prepared by the following method was used as the first intermediate layer material and the second intermediate layer material. Li2CO3, V2O5, and NH4H2PO4 were used as starting materials, and were weighed out to a molar ratio of 3:2:6. They were wet-mixed in a ball mill using water as a solvent for 16 hours, and then dehydrated and dried. The obtained powder was calcined in a nitrogen-hydrogen mixed gas at 850°C for 2 hours. The calcined product was coarsely crushed, wet-pulverized in a ball mill using ethanol as a solvent for 24 hours, and then dried to obtain a positive electrode active material powder. The average particle size of this powder was 0.3 μm. It was confirmed that the prepared powder was Li3V2(PO4)3 using an X-ray diffraction device. The obtained Li3V2(PO4)3 powder was then placed in an alumina crucible and calcined in air gas at 700°C for 1 hour. The calcined product was coarsely crushed and wet-pulverized in a ball mill using ethanol as a solvent for 12 hours, then mesh-passed and dried in an explosion-proof dryer. The dried powder was crushed and mesh-passed to obtain the first intermediate layer material and the second intermediate layer material. The average particle size of this powder was 1 μm. The peak of the original Li3V2(PO4)3 had disappeared from the produced powder, and no clear diffraction phenomenon was confirmed, and it was confirmed by an X-ray diffraction device that it was amorphous Li3V2(PO4)3 powder. In addition, the composition was confirmed by ICP emission spectroscopy. Except for using the first intermediate layer material and the second intermediate layer material produced in this way, all-solid-state batteries were produced in the same manner as in Example 1, Example 13, Example 16, and Example 19.
[0166] (Example 30) (Preparation of the first and second intermediate layer materials) Amorphous Li3V2(PO4)3 prepared by the following method was used as the first intermediate layer material and the second intermediate layer material. Li2CO3, V2O5, and NH4H2PO4 were used as starting materials, and were weighed out to a molar ratio of 3:2:6. They were wet-mixed in a ball mill using water as a solvent for 16 hours, and then dehydrated and dried. The obtained powder was calcined in a nitrogen-hydrogen mixed gas at 850°C for 2 hours. The calcined product was coarsely crushed, wet-pulverized in a ball mill using ethanol as a solvent for 24 hours, and then dried to obtain a positive electrode active material powder. The average particle size of this powder was 0.3 μm. It was confirmed that the prepared powder was Li3V2(PO4)3 using an X-ray diffraction device. The obtained Li3V2(PO4)3 powder was then placed in an alumina crucible and calcined in air gas at 700°C for 1 hour. The calcined product was coarsely crushed and wet-pulverized in a ball mill using ethanol as a solvent for 8 hours, then passed through a mesh, dried in an explosion-proof dryer, and the dried powder was crushed and passed through a mesh to obtain a first intermediate layer material and a second intermediate layer material. The average particle size of this powder was 2 μm. The peak of the original Li3V2(PO4)3 had disappeared from the produced powder, and no clear diffraction phenomenon was confirmed, and it was confirmed by an X-ray diffraction device that it was amorphous Li3V2(PO4)3 powder. In addition, the composition was confirmed by ICP emission spectroscopy. A solid-state battery was produced in the same manner as in Example 1, except that the first intermediate layer material and the second intermediate layer material produced in this way were used.
[0167] (Example 31) (Preparation of the first and second intermediate layer materials) Amorphous Li3V2(PO4)3 prepared by the following method was used as the first intermediate layer material and the second intermediate layer material. Li2CO3, V2O5, and NH4H2PO4 were used as starting materials, and were weighed out to a molar ratio of 3:2:6. They were wet-mixed in a ball mill using water as a solvent for 16 hours, and then dehydrated and dried. The obtained powder was calcined in a nitrogen-hydrogen mixed gas at 850°C for 2 hours. The calcined product was coarsely crushed, wet-pulverized in a ball mill using ethanol as a solvent for 24 hours, and then dried to obtain a positive electrode active material powder. The average particle size of this powder was 0.3 μm. It was confirmed that the prepared powder was Li3V2(PO4)3 using an X-ray diffraction device. The obtained Li3V2(PO4)3 powder was then placed in an alumina crucible and calcined in air gas at 700°C for 1 hour. The calcined product was coarsely crushed, and wet-milled in a ball mill using ethanol as a solvent for 6 hours, then passed through a mesh, dried in an explosion-proof dryer, and the dried powder was crushed and passed through a mesh to obtain a first intermediate layer material and a second intermediate layer material. The average particle size of this powder was 3 μm. The peak of the original Li3V2(PO4)3 had disappeared from the produced powder, and no clear diffraction phenomenon was confirmed, and it was confirmed by an X-ray diffraction device that it was amorphous Li3V2(PO4)3 powder. In addition, the composition was confirmed by ICP emission spectroscopy. A solid-state battery was produced in the same manner as in Example 1, except that the first intermediate layer material and the second intermediate layer material produced in this way were used.
