How to recover scandium

The use of an organic solvent and cellulose powder as a filter aid in the scandium recovery process addresses poor filterability issues, enhancing the filtration rate and recovery efficiency of scandium hydroxide.

JP7554573B2Active Publication Date: 2024-09-20JX NIPPON MINING & METALS CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020073068
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-04-15
Publication Date
2024-09-20
Estimated Expiration
2040-04-15

AI Technical Summary

Technical Problem

Existing methods for recovering scandium from solutions containing scandium hydroxide suffer from poor filterability, leading to decreased recovery rates.

Method used

A method involving the use of an organic solvent to prepare scandium hydroxide, followed by crystallization and filtration with an organic filter aid such as cellulose powder, and subsequent leaching with an acidic solution to improve filterability and recover scandium.

Benefits of technology

Enhances the filtration rate of scandium hydroxide, improving the recovery process efficiency and reducing the amount of impurities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554573000002
    Figure 0007554573000002
  • Figure 0007554573000003
    Figure 0007554573000003
  • Figure 0007554573000004
    Figure 0007554573000004
Patent Text Reader

Abstract

To provide a method for improving filterability of a solution containing solid scandium hydroxide.SOLUTION: A scandium recovery method includes the steps of: preparing an organic solvent containing scandium; adding an alkaline solution to the organic solvent and crystallizing and separating scandium as scandium hydroxide in an alkaline solution; and filtrating the scandium hydroxide contained in the alkaline solution after crystallization and separation. In the step of filtrating the scandium hydroxide, the scandium hydroxide is filtrated after a filtration aid consisting of organic matter is added.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for recovering scandium. [Background technology]

[0002] Titanium is produced from titanium ore by the Kroll process, in which titanium ore and coke are fed into a fluidized bed reactor, and chlorine gas is blown into the reactor from the bottom. As a result, gaseous titanium tetrachloride is produced, which is then recovered and reduced with magnesium, etc., to produce titanium sponge.

[0003] However, titanium ore contains other useful substances besides titanium. Patent Document 1 discloses a method for recovering useful metals from titanium ore. Specifically, the method involves chlorinating titanium ore and leaching the resulting crude chlorination furnace residue with HCl.

[0004] Patent Document 2 discloses a method for separating scandium from a solution containing titanium, zirconium, and scandium, and gives titanium ore as an example of a material containing scandium.

[0005] In addition, in a method for recovering scandium from a solution containing scandium, it is preferable to remove impurities as much as possible. As such a technique, Patent Document 3 focuses on thorium as an impurity and discloses a method for effectively separating scandium and thorium by leaching and / or neutralizing under specific conditions. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Application Publication No. 3-115534 [Patent Document 2] International Publication No. 2016 / 031699 [Patent Document 3] JP 2018-150588 A Summary of the Invention [Problem to be solved by the invention]

[0007] Patent Document 3 discloses a method for obtaining a stripped solution containing solid scandium hydroxide by stripping the scandium contained in the solvent with an alkaline solution such as sodium hydroxide when separating and purifying scandium from a scandium-containing solution obtained by leaching a scandium-containing ore or an intermediate product of the ore processing using a solvent extraction method. However, the resulting scandium hydroxide has poor filterability, and no method for improving the filterability is known. If the filterability of scandium hydroxide is poor, a problem occurs in that the recovery rate of scandium decreases.

[0008] In view of the above, an object of an embodiment of the present invention is to provide a method for improving the filterability of a solution containing solid scandium hydroxide. [Means for solving the problem]

[0009] As a result of intensive research, the present inventors have found that the above problems can be solved by filtering a solution containing solid scandium hydroxide under specific conditions. Based on this finding, the present invention is specified as follows.

