Polyamide resin composition and molded article obtained by molding the same

The semi-aromatic polyamide resin composition with carbon fiber reinforcement addresses the limitations of conventional thermoplastics by providing high heat resistance, low specific gravity, and improved fluidity, enabling high-speed rotation with reduced creep strain and energy consumption.

JP7554485B2Active Publication Date: 2024-09-20UNITIKA LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2021516083
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-04-26
Filing Date
2020-04-17
Publication Date
2024-09-20
Estimated Expiration
2040-04-17

AI Technical Summary

Technical Problem

Conventional thermoplastic resins used for high-speed rotating bodies like impellers and fans are expensive, require high-temperature molds, have poor fluidity, and high specific gravity, leading to weight and centrifugal force issues that limit rotational speed.

Method used

A resin composition comprising semi-aromatic polyamide with specific dicarboxylic and diamine components and carbon fiber reinforcement, optimized for low creep strain and improved fluidity, allowing molding at lower temperatures.

Benefits of technology

The composition achieves high heat resistance, low specific gravity, excellent fluidity, and reduced creep strain, enabling high-speed rotation with improved mechanical properties and reduced energy costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554485000003
    Figure 0007554485000003
  • Figure 0007554485000002
    Figure 0007554485000002
  • Figure 0007554485000001
    Figure 0007554485000001
Patent Text Reader

Abstract

A polyamide resin composition containing a semi-aromatic polyamide (A) having a melting point of 290-330°C and a fibrous reinforcing material (B), wherein the polyamide resin composition is characterized in that the creep strain in the flow direction after 100 hours under measurement conditions of a temperature of 100°C and a tensile load of 75 MPa is 2.0% or less.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyamide resin composition containing a semi-aromatic polyamide and a fibrous reinforcing material, and to a molded article obtained by molding the same. [Background technology]

[0002] In recent years, thermoplastic resins have been used instead of metals as materials for rotors such as impellers and fans in order to reduce weight. Rotating bodies have also come to rotate at high speeds, for example, rotors with a maximum outer diameter of about 25 mm rotate at high speeds of 100,000 rpm. Such high-speed rotating bodies require heat resistance, centrifugal strength, dimensional accuracy, and low specific gravity, and are required to have higher centrifugal strength than conventional materials and a small amount of tensile creep strain, which corresponds to dimensional accuracy, especially in high-temperature environments around 100°C.

[0003] As thermoplastic resins used as materials for impellers capable of high-speed rotation, Patent Document 1 discloses an alloy of nylon 66 and polyethersulfone, Patent Document 2 discloses an alloy of polyetherketone and polyetherimide, Patent Document 3 discloses polyetheretherketone, polyetherketone, and an alloy of polyetherketone and polyetherimide, and Patent Document 4 discloses polyimide, polyamideimide, bismaleimide triazine, and polyethersulfone. However, these thermoplastic resins are generally expensive, require high-temperature molds during molding, and have poor fluidity during molding, which results in poor design of the shape of the rotor, such as an impeller. In addition, these thermoplastic resins generally have a high specific gravity, so the rotor obtained is not only heavy, but also subject to a large centrifugal force when rotated at high speed, which results in a problem that the rotation speed cannot be increased above a certain level. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Utility Model Publication No. 63-063597 [Patent Document 2] Japanese Patent Application Publication No. 02-269766 [Patent Document 3] Japanese Patent Application Publication No. 06-042302 [Patent Document 4] Publication number 01-111102 Summary of the Invention [Problem to be solved by the invention]

[0005] The present invention aims to provide a resin composition which is less expensive, has a lower specific gravity, and has excellent flowability, and which can be used to mold molded articles with excellent appearance at a low mold temperature of 120°C or less, and which has excellent dimensional accuracy even in a high-temperature environment. [Means for solving the problem]

[0006] Means for Solving the Problems The inventors of the present invention conducted intensive research to solve the above problems and discovered that a resin composition containing a specific resin and a reinforcing material and having a specific amount of creep strain can solve the above problems, thereby completing the present invention.

