Positive electrode active material and lithium ion secondary battery

By using a lithium composite oxide with Li, Ni, Co, and Mn, and adding Li3BO3, Li3PO4, or Li2SO4 to the positive electrode, the battery's cycle characteristics and lithium ion conductivity are enhanced, addressing low capacity and charge/discharge efficiency issues in lithium ion secondary batteries.

JP7554287B2Active Publication Date: 2024-09-19NGK CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2022572094
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-03-26
Filing Date
2021-12-07
Publication Date
2024-09-19
Estimated Expiration
2041-12-07

AI Technical Summary

Technical Problem

Existing lithium ion secondary batteries face issues with low capacity and charge/discharge efficiency due to low packing density of powder-dispersed positive electrodes, and all-solid-state batteries using non-oriented sintered plates exhibit poor cycle characteristics and lithium ion conductivity.

Method used

Incorporating a lithium composite oxide with a layered rock salt structure containing Li, Ni, Co, and Mn, and adding at least one of Li3BO3, Li3PO4, and Li2SO4 as additives to form a positive electrode active material, which suppresses side reactions and stress relief at the grain boundaries, enhancing cycle characteristics.

Benefits of technology

The proposed solution significantly improves the cycle maintenance rate and lithium ion conductivity in lithium ion secondary batteries, leading to higher energy density and reduced degradation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554287000007
    Figure 0007554287000007
  • Figure 0007554287000006
    Figure 0007554287000006
  • Figure 0007554287000009
    Figure 0007554287000009
Patent Text Reader

Abstract

Provided is a positive electrode active material that is capable of dramatically improving cycle characteristics when incorporated into a lithium-ion secondary battery. This positive electrode active material includes a lithium composite oxide having a layered rock-salt structure including Li, Ni, Co, and Mn, said positive electrode active material further including at least one additive selected from Li3BO3, Li3PO4, and Li2SO4.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a positive electrode active material used in a lithium ion secondary battery, and to a lithium ion secondary battery. [Background technology]

[0002] As a positive electrode active material layer for a lithium ion secondary battery, a powder dispersion type positive electrode obtained by kneading and molding a powder of a lithium composite oxide (typically a lithium transition metal oxide) with additives such as a binder and a conductive agent is widely known. Such a powder dispersion type positive electrode contains a relatively large amount (for example, about 10% by weight) of a binder that does not contribute to the capacity, so the packing density of the lithium composite oxide as the positive electrode active material is low. For this reason, the powder dispersion type positive electrode has a large room for improvement in terms of capacity and charge / discharge efficiency. Therefore, attempts have been made to improve the capacity and charge / discharge efficiency by forming the positive electrode or the positive electrode active material layer from a lithium composite oxide sintered plate. In this case, since the positive electrode or the positive electrode active material layer does not contain a binder, it is expected that a high capacity and good charge / discharge efficiency can be obtained by increasing the packing density of the lithium composite oxide.

[0003] In addition, in lithium ion secondary batteries, a liquid electrolyte (electrolytic solution) using a flammable organic solvent as a diluting solvent has been conventionally used as a medium for transferring ions. In batteries using such an electrolyte, problems such as leakage of the electrolyte, fire, explosion, etc. may occur. In order to solve such problems, and to ensure essential safety, development of all-solid-state batteries is being promoted in which a solid electrolyte is used instead of a liquid electrolyte and all other elements are composed of solids. Since such all-solid-state batteries use a solid electrolyte, there is no risk of fire, they do not leak, and they are less likely to cause problems such as deterioration of battery performance due to corrosion.

[0004] Various all-solid-state batteries using a sintered body electrode and a solid electrolyte have been proposed. For example, in Patent Document 1 (WO2019 / 093222A1), an oriented positive electrode plate that is a lithium composite oxide sintered plate with a porosity of 10 to 50%, contains Ti, and can insert and desorb lithium ions at 0.4 V (vs. Li / Li + ), a negative electrode plate, and a solid electrolyte having a melting point lower than the melting point or decomposition temperature of the oriented positive electrode plate or the negative electrode plate are provided. A disclosed all-solid-state lithium battery. This document discloses various materials such as Li3OCl and xLiOH·yLi2SO4 (where x + y = 1 and 0.6 ≦ x ≦ 0.95) (for example, 3LiOH·Li2SO4) as such solid electrolytes having a low melting point. Such a solid electrolyte can penetrate into the voids of the electrode plate as a melt, and strong interfacial contact can be realized. As a result, it is said that a remarkable improvement in battery resistance and rate performance during charge and discharge, as well as a significant improvement in battery manufacturing yield can be achieved. Further, in Patent Document 2 (WO2015 / 151566A1), Li p (Ni x ,Co y ,Mn z )O2 (where 0.9 ≦ p ≦ 1.3, 0 < x < 0.8, 0 < y < 1, 0 ≦ z ≦ 0.7, x + y + z = 1), an oriented positive electrode plate having a layered rock salt structure of a basic composition, a solid electrolyte layer composed of a Li-La-Zr-O-based ceramic material and / or a lithium phosphate oxynitride (LiPON)-based ceramic material, and a negative electrode layer are provided. A disclosed all-solid-state lithium battery.

Prior Art Documents

Patent Documents

[0005]

Patent Document 1

Patent Document 2

Summary of the Invention

[0006] The present inventors have found that, among the above-mentioned low melting point solid electrolytes, LiOH·Li2SO4-based solid electrolytes such as 3LiOH·Li2SO4 exhibit high lithium ion conductivity. However, as disclosed as a comparative example in Patent Document 1, when a cell is constructed using a LiOH·Li2SO4-based solid electrolyte such as 3LiOH·Li2SO4 in a non-oriented sintered plate electrode and operated as a battery, there is a problem that the cycle characteristics are reduced. Since a non-oriented sintered plate has the advantage that the raw material powder is not easily restricted in controlling the microstructure such as the pore size, it would be convenient if the cycle characteristics could be improved using a non-oriented sintered plate. However, it goes without saying that the improvement of cycle characteristics is desired not only in sintered plate electrodes but also in composite electrodes.

[0007] The present inventors have now discovered that the cycle characteristics can be significantly improved by adding at least one additive selected from Li3BO3, Li3PO4, and Li2SO4 to a lithium composite oxide used in the positive electrode of a lithium ion secondary battery.

[0008] Therefore, an object of the present invention is to provide a positive electrode active material that can significantly improve the cycle characteristics when incorporated into a lithium ion secondary battery.

[0009] According to one aspect of the present invention, there is provided a positive electrode active material for use in a lithium ion secondary battery, comprising: The positive electrode active material includes a lithium composite oxide having a layered rock salt structure containing Li, Ni, Co, and Mn, and further includes at least one additive selected from Li3BO3, Li3PO4, and Li2SO4.

[0010] According to another aspect of the present invention, A positive electrode layer containing the positive electrode active material; a negative electrode layer including a negative electrode active material; a LiOH·Li2SO4-based solid electrolyte interposed between the positive electrode layer and the negative electrode layer; A lithium ion secondary battery is provided, comprising: [Brief description of the drawings]

[0011] [Figure 1] These are electron microscope photographs and EPMA mapping images of the cross section of the positive electrode active material (NCM) / solid electrolyte of the all-solid-state battery produced in Example 3. The image on the far left is the electron microscope photograph (the white parts correspond to the NCM, and the black parts to the solid electrolyte), and from there to the right, the EPMA mapping images of Mn, Co, and Ni are shown in order. [Diagram 2] Electron microscope photographs and EPMA mapping images of the cross section of the positive electrode active material (NCM) / solid electrolyte of the all-solid-state battery produced in Example 14. The image on the far left is the electron microscope photograph (the white parts correspond to the NCM, and the black parts correspond to the solid electrolyte), and EPMA mapping images of Mn, Co, and Ni are shown in order from there to the right. [Diagram 3] 1 is an electron microscope photograph (backscattered electron image) of a cross section of the positive electrode plate produced in Example 8. [Figure 4] 1 is an electron microscope photograph (backscattered electron image) of a cross section of a positive electrode plate produced in Example 12 after being filled with resin. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] positive electrode active material The positive electrode active material according to the present invention is used in a lithium ion secondary battery. This positive electrode active material includes a lithium composite oxide having a layered rock salt structure containing Li, Ni, Co, and Mn. This positive electrode active material further includes at least one additive selected from Li3BO3, Li3PO4, and Li2SO4. In this way, by incorporating at least one additive selected from Li3BO3, Li3PO4, and Li2SO4 into the lithium composite oxide used in the lithium ion secondary battery, the cycle characteristics (particularly the cycle retention rate) can be significantly improved.

[0013] As mentioned above, when a cell is constructed using a LiOH·Li2SO4-based solid electrolyte such as 3LiOH·Li2SO4 on a non-oriented sintered electrode and operated as a battery, there is a problem that the cycle characteristics are deteriorated. However, this invention conveniently solves this problem. For example, a lithium ion secondary battery having a positive electrode layer containing a positive electrode active material containing a lithium composite oxide to which at least one selected from Li3BO3, Li3PO4, and Li2SO4 is added, a LiOH·Li2SO4-based solid electrolyte, and a negative electrode layer has a higher cycle retention rate than a battery using an additive-free lithium composite oxide for the positive electrode. The mechanism is not clear, but is thought to be as follows. First, it is speculated that the causes of the deterioration of the cycle characteristics are (1) a side reaction occurs at the interface between the positive electrode and the solid electrolyte during charging and discharging, causing the solid electrolyte to deteriorate, and (2) fine cracks occur at the grain boundaries of the lithium composite oxide due to the expansion and contraction of the lithium composite oxide accompanying charging and discharging. In this regard, in the present invention, it is presumed that Li3BO3, Li3PO4 and / or Li2SO4 precipitated on at least a part of the surface of the lithium composite oxide suppresses side reactions against the above factor (1). Also, it is presumed that Li3BO3, Li3PO4 and / or Li2SO4 precipitated on at least a part of the grain boundaries relieves the stress of expansion and contraction against the above factor (2). Therefore, it is preferable that the additive is present in a state of being precipitated on at least a part of the grain boundaries and surface of the lithium composite oxide.