[0010] (1) preparing an organic solvent containing scandium; adding an alkaline solution to the organic solvent to crystallize and separate scandium as scandium hydroxide in the alkaline solution; a step of filtering the scandium hydroxide contained in the alkaline solution after the crystallization and stripping; having A method for recovering scandium, characterized in that in the step of filtering the scandium hydroxide, a filter aid made of an organic substance is added and then the scandium hydroxide is filtered. (2) filtering the scandium hydroxide and then leaching the scandium with an acidic solution to obtain a scandium leachate; adding oxalic acid to the scandium leachate to obtain scandium oxalate; calcining the scandium oxalate to obtain scandium oxide; The method for recovering scandium according to (1), further comprising: (3) The method for recovering scandium according to (2), wherein the acidic liquid is a hydrochloric acid solution. (4) The method for recovering scandium according to any one of (1) to (3), wherein the organic filter aid is cellulose powder. (5) The method for recovering scandium according to any one of (1) to (4), wherein the amount of the filter aid composed of the organic substance added to the alkaline solution after the crystallization and peeling is 0.3 times or more the mass of the scandium hydroxide contained in the solid state. (6) The method for recovering scandium according to any one of (1) to (5), wherein the extractant for scandium contained in the organic solvent is D2EHPA. (7) A method for recovering scandium according to any one of (1) to (6), wherein the organic solvent containing scandium is obtained through the following steps a) to d): a) a step of leaching titanium smelting chloride residue with an acidic solution to obtain leachate A; b) a step of neutralizing the leachate A obtained in a) and then removing the neutralized product as an impurity to obtain a neutralized solution; c) extracting scandium from the neutralized solution obtained in b) using an organic solvent; d) A step of removing impurities other than scandium from the organic solvent in which the scandium has been extracted in c). Effect of the Invention

[0011] According to an embodiment of the present invention, a method for improving the filterability of a solution containing solid scandium hydroxide can be provided. [Brief description of the drawings]

[0012] [Figure 1] 1 shows a flow chart of a scandium recovery process according to one embodiment of the present invention. [Diagram 2] 1 shows a graph of addition ratio (addition amount (g) of cellulose powder / mass (g) of scandium hydroxide contained in solid form) versus filtration time in the examples. [Diagram 3] 1 shows a graph of the addition ratio (amount (g) of cellulose powder added / mass (g) of scandium hydroxide contained in solid form) versus filtration rate in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, specific embodiments for carrying out the present invention will be described. The following description is intended to facilitate understanding of the present invention, and is not intended to limit the scope of the present invention.

[0014] <Raw materials> In the method for recovering scandium (Sc) according to the embodiment of the present invention, first, an organic solvent containing scandium is prepared. At this time, the organic solvent containing scandium is produced from a raw material containing scandium. In one embodiment, the raw material containing scandium may be an ore containing scandium. In a further embodiment, the ore containing scandium may be an ore containing scandium and thorium. In a further embodiment, the ore containing scandium may be a titanium ore which is a raw material for refining titanium (Ti). In a further embodiment, the raw material containing scandium may be a chlorination residue generated when refining Ti. In the following, although not limited thereto, a case where the raw material containing scandium is a titanium smelting chlorination residue will be described as an example of the raw material.

[0015] <Titanium Refining> Traditionally, titanium has generally been refined from titanium ore using the Kroll process. Titanium ore and coke are fed into a fluidized bed reactor. Chlorine gas is then blown into the reactor from the bottom. The titanium ore reacts with the chlorine gas to produce titanium tetrachloride, which is in a gaseous state at the temperature inside the reactor. This gaseous titanium tetrachloride is sent to the next cooling system and cooled. The cooled titanium tetrachloride becomes liquid and is recovered.

[0016] <Chloride residue> When the gaseous titanium tetrachloride is sent to the next cooling system, impurities in the form of fine powder are sent along with the gas flow to the cooling system. The impurities include substances other than titanium (iron, scandium, vanadium, niobium, zirconium, aluminum, silicon, thorium, etc., some of which are chlorides), unreacted ores, unreacted coke, etc. These impurities are recovered in the cooling system in solid form. In this specification, the recovered material is called chlorination residue. The chlorination residue may be made into a slurry or may be in the form of a dried particle group. Typically, valuable metals can be recovered using the slurry.

[0017] <Quality of chlorinated residue> The chlorinated residue obtained in the above-mentioned process contains various rare metals, and may contain useful elements such as Sc, V, Nb, Zr, Y, La, Ce, Pr, and Nd. If these elements can be recovered, the recovered materials can be used to improve profits. Although the present invention is not limited by the following theory, the chlorinated residue is a mixture generated during the titanium smelting process, and many of its components are derived from titanium concentrate. Titanium concentrate can be obtained by subjecting mined titanium ore to flotation, magnetic separation, specific gravity separation, etc. to increase the Ti grade. Therefore, it is believed that the Ti-containing particles, which are the target, tend to form relatively large particles, while other rare metal elements, which are impurities in Ti concentrate, are believed to be attached to the Ti concentrate as fine particles during concentrate production and mixed in.

