Method for producing reduced chlorine solid fuel

By heating, crushing, and separating heat-treated resin waste through wind sorting and water washing, the method effectively reduces chlorine content in solid fuel production, enhancing efficiency and machinery safety.

JP7554567B2Active Publication Date: 2024-09-20TAIHEIYO CEMENT CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020049767
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-03-19
Publication Date
2024-09-20
Estimated Expiration
2040-03-19

AI Technical Summary

Technical Problem

Existing methods struggle to efficiently produce solid fuel with reduced chlorine content from heat-treated resin waste due to varying particle sizes, fluidity, and floatability, leading to machinery damage and reduced washing efficiency.

Method used

A method involving heating, crushing, wind sorting, washing with water, and centrifugal separation to separate and remove chlorine from waste plastics, resulting in a chlorine-reduced solid fuel.

Benefits of technology

The method efficiently produces solid fuel with reduced chlorine content, preventing machinery damage and improving washing efficiency, while maintaining high combustibility and ease of handling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554567000001
    Figure 0007554567000001
Patent Text Reader

Abstract

To provide an effective manufacturing method of a solid fuel with reduced chlorine.SOLUTION: A manufacturing method of a chlorine-reduced solid fuel includes a first step of heating a chlorine-including waste; a second step of breaking the waste after the first step; a third step of separating the waste after the second step by wind power screening into a heavy-weight article and a light-weight article and recovering the light-weight article; a forth step of washing the recovered light-weight article with water; and a fifth step of separating the water-washed light-weight article from water.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a reduced chlorine solid fuel. [Background technology]

[0002] Conventionally, a large amount of incineration ash from resin waste has been disposed of in landfills, but in recent years, attempts have been made to effectively use it as fuel because resin contains a large amount of carbon. However, since resin waste contains chlorine-containing resins such as polyvinyl chloride, the incineration ash may contain dioxins.

[0003] Therefore, it has been proposed to remove chlorine from the fly ash and incineration ash of resin waste by washing with water and to remove certain substances other than chlorine, and then to separate the solids into liquid and use the solids as a material for mixing with cement (Patent Documents 1 to 3). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2006-15190 A [Patent Document 2] JP 2014-193456 A [Patent Document 3] JP 2005-279370 A Summary of the Invention [Problem to be solved by the invention]

[0005] The present inventors attempted to create a method for producing a solid fuel in which the chlorine content was reduced by washing with water from a heat-treated resin waste as described in the above-mentioned prior art, but encountered the following problems: Compared with the incineration ash (bottom ash, fly ash) of resin waste, the heat-treated resin waste has a broader particle size distribution, contains chlorine that is not dissolved by washing with water or washing with an acid such as vinyl chloride, and contains a wide variety of impurities such as resin that has not yet become embrittled, metals, glass, and fibers in addition to the heat residue of resin, and the properties such as fluidity and floating / sinking properties during washing with water and the elution characteristics of chlorine differ depending on the particles, making it difficult to remove chlorine from the heat-treated resin waste by washing with water. Therefore, it is considered to pulverize the heat-treated resin waste, but since the heat-treated resin waste contains metal, it is difficult to remove chlorine from the heat-treated resin waste by washing with water because the work is easily interrupted by wear of the blade or metal getting caught in the blade, and resins with different rates of embrittlement due to heating are mixed. It is also considered to roughly crush the heat-treated resin waste into pieces of about a few mm, but it is difficult to remove chlorine from the heat-treated resin waste by washing with water because the properties such as fluidity and floating / sinking during washing differ depending on the particle size and density, which reduces the washing efficiency, the pumps and piping are easily clogged when transporting, and the machines are damaged or worn out during dehydration. An object of the present invention is to provide a method for efficiently producing a solid fuel with reduced chlorine content. [Means for solving the problem]

[0006] As a result of studies in consideration of the above problems, the inventors have found that solid fuel with reduced chlorine content can be efficiently produced by heating chlorine-containing waste to embrittle it, crushing it, then wind-separating the crushed material, washing the light material thus selected with water, and recovering the solid matter by solid-liquid separation.