[0014] The positive electrode active material includes a lithium composite oxide having a layered rock-salt structure containing Li, Ni, Co, and Mn. This lithium composite oxide is also called lithium cobalt-nickel-manganese oxide, and is abbreviated as NCM. The layered rock-salt structure refers to a crystal structure in which lithium layers and transition metal layers other than lithium are alternately stacked with oxygen layers sandwiched between them (typically an α-NaFeO2 type structure: a structure in which transition metals and lithium are regularly arranged in the

[0111] axis direction of a cubic rock-salt type structure). A typical NCM is a p (Ni x ,Co y ,Mn z)O2 (where 0.9 ≦ p ≦ 1.3, 0 < x < 0.8, 0 < y < 1, 0 ≦ z ≦ 0.7, and x + y + z = 1, preferably 0.95 ≦ p ≦ 1.10, 0.1 ≦ x < 0.7, 0.1 ≦ y < 0.9, 0 ≦ z ≦ 0.6, and x + y + z = 1), for example, Li(Ni 0.5 Co 0.2 Mn 0.3 )O2 and Li(Ni 0.3 Co 0.6 Mn 0.1 )O2. Therefore, the molar ratio of Li / (Ni + Co + Mn) in the positive electrode active material is preferably 0.95 to 1.10, more preferably 0.97 to 1.08, and even more preferably 0.98 to 1.05.

[0015] As described above, the positive electrode active material according to the present invention is used in a lithium-ion secondary battery, and the positive electrode is preferably in the form of a sintered plate obtained by sintering a positive electrode raw material powder. That is, the positive electrode active material is preferably in the form of a sintered plate. In other words, the positive electrode active material preferably has a structure in which a plurality of primary particles having a layered rock salt structure containing Li, Ni, Co, and Mn are bonded. Since the sintered plate does not need to contain an electron conduction auxiliary agent or a binder, the energy density of the positive electrode can be increased. The sintered plate may be a dense body or a porous body, and the pores of the porous body may contain a solid electrolyte. However, the positive electrode may generally be in the form of a mixture of a positive electrode active material, an electron conduction auxiliary agent, a lithium ion conductive material, a binder, etc., which is generally called a composite electrode, or a mixture of a positive electrode active material, a LiOH·Li2SO4-based solid electrolyte, an electron conduction auxiliary agent, etc. (in the form of a composite material). In this case, the positive electrode active material may be in the form of a powder. Therefore, the positive electrode active material may be a mixed powder containing a powder of a lithium composite oxide and at least one powder selected from Li3BO3, Li3PO4, and Li2SO4.

[0016] The content of the additive in the positive electrode active material (i.e., the content ratio of the additive to the total content of the lithium composite oxide and the additive) is preferably 0.1 to 10% by weight, more preferably 0.5 to 7.0% by weight, and even more preferably 1.0 to 6.0% by weight, regardless of the form of the positive electrode (sintered plate or composite material), from the viewpoint of improving cycle characteristics. It is considered that the above content of the additive is almost the same between the amount of additive charged when preparing the positive electrode active material and the content of the additive in the finally obtained positive electrode active material. This can be inferred from the fact that there is almost no weight change when the additive alone is subjected to thermogravimetry (TG), for example.

[0017] When the positive electrode active material is in the form of a sintered plate, the sintered plate is measured by X-ray diffraction (XRD), and the diffraction intensity I due to the (104) plane in the XRD profile is

[0104] Diffraction intensity due to (003) plane for I

[0003] The degree of orientation I is defined as the ratio of

[0003] / I

[0104] is 1.2 to 3.6, preferably 1.2 to 3.5, more preferably 1.2 to 3.0, and further preferably 1.2 to 2.6. Here, lithium composite oxides having a layered rock salt type crystal structure such as NCM have crystal faces (faces other than the (003) face, for example the (101) face and (104) face) where lithium ions can easily enter and exit, and the (003) face where this is not the case. In this specification, the diffraction intensities by XRD of the (003) face and the (104) face are used as indexes for calculating the degree of orientation for the sake of convenience. When the sintered plate has an orientation degree I within the above-mentioned range,

[0003] / I

[0104] Then, the degree of orientation of the NCM powder, I

[0003] / I

[0104] Since this value is equivalent to or close to (for example, 1.4 (composition of Ni:Co:Mn=5:2:3) or 2.3 (composition of Ni:Co:Mn=3:6:1)), it can be said to be close to non-oriented (random), that is, essentially not oriented (or not very oriented). As mentioned above, non-oriented sintered bodies have the advantage that they are less subject to the limitations of the raw material powder when controlling the microstructure such as pore size, and this makes it easier to select raw material powders that are favorable for controlling the microstructure (pore size, for example) of the sintered body, making it easier to achieve improved cycle characteristics.

[0018] When the positive electrode active material is in the form of a sintered plate, the porosity of the sintered plate is preferably 20 to 40%, more preferably 20 to 38%, further preferably 20 to 36%, and particularly preferably 20 to 33%. Within such ranges, when a battery is produced, the pores can be sufficiently filled with the solid electrolyte, and the proportion of the positive electrode active material in the positive electrode increases, so that a high energy density of the battery can be realized.

[0019] In this specification, the term "porosity" refers to the volume ratio of pores in a sintered plate. This porosity can be measured by image analysis of a cross-sectional SEM image of the sintered plate. For example, the sintered plate is filled with resin, the cross-section is polished by ion milling, and then the polished cross-section is observed with a SEM (scanning electron microscope) to obtain a cross-sectional SEM image (for example, 500 to 1000 times magnification). The obtained SEM image is analyzed to calculate the ratio (%) of the area of ​​the part filled with resin to the total area of ​​the part of the electrode active material and the part filled with resin (the part that was originally a pore), and the porosity (%) of the sintered plate can be calculated. If the measurement can be performed with the desired accuracy, the porosity may be measured without filling the sintered plate with resin. For example, the porosity of a sintered plate (a positive electrode plate taken out of an all-solid-state secondary battery) whose pores are filled with a solid electrolyte can be measured while the solid electrolyte is still filled.

[0020] When the positive electrode active material is in the form of a sintered plate, the average pore size of the sintered plate is preferably 3.5 μm or more, more preferably 3.5 to 15.0 μm, even more preferably 3.5 to 10.0 μm, and particularly preferably 3.5 to 8.0 μm. Within such a range, the solid electrolyte portion (solid electrolyte portion at a distance away from the interface) that is less susceptible to deterioration due to side reactions between the solid electrolyte and the lithium composite oxide increases. Therefore, it is considered that element diffusion between the solid electrolyte and the lithium composite oxide is suppressed, the decrease in Li ion conductivity due to deterioration of the solid electrolyte is mitigated, and the discharge capacity and cycle characteristics are more effectively improved.

[0021] In this specification, the "average pore diameter" refers to the average value of the diameters of the pores contained in the sintered plate of the electrode. The "diameter" is typically the length of a line segment that bisects the projected area of ​​the pore (Martin diameter). In the present invention, the "average" is suitably calculated based on the number of pores. This average pore diameter can be measured by image analysis of a cross-sectional SEM image of the sintered plate. For example, the SEM image obtained in the above-mentioned porosity measurement is analyzed to separate the electrode active material portion and the resin-filled portion (the portion that was originally a pore) in the sintered plate, and then the maximum Martin diameter of each region in the resin-filled portion is obtained, and the average value of these is taken as the average pore diameter of the sintered plate. If the measurement can be performed with the desired accuracy, the average pore diameter may be measured without filling the sintered plate with resin. For example, the average pore diameter of a sintered plate (a positive electrode plate taken out of an all-solid-state secondary battery) whose pores are filled with a solid electrolyte can be measured while the solid electrolyte is still filled.

[0022] When the positive electrode active material is in the form of a sintered plate, the unit cross-sectional area of ​​the sintered plate is 1 μm 2The interface length per unit area is preferably 0.45 μm or less, more preferably 0.10 to 0.40 μm, further preferably 0.10 to 0.35 μm, and particularly preferably 0.10 to 0.30 μm. Within such a range, the number of places where side reactions occur between the lithium composite oxide and the solid electrolyte is reduced. Therefore, it is considered that element diffusion between the solid electrolyte and the lithium composite oxide is suppressed, the decrease in Li ion conductivity due to deterioration of the solid electrolyte is mitigated, and the discharge capacity and cycle characteristics are more effectively improved.

[0023] In this specification, "unit cross-sectional area 1 μm 2 The "interface length per unit cross-sectional area of ​​the sintered plate" is 2 It is the total length of all pore / active material interfaces contained in the unit cross-sectional area per unit cross-sectional area. This interface length can be measured by image analysis of a cross-sectional SEM image of the sintered plate. For example, the SEM image obtained in the above-mentioned porosity measurement is analyzed to separate the electrode active material portion and the resin-filled portion (the portion that was originally a pore) in the sintered plate, and then, in the region of the resin-filled portion, the perimeter of the entire region (i.e., the total length of the interfaces between the positive electrode active material portion and the resin-filled portion) and the area of ​​the entire analyzed region (i.e., the region consisting of both the positive electrode active material portion and the resin-filled portion) are calculated. The perimeter is then divided by the area of ​​the entire analyzed region to obtain the unit cross-sectional area of ​​1 μm. 2 If the measurement can be performed with the desired accuracy, the interface length may be measured without filling the sintered plate with resin. For example, the interface length of a sintered plate (a positive electrode plate removed from an all-solid-state secondary battery) whose pores are filled with a solid electrolyte can be measured while the solid electrolyte is still filled.

[0024] Regardless of the form of the positive electrode (sintered plate or composite material), the thickness of the positive electrode is preferably 30 to 300 μm, more preferably 50 to 300 μm, and further preferably 80 to 300 μm, from the viewpoint of improving the energy density of the battery.

[0025] Manufacturing method of lithium composite oxide sintered plate The lithium composite oxide sintered plate according to a preferred embodiment of the present invention may be produced by any method, but is preferably produced through (a) the preparation of an NCM raw material powder, (b) the preparation of an NCM green sheet, and (c) the sintering of the NCM green sheet.