[0018] <Pretreatment of chlorinated residues> The above-mentioned chlorinated residue is in a high temperature state immediately after being recovered during titanium smelting, and must be cooled before being subjected to a treatment for recovering valuable metals. The cooling method is not particularly limited, and cooling may be performed by air cooling, water cooling, or other means.

[0019] It is also preferable to wash the chlorinated residue with water before carrying out the classification described below. This is because washing with water makes it possible to remove water-soluble impurities such as FeCl2. In addition, if washing with water is performed, the above-mentioned cooling treatment can be carried out at the same time.

[0020] <Scandium recovery> An outline of scandium recovery in one embodiment is shown in Figure 1. Each step will be specifically described below.

[0021] (1) Scandium leaching process (Diagram 1 "Leaching") A leachate is obtained by leaching titanium smelting chloride residue with an acidic solution. The pH of the acidic solution is preferably adjusted to be in the range of 0.3 to 0.9 after leaching (or at the end of leaching). If the pH is less than 0.3, the amount of thorium leached increases when thorium is contained, which hinders separation from scandium. If the pH is more than 0.9, the amount of scandium leached decreases.

[0022] The temperature during the leaching step is not particularly limited, but the temperature of the acidic solution is preferably 60 to 90°C, and more preferably 80 to 90°C. If the temperature is lower than 60°C, when thorium is contained, the difference in the amount of leaching of scandium and thorium is difficult to be obtained, making separation difficult. Since the amount of leaching of thorium decreases as the temperature increases, it is preferable that the leaching temperature is high. However, due to reasons such as boiling of the solution, the typical upper limit may be 90°C. The time for the leaching reaction is not particularly limited, but may be at least 1 hour, typically 2 hours or more. The upper limit is also not particularly limited, but is typically 24 hours or less. Furthermore, the pulp concentration is not particularly limited, but may be 100 to 600 g / L, typically 200 to 500 g / L.

[0023] The components for achieving the above-mentioned acidic range are not particularly limited, but a strong acid can be used. For example, hydrochloric acid, sulfuric acid, nitric acid, hydrofluoric acid, bromic acid, or a mixture thereof can be used. The amount is not particularly limited, but it is sufficient to add an amount that can achieve the above-mentioned pH range.

[0024] (2) Leachate neutralization process (Figure 1 "Neutralization") The leached solution may be subjected to a neutralization step to adjust the pH, i.e., to a more alkaline pH than that at the time of leaching, which allows the thorium, if any, to precipitate out while leaving the scandium in solution.

[0025] The pH range in the neutralization step is preferably 1.3 to 2.5. If the pH is less than 1.3, thorium precipitation is unlikely to occur. On the other hand, if the pH exceeds 2.5, when thorium is contained, the amount of thorium precipitation does not increase, and rather thorium also precipitates. A more preferable range is a pH of 1.8 to 2.3. This allows most of the thorium to precipitate without scandium being lost due to precipitation.

[0026] In the neutralization step, the pH is adjusted to be more alkaline than during leaching, so it is preferable to use NaOH, Na2CO3, CaO, Ca(OH)2, CaCO3, LiOH, Li2CO3, KOH, K2CO3, Mg(OH)2, MgCO3, etc. The amount is not particularly limited, but it is sufficient to add an amount that can achieve the above-mentioned pH range.

[0027] From the viewpoint of ease of operation, it is preferable to carry out leaching and neutralization in the same tank. Of course, it is also possible to carry out solid-liquid separation (Figure 1 "Solid-liquid separation A") immediately after leaching (before neutralization) and carry out leaching and neutralization in different tanks.

[0028] (3) Solid-liquid separation (Figure 1 "Solid-liquid separation B") After the above precipitate is formed, solid-liquid separation can be performed. Then, by recovering the solution side containing a large amount of scandium, it is possible to reduce the contamination of thorium (as described above, thorium mainly moves to the precipitate side). By the solid-liquid separation, the neutralized product can be removed as an impurity, and a neutralized liquid can be obtained. The method of solid-liquid separation is not particularly limited, and a known method such as filtration can be used.