[0007] The polyamide resin composition of the present invention comprises: The present invention comprises a semi-aromatic polyamide (A) having a melting point of 290 to 330°C and a fibrous reinforcing material (B), It is characterized by a creep strain of 2.0% or less after 100 hours under measurement conditions of a temperature of 100°C and a tensile load of 75 MPa. According to the polyamide resin composition of the present invention, the semi-aromatic polyamide (A) contains a dicarboxylic acid component and a diamine component as constituent components, and it is preferred that the dicarboxylic acid component contains terephthalic acid as a main component and the diamine component contains 1,10-decanediamine as a main component. According to the polyamide resin composition of the present invention, the fibrous reinforcing material (B) is preferably a carbon fiber having a tensile strength of 4000 to 4800 MPa. The molded article of the present invention is obtained by molding the above polyamide resin composition. The molded body of the present invention is preferably a body of revolution. According to the molded article of the present invention, the rotating body is preferably an impeller. According to the molded article of the present invention, the rotating body is preferably a fan. Effect of the Invention

[0008] According to the present invention, it is possible to provide a resin composition which has high heat resistance, low specific gravity, excellent fluidity, and small creep strain in a high-temperature environment of about 100°C, and a molded article made from the resin composition and which has excellent appearance. The molded article of the present invention can be suitably used for rotating bodies such as impellers and fans. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a perspective view of an impeller, which is an example of a molded body according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The polyamide resin composition of the present invention contains a semi-aromatic polyamide (A) and a fibrous reinforcing material (B).

[0011] In the present invention, the semi-aromatic polyamide (A) contains a dicarboxylic acid component and a diamine component as constituent components, the dicarboxylic acid component containing an aromatic dicarboxylic acid, and the diamine component containing an aliphatic diamine. The dicarboxylic acid component constituting the semi-aromatic polyamide (A) preferably contains terephthalic acid (T) as a main component, and from the viewpoints of heat resistance and creep characteristics, the content of terephthalic acid in the dicarboxylic acid component is preferably 75 mol % or more, more preferably 85 mol % or more, and even more preferably 100 mol %. From the viewpoints of heat resistance and processability, the diamine component in the semi-aromatic polyamide (A) is preferably an aliphatic diamine having 8 to 12 carbon atoms. Examples of aliphatic diamines having 8 to 12 carbon atoms include 1,8-octanediamine, 1,9-nonanediamine, 1,10-decanediamine, 1,11-undecanediamine, and 1,12-dodecanediamine, which may be used alone or in combination. Among these, it is preferable that the diamine component contains 1,10-decanediamine as the main component because of its high versatility, and from the viewpoints of heat resistance and creep properties, the content of 1,10-decanediamine in the diamine component is preferably 75 mol% or more, more preferably 85 mol% or more, and even more preferably 100 mol%. In the present invention, specific examples of the semi-aromatic polyamide (A) include polyamide 8T, polyamide 9T, polyamide 10T, polyamide 11T, and polyamide 12T.

[0012] The dicarboxylic acid component of the semi-aromatic polyamide (A) may contain a dicarboxylic acid other than terephthalic acid. Examples of the dicarboxylic acid other than terephthalic acid include aromatic dicarboxylic acids such as phthalic acid, isophthalic acid, and naphthalenedicarboxylic acid, aliphatic dicarboxylic acids such as oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, and dodecanedioic acid, and alicyclic dicarboxylic acids such as cyclohexanedicarboxylic acid. The content of the dicarboxylic acid other than terephthalic acid in the dicarboxylic acid component is preferably less than 25 mol%, more preferably less than 15 mol%, and it is even more preferable that the dicarboxylic acid component does not substantially contain a dicarboxylic acid other than terephthalic acid.

[0013] The diamine component of the semi-aromatic polyamide (A) may contain other diamines other than the aliphatic diamines having 8 to 12 carbon atoms. Examples of the other diamines include aliphatic diamines such as 1,2-ethanediamine, 1,3-propanediamine, 1,4-butanediamine, 1,5-pentanediamine, 1,6-hexanediamine, 1,7-heptanediamine, 1,13-tridecanediamine, 1,14-tetradecanediamine, and 1,15-pentadecanediamine, alicyclic diamines such as cyclohexanediamine, and aromatic diamines such as xylylenediamine and benzenediamine. The content of other diamines other than the aliphatic diamines having 8 to 12 carbon atoms in the diamine component is preferably less than 25 mol%, more preferably less than 15 mol%, and it is even more preferable that the diamine component does not substantially contain other diamines other than the aliphatic diamines having 8 to 12 carbon atoms.

[0014] The semi-aromatic polyamide (A) may contain, as necessary, lactams such as caprolactam and laurolactam, and ω-aminocarboxylic acids such as aminocaproic acid and 11-aminoundecanoic acid. The content of these is preferably less than 10 mol% based on the total number of moles of the raw material monomers, and it is more preferable that the semi-aromatic polyamide (A) is substantially free of these.

