Method for modifying the surface polarity of rubber substrate
The use of chloride salts and peroxymonosulfate solutions for surface chlorination of elastomeric rubber substrates addresses the challenges of achieving strong, water-resistant bonds with non-elastomeric materials, providing a safer and more efficient alternative to traditional methods by enhancing adhesion and reducing reaction time.
Patent Information
- Application Number
- JP2021557757
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-03-29
- Filing Date
- 2020-03-23
- Publication Date
- 2024-09-19
- Estimated Expiration
- 2040-03-23
AI Technical Summary
Existing adhesive technologies for elastomeric materials face challenges in achieving strong, water-resistant bonds with non-elastomeric materials like metal, and conventional methods using organic solvents are undesirable due to health and safety concerns, while hypochlorite-based treatments suffer from stability issues and side reactions.
A method involving the use of an aqueous solution of chloride salts and peroxymonosulfate to chlorinate the surface of elastomeric rubber substrates, enhancing surface polarity and adhesion, which is safer and more efficient than traditional methods by minimizing free chlorine release and reaction time.
The method effectively increases the adhesion of common adhesives to elastomeric materials, allowing for strong bonds with metals at low curing temperatures, reducing reaction time and minimizing environmental hazards.
Smart Images

Figure 0007554205000001 
Figure 0007554205000002 
Figure 0007554205000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for modifying the surface polarity of an elastomeric rubber substrate to facilitate cold bonding with other rubber substrates or with dissimilar non-elastomeric substrates, preferably metals, by chlorinating the rubber substrate surface through treatment with a chloride-containing composition and a peroxymonosulfate-containing composition. Further aspects relate to the surface-modified rubber substrate thus obtained, a method for bonding the surface-modified rubber substrate to other substrates with an adhesive, and the bonded substrate thus obtained. [Background technology]
[0002] For various applications, preforms made of elastomeric materials need to be bonded to another elastomeric material or to a dissimilar material such as glass, metal or plastic. Achieving sufficient bond strength between these materials is difficult because existing adhesives for non-elastomeric materials do not bond or exhibit poor bonding to elastomers, and known adhesives for elastomers have poor water and steam resistance.
[0003] Although the use of hot melt adhesives can overcome some of the traditional disadvantages, most applications using epoxy adhesives require a low curing temperature, which is desirable because it saves energy and reduces the thermal impact on the substrate. In addition, it minimizes thermal stresses due to different heating rates or thermal expansion of the substrate.
[0004] In recent years, photochemical and chemical techniques such as halogenation, etching, grafting, oxidation, crosslinking, and physical methods such as corona discharge, plasma treatment, electron or ion beam treatment, flame or laser treatment, have been widely used to achieve the modification of rubber surfaces required to promote adhesion of common low-temperature curing adhesives to rubber substrates. The simplest mechanism is to mechanically roughen the surface, but its effectiveness is limited.
[0005] Regarding halogenation techniques, there are various types of surface treatments based on organic solvents (e.g. trichloroisocyanuric acid in ethyl acetate or N-haloamides in solvents) or aqueous solutions (e.g. sodium hypochlorite) known in the art. For example, US 4,500,685 A describes the use of N,N-dihalosulfonamides in a wax matrix for halogenating vulcanized rubber surfaces. WO 2000 / 05363 A1 describes the halogenation of rubber surfaces using acidified hypochlorite solutions, chlorine and hydrochloric acid in organic solvents, chlorine or fluorine-containing gases, and mixtures of two or more thereof. The use of trichloroisocyanuric acid is described, for example, by M. Virtudes Navarro-Banon in "Water-based chlorination treatment of SBS rubber soles to improve their adhesion to waterborne polyurethane adhesives in the footwear industry" (J. of Adhesion Science and Technology 2005, 19(11), pp. 947-74). All of these methods are based on activating the double bonds of the rubber chains to generate halogen-carbon atoms, increasing the surface polarity, which improves compatibility with commonly used 2K adhesives.
[0006] Existing organic solvent-based technologies are undesirable from health and safety perspectives due to the high content of toxic and flammable solvents. Hypochlorite-based technologies have been found to suffer from stability issues and side reactions that lead to reduced free oxygen reduction treatment performance. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] US 4,500,685 A [Patent Document 2] WO 2000 / 05363 A1 [Non-patent literature]
[0008] [Non-Patent Document 1] M. Virtudes Navarro-Banon, "Water-based chlorination treatment of SBS rubber soles to improve their adhesion to waterborne polyurethane adhesives in the footwear industry" (J. of Adhesion Science and Technology 2005, 19(11), pp. 947-74) Summary of the Invention [Problem to be solved by the invention]
[0009] Therefore, there is a need in the art for an alternative method that allows for halogenation of rubber surfaces to facilitate cold bonding without the drawbacks of existing methods. [Means for solving the problem]
[0010] The present invention meets this objective by providing a method for modifying the surface of an elastomeric rubber substrate using an aqueous solution of a chloride salt and an aqueous solution of a peroxymonosulfate salt. The newly discovered method is based on the property of persulfates to act as powerful oxidizing agents, which react readily with chlorides to produce sulfates and free chlorine. The free chlorine can then react with double bonds on the rubber surface, resulting in a chlorinated surface of the treated rubber substrate. This results in increased surface polarity of the rubber, improving the adhesion of commonly used adhesives to said surface.
[0011] Thus, in a first aspect, the present invention provides a method for producing a composition comprising: (a) Chloride (Cl - ), preferably sodium chloride, and a first composition which is an aqueous composition comprising peroxymonosulfate (HSO- / SO5 2- applying a second composition, which is an aqueous composition comprising a salt of an alkali metal peroxymonosulfate, more preferably potassium peroxymonosulfate (KHSO5), to the surface of the elastomeric rubber substrate; (b) optionally applying a third composition comprising activated carbon; and (c) incubating the first composition, the second composition, and optionally the third composition with a rubber substrate for a time and under conditions that permit chlorination of the elastomeric rubber surface. The present invention relates to a method for modifying the surface of an elastomeric rubber substrate, comprising:
[0012] In another aspect, the present invention relates to an elastomeric rubber substrate having a chlorinated surface obtainable by the process of the present invention.