[0029] (4) Scandium extraction After the solid-liquid separation B step, scandium is extracted from the neutralized liquid using an organic solvent. More specifically, when the neutralized liquid is subjected to solvent extraction using TBP as an extractant, Fe migrates to the organic phase, and other rare metals such as scandium remain in the aqueous phase. Fe stripping is performed on the organic phase, and the Fe stripping liquid is discarded as wastewater. Note that when the Fe content in the raw material is low and the amount of Fe leaching is low, this Fe extraction step may be omitted.

[0030] On the other hand, the aqueous phase undergoes solvent extraction using D2EHPA (Bis(2-ethylhexyl) phosphate) as the extractant ("Scandium Extraction" in Figure 1). This transfers scandium to the organic phase, while some elements other than scandium that are impurities (e.g., Nb, Y, La, Ce, Zr, Pr, or Nd, etc.) remain in the aqueous phase (post-scandium extraction solution). The post-scandium extraction solution can be used to recover elements other than scandium.

[0031] In the above "scandium extraction", D2EHPA is added to a solution containing scandium (the above-mentioned aqueous phase) to extract scandium into an organic phase, thereby obtaining an organic solvent containing scandium. Here, it is preferable to adjust the concentration of D2EHPA in the organic phase to 0.15 to 0.30 (mol / l), the extraction temperature during solvent leaching to 20 to 45°C, and the pH during extraction to -0.5 to 0.5. By performing the solvent extraction under such conditions, scandium can be extracted more efficiently.

[0032] (5) Scrubbing process Next, the leaching solution (organic solvent containing scandium) obtained by leaching with the organic solvent is scrubbed with an acid (Fig. 1 "Scrubbing"). This makes it possible to reduce the amount of impurities other than scandium, such as iron and thorium. The acid used here can be 1M to 4.2M HCl, NaCl, H2SO4, etc.

[0033] (6) Scandium stripping and calcination Next, the scrubbed solvent (the organic solvent containing scandium after the impurities have been removed) is subjected to crystallization stripping (Figure 1 "Sc crystallization stripping (Sc stripping)") using an alkaline solution such as 1.5 to 2.5 M NaOH to obtain scandium hydroxide (crude Sc(OH)3 slurry), which is then filtered (Figure 1 "solid-liquid separation C").

[0034] In the process of filtering the scandium hydroxide, a filter aid made of an organic substance is added, and then the scandium hydroxide is filtered. Scandium hydroxide has the property of solidifying into a gel, and if it is filtered as it is, the filtration speed is slow or sufficient filtration is difficult. In contrast, in the embodiment of the present invention, since the scandium hydroxide is filtered after the filter aid made of an organic substance is added, the scandium hydroxide is well dispersed and the filtration speed is good. This is because a cake containing a mixture of suspended matter and the filter aid is formed, and filtration with a high porosity and low filtration resistivity is possible. In addition, if an inorganic substance (e.g., diatomaceous earth) is used as the filter aid, impurities (e.g., Fe, Al, Si, etc.) in the filter aid are dissolved by the acid in the process of leaching scandium with an acidic liquid after filtering the scandium hydroxide. For this reason, when a carboxylic acid such as oxalic acid is added to precipitate scandium in the form of scandium carboxylate, as described below, the scandium is contaminated by impurities eluted from the filter aid. In contrast, in the embodiment of the present invention, an organic substance is used as the filter aid, so that the amount of impurity metals (e.g., Fe, Al, Si, etc.) dissolved in acid is smaller than that of inorganic filter aids, and when a carboxylic acid such as oxalic acid is added to precipitate scandium in the form of scandium carboxylate, as described below, the filter aid is not contaminated by impurities eluted from the filter aid. Furthermore, even if an organic filter aid is decomposed or dissolved by acid, the decomposition product is an organic substance such as glucose, and can be removed in the process of calcining the scandium carboxylate to obtain scandium oxide.

[0035] The organic filter aid is preferably a cellulose powder, which has the advantages of being easily available and not causing unintended reactions such as adsorption.

