Yellow pigment composition
Stabilizing bismuth vanadate pigments in thermoplastic molding compositions with ethylene and (meth)acrylic acid or maleic anhydride copolymers addresses thermal degradation, enhancing stability and color performance in polyamide-based materials.
Patent Information
- Application Number
- JP2021560081
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-04-11
- Filing Date
- 2020-04-07
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2040-04-07
AI Technical Summary
Existing bismuth vanadate pigments in thermoplastic molding compositions, particularly polyamide-containing ones, suffer from thermal degradation issues due to the absence of boric acid stabilization, leading to insufficient thermal stability.
A bismuth vanadate pigment composition is stabilized by dispersing it in a copolymer with ethylene and (meth)acrylic acid or maleic anhydride, which enhances thermal stability during compounding and processing.
The composition achieves stable thermal degradation resistance, improving color stability and performance in thermoplastic polymers, especially in injection molding applications.
Smart Images

Figure 0007553464000002 
Figure 0007553464000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a yellow pigment composition, to its use as a colorant in a thermoplastic polymer composition, to a corresponding thermoplastic molding composition, to its use for producing a fiber, a foil or a molding, and to the respective fiber, foil or molding. [Background technology]
[0002] Yellow inorganic and / or organic pigments can be used to obtain thermoplastic molding compositions. An example of an organic yellow pigment is the monoazo-ca-pigment BAYPLAST® Yellow G Gran. The inorganic yellow pigment bismuth vanadate is often used in the form of a masterbatch of bismuth vanadate stabilized against thermal degradation by adding boric acid. Typical commercial bismuth vanadate pigments are encapsulated with silicates or alumina. This encapsulation does not provide sufficient stability against thermal degradation, especially in polyamide molding compositions intended for injection molding.
[0003] Preferably, boric acid should no longer be used in thermoplastic molding compositions, so there is a need for alternative bismuth vanadate masterbatches that are stable against thermal degradation of the pigment. Simply excluding boric acid has not been successful because of the short thermal degradation that occurs. Summary of the Invention [Problem to be solved by the invention]
[0004] The object underlying the present invention is to provide a bismuth vanadate pigment composition which can be used as a masterbatch for pigmenting thermoplastic molding compositions, in particular polyamide-containing thermoplastic molding compositions, which do not contain boric acid or boron compounds and which are stable towards thermal degradation. [Means for solving the problem]
[0005] According to the invention, the object is to provide a copolymer of ethylene, (meth)acrylic acid, C 1~12 This is achieved by a pigment composition C comprising a bismuth vanadate pigment dispersed in a copolymer with at least one comonomer selected from the group consisting of alkyl (meth)acrylates and maleic anhydride. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0006] According to the present invention, the bismuth vanadate pigment is a copolymer of ethylene, (meth)acrylic acid, C 1~12 It has been found that the pigment composition can be stably dispersed in a copolymer with at least one comonomer selected from the group consisting of -alkyl (meth)acrylates and maleic anhydride, and that the resulting pigment composition is stable against thermal degradation during storage, during incorporation into thermoplastic polymers, and during processing of the thermoplastic polymers, for example to obtain molded articles by injection molding.
[0007] Simply omitting the boric acid from known bismuth vanadate masterbatches has not been successful because bismuth vanadate pigments suffer from rapid thermal degradation.
[0008] Also, the use of bismuth vanadate pigment in polyethylene masterbatches was insufficient to prevent thermal degradation.
[0009] Only by incorporating or dispersing in an ethylene copolymer having an organic acid group selected from acrylic acid, acrylate or maleic anhydride groups can a masterbatch of bismuth vanadate be obtained with the desired thermal stability. According to the invention, it has been found that the color stability of the bismuth vanadate pigment can be significantly improved by adding, in particular, an ethylene copolymer containing maleic anhydride. Preferably, a masterbatch is prepared from the bismuth vanadate pigment and the copolymer, which is then used as a colorant in compounding or injection molding the thermoplastic molding composition. It is also possible to directly compound the bismuth vanadate pigment and the copolymer as separate compounds to prepare the pigment composition or the thermoplastic molding composition.