[0013] Yet another aspect is a method of forming a bond between a first substrate and a second substrate, comprising the steps of: the first substrate is an elastomeric rubber substrate of the present invention or is an elastomeric rubber substrate obtained by the process of the present invention; the second substrate is a rubber or metal substrate; (a) applying an adhesive composition, preferably a 2K epoxy, polyurea, polyurethane or silicone adhesive, comprising a resin composition and a hardener composition to a joining surface of a rubber or metal substrate; (b) contacting the chlorinated rubber substrate surface with the metal substrate surface under pressure with the applied adhesive to form a bond; The present invention relates to a method comprising the steps of:
[0014] In yet another aspect, the present invention is directed to a bonded article obtainable by the method of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] As used herein, "at least one" refers to "at least one" of the referenced item, including 1, 2, 3, 4, 5, 6, 7, 8, 9 or more of the referenced item.
[0016] The present invention is based on the unexpected discovery by the inventors that the method described herein avoids the problems associated with the use of organic solvents, while the method of the present invention is more effective than known methods using hypochlorite, since no oxygen is generated during the reaction. In addition, due to the high reactivity of the persulfate used, the reaction time can be significantly reduced from about 8 hours for hypochlorite treatment to only about 5-60 minutes for persulfate-based reforming reactions. Finally, it has been found that the method of the present invention allows the use of higher concentrations of chloride than hypochlorite, which has stability problems at high concentrations, and therefore produces a larger amount of free chlorine, which can further enhance the performance of the method. It has also been found that the use of activated carbon advantageously binds unreacted chlorine. Thus, the release of free chlorine gas during the reaction can be minimized.
[0017] The first composition used is preferably an aqueous solution of a chloride salt and contains chloride ions. The chloride salt is preferably an alkali metal chloride salt such as potassium chloride or sodium chloride, with sodium chloride being particularly preferred due to its ready availability, cost and high solubility in water. The first composition preferably contains (Cl - It contains chloride ions at a concentration of 1M (mol / L) to 6M chloride (based on the ion), more preferably 4M to 6M chloride. The amount used is, in principle, limited only by the solubility of the salt.
[0018] In a preferred embodiment, the first composition is basic, preferably having a pH value of more than 8, more preferably more than 10, most preferably more than 12. Preferably, the first composition contains hydroxide, which is preferably added as an alkali metal hydroxide. More preferably, the first composition contains sodium hydroxide and / or potassium hydroxide, most preferably sodium hydroxide. The advantage of the further addition of hydroxide, especially sodium hydroxide and / or potassium hydroxide, is that the unreacted free chlorine released into the air is reduced. Furthermore, the additional hydroxide has the effect that the advantageous third component activated carbon is not required. Preferably, the first composition contains (OH - The aqueous solution contains hydroxide, particularly sodium hydroxide and / or potassium hydroxide, at a concentration of 0.5M (mol / L) to 3M, more preferably 1M to 3M (based on the ion).
[0019] The second composition is preferably an aqueous composition comprising peroxymonosulfate, and the peroxymonosulfate ion (HSO - / SO5 2- ). An alkali metal salt is preferred, especially potassium peroxymonosulfate (KHSO5). The concentration of the peroxymonosulfate is preferably in the range of 10M to 30M, more preferably 18 to 22M persulfate. The second composition may be a solution, but is preferably a paste of peroxymonosulfate in water. That is, the salt (e.g. potassium peroxymonosulfate) is simply wetted with water.
[0020] The first and second compositions may each include additional components in addition to the chloride and peroxymonosulfate salts, including, but not limited to, solvents, fillers, thickeners, etc. However, it is preferred that the first and second compositions are free of organic solvents, i.e., contain organic solvents at a concentration of less than 1% by volume.
[0021] The chloride-containing composition and the peroxymonosulfate-containing composition are used in amounts that maximize the production of free chlorine. The actual amounts used can be determined accordingly based on the respective concentrations of the solutions used. Typically, the first composition and the second composition are used in a weight ratio of about 3:1 to 1:3, preferably about 2:1 to 1:2, more preferably about 1.5:1 to 1:1.5, provided that the concentrations are within the ranges described herein.
[0022] In various embodiments, the amount of the first and / or second and / or third composition applied to the elastomeric rubber substrate surface is from 500 to 900 g / m 2 , preferably 600 to 700 g / m 2 This again depends on the concentrations used, but if the concentrations described herein are employed, the ranges described are particularly preferred.
[0023] The activated carbon (third composition) is preferably used in solid form, such as a powder or flakes, but may also be used in the form of an aqueous dispersion, in which case the activated carbon may contain additional ingredients as described above for the other compositions.
[0024] The incubation step (c) of the composition and the rubber surface is carried out for a length of time sufficient to allow the desired degree of surface modification. This again depends on the reaction conditions, but at ambient conditions (20° C., 1013 mbar) and using the concentrations described herein, reaction times of 5 to 60 minutes, preferably 15 to 30 minutes, have been found to be sufficient to obtain the desired halogenated surface.
[0025] Application of the composition can be by any suitable means known in the art. If the composition is a liquid, application can be by spraying, brushing, printing, dipping, casting, etc. Solid, or essentially solid, or paste compositions, such as activated carbon or water-wet peroxymonosulfate, can be applied by suitable solid application techniques.
[0026] Prior to application of the compositions described herein, the rubber substrate surface to be modified may be subjected to cleaning, degreasing, etc.
