Reinforcing fiber, its manufacturing method, and molded body using the same
Patent Information
- Application Number
- JP2020145629
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-08-31
- Publication Date
- 2024-09-20
- Estimated Expiration
- 2040-08-31
AI Technical Summary
Existing adhesive methods for reinforcing fibers in rubber products, such as those using RFL, isocyanate, and modified conjugated diene rubber, face issues of inferior adhesive strength, fiber deterioration, and equipment contamination, particularly when high temperatures are required for bonding, leading to reduced productivity and performance.
A reinforcing fiber is developed using a mixture of liquid conjugated diene rubber, an oil with low vapor pressure, and a surfactant, forming an emulsion that enhances adhesion to rubber while minimizing equipment contamination and maintaining fiber integrity.
The solution provides reinforcing fibers with excellent adhesion to rubber and abrasion resistance, enabling efficient production with reduced equipment contamination and improved manufacturing efficiency.
Smart Images

Figure 0007554607000001 
Figure 0007554607000006 
Figure 0007554607000007
Abstract
Description
[Technical field]
[0001] The present invention relates to a reinforcing fiber having excellent adhesion to rubber and abrasion resistance, a method for producing the same, and a molded article using the same. [Background technology]
[0002] In general, industrial rubber products such as tires, conveyor belts, and hoses (e.g., automotive oil brake hoses) are reinforced with synthetic fibers such as vinylon and rayon, or natural fibers such as cotton. In these products, in order to fully utilize the excellent physical properties of rubber (e.g., high strength and high elastic modulus), it is necessary to firmly bond the fiber and rubber. Conventionally, a method using an adhesive called RFL, whose main components are resorcinol-formaldehyde resin and rubber latex, has been widely known as such a method (Patent Documents 1 and 2).
[0003] However, since formaldehyde is suspected of being carcinogenic and resorcinol is suspected of being an environmental hormone, the development of alternative materials is desired. Specifically, Patent Document 3 proposes a technique using an adhesive containing an adhesive compound having an unsaturated carbon bond and an epoxy group that reacts with a vulcanizing agent used in vulcanization of rubber. Patent Document 4 proposes an adhesion method using an adhesive composition for organic fiber cords that contains a (blocked) isocyanate compound and / or an amine-based curing agent (A), an epoxy compound (B), and a rubber latex (C) and does not contain resorcinol or formaldehyde. Patent Document 5 proposes an adhesion method using an adhesive component that contains a modified conjugated diene rubber that has a hydrogen-bonding functional group in a part of the conjugated diene rubber. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 54-4976 [Patent Document 2] Japanese Patent Application Publication No. 58-2370 [Patent Document 3] JP 2011-111563 A [Patent Document 4] International Publication No. 2010 / 125992 [Patent Document 5] International Publication No. 2019 / 230700 Summary of the Invention [Problem to be solved by the invention]
[0005] The method using the adhesive described in Patent Document 3 had significantly inferior adhesion compared to the conventional method using RFL. Also, there is a description of adding a blocked isocyanate to improve adhesion, but in this case, a high temperature and / or long-term heat treatment is required to polymerize the blocked isocyanate on the coated fiber, which may deteriorate the coated fiber. The method using the adhesive described in Patent Document 4 has adhesive strength equal to or greater than that of the conventional method using RFL, but after forming an adhesive layer on the surface of the organic fiber cord, it is necessary to heat treat the cord at a high temperature (180°C and 240°C). When organic fibers such as PVA-based fibers and PET-based fibers, which are often used as reinforcing fibers, are treated by this method, there is a risk that their performance as reinforcing fibers will decrease due to deterioration. In addition, the technology described in Patent Document 5 has a risk that the highly viscous modified conjugated diene rubber attached to the fiber surface will fall off or be transferred during processing, thereby contaminating manufacturing equipment such as guides and rollers, thereby reducing productivity. Therefore, there was a need for a technology that could be used to achieve adhesive strength equivalent to that achieved by conventional RFL methods, but which would not cause degradation of general-purpose fibers, and which could be produced efficiently with less contamination of manufacturing equipment.
[0006] The present invention has been made in consideration of the above-mentioned problems in the conventional art, and aims to provide a reinforcing fiber which has excellent adhesion to rubber and abrasion resistance during processing and can be efficiently produced while suppressing contamination of the production equipment, a method for producing the same, and a molded article using the same. [Means for solving the problem]
[0007] As a result of intensive research to solve the above problems, the inventors have discovered that by using a mixture of liquid conjugated diene rubber, an oil having a specific vapor pressure, and a surfactant as an adhesive component, a reinforcing fiber having excellent adhesion to rubber and abrasion resistance can be obtained, and contamination of the manufacturing equipment can also be suppressed, thereby completing the present invention.
[0008] That is, the present invention provides the following [1] to
[13] . [1] A reinforcing fiber characterized by having, on at least a portion of the surface of the fiber, an adhesive component containing a liquid conjugated diene rubber, an oil having a vapor pressure of 10 Pa or less at 20°C, and a surfactant. [2] The reinforcing fiber according to [1] above, wherein the fiber is at least one type selected from the group consisting of polyvinyl alcohol-based fibers, regenerated cellulose-based fibers, polyester-based fibers, and polyamide-based fibers. [3] The reinforcing fiber according to [1] or [2] above, wherein the liquid conjugated diene rubber contains, in its molecule, a monomer unit derived from one or more selected from butadiene, isoprene, and farnesene. [4] The reinforcing fiber according to any one of the above [1] to [3], wherein the liquid conjugated diene rubber is a modified conjugated diene rubber having a hydrogen-bonding functional group in a portion of the conjugated diene rubber. [5] The reinforcing fiber according to [4] above, wherein the hydrogen-bonding functional group is at least one selected from a hydroxy group, an epoxy group, an aldehyde group, an acetalized aldehyde group, a carboxy group, a salt of a carboxy group, an esterified carboxy group, an acid anhydride of a carboxy group, a boronyl group, a salt of a boronyl group, an esterified boronyl group, a silanol group, and an esterified silanol group. [6] The reinforcing fiber according to any one of the above [1] to [5], wherein the surfactant is a nonionic surfactant. [7] The reinforcing fiber according to the above [6], wherein the HLB value of the nonionic surfactant is 6 to 17. [8] The reinforcing fiber according to any one of the above [1] to [7], wherein a content ratio of the surfactant to a total amount of the liquid conjugated diene rubber and the oil [surfactant / (liquid conjugated diene rubber+oil)] is 1 / 100 to 50 / 100 in mass ratio. [9] A method for producing a reinforcing fiber according to any one of the above items [1] to [8], comprising a step of mixing the liquid conjugated diene rubber, the oil and the surfactant to form an oil-in-water emulsion, and attaching the emulsion to a fiber.
[10] A woven or knitted fabric, at least in part comprising the reinforcing fiber according to any one of [1] to [8] above.
[11] A molded article using the reinforcing fiber according to any one of the above [1] to [8].
[12] The molded article according to
[11] above, further comprising a rubber component.
[13] The molded article according to the above
[11] or
[12] , which is a tire, a belt or a hose. Effect of the Invention
[0009] According to the present invention, it is possible to provide a reinforcing fiber that has excellent adhesion to rubber and abrasion resistance and can be efficiently produced while suppressing contamination of production equipment, a method for producing the same, and a molded article using the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] [Reinforcing fiber] The reinforcing fiber of the present invention is characterized in that at least a portion of the surface of the fiber has an adhesive component containing a liquid conjugated diene rubber, an oil having a vapor pressure of 10 Pa or less at 20° C., and a surfactant. According to the present invention, since a liquid conjugated diene rubber is used as an adhesive component, a reinforcing fiber having excellent adhesion to rubber can be obtained. In addition, in the present invention, by using a liquid conjugated diene rubber, an oil having a vapor pressure of 10 Pa or less at 20°C, and a surfactant in combination, the mixture can be made into an emulsion, which can be attached to the fiber more uniformly and efficiently, and the abrasion resistance of the obtained reinforcing fiber is excellent. In addition, the method is easy to handle, and the contamination of the manufacturing equipment can be suppressed, improving the manufacturing efficiency. In the present invention, "having an adhesive component containing a liquid conjugated diene rubber, an oil having a vapor pressure of 10 Pa or less at 20°C, and a surfactant on at least a portion of the surface of the fiber" may mean an embodiment in which the adhesive component is present on at least a portion of the surface of the fiber, for example, as a film or layer, or an embodiment in which the adhesive component is contained in the raw material of the fiber and the adhesive component is present on a portion of the surface of the fiber itself.
[0011] In addition, the adhesive component used in the present invention can obtain a reinforcing fiber having excellent adhesion to rubber even if it does not contain formaldehyde or a resin made from formaldehyde, which is harmful to the human body. In the present invention, if the adhesive component contains a resin made from formaldehyde, the resin may be, for example, a resorcinol / formaldehyde resin, a phenol / formaldehyde resin, a melamine / formaldehyde resin, or a derivative thereof. If the adhesive component contains the formaldehyde component, the content is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, even more preferably 3 parts by mass or less, even more preferably 1 part by mass or less, and particularly preferably substantially free of the formaldehyde component, relative to 100 parts by mass of the liquid conjugated diene rubber. The formaldehyde content can be measured by extracting the adhesive component from the reinforcing fiber with a solvent such as toluene, and then using HPLC or the like.
[0012] <Liquid conjugated diene rubber> The liquid conjugated diene rubber used in the present invention contains at least a monomer unit derived from a conjugated diene in the molecule (hereinafter also referred to as a "conjugated diene unit"). For example, it is preferable that the conjugated diene rubber contains 50 mol % or more of monomer units derived from a conjugated diene out of all monomer units in the conjugated diene rubber. Examples of the conjugated diene monomer include butadiene, 2-methyl-1,3-butadiene (hereinafter also referred to as "isoprene"), 2,3-dimethylbutadiene, 2-phenylbutadiene, 1,3-pentadiene, 2-methyl-1,3-pentadiene, 1,3-hexadiene, 1,3-octadiene, 1,3-cyclohexadiene, 2-methyl-1,3-octadiene, 1,3,7-octatriene, β-farnesene (hereinafter also referred to as "farnesene"), myrcene, and chloroprene. These conjugated dienes may be used alone or in combination of two or more. From the viewpoint of reactivity during vulcanization, the liquid conjugated diene rubber more preferably has monomer units derived from one or more selected from butadiene, isoprene, and farnesene.
