Non-oriented electrical steel sheet, iron core, manufacturing method of iron core, motor, and manufacturing method of motor
A non-oriented electrical steel sheet with controlled composition and grain size addresses the need for improved high-frequency core loss and magnetic properties, enhancing torque and energy efficiency in drive motors.
Patent Information
- Application Number
- JP2024506609
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-09-29
- Filing Date
- 2023-09-19
- Publication Date
- 2024-09-19
- Estimated Expiration
- 2043-09-19
AI Technical Summary
Existing non-oriented electrical steel sheets used in motors require further improvement in high-frequency core loss and magnetic properties to meet the demands of miniaturized, high-efficiency drive motors for hybrid and electric vehicles.
A non-oriented electrical steel sheet with specific chemical composition and controlled grain size and texture, including a base steel plate with defined thickness and crystal grain sizes, and an insulating coating, is developed to enhance high-frequency core loss and magnetic properties.
The solution results in a non-oriented electrical steel sheet with reduced high-frequency core loss and improved magnetic flux density, contributing to enhanced torque and energy efficiency in drive motors.
Smart Images

Figure 0007553877000052 
Figure 0007553877000053 
Figure 0007553877000027
Abstract
Description
[Technical field]
[0001] The present invention relates to a non-oriented electrical steel sheet, an iron core, a method for manufacturing an iron core, a motor, and a method for manufacturing a motor. More specifically, the present invention relates to a non-oriented electrical steel sheet having good high-frequency iron loss, an iron core including this non-oriented electrical steel sheet and a method for manufacturing an iron core, and a motor including this iron core and a method for manufacturing a motor. This application claims priority based on Japanese Patent Application No. 2022-156745, filed on September 29, 2022, the contents of which are incorporated herein by reference. [Background technology]
[0002] Due to the need to reduce greenhouse gases, products that consume less energy are being developed in the industrial sector. For example, in the automotive sector, there are fuel-efficient vehicles such as hybrid vehicles that combine a gasoline engine and a motor, and electric vehicles that are driven by a motor. The common technology in these fuel-efficient vehicles is the motor, and miniaturizing and increasing the efficiency of motors are key technologies.
[0003] For example, there is a growing demand for miniaturization of drive motors for hybrid and electric vehicles due to space restrictions and reduced fuel consumption through weight reduction. To miniaturize motors, it is necessary to increase the motor's torque. Therefore, there is a demand for further improvement in the magnetic properties of non-oriented electrical steel sheets used as the iron core material for motors.
[0004] In addition, there is a limit to the battery capacity that can be installed in an automobile, so there is an increasing demand for high efficiency drive motors. To increase the efficiency of a motor, it is necessary to reduce energy loss. Therefore, there is a demand for further reduction in iron loss in non-oriented electrical steel sheets used as the iron core material of motors. In particular, in the motors of hybrid drive vehicles and electric vehicles, attempts are being made to increase the rotation speed of the motor to compensate for the decrease in torque that accompanies miniaturization. Therefore, there is a demand for further reduction in iron loss in the high frequency range of non-oriented electrical steel sheets.
[0005] For example, Patent Document 1 discloses an electrical steel sheet that achieves both high magnetic flux density and low iron loss at high frequency by using a three-layer clad structure in which both sides of an inner layer of a grain-oriented electrical steel sheet are sandwiched between non-oriented electrical steel sheets to form a surface layer. Patent Document 2 discloses an Fe-based metal sheet that achieves both high magnetic flux density and high strength by changing the chemical composition in the thickness direction and changing the crystal grain size in the thickness direction. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2010-132938 A [Patent Document 2] JP 2016-183358 A Summary of the Invention [Problem to be solved by the invention]
[0007] Up until now, studies have been conducted on improving the magnetic flux density and iron loss characteristics of non-oriented electrical steel sheets used as the iron core material of motors. However, there is currently a demand for further improvement in the magnetic properties of non-oriented electrical steel sheets, particularly in terms of high-frequency iron loss.
[0008] One aspect of the present invention has been made in view of the above problems. An object of one aspect of the present invention is to provide a non-oriented electrical steel sheet having good high-frequency iron loss. Another object of one aspect of the present invention is to provide an iron core including this non-oriented electrical steel sheet, a method for manufacturing the iron core, and a motor including this iron core, and a method for manufacturing the motor. [Means for solving the problem]
[0009] (1) A non-oriented electrical steel sheet according to one aspect of the present invention has The steel plate has a base material and an insulating coating. The base steel sheet has a chemical composition, in mass%, Si: 1.0% or more and 5.0% or less, C: 0% or more and 0.0050% or less, Mn: 0% or more and 3.0% or less, P: 0% or more and 0.30% or less, S: 0% or more and 0.010% or less, Al: 0% or more and 3.0% or less, Zn: 0% or more and 0.10% or less, N: 0% or more and 0.010% or less, Sn: 0% or more and 0.10% or less, Sb: 0% or more and 0.10% or less, Ca: 0% or more and 0.010% or less, Cr: 0% or more and 5.0% or less, Ni: 0% or more and 5.0% or less, Cu: 0% or more and 5.0% or less, Ce: 0% or more and 0.10% or less, B: 0% or more and 0.10% or less, O: 0% or more and 0.10% or less, Mg: 0% or more and 0.10% or less, Ti: 0% or more and 0.10% or less, V: 0% or more and 0.10% or less, Zr: 0% or more and 0.10% or less, Nd: 0% or more and 0.10% or less, Bi: 0% or more and 0.10% or less, W: 0% or more and 0.10% or less, Mo: 0% or more and 0.10% or less, Nb: 0% or more and 0.10% or less, Y: 0% or more and 0.10% or less with the remainder being Fe and impurities, The thickness of the base steel plate is 0.10 mm or more and 0.35 mm or less, When the base steel plate is cut in a cross section parallel to the plate thickness direction, the average crystal grain size is 10 μm or less in a surface region from the surface of the base steel plate to 1 / 20 of the plate thickness. the law of nature, The average crystal grain size is 50 μm or more and 200 μm or less in an intermediate region from 1 / 20 of the plate thickness to 1 / 4 of the plate thickness based on the surface, The average crystal grain size is 50 μm or more and 200 μm or less in the central region from 1 / 4 of the plate thickness to 1 / 2 of the plate thickness based on the surface. do. ( 2 )the above (1)In the non-oriented electrical steel sheet described in The base steel sheet has a chemical composition, in mass%, Sn: 0% or more and less than 0.030% may be limited to ( 3 )(1) above Or (2) In the non-oriented electrical steel sheet described in When the base steel sheet is viewed at the cut surface, When the R value calculated using the Si content, Al content, and Mn content in mass% contained in the base steel sheet as the chemical composition is defined as R = 9.9 + 12.4 [Si] + 10.0 [Al] + 6.6 [Mn], In the region from the surface to 1 / 10 of the plate thickness, the R value is 60 or more and 250 or less, The R value may be 30 or more and less than 60 in a region from 1 / 10 of the plate thickness to 1 / 2 of the plate thickness with respect to the surface. ( 4 ) Above (1)~( 3 In the non-oriented electrical steel sheet according to any one of the above items, At 1 / 2 the sheet thickness with respect to the surface as a reference, the {100} plane intensity may be 2.4 or more, and the area ratio of {100} oriented grains may be 18% or more with respect to the observation field. ( 5 The iron core according to one aspect of the present invention is 4 ) The non-oriented electrical steel sheet may include the non-oriented electrical steel sheet according to any one of the above. ( 6 The method for producing an iron core according to one aspect of the present invention comprises the steps of (1) to ( 4 ) a step of laminating the non-oriented electrical steel sheets according to any one of the above items. ( 7 The motor according to one aspect of the present invention is 5 ) may be included in the iron core. ( 8 A method for manufacturing a motor according to one aspect of the present invention comprises the steps of (1) to ( 4 ) to obtain an iron core, and a step of assembling the iron core to obtain a motor. Effect of the Invention
[0010] According to the above aspects of the present invention, it is possible to provide a non-oriented electrical steel sheet having good high-frequency iron loss, and in addition to that, it is possible to provide an iron core including this non-oriented electrical steel sheet and a method for manufacturing the iron core, as well as a motor including this iron core and a method for manufacturing the motor. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a cross-sectional schematic diagram of a non-oriented electrical steel sheet according to an embodiment of the present invention. [Diagram 2] 1 is a flow diagram of a method for producing a non-oriented electrical steel sheet according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] A preferred embodiment of the present invention will be described in detail below. However, the present invention is not limited to the configuration disclosed in this embodiment, and various modifications are possible without departing from the spirit of the present invention. In addition, the numerical ranges described below include lower and upper limits. Numerical values indicated as "greater than" or "less than" are not included in the numerical range. "%" regarding the content of each element means "mass %".
[0013] [Non-oriented electrical steel sheet] The non-oriented electrical steel sheet according to this embodiment has the following features.
[0014] The non-oriented electrical steel sheet according to this embodiment includes a base steel sheet and an insulating coating, The base steel sheet has a chemical composition, in mass%, of: Si: 1.0% or more and 5.0% or less, C: 0% or more and 0.0050% or less, Mn: 0% or more and 3.0% or less, P: 0% or more and 0.30% or less, S: 0% or more and 0.010% or less, Al: 0% or more and 3.0% or less, Zn: 0% or more and 0.10% or less, N: 0% or more and 0.010% or less, Sn: 0% or more and 0.10% or less, Sb: 0% or more and 0.10% or less, Ca: 0% or more and 0.010% or less, Cr: 0% or more and 5.0% or less, Ni: 0% or more and 5.0% or less, Cu: 0% or more and 5.0% or less, Ce: 0% or more and 0.10% or less, B: 0% or more and 0.10% or less, O: 0% or more and 0.10% or less, Mg: 0% or more and 0.10% or less, Ti: 0% or more and 0.10% or less, V: 0% or more and 0.10% or less, Zr: 0% or more and 0.10% or less, Nd: 0% or more and 0.10% or less, Bi: 0% or more and 0.10% or less, W: 0% or more and 0.10% or less, Mo: 0% or more and 0.10% or less, Nb: 0% or more and 0.10% or less, Y: 0% or more and 0.10% or less with the remainder being Fe and impurities, The thickness of the base steel plate is 0.10 mm or more and 0.35 mm or less, When the base steel sheet is viewed on a cross section parallel to the sheet thickness direction, the average crystal grain size is 10 μm or less in a surface region from the surface of the base steel sheet to 1 / 20 of the sheet thickness.