[0027] In various embodiments of the method of the present invention, the rubber surface is first cleaned to remove oil, grease and dirt. After this optional step, a second composition is applied to the surface. A cloth is then placed over the surface to which the second composition has been applied, and preferably a third composition is applied. The first composition is then applied over the cloth. The surface is then covered with a foil, such as a plastic foil or similar covering, and allowed to react for about 5-30 minutes. The foil and cloth are then removed and the surface is washed with water and cleaned / dried with a cloth. The use of a first composition containing an additional hydroxide eliminates the need for a plastic foil.
[0028] In various embodiments of the invention, the method further comprises the step of cleaning and optionally drying the substrate surface after the incubation step (c).
[0029] The elastomeric rubber substrate may be made of rubber, for example, it may be a rubber sheet or it may have an elastomeric rubber surface. Rubber materials are widely known in the art and include, but are not limited to, natural rubber (NR), ethylene-propylene-diene rubber (EPDM), ethylene propylene rubber (EPM), acrylonitrile-butadiene rubber (NBR), polychloroprene, styrene-butadiene rubber (SBR), styrene-butadiene-styrene rubber (SBS), butadiene rubber (BR), isoprene rubber (IR), styrene ethylene butylene styrene rubber (SEBS), and all other rubbers based on any two or more copolymers of styrene, butadiene, ethylene and isoprene. Natural rubber and styrene-butadiene rubber are particularly preferred.
[0030] The other substrate to be joined may be made of any material. In various embodiments, such substrates are made of the same rubber material, another rubber material, or metal. The metal substrate may be any metal. Typically, the metals are iron, steel, aluminum, and their alloys. The metal substrate may be plated with other metals, such as zinc, or may be subjected to a surface treatment, such as a conversion treatment. The metal substrate may be composed of metal or may be surface-coated with metal.
[0031] The adhesive used according to the method described herein for the bonding process can be any common adhesive used in the art for bonding rubber substrates, preferably a 2K adhesive. Commonly used adhesives are epoxy, polyurea, silicone or polyurethane based adhesives. Such 2K adhesives usually comprise a resin and a hardener as separate compositions that are typically combined just before application. These compositions are designed such that, when combined, a polymerization reaction starts and proceeds until the composition is fully cured. The behavior and time of the cure depends on the resin and hardener used.
[0032] For the use of polyisocyanate-based adhesives, such as polyurea- or polyurethane-based adhesives, the adhesive crosslinks via components containing NCO groups and acid H groups. Examples include known NCO-group-containing prepolymers or polyisocyanates as resin components, while those that can be used as hardener components are known oligomers or polymers containing OH, NH, SH, COOH groups, preferably OH and / or NH groups, that can react with the NCO groups of the resin components. In order to obtain a network, it is preferred that at least two NCO groups and at least two, especially OH groups, are contained in the crosslinking component. Also additives known per se can be included in the adhesive. These are components that can adjust or influence the properties of the adhesive.
[0033] The resin component preferably contains at least one polyisocyanate and / or at least one polyurethane prepolymer having at least two isocyanate groups or a mixture thereof. The PU prepolymer can be obtained, for example, by reacting a stoichiometric excess of at least difunctional isocyanate with the polyol component.
[0034] PU prepolymers in the sense of the present invention are reaction products of compounds having OH or NH groups with excess polyisocyanates. They are polyols known for adhesive applications or corresponding compounds having secondary and / or primary amino groups. OH-containing starting compounds are preferred. Polyols having molecular weights (number average molecular weight, MN, which can be determined by GPC) of up to 20,000 g / mol, in particular between 200 and 10,000 g / mol, are particularly suitable for the synthesis of the prepolymers. They can be, for example, polyols based on polyethers, polyesters, polyolefins, polyacrylates, alkylene polyols. In another embodiment, such compounds having NH groups are used.
[0035] Polyisocyanates known per se having two or more isocyanate groups, such as aliphatic, cycloaliphatic or aromatic isocyanates, can be used directly or as polyisocyanates in the prepolymer synthesis. In one embodiment, monomeric, oligomeric or polymeric isocyanates are used as resin components. Mixtures of prepolymers and polyisocyanates are also possible. In principle, all known polyisocyanates can be used, specific examples being the isomers of methylene diisocyanate (MDI) or toluylene diisocyanate (TDI), tetramethylxylylene diisocyanate (TMXDI), 1-isocyanatomethyl-3-isocyanato-1,5,5-trimethylcyclohexane (IPDI), naphthalene-1,5-diisocyanate (NDI), hexane-1,6-diisocyanate (HDI). At least trifunctional isocyanates obtained by trimerization or oligomerization of diisocyanates, such as isocyanurates, carbodiimides or biurets, can also be used.
[0036] The hardener component of a suitable two-component polyisocyanate-based adhesive must contain at least one compound having at least two groups that react with isocyanate groups. These may be, for example, SH, COOH, NH or OH groups. Polyols and amines are preferred.
[0037] Many polyols are suitable as polyol components for use as the hardener component of polyurethane-based adhesives. They may be, for example, polyols with 2 to 10 OH groups per molecule. They may be aliphatic or aromatic compounds, and polymers with a suitable number of OH groups may also be used. They may have primary or secondary OH groups, as long as they have a suitable reactivity with isocyanate groups. The molecular weight of such polyols may vary within a wide range and may be, for example, 500 to 10,000 g / mol. The polyols already mentioned may also be included.
[0038] Examples of such polyols are low molecular weight aliphatic polyols, preferably having 2 to 10 OH groups, in particular C2 to C36 alcohols. Another group of suitable polyols is, for example, polyethers. These are reaction products of C2 to C4 alkylene oxides with di- or trifunctional low molecular weight alcohols. Polyether polyols should in particular have a molecular weight of 400 to 5000 g / mol. OH-containing poly(meth)acrylates or polyolefins are also suitable.