[0010] Bismuth vanadate is an inorganic compound with the formula BiVO4. It is a bright yellow solid that is a representative of complex inorganic color pigments (CICPs). More specifically, bismuth vanadate is a mixed metal oxide. Bismuth vanadate is also known as CI Pigment Yellow 184 in the Colour Index® International. When used as a pigment, it has high saturation and good hiding power. In nature, bismuth vanadate can be found as the minerals pukerite, clinobisvanite, and dryerite, depending on the particular polymorph formed.
[0011] Bismuth vanadate pigments are typically based on pure bismuth vanadate with monoclinic (clinobisvanite) or tetragonal (dolerylite) structure. They can be formed from a series of pH-controlled precipitation reactions (it is important to note that these reactions can be carried out in the presence or absence of molybdenum depending on the final phase desired). It is also possible to start with the parent oxides (Bi2O3 and V2O5) and perform high temperature calcinations to obtain the pure product.
[0012] The bismuth vanadate pigments can be coated with aluminum and / or silica.
[0013] A typical pigment composition according to the present invention preferably comprises bismuth vanadate in an amount of 5 to 60% by weight, more preferably 10 to 50% by weight, and most preferably 20 to 40% by weight, based on the amount of pigment composition.
[0014] Similarly, the amount of copolymer may be preferably from 5 to 60% by weight, more preferably from 10 to 50% by weight, and most preferably from 20 to 40% by weight.
[0015] The copolymer preferably contains 50-97% by weight, more preferably 60-95% by weight, and most preferably 70-90% by weight of ethylene, based on the total weight of the copolymer. The comonomers are preferably acrylic acid, C 1~6 - alkyl acrylate, maleic anhydride, or a mixture thereof.
[0016] Particularly preferred is the use of a copolymer of ethylene with acrylate, acrylic acid and maleic anhydride. In particular, preferred is the use of a copolymer of ethylene, n-butyl acrylate, acrylic acid and maleic anhydride. A suitable copolymer is available as Lupolen® KR 1270 from BASF SE. This copolymer is typically used in polyamide compositions as an impact-modifying polymer, see for example US 8,629,206 B2 and US 2016 / 0130381 A1.
[0017] The copolymer containing carboxylic acid groups can be used alone to prepare the pigment composition of the present invention, in which case the pigment composition consists of the bismuth vanadate pigment and the acid group-containing copolymer as the matrix polymer.
[0018] It is also possible to add further polymers to the pigment composition, preferably polyolefins. The polyolefins are preferably polyethylene, polypropylene or ethylene with at least one C as a comonomer. 3~12 -olefins. This copolymer should be different from the above copolymers containing carboxylic acid groups. Preferably, this further polymer is a copolymer of (meth)acrylic acid, C 1~12 - Free of alkyl (meth)acrylate and maleic anhydride comonomers.
[0019] Depending on the polyolefinic nature, this further (co)polymer can be homogeneously mixed with the copolymer described above. Among these further polyolefins, preferred are polyethylene, polypropylene or ethylene / propylene copolymers. Polyethylene is the most preferred.
[0020] The mass ratio of this polyolefin to the above copolymer is preferably in the range of 3:1 to 1:3, more preferably 2:1 to 1:2, and most preferably 1:1 to 5:3.
[0021] A preferred pigment composition C is 5 to 60% by mass, preferably 10 to 50% by mass, more preferably 20 to 40% by mass of bismuth vanadate as component C1; As component C2, 5 to 60 mass%, preferably 10 to 50 mass%, more preferably 20 to 40 mass% of ethylene and (meth)acrylic acid, C 1~12 - copolymers with at least one comonomer selected from the group consisting of alkyl (meth)acrylates and maleic anhydride, As component C3, 10 to 70 mass%, preferably 20 to 60 mass%, more preferably 30 to 50 mass% of polyethylene, polypropylene, or ethylene and at least one C as a comonomer. 3~12 - copolymers with olefins different from component C2, 0 to 10% by weight, preferably 0 to 5% by weight, more preferably 0 to 2% by weight of further components as component C4, wherein the total amount of components C1 to C4 is 100 mass %.
[0022] The further component C4 may be a further colorant, for example an organic pigment, in particular a yellow organic pigment, for example BAYPLAST® Yellow G. Additional further components may be commonly used adjuvants.