[0015] In addition, the non-oriented electrical steel sheet according to this embodiment has When the base steel plate is viewed on the above cut surface, The average crystal grain size is 50 μm or more and 200 μm or less in the intermediate region from 1 / 20 of the plate thickness to 1 / 4 of the plate thickness based on the above surface, It is preferable that the average crystal grain size is 50 μm or more and 200 μm or less in the central region from 1 / 4 of the sheet thickness to 1 / 2 of the sheet thickness based on the above-mentioned surface.
[0016] In addition, the non-oriented electrical steel sheet according to this embodiment has The base steel sheet has the above chemical composition, in mass%, Sn: 0% or more and less than 0.030% It is preferable to limit the
[0017] In addition, the non-oriented electrical steel sheet according to this embodiment has When the base steel plate is viewed on the above cut surface, When the R value calculated using the Si content, Al content, and Mn content in mass% contained in the base steel plate as the chemical composition is defined as R = 9.9 + 12.4 [Si] + 10.0 [Al] + 6.6 [Mn], In the area from the surface to 1 / 10 of the plate thickness, the R value is 60 or more and 250 or less, It is preferable that the R value is 30 or more and less than 60 in a region from 1 / 10 of the plate thickness to 1 / 2 of the plate thickness with respect to the above-mentioned surface.
[0018] In addition, the non-oriented electrical steel sheet according to this embodiment has It is preferable that the {100} plane intensity is 2.4 or more at 1 / 2 the plate thickness based on the above surface, and the area ratio of {100} oriented grains is 18% or more with respect to the observation field.
[0019] FIG. 1 shows a schematic cross-sectional view of a non-oriented electrical steel sheet according to this embodiment. The non-oriented electrical steel sheet 1 according to this embodiment has an insulating coating 11 and a base steel sheet 12. When viewed on a cut surface in which the cutting direction is parallel to the sheet thickness direction, the base steel sheet 12 may be divided into a surface region 12a extending from the surface of the base steel sheet 12 to 1 / 20 of the sheet thickness, an intermediate region 12b extending from 1 / 20 of the sheet thickness to 1 / 4 of the sheet thickness of the base steel sheet 12, and a central region 12c extending from 1 / 4 of the sheet thickness to 1 / 2 of the sheet thickness of the base steel sheet 12. Each feature of the non-oriented electrical steel sheet according to this embodiment will be described in detail below.
[0020] Plate Thickness In the non-oriented electrical steel sheet according to this embodiment, the thickness of the base steel sheet is set to 0.35 mm or less, preferably 0.30 mm or less. On the other hand, since excessive thinning significantly reduces the productivity of the steel sheet and the motor and may also deteriorate the magnetic properties, the thickness of the base steel sheet is set to 0.10 mm or more, preferably 0.15 mm or more.
[0021] The thickness of the base steel sheet may be measured with a micrometer. If the non-oriented electrical steel sheet to be measured has an insulating coating on its surface, the insulating coating is removed before the measurement. For example, the insulating coating may be removed by the following method.
[0022] A non-oriented electrical steel sheet having an insulating coating or the like is immersed in an aqueous solution of sodium hydroxide, an aqueous solution of sulfuric acid, and an aqueous solution of nitric acid in that order, and then washed. Finally, it is dried with hot air. In this way, a non-oriented electrical steel sheet (base steel sheet) from which the insulating coating has been removed can be obtained.
[0023] [Average grain size] In the non-oriented electrical steel sheet according to this embodiment, when the base steel sheet is viewed on a cut surface parallel to the sheet thickness direction, the average crystal grain size is 10 μm or less in a surface region from the surface of the base steel sheet to 1 / 20 of the sheet thickness. Note that, although the above surface region is described for one sheet surface of the base steel sheet, the above condition may be satisfied for both sheet surfaces of the base steel sheet.
[0024] In the surface region, the average crystal grain size is preferably 9 μm or less, and more preferably 8 μm or less. On the other hand, in the surface region, the lower limit of the average crystal grain size is not particularly limited. For example, in the surface region, the average crystal grain size may be 1 μm or more.
[0025] When the average crystal grain size satisfies the above condition in the surface region, high-frequency iron loss is preferably improved. For example, iron loss refers to a loss that combines eddy current loss and hysteresis loss. At commercial frequencies (e.g., about 50 Hz), the ratio of hysteresis loss in iron loss is higher than that of eddy current loss, and the skin effect is not as prominent at commercial frequencies as at higher frequencies. On the other hand, at high frequencies (e.g., about 1 kHz), the ratio of eddy current loss in iron loss increases, and the skin effect also becomes prominent. In this embodiment, it is estimated that by making the average crystal grain size finer in the surface region, i.e., by making the magnetic domain width smaller in the surface region, the iron loss in the presence of the skin effect, which becomes prominent at high frequencies, mainly the eddy current loss, is reduced.
[0026] The average crystal grain size in the surface region is controlled by manufacturing conditions specific to this embodiment, which will be described in detail later.
[0027] In addition, in the non-oriented electrical steel sheet according to the present embodiment, when the base steel sheet is viewed on the cut surface, it is preferable that the average crystal grain size is 50 μm or more and 200 μm or less in an intermediate region from 1 / 20 of the sheet thickness to 1 / 4 of the sheet thickness with respect to the surface, and the average crystal grain size is 50 μm or more and 200 μm or less in a central region from 1 / 4 of the sheet thickness to 1 / 2 of the sheet thickness with respect to the surface. Note that although the intermediate region and central region are described for one sheet surface of the base steel sheet, the above conditions may be satisfied for both sheet surfaces of the base steel sheet. The sheet thickness 1 / 2 corresponds to the center in the sheet thickness direction of the base steel sheet on the cut surface.
[0028] In the intermediate region, the average crystal grain size is preferably greater than 60 μm, and more preferably greater than 70 μm. In addition, in the intermediate region, the average crystal grain size is preferably less than 150 μm, and more preferably less than 120 μm. Similarly, in the central region, the average crystal grain size is preferably greater than 60 μm, and more preferably greater than 70 μm. In addition, in the central region, the average crystal grain size is preferably less than 150 μm, and more preferably less than 120 μm.
[0029] As described above, the intermediate region is a region from 1 / 20 of the plate thickness to 1 / 4 of the plate thickness based on the surface of the base steel plate. When the region from 1 / 20 of the plate thickness to 1 / 10 of the plate thickness is divided within this intermediate region based on the surface, it is preferable that the region from 1 / 20 of the plate thickness to 1 / 10 of the plate thickness also has an average crystal grain size equivalent to that of the intermediate region. For example, when the average crystal grain size of the intermediate region is more than 60 μm, it is preferable that the average crystal grain size of the region from 1 / 20 of the plate thickness to 1 / 10 of the plate thickness is also more than 60 μm. Similarly, when the average crystal grain size of the intermediate region is 150 μm or less, it is preferable that the average crystal grain size of the region from 1 / 20 of the plate thickness to 1 / 10 of the plate thickness is also 150 μm or less. It is preferable that the region from 1 / 10 of the plate thickness to 1 / 4 of the plate thickness also has an average crystal grain size equivalent to that of the intermediate region.
[0030] When the average crystal grain size satisfies the above conditions in the intermediate and central regions, the hysteresis loss and magnetic permeability are preferably improved. In particular, in low magnetic fields (e.g., excitation magnetization force of about 100 A / m) and medium magnetic fields (e.g., excitation magnetization force of about 1000 A / m), the magnetization process proceeds mainly by domain wall motion, so it is desirable to have few crystal grain boundaries that hinder domain wall motion. In this embodiment, it is estimated that by controlling the average crystal grain size to an appropriate size in the intermediate and central regions, the hysteresis loss is reduced and the magnetic permeability is increased in low to medium magnetic fields.
[0031] The average crystal grain size in the intermediate region and the central region is controlled by manufacturing conditions specific to this embodiment. The manufacturing conditions for controlling the average crystal grain size will be described in detail later.
[0032] In the conventional technology, when the crystal grain size is changed along the sheet thickness direction, the crystal grain size often changes little by little from the surface region toward the intermediate region and the central region. In this case, for example, the average crystal grain size in the intermediate region is often a value between the surface region and the central region. In particular, the average crystal grain size is often fine in the above-mentioned region from 1 / 20 of the sheet thickness to 1 / 10 of the sheet thickness. On the other hand, in this embodiment, the average crystal grain size is finely controlled only in the surface region, and the average crystal grain size in the intermediate region and the central region is controlled to an appropriate size. Specifically, in this embodiment, the average crystal grain size in the surface region is fine, but the average crystal grain size in the intermediate region is equivalent to that in the central region. As a result, the high-frequency iron loss can be favorably improved.
[0033] The average grain size of the base steel sheet may be measured by the cutting method specified in JIS G0551:2020. For example, the average grain size measured by the cutting method in a direction perpendicular to the sheet thickness direction in a longitudinal section microstructure photograph may be used. As the longitudinal section microstructure photograph, an optical microscope photograph may be used, and for example, a photograph taken at a magnification of 100 times or more may be used. Under the above conditions, the average grain size may be determined in each of the surface region, intermediate region, and central region.
[0034] [Collective tissue] In the non-oriented electrical steel sheet according to this embodiment, it is preferable that the {100} plane intensity is 2.4 or more at 1 / 2 the sheet thickness based on the surface of the base steel sheet, and the area ratio of {100} oriented grains is 18% or more with respect to the observation field.
[0035] In the above-mentioned half thickness portion, the {100} plane strength is preferably 3.5 or more, and more preferably 3.8 or more. Meanwhile, in the above-mentioned half thickness portion, the upper limit of the {100} plane strength is not particularly limited. For example, in the above-mentioned half thickness portion, the {100} plane strength may be 10 or less.
[0036] When the {100} plane strength satisfies the above condition at the half plate thickness portion, the high magnetic field magnetic properties are preferably improved. The crystal orientation near {100} is a texture that contributes to improving the magnetic flux density. For example, when the Si content or the like increases as the steel composition of the base steel sheet, the saturation magnetic flux density decreases, but when the {100} plane strength increases as the texture of the base steel sheet, the magnetic flux density improves. In this embodiment, the {100} plane strength is appropriately controlled together with other technical features, thereby improving the magnetic properties in a high magnetic field, mainly the magnetic flux density in a high magnetic field (for example, excitation magnetization force of about 5000 A / m).