[0013] In this specification, "liquid" means that the melt viscosity of the conjugated diene rubber measured at 38°C is 4,000 Pa·s or less. From the viewpoint of improving adhesiveness, the melt viscosity is preferably 0.1 Pa·s or more, more preferably 1 Pa·s or more, even more preferably 10 Pa·s or more, even more preferably 30 Pa·s or more, and even more preferably 50 Pa·s or more, and from the viewpoint of handleability, it is preferably 2,000 Pa·s or less, more preferably 1,500 Pa·s or less, and even more preferably 1,000 Pa·s or less. When the melt viscosity is within the above range, the adhesiveness of the conjugated diene rubber can be improved while improving handleability. The melt viscosity of the liquid conjugated diene rubber means a viscosity measured at 38° C. using a Brookfield viscometer (B-type viscometer).
[0014] The liquid conjugated diene rubber used in the present invention may contain units derived from other monomers than the conjugated diene monomers, so long as the units do not impair adhesion. Examples of other monomers include copolymerizable ethylenically unsaturated monomers and aromatic vinyl compounds. Examples of the ethylenically unsaturated monomer include olefins such as ethylene, 1-butene, and isobutylene. Examples of the aromatic vinyl compound include styrene, α-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 4-propylstyrene, 4-t-butylstyrene, 4-cyclohexylstyrene, 4-dodecylstyrene, 2,4-dimethylstyrene, 2,4-diisopropylstyrene, 2,4,6-trimethylstyrene, 2-ethyl-4-benzylstyrene, 4-(phenylbutyl)styrene, 1-vinylnaphthalene, 2-vinylnaphthalene, vinylanthracene, N,N-diethyl-4-aminoethylstyrene, vinylpyridine, 4-methoxystyrene, monochlorostyrene, dichlorostyrene, and divinylbenzene. These may be used alone or in combination of two or more. When the liquid conjugated diene rubber contains monomer units derived from monomers other than the conjugated diene monomer, the content thereof is preferably 30 mol % or less, more preferably 10 mol % or less, and further preferably 5 mol % or less.
[0015] The liquid conjugated diene rubber used in the present invention is preferably a modified conjugated diene rubber having a hydrogen-bonding functional group in a portion of the conjugated diene rubber, and more preferably a modified conjugated diene rubber containing a conjugated diene unit in at least a portion of the polymer chain and having a hydrogen-bonding functional group in a side chain or at an end of the polymer chain. When the modified conjugated diene rubber is used as the conjugated diene rubber, the modified conjugated diene rubber interacts with the adherend rubber and fiber, respectively, and thereby they can be bonded together. When the modified conjugated diene rubber and the adherend rubber are vulcanized to form a covalent bond, a strong cohesive force is generated, and the adhesion is further improved. Furthermore, when hydrophilic fibers are used as the fibers, it is believed that the hydrogen-bonding functional groups contained in the modified conjugated diene rubber form hydrogen bonds with the hydrophilic fibers, thereby improving adhesion.
[0016] In this specification, the term "hydrogen bond" refers to a bonding interaction formed between a hydrogen atom (donor) that is bonded to an atom with high electronegativity (O, N, S, etc.) and is electrically positively polarized, and an electronegative atom (acceptor) that has a lone pair of electrons.
[0017] In the present invention, the "hydrogen-bonding functional group" refers to a functional group that can function as a donor and an acceptor in the hydrogen bond. Specific examples of the functional group include a hydroxyl group, an epoxy group, an ether group, a mercapto group, a carboxyl group, a carbonyl group, an aldehyde group, an amino group, an imino group, an imidazole group, a urethane group, an amide group, a urea group, an isocyanate group, a nitrile group, a boronyl group, a silanol group, and derivatives thereof. An example of the derivative of the aldehyde group is an acetalized product thereof. An example of the derivative of the carboxyl group is a salt thereof, an esterified product thereof, an amidated product thereof, or an acid anhydride thereof. An example of the derivative of the boronyl group is a salt thereof, or an esterified product thereof. An example of the derivative of the silanol group is an esterified product thereof. An example of the carboxyl group is a group derived from a monocarboxylic acid or a group derived from a dicarboxylic acid. Among these, from the viewpoint of improving adhesion and ease of production of the liquid conjugated diene rubber, one or more selected from a hydroxy group, an aldehyde group, an acetalized product of an aldehyde group, a carboxy group, a salt of a carboxy group, an esterified product of a carboxy group, an acid anhydride of a carboxy group, a boronyl group, a salt of a boronyl group, an esterified product of a boronyl group, a silanol group, and an esterified product of an silanol group are preferred, one or more selected from a hydroxy group, an epoxy group, a carboxy group, a salt of a carboxy group, an esterified product of a carboxy group, an acid anhydride of a carboxy group, a boronyl group, a salt of a boronyl group, and an esterified product of a boronyl group are more preferred, one or more selected from a carboxy group, an esterified product of a carboxy group, an epoxy group, a boronyl group, and an esterified product of a boronyl group are even more preferred, and a group derived from a dicarboxylic acid and a boronyl group are even more preferred.
[0018] From the viewpoint of obtaining a reinforcing fiber having excellent rubber adhesion, the number of hydrogen-bonding functional groups in the modified conjugated diene rubber is, on average, preferably 0.5 or more, more preferably 2 or more, even more preferably 3 or more, and still more preferably 4 or more per molecule. Moreover, from the viewpoint of controlling the viscosity of the modified conjugated diene rubber within an appropriate range and improving handleability, the number of hydrogen-bonding functional groups is, on average, preferably 80 or less, more preferably 40 or less, even more preferably 30 or less, still more preferably 20 or less, and still more preferably 10 or less per molecule.
[0019] The average number of hydrogen-bonding functional groups per molecule of the modified conjugated diene rubber is calculated from the equivalent weight (g / eq) of the hydrogen-bonding functional groups of the modified conjugated diene rubber and the number-average molecular weight Mn in terms of styrene, based on the following formula: The equivalent weight of the hydrogen-bonding functional groups of the modified conjugated diene rubber means the mass of the conjugated diene bonded to each hydrogen-bonding functional group and the mass of other monomers other than the conjugated diene that are included as necessary. Average number of hydrogen-bonding functional groups per molecule = [(number average molecular weight (Mn)) / (molecular weight of styrene unit) x (average molecular weight of conjugated diene and other monomer units other than conjugated diene contained as necessary)] / (equivalent weight of hydrogen-bonding functional group) The method for calculating the equivalent weight of the hydrogen-bonding functional group can be appropriately selected depending on the type of the hydrogen-bonding functional group.
[0020] Examples of methods for obtaining a modified conjugated diene rubber include a method of adding a modifying compound to a polymer of a conjugated diene monomer (hereinafter also referred to as "production method (1)"), a method of oxidizing a conjugated diene polymer (hereinafter also referred to as "production method (2)"), a method of copolymerizing a conjugated diene monomer with a radically polymerizable compound having a hydrogen-bonding functional group (hereinafter also referred to as "production method (3)"), and a method of adding a modifying compound capable of reacting with a polymerization active terminal to a polymer of an unmodified conjugated diene monomer having a polymerization active terminal before adding a polymerization terminator (hereinafter also referred to as "production method (4)").
[0021] [Production method of modified conjugated diene rubber (1)] The production method (1) is a method in which a modifying compound is added to a polymer of a conjugated diene monomer, that is, an unmodified conjugated diene rubber (hereinafter also referred to as "unmodified conjugated diene rubber"). The unmodified conjugated diene rubber can be obtained by polymerizing a conjugated diene and, if necessary, a monomer other than the conjugated diene, for example, by emulsion polymerization or solution polymerization.
[0022] As the solution polymerization method, a known method or a method similar to a known method can be applied. For example, a predetermined amount of a monomer containing a conjugated diene is polymerized in a solvent using a Ziegler catalyst, a metallocene catalyst, or an anionically polymerizable active metal or active metal compound, if necessary in the presence of a polar compound. Examples of the solvent include aliphatic hydrocarbons such as n-butane, n-pentane, isopentane, n-hexane, n-heptane, and isooctane; alicyclic hydrocarbons such as cyclopentane, cyclohexane, and methylcyclopentane; and aromatic hydrocarbons such as benzene, toluene, and xylene.
[0023] Examples of the anionically polymerizable active metal include alkali metals such as lithium, sodium, potassium, etc., alkaline earth metals such as beryllium, magnesium, calcium, strontium, barium, etc., lanthanoid rare earth metals such as lanthanum, neodymium, etc. Among these anionically polymerizable active metals, alkali metals and alkaline earth metals are preferred, and alkali metals are more preferred. As the anionically polymerizable active metal compound, organic alkali metal compounds are preferred.As organic alkali metal compounds, for example, organic monolithium compounds such as methyl lithium, ethyl lithium, n-butyl lithium, sec-butyl lithium, t-butyl lithium, hexyl lithium, phenyl lithium, stilbene lithium, etc.; polyfunctional organic lithium compounds such as dilithiomethane, dilithionaphthalene, 1,4-dilithiobutane, 1,4-dilithio-2-ethylcyclohexane, 1,3,5-trilithiobenzene, etc.; sodium naphthalene, potassium naphthalene, etc. are included.Among these organic alkali metal compounds, organic lithium compounds are preferred, and organic monolithium compounds are more preferred.
[0024] The amount of the organic alkali metal compound used can be appropriately set depending on the melt viscosity, molecular weight, etc. of the target unmodified conjugated diene rubber and modified conjugated diene rubber, but it is usually used in an amount of 0.01 to 3 parts by mass per 100 parts by mass of all monomers including conjugated diene. The above organic alkali metal compounds can also be reacted with secondary amines such as dibutylamine, dihexylamine, dibenzylamine, etc. to form organic alkali metal amides.
[0025] In anionic polymerization, polar compounds are usually used to adjust the microstructure of the conjugated diene moiety without deactivating the reaction. Examples of polar compounds include ether compounds such as dibutyl ether, tetrahydrofuran, ethylene glycol diethyl ether, and 2,2-di(2-tetrahydrofuryl)propane; tertiary amines such as tetramethylethylenediamine and trimethylamine; alkali metal alkoxides, and phosphine compounds. The polar compounds are usually used in an amount of 0.01 to 1000 mol relative to the organic alkali metal compound. The temperature for the solution polymerization is usually in the range of −80 to 150° C., preferably in the range of 0 to 100° C., and more preferably in the range of 10 to 90° C. The polymerization mode may be either a batch system or a continuous system. The polymerization reaction can be terminated by adding a polymerization terminator. Examples of the polymerization terminator include alcohols such as methanol and isopropanol. The resulting polymerization reaction liquid is poured into a poor solvent such as methanol to precipitate the polymerized product, or the polymerization reaction liquid is washed with water, separated, and then dried to isolate the unmodified conjugated diene rubber. Of the above methods, the solution polymerization method is preferred as the method for producing the unmodified conjugated diene rubber.