[0026] (a) Preparation of NCM raw powder First, the NCM raw material powder is prepared. The preferred NCM raw material powder is Li(Ni 0.5 Co 0.2 Mn 0.3 )O2 powder, or Li(Ni 0.3 Co 0.6 Mn 0.1 )O2 powder. Li(Ni 0.5 Co 0.2 Mn 0.3 The Li / (Ni+Co+Mn) molar ratio was 1.00 to 1.30. 0.5 Co 0.2 Mn 0.3 It can be prepared by mixing Li(OH)2 powder and Li2CO3 powder and then sintering the mixture at 700 to 1200°C (preferably 750 to 1000°C) for 1 to 24 hours (preferably 2 to 15 hours). 0.3 Co 0.6 Mn 0.1 The Li / (Ni+Co+Mn) molar ratio was 1.00 to 1.30. 0.3 Co 0.6 Mn 0.1 It can be preferably produced by mixing (OH)2 powder and Li2CO3 powder, and then firing the mixture at 700 to 1200°C (preferably 750 to 1000°C) for 1 to 24 hours (preferably 2 to 15 hours).

[0027] In order to control the specific microstructure (particularly pores) in the lithium composite oxide sintered plate of this embodiment, it is preferable to prepare a larger NCM raw material powder having a volumetric D50 particle size of 3 to 20 μm (preferably 5 to 15 μm) and a smaller NCM raw material powder having a volumetric D50 particle size of 0.05 to 1 μm (preferably 0.1 to 0.6 μm) and mix them to obtain a mixed powder. The proportion of the larger NCM raw material powder in these two types of mixed powders, large and small, is preferably 50 to 99% by weight, more preferably 70 to 95% by weight. The smaller NCM raw material powder may be prepared by pulverizing the larger NCM raw material powder by a known method such as a ball mill.

[0028] Additives such as Li3BO3, Li3PO4, and Li2SO4 may be added to the sintered NCM raw material powder prepared as described above, or (Ni 0.5 Co 0.2 Mn 0.3 )(OH)2 powder and (Ni 0.3 Co 0.6 Mn 0.1 The additive may be added to the NCM precursor powder before calcination, such as 2-compound NCM precursor powder, such as 2-compound NCM precursor powder, 2-compound NCM precursor powder, or 2-compound NCM precursor powder. When preparing the two types of mixed powder, large and small, as described above, the additive may be added to at least one of the larger NCM raw material powder and the smaller NCM raw material powder.

[0029] (b) Preparation of NCM green sheets A paste is prepared by mixing an NCM raw material powder (preferably the above-mentioned NCM mixed powder), a solvent, a binder, a plasticizer, and a dispersant. The viscosity of the paste is adjusted, and the paste is then formed into a sheet to produce an NCM green sheet.

[0030] (c) Preparation of NCM sintered plate The NCM green sheet thus produced is cut into a desired size and shape, placed in a sintering sheath, and sintered. The sintering is desirably performed by increasing the temperature to 800-1000°C (preferably 850-970°C) at a rate of 50-600°C / h (preferably 100-300°C / h) and holding the temperature for 1-24 hours (preferably 2-12 hours). In this way, a lithium composite oxide sintered plate (NCM sintered plate) is obtained.

[0031] Lithium-ion secondary battery The positive electrode active material according to the present invention is used in a lithium ion secondary battery (typically an all-solid-state battery). Therefore, according to a preferred embodiment of the present invention, a lithium ion secondary battery is provided that includes a positive electrode layer containing the positive electrode active material of the present invention, a negative electrode layer, and a LiOH·Li2SO4-based solid electrolyte. The negative electrode layer contains the negative electrode active material. The LiOH·Li2SO4-based solid electrolyte is interposed between the positive electrode layer and the negative electrode layer. As described above, a lithium ion secondary battery using a lithium composite oxide to which Li3BO3, Li3PO4, and / or Li2SO4 is added in the positive electrode layer can exhibit a higher cycle retention rate than a lithium ion secondary battery using a conventional lithium composite oxide without an additive in the positive electrode layer.

[0032] The positive electrode layer is preferably in the form of a sintered plate obtained by sintering the positive electrode raw material powder. That is, the positive electrode active material is preferably in the form of a sintered plate. The sintered plate does not need to contain an electronic conductive assistant or a binder, so that the energy density of the positive electrode layer can be increased. The sintered plate may be a dense body or a porous body, and the pores of the porous body may contain a solid electrolyte. However, the positive electrode layer may be in the form of a composite material, which is generally called a composite electrode, and is a mixture of a positive electrode active material, an electronic conductive assistant, a lithium ion conductive material, a binder, etc., or a mixture of a positive electrode active material, a LiOH·Li2SO4-based solid electrolyte, an electronic conductive assistant, etc. That is, the positive electrode layer may contain particles of a positive electrode active material, particles of a LiOH·Li2SO4-based solid electrolyte, and an electronic conductive assistant in the form of a composite material. The density (filling rate) of the positive electrode active material in the composite positive electrode is preferably 50 to 80 volume %, more preferably 55 to 80 volume %, further preferably 60 to 80 volume %, and particularly preferably 65 to 75 volume %. With a density within such a range, the solid electrolyte can be sufficiently filled into the voids in the positive electrode active material, and the proportion of the positive electrode active material in the positive electrode increases, so that a high energy density as a battery can be realized. Note that the value of the density (filling rate) in this composite form corresponds to the value obtained by subtracting the proportion of the portion other than the positive electrode active material (including pores) from 100.

[0033] The negative electrode layer (typically, a negative electrode plate) contains a negative electrode active material. As the negative electrode active material, a negative electrode active material generally used in lithium ion secondary batteries can be used. Examples of such general negative electrode active materials include carbon-based materials, metals or semimetals such as Li, In, Al, Sn, Sb, Bi, and Si, or alloys containing any of these. In addition, oxide-based negative electrode active materials may be used.

[0034] Particularly preferred negative electrode active materials are those with a voltage of 0.4V (vs. Li / Li + ) or more and capable of inserting and extracting lithium ions, and preferably contains Ti. A negative electrode active material that satisfies such conditions is preferably an oxide that contains at least Ti. A preferred example of such a negative electrode active material is lithium titanate Li4Ti5O12 Examples of the lithium-ion-conducting oxide include Li4Ti5O (hereinafter sometimes referred to as LTO), niobium titanium composite oxide Nb2TiO7, and titanium oxide TiO2. More preferred are LTO and Nb2TiO7, and even more preferred is LTO. Although LTO is known to have a typical spinel structure, it can also adopt other structures during charging and discharging. For example, LTO has a structure of Li4Ti5O 12 (spinel structure) and Li7Ti5O 12 The reaction proceeds in the coexistence of two phases, i.e., spinel and tetrahydrofuran (rock salt structure). Therefore, LTO is not limited to a spinel structure.

[0035] The negative electrode may be in the form of a mixture of a negative electrode active material, an electronic conductive assistant, a lithium ion conductive material, a binder, etc., generally called a composite electrode, or a mixture of a negative electrode active material, a LiOH·Li2SO4-based solid electrolyte, an electronic conductive assistant, etc., formed into a composite. That is, the negative electrode may contain particles of a negative electrode active material, particles of a LiOH·Li2SO4-based solid electrolyte, and an electronic conductive assistant in the form of a composite. However, the negative electrode is preferably in the form of a sintered plate obtained by sintering a negative electrode raw material powder. That is, the negative electrode or the negative electrode active material is preferably in the form of a sintered plate. Since the sintered plate does not need to contain an electronic conductive assistant or a binder, the energy density of the negative electrode can be increased. The sintered plate may be a dense body or a porous body, and the pores of the porous body may contain a solid electrolyte. In the form of a composite, the preferable particle size of the negative electrode active material particles is 0.05 to 50 μm, more preferably 0.1 to 30 μm, and even more preferably 0.5 to 20 μm. The preferred particle size of the LiOH·Li2SO4-based solid electrolyte particles is 0.01 to 50 μm, more preferably 0.05 to 30 μm, and even more preferably 0.1 to 20 μm. The electron-conducting assistant is not particularly limited as long as it is an electron-conducting substance generally used in electrodes, but is preferably a carbon material. Preferred examples of the carbon material include carbon black, graphite, carbon nanotubes, graphene, reduced graphene oxide, and any combination thereof, but are not limited thereto, and various other carbon materials can also be used.

[0036] The density (filling rate) of the negative electrode active material in the negative electrode is preferably 55 to 80% by volume, more preferably 60 to 80%, and even more preferably 65 to 75%, regardless of the form of the negative electrode (sintered plate or composite). With a density within this range, the solid electrolyte can be sufficiently filled into the voids in the negative electrode active material, and the proportion of the negative electrode active material in the negative electrode increases, so that a high energy density as a battery can be realized. Note that the value of the density (filling rate) in the composite form corresponds to the value obtained by subtracting the proportion of the portion other than the negative electrode active material (including pores) from 100.

[0037] Regardless of the form of the negative electrode (sintered plate or composite material), the thickness of the negative electrode is preferably 40 to 410 μm, more preferably 65 to 410 μm, further preferably 100 to 410 μm, and particularly preferably 107 to 270 μm, from the viewpoint of improving the energy density of the battery.