[0037] In addition, in the above-mentioned half-thickness portion, the area ratio of the {100} oriented grains is preferably 20% or more, more preferably 22% or more, relative to the observation field. Meanwhile, in the above-mentioned half-thickness portion, the upper limit of the area ratio of the {100} oriented grains is not particularly limited. For example, in the above-mentioned half-thickness portion, the area ratio of the {100} oriented grains may be 100% or less, and may be 35% or less.
[0038] When the area ratio of the {100} oriented grains at the half thickness portion satisfies the above condition, the high magnetic field magnetic properties are preferably improved. The crystal orientation near {100} is a texture that contributes to improving the magnetic flux density. For example, when the Si content or the like is increased as the steel composition of the base steel sheet, the saturation magnetic flux density decreases, but when the area ratio of the {100} oriented grains at the half thickness portion of the base steel sheet increases, the magnetic flux density improves. In this embodiment, the area ratio of the {100} oriented grains is appropriately controlled together with other technical features, thereby improving the magnetic properties in a high magnetic field, mainly the magnetic flux density in a high magnetic field (for example, excitation magnetization force of about 5000 A / m).
[0039] The {100} plane strength and the area ratio of {100} oriented grains at the half thickness portion are controlled by manufacturing conditions specific to this embodiment. The manufacturing conditions for controlling the average crystal grain size will be described in detail later.
[0040] The {100} plane intensity of the base steel sheet may be measured by comparing the integrated intensity of the diffraction of the {100} plane from the X-ray diffraction profile with the ideal intensity ratio for a randomly oriented material. Measurements can be performed using, for example, a horizontal sample type high-power X-ray diffractometer RINT-TTR3 or a powder X-ray diffractometer RINT-2000 manufactured by Rigaku Corporation, but the measurement results are essentially independent of the measuring device. Under the above conditions, the {100} plane intensity at 1 / 2 the sheet thickness may be obtained. The 1 / 2 sheet thickness may be revealed by polishing the surface of the base steel sheet parallel to the plate and gradually reducing the thickness.
[0041] The area ratio of the {100} oriented grains of the base steel sheet may be measured by a scanning electron microscope with electron backscatter diffraction (SEM-EBSD). The measurement may be performed, for example, using a scanning electron microscope JSM-6400 manufactured by JEOL, an EBSD detector HIKARI manufactured by TSL, or an OIM analysis manufactured by TSL, but the measurement results are essentially independent of the measurement equipment. For example, the measurement may be performed using a sample polished for EBSD with care so that no polishing strain remains on the surface, with the step interval set to 2 μm, the measurement area set to 8000 μm × 2400 μm, the grain boundary judgment set to an angle difference of 15° or more in the crystal orientation, and the extraction of the area ratio of the {100} oriented grains set to a tolerance of 20°. Under the above conditions, the area ratio of the {100} oriented grains at 1 / 2 the sheet thickness may be obtained. The 1 / 2 sheet thickness may be revealed by polishing the sheet surface of the base steel sheet in parallel and gradually reducing the thickness as described above. The half of the plate thickness corresponds to the center of the base steel plate in the plate thickness direction.
[0042] [Chemical composition] In the non-oriented electrical steel sheet according to this embodiment, the base steel sheet has a chemical composition that contains Si, optionally contains selected elements, and the balance is Fe and impurities.
[0043] Specifically, the base steel sheet has a chemical composition, in mass%, of: Si: 1.0% or more and 5.0% or less, C: 0% or more and 0.0050% or less, Mn: 0% or more and 3.0% or less, P: 0% or more and 0.30% or less, S: 0% or more and 0.010% or less, Al: 0% or more and 3.0% or less, Zn: 0% or more and 0.10% or less, N: 0% or more and 0.010% or less, Sn: 0% or more and 0.10% or less, Sb: 0% or more and 0.10% or less, Ca: 0% or more and 0.010% or less, Cr: 0% or more and 5.0% or less, Ni: 0% or more and 5.0% or less, Cu: 0% or more and 5.0% or less, Ce: 0% or more and 0.10% or less, B: 0% or more and 0.10% or less, O: 0% or more and 0.10% or less, Mg: 0% or more and 0.10% or less, Ti: 0% or more and 0.10% or less, V: 0% or more and 0.10% or less, Zr: 0% or more and 0.10% or less, Nd: 0% or more and 0.10% or less, Bi: 0% or more and 0.10% or less, W: 0% or more and 0.10% or less, Mo: 0% or more and 0.10% or less, Nb: 0% or more and 0.10% or less, Y: 0% or more and 0.10% or less and the balance being Fe and impurities.
[0044] Each element will be described below. Note that the chemical composition of the base steel sheet described below is an average value for the entire base steel sheet.
[0045] Si: 1.0% or more and 5.0% or less Silicon (Si) is an element that is effective in increasing the resistivity of steel sheet and reducing iron loss. Therefore, the Si content is set to 1.0% or more. The Si content is preferably 1.5% or more, and more preferably 2.0% or more. On the other hand, excessive inclusion of silicon significantly reduces the magnetic flux density. Therefore, the Si content is set to 5.0% or less. The Si content is preferably 4.0% or less, and more preferably 3.50% or less.
[0046] C: 0% or more and 0.0050% or less C (carbon) is an optional element. However, if it is contained in excess, the magnetic properties deteriorate. Therefore, the C content is set to 0.0050% or less. The C content is preferably 0.0030% or less. On the other hand, since it is preferable that the C content is low, there is no need to set a lower limit, and the lower limit may be 0%. However, since it is not easy to set the C content to 0% industrially, the lower limit may be set to more than 0%, or may be set to 0.0010%.
[0047] Mn: 0% or more and 3.0% or less Mn (manganese) is an optional element. Mn has the effect of increasing the resistivity of the steel sheet and reducing iron loss. However, since Mn has a higher alloying cost than Si and Al, a high Mn content is economically disadvantageous. For this reason, the Mn content is set to 3.0% or less, and preferably 2.50% or less. There is no need to limit the lower limit of Mn, and the lower limit may be 0%. However, in order to more reliably obtain the above effect, the Mn content is preferably more than 0%, preferably 0.0010% or more, and more preferably 0.010% or more.
[0048] P: 0% or more and 0.30% or less P (phosphorus) is an optional element. P has the effect of improving the texture of non-oriented electrical steel sheet and improving the magnetic properties. However, since P is also a solid solution strengthening element, if the P content is excessive, the steel sheet becomes hard and cold rolling becomes difficult. For this reason, the P content is set to 0.30% or less. The P content is preferably 0.20% or less. There is no need to limit the lower limit of P, and the lower limit may be 0%. However, in order to more reliably obtain the above effects, the P content is preferably more than 0%, preferably 0.0010% or more, and more preferably 0.0150% or more.
[0049] S: 0% or more and 0.010% or less S (sulfur) is an optional element. However, S combines with Mn in the steel to form fine MnS, which inhibits the growth of crystal grains during annealing and may deteriorate the magnetic properties of the non-oriented electrical steel sheet. For this reason, the S content is set to 0.010% or less. The S content is preferably 0.0050% or less, and more preferably 0.0030% or less. Since a small S content is preferable, there is no need to limit the lower limit, and the lower limit may be 0%. However, since it is not easy to industrially set the content to 0%, the lower limit may be set to more than 0% or may be set to 0.00010%.
[0050] Al: 0% or more and 3.0% or less Al (aluminum) is an optional element. Al is an optional element that is effective in increasing the resistivity of the steel sheet and reducing iron loss, but if it is contained in excess, the magnetic flux density drops significantly. For this reason, the Al content is set to 3.0% or less. There is no need to limit the lower limit of Al, and the lower limit may be 0%. However, in order to more reliably obtain the effects of the above action, it is preferable that the Al content is 0.10% or more. In this embodiment, Al means acid-soluble aluminum.
[0051] Zn: 0% or more and 0.10% or less Zn (zinc) is an optional element. Zn is an effective element for improving magnetic flux density, core loss characteristics, and punchability, but if it is contained in excess, the above effects will saturate. For this reason, the Zn content is set to 0.10% or less. There is no need to set a lower limit for Zn, and the lower limit may be 0%. However, in order to more reliably obtain the effects due to the above actions, it is preferable that the Zn content is set to 0.0010% or more.
[0052] N: 0% or more and 0.010% or less N (nitrogen) is an optional element. However, N combines with Al to form fine AlN, which may inhibit the growth of crystal grains during annealing and deteriorate the magnetic properties. For this reason, the N content is set to 0.010% or less. The N content is preferably 0.0050% or less, and more preferably 0.0030% or less. Since it is preferable that the N content is low, there is no need to limit the lower limit, and the lower limit may be 0%. However, since it is not easy to industrially set the content to 0%, the lower limit may be more than 0%, may be 0.00010% or more, may be more than 0.00150%, or may be 0.00250% or more.
[0053] Sn: 0% or more and 0.10% or less Sb: 0% or more and 0.10% or less Sn (tin) and Sb (antimony) are optional elements. Sn and Sb have the effect of improving the texture of non-oriented electrical steel sheets and improving magnetic properties (e.g., magnetic flux density). However, excessive inclusion of these elements may embrittle the steel, causing cold rolling fracture, and may also deteriorate the magnetic properties. For this reason, the contents of Sn and Sb are each set to 0.10% or less. In order to finely control the average crystal grain size in the surface region of the base steel sheet, the Sn content is preferably less than 0.030%. On the other hand, there is no need to limit the lower limit of Sn and Sb, and the lower limit may be 0%. However, in order to more reliably obtain the above effects, the Sn content is preferably more than 0%, preferably 0.0010% or more, and more preferably 0.010% or more. In addition, the Sb content is preferably more than 0%, more preferably 0.0010% or more, more preferably 0.0020% or more, even more preferably 0.010% or more, and even more preferably more than 0.0250%.
[0054] Ca: 0% or more and 0.010% or less Ca (calcium) is an optional element. Ca suppresses the precipitation of fine sulfides (MnS, Cu2S, etc.) by generating coarse sulfides, so it is effective in inclusion control. When Ca is added in an appropriate amount, it has the effect of improving the crystal grain growth and improving magnetic properties (for example, iron loss). However, if it is contained in an excessive amount, the above effect saturates and leads to an increase in cost. Therefore, the Ca content is set to 0.010% or less. The Ca content is preferably 0.0080% or less, and more preferably 0.0050% or less. There is no need to limit the lower limit of Ca, and the lower limit may be 0%. However, in order to obtain the above effect more reliably, the Ca content is preferably more than 0%, and is preferably 0.00030% or more. The Ca content is preferably 0.0010% or more, and more preferably 0.0030% or more.