[0023] The pigment composition C can be used as a colorant in thermoplastic polymer compositions. These thermoplastic polymer compositions can be based on typical thermoplastic polymers that can be injection molded. Preferably, the thermoplastic polymer contains at least one polyamide. More preferably, in the thermoplastic polymer composition, the majority of the polymer is a polyamide, in particular an aliphatic polyamide.
[0024] A preferred thermoplastic molding composition comprises a thermoplastic polymer and a pigment composition in an amount such that the bismuth vanadate content of the thermoplastic molding composition is in the range of 0.1 to 2.0% by weight, preferably 0.2 to 1.0% by weight, more preferably 0.3 to 0.5% by weight.
[0025] The polymer in which the pigment composition is contained can be selected from any desired suitable polymer, including, for example, polyamides, polyesters, polycarbonates, polyethers, polyurethanes, polysulfones, polyolefins, or blends of polymers made of two or more of these.
[0026] The present invention also provides a method for producing a semiconductor device comprising the steps of: as component A, 30 to 95% by weight of at least one, for example aliphatic, polyamide or copolyamide, Component B: 0 to 50 mass% glass fiber; as component C, 0.2 to 7% by weight of a pigment composition as defined above, as component D, 0 to 2% by weight of at least one organic pigment, As component E, 0 to 50% by weight of further additives It also relates to a thermoplastic molding composition comprising Here, the total amount of components A to E is 100 mass %.
[0027] The thermoplastic molding composition preferably has a bismuth vanadate content of 0.1 to 2.0% by weight, more preferably 0.2 to 1.0% by weight, most preferably 0.3 to 0.5% by weight.
[0028] It is particularly preferred that component A comprises a polyamide or copolyamide present in an amount of from 30 to 95% by weight, preferably from 40 to 89.5% by weight, more preferably from 26 to 74% by weight.
[0029] The polyamides preferably used in the present invention are prepared by reaction of starting monomers selected from, for example, dicarboxylic acids and diamines, or salts of dicarboxylic acids and diamines, aminocarboxylic acids, aminonitriles, lactams, and mixtures thereof. Any desired starting monomers of aliphatic polyamides can be included here. The polyamides can be amorphous, crystalline, or semi-crystalline. Furthermore, the polyamides can have any desired suitable viscosity and respective molecular weight. Particularly suitable polyamides have any type of aliphatic, semi-crystalline, or semi-aromatic, or amorphous structure.
[0030] The intrinsic viscosity of these polyamides is generally between 90 and 350 ml / g, preferably between 110 and 240 ml / g, determined according to ISO 307 in a 0.5% by weight solution in 96% by weight sulfuric acid at 25° C.
[0031] Semicrystalline or amorphous resins having a molecular weight (weight average) of at least 5000 are preferred, and are described, for example, in the following U.S. Patents Nos. 2,071,250, 2,071,251, 2,130,523, 2,130,948, 2,241,322, 2,312,966, 2,512,606 and 3,393,210. Examples of these are polyamides derived from lactams having 7 to 11 ring members, such as polycaprolactam and polycapryllactam, and also polyamides obtained by reaction of dicarboxylic acids with diamines.
[0032] Dicarboxylic acids which can be used are alkanedicarboxylic acids having 6 to 12, in particular 6 to 10, carbon atoms, and aromatic dicarboxylic acids, examples of which include adipic acid, azelaic acid, sebacic acid and dodecanedioic acid (=decanedicarboxylic acid).
[0033] Particularly suitable diamines are alkanediamines having 2 to 12, in particular 6 to 8, carbon atoms, and also di(4-aminocyclohexyl)methane or 2,2-di(4-aminocyclohexyl)propane.
[0034] The preferred polyamides and copolyamides are aliphatic.
[0035] Preferred polyamides are polyhexamethylene adipamide (PA 66) and polyhexamethylene sebacamide (PA 610), polycaprolactam (PA 6), and also nylon-6 / 6,6 copolyamide, in particular with a proportion of caprolactam units between 5 and 95% by weight. PA 6, PA 66 and nylon-6 / 6,6 copolyamide are particularly preferred.
[0036] Mention may also be made, for example, of polyamides obtainable by condensation of 1,4-diaminobutane with adipic acid at high temperature (nylon-4,6). Methods for the preparation of polyamides having this structure are described, for example, in EP-A 38 094, EP-A 38 582 and EP-A 39 524.