[0015] The semi-aromatic polyamide (A) preferably contains a monocarboxylic acid component as a constituent. By containing a monocarboxylic acid, the semi-aromatic polyamide can maintain a low amount of free amino groups at the terminals, suppressing decomposition and discoloration of the polyamide due to thermal or oxidative degradation when exposed to heat, and can have low water absorption because the terminals become hydrophobic. As a result, the heat resistance and low water absorption of the resulting resin composition can be improved.

[0016] The content of the monocarboxylic acid component is preferably 0.3 to 4.0 mol%, more preferably 0.3 to 3.0 mol%, further preferably 0.3 to 2.5 mol%, and particularly preferably 0.8 to 2.5 mol% based on the total monomer components constituting the semi-aromatic polyamide (A). By making the content of the monocarboxylic acid component 0.3 to 4.0 mol%, it is possible to reduce the molecular weight distribution during polymerization, improve the mold releasability during molding, and suppress the amount of gas generated during molding. On the other hand, if the content of the monocarboxylic acid component exceeds 4.0 mol%, the mechanical properties may be deteriorated. In the present invention, the content of the monocarboxylic acid refers to the proportion of the residue of the monocarboxylic acid in the semi-aromatic polyamide (A), that is, the residue of the monocarboxylic acid from which the terminal hydroxyl group is eliminated.

[0017] Examples of the monocarboxylic acid component include aliphatic monocarboxylic acids, alicyclic monocarboxylic acids, and aromatic monocarboxylic acids. Among them, aliphatic monocarboxylic acids are preferred because they can reduce the amount of gas generated by the semi-aromatic polyamide-derived components, improve the fluidity of the resin composition, reduce mold fouling, and improve mold releasability.

[0018] The monocarboxylic acid component is preferably a monocarboxylic acid having a molecular weight of 140 or more, more preferably a monocarboxylic acid having a molecular weight of 170 or more. By using a monocarboxylic acid having a molecular weight of 140 or more, mold releasability can be improved, the amount of gas generated at the temperature during molding can be suppressed, and molding flowability can be improved. Examples of aliphatic monocarboxylic acids having a molecular weight of 140 or more include caprylic acid, nonanoic acid, decanoic acid, lauric acid, myristic acid, palmitic acid, stearic acid, and behenic acid. Examples of alicyclic monocarboxylic acids having a molecular weight of 140 or more include 4-ethylcyclohexanecarboxylic acid, 4-hexylcyclohexanecarboxylic acid, and 4-laurylcyclohexanecarboxylic acid. Examples of aromatic monocarboxylic acids having a molecular weight of 140 or more include 4-ethylbenzoic acid, 4-hexylbenzoic acid, 4-laurylbenzoic acid, 1-naphthoic acid, 2-naphthoic acid, and derivatives thereof. The monocarboxylic acid components may be used alone or in combination. Also, a monocarboxylic acid having a molecular weight of 140 or more may be used in combination with a monocarboxylic acid having a molecular weight of less than 140. In the present invention, the molecular weight of the monocarboxylic acid refers to the molecular weight of the monocarboxylic acid as a raw material.

[0019] In the present invention, the semi-aromatic polyamide (A) must have a melting point of 290 to 330° C. The polyamide resin composition of the present invention can reduce the creep strain by containing the semi-aromatic polyamide (A) having a melting point of 290 to 330° C. and the fibrous reinforcing material (B). If the melting point of the semi-aromatic polyamide (A) is less than 290° C., the polyamide resin composition will have low heat resistance and a large creep strain. On the other hand, if the semi-aromatic polyamide (A) has a melting point of more than 330° C., the melt processing temperature will be close to the decomposition temperature, and the polyamide will decompose during melt processing, making it difficult to process. This is not preferable.

[0020] The semi-aromatic polyamide (A) used in the present invention can be produced by a conventionally known method such as a thermal polymerization method or a solution polymerization method. The thermal polymerization method is preferably used because of its industrial advantages. The thermal polymerization method includes a method comprising a step (i) of obtaining a reaction product from an aromatic dicarboxylic acid component and a diamine component, and a step (ii) of polymerizing the obtained reaction product.