[0039] Polyester polyols are another suitable group of polyol compounds for use in component B. Polyester polyols known for adhesives can be used. They can be, for example, reaction products of diols, especially low molecular weight alkylene diols or polyether diols, with dicarboxylic acids. They can be aliphatic or aromatic carboxylic acids or mixtures thereof. Such polyester polyols are known to the skilled artisan in various forms and are commercially available. These polyester polyols should in particular have a molecular weight of 200 to 3000 g / mol. These also include polymeric lactones or polyacetals, as long as they have at least two functional groups and the corresponding appropriate molecular weight.
[0040] The amine used as the hardener component for polyurea-based adhesive is preferably a sterically hindered amine.Suitable sterically hindered amines having two or more amine groups, preferably two amine groups, are aspartic acid ester amines or aromatic diamines.Examples of aromatic diamines are those that have steric hindrance to reduce reactivity when combined with the polymeric isocyanate of the resin component. Such aromatic amines include, but are not limited to, toluenediamine, 1-methyl-3,5-diethyl-2,4-diaminobenzene, 1-methyl-3,5-diethyl-2,6-diaminobenzene (also known as DETDA or diethyltoluenediamine), di(methylthio)toluenediamine, 1,3,5-triethyl-2,6-diaminobenzene, toluenediamine derivatives containing halogen, cyano, alkoxy, alkylthio, alkenyl or carbonyl groups, m-phenylenediamine, p-phenylenediamine, 4',4'-methylenedianiline, 4,4'-diaminodiphenylsulfone, 2,6-diamino-pyridine, 4,4'-methylene-bis-(3-chloroaniline), 4,4'-methylene-bis-(3-chloro-2,6-diethylaniline), 4,4 ... chloro-2,5-diethylaniline, 3,3'-di-isopropyl-4,4'-diaminodiphenylmethane, 4,4'-bis-(sec-butylamino)diphenylmethane (SBMDA), 3,5,3',5'-tetraethyl-4,4'-diaminodiphenylmethane, propylene-di-4-aminobenzoate, isobutyl 4-chloro-3,5-diaminobenzoate, bis-(2-aminophenyl)disulfide, bis-(4-aminophenyl)disulfide, 3,3'-carbomethoxy-4,4'-diaminodiphenylmethane, 1,2-bis(2-aminophenylthio)ethane, dimethylthiotoluenediamine (DMTDA), 0,1,8-diamino-p-menthane, α,α,α',α'-tetramethylxylenediamine, N,N'-ditertiary-butylethylenediamine, and mixtures thereof.
[0041] In the case of silicone-based adhesives, known one-component or two-component silicone adhesives can be used. Two-component silicone adhesives are preferred. Silicone adhesives comprise one or more poly(diorganosiloxanes). These poly(diorganosiloxanes) are crosslinkable. Crosslinking can occur via reactive end groups or by end groups of the poly(diorganosiloxanes) that can be converted into reactive groups. All common poly(diorganosiloxanes) can be used. For example, such poly(diorganosiloxanes) are well known and commercially available for the manufacture of adhesives or sealants.
[0042] The poly(diorganosiloxane) may preferably be a hydroxyl-terminated poly(diorganosiloxane) and / or an alkoxysilyl-terminated poly(diorganosiloxane). Hydroxyl-terminated poly(diorganosiloxane) and alkoxysilyl-terminated poly(diorganosiloxane) are known and commercially available. The poly(diorganosiloxane) is preferably a poly(dialkylsiloxane) in which the alkyl group preferably has 1 to 5, more preferably 1 to 3 carbon atoms, and is particularly preferably a methyl group. Hydroxyl-terminated poly(dimethylsiloxane) and methoxysilyl-terminated poly(dimethylsiloxane) are most preferred, and are preferably used in combination containing each of them in one component of the 2K silicone-based adhesive.
[0043] The silicone adhesive further comprises one or more crosslinkers for poly(diorganosiloxanes). These may be any of the crosslinkers known in the art for this purpose. For example, the crosslinker is preferably selected from tetraalkoxysilanes, organotrialkoxysilanes, diorganodialkoxysilanes and / or oligo(organoalkoxysilanes), tetrakisketoximosilanes, organotrisketoximosilanes, diorganobisketoximosilanes and / or oligo(organoketoximosilanes), or mixtures thereof, which may be optionally functionalized with one or more heteroatoms in the organyl group. Suitable examples are methyltrimethoxysilane, chloromethyltrimethoxysilane, ethyltrimethoxysilane, propyltrimethoxysilane, vinyltrimethoxysilane, methyltriethoxysilane, vinyltriethoxysilane, phenyltriethoxysilane, methyltrippropoxysilane, phenyltrippropoxysilane, tetramethoxysilane, tetraethoxysilane, tetra-n-propoxysilane, tetra-n-butoxysilane, methyltris(methylethylketoximo)silane, phenyltris(methylethylketoximo)silane, vinyltris(methylethylketoximo)silane, methyltris(isobutylketoximo)silane or tetra(methylethylketoximo)silane. Methyltrimethoxysilane, vinyltrimethoxysilane, tetraethoxysilane, methyltris(methylethylketoximo)silane, vinyltris(methylethylketoximo)silane and methyltris(isobutylketoximo)silane.