[0037] Other examples include polyamides obtainable by copolymerization of two or more of the abovementioned monomers, and mixtures of several polyamides in any desired mixing ratio.
[0038] The following non-exhaustive list includes the polyamides mentioned above, and also other polyamides for the purposes of the present invention (monomers are listed between brackets): PA 26 (Ethylenediamine, Adipic Acid) PA 210 (Ethylenediamine, Sebacic acid) PA 46 (Tetramethylenediamine, adipic acid) PA 66 (Hexamethylenediamine, Adipic Acid) PA 69 (Hexamethylenediamine, Azelaic acid) PA 610 (Hexamethylenediamine, Sebacic acid) PA 612 (Hexamethylenediamine, Decanedicarboxylic acid) PA 613 (Hexamethylenediamine, Undecanedicarboxylic acid) PA 1212 (1,12-dodecanediamine, decanedicarboxylic acid) PA 1313 (1,13-diaminotridecane, undecanedicarboxylic acid) PA 4 (Pyrrolidone) PA 6 (ε-caprolactam) PA 7 (ethanolactam) PA 8 (Capryllactam) PA9 (9-aminononanoic acid) PA11 (11-aminoundecanoic acid) PA12 (Laurolactam).
[0039] These polyamides and their preparation are known. Details concerning their preparation can be found by the skilled artisan in Ullmanns Enzyklopaedie der Technischen Chemie [Ullmann's Encyclopedia Of Industrial Chemistry], 4th edition, volume 19, pages 39-54, Verlag Chemie, Weinheim, 1980, and also in Ullmann's Encyclopedia of Industrial Chemistry, volume A21, pages 179-206, VCH Verlag, Weinheim 1992, and also in Stoeckhert, Kunststoff Lexikon [Plastics Encyclopedia], pages 425-428, Hanser Verlag, Munich 1992 (see the keyword "Polyamides").
[0040] Particularly preferably, nylon-6 or nylon-6,6 is used.
[0041] Furthermore, in the present invention, it is possible to provide the polyamide with functionalizing compounds, which can be bonded to the carboxy or amino groups, for example having at least one carboxy, hydroxy or amino group. These are preferably monomers with branching effect, for example having at least three carboxy or amino groups, such as monomers that can be bonded to the carboxy or amino groups by epoxy groups, hydroxy groups, isocyanato groups, amino and / or carboxy groups, and have functional groups selected from hydroxy groups, ether groups, ester groups, amide groups, imine groups, imide groups, halogen groups, cyano groups, nitro groups, CC double bonds or CC triple bonds, or polymer blocks that can be bonded to the carboxy or amino groups.
[0042] By using functionalizing compounds, the property profile of the resulting polyamide can be tailored within wide limits as desired.
[0043] For example, triacetonediamine compounds can be used as functionalized monomers. These preferably include 4-amino-2,2,6,6-tetramethylpiperidine or 4-amino-1-alkyl-2,2,6,6-tetramethylpiperidines, the alkyl groups of which have 1 to 18 carbon atoms or are substituted by benzyl groups. The amount of triacetonediamine compounds present is preferably 0.03 to 0.8 mol %, particularly preferably 0.06 to 0.4 mol %, in each case based on amide groups of one mole of polyamide. For further details, reference can be made to DE-A-44 13 177.
[0044] As component B, the thermoplastic molding composition may contain glass fibres. If present, the amount of glass fibres is preferably 5-50% by weight, more preferably 10-40% by weight, most preferably 25-35% by weight. Any desired suitable glass fibres can be used in the form of chopped glass or in the form of rovings. The chopped glass fibres preferably have a diameter of about 10 μm. The glass fibres can be surface treated, for example silanized. The simultaneous use of glass fibres is particularly advantageous.
[0045] Component C is as described above. The amount of component C is preferably 0.3 to 5.0% by mass, and more preferably 0.5 to 2.0% by mass.
[0046] When component D is present, it is preferably used in an amount of 0.1 to 2.0% by weight, more preferably 0.2 to 1.0% by weight, and most preferably 0.3 to 0.5% by weight, based on the total amount of components A to E. The at least one organic pigment is preferably at least one yellow organic pigment. If such a pigment is already present as part of component C, e.g., component C4, component D is not present.