[0021] As an example of step (i), a method is given in which a dicarboxylic acid powder is heated in advance to a temperature equal to or higher than the melting point of the diamine and equal to or lower than the melting point of the dicarboxylic acid, and the diamine is added to the dicarboxylic acid powder at this temperature without substantially containing water so as to maintain the powder state of the dicarboxylic acid. As another method, a suspension of a molten diamine and a solid dicarboxylic acid is stirred and mixed to obtain a mixed liquid, and then a reaction of the dicarboxylic acid and the diamine to form a salt and a reaction of the generated salt to form a low polymer are carried out at a temperature lower than the melting point of the semi-aromatic polyamide to be finally produced, thereby obtaining a mixture of the salt and the low polymer. In this case, the crushing may be carried out during the reaction, or the reaction may be carried out after the reaction and the mixture is taken out and crushed. As step (i), the former is preferred because it is easy to control the shape of the reaction product.

[0022] As an example of step (ii), the reaction product obtained in step (i) is solid-phase polymerized at a temperature lower than the melting point of the semi-aromatic polyamide to be finally produced, and the molecular weight is increased to a predetermined molecular weight to obtain a semi-aromatic polyamide. The solid-phase polymerization is preferably carried out in an inert gas stream such as nitrogen at a polymerization temperature of 180 to 270°C and a reaction time of 0.5 to 10 hours.

[0023] The reaction apparatus for step (i) and step (ii) is not particularly limited, and any known apparatus may be used. Step (i) and step (ii) may be carried out in the same apparatus or in different apparatuses.

[0024] In the production of the semi-aromatic polyamide (A), a polymerization catalyst may be used to increase the efficiency of polymerization. Examples of the polymerization catalyst include phosphoric acid, phosphorous acid, hypophosphorous acid, and salts thereof. The amount of the polymerization catalyst added is usually preferably 2.0 mol% or less based on the total monomers constituting the semi-aromatic polyamide (A).

[0025] The polyamide resin composition of the present invention must contain a fibrous reinforcing material (B). Examples of the fibrous reinforcing material (B) include glass fibers, carbon fibers, boron fibers, asbestos fibers, polyvinyl alcohol fibers, polyester fibers, acrylic fibers, aramid fibers, polybenzoxazole fibers, kenaf fibers, bamboo fibers, hemp fibers, bagasse fibers, high-strength polyethylene fibers, alumina fibers, silicon carbide fibers, potassium titanate fibers, brass fibers, stainless steel fibers, steel fibers, ceramic fibers, and basalt fibers.

[0026] Among these, the fibrous reinforcing material (B) is preferably a carbon fiber having a tensile strength of 4000 to 4800 MPa. By containing carbon fibers having a tensile strength of 4000 MPa or more, the polyamide resin composition is likely to have a creep strain in the flow direction of 2.0% or less after 100 hours under measurement conditions of a temperature of 100°C and a tensile load of 75 MPa. On the other hand, the carbon fiber contained in the polyamide resin composition preferably has a tensile strength not exceeding 4800 MPa for the following reasons. That is, in the polyamide resin composition of the present invention, since the melting point of the semi-aromatic polyamide (A) is 290 to 330°C, the actual processing temperature in melt kneading reaches about 330 to 400°C. If the resin composition contains high-strength carbon fibers with a tensile strength exceeding 4800 MPa, excessive shear heat is generated during melt kneading, and the temperature further rises, causing decomposition of the resin and the surface treatment agent of the fibers, and poor dispersion of the fibers due to a decrease in viscosity. Therefore, even if the resin composition contains high-strength carbon fibers with a tensile strength exceeding 4800 MPa, not only is the strain amount and other mechanical properties not improved, but they may be reduced. In addition, even if decomposition or viscosity reduction during melt kneading does not occur due to the inclusion of high-strength carbon fibers with a tensile strength exceeding 4800 MPa, the resin composition becomes hard and the flowability decreases due to the influence of the strength of the carbon fibers. In order to suppress shear heat generation, it is possible to melt-knead using a small-scale extruder or to melt-knead by setting the discharge rate and rotation speed low, but this significantly reduces productivity.

[0027] The carbon fiber having a tensile strength of 4000 to 4800 MPa preferably has a fiber length of 0.1 to 7 mm, more preferably 0.5 to 6 mm. The carbon fiber has a fiber length of 0.1 to 7 mm, which can improve the mechanical properties of the resin composition without adversely affecting moldability. The carbon fiber also has a fiber diameter of 3 to 20 μm, more preferably 5 to 13 μm. The carbon fiber has a fiber diameter of 3 to 20 μm, which can improve the mechanical properties of the resin composition while reducing breakage during melt kneading. The cross-sectional shape of the carbon fiber is preferably a circular cross-section, but may be a rectangular, elliptical, or other irregular cross-section as necessary.