[0044] As an optional component, the silicone adhesive, more particularly the two-component silicone composition, may further comprise one or more condensation catalysts, which act as catalysts for crosslinking polydiorganosiloxane.Preferred condensation catalysts are in particular metal or metalloid complexes from group Ia, IIa, IIIa, IVa, IVb or IIb of the periodic table of the elements, such as Sn compounds, Ti compounds such as titanates, borates, and / or organyl compounds or mixtures thereof. Preferred organotin compounds are, for example, dialkyltin compounds selected from dimethyltin di-2-ethylhexanoate, dimethyltin dilaurate, di-n-butyltin diacetate, di-n-butyltin di-2-ethylhexanoate, di-n-butyltin dicaprylate, di-n-butyltin di-2,2-dimethyloctanoate, di-n-butyltin dilaurate, di-n-butyltin distearate, di-n-butyltin dimaleinate, di-n-butyltin dioleate, di-n-butyltin diacetate, di-n-octyltin di-2-ethylhexanoate, di-n-octyltin di-2,2-dimethyloctanoate, di-n-octyltin dimaleinate and di-n-octyltin dilaurate.
[0045] When using an epoxy-based adhesive in an epoxy resin composition that is a 2K epoxy adhesive, the epoxy resin may comprise any epoxy resin that is commonly known and used. Suitable epoxy resins preferably comprise epoxy resins having 1 to 10 epoxy groups per molecule. These epoxy groups may be 1,2-epoxy groups. Epoxy resins may in principle be saturated or unsaturated, cyclic or acyclic, aliphatic, alicyclic, aromatic or heterocyclic polyepoxy compounds. Examples of suitable epoxy resins include polyglycidyl ethers, which are generally prepared by reacting epichlorohydrin or epibromohydrin with polyphenols in the presence of alkali, polyglycidyl ethers of phenol formaldehyde novolac resins, alkyl-substituted phenol formaldehyde resins (epoxy novolac resins), phenol hydroxybenzaldehyde resins, cresol hydroxybenzaldehyde resins, dicyclopentadiene phenol resins, and dicyclopentadiene substituted phenol resins. Suitable polyphenols for this purpose include, for example, resorcinol, pyrocatechol, hydroquinone, bisphenol A (2,2-bis(4-hydroxyphenyl)propane), bisphenol F (bis(4-hydroxyphenyl)methane), 1,1-bis(4-hydroxyphenyl)isobutane, 4,4'-dihydroxybenzophenone, 1,1-bis(4-hydroxyphenyl)ethane, 1,5-hydroxynaphthalene. Also suitable are, for example, the diglycidyl ether of ethoxylated resorcinol (DGER) from Indspec Chemical Corporation, resorcinol, catechol, hydroquinone, bisphenol, bisphenol A, bisphenol AP (1,1-bis(4-hydroxyphenyl)-1-phenylethane), bisphenol F, bisphenol K, bisphenol M, bisphenol S, diglycidyl ether of tetramethylbiphenol; C 2~20 They are diglycidyl ethers of alkylene glycols and poly(ethylene oxide) glycol or poly(propylene oxide) glycol.
[0046] Additionally suitable epoxy resins are polyglycidyl ethers of polyalcohols or diamines, which are derived from polyalcohols such as ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propylene glycol, 1,4-butylene glycol, triethylene glycol, 1,5-pentanediol, 1,6-hexanediol or trimethylolpropane.
[0047] Other suitable epoxy resins are polyglycidyl esters of polycarboxylic acids, examples of which are the reaction products of glycidol or epichlorohydrin with aliphatic or aromatic polycarboxylic acids, such as oxalic acid, succinic acid, glutaric acid, terephthalic acid or dimer fatty acids.
[0048] Other suitable epoxy resins are derived from the epoxidation products of olefinically unsaturated alicyclic compounds, or from natural oils and fats.
[0049] In a preferred embodiment, the epoxy resin has 1 to 10 epoxy groups and is selected from the group consisting of resorcinol, catechol, hydroquinone, bisphenol, bisphenol A, bisphenol AP (1,1-bis(4-hydroxyphenyl)-1-phenylethane), bisphenol F, bisphenol K, bisphenol M, bisphenol S, diglycidyl ether of tetramethylbiphenol, C 2~20 diglycidyl ethers of alkylene glycols and poly(ethylene oxide) or poly(propylene oxide); polyglycidyl ethers of phenol formaldehyde novolac resins, alkyl substituted phenol formaldehyde resins (epoxy novolac resins), phenol hydroxybenzaldehyde resins, cresol hydroxybenzaldehyde resins, dicyclopentadiene phenolic resins and dicyclopentadiene substituted phenolic resins, and any combination thereof, preferably selected from the group consisting of diglycidyl ethers of bisphenol F, diglycidyl ethers of bisphenol A, and any combination thereof.
[0050] Particularly preferred are epoxy resins derived from the reaction of bisphenol A or bisphenol F with epichlorohydrin. It may be advantageous to use liquid epoxy resins, which are preferably based on bisphenol A and have a sufficiently low molecular weight. Epoxy resins which are liquid at room temperature generally have an epoxy equivalent weight of 150 to about 220. Such epoxy resins are available from Dow as DER TM It is commercially available under the trade name.
[0051] The resin composition may contain many other components, all of which are well known to those skilled in the art, including, but not limited to, commonly used auxiliaries and additives. Examples are fillers, plasticizers, reinforcing agents, reactive and / or non-reactive diluents, flow agents, coupling agents (e.g. silanes), adhesion promoters, humectants, tackifiers, flame retardants, wetting agents, thixotropic and / or rheological agents (e.g. fumed silica), aging and / or corrosion inhibitors, stabilizers and / or colorants. Based on the requirements of the adhesive and its use, and in view of its manufacture, flexibility, strength, and adhesive bonding to substrates, the auxiliaries and additives are added in various amounts in the composition. In various embodiments, the resin composition contains fillers and / or colorants, typically in an amount of 10% by weight or less based on the resin composition.
[0052] In various embodiments, the hardener composition comprises a compound that can crosslink with the epoxy groups on the epoxy resin. Any hardener suitable for 2K epoxy may be used. Preferred hardeners include mercaptans, polymeric amines (polyamines) and polymeric amides (polyamides), including, for example, polyamidoamines, low molecular weight amines, and combinations thereof. Adducts of the above hardeners with epoxy resins, such as the above epoxy resins, are also preferred.