[0168] (Examples 32, 36, 40, and 44) (Preparation of the first and second intermediate layer materials) Amorphous Li3V2(PO4)3 prepared by the following method was used as the first intermediate layer material and the second intermediate layer material. Li2CO3, V2O5, and NH4H2PO4 were used as starting materials, and were weighed out to a molar ratio of 3:2:6. They were wet-mixed in a ball mill using water as a solvent for 16 hours, and then dehydrated and dried. The obtained powder was calcined in a nitrogen-hydrogen mixed gas at 850°C for 2 hours. The calcined product was coarsely crushed, wet-pulverized in a ball mill using ethanol as a solvent for 24 hours, and then dried to obtain a positive electrode active material powder. The average particle size of this powder was 0.3 μm. It was confirmed that the prepared powder was Li3V2(PO4)3 using an X-ray diffraction device. The obtained Li3V2(PO4)3 powder was then placed in an alumina crucible and calcined in air gas at 700°C for 1 hour. The calcined product was coarsely crushed and wet-pulverized in a ball mill using ethanol as a solvent for 4 hours, then mesh-passed and dried in an explosion-proof dryer. The dried powder was crushed and mesh-passed to obtain the first intermediate layer material and the second intermediate layer material. The average particle size of this powder was 5 μm. The peak of the original Li3V2(PO4)3 had disappeared from the produced powder, and no clear diffraction phenomenon was confirmed, and it was confirmed by an X-ray diffraction device that it was amorphous Li3V2(PO4)3 powder. In addition, the composition was confirmed by ICP emission spectroscopy. Except for using the first intermediate layer material and the second intermediate layer material produced in this way, all-solid-state batteries were produced in the same manner as in Example 1, Example 13, Example 16, and Example 19.
[0169] Comparative Example 1 An all-solid-state battery was produced in the same manner as in Example 1, except that the first intermediate layer and the second intermediate layer were not provided.
[0170] Comparative Example 2 An all-solid-state battery was produced in the same manner as in Example 13, except that the first intermediate layer and the second intermediate layer were not provided.
[0171] Comparative Example 3 An all-solid-state battery was produced in the same manner as in Example 16, except that the first intermediate layer and the second intermediate layer were not provided.
[0172] Comparative Example 4 An all-solid-state battery was produced in the same manner as in Example 19, except that the first intermediate layer and the second intermediate layer were not provided.
[0173] (Cycle characteristic evaluation) The terminal electrodes of the all-solid-state batteries produced in Examples 1 to 44 and Comparative Examples 1 to 4 were attached to a jig of the type that is fixed with a spring pin.
[0174] The all-solid-state batteries of Examples 1 to 12, 22 to 32, and Comparative Example 1 were charged at a constant current of 1 μA to a cut-off voltage of 2.6 V, and then discharged at a constant current of 1 μA to a cut-off voltage of 0 V. This was repeated for 100 cycles. The capacity retention rate after 100 cycles was measured to evaluate the cycle characteristics. The capacity retention rate was calculated as 1-(discharge capacity after 100 cycles / discharge capacity after 1 cycle)×100.
[0175] The all-solid-state batteries of Examples 13 to 15, 33 to 36, and Comparative Example 2 were charged at a constant current of 1 μA to a cut-off voltage of 2.8 V, and then discharged at a constant current of 1 μA to a cut-off voltage of 1.8 V. This was repeated for 100 cycles. The capacity retention rate after 100 cycles was measured to evaluate the cycle characteristics.
[0176] The all-solid-state batteries of Examples 16 to 18, 37 to 40, and Comparative Example 3 were charged at a constant current of 1 μA to a cut-off voltage of 2.8 V, and then discharged at a constant current of 1 μA to a cut-off voltage of 1.9 V. This was repeated for 100 cycles. The capacity retention rate after 100 cycles was measured to evaluate the cycle characteristics.
[0177] The all-solid-state batteries of Examples 19 to 21, 41 to 44, and Comparative Example 4 were charged at a constant current of 1 μA to a cut-off voltage of 3.2 V, and then discharged at a constant current of 1 μA to a cut-off voltage of 2.5 V. This was repeated for 100 cycles. The capacity retention rate after 100 cycles was measured to evaluate the cycle characteristics.