[0028] The content of carbon fiber having a tensile strength of 4000 to 4800 MPa is preferably 1 to 60% by mass, and more preferably 1 to 50% by mass since the mechanical strength is improved. Among them, the content of carbon fiber is more preferably 15 to 50% by mass since the specific gravity is lower than that of conventional resin compositions and the effect of improving the mechanical strength is large. If the content of carbon fiber in the polyamide resin composition exceeds 60% by mass, not only the effect of improving the mechanical properties of the resin is saturated and no further improvement can be expected, but also the flowability is extremely reduced, so that it may be difficult to obtain a molded product.

[0029] The polyamide resin composition of the present invention may further contain additives such as stabilizers, colorants, antistatic agents, flame retardants, flame retardant assistants, and carbonization inhibitors, as necessary. Examples of colorants include pigments such as titanium oxide, zinc oxide, and carbon black, and dyes such as nigrosine. Examples of stabilizers include hindered phenol-based antioxidants, phosphorus-based antioxidants, sulfur-based antioxidants, light stabilizers, heat stabilizers made of copper compounds, and heat stabilizers made of alcohols. Examples of flame retardants include bromine-based flame retardants, phosphorus-based flame retardants made of metal phosphinates, and flame retardants made of phosphazene compounds. Examples of flame retardant assistants include metal salts such as zinc stannate, zinc borate, antimony trioxide, antimony pentoxide, and sodium antimonate. Carbonization inhibitors are additives that improve tracking resistance, and examples of such additives include inorganic substances such as metal hydroxides and metal borates.

[0030] The polyamide resin composition of the present invention must have a creep strain of 2.0% or less after 100 hours under the measurement conditions of a temperature of 100°C and a tensile load of 75 MPa, preferably 1.5% or less, and more preferably 1.0% or less. If the polyamide resin composition has a creep strain of more than 2.0%, the rotation speed of the resulting rotor such as an impeller or fan may be limited. The polyamide resin composition of the present invention can have a creep strain of 2.0% or less by containing a semi-aromatic polyamide (A) and a fibrous reinforcing material (B).

[0031] The polyamide resin composition of the present invention preferably has a flexural strength of 180 MPa or more, more preferably 250 MPa or more, measured in accordance with ISO 178, and preferably has a flexural modulus of 5 GPa or more, more preferably 10 GPa or more, measured in accordance with ISO 178. When the polyamide resin composition has a flexural strength of 180 MPa or more and a flexural modulus of 5 GPa or more, the resulting rotating body such as an impeller or fan undergoes little dimensional change and can be rotated at a higher speed.

[0032] The polyamide resin composition of the present invention is preferably produced by blending the semi-aromatic polyamide (A), the fibrous reinforcing material (B), and additives added as required, followed by melt kneading. Examples of the melt kneading method include a method using a batch kneader such as a Brabender, a Banbury mixer, a Henschel mixer, a helical rotor, a roll, a single-screw extruder, a twin-screw extruder, or the like.

[0033] Methods for processing the polyamide resin composition into various shapes include, for example, a method in which the molten mixture is extruded into a strand shape and then formed into a pellet shape, a method in which the molten mixture is hot-cut or underwater-cut into a pellet shape, a method in which the mixture is extruded into a sheet shape and then cut, and a method in which the mixture is extruded into a block shape and then pulverized into a powder shape.

[0034] The molded article of the present invention is obtained by molding the above-mentioned polyamide resin composition, and can be used for rotating bodies such as impellers and fans. Typically, the impeller is housed in a housing, and when the impeller rotates, a flow is generated in the space between the outer surface of the impeller and the inner surface of the housing; the faster the impeller rotates and the smaller the space, the faster the flow that is generated. On the other hand, an impeller rotating at high speed is subjected to a large stress (centrifugal force) in the centrifugal direction proportional to its mass, and furthermore, bending stress is applied in the opposite direction to the rotation due to resistance with the fluid, so that the impeller is always slightly deformed when rotating. If high-speed rotation continues for a long period of time, the impeller will gradually deform in the centrifugal direction. The degree of this continuous deformation can be evaluated by the creep deformation of the impeller material. Also, the degree of instantaneous deformation can be evaluated by the elastic modulus of the impeller material. In order to improve performance, the impeller is designed to reduce the gap formed by the dimensional difference between the impeller outer diameter and the housing inner diameter and to rotate faster, so the material constituting the high-performance impeller is more suitable for a material with a lower specific gravity, a higher elastic modulus, and a smaller creep deformation. The polyamide resin composition of the present invention has high heat resistance and high creep strength, so it can be suitably used as a rotating body such as a propeller, an impeller, a fan, an axial fan, a blade, an impeller, and a sliding member such as an actuator and a bearing. It can be particularly suitably used for rotating body applications that are small, have thin blades, and are used at high speeds of 10,000 revolutions per minute or more.