[0053] In various embodiments, preferred polyamines include polyetheramine-epoxy adducts, i.e., the reaction product of a stoichiometric excess of an amine prepolymer with an epoxy resin. Polyamine curing agents tend to react slower than lower molecular weight amines, but can impart flexibility to the cured adhesive. The amine prepolymer used to form the adduct can be any amine prepolymer having at least two amine groups for crosslinking. The amine prepolymer contains primary and / or secondary amine groups, preferably primary amine groups. Suitable amine prepolymers include polyetherdiamines, polyethertriamines, and mixtures thereof. Polyetherdiamines are preferred. The polyetheramines can be linear, branched, or mixed. Branched polyetheramines are preferred. Polyetheramines of any molecular weight may be used. Molecular weights from 200 to 6000 or more are suitable. The molecular weight can be greater than 1000, or more preferably greater than 3000. Molecular weights of 3000 or 5000 are preferred.
[0054] Suitable commercially available polyetheramines that can be used for adduct formation or as such include those sold under the Jeffamine® name by Huntsman. Suitable polyetherdiamines include the D, ED and DR series of Jeffamines. These include Jeffamine D-230, D-400, D-2000, D-4000, HK-511, ED-600, ED-900, ED-2003, EDR-148 and EDR-176. Suitable polyethertriamines include the T series of Jeffamines. These include Jeffamine T-403, T-3000 and T-5000. Polyetherdiamines are preferred, with polyetherdiamines of molecular weight about 400 (e.g. Jeffamine D-400) being most preferred. Also, equivalents of any of the above may be used as partial or total replacements.
[0055] When polyamides are included, any polyamide curing agent may be used. Some preferred polyamides include the reaction products of dimerized fatty acids and polyamines. Examples of such polyamides include those available under the trade name Versamid®.
[0056] Suitable mercaptans include difunctional mercaptans, either as monomers or epoxy adducts, such as 1,8-dimercapto-3,6-dioxaoctane (DMDO), i.e., the reaction product of a stoichiometric excess of a mercaptan with an epoxy resin. Difunctional mercaptan epoxy resin adducts are particularly preferred.
[0057] The hardener composition may include a low molecular weight (non-polymeric) amine hardener. Preferred compounds include primary and / or secondary amines with molecular weights up to 300 g / mol, 250 g / mol or 200 g / mol. Aliphatic amine hardeners include those sold under the trade name Ancamine® by Evonik.
[0058] In all of the above adducts, the epoxy resin can be any of the epoxy resins described above, but is preferably a bisphenol diglycidyl ether, such as the reaction product of bisphenol A with epichlorohydrin.
[0059] Any amount of the above curing agents may be used in the present invention.
[0060] The hardener composition preferably uses one or more accelerators (catalysts) to increase the curing speed of the adhesive. The accelerators preferably work by catalyzing the reaction between the polyamine / polyamide / mercaptan hardener on the one hand and the epoxy resin on the other hand. The accelerators preferably include tertiary amines. A preferred example is 2,4,6-tris(dimethylaminomethyl)phenol, available from Cognis under the name Versamine® EH30. Other suitable polyamines are described in U.S. Pat. No. 4,659,779 (and its family of U.S. Pat. Nos. 4,713,432 and 4,734,332; and EP-A-0 197 892).
[0061] The curing accelerator may be present in an amount that adequately accelerates the cure of the epoxy adhesive. Preferably, the curing accelerator is present in an amount of less than 5% by weight, more preferably 0.5 to 2% by weight, based on the weight of the curing agent composition.
[0062] The curing temperature is preferably below 60° C., or below 50° C., or below 40° C. The epoxy adhesive composition preferably cures at ambient temperature, for example at about 20° C. or 25° C. Thus, the method of the present invention is preferably carried out at ambient temperature, i.e. within a temperature range of about 15-40° C. It is possible, but not preferred, to heat the epoxy adhesive of the present invention, for example to further shorten the curing time or to obtain a more complete cure.
[0063] As used herein, "about" in relation to a numerical value means the numerical value plus or minus 10%.
[0064] In various embodiments, the curing agent may include any one of the additives and auxiliaries described above in connection with the resin composition, such as a filler, such as calcium carbonate or silica.
[0065] In the bonding step, step (b) may be carried out at a temperature of 15 to 30° C. and a relative humidity of 85% or less.
[0066] Prior to steps (a) and / or (b) of the described bonding method, the rubber and / or metal substrate surfaces may be cleaned to remove dirt, oil, grease, etc., all of which may interfere with the bonding process. Suitable cleaning agents are well known in the art and include Loctite® SF 7063 from Henkel.
[0067] Mixing, application and / or dispensing of the adhesive can be performed using simple manual equipment or fully automated systems, all of which are known and readily available to those skilled in the art.
[0068] The step of contacting the two substrates to form a bond under pressure can be carried out using known devices such as rolls, plates or other suitable devices. In a preferred embodiment, step (b) is carried out by rolling.
[0069] In various embodiments, all steps can be automated.
[0070] As noted above, the present invention also includes articles obtained by joining two substrates in the manner described herein.
[0071] All aspects described herein with respect to the methods and compositions described herein are equally applicable to the articles of the invention, and vice versa. All references cited herein are hereby incorporated by reference in their entirety.