[0026] The emulsion polymerization method may be a known method or a method similar to a known method, for example, a monomer containing a predetermined amount of conjugated diene is emulsified and dispersed in the presence of an emulsifier, and emulsion-polymerized by a radical polymerization initiator. Examples of the emulsifier include salts of long-chain fatty acids having 10 or more carbon atoms, rosin acid salts, etc. Examples of the long-chain fatty acid salts include potassium salts or sodium salts of fatty acids such as capric acid, lauric acid, myristic acid, palmitic acid, oleic acid, and stearic acid. As the dispersion solvent, water is usually used, and it may contain a water-soluble organic solvent such as methanol or ethanol within a range that does not impair the stability during polymerization. Examples of the radical polymerization initiator include persulfates such as ammonium persulfate and potassium persulfate, organic peroxides, and hydrogen peroxide. A chain transfer agent may be used to adjust the molecular weight of the resulting unmodified conjugated diene rubber. Examples of the chain transfer agent include mercaptans such as t-dodecyl mercaptan and n-dodecyl mercaptan; carbon tetrachloride, thioglycolic acid, diterpene, terpinolene, γ-terpinene, and α-methylstyrene dimer.
[0027] The temperature of the emulsion polymerization can be appropriately set depending on the type of radical polymerization initiator used, etc., but is usually in the range of 0 to 100° C., preferably in the range of 0 to 60° C. The polymerization mode may be either continuous polymerization or batch polymerization.
[0028] The polymerization reaction can be terminated by adding a polymerization terminator, such as an amine compound such as isopropylhydroxylamine, diethylhydroxylamine, or hydroxylamine, a quinone compound such as hydroquinone or benzoquinone, or sodium nitrite.
[0029] After the polymerization reaction is stopped, an antioxidant may be added as necessary. After the polymerization reaction is stopped, unreacted monomers are removed from the obtained latex as necessary, and then the polymerized product is coagulated using salts such as sodium chloride, calcium chloride, and potassium chloride as a coagulant, and an acid such as nitric acid or sulfuric acid is added as necessary to adjust the pH of the coagulation system to a predetermined value, and then the dispersion solvent is separated to recover the polymerized product. Next, the polymerized product is washed with water, dehydrated, and dried to obtain an unmodified conjugated diene rubber. During the coagulation, the latex and an extender oil that has been previously made into an emulsified dispersion may be mixed as necessary, and the product may be recovered as an oil-extended unmodified conjugated diene rubber.
[0030] (Modifying compound used in production method (1)) The modified compound used in the manufacturing method (1) is not particularly limited, but from the viewpoint of improving the adhesiveness of the reinforcing fiber, it is preferable to use a compound having a hydrogen-bonding functional group. Examples of the hydrogen-bonding functional group include the same as those described above. Among them, from the viewpoint of the strength of the hydrogen bond, a hydroxyl group, an epoxy group, an aldehyde group, an acetalized product of an aldehyde group, a carboxyl group, a salt of a carboxyl group, an esterified product of a carboxyl group, an acid anhydride of a carboxyl group, a boronyl group, a salt of a boronyl group, an esterified product of a boronyl group, a silanol group, and an esterified product of a silanol group are preferable. From the viewpoint of the adhesiveness with the reinforcing fiber, a functional group capable of forming a covalent bond in addition to a hydrogen bond is more preferable, and for example, for polyester fiber or vinylon, a hydroxyl group, an epoxy group, a carboxyl group, a salt of a carboxyl group, an acid anhydride of a carboxyl group, a boronyl group, a salt of a boronyl group, an esterified product of a boronyl group, and the like are examples. The modified compounds having these hydrogen-bonding functional groups may be used alone or in combination of two or more kinds.
[0031] Examples of the modifying compound include unsaturated carboxylic acids such as maleic acid, fumaric acid, citraconic acid, perpropionic acid, and itaconic acid; unsaturated carboxylic anhydrides such as maleic anhydride, citraconic anhydride, 2,3-dimethylmaleic anhydride, and itaconic anhydride; unsaturated carboxylic esters such as maleic acid esters, fumaric acid esters, citraconic acid esters, and itaconic acid esters; unsaturated carboxylic amides such as maleic acid amides, fumaric acid amides, citraconic acid amides, and itaconic acid amides; unsaturated carboxylic imides such as maleic acid imides, fumaric acid imides, citraconic acid imides, and itaconic acid imides; vinyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane, mercaptomethylmethyldiethoxysilane, mercaptomethyltrieth ... Examples of the silane compounds include silane, 2-mercaptoethyltrimethoxysilane, 2-mercaptoethyltriethoxysilane, 2-mercaptoethylmethoxydimethylsilane, 2-mercaptoethylethoxydimethylsilane, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 3-mercaptopropyldimethoxymethylsilane, 3-mercaptopropyldiethoxymethylsilane, 3-mercaptopropyldimethoxyethylsilane, 3-mercaptopropyldiethoxyethylsilane, 3-mercaptopropylmethoxydimethylsilane, and 3-mercaptopropylethoxydimethylsilane; and boronate esters such as triethyl borate, tripropyl borate, triisopropyl borate, and tributyl borate.
[0032] The amount of the modifying compound used is preferably 0.1 to 100 parts by mass, more preferably 0.5 to 50 parts by mass, and further preferably 1 to 30 parts by mass, based on 100 parts by mass of the unmodified conjugated diene rubber. The reaction temperature is usually preferably in the range of 0 to 200°C, more preferably in the range of 50 to 200°C. Alternatively, the unmodified conjugated diene rubber may be grafted with the modifying compound to introduce a hydrogen-bonding functional group, and then a modifying compound capable of reacting with the functional group may be added to introduce another hydrogen-bonding functional group into the polymer.Specifically, for example, a method may be used in which maleic anhydride is grafted onto an unmodified conjugated diene rubber obtained by living anionic polymerization, and then a compound having a hydroxyl group, such as 2-hydroxyethyl methacrylate or methanol, or a compound such as water is reacted therewith.
[0033] The amount of the modified compound added to the modified conjugated diene rubber is preferably 0.5 to 40 parts by mass, more preferably 1 to 30 parts by mass, and even more preferably 1.5 to 20 parts by mass, based on 100 parts by mass of the unmodified conjugated diene rubber. The amount of the modified compound added to the modified conjugated diene rubber can be calculated based on the acid value of the modified compound, or can be determined using various analytical instruments such as infrared spectroscopy and nuclear magnetic resonance spectroscopy.
[0034] The method of adding the modifying compound to the unmodified conjugated diene rubber is not particularly limited, and examples thereof include a method of adding a liquid unmodified conjugated diene rubber, one or more modifying compounds selected from unsaturated carboxylic acids, unsaturated carboxylic acid derivatives, boronic acid derivatives, and silane compounds, and further adding a radical generator as necessary, and heating the resulting mixture in the presence or absence of an organic solvent. There is no particular limit to the radical generator used, and commercially available organic peroxides, azo compounds, hydrogen peroxide, etc. can be used. The organic solvent used in the above method generally includes hydrocarbon solvents and halogenated hydrocarbon solvents. Among these organic solvents, hydrocarbon solvents such as n-butane, n-hexane, n-heptane, cyclohexane, benzene, toluene, and xylene are preferred.
[0035] Furthermore, when the reaction of adding the modified compound is carried out by the above method, an antioxidant may be added from the viewpoint of suppressing side reactions, etc. The antioxidant can be a commercially available one, such as butylated hydroxytoluene (BHT), N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine (Nocrac 6C), etc. The amount of the antioxidant added is preferably 0.01 to 10 parts by mass, more preferably 0.05 to 5 parts by mass, based on 100 parts by mass of the unmodified conjugated diene rubber. When the amount of the antioxidant added is within the above range, side reactions can be suppressed, and the modified conjugated diene rubber can be obtained in good yield.
[0036] [Production method of modified conjugated diene rubber (2)] The production method (2) includes a method of obtaining an oxidized conjugated diene rubber having a functional group or bond containing oxygen generated by an oxidation reaction in the molecule by oxidizing a raw material conjugated diene rubber, specifically, a hydroxy group, an aldehyde group, a carbonyl group, a carboxy group, an ether bond, etc. The method for oxidizing the raw material conjugated diene rubber includes a method of heat treating the raw material conjugated diene rubber at a temperature equal to or higher than the oxidation temperature (hereinafter also referred to as "production method (2-1)"), a method of irradiating the raw material conjugated diene rubber with light having an absorption wavelength to activate the raw material conjugated diene rubber and reacting it with oxygen (hereinafter also referred to as "production method (2-2)"), etc. Among them, the method of heat treating the raw material conjugated diene rubber at a temperature equal to or higher than the oxidation temperature (production method (2-1)) is preferred. The stage at which the oxidation reaction of the conjugated diene rubber is carried out is not particularly limited, and may be carried out before the conjugated diene rubber, oil, and surfactant are mixed, may be carried out after the conjugated diene rubber, oil, and surfactant are mixed, or may be carried out after the conjugated diene rubber, oil, and surfactant are mixed and attached to the fibers.
[0037] [Production method of oxidized conjugated diene rubber (2-1)] The production method (2-1) is a method in which a raw material conjugated diene rubber is heat-treated at a temperature equal to or higher than its oxidation temperature in an atmosphere containing oxygen, preferably in an air atmosphere. The heat treatment temperature is not particularly limited as long as it is a temperature at which the raw material conjugated diene rubber is oxidized, but from the viewpoint of increasing the reaction rate of the oxidation and improving productivity, it is preferably 150° C. or higher, more preferably 170° C. or higher, and even more preferably 190° C. or higher. When the raw material conjugated diene rubber is oxidized on the surface of the hydrophilic fiber as described below, the heat treatment temperature is preferably 240° C. or lower, and more preferably 220° C. or lower, from the viewpoint of preventing deterioration of the fiber. The heat treatment time is not particularly limited as long as the raw material conjugated diene rubber does not deteriorate, but is preferably 30 minutes or less, more preferably 20 minutes or less. Furthermore, the temperature required for the oxidation reaction can be lowered by adding a thermal radical generator to the raw material conjugated diene rubber.