[0055] Cr: 0% or more and 5.0% or less Cr (chromium) is an optional element. Cr has the effect of increasing resistivity and improving magnetic properties (for example, iron loss). However, excessive inclusion of Cr may reduce saturation magnetic flux density, and the above effect is saturated, resulting in increased costs. Therefore, the Cr content is set to 5.0% or less. The Cr content is preferably 2.0% or less, and more preferably 1.0% or less. There is no need to limit the lower limit of Cr, and the lower limit may be 0%. However, in order to obtain the above effect more reliably, the Cr content is preferably more than 0%, and is preferably 0.0010% or more. In addition, Cr suppresses the formation of Kirkendall voids in the base steel sheet. Therefore, the Cr content is preferably 0.50% or more.
[0056] Ni: 0% or more and 5.0% or less Ni (nickel) is an optional element. Ni has the effect of improving magnetic properties (e.g., saturation magnetic flux density). However, if excessively contained, the above effect saturates, resulting in increased costs. Therefore, the Ni content is set to 5.0% or less. The Ni content is preferably 0.50% or less, and more preferably 0.10% or less. There is no need to set a lower limit for Ni, and the lower limit may be 0%. However, in order to obtain the above effect more reliably, the Ni content is preferably more than 0%, and is preferably 0.0010% or more.
[0057] Cu: 0% or more and 5.0% or less Cu (copper) is an optional element. Cu has the effect of improving the strength of the steel sheet. However, excessive Cu content may decrease the saturation magnetic flux density, and the above effect may saturate, resulting in an increase in costs. Therefore, the Cu content is set to 5.0% or less. The Cu content is preferably 0.10% or less. There is no need to set a lower limit for Cu, and the lower limit may be 0%. However, in order to more reliably obtain the above effect, the Cu content is preferably more than 0%, and is preferably 0.0010% or more.
[0058] Ce: 0% or more and 0.10% or less Ce (cerium) is an optional element. Ce has the effect of suppressing the precipitation of fine sulfides (MnS, Cu2S, etc.) by generating coarse sulfides and oxysulfides, improving grain growth, and reducing iron loss. However, if it is contained in excess, oxides are also generated in addition to sulfides and oxysulfides, which may deteriorate iron loss, and the above effect will saturate and lead to an increase in costs. Therefore, the Ce content is set to 0.10% or less. The Ce content is preferably 0.010% or less, more preferably 0.0090% or less, and even more preferably 0.0080% or less. There is no need to limit the lower limit of Ce, and the lower limit may be 0%. However, in order to obtain the above effect more reliably, the Ce content is preferably more than 0%, and is preferably 0.0010% or more. The Ce content is more preferably 0.0020% or more, even more preferably 0.0030% or more, and even more preferably 0.0050% or more.
[0059] The chemical composition of the base steel sheet of the non-oriented electrical steel sheet according to this embodiment may contain, in addition to the above elements, optional elements such as B, O, Mg, Ti, V, Zr, Nd, Bi, W, Mo, Nb, and Y. The contents of these optional elements may be controlled based on known knowledge. For example, the contents of these optional elements may be as follows. The lower limit of these optional elements may be more than 0%. B: 0% or more and 0.10% or less, O: 0% or more and 0.10% or less, Mg: 0% or more and 0.10% or less, Ti: 0% or more and 0.10% or less, V: 0% or more and 0.10% or less, Zr: 0% or more and 0.10% or less, Nd: 0% or more and 0.10% or less, Bi: 0% or more and 0.10% or less, W: 0% or more and 0.10% or less, Mo: 0% or more and 0.10% or less, Nb: 0% or more and 0.10% or less, Y: 0% or more and 0.10% or less.
[0060] In addition, the base steel sheet of the non-oriented electrical steel sheet according to this embodiment has a chemical composition, in mass%, C: 0.0010% or more and 0.0050% or less, Mn: 0.0010% or more and 3.0% or less, P: 0.0010% or more and 0.30% or less, S: 0.00010% or more and 0.010% or less, N: more than 0.00150% and less than 0.010%, B: 0.00010% or more and 0.10% or less, O: 0.00010% or more and 0.10% or less, Mg: 0.00010% or more and 0.10% or less, Ca: 0.00030% or more and 0.010% or less, Ti: 0.00010% or more and 0.10% or less, V: 0.00010% or more and 0.10% or less, Cr: 0.0010% or more and 5.0% or less, Ni: 0.0010% or more and 5.0% or less, Cu: 0.0010% or more and 5.0% or less, Zr: 0.00020% or more and 0.10% or less, Sn: 0.0010% or more and 0.10% or less, Sb: 0.0010% or more and 0.10% or less, Ce: 0.0010% or more and 0.10% or less, Nd: 0.0020% or more and 0.10% or less, Bi: 0.0020% or more and 0.10% or less, W: 0.0020% or more and 0.10% or less, Mo: 0.0020% or more and 0.10% or less, Nb: 0.00010% or more and 0.10% or less, Y: 0.0020% or more and 0.10% or less, It is preferable that the compound contains at least one of the above.
[0061] Also, the B content is preferably 0.010% or less, the O content is preferably 0.010% or less, the Mg content is preferably 0.0050% or less, the Ti content is preferably 0.0020% or less, the V content is preferably 0.0020% or less, the Zr content is preferably 0.0020% or less, the Nd content is preferably 0.010% or less, the Bi content is preferably 0.010% or less, the W content is preferably 0.010% or less, the Mo content is preferably 0.01% or less, the Nb content is preferably 0.0020% or less, and the Y content is preferably 0.010% or less. Also, the Ti content is preferably 0.0010% or more, the V content is preferably 0.0020% or more, and the Nb content is preferably 0.0020% or more.
[0062] The above-mentioned chemical composition may be measured by a general analysis method for steel. For example, the chemical composition may be measured by ICP-AES (Inductively Coupled Plasma-Atomic Emission Spectrometry). Al may be measured as acid-soluble Al by ICP-AES using the filtrate obtained by thermally decomposing a sample with acid. C and S may be measured by the combustion-infrared absorption method, N by the inert gas fusion-thermal conductivity method, and O by the inert gas fusion-non-dispersive infrared absorption method.
[0063] The above-mentioned chemical composition of the base steel sheet is an average value of the entire base steel sheet. However, in the non-oriented electrical steel sheet according to the present embodiment, when the base steel sheet is viewed on the cut surface and the R value calculated using the Si content, Al content, and Mn content in mass% contained in the base steel sheet as chemical composition is defined as R=9.9+12.4[Si]+10.0[Al]+6.6[Mn], it is preferable that the R value is 60 or more and 250 or less in the region from the surface to 1 / 10 of the sheet thickness, and the R value is 30 or more and less than 60 in the region from 1 / 10 of the sheet thickness to 1 / 2 of the sheet thickness based on the surface. Note that, although the above-mentioned regions are described for one sheet surface of the base steel sheet, the above conditions may be satisfied for both sheet surfaces of the base steel sheet.
[0064] In the region from the surface to 1 / 10 of the plate thickness, the R-value is preferably 65 or more, and more preferably 70 or more. In this region, the R-value is preferably 240 or less, and more preferably 230 or less. On the other hand, in the region from 1 / 10 of the plate thickness to 1 / 2 of the plate thickness based on the surface, the R-value is preferably 35 or more, and more preferably 40 or more. In this region, the R-value is preferably 58 or less, and more preferably 56 or less.
[0065] When the R-value satisfies the above conditions in the region from the surface to 1 / 10 of the plate thickness and in the region from 1 / 10 to 1 / 2 of the plate thickness, and particularly when the R-value satisfies the above conditions in the region from the surface to 1 / 10 of the plate thickness, high-frequency iron loss is favorably improved. When the R-value is controlled as above, it is presumed that the resistivity near the surface of the steel sheet is increased, and as a result, iron loss, mainly eddy current loss, which is noticeable at high frequencies when there is a skin effect is reduced.
[0066] The R-values in the region from the surface to 1 / 10 of the plate thickness and in the region from 1 / 10 of the plate thickness to 1 / 2 of the plate thickness are controlled by manufacturing conditions specific to this embodiment. The manufacturing conditions for controlling the R-values will be described in detail later.
[0067] The R-value can be confirmed by checking a cut surface parallel to the plate thickness direction with an EPMA (Electron Probe Micro Analyzer). Specifically, a test piece is cut out from the base steel plate so that the cutting direction is parallel to the plate thickness direction. The cross-sectional structure of this cut surface is observed with the EPMA at a magnification that allows the plate thickness of the base steel plate to fit within the observation field. If the plate thickness of the base steel plate does not fit within the observation field, the cross-sectional structure is observed in multiple consecutive fields of view.
[0068] The base steel sheet in the above-mentioned observation field is subjected to a line analysis along the sheet thickness direction by EPMA to determine the Si content, Al content, and Mn content in the region from the surface of the base steel sheet to 1 / 10 of the sheet thickness, and the Si content, Al content, and Mn content in the region from 1 / 10 of the sheet thickness to 1 / 2 of the sheet thickness. From such line analysis results, the R values in the region from the surface to 1 / 10 of the sheet thickness and the region from 1 / 10 of the sheet thickness to 1 / 2 of the sheet thickness can be determined. Note that 1 / 2 of the sheet thickness corresponds to the center in the sheet thickness direction of the base steel sheet on the above-mentioned cut surface.
[0069] [Manufacturing method of non-oriented electrical steel sheets] An example of a method for manufacturing the non-oriented electrical steel sheet according to the present embodiment will be described below. Note that the manufacturing method of the non-oriented electrical steel sheet according to the present embodiment is not particularly limited as long as it has the above-mentioned configuration. The manufacturing method described below is one example for manufacturing the non-oriented electrical steel sheet according to the present embodiment, and is a suitable example of the method for manufacturing the non-oriented electrical steel sheet according to the present embodiment.
[0070] For example, the method for manufacturing the non-oriented electrical steel sheet according to this embodiment may include a casting step, a hot rolling step, a cold rolling step, a finish annealing step, a nitriding annealing step, and a coating forming step.