[0007] That is, the present invention provides the following [1] to [7]. [1] A first step of heating a waste material containing chlorine; A second step of crushing the waste after the first step; A third process in which the waste from the second process is separated into heavy and light waste by wind sorting and the light waste is collected; A fourth step of washing the recovered lightweight materials; The fifth process is solid-liquid separation of the light materials after washing. A method for producing a reduced chlorine solid fuel, comprising: [2] The method for producing reduced chlorine solid fuel according to [1] above, wherein the waste material is waste plastic. [3] The method for producing a reduced-chlorine solid fuel according to [1] or [2] above, wherein in the first step, heating is performed at 250 to 500°C. [4] The method for producing a reduced-chlorine solid fuel according to any one of [1] to [3] above, wherein in the second step, the waste is crushed so that the major axis of the waste is 30 mm or less. [5] The method for producing reduced-chlorine solid fuel according to any one of [1] to [4] above, wherein in the third step, the wind speed of the wind separation is 5 m / s or more. [6] The method for producing a reduced-chlorine solid fuel according to any one of [1] to [5] above, wherein in the fifth step, solid-liquid separation is carried out by centrifugal filtration and / or centrifugal sedimentation. [7] The method for producing a reduced-chlorine solid fuel according to any one of the above [1] to [6], further comprising a step of recovering solid matter from the wastewater after the fifth step. Effect of the Invention

[0008] According to the present invention, a solid fuel having a reduced chlorine content can be efficiently produced by a simple operation. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The method for producing a reduced-chlorine solid fuel of the present invention includes steps 1 to 5. Each step will be described below.

[0010] [First step] The first step is to heat the waste. This causes the waste to decompose, resulting in the formation of voids on the surface and inside of the waste, which reduces its strength. In other words, this process makes the waste more brittle, allowing for more efficient crushing in the next step. The waste usable in the present invention is not particularly limited as long as it contains chlorine, and examples thereof include waste plastics containing chlorine. Examples of waste plastics containing chlorine include shredder dust, construction waste plastics, agricultural waste plastics, fishery waste plastics, and marine waste plastics. These waste plastics usually contain chlorine-containing resins such as polyvinyl chloride and polyvinylidene chloride. Here, in this specification, "shredder dust" refers to a mixture of fragments that are discarded after industrial waste or general waste is crushed with an industrial shredder and metals are recovered. Examples of the waste include scrapped automobiles, scrapped home appliances, vending machines, and office automation equipment.

[0011] The heating temperature is not particularly limited as long as it can embrittle the waste, but from the viewpoint of preventing dioxin generation, it is preferably a temperature equal to or higher than the melting temperature and lower than the combustion temperature. Specifically, it is preferably 250 to 500°C, more preferably 275 to 475°C, and even more preferably 300 to 450°C. The heating time is not particularly limited as long as it is possible to embrittle the waste material, but it is usually 0.5 to 5 hours, preferably 0.5 to 4 hours, and more preferably 1 to 3 hours. The heating device is not particularly limited as long as it can accommodate the waste and set the above temperature, but examples include a fixed furnace, a stoker furnace, a rotary kiln furnace, a fluidized bed furnace, a vertical furnace, and a multi-stage furnace.

[0012] [Second step] The second step is to crush the waste after the first step. This step breaks the waste into particles, which makes it easier to efficiently separate the waste by air and makes it easier to remove chlorine. The waste after the first step has its strength reduced by heating, so it can be easily crushed into particles, usually using a crusher. The crusher is not particularly limited as long as it can crush waste, but an impact crusher is preferred, such as an impact crusher, a hammer crusher, a roll crusher, or a rotary crusher. In this step, from the viewpoint of reducing chlorine and production efficiency, the major axis of the crushed waste is preferably 30 mm or less, more preferably 20 mm or less, and even more preferably 15 mm or less. Here, in this specification, the "major axis" refers to the value obtained by taking the largest crushed piece from among the crushed pieces and measuring the point where the diameter of the crushed piece is the largest. In this process, it is preferable to remove any waste with a major axis exceeding 30 mm after crushing. This allows impurities such as uncrushed metals contained in the waste to be removed, improving the efficiency of the wind sorting and water washing in the next process and preventing damage, wear, and other issues to the machinery.