[0038] The solid electrolyte is a LiOH·Li2SO4-based solid electrolyte. The LiOH·Li2SO4-based solid electrolyte is a composite compound of LiOH and Li2SO4, and has a typical composition represented by the general formula: xLiOH·yLi2SO4 (wherein x+y=1, 0.6≦x≦0.95). A representative example is 3LiOH·Li2SO4 (wherein x=0.75, y=0.25 in the above general formula). Preferably, the LiOH·Li2SO4-based solid electrolyte includes a solid electrolyte identified as 3LiOH·Li2SO4 by X-ray diffraction. This preferred solid electrolyte contains 3LiOH·Li2SO4 as the main phase. Whether or not the solid electrolyte contains 3LiOH·Li2SO4 can be confirmed by identifying it using 032-0598 of the ICDD database in the X-ray diffraction pattern. Here, "3LiOH·Li2SO4" refers to a material whose crystal structure can be regarded as the same as that of 3LiOH·Li2SO4, and the crystal composition does not necessarily have to be the same as that of 3LiOH·Li2SO4. In other words, as long as it has the same crystal structure as that of 3LiOH·Li2SO4, the material whose composition is outside of LiOH:Li2SO4=3:1 is also included in "3LiOH·Li2SO4". Therefore, even if the solid electrolyte contains a dopant such as boron (for example, 3LiOH·Li2SO4 in which boron is dissolved and the X-ray diffraction peak is shifted to the high angle side), it is referred to as 3LiOH·Li2SO4 in this specification as long as the crystal structure can be regarded as the same as that of 3LiOH·Li2SO4. Similarly, the solid electrolyte used in the present invention is also allowed to contain inevitable impurities.

[0039] Therefore, the LiOH·Li2SO4-based solid electrolyte may contain a heterogeneous phase in addition to the main phase 3LiOH·Li2SO4. The heterogeneous phase may contain a plurality of elements selected from Li, O, H, S, and B, or may consist of only a plurality of elements selected from Li, O, H, S, and B. Examples of the heterogeneous phase include LiOH, Li2SO4, and / or Li3BO3 derived from the raw materials. These heterogeneous phases are considered to be unreacted raw materials remaining when 3LiOH·Li2SO4 is formed, but since they do not contribute to lithium ion conduction, it is desirable that the amount of them other than Li3BO3 is small. However, the heterogeneous phase containing boron such as Li3BO3 may be contained in a desired amount because it can contribute to improving the lithium ion conductivity after long-term storage at high temperatures. However, the solid electrolyte may be composed of a single phase of 3LiOH·Li2SO4 in which boron is dissolved.

[0040] It is preferable that the LiOH·Li2SO4-based solid electrolyte (particularly 3LiOH·Li2SO4) further contains boron. By further containing boron in the solid electrolyte identified as 3LiOH·Li2SO4, it is possible to significantly suppress the decrease in lithium ion conductivity even after long-term storage at high temperatures. It is presumed that boron is incorporated into one of the sites of the crystal structure of 3LiOH·Li2SO4, improving the stability of the crystal structure against temperature. The molar ratio (B / S) of boron B to sulfur S contained in the solid electrolyte is preferably more than 0.002 and less than 1.0, more preferably 0.003 to 0.9, and even more preferably 0.005 to 0.8. If the B / S is within the above range, it is possible to improve the retention rate of lithium ion conductivity. In addition, if the B / S is within the above range, the content of unreacted heterogeneous phases containing boron is low, and therefore the absolute value of lithium ion conductivity can be increased.

[0041] The LiOH·Li2SO4-based solid electrolyte may be a compact of powder obtained by pulverizing a molten solid, but a molten solid (i.e., solidified after heating and melting) is preferable. The method for pulverizing the molten solid is not particularly limited, but a method using a general mortar, ball mill, jet mill, roller mill, cutter mill, ring mill, etc. can be adopted, and either a wet method or a dry method can be used.

[0042] The LiOH·Li2SO4-based solid electrolyte is preferably filled into the pores of the positive electrode layer and / or the negative electrode layer, or incorporated into the positive electrode layer and / or the negative electrode layer (as one component of a composite material). From the viewpoints of charge / discharge rate characteristics and insulating properties of the solid electrolyte, the thickness of the solid electrolyte layer (excluding the portion that has entered the pores in the positive electrode layer and the negative electrode layer) is preferably 1 to 500 μm, more preferably 3 to 50 μm, and even more preferably 5 to 40 μm.

[0043] Manufacture of lithium-ion secondary batteries In the case of using a sintered plate electrode, the lithium ion secondary battery can be manufactured by i) preparing a positive electrode (with a current collector formed as necessary) and a negative electrode (with a current collector formed as necessary), and ii) sandwiching a solid electrolyte between the positive electrode and the negative electrode and applying pressure, heat, or the like to integrate the positive electrode, the solid electrolyte, and the negative electrode. The positive electrode, the solid electrolyte, and the negative electrode may be bonded by other methods. In this case, examples of the method for forming the solid electrolyte between the positive electrode and the negative electrode include a method of placing a molded body or powder of the solid electrolyte on one electrode, a method of applying a paste of the solid electrolyte powder on the electrode by screen printing, a method of impacting and solidifying the powder of the solid electrolyte by an aerosol deposition method or the like using the electrode as a substrate, and a method of depositing the solid electrolyte powder on the electrode by electrophoresis to form a film. On the other hand, when a composite electrode is used, the all-solid-state secondary battery can be manufactured by, for example, putting a positive electrode composite powder (including positive electrode active material particles, solid electrolyte particles, and an electronic conductive assistant), a solid electrolyte powder, and a negative electrode composite powder (including negative electrode active material particles, solid electrolyte particles, and an electronic conductive assistant) into a press mold and applying pressure. In this case, the powders may be put in and pressed in any order so that the final order is the positive electrode layer, the solid electrolyte layer, and the negative electrode layer. As described above, the positive electrode active material particles may be in the form of a mixed powder containing a lithium composite oxide powder and at least one powder selected from Li3BO3, Li3PO4, and Li2SO4. EXAMPLES

[0044] The present invention will be described in more detail with reference to the following examples. 0.5 Co 0.2 Mn 0.3 )O2, Li(Ni 0.3 Co 0.6 Mn 0.1 Lithium composite oxides with a layered rock salt structure containing Li, Ni, Co, and Mn, such as Li4Ti5O2, are abbreviated as "NCM" and Li4Ti5O 12 shall be abbreviated as "LTO."

[0045] <Examples 1 to 18> The example described below is an example relating to an all-solid-state secondary battery in which the positive electrode and the negative electrode are in the form of a sintered plate.

[0046] First, NCM raw material powders 1 to 22 for producing a positive electrode plate were prepared as shown below. The characteristics of these raw material powders are summarized in Tables 1A to 1C.

[0047] [Preparation of NCM raw powder 1] Commercially available (Ni 0.5 Co 0.2 Mn 0.3 After mixing Li2CO3 powder (average particle size 3 μm) with 1H2O3 powder (average particle size 9-10 μm), the mixture was kept at 750°C for 10 hours to obtain NCM raw material powder 1. The volumetric D50 particle size of this powder was 8 μm.

[0048] [Preparation of NCM raw powder 2] Li3BO3 was added to NCM raw material powder 1 at 2.45 wt% (based on the total amount of NCM raw material powder 1 and Li3BO3), and the volume-based D50 particle size was adjusted to approximately 0.4 μm by wet pulverization in a ball mill. NCM raw material powder 2 was then obtained by drying.

[0049] [Preparation of NCM raw material powder 3] Li3BO3 was added to NCM raw material powder 1 in an amount of 9.2 wt% (based on the total amount of NCM raw material powder 1 and Li3BO3), and the volume-based D50 particle size was adjusted to approximately 0.4 μm by wet pulverization in a ball mill. NCM raw material powder 3 was then obtained by drying.

[0050] [Preparation of NCM raw material powder 4] NCM raw material powder 1 was adjusted to a volumetric D50 particle size of about 5.5 μm by wet pulverization in a ball mill, and then dried to obtain NCM raw material powder 4.

[0051] [Preparation of NCM raw material powder 5] Li3PO4 was added to NCM raw material powder 1 at 1.0 wt% (based on the total amount of NCM raw material powder 1 and Li3PO4), and the volume-based D50 particle size was adjusted to approximately 5.5 μm by wet pulverization in a ball mill. NCM raw material powder 5 was then obtained by drying.

[0052] [Preparation of NCM raw material powder 6] Li3PO4 was added to NCM raw material powder 1 at 5.0 wt% (based on the total amount of NCM raw material powder 1 and Li3PO4), and the volume-based D50 particle size was adjusted to approximately 5.5 μm by wet pulverization in a ball mill. NCM raw material powder 6 was then obtained by drying.

[0053] [Preparation of NCM raw material powder 7] Commercially available (Ni 0.3 Co 0.6 Mn 0.1 After mixing Li2CO3 powder (average particle size 3 μm) with 1H2O3 powder (average particle size 3 μm), the mixture was kept at 850°C for 10 hours to obtain NCM raw material powder 7. The volumetric D50 particle size of this powder was 6.5 μm.

[0054] [Preparation of NCM raw material powder 8] Li3BO3 was added to NCM raw material powder 7 in an amount of 9.2 wt% (based on the total amount of NCM raw material powder 7 and Li3BO3), and the volume-based D50 particle size was adjusted to approximately 0.4 μm by wet pulverization in a ball mill. NCM raw material powder 8 was then obtained by drying.

[0055] [Preparation of NCM raw material powder 9] Li3BO3 was added to NCM raw material powder 7 in an amount of 16.8 wt% (based on the total amount of NCM raw material powder 7 and Li3BO3), and the volume-based D50 particle size was adjusted to approximately 0.4 μm by wet pulverization in a ball mill. NCM raw material powder 9 was then obtained by drying.

[0056] [Preparation of NCM raw material powder 10] Li3BO3 was added to NCM raw material powder 7 in an amount of 51 wt% (based on the total amount of NCM raw material powder 7 and Li3BO3), and the volume-based D50 particle size was adjusted to approximately 0.4 μm by wet pulverization in a ball mill. NCM raw material powder 10 was then obtained by drying.

[0057] [Preparation of NCM raw material powder 11] Li2SO4 was added to NCM raw material powder 7 in an amount of 16.8% by weight (based on the total amount of NCM raw material powder 7 and Li2SO4), and the volume-based D50 particle size was adjusted to approximately 0.4 μm by wet pulverization in a ball mill. NCM raw material powder 11 was then obtained by drying.

[0058] [Preparation of NCM raw material powder 12] Li2SO4 was added to NCM raw material powder 7 in an amount of 51% by weight (based on the total amount of NCM raw material powder 7 and Li2SO4), and the volume-based D50 particle size was adjusted to approximately 0.4 μm by wet pulverization in a ball mill. NCM raw material powder 12 was then obtained by drying.