[0036] The amount of the filter aid made of the organic substance added to the alkaline solution after crystallization peeling is preferably 0.3 times or more relative to the mass of scandium hydroxide contained in the solid state. According to such a configuration, the filtration rate of scandium hydroxide is further improved. The amount of the filter aid made of the organic substance added to the alkaline solution after crystallization peeling is more preferably 0.6 times or more relative to the mass of scandium hydroxide contained in the solid state, and more preferably 0.9 times or more. In addition, the upper limit of the amount of the filter aid made of the organic substance added to the alkaline solution after crystallization peeling is preferably 2.4 times or less relative to the mass of scandium hydroxide contained in the solid state, and more preferably 2.0 times or less, from the viewpoint of increasing the scandium concentration in the recovered scandium hydroxide cake and reducing the amount of material handled in the subsequent process and from the viewpoint of reducing the amount of cellulose powder used.

[0037] The scandium hydroxide is then calcined (Figure 1 "calcination"), and finally, it can be recovered in the form of scandium oxide (Sc2O3). Alternatively, the resulting Sc(OH)3 is leached with an acidic solution such as hydrochloric acid to obtain a scandium leachate. Next, a carboxylic acid such as oxalic acid is added to the scandium leachate to precipitate scandium in the form of scandium carboxylate, which is then calcined and recovered in the form of scandium oxide (Sc2O3).

[0038] (6) Classification process In one embodiment, the raw material containing scandium may be a chlorination residue as described above. In this embodiment, after washing the chlorination residue with water, the chlorination residue can be classified into coarse particles and fine particles. The classification method is not particularly limited, and may be a dry method or a wet method. A wet method is more preferable. This is because when the chlorination residue is washed with water, the trouble of drying is not required. In addition, a sieve with a specific size of opening may be used as a classification method. For wet classification, a classification machine such as a hydraulic classifier, a horizontal water flow classifier, or a centrifugal settler may be used. For dry classification, an air separator or an air classifier may be used.

[0039] The classification standard value is not particularly limited, and the size range in which rare metals (e.g., Sc, V, Nb, Zr, Y, La, Ce, Pr, or Nd) are contained in large amounts may be adopted as the upper limit value. For example, the upper limit of the standard value may be 55 μm or less, 40 μm or less, or 25 μm or less. The lower limit of the standard value may be 10 μm or more, 15 μm or more, or 20 μm or more. This makes it possible to recover, for example, at least about 82% (when the standard value is set to 25 μm), about 84% (when the standard value is set to 38 μm), or about 88% (when the standard value is set to 53 μm) of the scandium present in the chlorination residue. On the other hand, the amount of material to be recovered can be reduced. Furthermore, many of the other impurities (e.g., Fe, coke, unreacted titanium, etc.) are distributed to the coarse particle side.

[0040] When using a sieve as a classification means, the mesh size can be appropriately determined based on the above classification standard value. For example, when classifying with a standard value of 25 μm, a mesh size of 25 μm (500 mesh in the JIS standard) is used. Then, the material that passes through the sieve is called fine particles, and the material that remains on the sieve is called coarse particles.

[0041] The fine particles obtained after classification can be subjected to a leaching process under the conditions described above to recover scandium. EXAMPLES

[0042] In the following, more specific examples will be disclosed to facilitate understanding of the present invention.

[0043] (Test Example 1) Scandium was extracted from the neutralized liquid using an organic solvent containing 7.5 vol.% extractant (D2EHPA), 3 vol.% modifier (TBP), and 89.5 vol.% diluent (Shellsol D70), and impurities were removed by scrubbing to prepare an organic solvent containing scandium. Next, the organic solvent containing the scandium was subjected to crystallization stripping using a 2M NaOH solution (Figure 1 "Sc crystallization stripping (Sc stripping)") to obtain a crude Sc(OH)3 slurry. Next, the obtained crude Sc(OH)3 slurry (slurry concentration: 19 g / l) was filtered with a membrane filter (pore size: 1 μm). Separately, cellulose powder (KC Flock (registered trademark) W-200Y manufactured by Nippon Paper Industries Co., Ltd., particle size (%): 200 mesh pass 90 or more, apparent specific gravity (g / ml): 0.30 to 0.36, average particle size: about 32 μm) was added at 25 g / L as an organic filter aid to the obtained crude Sc(OH)3 slurry, and the mixture was filtered with a filter cloth (type: P-9310, air permeability: 1 (ml / cm 2 ) / sec). As a result, when filtered through a membrane filter, the filtration rate was 72 (ml / min) / m 2 When cellulose powder was added and the filtration was performed, the flow rate was 2095 (ml / min) / m 2 The filtration rate increased by about 30 times.