[0013] [Third step] The third process is to separate the waste from the second process into heavy and light items by wind sorting, and to recover the light items. This makes it possible to remove the heavy items, which are mainly metals, glass, undecomposed resins, and large particles, preventing operational problems in the following processes and allowing the process to be carried out efficiently. Wind sorting can be carried out using a wind sorter. The air sorting machine is not particularly limited, and for example, known devices such as a zigzag type or an internal circulation type can be used. In wind sorting, it is preferable to set the wind speed so that the heavy products mainly consist of metals, glass, undecomposed resins, and large particles. Specifically, the wind speed is preferably 5 m / s or more, more preferably 7.5 m / s or more, and even more preferably 10 m / s or more. The upper limit of the wind force can be set appropriately depending on the type of waste, but is usually 30 m / s or less, and preferably 25 m / s or less.

[0014] [Fourth step] The fourth process is to wash the collected light materials. This process removes the chlorine contained in the light materials. In addition, since the washing process does not include heavy products, operational problems during washing are prevented and production efficiency is improved. The method for washing the lightweight object with water is not particularly limited as long as it is possible to bring the lightweight object into contact with water. For example, the method may include a method of placing the lightweight object in a water tank and stirring the object, a method of immersing the lightweight object in water, and a method of spraying water on the lightweight object. From the viewpoints of reducing chlorine and production efficiency, the amount of water used is preferably 1 or more, more preferably 1.5 or more, and even more preferably 2 or more, in terms of the mass ratio of water to lightweight materials (water / lightweight materials), and is preferably 30 or less, more preferably 20 or less, and even more preferably 10 or less. The washing time can be appropriately set depending on the amount of lightweight objects and the amount of water used, but is usually 2 to 30 minutes. The water temperature is usually room temperature (20°C ± 15°C).

[0015] [Fifth step] The fifth step is a step of separating the light materials after washing into solid and liquid, which allows the recovery of solid fuel with reduced chlorine content as a solid material. The solid-liquid separation is not particularly limited as long as it can separate solid matter from water, but for example, centrifugation can be used. The operation method of centrifugation may be continuous or batchwise. Examples of the centrifugation include centrifugal filtration and centrifugal sedimentation. Centrifugation may be performed multiple times, or centrifugal sedimentation and centrifugal filtration may be combined.

[0016] Centrifugal filtration can be carried out using a centrifugal filter. There are various types of centrifugal filters, but they are not particularly limited in this step. Among them, a continuous screw discharge type is preferred from the viewpoint of production efficiency. Examples of filter media for the centrifugal filter include filter cloth and screens. The use of a screen with a pore size of 0.05 mm or more is preferred in terms of efficient solid-liquid separation. The centrifugal force in the centrifugal filtration is usually 200 to 2000 G, but from the viewpoint of production efficiency, 300 to 1500 G is preferable.

[0017] Centrifugal sedimentation can be carried out using a centrifugal settler. There are various types of centrifugal settlers, but they are not particularly limited in this step. Among them, a continuous decanter type is preferred from the viewpoint of production efficiency. The centrifugal force in the centrifugal sedimentation is usually 1000 to 3000 G, but from the viewpoint of production efficiency, 1500 to 3000 G is preferable.

[0018] The wastewater from the fifth step may contain a large amount of fine particles. Therefore, after the fifth step, a step of recovering solid matter from the wastewater may be included. For example, a dehydrator may be used for the wastewater treatment. For example, a centrifugal sedimenter may be used as the dehydrator. The dehydration treatment may be performed multiple times.

[0019] In this way, the reduced chlorine solid fuel of the present invention can be produced, and the obtained solid fuel has reduced chlorine and metals. In addition, the moisture content is reduced to 20% or less, and it is easy to handle and has excellent combustibility, so it can be used as it is as a pre-kiln fuel. It may also be mixed with waste plastics, waste tatami mats, pulverized coal, waste oil, etc. and used as fuel before kiln firing. It may also be put into a coal mill together with coal to be dried and pulverized.

[0020] Although the present invention has been described in detail based on the embodiment, the present invention is not limited to the above embodiment. The present invention can be modified in various ways without departing from the gist of the invention. For example, after the crushing in the second step and before the wind separation in the third step, the crushed waste material can be subjected to a magnetic separation step.

[0021] In the magnetic separation process, the waste from the second process is magnetically separated to separate it into magnetic and non-magnetic materials, and the non-magnetic materials can be recovered. The non-magnetic materials are then subjected to wind separation in the third process. This allows magnetic metals such as iron scraps contained in the waste to be recovered, which not only increases the amount of light materials recovered in the third process but also allows the production of a higher quality reduced chlorine solid fuel.