[0059] [Preparation of NCM raw material powder 13] The NCM raw material powder 7 was subjected to wet pulverization in a ball mill to adjust the volumetric D50 particle size to about 0.4 μm, and then dried to obtain the NCM raw material powder 13.

[0060] [Preparation of NCM raw material powder 14] The NCM raw material powder 7 was subjected to wet pulverization in a ball mill to adjust the volumetric D50 particle size to about 4.3 μm, and then dried to obtain the NCM raw material powder 14.

[0061] [Preparation of NCM raw material powder 15] Commercially available (Ni 0.3 Co 0.6 Mn 0.1 After mixing (OH)2 powder (average particle size 7-8 μm) and Li2CO3 powder (average particle size 3 μm), the mixture was kept at 950°C for 10 hours. The resulting powder was wet-pulverized in a ball mill to adjust the volumetric D50 particle size to approximately 1.9 μm, and then dried to obtain NCM raw material powder 15.

[0062] [Preparation of NCM raw powder 16] Commercially available (Ni 0.3 Co 0.6 Mn 0.1 0.74 wt% of Li3PO4 powder (average particle size 0.5 μm) (based on the total amount of NCM hydroxide, Li2CO3, and Li3PO4) was added to )(OH)2 powder (average particle size 9-10 μm) and Li2CO3 powder (average particle size 3 μm), mixed, and then held at 870°C for 10 hours to obtain NCM raw material powder 16. The volumetric D50 particle size of this powder was 7.4 μm.

[0063] [Preparation of NCM raw material powder 17] Commercially available (Ni 0.3 Co 0.6 Mn 0.1 1.8 wt% of Li3PO4 powder (average particle size 0.5 μm) (based on the total amount of NCM hydroxide, Li2CO3, and Li3PO4) was added to )(OH)2 powder (average particle size 9-10 μm) and Li2CO3 powder (average particle size 3 μm) and mixed, and then the mixture was kept at 870°C for 10 hours to obtain NCM raw material powder 17. The volumetric D50 particle size of this powder was 7.5 μm.

[0064] [Preparation of NCM raw material powder 18] Commercially available (Ni 0.3 Co 0.6 Mn 0.1 3.6 wt% of Li3PO4 powder (average particle size 0.5 μm) (based on the total amount of NCM hydroxide, Li2CO3, and Li3PO4) was added to )(OH)2 powder (average particle size 9-10 μm) and Li2CO3 powder (average particle size 3 μm) and mixed, and then the mixture was kept at 870°C for 10 hours to obtain NCM raw material powder 18. The volumetric D50 particle size of this powder was 7.7 μm.

[0065] [Preparation of NCM raw material powder 19] Commercially available (Ni 0.3 Co 0.6Mn 0.1 )(OH)2 powder (average particle size 9-10 μm) and Li2CO3 powder (average particle size 3 μm) were mixed and then held at 750°C for 10 hours to obtain NCM raw material powder 19. The volumetric D50 particle size of this powder was 7.0 μm.

[0066] [Preparation of NCM raw material powder 20] To NCM raw material powder 19, 9.2 wt% Li3BO3 (based on the total amount of NCM raw material powder 19 and Li3BO3) and 1.0 wt% Li3PO4 (based on the total amount of NCM raw material powder 19 and Li3PO4) were added, and the volume-based D50 particle size was adjusted to approximately 0.5 μm by wet grinding in a ball mill, and then dried to obtain NCM raw material powder 20.

[0067] [Preparation of NCM raw material powder 21] To NCM raw material powder 19, 9.2 wt% Li3BO3 (based on the total amount of NCM raw material powder 19 and Li3BO3) and 2.5 wt% Li3PO4 (based on the total amount of NCM raw material powder 19 and Li3PO4) were added, and the volume-based D50 particle size was adjusted to approximately 0.5 μm by wet grinding in a ball mill, and then dried to obtain NCM raw material powder 21.

[0068] [Preparation of NCM raw material powder 22] To NCM raw material powder 19, 9.2 wt% Li3BO3 (based on the total amount of NCM raw material powder 19 and Li3BO3) and 5.0 wt% Li3PO4 (based on the total amount of NCM raw material powder 19 and Li3PO4) were added, and the volume-based D50 particle size was adjusted to approximately 0.5 μm by wet grinding in a ball mill, and then dried to obtain NCM raw material powder 22.

[0069] Positive electrode plates and batteries were produced using the above raw material powders 1 to 22 as described below, and various evaluations were carried out.

[0070] Example 1 (1) Preparation of the positive electrode plate (1a) Preparation of NCM green sheet First, NCM raw material powders 1 and 2 were uniformly mixed at a mixing ratio (weight ratio) of 80:20 as shown in Tables 1A to 1C to prepare NCM mixed powder A. This mixed powder A was mixed with a solvent, binder, plasticizer, and dispersant for tape casting. After adjusting the viscosity of the obtained paste, it was molded into a sheet on a PET (polyethylene terephthalate) film to produce an NCM green sheet. The thickness of the NCM green sheet was adjusted so that the thickness after firing would be 100 μm.

[0071] (1b) Preparation of NCM sintered plate The NCM green sheet peeled off from the PET film was punched out into a circle with a diameter of 11 mm and placed in a sintering sheath. The temperature was raised to 940°C at a rate of 200°C / h and held for 10 hours for sintering. The thickness of the resulting sintered plate was approximately 100 μm as determined by SEM observation. A Au film (thickness 100 nm) was formed as a current collecting layer on one side of the NCM sintered plate by sputtering. In this way, a positive electrode plate was obtained.

[0072] (2) Preparation of negative electrode plate (2a) Preparation of LTO green sheet Commercially available TiO2 powder (average particle size 1μm or less) and Li2CO3 powder (average particle size 3μm) were mixed so that the molar ratio of Li / Ti was 0.84, and then held at 1000℃ for 2 hours to obtain a powder consisting of LTO particles. This powder was adjusted to an average particle size of about 2μm by wet grinding in a ball mill, and then mixed with a solvent, binder, plasticizer, and dispersant for tape casting. After adjusting the viscosity of the obtained paste, this paste was molded into a sheet on a PET film to produce an LTO green sheet. The thickness of the LTO green sheet was adjusted so that the thickness after firing would be 130μm.

[0073] (2b) Preparation of LTO sintered plate The LTO green sheet peeled off from the PET film was punched out into a circle with a diameter of 11 mm and placed in a sintering sheath. The temperature was raised to 850°C at a rate of 200°C / h and held for 2 hours for sintering. The thickness of the resulting sintered plate was approximately 130 μm according to SEM observation. A Au film (thickness 100 nm) was formed as a current collecting layer on one side of this LTO sintered plate by sputtering. In this way, a negative electrode plate was obtained.

[0074] (3) Preparation of solid electrolyte (3a) Preparation of raw material powder mixture Li2SO4 powder (commercial product, purity 99% or more), LiOH powder (commercial product, purity 98% or more), and Li3BO3 (commercial product, purity 99% or more) were mixed in a molar ratio of Li2SO4:LiOH:Li3BO3 = 1:2.6:0.05 to obtain a raw material mixed powder. These powders were handled in a glove box in an Ar atmosphere, and care was taken to prevent deterioration such as moisture absorption.

[0075] (3b) Melt synthesis The raw material powder mixture was placed in a high-purity alumina crucible in an Ar atmosphere. The crucible was then placed in an electric furnace and heat-treated at 430°C for 2 hours in an Ar atmosphere to produce a melt. The melt was then cooled in the electric furnace at 100°C / h to form a solid.

[0076] (3c) Mortar grinding The obtained solidified product was pulverized in a mortar in a glove box in an Ar atmosphere to obtain a solid electrolyte powder having a volume-based D50 particle size of 5 to 50 μm.

[0077] (4) Fabrication of all-solid-state batteries The solid electrolyte powder was placed on the positive plate, and the negative plate was placed on top of that. A weight was then placed on the negative plate, and the plate was heated at 400°C for 45 minutes in an electric furnace. During this process, the solid electrolyte powder melted, and after subsequent solidification, a solid electrolyte layer was formed between the electrode plates. A battery was fabricated using the resulting cell consisting of a positive plate / solid electrolyte / negative plate.

[0078] (5) Evaluation (5a) Degree of orientation XRD (X-ray diffraction) measurement was performed on the positive electrode plate prepared in (1) above. This measurement was performed using an XRD device (BRUKER, D8 ADVANCE) by measuring the XRD profile when X-rays were irradiated onto the plate surface of the positive electrode plate. From this XRD profile, the diffraction intensity (peak height) I due to the (104) plane of NCM was

[0104] Diffraction intensity (peak height) due to the (003) plane for I

[0003] is the ratio of I

[0003] / I

[0104] was calculated and this was taken as the degree of orientation.

[0079] (5b) Thickness and porosity measurements The thickness and porosity (volume%) of the positive electrode plate (NCM sintered plate not containing a solid electrolyte) prepared in (1) above and the negative electrode plate (LTO sintered plate not containing a solid electrolyte) prepared in (2) above were measured as follows. First, the positive electrode plate (or negative electrode plate) was filled with resin, and then the cross section was polished by ion milling, and the polished cross section was observed with an SEM to obtain a cross-sectional SEM image. The thickness was calculated from this SEM image. The SEM images for porosity measurement were images with magnifications of 1000 times and 500 times. The obtained images were binarized using image analysis software (Image-Pro Premier, manufactured by Media Cybernetics), and the ratio (%) of the area of ​​the resin-filled part to the total area of ​​the positive electrode active material (or negative electrode active material) part and the resin-filled part (originally a pore part) in the positive electrode plate (or negative electrode plate) was calculated to obtain the porosity (%) of the positive electrode plate (or negative electrode plate). The threshold for binarization was set using Otsu's binarization as a discriminant analysis method. The porosity of the positive electrode plate is as shown in Table 2, and the porosity of the negative electrode plate was 38% (i.e., density 62%).