[0071] Specifically, the method for producing the non-oriented electrical steel sheet according to this embodiment includes the steps of: The method includes a casting process, a hot rolling process, a cold rolling process, a finish annealing process, a nitriding annealing process, and a coating process, In the casting process, the chemical composition is, in mass%, Si: 1.0% or more and 5.0% or less, C: 0% or more and 0.0050% or less, Mn: 0% or more and 3.0% or less, P: 0% or more and 0.30% or less, S: 0% or more and 0.010% or less, Al: 0% or more and 3.0% or less, Zn: 0% or more and 0.10% or less, N: 0% or more and 0.010% or less, Sn: 0% or more and 0.10% or less, Sb: 0% or more and 0.10% or less, Ca: 0% or more and 0.010% or less, Cr: 0% or more and 5.0% or less, Ni: 0% or more and 5.0% or less, Cu: 0% or more and 5.0% or less, Ce: 0% or more and 0.10% or less, B: 0% or more and 0.10% or less, O: 0% or more and 0.10% or less, Mg: 0% or more and 0.10% or less, Ti: 0% or more and 0.10% or less, V: 0% or more and 0.10% or less, Zr: 0% or more and 0.10% or less, Nd: 0% or more and 0.10% or less, Bi: 0% or more and 0.10% or less, W: 0% or more and 0.10% or less, Mo: 0% or more and 0.10% or less, Nb: 0% or more and 0.10% or less, Y: 0% or more and 0.10% or less and the balance being Fe and impurities, In the hot rolling step, the slab is hot rolled, In the cold rolling step, the steel sheet is subjected to cold rolling, In the above-mentioned finish annealing process, In the oxidation process, the steel sheet is heated from room temperature and held in an atmosphere containing 5% by volume or more and 15% by volume or less of hydrogen with a dew point of 40°C or more and 60°C or less at a temperature range of 170°C or more and 190°C or less for 90 seconds or more and 110 seconds or less. In the heating process, the steel sheet after the oxidation process is heated to a temperature range of 680°C to 720°C at an average heating rate of 40°C / s to 60°C / s in an atmosphere containing 5% by volume to 15% by volume of hydrogen and a dew point of 40°C to 60°C, Then, in an atmosphere containing 5% by volume or more and 25% by volume or less of hydrogen and a dew point of -20°C or more and 20°C or less, the temperature is increased to a range of 780°C or more and 1050°C or less at an average heating rate of 40°C / sec or more and 60°C / sec or less, In the soaking process, the steel sheet after the heating process is held in an atmosphere containing 5% by volume or more and 25% by volume or less of hydrogen with a dew point of -20°C or more and 20°C or less at a temperature range of 780°C or more and 1050°C or less for 10 seconds or more and 20 seconds or less, In the cooling process, the steel plate after the soaking process is cooled to a temperature range of room temperature to 720°C or lower. In the above nitriding annealing process, The steel sheet after the final annealing process is held in an atmosphere of 95% by volume or more and 100% by volume or less with a dew point of -50°C or more and 0°C or less at a temperature range of 680°C or more and 720°C or less for 70 seconds or more and 90 seconds or less, In the coating forming step, In the coating formation process, a coating is formed on the steel sheet after the nitriding annealing process, In the annealing process, the steel sheet may be held at a temperature in the range of 750° C. to 850° C. for 30 minutes to 150 minutes, as required.
[0072] The method for producing a non-oriented electrical steel sheet according to this embodiment may further include a hot-rolled sheet annealing step after the hot rolling step. The method for producing a non-oriented electrical steel sheet according to this embodiment may further include a pickling step after the hot rolling step or after the hot-rolled sheet annealing step. The method for producing a non-oriented electrical steel sheet according to this embodiment may further include a surface treatment step after the hot rolling step, the hot-rolled sheet annealing step, the pickling step, or after the cold rolling step.
[0073] A flow chart of the method for producing a non-oriented electrical steel sheet according to this embodiment is shown in Figure 2. Each step will be described in detail below.
[0074] [Casting process] In the casting process, a slab (steel billet) having the above-mentioned chemical composition may be cast. The chemical composition of the slab is substantially the same as the chemical composition of the base steel sheet of the non-oriented electrical steel sheet.
[0075] In order to finely control the average crystal grain size in the surface region from the surface of the base steel sheet of the final non-oriented electrical steel sheet to 1 / 20 of the sheet thickness, the Sn content is preferably less than 0.030%. In order to favorably nitride the steel sheet surface in the subsequent nitriding annealing process, it is preferable that Sn does not segregate in the surface layer of the steel sheet or that the Sn content itself is low.
[0076] The casting method is not particularly limited, but for example, a slab may be produced by a continuous casting method, or an ingot may be produced by using molten steel and then blooming the ingot to produce a slab. Alternatively, a slab may be produced by other methods.
[0077] The thickness of the slab is not particularly limited, but may be, for example, 150 mm or more and 350 mm or less. The thickness of the slab is preferably 220 mm or more and 280 mm or less. As the slab, a so-called thin slab having a thickness of 10 mm or more and 70 mm or less may be used.
[0078] In order to favorably control the {100} plane strength and the area ratio of {100} oriented grains at half the plate thickness of the base steel sheet of the final non-oriented electrical steel sheet, a thin slab continuous casting method is adopted, the slab thickness is set to 30 mm or more and 60 mm or less, columnar grains in which the {100} plane is parallel to the steel sheet surface are sufficiently developed in the thin slab, and the {100} obtained by processing the columnar grains by hot rolling is used. <011> It is preferable to leave the orientation in the hot-rolled sheet. For this purpose, it is preferable not to perform electromagnetic stirring in the continuous casting, and it is also preferable to reduce fine inclusions in the molten steel that promote solidification nucleation as much as possible.
[0079] The fine inclusions in molten steel can be reduced, for example, by reducing the content of elements that form the fine inclusions, such as Ti. The fine inclusions in molten steel can be measured, for example, by quenching a sample taken from the molten steel to obtain a steel ingot, subjecting the ingot to electrolytic extraction, and analyzing the residue.
[0080] [Hot rolling process] In the hot rolling process, the slab is hot rolled to obtain a hot rolled steel sheet. The hot rolling conditions are not particularly limited, but for example, the thickness (finishing thickness) of the hot rolled steel sheet is preferably 1.0 mm or more and 2.5 mm or less. If the thickness is 1.0 mm or more, the load on the hot rolling machine is small, and the productivity in the hot rolling process is high.
[0081] The heating temperature of the slab before hot rolling is not particularly limited, but may be 1000° C. or more and 1300° C. or less from the viewpoint of costs, etc. In the finish hot rolling after the rough rolling, the final rolling temperature of the finish hot rolling is preferably 900° C. or more, and more preferably 950° C. or more.
[0082] [Cold rolling process] In the cold rolling process, the steel sheet is cold-rolled to obtain a cold-rolled steel sheet. In the cold rolling process, the thickness (finishing thickness) of the cold-rolled steel sheet may be 0.10 mm or more and 0.35 mm or less. The steel sheet to be cold-rolled may be any of a steel sheet after a hot rolling process, a steel sheet after a hot-rolled sheet annealing process, a steel sheet after a pickling process, and a steel sheet after a surface treatment process.
[0083] Other cold rolling conditions are not particularly limited, but for example, the cumulative reduction in cold rolling is preferably 60% to 95%. When the reduction is 60% or more, the effect of P on the texture of the non-oriented electrical steel sheet can be more stably obtained. Also, when the reduction is 95% or less, the non-oriented electrical steel sheet can be stably produced on an industrial scale.
[0084] The temperature of the steel sheet during cold rolling may be room temperature. Alternatively, the cold rolling may be warm rolling in which the steel sheet temperature is 100° C. to 200° C. In order to heat the steel sheet to a temperature of 100° C. to 200° C., the steel sheet may be preheated or the rolls may be preheated.
[0085] [Finishing annealing process] In the final annealing step, the steel sheet may be subjected to an oxidation step, a temperature increase step, a soaking step, and a cooling step. In this final annealing step, it is preferable to perform a pretreatment for favorably nitriding the steel sheet surface in the subsequent nitriding annealing step. The steel sheet to be subjected to the final annealing may be either a steel sheet after a cold rolling step or a steel sheet after a surface treatment step.
[0086] [Oxidation process] In the oxidation process of the final annealing process, the steel sheet after the cold rolling process or the surface treatment process is held in an atmosphere containing 5% by volume or more and 15% by volume or less of hydrogen and a dew point of 40°C or more and 60°C or less at a temperature range of 170°C or more and 190°C or less for 90 seconds or more and 110 seconds or less.
[0087] The hydrogen in the atmosphere during the oxidation process is preferably 7% by volume or more, more preferably 9% by volume or more. On the other hand, the hydrogen is preferably 13% by volume or less, more preferably 11% by volume or less. The dew point of the atmosphere during the oxidation process is preferably 42°C or more, more preferably 44°C or more. On the other hand, the dew point is preferably 58°C or less, more preferably 56°C or less. The temperature range maintained during the oxidation process is preferably 173°C or more, more preferably 175°C or more. On the other hand, the temperature range is preferably 188°C or less, more preferably 185°C or less. The time during the oxidation process maintained within the above temperature range is preferably 93 seconds or more, more preferably 95 seconds or more. On the other hand, the time is preferably 108 seconds or less, more preferably 105 seconds or less.
[0088] In the above oxidation process, it is preferable that the atmosphere is a wet atmosphere so that fayalite (Fe2SiO4) is formed on the surface layer of the steel sheet. Conventionally, nitriding annealing has rarely been performed as a process after the finish annealing, and in addition, there has been no knowledge of actively forming oxides on the surface layer of the steel sheet in the finish annealing for the nitriding annealing, which is a process after the finish annealing. In addition, it has generally been thought that if oxides are formed on the surface layer of the steel sheet, nitriding is inhibited in the subsequent process. The present inventors have found that by forming fayalite on the surface layer of the steel sheet in the oxidation process of the finish annealing process, nitriding is preferably performed in the subsequent process. It is thought that this fayalite has a catalytic effect and promotes nitriding in the subsequent process.