[0047] The thermoplastic molding composition of the invention may contain 0 to 50% by weight, preferably 0 to 30% by weight, more preferably 0 to 20% by weight, of further additives as component E. Said additives may include other fillers, stabilizers, oxidation retardants, protection agents against thermal and UV degradation, flame retardants, lubricants and release agents, colorants such as dyes and pigments, nucleating agents, plasticizers, etc. For details of usable additives, reference may also be made to pages 31 to 37 of WO 2008 / 074687.
[0048] Most preferably, 0.1 to 20% by weight of component E is present (the amount of component A is reduced accordingly), where component E comprises a stabilizer and a lubricant. For example, zinc oxide can be used as a stabilizer and calcium stearate as a lubricant. Conventional polyamide molding composition antioxidants can be used, for example those sold under the trademark Irganox® by BASF SE.
[0049] The phosphorus-containing organic polymers can be used as (part of) component E, alone or in combination with other flame retardant materials and synergists.
[0050] Other flame retardant materials include, for example, red phosphorus, cyclic phenoxyphosphazenes having at least a phenoxyphosphazene unit, or (di)phosphinates.
[0051] It is further possible to use reaction products of melamine with phosphoric acid or to use metal borates.
[0052] Preferred reaction products of melamine with phosphoric acid are those obtained by reacting essentially equimolar amounts of melamine or condensates of melamine with phosphoric acid, pyrophosphoric acid or polyphosphoric acid in a suitable process. It is particularly preferred to use melamine polyphosphate, which can be obtained by condensing melamine phosphate by heating under nitrogen. The general formula of melamine polyphosphate is (C3H6N6HPO3) n It is.
[0053] The phosphoric acid component in the melamine phosphate can be, for example, orthophosphoric acid, phosphorous acid, hypophosphorous acid, metaphosphoric acid, pyrophosphoric acid, triphosphoric acid or tetraphosphoric acid. Particularly preferred are melamine polyphosphates obtained by condensing an adduct of orthophosphoric acid or pyrophosphoric acid with melamine. The degree of condensation of the melamine polyphosphate is preferably 5 or more. Alternatively, the melamine polyphosphate can be an equimolar addition salt of polyphosphoric acid and melamine. It is also possible to use cyclic polymetaphosphoric acid together with acyclic polyphosphoric acid. The addition salts of melamine polyphosphate are generally powders obtained by reacting an aqueous slurry of a mixture of melamine and polyphosphoric acid, followed by separation by filtration, washing and drying. The particle size of the melamine polyphosphate can be adjusted within wide limits, and in this connection reference can also be made to paragraph
[0026] of EP-A-2 100 919.
[0054] Suitable phosphinate salts have the general formula [R 1 R 2 P(=O)-O] - m M m+ Suitable (di)phosphinates have the general formula [OP(=O)R 1 -OR 3 -OP(=O)R 2 -O] 2- n M x m+ (In the formula, R 1 and R 2 are each independently a linear or branched C 1~6 -Alkyl moiety or C 6~10 -aryl moiety, R 3 is a linear or branched C 1~10 -Alkylene moiety, C 6~10 -Arylene moiety, C 7~10 -alkylarylene moiety, or C 7~10 -aryl-alkylene moiety, M being Ca, Mg, Al or Zn, m being the valence of M determined from 2n=mx, n having a value of 1 or 3 and x having a value of 1 or 2. When the value of m or n is 2 or more, the moiety R1 ~R 3 can be freely selected at each position.
[0055] Examples of suitable phosphinates include dimethylphosphinate, ethylmethylphosphinate, diethylphosphinate, methyl-n-propylphosphinate, methanedi(methylphosphinate), benzene-1,4-di(methylphosphinate), methylphenylphosphinate, and diphenylphosphinate. The metal component M is a calcium ion, a magnesium ion, an aluminum ion, or a zinc ion.
[0056] Examples of suitable phosphinate salts include calcium dimethylphosphinate, magnesium dimethylphosphinate, aluminum dimethylphosphinate, zinc dimethylphosphinate, calcium ethyl methylphosphinate, magnesium ethyl methylphosphinate, aluminum ethyl methylphosphinate, zinc ethyl methylphosphinate, calcium diethylphosphinate, magnesium diethylphosphinate, aluminum diethylphosphinate, zinc diethylphosphinate, calcium methyl-n-propylphosphinate, magnesium methyl-n-propylphosphinate, aluminum methyl-n-propylphosphinate, zinc methyl-n-propylphosphinate, calcium methylphenylphosphinate, magnesium methylphenylphosphinate, aluminum methylphenylphosphinate, zinc methylphenylphosphinate, calcium diphenylphosphinate, magnesium diphenylphosphinate, aluminum diphenylphosphinate, and zinc diphenylphosphinate.