[0080] (5c) Measurement of average pore size The average pore size was measured using the SEM image used in the above porosity measurement as follows. Using image analysis software (Media Cybernetics, Image-Pro Premier), binarization was performed to separate the positive electrode plate (or negative electrode plate) into the positive electrode active material (or negative electrode active material) and the resin-filled portion (the portion that was originally pores). Then, in the region of the resin-filled portion, the maximum Martin diameter of each region was obtained, and the average value thereof was taken as the average pore size (μm) of the positive electrode plate (or negative electrode plate). The average pore size of the positive electrode plate was as shown in Table 2, and the average pore size of the negative electrode plate was 2.1 μm.

[0081] (5d) Unit cross-sectional area 1 μm 2 Measurement of the interfacial length at contact Using the SEM image used for the above porosity measurement, the unit cross-sectional area of ​​1 μm 2 The interface length per unit area was measured. Using image analysis software (Image-Pro Premier, manufactured by Media Cybernetics), binarization was performed to separate the positive electrode plate into the positive electrode active material portion and the resin-filled portion (the portion that was originally an air hole). After that, in the region of the portion filled with resin, the perimeter of the entire region (i.e., the total length of the interface between the positive electrode active material portion and the resin-filled portion) and the area of ​​the entire analyzed region (i.e., the region consisting of both the positive electrode active material portion and the resin-filled portion) were calculated. The perimeter was divided by the area of ​​the entire analyzed region to obtain a unit cross-sectional area of ​​1 μm 2 The results are shown in Table 2.

[0082] (5e) Measurement of the molar ratio of metal elements in the positive electrode plate The molar ratio Li / (Ni+Co+Mn) of the Li content to the total content of Ni, Co, and Mn in the positive electrode plate prepared in (1) above was calculated from the measurement results of metal element analysis by inductively coupled plasma atomic emission spectroscopy (ICP-AES method). The results are shown in Table 2.

[0083] (5f) Identification of solid electrolyte by XRD The LiOH·Li2SO4-based solid electrolyte obtained in (3c) above was analyzed by X-ray diffraction (XRD) and identified as 3LiOH·Li2SO4.

[0084] (5g) Charge / discharge evaluation (cycle maintenance rate) The discharge capacity of the battery prepared in (4) above was measured in the voltage range of 2.5V-1.5V at an operating temperature of 150°C. This measurement was performed by charging the battery at a constant current and constant voltage until the battery voltage reached the upper limit of the voltage range, and then discharging the battery until it reached the lower limit of the voltage range. This test was repeated (cycle test), and the retention rate of the discharge capacity at a specified cycle was calculated (=100×(discharge capacity at a specified cycle) / (initial discharge capacity)). The results are shown in Table 2.

[0085] Example 2 A positive electrode plate and a battery were produced in the same manner as in Example 1, except that in the preparation of the positive electrode plate in (1) above, 1) mixed powder A was replaced with NCM mixed powder B containing NCM raw material powders 1 and 3 shown in Tables 1A to 1C in a mixing ratio (weight ratio) of 90:10, and 2) the firing temperature was 950°C. Then, various evaluations were performed on the positive electrode plate and the battery.

[0086] Example 3 A positive plate and a battery were prepared in the same manner as in Example 1, except that in the preparation of the positive plate in (1) above, 1) only NCM raw material powder 5 shown in Tables 1A to 1C was used instead of mixed powder A, and 2) the firing temperature was set to 920°C. Various evaluations were performed. The battery prepared in this example was disassembled in a glove box, and the interface between the positive plate and the solid electrolyte was observed under an electron microscope and elemental mapping was performed using an electron probe microanalyzer (EPMA). Figure 1 shows an electron microscope photograph and an EPMA mapping image of the cross section of the positive active material (NCM) / solid electrolyte of the all-solid-state battery prepared in this example. The image located at the far left in Figure 1 is an electron microscope photograph (the white part corresponds to the NCM, and the black part corresponds to the solid electrolyte), and EPMA mapping images of Mn, Co, and Ni are shown in order from there to the right.

[0087] Example 4 A positive electrode plate and a battery were produced in the same manner as in Example 1, except that in the preparation of the positive electrode plate in (1) above, 1) only NCM raw material powder 6 shown in Tables 1A to 1C was used instead of mixed powder A, and 2) the firing temperature was set to 920°C, and various evaluations were performed.

[0088] Example 5 A positive electrode plate and a battery were produced in the same manner as in Example 1, except that in the preparation of the positive electrode plate in (1) above, 1) mixed powder A was replaced with NCM mixed powder C containing NCM raw material powders 7 and 8 shown in Tables 1A to 1C in a mixing ratio (weight ratio) of 90:10, and 2) the firing temperature was set to 920°C. Then, various evaluations were performed on the positive electrode plate and the battery.

[0089] Example 6 A positive electrode plate and a battery were produced in the same manner as in Example 1, except that in the preparation of the positive electrode plate in (1) above, 1) mixed powder A was replaced with NCM mixed powder D containing NCM raw material powders 7 and 8 shown in Tables 1A to 1C in a blend ratio (weight ratio) of 95:5, and 2) the firing temperature was 950°C. Then, various evaluations were performed on the positive electrode plate and the battery.

[0090] Example 7 A positive electrode plate and a battery were produced in the same manner as in Example 1, except that in the preparation of the positive electrode plate in (1) above, 1) mixed powder A was replaced with NCM mixed powder E containing NCM raw material powders 7 and 9 shown in Tables 1A to 1C in a mixing ratio (weight ratio) of 95:5, and 2) the firing temperature was set to 920°C. Then, various evaluations were performed on the positive electrode plate and the battery.

[0091] Example 8 A positive electrode plate and a battery were produced and evaluated in the same manner as in Example 1, except that in the preparation of the positive electrode plate in (1) above, 1) NCM mixed powder F containing NCM raw material powders 7 and 10 shown in Tables 1A to 1C in a blending ratio (weight ratio) of 95:5 was used instead of mixed powder A, and 2) the firing temperature was set to 920° C. In addition, an electron microscope photograph (backscattered electron image) of the cross section of the positive electrode plate prepared in this example is shown in FIG.

[0092] Example 9 A positive electrode plate and a battery were produced in the same manner as in Example 1, except that in the preparation of the positive electrode plate in (1) above, 1) mixed powder A was replaced with NCM mixed powder G containing NCM raw material powders 7 and 11 shown in Tables 1A to 1C in a blend ratio (weight ratio) of 95:5, and 2) the firing temperature was set to 920°C. Then, various evaluations were performed on the positive electrode plate and the battery.

[0093] Example 10 A positive electrode plate and a battery were produced in the same manner as in Example 1, except that in the preparation of the positive electrode plate in (1) above, 1) mixed powder A was replaced with NCM mixed powder H containing NCM raw material powders 7 and 12 shown in Tables 1A to 1C in a mixing ratio (weight ratio) of 95:5, and 2) the firing temperature was set to 920°C. Then, various evaluations were performed on the positive electrode plate and the battery.

[0094] Example 11 A positive electrode plate and a battery were produced in the same manner as in Example 1, except that in the preparation of the positive electrode plate in (1) above, 1) mixed powder A was replaced with NCM mixed powder I containing NCM raw material powders 16 and 20 shown in Tables 1A to 1C in a blend ratio (weight ratio) of 90:10, and 2) the firing temperature was set to 920°C. Then, various evaluations were performed on the positive electrode plate and the battery.

[0095] Example 12 A positive plate and a battery were produced and evaluated in the same manner as in Example 1, except that in the preparation of the positive plate in (1) above, 1) mixed powder A was replaced with NCM mixed powder J containing NCM raw material powders 17 and 21 shown in Tables 1A to 1C in a blending ratio (weight ratio) of 90:10, and 2) the firing temperature was set to 920° C. In addition, Fig. 4 shows an electron microscope photograph (backscattered electron image) of the cross section of the positive plate produced in this example after being filled with resin.

[0096] Example 13 A positive electrode plate and a battery were produced in the same manner as in Example 1, except that in the preparation of the positive electrode plate in (1) above, 1) mixed powder A was replaced with NCM mixed powder K containing NCM raw material powders 18 and 22 shown in Tables 1A to 1C in a mixing ratio (weight ratio) of 90:10, and 2) the firing temperature was set to 920°C. Then, various evaluations were performed on the positive electrode plate and the battery.

[0097] Example 14 (comparison) A positive plate and a battery were prepared in the same manner as in Example 1, except that in the preparation of the positive plate in (1) above, 1) only NCM raw material powder 4 shown in Tables 1A to 1C was used instead of mixed powder A, and 2) the sintering temperature was set to 920°C. Various evaluations were performed. The battery prepared in this example was disassembled in a glove box, and the interface between the positive plate and the solid electrolyte was observed under an electron microscope and elemental mapping was performed using an electron probe microanalyzer (EPMA). Figure 2 shows an electron microscope photograph and an EPMA mapping image of the cross section of the positive active material (NCM) / solid electrolyte of the all-solid-state battery prepared in this example. The image located at the leftmost position in Figure 2 is an electron microscope photograph (the white part corresponds to the NCM, and the black part corresponds to the solid electrolyte), and EPMA mapping images of Mn, Co, and Ni are shown in order from there to the right.

[0098] Example 15 (comparison) A positive electrode plate and a battery were produced in the same manner as in Example 1, except that in the preparation of the positive electrode plate in (1) above, 1) only NCM raw material powder 14 shown in Tables 1A to 1C was used instead of mixed powder A, and 2) the firing temperature was set to 920°C, and various evaluations were performed.

[0099] Example 16 (comparison) A positive electrode plate and a battery were produced in the same manner as in Example 1, except that in the preparation of the positive electrode plate in (1) above, 1) only NCM raw material powder 15 shown in Tables 1A to 1C was used instead of mixed powder A, and 2) the firing temperature was set to 890°C, and various evaluations were performed.

[0100] Example 17 (comparison) A positive electrode plate and a battery were produced in the same manner as in Example 1, except that in the preparation of the positive electrode plate in (1) above, 1) mixed powder A was replaced with NCM mixed powder L containing NCM raw material powders 7 and 13 shown in Tables 1A to 1C in a mixing ratio (weight ratio) of 90:10, and 2) the firing temperature was 950°C. Then, various evaluations were performed.