[0178] Tables 1 and 2 show the joining rates and capacity maintenance rates for Examples 1 to 44 and Comparative Examples 1 to 4.
[0179] [Table 1]
[0180] [Table 2]
[0181] The all-solid-state batteries produced in Examples 1 to 44 exhibited high capacity retention rates, and all-solid-state batteries having high cycle characteristics were obtained. On the other hand, a significant decrease in capacity retention rates was confirmed in the all-solid-state batteries produced in Comparative Examples 1 to 4. [Industrial Applicability]
[0182] As described above, the all-solid-state battery according to the present invention is effective in improving cycle characteristics. Providing an all-solid-state battery with improved cycle characteristics will greatly contribute, particularly in the fields of energy and electronics. [Explanation of symbols]
[0183] 50: All-solid-state battery 51: Positive electrode current collector layer 52: Positive electrode active material layer 53: Negative electrode current collector layer 54: Negative electrode active material layer 55: Solid electrolyte layer 56: First middle layer 57: Second middle class 58:Terminal electrode 10: Power storage unit 11: Positive electrode current collector layer 12: Positive electrode active material layer 13: Negative electrode current collector layer 14: Negative electrode active material layer 15: Solid electrolyte layer 16: First middle layer 17: Second middle layer
Claims
1. a positive electrode current collector layer, a positive electrode active material layer, a negative electrode current collector layer, a negative electrode active material layer, and a solid electrolyte layer made of a solid electrolyte and disposed between the positive electrode active material layer and the negative electrode active material layer; at least one of a first intermediate layer formed between the positive electrode current collector layer and the positive electrode active material layer and a second intermediate layer formed between the negative electrode current collector layer and the negative electrode active material layer, At least one of the first intermediate layer and the second intermediate layer contains a constituent material containing at least an anion, At least one of the first intermediate layer and the second intermediate layer is an amorphous material containing at least two or more elements selected from the group consisting of Li, V, Si, Al, Ge, Sb, Sn, Ga, In, Fe, Co, Ni, Ti, Mn, Ca, Ba, La, Zr, Ce, Cu, Mg, Sr, Cr, Mo, Nb, Zn, and P; At least one of the first intermediate layer and the second intermediate layer is made of lithium vanadium phosphate (Li3V2(PO4)3 or LiVOPO4), olivine type LiMbPO4 (wherein Mb is one or more elements selected from Co, Ni, Mn, Fe, Mg, Nb, Ti, Al, and Zr), lithium cobalt oxide (LiCoO2), or lithium manganese composite oxide Li2M nx3Ma1-x3O3 (0.8≦x3≦1, Ma=Co, Ni), lithium nickel oxide (LiNiO2), lithium manganese spinel (LiMn2O4), composite metal oxides represented by the general formula: LiNix4Coy4Mnz4O2 (x4+y4+z4=1, 0≦x4≦1, 0≦y4≦1, 0≦z4≦1), lithium vanadium compounds (LiV2O5), Li-excess solids Li2MnO3-LiMcO2 (Mc = Mn, Co, Ni), lithium titanate (Li4Ti5O12), complex metal oxide represented by LiaNix5Coy5Alz5O2 (0.9 < a < 1.3, 0.9 < x5 + y5 + z5 < 1.1), La0.5Li0.5TiO3, Li14Zn(GeO4)4, Li7La3Zr2O12, LiTi2(PO4)3, Li An all-solid-state battery comprising Ge2(PO4)3, LiZr2(PO4)3, LiZr2(PO4)3, Li1.5Ca0.5Zr1.5(PO4)3, Li1.3Al0.3Ti1.7(PO4)3, Li1.5Al0.5Ge1.5(PO4)3, Li3.5Si0.5P0.5O4, Li3.25Ge0.25P0.75S4, or Li2O-V2O5-SiO2.
2. 2. The all-solid-state battery according to claim 1, wherein a bonding rate of the first intermediate layer or the second intermediate layer to the positive electrode current collector layer or the negative electrode current collector layer is greater than 1%.
3. The all-solid-state battery according to claim 2 , wherein the bonding rate is greater than 30%.
4. The all-solid-state battery according to any one of claims 1 to 3, wherein the first intermediate layer or the second intermediate layer is amorphous.
5. The all-solid-state battery according to any one of claims 1 to 4, wherein the first intermediate layer or the second intermediate layer has a thickness of 0.1 µm or more and 10 µm or less.
Citation Information
Patent Citations
Farm machine
JP1980012293A
Electrode plate for secondary battery
JP2003272610A
Lithium battery
JP2009032597A
Lithium battery
JP2009170183A
Method of manufacturing solid electrolyte battery, and solid electrolyte battery
JP2010251113A