[0038] Examples of the thermal radical generator include peroxides, azo compounds, redox initiators, etc. Among them, peroxides are preferred from the viewpoint that the thermal radical generator bonds with the conjugated diene rubber and a structure containing oxygen is added to the conjugated diene rubber. Examples of the peroxides include t-butyl hydroperoxide, cumene hydroperoxide, t-butyl peroxyacetate, t-butyl peroxybenzoate, t-butyl peroxyoctanoate, t-butyl peroxyneodecanoate, t-butyl peroxyisobutyrate, lauroyl peroxide, t-amyl peroxypivalate, t-butyl peroxypivalate, dicumyl peroxide, benzoyl peroxide, potassium persulfate, and ammonium persulfate.
[0039] Examples of the azo compound include azobisisobutyronitrile (AIBN), 2,2'-azobis(isobutyronitrile), 2,2'-azobis(2-butanenitrile), 4,4'-azobis(4-pentanoic acid), 1,1'-azobis(cyclohexanecarbonitrile), 2-(t-butylazo)-2-cyanopropane, and 2,2'-azobis[2-methyl-N-(1,1)-bis(hydroxymethyl)-2-hydroxyethyl]propane. Examples of the thermal radical generator include pionamide, 2,2'-azobis(2-methyl-N-hydroxyethyl)propionamide, 2,2'-azobis(N,N'-dimethyleneisobutylamidine) dichloride, 2,2'-azobis(N,N-dimethyleneisobutylamide), 2,2'-azobis(2-methyl-N-[1,1-bis(hydroxymethyl)-2-hydroxyethyl]propionamide), 2,2'-azobis(isobutylamide) dihydrate, etc. The thermal radical generator may be used alone or in combination of two or more.
[0040] The thermal radical generator may also be a redox initiator, such as a combination of persulfate, acidic sodium sulfite, and ferrous sulfate, a combination of t-butyl hydroperoxide, acidic sodium sulfite, and ferrous sulfate, or a combination of p-menthane hydroperoxide, ferrous sulfate, sodium ethylenediaminetetraacetate, and sodium formaldehyde sulfoxylate.
[0041] [Production method of oxidized conjugated diene rubber (2-2)] The production method (2-2) is a method in which a raw material conjugated diene rubber is activated by being irradiated with light having an absorption wavelength of the raw material conjugated diene rubber, and reacted with oxygen. The production method (2-2) is carried out in an atmosphere containing oxygen, preferably in an air atmosphere. The wavelength of the light used is not particularly limited as long as it is absorbed by the raw material conjugated diene rubber and causes a radical reaction, but ultraviolet light, which is strongly absorbed by the raw material conjugated diene rubber, is preferred. Furthermore, by adding a photoradical generator to the raw material conjugated diene rubber, the amount of light irradiation required for the oxidation reaction can be reduced.
[0042] Examples of the photoradical generator include acetophenone, acetophenone benzyl ketal, 1-hydroxycyclohexyl phenyl ketone, 2,2-dimethoxy-1,2-diphenylethan-1-one, xanthone, fluorenone, benzaldehyde, fluorene, anthraquinone, triphenylamine, carbazole, 3-methylacetophenone, 4,4'-dimethoxybenzophenone, benzoin propyl ether, benzyl dimethyl ketal, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropan-1-one, 2-hydroxyphenyl ... Examples of the photoradical generator include thio-2-methyl-1-phenylpropan-1-one, thioxanthone, diethylthioxanthone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-propan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1,4-(2-hydroxyethoxy)phenyl-(2-hydroxy-2-propyl)ketone, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, bis-(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide, etc. The photoradical generator may be used alone or in combination of two or more.
[0043] [Production method of modified conjugated diene rubber (3)] The production method (3) includes a method in which a conjugated diene monomer and a radically polymerizable compound having a hydrogen-bonding functional group are randomly copolymerized, block copolymerized, or graft copolymerized by a known method.
[0044] (Radically polymerizable compound having a hydrogen-bonding functional group used in production method (3)) The radical polymerizable compound having a hydrogen-bonding functional group used in the production method (3) is not particularly limited as long as it is a compound having both a hydrogen-bonding functional group and a reactive multiple bond in the molecule.Specific examples thereof include an aldehyde having a reactive multiple bond, an acetalized product of the aldehyde; a monocarboxylic acid having a reactive multiple bond, a salt of the monocarboxylic acid, an esterified product of the monocarboxylic acid, an acid anhydride of the monocarboxylic acid; an epoxy having a reactive multiple bond; a dicarboxylic acid having a reactive multiple bond, a salt of the dicarboxylic acid, an esterified product of the dicarboxylic acid, an acid anhydride of the dicarboxylic acid; and an amine compound having a reactive multiple bond.
[0045] Among the aldehydes having a multiple bond, examples of aldehydes having a reactive carbon-carbon double bond include acrolein, methacrolein, crotonaldehyde, 3-butenal, 2-methyl-2-butenal, 2-methyl-3-butenal, 2,2-dimethyl-3-butenal, 3-methyl-2-butenal, 3-methyl-3-butenal, 2-pentenal, 2-methyl-2-pentenal, 3-pentenal, and 3-methyl -4-Pentenal, 4-Pentenal, 4-Methyl-4-pentenal, 2-Hexenal, 3-Hexenal, 4-Hexenal, 5-Hexenal, 7-Octenal, 10-Undecenal, 2-Ethylcrotonaldehyde, 3-(Dimethylamino)acrolein, Myristoleinaldehyde, Palmitoleinaldehyde, Oleinaldehyde, Elaidinaldehyde, Bucksenaldehyde, Gadoleinaldehyde, El Alkenals having 3 to 30 carbon atoms, preferably 3 to 25 carbon atoms, such as kaolin aldehyde, nervonaldehyde, linolealdehyde, citronellal, cinnamaldehyde, and vanillin; alkadienals having 5 to 30 carbon atoms, preferably 5 to 25 carbon atoms, such as 2,4-pentadienal, 2,4-hexadienal, 2,6-nonadienal, and citral; linolenic aldehyde, eleostearic aldehyde, Examples of the unsaturated aldehydes include alkatrienals having 7 to 30 carbon atoms, such as aldehyde, preferably alkatrienals having 7 to 25 carbon atoms; alkatetraenals having 9 to 30 carbon atoms, such as stearidone aldehyde and arachidone aldehyde, preferably alkatetraenals having 9 to 25 carbon atoms; alkapentaenals having 11 to 30 carbon atoms, such as eicosapentaene aldehyde, preferably alkapentaenals having 11 to 25 carbon atoms. In addition, the aldehydes having cis-trans isomers include both cis and trans isomers. These aldehydes may be used alone or in combination of two or more kinds.
[0046] Among the acetalized products of aldehydes having a multiple bond, examples of the acetalized products of aldehydes having a reactive carbon-carbon double bond include acetalized products of the aldehydes, specifically, 3-(1,3-dioxalan-2-yl)-3-methyl-1-propene which is an acetalized product of 2-methyl-3-butenal, and 3-(1,3-dioxalan-2-yl)-2-methyl-1-propene which is an acetalized product of 3-methyl-3-butenal.
[0047] Among the aldehydes having a multiple bond and acetalized products of the aldehydes, examples of the aldehydes having a reactive carbon-carbon triple bond and acetalized products thereof include aldehydes having a carbon-carbon triple bond such as propioaldehyde, 2-butyn-1-al, and 2-pentyn-1-al, and acetalized products of the aldehydes.
[0048] Among the aldehydes having a multiple bond and the acetalized products of the aldehydes, aldehydes having a reactive carbon-carbon double bond are preferred, such as acrolein, methacrolein, crotonaldehyde, 3-butenal, 2-methyl-2-butenal, 2-methyl-3-butenal, 2,2-dimethyl-3-butenal, 3-methyl-2-butenal, 3-methyl-3-butenal, 2-pentenal, At least one selected from 2-pentenal, 2-methyl-2-pentenal, 3-pentenal, 3-methyl-4-pentenal, 4-pentenal, 4-methyl-4-pentenal, 2-hexenal, 3-hexenal, 4-hexenal, 5-hexenal, 7-octenal, 2-ethylcrotonaldehyde, 3-(dimethylamino)acrolein, and 2,4-pentadienal is preferred. Among them, at least one selected from acrolein, methacrolein, crotonaldehyde, and 3-butenal is more preferred because of their good reactivity during copolymerization.
[0049] Examples of the epoxy having a multiple bond include allyl glycidyl ether, methallyl glycidyl ether, glycidyl acrylate, glycidyl methacrylate, butadiene monoxide, and 1,4-cyclopentadiene monoepoxide, with allyl glycidyl ether being particularly preferred.
[0050] Examples of the monocarboxylic acid having a multiple bond, the salt of the monocarboxylic acid, the ester of the monocarboxylic acid, and the acid anhydride of the monocarboxylic acid include (meth)acrylic acid, a sodium salt of (meth)acrylic acid, a potassium salt of (meth)acrylic acid, methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, propyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2 ... butyl, 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, vinyl (meth)acrylate, 2-(trifluoromethyl)acrylic acid, methyl 2-trifluoromethylacrylate, ethyl 2-trifluoromethylacrylate, propyl 2-trifluoromethylacrylate, 2-butyl 2-trifluoromethylacrylate, 2-hydroxyethyl 2-trifluoromethylacrylate, vinyl 2-trifluoromethylacrylate, methyl cinnamate, vinyl cinnamate, methyl crotonate, vinyl crotonate, 3 -Methyl-3-butenoate, vinyl 3-methyl-3-butenoate, methyl 4-pentenoate, vinyl 4-pentenoate, methyl 2-methyl-4-pentenoate, vinyl 2-methyl-4-pentenoate, methyl 5-hexenoate, vinyl 5-hexenoate, methyl 3,3-dimethyl-4-pentenoate, vinyl 3,3-dimethyl-4-pentenoate, methyl 7-octenoate, vinyl 7-octenoate, methyl trans-3-pentenoate, vinyl trans-3-pentenoate, methyl trans-4-decenoate, vinyl trans-4-decenoate, 3-methyl-3- Ethyl butenoate, Ethyl 4-pentenoate, Ethyl 2-methyl-4-pentenoate, Ethyl 5-hexenoate, Ethyl 3,3-dimethyl-4-pentenoate, Ethyl 7-octenoate, Ethyl trans-3-pentenoate, Ethyl trans-4-decenoate, Methyl 10-undecenoate, Vinyl 10-undecenoate, (meth)acrylic anhydride, 2-(trifluoromethyl)acrylic anhydride, Cinnamic anhydride, Crotonic anhydride, 3-methyl-3-butenoic anhydride, 4-pentenoic anhydride, 2-methyl-4-pentenoic anhydride, 5-hexenoic anhydride, 3,Examples of the carboxylic acids having a reactive carbon-carbon double bond include 3-dimethyl-4-pentenoic anhydride, 7-octenoic anhydride, trans-3-pentenoic anhydride, trans-4-decenoic anhydride, 3-methyl-3-butenoic anhydride, 4-pentenoic anhydride, 2-methyl-4-pentenoic anhydride, and 10-undecenoic anhydride; and carboxylic acids having a reactive carbon-carbon triple bond and esters of the carboxylic acids, such as propiolic acid, methyl propiolate, ethyl propiolate, vinyl propiolate, tetrol acid, methyl tetrolate, ethyl tetrolate, and vinyl tetrolate. In this specification, the term "(meth)acrylic acid" collectively refers to "acrylic acid" and "methacrylic acid".