[0101] Example 18 (comparison) In the preparation of the positive electrode plate in (1) above, 1) mixed powder A was replaced with NCM mixed powder M containing NCM raw material powders 7 and 13 shown in Tables 1A to 1C in a mixing ratio (weight ratio) of 95:5, and 2) the firing temperature was set to 950°C. In the same manner as in Example 1, except for this, a positive electrode plate and a battery were prepared and various evaluations were performed.

[0102] result The specifications of the positive electrode plates and the evaluation results of the cells produced in each example are shown in Table 2. The charge / discharge characteristics were compared at the same rate and the same number of cycles, and the retention rate of discharge capacity at a specified cycle (= 100 x (discharge capacity at a specified cycle) / (initial discharge capacity)) was calculated and shown in Table 2. The LiOH·Li2SO4-based solid electrolyte in each example was analyzed by X-ray diffraction (XRD) and identified as 3LiOH·Li2SO4.

[0103] [Table 1A]

[0104] [Table 1B]

[0105] [Table 1C]

[0106] [Table 2]

[0107] From SEM observation and elemental mapping by EPMA (Figures 1 and 2), it was confirmed that the diffusion of transition metals into the solid electrolyte portion in the voids of the positive plate is suppressed in the NCM with the additive (Li3PO4) added (Example 3; see Figure 1) compared to the pure NCM without additives such as Li3PO4 (Example 14 (comparison); see Figure 2). From this, it is considered that the decrease in Li ion conductivity due to the deterioration of the solid electrolyte is mitigated in the positive plate using the NCM with Li3PO4 added (Examples 3, 4, and 11 to 13), which resulted in an improvement in the cycle retention rate. In addition, since the cycle retention rate is improved in the NCM with Li3BO3 or Li2SO4 added (Examples 1, 2, and 5 to 10) compared to the pure NCM, the addition of Li3BO3 or Li2SO4 is considered to have the same effect as the addition of Li3PO4.

[0108] From Fig. 3 showing the SEM image (backscattered electron image) of the cross section of the positive electrode plate obtained in Example 8, it was confirmed that elements other than Ni, Co, and Mn were present in the NCM bulk. That is, this element is considered to be B (boron), which is an element lighter than Ni, Co, and Mn, because it has a darker color than the NCM part in Fig. 3. And, this B is considered to be present in the grain boundaries.

[0109] From Figure 4, which shows an SEM image (backscattered electron image) of the cross section of the resin-filled positive plate obtained in Example 12, it was confirmed that other elements were present, covering the pores of the sintered plate. Three colored areas can be confirmed in this SEM image, with the lightest colored area being the NCM and the darkest colored area being the resin (C: carbon), and the intermediate colored areas are thought to be areas containing other elements present on the surface of the NCM. As this intermediate colored area is darker than the NCM and lighter than the resin, it is thought to contain B (boron) and P (phosphorus) contained in the additive. It is believed that this B and P are precipitated on the surface of the NCM.

[0110] The batteries of Examples 1 to 13 using the positive electrode active material satisfying the requirements of the present invention showed significantly higher cycle retention rates than the batteries of Examples 14 to 18 (Comparative Examples) not satisfying the requirements of the present invention. This is believed to be due to the fact that Li3BO3, Li3PO4 and / or Li2SO4 precipitated on a part of the surface of the lithium composite oxide suppressed the side reaction between the lithium composite oxide and the solid electrolyte, and Li3BO3, Li3PO4 and / or Li2SO4 precipitated on a part of the grain boundaries alleviated the stress of expansion and contraction of the positive electrode active material. This is believed to have led to the improvement of the cycle retention rate by alleviating phenomena such as the decrease in Li ion conductivity due to deterioration of the solid electrolyte, the formation of a high resistance layer that inhibits Li ion conduction at the interface between the positive electrode layer and the solid electrolyte, and the increase in diffusion resistance between the positive electrode active materials.

[0111] <Examples 19-33> The example described below is an example relating to an all-solid-state secondary battery in which the positive electrode and the negative electrode are in the form of a composite material.

[0112] Example 19 (1) Preparation of positive electrode active material powder Commercially available (Ni 0.3 Co 0.6 Mn 0.1 )(OH)2 powder (average particle size 9-10 μm) and Li2CO3 powder (average particle size 3 μm) were mixed and then held at 950° C. for 10 hours to obtain NCM raw material powder 23. 1.0 wt % of Li3BO3 (based on the total amount of NCM raw material powder 23 and Li3BO3) and 1.0 wt % of Li3PO4 (based on the total amount of NCM raw material powder 23 and Li3PO4) were added to the obtained NCM raw material powder 23 and mixed, and then held at 950° C. for 10 hours to obtain NCM powder.

[0113] (2) Preparation of negative electrode active material powder Commercially available carbon powder (average particle size: 10 to 14 μm) was prepared.

[0114] (3) Preparation of solid electrolyte (3a) Preparation of raw powder Li2SO4 powder (commercial product, purity 99% or more), LiOH powder (commercial product, purity 98% or more), and Li3BO3 (commercial product, purity 99% or more) were mixed in a molar ratio of Li2SO4:LiOH:Li3BO3 = 1:2.2:0.05 to obtain a raw material mixed powder. These powders were handled in a glove box in an Ar atmosphere, and care was taken to prevent deterioration such as moisture absorption.

[0115] (3b) Melt synthesis The raw material powder mixture was placed in a high-purity alumina crucible in an Ar atmosphere. The crucible was then placed in an electric furnace and heat-treated at 430°C for 2 hours in an Ar atmosphere to produce a melt. The melt was then cooled in the electric furnace at 100°C / h to form a solid.

[0116] (3c) Crushing The obtained solidified product was pulverized in a mortar in a glove box in an Ar atmosphere, and further pulverized using balls to obtain a solid electrolyte powder having an average particle size D50 of 1 to 20 μm.

[0117] (4) Fabrication of all-solid-state batteries (4a) Preparation of Positive Electrode Mixture Powder and Negative Electrode Mixture Powder The positive electrode active material powder obtained in (1) above, the solid electrolyte powder obtained in (3) above, and an electron conductive assistant (acetylene black (commercially available)) were weighed out to a volume ratio of 60:40:2, and mixed in a mortar to prepare a positive electrode composite powder. Similarly, the negative electrode active material powder obtained in (2) above, the solid electrolyte powder obtained in (3) above, and an electron conductive assistant (acetylene black (commercially available)) were weighed out to a volume ratio of 60:40:2, and mixed in a mortar to prepare a negative electrode composite powder.

[0118] (4b) Press molding Powders were poured into a press mold with a hole diameter of 10 mm, and a pressure of 100 MPa was applied to each layer so that the thicknesses of the positive electrode layer, the solid electrolyte layer, and the negative electrode layer were 100 μm, 500 μm, and 110 μm, respectively. After stacking the three layers in this way, the laminate was pressed at 150 MPa to obtain a press molded body.

[0119] (4c) Attaching the pressure tool The press-molded body was sandwiched between a pair of stainless steel plates to form a layer structure of stainless steel plate / positive electrode layer / solid electrolyte layer / negative electrode layer / stainless steel plate, and the press-molded body together with the stainless steel plates was held at 150 MPa to obtain an all-solid-state battery as an evaluation cell.

[0120] (5) Evaluation (5a) Measurement of the molar ratio of metal elements in the positive electrode layer The molar ratio Li / (Ni+Co+Mn) of the Li content to the total content of Ni, Co, and Mn in the positive electrode layer prepared in (1) above was calculated from the measurement results of metal element analysis by inductively coupled plasma atomic emission spectroscopy (ICP-AES method). The results are shown in Table 3.

[0121] (5b) Identification of solid electrolyte by XRD The LiOH·Li2SO4-based solid electrolyte obtained in (3c) above was analyzed by X-ray diffraction (XRD) and identified as 3LiOH·Li2SO4.

[0122] (5c) Charge / discharge evaluation (cycle retention rate) The discharge capacity of the battery prepared in (4) above at an operating temperature of 150°C was measured in the voltage range of 4.15 V to 2.0 V. This measurement was performed by charging the battery at a constant current and constant voltage until the battery voltage reached the upper limit of the voltage range, and then discharging the battery until it reached the lower limit of the voltage range. This test was repeated (cycle test), and the retention rate of the discharge capacity at a specified cycle was calculated (= 100 × (discharge capacity at a specified cycle) / (initial discharge capacity)). The results are shown in Table 3.

[0123] (5d) Measurement of filling rate The filling rate (volume %) of the active material in each of the positive electrode and the negative electrode of the all-solid-state battery prepared in (4) above was measured as follows. First, the cross section of the all-solid-state battery was polished by ion milling, and then the cross section of the polished positive electrode (or negative electrode) was observed by SEM to obtain a cross-sectional SEM image. The SEM image was an image with a magnification of 1000 times. The obtained image was subjected to binarization processing using image analysis software (Image-Pro Premier, manufactured by Media Cybernetics). The threshold value for binarization was set using Otsu's binarization as a discriminant analysis method. Based on the obtained binarized image, the filling rate F (%) of the positive electrode active material (or negative electrode active material) in the positive electrode (or negative electrode) was calculated using the following formula: Filling rate F=[S A / (S A +S B )] x 100 (In the formula, S A is the area of ​​the positive electrode active material (or negative electrode active material) in the binarized image, and S B is the area of ​​the part other than the positive electrode active material (or negative electrode active material) in the binarized image, and includes the area occupied by the solid electrolyte, the electronic conductive assistant, and the voids. The results are shown in Table 3.

[0124] Example 20 A battery was prepared and evaluated in the same manner as in Example 19, except that a negative electrode active material powder was prepared as follows, and that in the charge / discharge evaluation in (5c) above, the discharge capacity of the battery at an operating temperature of 150°C was measured in a voltage range of 2.7 V to 1.5 V.

[0125] (Preparation of negative electrode active material powder) Commercially available TiO2 powder (average particle size less than 1 μm) and Li2CO3 powder (average particle size 3 μm) were mixed so that the molar ratio of Li / Ti was 0.84, and then held at 1000°C for 2 hours to obtain a powder composed of LTO particles with an average particle size of approximately 3.5 μm.