[0072] The present invention will now be further illustrated by the following non-limiting examples. Preferred aspects of the present invention include the following. [1] (a) Chloride (Cl - ), preferably sodium chloride, and a first composition which is an aqueous composition comprising peroxymonosulfate (HSO 5 - / SO 5 2- ), preferably an alkali metal peroxymonosulfate, more preferably potassium peroxymonosulfate (KHSO 5 applying a second composition, the second composition being an aqueous composition comprising: (b) optionally applying a third composition comprising activated carbon; and (c) incubating the first composition, the second composition, and optionally the third composition with a rubber substrate for a time and under conditions that permit chlorination of the elastomeric rubber surface. 1. A method for modifying a surface of an elastomeric rubber substrate, comprising: [2] The method according to [1], wherein the first composition is an aqueous solution of sodium chloride having a sodium chloride concentration of preferably 1 M to 6 M, more preferably 4 M to 6 M. [3] The method according to [1] or [2], wherein the second composition is an aqueous solution of a persulfate, preferably potassium monopersulfate, having a concentration of persulfate of preferably 10 M to 30 M, more preferably 18 M to 22 M. [4] The method according to any one of [1] to [3], wherein the first composition and the second composition are used in a weight ratio of about 3:1 to 1:3, preferably about 2:1 to 1:2, and more preferably about 1.5:1 to 1:1.5. [5] The amount of the first and / or second and / or third composition applied to the surface of the elastomeric rubber substrate is 500 to 900 g / m 2 , preferably 600 to 700 g / m 2 The method according to any one of [1] to [4], wherein the range is [6] The method according to any one of [1] to [5], wherein step (c) is carried out for 5 to 60 minutes, preferably 15 to 30 minutes. [7] The method according to any one of [1] to [6], further comprising a step of cleaning the surface of the substrate after the step (c). [8] The method according to any one of [1] to [7], wherein the first composition further contains a hydroxide, preferably sodium hydroxide and / or potassium hydroxide. [9] The first composition is - The method according to [8], wherein the hydroxide is present at a concentration of 0.5M (mol / L) to 3M (based on the ion).
[10] An elastomer rubber substrate having a chlorinated surface, obtained by the method according to any one of [1] to [9].
[11] A method for forming a bond between a first substrate and a second substrate, comprising the steps of: The first substrate is an elastomer rubber substrate according to the item [8] or an elastomer rubber substrate obtained by the method according to any one of the items [1] to [9]; the second substrate is a rubber or metal substrate; (a) applying an adhesive composition, preferably a 2K epoxy, polyurea, silicone or polyurethane adhesive, comprising a resin composition and a hardener composition to a joining surface of a rubber or metal substrate; (b) contacting the chlorinated rubber substrate surface with the metal substrate surface under pressure with the applied adhesive to form a bond; A method comprising:
[12] The method according to
[11] , further comprising cleaning the rubber and / or metal substrate surface prior to steps (a) and / or (b).
[13] The method according to
[11] or
[12] , wherein step (b) is carried out at a temperature of 15 to 30°C and a relative humidity of 85% or less.
[14] The method according to any one of
[11] to
[13] , wherein step (b) is carried out by rolling.
[15] A bonded article obtained by the method described in any one of [9] to
[13] . EXAMPLES
[0073] Working Example Example 1 First composition: 27% by weight sodium chloride, 73% by weight deionized water Second composition: 70% by weight potassium peroxymonosulfate (KHSO5), 30% by weight deionized water Mixing ratio of the first composition to the second composition: weight ratio 1:1 Third composition: 100% by weight of activated carbon (flakes) 2K Polyurea Adhesive Hardener composition: 100% by weight Ethacure 420 (hindered secondary amine hardener; Albemarle (USA)) Resin composition: 100% by weight of Desmodur N3900 (aliphatic polyisocyanate; Covestro, Germany) The hardener and resin were mixed in a weight ratio of 1:1.3.
[0074] preparation The sodium chloride and water were shaken until the sodium chloride was completely dissolved. The potassium peroxymonosulfate and water were mixed until the potassium peroxymonosulfate was well wetted.
[0075] method 1) The substrates to be joined (mild steel, SBR, NR) were thoroughly cleaned with Loctite 7063 (Henkel, Germany) to remove dirt, oil and grease. 2) The metal substrate was sandblasted and cleaned again with Loctite 7063. 3) A second composition containing a peroxymonosulfate was applied to the rubber surface using a plastic spatula. 4) The rubber was covered with a cloth and activated carbon was applied onto it, followed by the first composition, the surface was covered with plastic foil and allowed to react for 15 minutes. 5) The cloth and plastic foil were removed and the surface was washed with water and cleaned with a cloth. 6) The resin and hardener components of the adhesive were mixed by hand and applied as a single coat onto the metal surface for roll peel specimens or onto the rubber surface for T-peel specimens. 7) Roll peel test specimens (rubber and metal substrate) and T-peel test specimens (rubber and rubber substrate) were bonded by rolling (20°C, relative humidity less than 85%).
[0076] TIFF0007554205000001.tif29153
[0077] Example 2 First composition: 27% by weight sodium chloride, 73% by weight deionized water Second composition: 70% by weight potassium peroxymonosulfate (KHSO5), 30% by weight deionized water Mixing ratio of the first composition to the second composition: weight ratio 1:1 Third composition: 100% by weight of activated carbon (flakes) 2K epoxy adhesive Resin composition: 99% by weight of DER 356 P (bisphenol A / F based epoxy resin, Dow); 0.01% by weight of Defoamer 1244 (defoamer, Solutia); 0.99% by weight of Silane A187 (epoxy silane, Momentive) Hardener composition: 95.99 wt% Ancamine 1922A (Evonik), 3.00 wt% fumed silica, 1.00 wt% tris(dimethylaminomethyl)phenol, 0.01 wt% defoamer (Solutia) The hardener and resin were mixed in a weight ratio of 31:100.