[0057] Examples of suitable diphosphinate salts include calcium methane di(methylphosphinate), magnesium methane di(methylphosphinate), aluminum methane di(methylphosphinate), zinc methane di(methylphosphinate), calcium benzene-1,4-di(methylphosphinate), magnesium benzene-1,4-di(methylphosphinate), aluminum benzene-1,4-di(methylphosphinate), zinc benzene-1,4-di(methylphosphinate).
[0058] Particular preference is given to using phosphinate salts, in particular aluminum ethyl methyl phosphinate, aluminum diethyl phosphinate and zinc diethyl phosphinate. Particular preference is given to using aluminum diethyl phosphinate.
[0059] The (di)phosphinate salts can be used in any desired suitable particle size, see EP-A-2 100 919, paragraph
[0032] .
[0060] Also, together with or instead of the above flame retardants, other flame retardants, such as those based on triazines, metal hydrates, and silicones, can be used as additives in component E. A typical triazine-based flame retardant is melamine cyanurate.
[0061] Other further flame retardant substances can be metal compounds, such as magnesium hydroxide, aluminium hydroxide, zinc sulphate, iron oxide and boron oxide, see also EP-A-2 100 919, paragraphs
[0046] to
[0048] .
[0062] Other flame retardant substances having synergistic effects are described, for example, in US 2010 / 0261818, paragraphs
[0064] and
[0065] .
[0063] The thermoplastic molding composition may comprise, as component E, at least one impact-modifying polymer.
[0064] The component E used comprises 0 to 20% by weight, preferably 0 to 10% by weight, in particular 0 to 8% by weight, of at least one impact-modifying polymer different from the copolymer of component C. If an impact-modifying polymer is present, its minimum amount is 0.1% by weight, preferably 1% by weight, in particular 3% by weight. The maximum possible amount of component A is reduced accordingly, so that the total amount of components A to E is 100% by weight. The use of component E in combination is not essential, but its use can improve the impact resistance of the resulting polyamide molding composition. The impact-modifying polymers involved here are those typically used for impact modification of the polyamides of component A. It is preferred that elastomers, such as natural or synthetic rubbers and other elastomers, are included.
[0065] Among the synthetic rubbers that can be used are ethylene-propylene-diene rubber (EPDM), styrene-butadiene rubber (SBR), butadiene rubber (BR), nitrile rubber (NBR), hydrin rubber (ECO), and acrylate rubber (ASA). It is also possible to use silicone rubber, polyoxyalkylene rubber, and other rubbers.
[0066] Thermoplastic elastomers include thermoplastic polyurethanes (TPUs), styrene-butadiene-styrene block copolymers (SBS), styrene-isoprene-styrene block copolymers (SIS), styrene-ethylene-butylene-styrene block copolymers (SEBS), and styrene-ethylene-propylene-styrene block copolymers (SEPS).
[0067] Furthermore, resins such as urethane resins, acrylic resins, fluororesins, silicone resins, imide resins, amide-imide resins, epoxy resins, urea resins, alkyd resins, or melamine resins can be used as blend polymers.
[0068] Furthermore, ethylene copolymers, such as copolymers of ethylene with 1-octene, 1-butene or propylene, can be used as blend polymers, and are described in WO 2008 / 074687. The molar mass of the above-mentioned type of ethylene-α-olefin copolymers is preferably in the range of 10000 to 500000 g / mol, preferably 15000 to 400000 g / mol (number average molar mass). It is also possible to use linear polyolefins, such as polyethylene or polypropylene.
[0069] Further additives are compounds or materials that do not form part of the other components A to D. Thus, for example, if a polyolefin is used in component C, such a polymer cannot form part of component E. However, if component C does not contain a polyolefin having no carboxyl groups, such a polymer can form part of component E. Thus, the different components A to E, and C1 to C4, are mutually exclusive.