[0089] [Temperature rise process] In the temperature rising process of the final annealing step, the steel sheet after the oxidation process may be heated to a temperature range of 680° C. to 720° C. at an average heating rate of 40° C. / sec to 60° C. / sec in an atmosphere of 5% to 15% by volume of hydrogen and a dew point of 40° C. to 60° C. After that, the steel sheet may be heated to a temperature range of 780° C. to 1050° C. at an average heating rate of 40° C. / sec to 60° C. / sec in an atmosphere of 5% to 25% by volume of hydrogen and a dew point of -20° C. to 20° C.
[0090] The hydrogen in the atmosphere in the first half of the temperature rise process is preferably 7% by volume or more, more preferably 9% by volume or more. On the other hand, this hydrogen is preferably 13% by volume or less, more preferably 11% by volume or less. The dew point of the atmosphere in the first half of the temperature rise process is preferably 42°C or more, more preferably 44°C or more. On the other hand, this dew point is preferably 58°C or less, more preferably 56°C or less. The average temperature rise rate in the first half of the temperature rise process is preferably 43°C / sec or more, more preferably 45°C / sec or more. On the other hand, this average temperature rise rate is preferably 58°C / sec or less, more preferably 55°C / sec or less. The average temperature rise rate means the value obtained by dividing the temperature rise from the temperature rise start temperature to the temperature rise end temperature by the temperature rise time from the temperature rise start temperature to the temperature rise end temperature. The temperature range in the first half of the temperature rise process is preferably 685°C or more, more preferably 690°C or more. On the other hand, this temperature range is preferably 715°C or less, and more preferably 710°C or less.
[0091] The hydrogen in the atmosphere in the latter half of the temperature rise process is preferably 7% by volume or more, more preferably 9% by volume or more. On the other hand, this hydrogen is preferably 23% by volume or less, more preferably 21% by volume or less. The dew point of the atmosphere in the latter half of the temperature rise process is preferably -18°C or more, more preferably -16°C or more. On the other hand, this dew point is preferably 18°C or less, more preferably 16°C or less. The average temperature rise rate in the latter half of the temperature rise process is preferably 43°C / sec or more, more preferably 45°C / sec or more. On the other hand, this average temperature rise rate is preferably 58°C / sec or less, more preferably 55°C / sec or less. The average temperature rise rate means the value obtained by dividing the temperature rise from the temperature rise start temperature to the temperature rise end temperature by the temperature rise time from the temperature rise start temperature to the temperature rise end temperature. The temperature range in the latter half of the temperature rise process is preferably 785°C or more, more preferably 790°C or more. On the other hand, this temperature range is preferably 1040° C. or less, and more preferably 1030° C. or less.
[0092] [Soaking process] In the soaking process of the final annealing step, the steel sheet after the heating process is soaked in an atmosphere containing 5% by volume to 25% by volume of hydrogen and having a dew point of -20°C to 20°C in a temperature range of 780°C to 1050°C for 10 seconds to 20 seconds.
[0093] The hydrogen in the atmosphere during the soaking process is preferably 7% by volume or more, more preferably 9% by volume or more. On the other hand, the hydrogen is preferably 23% by volume or less, more preferably 21% by volume or less. The dew point of the atmosphere during the soaking process is preferably -18°C or more, more preferably -16°C or more. On the other hand, the dew point is preferably 18°C or less, more preferably 16°C or less. The temperature range held during the soaking process is preferably 785°C or more, more preferably 790°C or more. On the other hand, this temperature range is preferably 1040°C or less, more preferably 1030°C or less. The time held within the above temperature range during the soaking process is preferably 12 seconds or more, more preferably 14 seconds or more. On the other hand, this time is preferably 18 seconds or less, more preferably 16 seconds or less.
[0094] [Cooling process] In the cooling process of the final annealing step, the steel sheet after the soaking process may be cooled to a temperature range of room temperature or higher and 720°C or lower.
[0095] The temperature range for cooling during the cooling process is preferably 100°C or higher, and more preferably 150°C or higher. Meanwhile, this temperature range is preferably 700°C or lower, and more preferably 650°C or lower. The average cooling rate during the cooling process is not particularly limited. However, this average cooling rate is preferably 5°C / sec or higher, and more preferably 7°C / sec or higher. Meanwhile, this average cooling rate is preferably 20°C / sec or lower, and more preferably 15°C / sec or lower. The average cooling rate means the value obtained by dividing the temperature from the soaking temperature to the completion of cooling by the cooling time from the soaking temperature to the completion of cooling.
[0096] [Nitriding annealing process] In the nitriding annealing process, the steel sheet after the finish annealing process may be held in an atmosphere of 95% by volume to 100% by volume of nitrogen with a dew point of -50°C to 0°C at a temperature range of 680°C to 720°C for 70 seconds to 90 seconds.
[0097] The nitrogen in the atmosphere of the nitriding annealing step is preferably 96% by volume or more, more preferably 97% by volume or more. On the other hand, the nitrogen is preferably 99% by volume or less, more preferably 98% by volume or less. The dew point of the atmosphere of the nitriding annealing step is preferably -45°C or more, more preferably -40°C or more. On the other hand, this dew point is preferably -5°C or less, more preferably -10°C or less. The temperature range held in the nitriding annealing step is preferably 685°C or more, more preferably 690°C or more. On the other hand, this temperature range is preferably 715°C or less, more preferably 710°C or less. The time held in the above temperature range in the nitriding annealing step is preferably 73 seconds or more, more preferably 75 seconds or more. On the other hand, this time is preferably 88 seconds or less, more preferably 85 seconds or less.
[0098] The above nitriding annealing forms nitrides (e.g., AlN) in the surface layer of the steel sheet, and the average grain size is finely controlled by these nitrides in the surface region from the surface of the base steel sheet of the final non-oriented electrical steel sheet to 1 / 20 of the sheet thickness. Conventionally, when manufacturing a non-oriented electrical steel sheet, nitrides were not actively formed in the surface layer of the steel sheet, unlike the present embodiment. In addition, it has generally been thought that the formation of nitrides in the surface layer of the steel sheet adversely affects the magnetic properties of the non-oriented electrical steel sheet. The present inventors have found that by performing nitriding annealing after finish annealing, the average grain size in the surface region of the base steel sheet of the final non-oriented electrical steel sheet is finely controlled, and as a result, the iron loss, mainly the eddy current loss, in the presence of the skin effect, which becomes significant at high frequencies, is reduced.
[0099] [Film formation process] In the coating formation step, the steel sheet after the nitriding annealing step is subjected to a coating formation process and, if necessary, an annealing process.
[0100] [Film formation process] The film formation conditions in the film formation process are not particularly limited and may be known conditions. For example, an insulating film consisting of only organic components, only inorganic components, or an organic-inorganic composite may be applied to the surface of the steel sheet to form the film. From the viewpoint of reducing the environmental load, an insulating film that does not contain chromium may be formed. The film formation process may also be a process of applying an insulating coating that exhibits adhesive properties by heating and pressing. Coating materials that exhibit adhesive properties include acrylic resins, phenolic resins, epoxy resins, and melamine resins.
[0101] [Annealing process] In the annealing process, the steel sheet may be held at a temperature in the range of 750° C. to 850° C. for 30 minutes to 150 minutes. The steel sheet subjected to the annealing process may be either a steel sheet after a coating process or a steel sheet that has been subjected to a punching process or other process to give a shape for forming an iron core after the coating process.
[0102] The temperature range maintained during the annealing process is preferably 760°C or higher, and more preferably 770°C or higher. On the other hand, this temperature range is preferably 840°C or lower, and more preferably 830°C or lower. Furthermore, the time maintained within the above temperature range during the annealing process is preferably 45 minutes or longer, and more preferably 60 minutes or longer. On the other hand, this time is preferably 135 minutes or shorter, and more preferably 120 minutes or shorter.
[0103] This annealing process removes residual strain in the steel, recrystallizes the steel, and grows the crystal grains to a preferred grain size. At this time, the average grain size in the surface region of the base steel sheet is controlled to be fine by the nitrides. The non-oriented electrical steel sheet manufactured by subjecting it to the annealing process in the coating formation step has the above-mentioned characteristics of the non-oriented electrical steel sheet.
[0104] The atmosphere in the annealing process is not particularly limited. For example, the atmosphere in the annealing process may be a nitrogen atmosphere, a hydrogen atmosphere, or a mixed atmosphere of nitrogen and hydrogen. The dew point of the atmosphere in the annealing process is preferably -50°C or higher, more preferably -40°C or higher. On the other hand, the dew point is preferably 0°C or lower, more preferably -10°C or lower.
[0105] [Hot-rolled sheet annealing process] The method for producing a non-oriented electrical steel sheet according to the present embodiment may include a hot-rolled sheet annealing step after the hot rolling step. By carrying out the hot-rolled sheet annealing, preferable magnetic properties can be obtained. This hot-rolled sheet annealing may be a heat retention treatment in which the hot-rolled steel sheet is kept at a temperature during cooling after the hot rolling.
[0106] The conditions for the hot-rolled sheet annealing are not particularly limited and may be known conditions. For example, when box annealing is performed, it is preferable to hold the sheet in a temperature range of 700° C. to 900° C. for 60 minutes to 20 hours. When continuous annealing is performed, it is preferable to hold the sheet in a temperature range of 900° C. to 1100° C. for 1 second to 180 seconds.
[0107] [Pickling process] The method for producing a non-oriented electrical steel sheet according to the present embodiment may include a pickling step after the hot rolling step or the hot-rolled sheet annealing step. The pickling step may remove scale formed on the surface of the steel sheet. The pickling conditions are not particularly limited and may be known conditions.
[0108] [Surface treatment process] The method for producing a non-oriented electrical steel sheet according to this embodiment may include a surface treatment step after the hot rolling step, the hot-rolled sheet annealing step, the pickling step, the cold rolling step, the finish annealing step, or the nitriding annealing step.
[0109] In the surface treatment process, the surface of the steel sheet may be plated with AlSi, AlMn, AlSiMn, etc. These plating alloys are diffused into the steel sheet by finish annealing, nitriding annealing, or film-forming annealing, and the R-value is preferably controlled in the region from the surface to 1 / 10 of the sheet thickness and in the region from 1 / 10 to 1 / 2 of the sheet thickness of the base steel sheet of the final non-oriented electrical steel sheet.