[0035] Examples of methods for producing a molded article by molding the polyamide resin composition include injection molding, extrusion molding, blow molding, and sinter molding. Among these, injection molding is preferred because it has a large effect of improving mechanical properties and moldability.

[0036] The injection molding machine is not particularly limited, and examples thereof include a screw in-line type injection molding machine and a plunger type injection molding machine. The polyamide resin composition heated and melted in the cylinder of the injection molding machine is measured for each shot, injected in a molten state into a mold, cooled and solidified in a predetermined shape, and then removed from the mold as a molded body. The resin temperature during injection molding is preferably equal to or higher than the melting point (Tm) of the semi-aromatic polyamide (A), and more preferably lower than (Tm+50°C).

[0037] The mold temperature during molding is not particularly limited, but is preferably 80 to 150° C. When the polyamide resin composition of the present invention is used in a mold within this temperature range, a molded article having a high degree of crystallinity can be obtained, and thus a molded article having excellent heat resistance and low water absorption can be obtained. Conventional resins used as materials for impellers capable of high speed rotation all require a mold temperature of 200° C. or higher during molding. The polyamide resin composition of the present invention can be molded using a mold at a lower temperature than conventional resins, making it possible to reduce energy costs during mass molding production.

[0038] In addition, when the resin composition is heated and melted, it is preferable to use a resin composition pellet that has been sufficiently dried. If the resin composition contains a large amount of moisture, it may foam in the cylinder of the injection molding machine, making it difficult to obtain an optimal molded product. The moisture content of the resin composition pellet used for injection molding is preferably less than 0.3% by mass, more preferably less than 0.1% by mass. EXAMPLES

[0039] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. 1.Measurement method The properties of the polyamide resin composition and the molded article were measured and evaluated by the following methods. (1) Melting point Using a differential scanning calorimeter (PerkinElmer DSC-7), the sample was heated to 360°C at a rate of 20°C / min, held at 360°C for 5 minutes, cooled to 25°C at a rate of 20°C / min, held at 25°C for a further 5 minutes, and then heated again at a rate of 20°C / min. The top of the endothermic peak was taken as the melting point.

[0040] (2) Density After the obtained pellets of the resin composition were thoroughly dried, they were injection molded using an injection molding machine (FANUC S2000i-100B type) under the conditions of a cylinder temperature (melting point + 15°C) and a molding cycle of 35 seconds to prepare dumbbell test pieces. In the cases of Examples 1 to 12 and Comparative Examples 1 to 10 and 12, the mold temperature was set to 120°C, and in the case of Comparative Example 11, the mold temperature was set to 90°C. The density of the obtained dumbbell test pieces was measured in accordance with ISO 1183.

[0041] (3) Mechanical properties The flexural strength and flexural modulus were measured in accordance with ISO 178 using dumbbell test pieces prepared in the same manner as described in (2) above. In addition, a tensile creep test was carried out using the prepared dumbbell test pieces under a tensile load of 75 MPa in an atmosphere at a temperature of 100°C, with reference to ISO899-1, and the creep strain after 100 hours was measured.

[0042] (4) Appearance (arithmetic mean height) The obtained pellets of the resin composition were thoroughly dried, and then test pieces of 40 mm x 40 mm x 3.0 mmt were produced using an injection molding machine (J35-AD manufactured by Japan Steel Works, Ltd.) under the following conditions: cylinder temperature (melting point + 15°C), mold surface roughness (arithmetic mean height (Sa)) of 1 μm, mold temperature of 180°C, and molding cycle of 30 seconds. Similarly, test pieces were prepared at a mold temperature of 120°C. Using a 3D shape measuring machine (Keyence VR-3200), the arithmetic mean height (Sa) was measured at a magnification of 12x within a 25mm x 25mm area in the center of the test piece. In the present invention, an arithmetic mean height (Sa) of 5 μm or less was considered to be acceptable.

[0043] (5) Liquidity The obtained pellets of the resin composition were thoroughly dried, and then a 0.5 mm thick test piece for measuring the flow length was produced using an injection molding machine (J35-AD manufactured by Japan Steel Works, Ltd.) under conditions of a cylinder temperature (melting point + 15°C), a mold temperature of 120°C, and a molding cycle of 30 seconds. In the present invention, a flow length of 8 mm or more is considered acceptable, and a flow length of 15 mm or more is preferable.