[0051] Examples of the dicarboxylic acid having a multiple bond, the salt of the dicarboxylic acid, the ester of the dicarboxylic acid, and the acid anhydride of the dicarboxylic acid include dicarboxylic acids having a reactive carbon-carbon double bond, salts of the dicarboxylic acid, esters of the dicarboxylic acid, and acid anhydrides of the dicarboxylic acid, such as maleic acid, sodium maleate, potassium maleate, methyl maleate, dimethyl maleate, maleic anhydride, itaconic acid, methyl itaconate, dimethyl itaconate, itaconic anhydride, himic acid, methyl himic acid, dimethyl himic acid, and himic acid anhydride.
[0052] As the monocarboxylic acid having a multiple bond, the salt of the monocarboxylic acid, the ester of the monocarboxylic acid, the monocarboxylic anhydride, the dicarboxylic acid having a multiple bond, the salt of the dicarboxylic acid, the ester of the dicarboxylic acid, and the acid anhydride of the dicarboxylic acid, a compound having a reactive carbon-carbon double bond is preferred, and among them, one or more selected from methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, vinyl (meth)acrylate, (meth)acrylic anhydride, 2-(trifluoromethyl)acrylic anhydride, cinnamic anhydride, crotonic anhydride, methyl maleate, dimethyl maleate, maleic anhydride, methyl itaconate, dimethyl itaconate, and itaconic anhydride are more preferred because of their good reactivity during copolymerization.
[0053] Among the amine compounds having multiple bonds, examples of amine compounds having a reactive carbon-carbon double bond include allylamine, 3-butenylamine, 4-pentenylamine, 5-hexenylamine, 6-heptenylamine, 7-octenylamine, oleylamine, 2-methylallylamine, 4-aminostyrene, 4-vinylbenzylamine, 2-allylglycine, S-allylcysteine, α-allylalanine, 2-allylaniline, geranylamine, vigabatrin, 4-vinylaniline, and 4-vinyloxyaniline, etc. Among these, one or more selected from allylamine, 3-butenylamine, and 4-pentenylamine are preferred because of their good reactivity during copolymerization.
[0054] [Production method of modified conjugated diene rubber (4)] The production method (4) is a method in which a modifying compound capable of reacting with the polymerization active terminal is added to a polymerized product of an unmodified conjugated diene monomer having a polymerization active terminal (unmodified conjugated diene rubber) before adding a polymerization terminator. The unmodified conjugated diene rubber having a polymerization active terminal can be obtained by polymerizing a conjugated diene monomer and, if necessary, a monomer other than the conjugated diene, for example, by emulsion polymerization or solution polymerization, as in the production method (1). Examples of modifying compounds that can be used in the production method (4) include dimethyldiethoxysilane, tetramethoxysilane, tetraethoxysilane, 3-aminopropyltriethoxysilane, tetraglycidyl-1,3-bisaminomethylcyclohexane, 2,4-tolylene diisocyanate, carbon dioxide, ethylene oxide, succinic anhydride, boronic acid esters such as triethyl borate, tripropyl borate, triisopropyl borate, and tributyl borate, boronic acid anhydride groups, boronic acid anhydrides such as phenylboronic acid anhydride, 4,4'-bis(diethylamino)benzophenone, N-vinylpyrrolidone, N-methylpyrrolidone, 4-dimethylaminobenzylideneaniline, and dimethylimidazolidinone, as well as other modifying agents described in JP2011-132298A.
[0055] In the production method (4), the amount of the modifying compound used is preferably in the range of 0.01 to 100 molar equivalents relative to the organic alkali metal compound, for example, when the polymerization is carried out using an organic alkali metal compound. The reaction temperature is usually in the range of -80 to 150°C, preferably 0 to 100°C, more preferably 10 to 90°C. Alternatively, the modifying compound may be added before the addition of the polymerization terminator to introduce a hydrogen-bonding functional group into the unmodified conjugated diene rubber, and then a modifying compound capable of reacting with the functional group may be added to introduce another hydrogen-bonding functional group into the polymer.
[0056] The modified conjugated diene rubber may contain units derived from other monomers than the conjugated diene monomer and the radical polymerizable compound having a hydrogen-bonding functional group, so long as the units do not impair adhesion. Examples of the other monomers include copolymerizable ethylenically unsaturated monomers and aromatic vinyl compounds, and the specific compounds and contents are the same as those described above.
[0057] The method for producing the modified conjugated diene rubber is not particularly limited, but from the viewpoint of productivity, it is preferable to produce it by the production method (1), (2) or (3), more preferably by the production method (1) or (3), and even more preferably by the production method (1).
[0058] [Physical Properties of Liquid Conjugated Diene Rubber] The weight average molecular weight (Mw) of the liquid conjugated diene rubber is not particularly limited, but from the viewpoint of improving adhesion, it is preferably 2,000 or more, more preferably 5,000 or more, even more preferably 10,000 or more, even more preferably 15,000 or more, even more preferably 20,000 or more, and particularly preferably 25,000 or more, and from the viewpoint of handleability, it is preferably 150,000 or less, more preferably 120,000 or less, even more preferably 100,000 or less, even more preferably 75,000 or less, and even more preferably 50,000 or less.
[0059] The number average molecular weight (Mn) of the liquid conjugated diene rubber is not particularly limited, but from the viewpoint of improving adhesion, it is preferably 2,000 or more, more preferably 5,000 or more, even more preferably 10,000 or more, even more preferably 15,000 or more, even more preferably 20,000 or more, and particularly preferably 25,000 or more, and from the viewpoint of handleability, it is preferably 120,000 or less, more preferably 75,000 or less, even more preferably 50,000 or less, and even more preferably 45,000 or less. The Mw and Mn of the liquid conjugated diene rubber are the weight average molecular weight and number average molecular weight in terms of polystyrene determined by gel permeation chromatography (GPC).
[0060] The molecular weight distribution (Mw / Mn) of the liquid conjugated diene rubber is preferably 1.0 to 5.0, more preferably 1.0 to 3.0, even more preferably 1.0 to 2.0, even more preferably 1.0 to 1.5, and particularly preferably 1.0 to 1.3. When Mw / Mn is within the above range, the viscosity of the liquid conjugated diene rubber varies little, making it easy to handle. The molecular weight distribution (Mw / Mn) means the ratio of weight average molecular weight (Mw) / number average molecular weight (Mn) calculated in terms of standard polystyrene, determined by GPC measurement.
[0061] The glass transition temperature (Tg) of the liquid conjugated diene rubber may vary depending on the vinyl content of the conjugated diene unit, the type of conjugated diene, the content of units derived from monomers other than the conjugated diene, etc., but is preferably −100 to 10° C., more preferably −100 to −10° C., and even more preferably −100 to −20° C. If the Tg is within the above range, the viscosity can be prevented from increasing, making the rubber easy to handle.
[0062] <Oil> In the present invention, a so-called non-volatile oil having a vapor pressure of 10 Pa or less at 20° C. is used. If the vapor pressure of the oil at 20° C. exceeds 10 Pa, the oil may volatilize after the adhesive component is applied to the surface of the fiber, causing wear of the reinforcing fiber. In addition, the adhesive component may be easily coated unevenly, reducing the adhesiveness of the adhesive component and further contaminating the manufacturing equipment during production. From this viewpoint, the vapor pressure of the oil at 20° C. is preferably 5 Pa or less, more preferably 1 Pa or less, and more preferably 1.0×10 -1 Pa or less is more preferable, and 1.0×10 -2 Pa or less is even more preferable, and 1.0×10 -5 Pa or less is even more preferable. In the present invention, the vapor pressure of oil at 20° C. refers to a value calculated from the best fit curve obtained by applying the Antoine equation to the measured value measured by the gas flow method.
[0063] The oil having a vapor pressure of 10 Pa or less at 20° C. that can be used in the present invention is not particularly limited as long as it is compatible with the liquid conjugated diene rubber, and examples of the oil include natural oils and synthetic oils. Examples of the natural oil include mineral oils and vegetable oils. Examples of mineral oils include paraffinic mineral oils, aromatic mineral oils, and naphthenic mineral oils obtained by conventional refining methods such as solvent refining and hydrogenation refining, as well as wax produced by the Fischer-Tropsch process (gas-to-liquid wax) and mineral oils produced by isomerizing wax. Commercially available paraffinic mineral oils include the "Diana Process Oil" series manufactured by Idemitsu Kosan Co., Ltd. and the "Super Oil" series manufactured by JX Nippon Oil & Energy Corporation. Examples of vegetable oils include linseed oil, camellia oil, macadamia nut oil, corn oil, mink oil, olive oil, avocado oil, camellia oil, castor oil, safflower oil, jojoba oil, sunflower oil, almond oil, rapeseed oil, sesame oil, soybean oil, peanut oil, cottonseed oil, coconut oil, palm kernel oil, and rice bran oil. Examples of synthetic oils include hydrocarbon synthetic oils, ester synthetic oils, and ether synthetic oils. Examples of hydrocarbon synthetic oils include α-olefin oligomers such as polybutene, polyisobutylene, 1-octene oligomers, 1-decene oligomers, and ethylene-propylene copolymers, or hydrogenated products thereof, alkylbenzenes, and alkylnaphthalenes. Examples of ester synthetic oils include triglycerin fatty esters, diglycerin fatty acid esters, monoglycerin fatty acid esters, monoalcohol fatty acid esters, and polyhydric alcohol fatty acid esters. Examples of ether synthetic oils include polyoxyalkylene glycols and polyphenyl ethers. Commercially available synthetic oils include the "Linearene" series manufactured by Idemitsu Kosan Co., Ltd., "FGC32", "FGC46", and "FGC68" manufactured by ANDEROL, and "Excepearl TGO" manufactured by Kao Corporation.