[0110] The Al contained in the plating disposed on the surface of the steel sheet is preferably 90% by mass or more, and more preferably 95% by mass or more. On the other hand, this Al is preferably 100% by mass or less, and more preferably 99% by mass or less. Furthermore, the Si contained in the plating disposed on the surface of the steel sheet is preferably 0.1% by mass or more, and more preferably 0.3% by mass or more. On the other hand, this Si is preferably 10% by mass or less, and more preferably 7% by mass or less. Furthermore, the Mn contained in the plating disposed on the surface of the steel sheet is preferably 0.01% by mass or more, and more preferably 0.1% by mass or more. On the other hand, this Mn is preferably 5% by mass or less, and more preferably 3% by mass or less.
[0111] The thickness of the plating applied to the surface of the steel sheet is preferably 5 μm or more, more preferably 7 μm or more. On the other hand, this thickness is preferably 30 μm or less, more preferably 25 μm or less. When plating is applied before cold rolling, the thickness of the plating is reduced to about 1 / 5 by cold rolling, so it is preferable to set the thickness taking into account the thickness reduction by cold rolling. For example, it is preferable to set the thickness within the above-mentioned numerical range of 25 μm to 35 μm.
[0112] The method for plating the surface of the steel sheet is not particularly limited, but may be, for example, hot-dip plating, electroplating, molten salt electrolysis, PVD (Physical Vapor Deposition), CVD (Chemical Vapor Deposition), etc. Among these, hot-dip plating is preferred in consideration of the fact that the steel sheet is a material for motors and the processing costs.
[0113] [Iron core] The iron core according to the present embodiment may include the above-mentioned non-oriented electromagnetic steel sheet. More specifically, the iron core may be a laminated body formed by stacking and integrating non-oriented electromagnetic steel sheets having the above-mentioned characteristics and a shape for forming the iron core. The iron core according to the present embodiment may be an integral punched core or a split core.
[0114] [Manufacturing method of iron core] The manufacturing method of the iron core according to this embodiment may include a step of stacking the non-oriented electromagnetic steel sheets described above. More specifically, the manufacturing method of the iron core may include a stacking step of stacking and integrating non-oriented electromagnetic steel sheets having the above-mentioned characteristics and a shape for forming the iron core. The number of stacked non-oriented electromagnetic steel sheets and the stacking conditions may be adjusted according to the purpose.
[0115] In addition, when the steel plate to be used in the method for manufacturing an iron core according to this embodiment does not have a shape for forming an iron core, a punching process may be performed before the lamination process to obtain a punched member by punching the steel plate. The punched shape and punching conditions of the steel plate may be adjusted according to the purpose.
[0116] Furthermore, the method for manufacturing an iron core according to this embodiment may include a stress relief annealing step after the above punching step or after the above lamination step.
[0117] When the strain relief annealing step is performed in the manufacturing method of the iron core according to the present embodiment, the annealing step of the coating step may be omitted in the manufacturing method of the non-oriented electrical steel sheet described above. For example, the steel sheet after the above-mentioned nitriding annealing step may be subjected to the coating step of the coating step, and the steel sheet after the coating step may be subjected to the punching step without being subjected to the annealing step of the coating step, and the punched member may be subjected to the lamination step. Then, the strain relief annealing step may be performed after the above-mentioned punching step or after the above-mentioned lamination step.
[0118] This stress relief annealing process removes residual strain in the steel, recrystallizes the steel, and grows the crystal grains to a preferred grain size. At this time, the average grain size in the surface region of the base steel sheet of the punched member is controlled to be fine by the above-mentioned nitrides. That is, the punched member after this stress relief annealing process (or the punched member constituting the laminate after the stress relief annealing process) has the characteristics of the non-oriented electrical steel sheet described above. Therefore, it is possible to determine whether the non-oriented electrical steel sheet extracted by disassembling the core has the characteristics of the non-oriented electrical steel sheet described above.
[0119] In the stress relief annealing step, the punched member or the laminate may be held at a temperature in the range of 750°C to 850°C for 30 minutes to 150 minutes. The atmosphere in the stress relief annealing step is not particularly limited. For example, the atmosphere in the stress relief annealing step may be a nitrogen atmosphere, a hydrogen atmosphere, or a mixed atmosphere of nitrogen and hydrogen. The dew point of the atmosphere in the stress relief annealing step may be -50°C to 0°C.
[0120] [Motor] The motor according to this embodiment may include the above-mentioned iron core. More specifically, the motor mainly includes a stator, a rotor, bearings, a bracket, and lead wires, and the motor according to this embodiment may include the above-mentioned iron core as the iron core of the stator or rotor. The motor according to this embodiment is preferably a drive motor for a hybrid drive vehicle or an electric vehicle, and is preferably a PM motor such as an IPM motor or an SPM motor.
[0121] [Motor manufacturing method] The manufacturing method of the motor according to this embodiment may include a step of laminating the above-mentioned non-oriented electromagnetic steel sheets to obtain an iron core, and a step of assembling this iron core to obtain a motor. More specifically, the manufacturing method of this motor may include a lamination step of laminating non-oriented electromagnetic steel sheets having the above-mentioned characteristics and a shape for forming an iron core to obtain an iron core, and an assembly step of assembling this iron core as a stator core or a rotor core to obtain a motor. The number of layers of the non-oriented electromagnetic steel sheets, the lamination conditions, and the assembly conditions of the iron core may be adjusted according to the purpose.
[0122] As in the above-described method for manufacturing an iron core, if the steel plate used in the method for manufacturing a motor according to this embodiment does not have a shape for forming an iron core, a punching step may be included before the lamination step, in which the steel plate is punched to obtain a punched member. The punched shape and punching conditions of the steel plate may be adjusted according to the purpose.
[0123] Also, like the above-mentioned method for manufacturing the iron core, the method for manufacturing the motor according to this embodiment may include a stress relief annealing step after the punching step or after the lamination step. When this stress relief annealing step is performed, the annealing process of the coating formation step may be omitted in the above-mentioned method for manufacturing the non-oriented electrical steel sheet. As described above, the member after this stress relief annealing step has the characteristics of the above-mentioned non-oriented electrical steel sheet. Therefore, it is possible to identify whether or not the non-oriented electrical steel sheet taken out by disassembling the motor has the characteristics of the above-mentioned non-oriented electrical steel sheet. The stress relief annealing conditions in the method for manufacturing the motor according to this embodiment may be the same as the stress relief annealing conditions in the above-mentioned method for manufacturing the iron core. EXAMPLES
[0124] The effects of one aspect of the present invention will be explained in more detail by way of examples, but the conditions in the examples are merely examples of conditions adopted to confirm the feasibility and effects of the present invention, and the present invention is not limited to these examples. Various conditions may be adopted in the present invention as long as they do not deviate from the gist of the present invention and the object of the present invention is achieved. The present invention will be explained in detail below by way of examples of the present invention and comparative examples.
[0125] Using the slabs with the adjusted chemical composition, non-oriented electrical steel sheets were manufactured by carrying out each step under the conditions shown in Tables 7 to 42. In each manufacturing process, the slabs were manufactured by a continuous casting method, and pickling was carried out after hot-rolled sheet annealing. In addition, hot-dip galvanizing was carried out as a surface treatment on the steel sheets after cold rolling, if necessary.
[0126] In addition, except for Test No. 136 shown in the table, the nitriding annealing process was performed after the final annealing process. On the other hand, Test No. 136 was performed after the nitriding annealing process. The nitriding annealing of Test No. 136 was performed in an atmosphere containing 100% nitrogen, with an atmospheric dew point of -25°C, an annealing temperature of 770°C, and an annealing time of 80 seconds. In addition, in the coating process, except for Test No. 137 shown in the table, the annealing process was carried out after the coating formation process. On the other hand, in Test No. 137, after the coating formation process, punching or the like was carried out to give a shape for forming the iron core, and then stress relief annealing was carried out at 800°C for 60 minutes as the annealing process.
[0127] In the table, "Whether electromagnetic stirring was performed or not" indicates whether electromagnetic stirring was performed during continuous casting. "Whether fine inclusions were present or not" indicates whether fine inclusions that promote solidification nucleation were present in the molten steel. "Cooling temperature" indicates the cooling completion temperature controlled when cooling the steel sheet after the soaking process. "Type of coating" indicates the type of insulating coating formed on the steel sheet after the nitriding annealing process.
[0128] The chemical composition, sheet thickness, average crystal grain size, R value, surface strength and area ratio of {100} oriented grains were measured for the manufactured non-oriented electrical steel sheets. The measurement methods are as described above. The measurement results are shown in Tables 1 to 51. The average crystal grain size and R value were equivalent on both sheet surfaces of the base steel sheet. The sheet thickness of the base steel sheet was the same as the finished sheet thickness of the steel sheet after the cold rolling process. The chemical composition of the base steel sheet of the manufactured non-oriented electrical steel sheets was the same as the chemical composition of the slab, except for Al, Si and Mn. The elements represented by "-" in the tables indicate that they were not consciously controlled or manufactured.
[0129] The magnetic flux density, magnetic permeability, and core loss characteristics of the manufactured non-oriented electrical steel sheets were evaluated.
[0130] The magnetic flux density, magnetic permeability, and iron loss characteristics were evaluated based on the Single Sheet Tester (SST) specified in JIS C2556:2015. Instead of taking test pieces of the size specified in JIS, smaller test pieces, for example, test pieces of 55 mm wide x 55 mm long, may be taken and measurements in accordance with the Single Sheet Magnetic Property Tester may be performed. If test pieces of 55 mm wide x 55 mm long cannot be taken, two test pieces of 8 mm wide x 16 mm long may be used to make a test piece of 16 mm wide x 16 mm long and to perform measurements in accordance with the Single Sheet Magnetic Property Tester. In this case, the Epstein equivalent value converted to the measurement value using the Epstein tester specified in JIS C2550:2011 may be used.
[0131] As a high magnetic field magnetic flux density, the magnetic flux density B in the rolling direction when a steel sheet is magnetized with a magnetizing force of 5000 A / m 50 The magnetic flux density B is measured in Tesla (T). 50 The magnetic flux density B was judged to be 1.60T or more. 50 However, when the magnetic flux density exceeds 1.63 T, it is determined that the high magnetic field magnetic flux density is preferably excellent.
[0132] As the high-frequency iron loss characteristics, the iron loss W in the rolling direction when a steel sheet is magnetized at 1 kHz with a magnetic flux density of 1.0 T is10 / 1k The iron loss was measured in units of W / kg. 10 / 1k The iron loss W was judged to be acceptable if it was 36W / kg or less. 10 / 1k However, it was determined that the high frequency core loss characteristics were preferably excellent when the high frequency core loss was less than 35 W / kg.