[0044] (6) Productivity In the examples, the melt kneading conditions for producing the resin composition pellets (screw rotation speed (Ns) 250 rpm, output rate (Q) 25 kg / h) were used, and the extrusion rate per revolution of the screw (Q / Ns) was kept constant while the output rate (Q) was increased. The upper limit of the producible output rate (Q) until the torque of the extruder increased or the torque fluctuation became large and melt kneading became difficult was determined as the maximum output rate. The higher the maximum output rate, the easier the polyamide resin composition is to knead, and the higher the productivity and production efficiency.

[0045] (7) Continuous durability test An impeller having a maximum outer diameter of 25 mm was produced by the molding method described in (2) above, except that the mold for molding the impeller in Figure 1 was used instead of the mold for producing the dumbbell test specimen. The obtained impeller was placed in a housing with a gap of 500 μm formed by the dimensional difference between the outer diameter of the impeller and the inner diameter of the housing, and a continuous durability test was performed for 200 hours at a rotation speed of 100,000 rpm using a spin tester. The continuous durability of the impeller was evaluated in terms of the fatigue of the impeller, creep life, and the time until the impeller was destroyed due to the impeller coming into contact with the housing due to deformation of the blades, causing the impeller to crack or chip.

[0046] (8) Contact test of wing Using a spin tester, the gap formed by the dimensional difference between the outer diameter of the impeller and the inner diameter of the spin tester was set to two values, 500 μm and 100 μm, and five impellers each manufactured by the same method as in (7) above were rotated at a rotation speed of 120,000 rpm for one minute, and the percentage of impellers that were destroyed due to contact between the blades, cracks being generated in the impeller, chipping, etc. was measured.

[0047] 2.Raw materials The raw materials used in the examples and comparative examples are shown below. (1) Polyamide Semi-aromatic polyamide (PA10T-1) 4.81 kg of powdered terephthalic acid (TPA) as a dicarboxylic acid component, 0.15 kg of stearic acid (STA) as a monocarboxylic acid component, and 9.3 g of sodium hypophosphite monohydrate as a polymerization catalyst were placed in a ribbon blender-type reactor, and heated to 170°C while stirring at a rotation speed of 30 rpm under nitrogen sealing. Then, while maintaining the temperature at 170°C and the rotation speed at 30 rpm, 5.04 kg of 1,10-decanediamine (DDA) heated to 100°C as a diamine component was continuously added (continuous liquid injection method) using a liquid injection device over 2.5 hours to obtain a reaction product. The molar ratio of the raw material monomers was TPA:DDA:STA = 49.3:49.8:0.9 (the equivalent ratio of the functional groups of the raw material monomers was TPA:DDA:STA = 49.5:50.0:0.5). The resulting reaction product was then polymerized in the same reactor at 250° C. for 8 hours at a rotation speed of 30 rpm under a nitrogen stream to produce polyamide powder. Thereafter, the obtained polyamide powder was formed into strands using a twin-screw kneader, the strands were passed through a water tank to cool and solidify, and the strands were cut with a pelletizer to obtain pellets of semi-aromatic polyamide (PA10T-1).

[0048] ·Semi-aromatic polyamide (PA10T-2, PA10T / 10I-1, 2, 3, PA10T / 6T-1, 2, PA9T-1, 2, 3, 4) Except for changing the resin composition as shown in Table 1, semi-aromatic polyamide pellets were obtained in the same manner as for PA10T-1.

[0049] The resin composition and properties of the obtained semi-aromatic polyamide are shown in Table 1.

[0050] [Table 1]

[0051] PA66: Polyamide 66 (Unitika nylon 66 A125J, manufactured by Unitika Ltd.), melting point 260℃ (2) PEEK Polyetheretherketone (VESTAKEEP 2000G, Daicel-Evonik), melting point 340°C

[0052] (3) Fibrous reinforcing materials CF1: Carbon fiber (Toray T800SC-24K) Tensile strength 5880MPa CF2: Carbon fiber (Mitsubishi Rayon TR06NEB4J) Tensile strength 4900MPa CF3: Carbon fiber (Mitsubishi Rayon TR06NLB5K) Tensile strength 4120MPa CF4: Carbon fiber (Teijin Carbon Tenax HTA-C6-NR) Tensile strength 3920MPa CF5: Carbon fiber (Mitsubishi Rayon 223HE) Tensile strength 3800MPa GF: Glass fiber (Nippon Electric Glass Co., Ltd. T-262H) Tensile strength 3200MPa