[0064] The oil may be one selected from the above natural oils and synthetic oils, or a mixture of two or more natural oils, two or more synthetic oils, or one or more natural oils and one or more synthetic oils.
[0065] The flash point of the oil used in the present invention is preferably 70° C. or higher from the viewpoint of safety. From this viewpoint, the flash point of the oil is more preferably 100° C. or higher, even more preferably 130° C. or higher, and even more preferably 140° C. or higher. There is no particular upper limit to the flash point of the oil, but it is preferably 320° C. or lower, more preferably 260° C. or lower, and even more preferably 200° C. or lower.
[0066] <Surfactant> The surfactant used in the present invention is not particularly limited, and examples thereof include cationic surfactants, anionic surfactants, nonionic surfactants, and amphoteric surfactants. Among these, nonionic surfactants are preferred from the viewpoint of compatibility between the adhesive component and the rubber. These surfactants may be used alone or in combination of two or more.
[0067] Examples of nonionic surfactants include polyoxyalkylene-type nonionic surfactants such as higher alcohol alkylene oxide adducts, alkylphenol alkylene oxide adducts, styrenated phenol alkylene oxide adducts, fatty acid alkylene oxide adducts, polyhydric alcohol aliphatic ester alkylene oxide adducts, higher alkylamine alkylene oxide adducts, and fatty acid amide alkylene oxide adducts, as well as polyhydric alcohol-type nonionic surfactants such as alkylglycoxides and sucrose fatty acid esters. These nonionic surfactants may be used alone, or, if necessary, two or more of them may be used in combination. Commercially available nonionic surfactants include "Adekator PC-6", "Adekator PC-8", "Adekator PC-10", and "Adekator SO-80" manufactured by ADEKA CORPORATION.
[0068] Examples of cationic surfactants include alkyl ammonium acetate salts, alkyl dimethyl benzyl ammonium salts, alkyl trimethyl ammonium salts, dialkyl dimethyl ammonium salts, alkyl pyridinium salts, oxyalkylene alkyl amines, polyoxyalkylene alkyl amines, etc. These cationic surfactants may be used alone or, if necessary, in combination of two or more kinds.
[0069] Examples of anionic surfactants include carboxylates such as fatty acid soaps, higher alcohol sulfates, higher alkyl polyalkylene glycol ether sulfates, sulfates of styrenated phenol alkylene oxide adducts, sulfates of alkylphenol alkylene oxide adducts, sulfates of sulfated oils, sulfated fatty acid esters, sulfated fatty acids, sulfated olefins, etc., alkylbenzene sulfonates, alkylnaphthalene sulfonates, naphthalene sulfonates, formalin condensates such as naphthalene sulfonic acid, α-olefin sulfonates, paraffin sulfonates, sulfonates such as sulfosuccinic acid diesters, higher alcohol phosphates, etc. These anionic surfactants may be used alone, or, if necessary, two or more of them may be used in combination. If necessary, a nonionic surfactant and an anionic surfactant may be used in combination.
[0070] Examples of the zwitterionic surfactant include alkylcarboxybetaines.
[0071] The HLB (Hydrophilic-Lipophilic Balance) value of the nonionic surfactant is preferably 6 to 17. When the HLB value is within the above range, the compatibility with liquid conjugated diene rubber and oil having a vapor pressure of 10 Pa or less at 20°C is good, and a reinforcing fiber having good adhesion to rubber can be obtained. In addition, from the viewpoint of safety of the usage environment and operability, it is preferable that the adhesive component is applied to the fiber as an oil-in-water emulsion. From the viewpoint of storage stability in water, the lower limit of the HLB value is more preferably 8 or more, and even more preferably 10 or more. From the viewpoint of compatibility of the adhesive component and adhesion to rubber, the upper limit of the HLB value is more preferably 16 or less, and even more preferably 14 or less. The HLB value is an index showing the balance between hydrophilicity and lipophilicity, and is expressed as a value from 0 to 20. For example, the HLB value can be calculated by the following formula (I) based on the Griffin method. HLB value = 20 × sum of hydrophilic moieties / molecular weight (I) Nonionic surfactants are identified by detecting and measuring their molecular weight and structural units using mass spectrometry. 1 H and 13 Since the structure can be detected and measured using C-NMR and identified based on the information obtained, it is possible to calculate the HLB value using formula (I). As a method for separating the nonionic surfactant from the adhesive component, for example, a method of fractionating and isolating the nonionic surfactant using reverse phase liquid chromatography can be mentioned.
[0072] <Viscosity of adhesive components at 30℃> The adhesive component preferably has a viscosity of 10.0 Pa·s or less, measured at 30°C. When the viscosity is within the above range, the adhesive component can be efficiently attached to the fibers, and the adhesive component is less likely to adhere to the manufacturing equipment, thereby suppressing contamination of the manufacturing equipment. From this viewpoint, the viscosity of the adhesive component measured at 30°C is more preferably 8.0 Pa·s or less, even more preferably 6.0 Pa·s or less, and even more preferably 4.0 Pa·s or less. The lower the viscosity, the better the handleability and the degree of process contamination. The viscosity of the adhesive component at 30° C. means the viscosity measured using a Brookfield viscometer (B-type viscometer) at 30° C. The rotor and rotation speed during measurement are appropriately set so as to be close to full scale.
[0073] <Composition of adhesive components> From the viewpoint of improving adhesive strength with rubber, the content of the liquid conjugated diene rubber in the adhesive component is preferably 5% by mass or more, more preferably 10% by mass or more, even more preferably 20% by mass or more, and is preferably 65% by mass or less, more preferably 50% by mass or less, even more preferably 40% by mass or less. When the content of the liquid conjugated diene rubber in the adhesive component is within the above range, it is possible to prevent the viscosity of the adhesive component from becoming extremely high while obtaining sufficient adhesive strength.
[0074] The content of the oil in the adhesive component is preferably 20% by mass or more, more preferably 35% by mass or more, even more preferably 50% by mass or more, and is preferably 90% by mass or less, more preferably 85% by mass or less, even more preferably 75% by mass or less. When the content of the oil in the adhesive component is within the above range, the viscosity of the adhesive component can be prevented from becoming extremely high, and contamination of the manufacturing equipment can be suppressed.
[0075] The content of the surfactant in the adhesive component is preferably 1% by mass or more, more preferably 2.5% by mass or more, and even more preferably 4% by mass or more. If the content of the surfactant is 1% by mass or more, a stable emulsion can be prepared when the adhesive component is made into an oil-in-water emulsion. Since a certain amount of surfactant is sufficient to obtain emulsion stability, it is preferable to make the content 15% by mass or less from the viewpoint of cost.
[0076] Furthermore, the content ratio of the surfactant to the total amount of the liquid conjugated diene rubber and the oil [surfactant / (liquid conjugated diene rubber+oil)] is preferably 1 / 100 to 50 / 100 by mass, more preferably 3 / 100 to 30 / 100, and even more preferably 5 / 100 to 10 / 100. When the content ratio of the surfactant is within the above range, a stable emulsion can be prepared when the adhesive component is made into an oil-in-water emulsion.
[0077] The liquid conjugated diene rubber may be used alone or in combination of two or more kinds. The oil may be used alone or in combination of two or more kinds. The surfactant may be used alone or in combination of two or more kinds.
[0078] Furthermore, the adhesive component in the present invention may contain other components in addition to the liquid conjugated diene rubber, oil and surfactant, within the range that does not impair the adhesive strength with the rubber. Examples of the other components include other polymers (for example, unmodified conjugated diene rubbers), acids, alkalis, antioxidants, curing agents, dispersants, pigments, dyes, adhesion aids, and carbon black. When the adhesive component contains other components, the content thereof is preferably 10,000 parts by mass or less, more preferably 1,000 parts by mass or less, even more preferably 100 parts by mass or less, still more preferably 50 parts by mass or less, still more preferably 25 parts by mass or less, and still more preferably 10 parts by mass or less, relative to 100 parts by mass of the liquid conjugated diene rubber.
[0079] <Textile> Although there is no particular limitation on the fibers used as the reinforcing fibers of the present invention, hydrophilic fibers are preferred from the viewpoint of affinity with the adhesive component. In the present invention, the term "fiber" includes not only monofilaments and long fibers, but also nonwoven fabrics, woven fabrics, knitted fabrics, felts, sponges, and other forms.
[0080] Examples of hydrophilic synthetic fibers include synthetic fibers made of a thermoplastic resin having hydrophilic functional groups such as hydroxyl groups, carboxyl groups, sulfonic acid groups, and amino groups, and / or hydrophilic bonds such as amide bonds. Specific examples of such thermoplastic resins include polyvinyl alcohol-based resins, polyamide-based resins (aliphatic polyamides such as polyamide 6, polyamide 66, polyamide 11, polyamide 12, polyamide 610, polyamide 612, and polyamide 9C (a polyamide composed of nonanediamine and cyclohexanedicarboxylic acid); semi-aromatic polyamides synthesized from aromatic dicarboxylic acids and aliphatic diamines, such as polyamide 9T (a polyamide composed of nonanediamine and terephthalic acid); wholly aromatic polyamides synthesized from aromatic dicarboxylic acids and aromatic diamines, such as polyparaphenylene terephthalamide), and polyacrylamide-based resins). Among these, polyvinyl alcohol-based resins and polyamide-based resins are preferred. The hydrophilic synthetic fibers may be used alone or in combination of two or more. In addition, these hydrophilic synthetic fibers may be further subjected to a hydrophilization treatment described below in order to further enhance the hydrophilicity.
[0081] Examples of hydrophilic natural fibers include natural cellulose fibers such as wood pulp, e.g., kraft pulp, and non-wood pulp, e.g., cotton pulp and straw pulp. Hydrophilic regenerated fibers include regenerated cellulosic fibers such as rayon, lyocell, cupra, and polynosic. These natural fibers and regenerated fibers may be used alone or in combination of two or more. Furthermore, these hydrophilic natural fibers and regenerated fibers may be further subjected to a hydrophilization treatment described later in order to further enhance the hydrophilicity.