[0044] (Test Example 2) In order to determine the optimal amount of cellulose powder to be added as a filter aid, a crude Sc(OH)3 slurry (slurry concentration: 20 g / l) equivalent to that in Test Example 1 was prepared according to the following steps (1) to (4), and a filtration rate measurement test was carried out according to the following steps (5) to (8). (1) Prepare 21 ml of ScCl3 solution with an Sc concentration of 213 g / L. (2) Weigh out 38 g of NaOH and dissolve it in 400 ml of water. (3) Gradually add the ScCl3 solution while stirring. (4) Finally, dilute to 480 ml. (5) Divide into 80 ml portions and place each into a 100 ml container as samples of Example 2-1 to Example 2-6. (6) Add the specified amount of cellulose powder used in Test Example 1 to each flask and stir. (7) Filter using a φ55 Nutsche filter and the filter cloth used in Test Example 1. At this time, the initial filtrate may leak out, so filter in small amounts at a time. (8) When the filtrate becomes clear, add back all of the liquid that was removed, start filtration, and measure the filtration time until the filtration is completed. The test conditions and evaluation results are shown in Table 1.

[0045] [Table 1]

[0046] Fig. 2 shows a graph of the addition ratio (amount of cellulose powder added (g) / mass of scandium hydroxide contained in solid form (g)) versus filtration time. Fig. 3 shows a graph of the addition ratio (amount of cellulose powder added (g) / mass of scandium hydroxide contained in solid form (g)) versus filtration speed.

[0047] According to the above test results, when the amount of cellulose powder added is 0.3 times or more the mass of the solid scandium hydroxide, the filtration rate is 312 (ml / min) / m 2 From the above, it was confirmed that the filtration rate was significantly improved compared to the filtration using the membrane filter in Test Example 1 described above.

[0048] Above, specific embodiments of the present invention have been described. The above embodiments are merely specific examples of the present invention, and the present invention is not limited to the above embodiments. For example, a technical feature disclosed in one of the above embodiments can be provided in other embodiments. In addition, for a particular method, the order of some steps can be replaced with other steps, and an additional step can be added between two specific steps. The scope of the present invention is defined by the claims.

Claims

1. providing an organic solvent containing scandium; adding an alkaline solution to the organic solvent to crystallize and separate scandium as scandium hydroxide in the alkaline solution; a step of filtering the scandium hydroxide contained in the alkaline solution after the crystallization and stripping; having A method for recovering scandium, characterized in that in the step of filtering the scandium hydroxide, only a filter aid which is cellulose powder is added, and then the scandium hydroxide is filtered.

2. The method for recovering scandium according to claim 1, wherein the amount of the filter aid, which is the cellulose powder, added to the alkaline solution after the crystallization and peeling is 0.9 to 2.0 times the mass of the scandium hydroxide contained in the solid state.

3. filtering the scandium hydroxide and then leaching the scandium with an acidic solution to obtain a scandium leachate; adding oxalic acid to the scandium leachate to obtain scandium oxalate; calcining the scandium oxalate to obtain scandium oxide; 3. The method for recovering scandium according to claim 1 or 2, further comprising:

4. 4. The method for recovering scandium according to claim 3, wherein the acidic liquid is a hydrochloric acid solution.

5. The method for recovering scandium according to any one of claims 1 to 4, wherein the extractant for scandium contained in the organic solvent is D2EHPA.

6. The method for recovering scandium according to any one of claims 1 to 5, wherein the organic solvent containing scandium is obtained through the following steps a) to d): a) leaching titanium smelting chloride residue with an acidic liquid to obtain leachate A; b) a step of neutralizing the leachate A obtained in a) and then removing the neutralized product as an impurity to obtain a neutralized solution; c) extracting scandium from the neutralized solution obtained in b) using an organic solvent; d) A step of removing impurities other than scandium from the organic solvent in which the scandium has been extracted in c).

Citation Information

Patent Citations

  • A method for recycling tombarthite from weathering crust elution-deposited tombarthite ores

    CN109097566A

  • Method for extracting titanium and scandium from a titanium ore

    JP1991115534A

  • Recovering method of rare earth metal

    JP1997291320A

  • Method for recovering scandium

    JP2018150588A

  • Method for separating scandium

    WO2016031699A1