[0133] The magnetic permeability was measured in the rolling direction when the steel sheet was magnetized at 1.0 T in a DC magnetic field, and the unit of magnetic permeability was H / m. A magnetic permeability of 0.007 H / m or more was judged to be acceptable. A magnetic permeability of 0.010 H / m or more was judged to be preferably excellent, and a magnetic permeability of 0.013 H / m or more was judged to be more preferably excellent.
[0134] In addition, the commercial frequency iron loss is the iron loss W in the rolling direction when the steel sheet is magnetized at 50 Hz with a magnetic flux density of 1.5 T. 15 / 50 The iron loss was measured in units of W / kg. 15 / 50 The iron loss W was judged to be acceptable if it was 2.22 W / kg or less. 15 / 50 When the power frequency iron loss was 2.20 W / kg or less, it was determined that the power frequency iron loss was preferably excellent, and when it was less than 2.10 W / kg, it was determined that the power frequency iron loss was even more preferably excellent.
[0135] As shown in Tables 1 to 51, among Test Nos. 1 to 214, the inventive examples were all non-oriented electrical steel sheets in which the chemical composition, sheet thickness, and average crystal grain size were preferably controlled, and they were excellent in high-frequency iron loss. In addition, although not shown in the tables, the inventive examples had the same average crystal grain size in the intermediate region as the region from 1 / 20 of the sheet thickness to 1 / 10 of the sheet thickness. On the other hand, among Test Nos. 1 to 214, at least one of the chemical composition, sheet thickness, and average crystal grain size was not preferably controlled in the comparative examples. Note that the non-oriented electrical steel sheet of Test No. 124 did not have an insulating coating, and since it is clear that the magnetic properties deteriorate when non-oriented electrical steel sheets are laminated, the magnetic flux density and core loss properties were not evaluated.
[0136] Next, the manufactured non-oriented electromagnetic steel sheet was punched as necessary, and the punched parts were laminated to manufacture an iron core. The manufactured iron core contained the above-mentioned non-oriented electromagnetic steel sheet. In addition, the manufactured iron core was subjected to stress relief annealing as necessary, and the iron core was used as a stator core or a rotor core and assembled to manufacture a motor. The manufactured motor contained the above-mentioned iron core. In the above-mentioned stress relief annealing, the iron core was held in a temperature range of 750°C to 850°C for 30 minutes to 150 minutes.
[0137] The manufactured motor was connected to a load motor via a torque sensor (MAGTROL TM308). The manufactured motor was driven by supplying three-phase AC current from an inverter. The current and voltage supplied from the inverter were measured with a power meter (Yokogawa Electric Model WT1804E) and used as the input. From the torque T (unit: N m) measured by the torque sensor and the rotation speed N (rpm), 2πTN / 60 = output (W) was calculated. Efficiency (%) was calculated as output / input x 100.
[0138] The manufactured iron cores and motors had excellent torque characteristics and energy efficiency when using the non-oriented electrical steel sheets that were examples of the present invention from among the above-mentioned Test Nos. 1 to 214. On the other hand, when the manufactured iron cores and motors used the non-oriented electrical steel sheets that were comparative examples from among the above-mentioned Test Nos. 1 to 214, the torque characteristics and energy efficiency were not superior to those when using the non-oriented electrical steel sheets that were examples of the present invention.
[0139] In addition, in the case of the non-oriented electrical steel sheet of Test No. 125, the annealing temperature in the annealing process of the coating formation process was 700°C, so the average crystal grain size in the middle and central regions of the base steel sheet was not preferably controlled. However, in the motor manufactured using the non-oriented electrical steel sheet of Test No. 125, the average crystal grain size in the middle and central regions was preferably controlled by stress relief annealing, so the torque characteristics and energy efficiency as a motor were equivalent to those of the motor manufactured using the non-oriented electrical steel sheet of Test No. 9. Furthermore, the non-oriented electrical steel sheets taken out by disassembling the cores and motors manufactured using the non-oriented electrical steel sheets which were examples of the present invention among the above-mentioned Test Nos. 1 to 214 had preferably controlled chemical composition, sheet thickness, and average crystal grain size, similar to the results described above.
[0140] [Table 1]
[0141] [Table 2]
[0142] [Table 3]
[0143] [Table 4]
[0144] [Table 5]
[0145] [Table 6]
[0146] [Table 7]
[0147] [Table 8]
[0148] [Table 9]
[0149]
Table 10
[0150]
Table 11
[0151]
Table 12
[0152]
Table 13
[0153]
Table 14
[0154]
Table 15
[0155]
Table 16
[0156]
Table 17
[0157]
Table 18
[0158]
Table 19
[0159]
Table 20
[0160]
Table 21
[0161]
Table 22
[0162]
Table 23
[0163]
Table 24
[0164]
Table 25
[0165]
Table 26
[0166]
Table 27
[0167]
Table 28
[0168]
Table 29
[0169]
Table 30
[0170]
Table 31
[0171]
Table 32
[0172]
Table 33
[0173]
Table 34
[0174]
Table 35
[0175]
Table 36
[0176]
Table 37
[0177]
Table 38
[0178]
Table 39
[0179]
Table 40
[0180]
Table 41
[0181]
Table 42
[0182]
Table 43
[0183]
Table 44
[0184]
Table 45
[0185]
Table 46
[0186]
Table 47
[0187]
Table 48
[0188]
Table 49
[0189]
Table 50
[0190]
Table 51
[0191] According to the above aspects of the present invention, it is possible to provide a non-oriented electrical steel sheet with good high-frequency iron loss, and in addition, it is possible to provide an iron core including this non-oriented electrical steel sheet, a method for manufacturing an iron core, and a motor including this iron core, and a method for manufacturing a motor, which have high industrial applicability. [Explanation of symbols]
[0192] 1 Non-oriented electrical steel sheet 11 Insulation coating 12 Base steel plate 12a Surface area from the surface of the base steel plate to 1 / 20 of the plate thickness 12b Intermediate region from 1 / 20 to 1 / 4 of the thickness of the base steel plate 12c Central region from 1 / 4 to 1 / 2 of the plate thickness of the base steel plate
Claims
1. A non-oriented electrical steel sheet having a base steel sheet and an insulating coating, The base steel sheet has a chemical composition, in mass%, Si: 1.0% or more and 5.0% or less, C: 0% or more and 0.0050% or less, Mn: 0% or more and 3.0% or less, P: 0% or more and 0.30% or less, S: 0% or more and 0.010% or less, Al: 0% or more and 3.0% or less, Zn: 0% or more and 0.10% or less, N: 0% or more and 0.010% or less, Sn: 0% or more and 0.10% or less, Sb: 0% or more and 0.10% or less, Ca: 0% or more and 0.010% or less, Cr: 0% or more and 5.0% or less, Ni: 0% or more and 5.0% or less, Cu: 0% or more and 5.0% or less, Ce: 0% or more and 0.10% or less, B: 0% or more and 0.10% or less, O: 0% or more and 0.10% or less, Mg: 0% or more and 0.10% or less, Ti: 0% or more and 0.10% or less, V: 0% or more and 0.10% or less, Zr: 0% or more and 0.10% or less, Nd: 0% or more and 0.10% or less, Bi: 0% or more and 0.10% or less, W: 0% or more and 0.10% or less, Mo: 0% or more and 0.10% or less, Nb: 0% or more and 0.10% or less, Y: 0% or more and 0.10% or less with the remainder being Fe and impurities, The thickness of the base steel plate is 0.10 mm or more and 0.35 mm or less, When the base steel sheet is viewed on a cut surface whose cutting direction is parallel to the sheet thickness direction, the average crystal grain size is 10 μm or less in a surface region from the surface of the base steel sheet to 1 / 20 of the sheet thickness, The average crystal grain size is 50 μm or more and 200 μm or less in an intermediate region from 1 / 20 of the plate thickness to 1 / 4 of the plate thickness based on the surface, The average crystal grain size is 50 μm or more and 200 μm or less in a central region from 1 / 4 of the plate thickness to 1 / 2 of the plate thickness based on the surface. A non-oriented electrical steel sheet.
2. The base steel sheet has a chemical composition, in mass%, Sn: 0% or more and less than 0.030% Limited to The non-oriented electrical steel sheet according to claim 1 .
3. When the base steel sheet is viewed at the cut surface, When the R value calculated using the Si content, Al content, and Mn content in mass% contained in the base steel sheet as the chemical composition is defined as R = 9.9 + 12.4 [Si] + 10.0 [Al] + 6.6 [Mn], In the region from the surface to 1 / 10 of the plate thickness, the R value is 60 or more and 250 or less, The R value is 30 or more and less than 60 in the region from 1 / 10 of the plate thickness to 1 / 2 of the plate thickness based on the surface. The non-oriented electrical steel sheet according to claim 1 .
4. At 1 / 2 of the plate thickness based on the surface, the {100} plane intensity is 2.4 or more, and the area ratio of {100} oriented grains is 18% or more with respect to the observation field. The non-oriented electrical steel sheet according to claim 1 .
5. At 1 / 2 of the plate thickness based on the surface, the {100} plane intensity is 2.4 or more, and the area ratio of {100} oriented grains is 18% or more with respect to the observation field. The non-oriented electrical steel sheet according to claim 3 .
6. An iron core comprising the non-oriented electrical steel sheet according to any one of claims 1 to 5.
7. A method for manufacturing an iron core, comprising a step of stacking the non-oriented electrical steel sheets according to any one of claims 1 to 5.
8. A motor including the iron core according to claim 6.
9. A method for manufacturing a motor, comprising the steps of: laminating the non-oriented electrical steel sheets according to any one of claims 1 to 5 to obtain an iron core; and assembling the iron core to obtain a motor.
Citation Information
Patent Citations
Low-iron-loss non-oriented electrical steel adapting to high-frequency working condition and production method thereof
CN113512635A
Non-oriented silicon steel sheet excellent in yield strength, and it production
JP2005113252A
Clad type electromagnetic steel sheet
JP2010132938A
HIGH STRENGTH AND HIGH MAGNETIC FLUX DENSITY Fe-BASED METAL PLATE AND MANUFACTURING METHOD THEREFOR
JP2016183358A
Non-oriented electromagnetic steel plate and manufacturing method thereof
JP2019012777A