[0082] The hydrophilic fiber may have at least a hydrophilic surface, and may be, for example, a hydrophobic fiber whose surface has been hydrophilized, or a core-sheath type composite fiber in which a hydrophobic resin is used as the core and a hydrophilic resin is used as the sheath. For examples of hydrophilic resins constituting the sheath, the description of hydrophilic synthetic fibers is cited. Examples of hydrophobic fibers made of hydrophobic resins include polyolefin fibers such as polyethylene and polypropylene, polyester fibers such as polyethylene terephthalate, and wholly aromatic polyester fibers, and among these, polyester fibers are preferred.
[0083] The hydrophilization treatment is not particularly limited as long as it is a treatment that chemically or physically imparts hydrophilic functional groups to the fiber surface. For example, the hydrophilic treatment can be carried out by a method in which a hydrophobic fiber made of the hydrophobic resin is modified with a compound containing a hydrophilic functional group such as an isocyanate group, an epoxy group, a hydroxyl group, an amino group, an ether group, an aldehyde group, a carbonyl group, a carboxyl group, or a urethane group, or a derivative thereof, or by a method in which the surface is modified by electron beam irradiation.
[0084] As the fibers used in the present invention, from the viewpoint of being used as reinforcing fibers, synthetic fibers and regenerated fibers are preferred, and among them, one or more types selected from polyvinyl alcohol-based fibers made from polyvinyl alcohol-based resins, regenerated cellulose-based fibers, polyester-based fibers, and polyamide-based fibers are preferred. In addition, polyester-based fibers are preferably subjected to the above-mentioned hydrophilization treatment. In the present invention, by using hydrophilic fibers, a strong affinity effect is exerted between the liquid conjugated diene rubber contained in the adhesive component and the hydrophilic fibers, and the adhesive component and the hydrophilic fibers are firmly bound to each other, thereby making it possible to improve the adhesive strength to the rubber. From the viewpoint of suitably using the reinforcing fiber of the present invention for automobile hoses, particularly automobile brake oil hoses, polyvinyl alcohol-based fibers that can be suitably used are commercially available from Kuraray Co., Ltd. under the product name "Vinylon" and have a single fiber fineness of about 0.1 to 30 dtex. In the present invention, one type of fiber may be used alone, or two or more types may be used in combination.
[0085] [Method of manufacturing reinforcing fibers] The method for producing the reinforcing fiber of the present invention is not particularly limited as long as it includes a step of mixing the liquid conjugated diene rubber, the oil, and the surfactant to form an oil-in-water emulsion and adhering the emulsion to fibers. By mixing the liquid conjugated diene rubber, the oil, and the surfactant to form an oil-in-water emulsion, it is possible to suppress high viscosity and improve handleability. In addition, by adhering the oil-in-water emulsion to fibers, it is possible to more uniformly and efficiently adhere the adhesive component containing the liquid conjugated diene rubber, the oil, and the surfactant to the fibers, and it is also possible to suppress contamination of the production equipment.
[0086] The order in which the liquid conjugated diene rubber, the oil, and the surfactant are mixed is not particularly limited, and the liquid conjugated diene rubber, the oil, and the surfactant may be mixed simultaneously, or the liquid conjugated diene rubber and the oil may be mixed, and the surfactant may be mixed into the resulting mixture.
[0087] The oil-in-water emulsion had a viscosity of 3.0×10 -1 It is preferable that the density is less than 1.0×10 Pa s. -1 Pa s or less is more preferable, and 6.0×10 -2 More preferably, it is 3.0×10 Pa s or less. -2 It is even more preferable that the viscosity is not more than Pa s. When the viscosity is within the above range, the adhesive component can be adhered to the fibers more uniformly and efficiently, and the adhesive component is less likely to adhere to the production equipment, thereby suppressing contamination of the production equipment. The viscosity of the oil-in-water emulsion at 20° C. means the viscosity measured using a Brookfield viscometer (B-type viscometer) at 20° C. The rotor and rotation speed during the measurement are appropriately set so as to be close to full scale.
[0088] The adhesive component is preferably applied to the fibers by one or more methods selected from immersion, roll coater, oiling roller, oiling guide, nozzle (spray) application, brush application, and the like.
[0089] From the viewpoint of improving adhesion between the reinforcing fibers and the rubber, the amount of the adhesive component attached is preferably 0.01% by mass or more, more preferably 0.1% by mass or more, and even more preferably 1% by mass or more, relative to 100% by mass of the fibers, and from the viewpoint of the balance between production cost and effect, it is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 3% by mass or less.
[0090] In the present invention, since a liquid conjugated diene rubber, a specific oil, and a surfactant are used in combination, the reinforcing fiber of the present invention can be obtained by adhering the adhesive component to the fiber and then allowing it to blend for about 3 to 10 days at room temperature of about 20°C. In some cases, the fiber may be subjected to a heat treatment after the adhesive component is adhered to the fiber. The heat treatment is preferably carried out at a treatment temperature of 100 to 200° C. for a treatment time of 0.1 seconds to 2 minutes. Since the liquid conjugated diene rubber contained in the adhesive component has reactive multiple bonds, the heat treatment in the presence of oxygen is preferably carried out at 200° C. or less, and more preferably at 175° C. or less. When the heat treatment temperature is within the above range, the amount of reactive multiple bonds in the liquid conjugated diene rubber is not reduced, and the adhesive strength can be improved, fiber deterioration is suppressed, and quality such as coloring is also improved.
[0091] The reinforcing fiber may contain other components in addition to the hydrophilic fiber and the adhesive component, such as a crosslinking agent, an acid, a base, an inorganic salt, an organic salt, a pigment, a dye, an antioxidant, a polymerization initiator, and a plasticizer. The total content of the hydrophilic fibers and the adhesive component in the reinforcing fibers is preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more, from the viewpoint of improving adhesive strength with rubber and reinforcing strength.
[0092] <Properties of reinforcing fibers> The reinforcing fiber is preferably a multifilament having a single yarn fineness of 0.1 dtex or more and 30 dtex or less. The single yarn fineness may be less than 0.1 dtex, but is preferably 0.1 dtex or more since it is difficult to produce industrially. Furthermore, if the single yarn fineness is 30 dtex or less, the surface area of the fiber when used as a reinforcing fiber is large, thereby improving adhesion to rubber. From this viewpoint, the reinforcing fiber of the present invention is preferably a multifilament having a single yarn fineness of more preferably 0.3 dtex or more, even more preferably 0.5 dtex or more, even more preferably 1 dtex or more, and more preferably 20 dtex or less, even more preferably 15 dtex or less, and even more preferably 10 dtex or less.
[0093] The rubber adhesive strength of the reinforcing fiber of the present invention is preferably 15N / 25.4mm or more, more preferably 20N / 25.4mm or more, even more preferably 25N / 25.4mm or more, even more preferably 30N / 25.4mm or more, and usually 200N / 25.4mm or less. When the rubber adhesive strength of the reinforcing fiber is the lower limit value or more, a woven fabric, knitted fabric, and molded article having excellent reinforcing strength can be obtained. The adhesive strength of the reinforcing fiber to rubber can be measured by the method described in the Examples.
[0094] The reinforcing fiber of the present invention preferably has an initial tensile resistance of 60 cN / dtex or more, measured according to JIS L 1013:2010. If the initial tensile resistance of the reinforcing fiber is 60 cN / dtex or more, the reinforcing strength when the reinforcing fiber and rubber are bonded together is improved. From this viewpoint, the initial tensile resistance is more preferably 100 cN / dtex or more, even more preferably 130 cN / dtex or more, even more preferably 160 cN / dtex or more, and particularly preferably 200 cN / dtex or more. There is no particular upper limit to the initial tensile resistance, but it is usually 1,000 cN / dtex or less.
[0095] The reinforcing fiber of the present invention can be used in any shape, but is preferably used in the form of a fiber cord, woven fabric, knitted fabric, etc., which contains the reinforcing fiber at least in part, and is more preferably used as a woven fabric or knitted fabric which contains the reinforcing fiber at least in part. For example, it can be used as a knitted fabric to be bonded to rubber, as described later. It can also be used as a reinforcing fiber to be embedded in resin, cement, etc.
[0096] [Molded body] The molded article of the present invention is not particularly limited as long as it uses the reinforcing fiber. Among them, a molded article using the reinforcing fiber and a rubber component (hereinafter also referred to as a "rubber molded article") is particularly preferred, since the reinforcing fiber has excellent adhesion to rubber. From the viewpoint of maintaining the shape of the rubber, the reinforcing fiber used in the rubber molded article is preferably used as a woven or knitted fabric containing the reinforcing fiber at least in part, and more preferably used as a laminate in which a reinforcing layer made of a woven or knitted fabric containing the reinforcing fiber at least in part is laminated with a rubber layer.
[0097] The rubber molded article can be used as a component of rubber products such as tires, e.g., automobile tires, belts, e.g., conveyor belts, timing belts, hoses, and vibration-proof rubber. Among these, it is more preferable to use the rubber molded article as a tire, a belt, or a hose. In the automobile tires, the present invention can be used for various members, such as belts, carcass plies, breakers, bead tapes, etc., which are made of composite materials of reinforcing fibers and rubber components. The hose can be used for the purpose of transporting various fluids in various applications, and is suitable, for example, as a hose for transporting fluids in automobiles. In particular, it is preferable to use the hose as a hose for liquid fuels in automobiles, a brake oil hose, and a hose for refrigerants in automobiles, and it is more preferable to use the hose as a brake oil hose in automobiles.
[0098] The rubber molded article is preferably molded using the reinforcing fibers and a rubber composition obtained by compounding a rubber component with compounding agents usually used in the rubber industry. The rubber component is not particularly limited, and examples thereof include NR (natural rubber), IR (polyisoprene rubber), BR (polybutadiene rubber), SBR (styrene-butadiene rubber), NBR (nitrile rubber), EPM (ethylene-propylene copolymer rubber), EPDM (ethylene-propylene-non-conjugated diene copolymer rubber), IIR (butyl rubber), halogenated butyl rubber, and CR (chloroprene rubber). Among these, it is preferable to use NR, IR, BR, SBR, EPDM, and CR, and it is more preferable to use EPDM. These rubber components may be used alone or in combination of two or more. For tire applications, those generally used in the tire industry can be used. Among these, it is preferable to use natural rubber alone or in combination with SBR. When natural rubber and SBR are combined, from the viewpoint of suppressing the deterioration of physical properties due to reversion of rubber, it is preferable that the mass ratio of natural rubber to SBR (natural rubber / SBR) is in the range of 50 / 50 to 90 / 10.