[0126] Example 21 In the preparation of the positive electrode active material powder in (1) above, 1.0 wt% Li3BO3 (based on the total amount of NCM raw material powder 23 and Li3BO3) and 2.5 wt% Li3PO4 (based on the total amount of NCM raw material powder 23 and Li3PO4) were added to and mixed with NCM raw material powder 23, and then the mixture was held at 950°C for 10 hours to obtain NCM powder. A battery was prepared and evaluated in the same manner as in Example 19, except that the NCM powder was obtained by mixing the mixture at 950°C for 10 hours.

[0127] Example 22 In the preparation of the positive electrode active material powder in (1) above, 1.0 wt% Li3BO3 (based on the total amount of NCM raw material powder 23 and Li3BO3) and 5.0 wt% Li3PO4 (based on the total amount of NCM raw material powder 23 and Li3PO4) were added to and mixed with NCM raw material powder 23, and then the mixture was held at 950°C for 10 hours to obtain NCM powder. A battery was prepared and evaluated in the same manner as in Example 19, except that the NCM powder was obtained by mixing the mixture at 950°C for 10 hours.

[0128] Example 23 A battery was prepared and evaluated in the same manner as in Example 19, except that in the preparation of the positive electrode active material powder in (1) above, 1.0 wt.% Li3PO4 (relative to the total amount of NCM raw material powder 23 and Li3PO4) was added to and mixed with the NCM raw material powder 23, and then the mixture was held at 950°C for 10 hours to obtain an NCM powder.

[0129] Example 24 In the preparation of the positive electrode active material powder in (1) above, 5.0 wt.% of Li3PO4 (relative to the total amount of NCM raw material powder 23 and Li3PO4) was added to and mixed with NCM raw material powder 23, and then the mixture was held at 950°C for 10 hours to obtain NCM powder. A battery was prepared and evaluated in the same manner as in Example 19, except that the NCM powder was obtained by mixing the NCM raw material powder 23 and Li3PO4 at 5.0 wt.% (relative to the total amount of NCM raw material powder 23 and Li3PO4).

[0130] Example 25 A battery was produced and evaluated in the same manner as in Example 19, except that in the preparation of the positive electrode active material powder in (1) above, 1.0 wt.% Li2SO4 (relative to the total amount of NCM raw material powder 23 and Li2SO4) was added to and mixed with NCM raw material powder 23, and then the mixture was held at 950°C for 10 hours to obtain NCM powder.

[0131] Example 26 A battery was produced and evaluated in the same manner as in Example 19, except that in the preparation of the positive electrode active material powder in (1) above, 5.0 wt.% Li2SO4 (relative to the total amount of NCM raw material powder 23 and Li2SO4) was added to and mixed with NCM raw material powder 23, and then the mixture was held at 950°C for 10 hours to obtain NCM powder.

[0132] Example 27 A battery was prepared and evaluated in the same manner as in Example 19, except that in the preparation of the positive electrode active material powder in (1) above, 1.0 wt.% Li3BO3 (relative to the total amount of NCM raw material powder 23 and Li3BO3) was added to and mixed with NCM raw material powder 23, and then the mixture was held at 950°C for 10 hours to obtain NCM powder.

[0133] Example 28 A battery was prepared and evaluated in the same manner as in Example 19, except that in the preparation of the positive electrode active material powder in (1) above, 5.0 wt.% Li3BO3 (relative to the total amount of NCM raw material powder 23 and Li3BO3) was added to and mixed with NCM raw material powder 23, and then the mixture was held at 950°C for 10 hours to obtain NCM powder.

[0134] Example 29 A battery was produced and evaluated in the same manner as in Example 19, except that a positive electrode active material powder was produced as follows.

[0135] (1') Preparation of positive electrode active material powder Commercially available (Ni 0.5 Co 0.2 Mn 0.3)(OH)2 powder (average particle size 9 μm) and Li2CO3 powder (average particle size 3 μm) were mixed and then held at 920° C. for 10 hours to obtain NCM raw material powder 24. 1.0 wt % Li3BO3 (based on the total amount of NCM raw material powder 24 and Li3BO3) and 1.0 wt % Li3PO4 (based on the total amount of NCM raw material powder 24 and Li3PO4) were added to the obtained NCM raw material powder 24 and mixed, and then held at 920° C. for 10 hours to obtain NCM powder.

[0136] Example 30 A battery was prepared and evaluated in the same manner as in Example 29, except that in the preparation of the positive electrode active material powder (1') above, 1.0 wt% Li3PO4 (relative to the total amount of NCM raw material powder 24 and Li3PO4) was added to and mixed with NCM raw material powder 24, and then the mixture was held at 920°C for 10 hours to obtain NCM powder.

[0137] Example 31 (comparison) A battery was prepared and evaluated in the same manner as in Example 19, except that in the preparation of the positive electrode active material powder in (1) above, the addition of Li3BO3 and Li3PO4 and the subsequent heat treatment were not performed (i.e., the NCM raw material powder 23 was used as it is as the positive electrode active material powder).

[0138] Example 32 (comparison) A battery was prepared and evaluated in the same manner as in Example 20, except that in the preparation of the positive electrode active material powder in (1) above, the addition of Li3BO3 and Li3PO4 and the subsequent heat treatment were not performed (i.e., NCM raw material powder 23 was used as it is as the positive electrode active material powder).

[0139] Example 33 (comparison) A battery was prepared and evaluated in the same manner as in Example 29, except that in the preparation of the positive electrode active material powder (1') above, the addition of Li3BO3 and Li3PO4 and the subsequent heat treatment were not performed (i.e., NCM raw material powder 24 was used as it is as the positive electrode active material powder).

[0140] result The specifications of the composite cells prepared in each example and the evaluation results of the cells are shown in Table 3. The charge / discharge characteristics were compared at the same rate and the same number of cycles, and the retention rate of discharge capacity at a specified cycle (= 100 x (discharge capacity at a specified cycle) / (initial discharge capacity)) was calculated and shown in Table 3. The LiOH·Li2SO4-based solid electrolyte in each example was analyzed by X-ray diffraction (XRD) and identified as 3LiOH·Li2SO4.

[0141] [Table 3]

[0142] In the all-solid-state secondary batteries in which the positive and negative electrodes are in the form of a composite material, the batteries of Examples 19 to 30 using the positive electrode active material satisfying the requirements of the present invention showed significantly higher cycle retention rates than the batteries of Examples 31 to 33 (comparative examples) not satisfying the requirements of the present invention. The fact that Li3BO3, Li3PO4 and / or Li2SO4 precipitated on a part of the surface of the lithium composite oxide suppressed side reactions between the lithium composite oxide and the solid electrolyte, and that Li3BO3, Li3PO4 and / or Li2SO4 precipitated on a part of the grain boundaries relaxed the stress of expansion and contraction of the positive electrode active material, which were confirmed in the all-solid-state secondary batteries in which the positive and negative electrodes are in the form of sintered plates, also occurred in the batteries in the form of a composite material, which is considered to have led to the improvement in cycle retention rate.

Claims

1. A positive electrode active material for use in a lithium ion secondary battery, The positive electrode active material includes a lithium composite oxide having a layered rock salt structure containing Li, Ni, Co, and Mn, and Li 3 B.O. 3 , Li 3 P.O. 4 and Li 2 SO 4 and further comprising at least one additive selected from the content of the additive is 0.1 to 10% by weight based on the total content of the lithium composite oxide and the additive, The additive is present in a state of being precipitated on at least a part of the grain boundaries and surfaces of the lithium composite oxide.

2. 10. The cathode active material of claim 1, wherein the cathode active material is in the form of a sintered plate.

3. The sintered plate has a diffraction intensity I due to the (104) plane in an XRD profile measured by X-ray diffraction (XRD). [104] Diffraction intensity I due to the (003) plane [003] The degree of orientation I is defined as the ratio of [003] / I [104] The positive electrode active material according to claim 2, wherein the positive electrode active material is 1.2 to 3.

6.

4. The unit cross-sectional area of ​​the sintered plate is 1 μm 2 The positive electrode active material according to claim 2 or 3, wherein the interface length per unit area is 0.45 μm or less.

5. The positive electrode active material according to any one of claims 2 to 4, wherein the porosity of the sintered plate is 20 to 40%.

6. The positive electrode active material according to any one of claims 2 to 5, wherein the sintered plate has an average pore diameter of 3.5 µm or more.

7. The positive electrode active material according to any one of claims 2 to 6, wherein the sintered plate has a thickness of 30 to 300 µm.

8. 10. The cathode active material of claim 1, wherein the cathode active material is in the form of a powder.

9. The positive electrode active material according to any one of claims 1 to 8, wherein the molar ratio of Li / (Ni+Co+Mn) in the positive electrode active material is 0.95 to 1.

10.

10. A positive electrode layer comprising the positive electrode active material according to any one of claims 1 to 9; a negative electrode layer including a negative electrode active material; LiOH.Li interposed between the positive electrode layer and the negative electrode layer 2 SO 4 a solid electrolyte based on ZnO; A lithium ion secondary battery comprising:

11. The positive electrode layer is composed of particles of the positive electrode active material, the LiOH. 2 SO 4 The lithium ion secondary battery according to claim 10, comprising particles of the base solid electrolyte and an electronic conductive assistant in the form of a mixture.

12. The negative electrode active material is Li 4 Ti 5 O 12 The lithium ion secondary battery according to claim 10 or 11,

13. The LiOH.Li 2 SO 4 The solid electrolyte was found to be 3LiOH.Li by X-ray diffraction. 2 SO 4 The lithium ion secondary battery according to any one of claims 10 to 12, comprising a solid electrolyte identified as:

Citation Information

Patent Citations

  • Negative potential treating appliance

    JP1981001157A

  • Method for producing lithium-ion cathode material

    JP2006520525A

  • Method of manufacturing positive electrode active material for solid battery

    JP2016170942A

  • Nonaqueous electrolyte secondary battery

    JP2018206609A

  • JPP6780140B