[0070] For suitable polyurethanes, reference can be made to EP-B-1 984 438, DE-A-10 2006 045 869 and EP-A-2 223 904.
[0071] Other suitable thermoplastic resins are described in paragraph
[0028] of JP-A-2009-155436.
[0072] Other polymers suitable as component E are described in EP-A-2 100 919, paragraph
[0044] . 0119]. Other fillers which can be used as (part of) component E are carbon fibres, aromatic polyamide fibres and other fillers such as gypsum fibres, synthetic calcium silicate, kaolin, calcined kaolin, wollastonite, talc powder, chalk.
[0073] The molding compositions of the invention are prepared by mixing components A to E. For this purpose, extruders, such as single-screw or twin-screw extruders, or other conventional plastic processing equipment, such as Brabender or Banbury mixers, are advantageously used.
[0074] Here, the order of mixing of the individual components can be freely selected.
[0075] The molding compositions of the invention are characterized by improved flame retardancy combined with improved tensile strain at break and Charpy impact resistance. They are suitable for the production of moldings, fibers or foils.
[0076] The invention also provides corresponding moldings, fibers or foils made from the above-described thermoplastic molding compositions.
[0077] The following examples provide further illustration of the invention. EXAMPLES
[0078] First, a pigment masterbatch was prepared. The masterbatch was prepared using a twin screw extruder at a temperature of 220° C. The color value was obtained using a color difference meter or a spectrophotometer.
[0079] [Table 1]
[0080] These masterbatches were used as colorants in glass fiber reinforced polyamide 6 molding compositions, and the results are shown in Table 2.
[0081] All masses are in mass percent.
[0082] [Table 2]
Claims
1. A pigment composition comprising a bismuth vanadate pigment dispersed in a copolymer of ethylene, a C 1-6 -alkyl acrylate, acrylic acid, and maleic anhydride, Component C1: 5 to 60% by mass of bismuth vanadate; as component C2, 5 to 60% by weight of a copolymer of ethylene, C 1-6 -alkyl acrylate, acrylic acid and maleic anhydride; As component C3, 10 to 70% by weight of polyethylene, polypropylene or ethylene with at least one C as a comonomer 3~12 - copolymers with olefins different from component C2, 0 to 10% by weight of further components as component C4, Including, A pigment composition, wherein the total amount of components C1 to C4 is 100% by mass.
2. The composition of claim 1, wherein the C 1-6 -alkyl acrylate is n-butyl acrylate.
3. The composition of claim 1 or 2, wherein the composition is free of boric acid.
4. Use of the pigment composition according to any one of claims 1 to 3 as a colourant in a thermoplastic polymer composition.
5. 4. A thermoplastic molding composition comprising a thermoplastic polymer and the pigment composition according to claim 1 in an amount such that the bismuth vanadate content of the thermoplastic molding composition is in the range from 0.1 to 2.0% by weight.
6. as component A, 30 to 95% by weight of at least one polyamide or copolyamide, Component B: 0 to 50% by mass of glass fibers; As component C, 0.2 to 7% by weight of the pigment composition according to any one of claims 1 to 3, as component D, 0 to 2% by weight of at least one organic pigment, As component E, 0 to 50% by weight of further additives A thermoplastic molding composition comprising: A thermoplastic molding composition, the total amount of components A to E being 100% by weight.
7. 7. The molding composition according to claim 6, having a bismuth vanadate content of the thermoplastic molding composition in the range from 0.1 to 2.0% by weight.
8. 8. The molding composition according to claim 6, wherein the composition comprises, as component D, 0.1 to 2.0% by weight of at least one yellow organic pigment.
9. A process for preparing a pigment composition according to any one of claims 1 to 3 or a thermoplastic moulding composition according to any one of claims 5 to 8, comprising mixing the components of the composition.
10. Use of the thermoplastic molding composition according to any one of claims 5 to 8 for the production of fibres, foils or moulded articles.
11. 9. Mouldings, fibres or foils made from the thermoplastic moulding composition according to any one of claims 5 to 8.
Citation Information
Patent Citations
Coloring resin composition
JP1988008458A
Resin composition for coloring and its production
JP1997124799A
Bismuth vanadate pigment powder mixture
JP1998114864A
Resin composition for coloring
JP2000327794A
Coated bismuth oxyhalide pigment
JP2018538414A