[0053] Example 1 90 parts by mass of PA10T-1 was measured using a loss-in-weight type continuous quantitative feeder (KUBOTA CE-W-1 type) and fed to the main feed port of a same-direction twin-screw extruder (Toshiba Machine TEM26SS type) with a screw diameter of 26 mm and L / D 50, and melt-kneaded. During the process, 10 parts by mass of CF3 was fed from a side feeder, and melt-kneaded further. After being taken out of the die in the form of a strand, it was passed through a water tank to be cooled and solidified, and then cut with a pelletizer to obtain pellets of the resin composition. The barrel temperature of the extruder was set to (melting point of PA10T-1 -5 to +15 ° C), the screw rotation speed was 250 rpm, and the discharge rate was 25 kg / h.

[0054] Examples 2 to 12, Comparative Examples 1 to 12 Except for changing the formulation of the resin composition as shown in Table 2, the same procedure as in Example 1 was carried out to obtain pellets of the resin composition.

[0055] The resin composition and evaluation results of the obtained resin composition are shown in Table 2.

[0056] [Table 2]

[0057] The polyamide resin compositions of Examples 1 to 12 had components within the ranges specified by the present invention, and therefore had creep strains of 2.0% or less. Furthermore, the molded articles molded at mold temperatures of 120°C and 180°C had small surface roughness (arithmetic mean height (Sa)) and excellent appearance. The polyamide resin compositions of Examples 11 and 12 had slightly poor fluidity due to the high tensile strength of the carbon fibers. The polyamide resin compositions of Examples 1 and 2 had a small content of fibrous reinforcing material, and the polyamide resin compositions of Examples 6 to 10 had a slightly large amount of creep strain due to the low melting point and low heat resistance of the semi-aromatic polyamide resin. The resin compositions of Examples 3 and 9 contained semi-aromatic polyamide (A) whose monocarboxylic acid component was stearic acid, and therefore had longer flow lengths than the resin compositions of Examples 5 and 10, whose semi-aromatic polyamide (A) contained benzoic acid as its monocarboxylic acid component. The resin composition of Comparative Example 1 did not contain a fibrous reinforcing material, the resin compositions of Comparative Examples 2 and 3 used carbon fibers with a tensile strength of less than 4000 MPa, and the resin compositions of Comparative Examples 4 and 5 used glass fibers without carbon fibers, so all of them had large creep strains. In Comparative Example 6, the content of the fibrous reinforcing material was too high, so that melt kneading was not possible, and a resin composition could not be obtained. The resin compositions of Comparative Examples 7 to 11 had large creep strains because they used polyamide resins with low melting points, and the resin composition of Comparative Example 12 had high density because it used polyether ether ketone, and the molded article molded in a low-temperature mold had high surface roughness (Sa) and poor appearance.

[0058] The impeller molded from the resin composition obtained in the comparative example was destroyed within 50 hours in the continuous durability test, but the impeller molded from the resin composition of the example had a lifespan of 100 hours or more. When the load is discontinuous, the influence of heat generation is reduced and a strain recovery effect can be expected, so that an impeller having a lifespan of 100 hours or more in the continuous durability test can be said to have sufficient durability. The impellers of Examples 3 to 5, 11, and 12 can change the gap with the housing from 500 μm to 100 μm, and a compressor using this can improve the compression efficiency.

Claims

1. The impeller is characterized in that it is molded from a polyamide resin composition containing a semi-aromatic polyamide (A) having a melting point of 290 to 330°C and a fibrous reinforcing material (B), and in that the amount of creep strain after 100 hours under measurement conditions of a temperature of 100°C and a tensile load of 75 MPa is 2.0% or less, and is used at a rotation speed of 10,000 revolutions per minute or more.

2. The impeller according to claim 1, characterized in that the semi-aromatic polyamide (A) contains a dicarboxylic acid component and a diamine component as constituent components, the dicarboxylic acid component containing terephthalic acid as a main component, and the diamine component containing 1,10-decanediamine as a main component.

3. 3. The impeller according to claim 1, wherein the fibrous reinforcing material (B) is carbon fiber having a tensile strength of 4000 to 4800 MPa.

Citation Information

Patent Citations

  • Impeller

    JP1988063597U

  • JP1989111102U

  • Internal combustion engine part and auxiliary machinery part

    JP1990269766A

  • Fiber reinforced resin-made impeller

    JP1994042302A

  • Fiber reinforcement substrate

    JP2013049749A