[0022] In the magnetic separation step, a known magnetic separator such as a drum type magnetic separator, a roll type magnetic separator, or a hanging type magnetic separator can be appropriately selected and used. From the viewpoint of efficient removal of magnetized substances, the surface magnetic flux density of the magnetic separator is, for example, preferably from 500 to 12,000 gausses, and more preferably from 1,000 to 10,000 gausses.

[0023] In addition, for example, after the third step and before the fourth step, the light materials may be subjected to an eddy current sorting step, which allows valuable metals such as gold, silver, palladium, platinum, and copper to be recovered, thereby producing a higher-quality reduced-chlorine solid fuel. EXAMPLES

[0024] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to the following examples.

[0025] The apparatus used in this example is as follows: (1) Crusher: Manufactured by Oike Iron Works, Model: MHM-75 (2) Wind sorting machine: manufactured by Oike Iron Works, model: zigzag type (3) Centrifugal filter: Kotobuki Giken Kogyo Co., Ltd., model: N452K

[0026] The chlorine-containing waste materials used in this example are as follows: Raw material A: Automobile shredder dust mainly composed of plastic, rubber, and rubber Raw material B: Waste plastics, mainly consisting of crushed detergent and shampoo containers and packaging and textile waste

[0027] Example 1 1,000 kg of raw material A was heated at 325°C for 60 minutes and then crushed in a crusher. The major axis of the crushed waste was 15 mm. The crushed material was then air-sorted at a wind speed of 10 m / s to recover the lighter materials, which were then washed with water at a water / lighter mass ratio of 3, and centrifugal filtered at 400 G to recover the solid fuel.

[0028] Example 2 A solid fuel was produced in the same manner as in Example 1, except that raw material A was changed to raw material B and the wind force in the wind sorting step was changed to 7 m / s.

[0029] Comparative Example 1 A solid fuel was produced in the same manner as in Example 1, except that the wind separation step was not carried out.

[0030] Comparative Example 2 A solid fuel was produced in the same manner as in Example 2, except that the wind separation step was not carried out.

[0031] Chlorine content analysis In Examples 1 and 2, the chlorine content of the light material was analyzed before and after washing after the third step (air sorting step), and in Comparative Examples 1 and 2, the chlorine content of the crushed material was analyzed before and after washing after the second step (crushing step). The chlorine content was analyzed according to ISO 587 Solid mineral fuels - Determination of chlorine using Eschka mixture. The results are shown in Table 1.

[0032] [Table 1]

[0033] Table 1 shows that by using air to separate the crushed waste after heating and washing the lighter materials with water, solid fuel with even lower chlorine content can be efficiently produced.

Claims

1. A first step of heating the chlorine-containing waste in a heating device at a temperature equal to or higher than the melting temperature and lower than the combustion temperature; A second step of crushing the waste after the first step; A third step of separating the waste after the second step by wind power sorting at a wind speed of 5 m / s or more into heavy and light items and recovering the light items; A fourth step of washing the recovered light materials with water; The fifth step is to separate the light material after washing into solid and liquid. Including, The combustion temperature is 300 to 450°C. A method for producing reduced chlorine solid fuel (excluding the case where alkali is introduced into the heating device).

2. 2. The method for producing a reduced chlorine solid fuel according to claim 1, wherein the waste material is waste plastic.

3. 3. The method for producing reduced-chlorine solid fuel according to claim 1 or 2, wherein in the second step, the waste is crushed so that the major axis of the waste is 30 mm or less.

4. The method for producing a reduced-chlorine solid fuel according to any one of claims 1 to 3, wherein in the fifth step, solid-liquid separation is carried out by centrifugal filtration and / or centrifugal sedimentation.

5. The method for producing a reduced-chlorine solid fuel according to any one of claims 1 to 4, further comprising a step of recovering solid matter from the wastewater after the fifth step.

Citation Information

Patent Citations

  • Production of fuel having low chlorine content

    JP2000096066A

  • Method and apparatus for treating dry distillation residue of combustible waste

    JP2004305960A

  • Method and apparatus for washing incinerated ash and cement kiln dust with water

    JP2005279370A

  • Method for treating fly ash

    JP2006015190A

  • Method for treating waste

    JP2013199542A