[0078] preparation The sodium chloride and water were shaken until the sodium chloride was completely dissolved. The potassium peroxymonosulfate and water were mixed until the potassium peroxymonosulfate was well wetted. The DER356, Defoamer and epoxy silane were dispersed under dynamic vacuum using a high speed dispenser until a uniform mixture was obtained. The Ancamine 1922A, fumed silica, tris(dimethylaminomethyl)phenol and defoamer were dispersed under dynamic vacuum using a high speed dispenser until a uniform mixture was obtained.
[0079] method 1) The substrates to be joined (mild steel, SBR, NR) were thoroughly cleaned with Loctite 7063 (Henkel, Germany) to remove dirt, oil and grease. 2) The metal substrate was sandblasted and cleaned again with Loctite 7063. 3) A second composition containing a peroxymonosulfate was applied to the rubber surface using a plastic spatula. 4) The rubber was covered with a cloth and activated carbon was applied onto it, followed by the first composition, the surface was covered with plastic foil and allowed to react for 15 minutes. 5) The cloth and plastic foil were removed and the surface was washed with water and cleaned with a cloth. 6) The resin and hardener components of the adhesive were mixed by hand and applied as a single coat onto the metal surface for roll peel specimens or onto the rubber surface for T-peel specimens. 7) Roll peel test specimens (rubber and metal substrate) and T-peel test specimens (rubber and rubber substrate) were bonded by rolling (20°C, relative humidity less than 85%).
[0080] TIFF0007554205000002.tif29153
[0081] Example 3 First composition: 21% by weight sodium chloride, 8% by weight sodium hydroxide, 71% by weight deionized water Second composition: 70% by weight potassium peroxymonosulfate (KHSO5), 30% by weight deionized water Mixing ratio of the first composition to the second composition: weight ratio 1:1 2K Silicone Adhesive Hardener composition: LOCTITE SI 5610 B Resin composition: LOCTITE SI 5610 A The hardener and resin were mixed in a 1:2 volume ratio.
[0082] preparation The sodium chloride, sodium hydroxide and water were shaken until the sodium chloride was completely dissolved. The potassium peroxymonosulfate and water were mixed until the potassium peroxymonosulfate was well wetted.
[0083] method 1) The substrates to be joined (mild steel, SBR, NR) were thoroughly cleaned with Loctite 7063 (Henkel, Germany) to remove dirt, oil and grease. 2) The metal substrate was sandblasted and cleaned again with Loctite 7063. 3) A second composition containing a peroxymonosulfate was applied to the rubber surface using a plastic spatula. 4) The rubber was covered with a cloth and the first composition was applied and allowed to react for 15 minutes. 5) The cloth was removed and the surface was washed with water and cleaned with a cloth. 6) Using an air gun, the resin and hardener components of the adhesive were applied as a single coat onto the metal surface for roll peel specimens or onto the rubber surface for T-peel specimens. 7) Roll peel test specimens (rubber and metal substrate) and T-peel test specimens (rubber and rubber substrate) were bonded by rolling (20°C, relative humidity less than 85%).
[0084] TIFF0007554205000003.tif17153
Claims
1. (a) Chloride (Cl - and a first composition, which is an aqueous composition comprising a peroxymonosulfate (HSO 5 - / SO 5 2- applying a second composition, the second composition being an aqueous composition comprising: (b) optionally applying a third composition comprising activated carbon; and (c) incubating the first composition, the second composition, and optionally the third composition with an elastomeric rubber substrate.
2. A method for producing an elastomeric rubber substrate having a chlorinated surface, comprising:
2. 10. The method of claim 1, wherein the first composition is an aqueous solution of sodium chloride.
3. 3. The method of claim 1 or 2, wherein the second composition is an aqueous solution of a peroxymonosulfate salt.
4. The method according to any one of claims 1 to 3, wherein the first composition and the second composition are used in a weight ratio of from 3:1 to 1:
3.
5. The method according to any of claims 1 to 4, wherein the amount of the first and / or second and / or third composition applied to the elastomeric rubber substrate surface is in the range of 500 to 900 g / m2.
6. The method according to any one of claims 1 to 5, wherein step (c) is carried out for 5 to 60 minutes.
7. The method of any one of claims 1 to 6, further comprising the step of cleaning the substrate surface after step (c).
8. The method of any one of claims 1 to 7, wherein the first composition further comprises a hydroxide.
9. The first composition is (OH - The method of claim 8, comprising the step of: containing hydroxide at a concentration of 0.5M (mol / L) to 3M (based on ion).
10. A method for manufacturing a bonded article of a first substrate which is an elastomeric rubber substrate and a second substrate which is a rubber or metal substrate, comprising the steps of: (a) applying a first composition, which is an aqueous composition comprising chloride (Cl-), and a second composition, which is an aqueous composition comprising peroxymonosulfate (HSO5- / SO52-), to an elastomeric rubber substrate surface; (b) optionally applying a third composition comprising activated carbon; (c) incubating the first composition, the second composition, and optionally the third composition with an elastomeric rubber substrate; (d) applying the adhesive composition to a bonding surface of a rubber or metal substrate; and (e) contacting the chlorinated elastomeric rubber substrate surface with a rubber or metal substrate surface under pressure with the applied adhesive composition to obtain a bonded article. A method comprising:
11. 11. The method of claim 10, further comprising the step of cleaning the rubber and / or metal substrate surface prior to steps (d) and / or (e).
12. The method according to claim 10 or 11, wherein step (e) is carried out at a temperature of from 15 to 30° C. and a relative humidity of not more than 85%.
13. The method according to any one of claims 10 to 12, wherein step (e) is carried out by rolling.
Citation Information
Patent Citations
Rubber articles having specific rubber surface zones suitable for making signs
JP1978117080A
Bonding of vulcanized rubber with another material
JP1987041232A
Preparation of vulcanized rubber-synthetic resin composite
JP1990084310A
Method for adhesion between vulcanized rubber and hard member
JP2002069389A
Improved membrane monopersulfate treatment
JP2009543675A