[0099] Examples of the natural rubber include natural rubber commonly used in the tire industry, such as TSR (Technically Specified Rubber) including SMR (Malaysian TSR), SIR (Indonesian TSR), and STR (Thailand TSR), and RSS (Ribbed Smoked Sheet); highly purified natural rubber, modified natural rubber including epoxidized natural rubber, hydroxylated natural rubber, hydrogenated natural rubber, and grafted natural rubber.
[0100] The SBR may be any of those commonly used in tires, but more specifically, the styrene content is preferably 0.1 to 70% by mass, more preferably 5 to 50% by mass, and even more preferably 15 to 35% by mass, and the vinyl content is preferably 0.1 to 60% by mass, and more preferably 0.1 to 55% by mass. The weight average molecular weight (Mw) of the SBR is preferably 100,000 to 2,500,000, more preferably 150,000 to 2,000,000, and even more preferably 200,000 to 1,500,000. Within the above range, both processability and mechanical strength can be achieved. The weight average molecular weight of the SBR is the weight average molecular weight calculated in terms of polystyrene and determined by gel permeation chromatography (GPC). The SBR may be modified SBR in which a functional group has been introduced into the SBR, as long as the effect of the present invention is not impaired. Examples of the functional group include an amino group, an alkoxysilyl group, a hydroxy group, an epoxy group, and a carboxy group.
[0101] The rubber composition may further contain a filler in addition to the rubber component. Examples of the filler include inorganic fillers such as carbon black, silica, clay, mica, calcium carbonate, magnesium hydroxide, aluminum hydroxide, barium sulfate, titanium oxide, glass fiber, fibrous filler, and glass balloons; and organic fillers such as resin particles, wood powder, and cork powder. By including such a filler in the rubber composition, it is possible to improve physical properties such as mechanical strength, heat resistance, and weather resistance, adjust hardness, and increase the amount of rubber. From the viewpoint of improving physical properties such as mechanical strength, carbon black and silica are preferred among the above fillers.
[0102] Examples of the carbon black include furnace black, channel black, thermal black, acetylene black, and ketjen black. Among these carbon blacks, furnace black is preferred from the viewpoint of improving the crosslinking rate and mechanical strength. The average particle size of the carbon black is preferably 5 to 100 nm, more preferably 5 to 80 nm, and even more preferably 5 to 70 nm. The average particle size of the carbon black can be determined by measuring the diameter of the particles using a transmission electron microscope and calculating the average value.
[0103] Examples of the silica include wet silica (hydrated silicic acid), dry silica (anhydrous silicic acid), calcium silicate, aluminum silicate, etc. Among these silicas, wet silica is preferred. The average particle size of the silica is preferably from 0.5 to 200 nm, more preferably from 5 to 150 nm, and even more preferably from 10 to 100 nm. The average particle size of the silica can be determined by measuring the diameter of the particles using a transmission electron microscope and calculating the average value.
[0104] In the rubber composition, the amount of the filler per 100 parts by mass of the rubber component is preferably 20 to 150 parts by mass, more preferably 25 to 130 parts by mass, and further preferably 25 to 110 parts by mass. When a filler other than silica and carbon black is used as the filler, the content thereof is preferably 20 to 120 parts by mass, more preferably 20 to 90 parts by mass, and further preferably 20 to 80 parts by mass, based on 100 parts by mass of the rubber component. These fillers may be used alone or in combination of two or more.
[0105] The rubber composition may further contain a crosslinking agent to crosslink the rubber component. Examples of the crosslinking agent include sulfur, sulfur compounds, oxygen, organic peroxides, phenolic resins, amino resins, quinone and quinone dioxime derivatives, halogen compounds, aldehyde compounds, alcohol compounds, epoxy compounds, metal halides and organometallic halides, and silane compounds. These crosslinking agents may be used alone or in combination of two or more. From the viewpoint of the mechanical properties of the crosslinked product, the crosslinking agent is contained in an amount of usually 0.1 to 10 parts by mass, preferably 0.5 to 10 parts by mass, and more preferably 0.8 to 5 parts by mass, per 100 parts by mass of the rubber component.
[0106] The rubber composition may further contain a vulcanization accelerator when sulfur, a sulfur compound, etc. are contained as a crosslinking agent for crosslinking (vulcanizing) the rubber component. Examples of the vulcanization accelerator include guanidine-based compounds, sulfenamide-based compounds, thiazole-based compounds, thiuram-based compounds, thiourea-based compounds, dithiocarbamic acid-based compounds, aldehyde-amine-based compounds, aldehyde-ammonia-based compounds, imidazoline-based compounds, and xanthate-based compounds. These vulcanization accelerators may be used alone or in combination of two or more. The vulcanization accelerator is usually contained in an amount of 0.1 to 15 parts by mass, preferably 0.1 to 10 parts by mass, based on 100 parts by mass of the rubber component.
[0107] When the rubber composition contains sulfur or a sulfur compound as a crosslinking agent for crosslinking (vulcanizing) the rubber component, the rubber composition may further contain a vulcanization aid. Examples of the vulcanization aid include fatty acids such as stearic acid, metal oxides such as zinc oxide, and fatty acid metal salts such as zinc stearate. These vulcanization aids may be used alone or in combination of two or more. The vulcanization aid is usually contained in an amount of 0.1 to 15 parts by mass, preferably 1 to 10 parts by mass, based on 100 parts by mass of the rubber component.
[0108] When the rubber composition contains silica as a filler, it is preferable that the rubber composition further contains a silane coupling agent, such as a sulfide compound, a mercapto compound, a vinyl compound, an amino compound, a glycidoxy compound, a nitro compound, or a chloro compound. These silane coupling agents may be used alone or in combination of two or more. The silane coupling agent is preferably contained in an amount of 0.1 to 30 parts by mass, more preferably 0.5 to 20 parts by mass, and even more preferably 1 to 15 parts by mass, based on 100 parts by mass of silica. When the content of the silane coupling agent is within the above range, dispersibility, coupling effect, and reinforcing property are improved.
[0109] The rubber composition may contain, as needed, a softener such as silicone oil, aromatic oil, TDAE (Treated Distilled Aromatic Extracts), MES (Mild Extracted Solvates), RAE (Residual Aromatic Extracts), process oil such as paraffin oil or naphthene oil, aliphatic hydrocarbon resin, alicyclic hydrocarbon resin, C9 resin, rosin resin, coumarone-indene resin, or phenol resin, for the purpose of improving processability, flowability, etc., within a range that does not impair the effects of the present invention. When the rubber composition contains the process oil as a softener, the content thereof is preferably less than 50 parts by mass per 100 parts by mass of the rubber component.
[0110] The rubber composition may contain additives such as antiaging agents, waxes, antioxidants, lubricants, light stabilizers, scorch inhibitors, processing aids, colorants such as pigments and dyes, flame retardants, antistatic agents, matting agents, antiblocking agents, UV absorbers, release agents, foaming agents, antibacterial agents, antifungal agents, and fragrances, as necessary, for the purpose of improving weather resistance, heat resistance, oxidation resistance, and the like, within a range that does not impair the effects of the present invention. Examples of the antioxidant include hindered phenol compounds, phosphorus compounds, lactone compounds, and hydroxyl compounds. Examples of the antiaging agents include amine-ketone compounds, imidazole compounds, amine compounds, phenol compounds, sulfur compounds, and phosphorus compounds. These additives may be used alone or in combination of two or more.
[0111] As a method for producing the rubber molded body, for example, the reinforcing fibers are embedded in the unvulcanized rubber composition, and the rubber composition is vulcanized to obtain a molded body in which the hydrophilic fibers and the rubber component are bonded via the adhesive component.
[0112] The brake oil hose for automobiles may, for example, have an inner rubber layer and an outer rubber layer, with one or two reinforcing layers made of the reinforcing fibers between the inner rubber layer and the outer rubber layer. Examples of the rubber components constituting the inner rubber layer and the outer rubber layer include those mentioned above. Among them, examples of the rubber components constituting the inner rubber layer include EPDM, SBR, etc., and examples of the rubber components constituting the outer rubber layer include EPDM, CR, etc. The reinforcing layer can be formed by braiding reinforcing fibers. In the method for producing the brake oil hose, a reinforcing layer (first reinforcing layer) made by braiding the reinforcing fibers is formed on the outer surface of the inner rubber layer. When forming two reinforcing layers, an intermediate rubber layer may be further formed on the outer surface of the first reinforcing layer, and a reinforcing layer (second reinforcing layer) made by braiding the reinforcing fibers may be formed on the outer surface of the intermediate rubber layer. Then, the outer rubber layer is formed on the outer surface of the reinforcing layer (first reinforcing layer or second reinforcing layer), and the hose can be produced by vulcanizing the outer rubber layer. The vulcanization temperature can be appropriately selected depending on the type of constituent materials of each layer of the brake oil hose, but it is preferable that the vulcanization temperature be 200°C or lower from the viewpoint of suppressing deterioration of the rubber and reinforcing fibers and improving the adhesive strength between the rubber and the reinforcing fibers. EXAMPLES
[0113] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way.
[0114] [Production of modified conjugated diene rubber] Production of modified conjugated diene rubber having a monomer unit represented by the following formula (1a):
[0115] [ka]
[0116] Production Example 1: Production of modified conjugated diene rubber (A-1) A 5L autoclave that was thoroughly dried was purged with nitrogen, and 1260g of hexane and 36.3g of n-butyllithium (17% by mass hexane solution) were charged. The temperature was raised to 50°C, and then 1260g of butadiene was successively added while controlling the polymerization temperature to 50°C under stirring conditions, and polymerization was carried out for 1 hour. Methanol was then added to terminate the polymerization reaction, and a polymer solution was obtained. Water was added to the obtained polymer solution, and the mixture was stirred, and the polymer solution was washed with water. After stopping the stirring, it was confirmed that the polymer solution phase and the water phase were separated, and then the water was separated. The polymer solution after washing was vacuum dried at 70°C for 24 hours to obtain an unmodified liquid polybutadiene (A'-1). Next, 500 g of the obtained unmodified liquid polybutadiene (A'-1) was charged into a 1 L autoclave that had been purged with nitrogen, and 25 g of maleic anhydride and 0.5 g of N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine (product name "Nocrac 6C", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) were added, and the mixture was reacted at 170°C for 24 hours to obtain maleic anhydride modified liquid polybutadiene (A"-1). To 500 g of the resulting maleic anhydride modified liquid polybutadiene (A″-1), 8.1 g of methanol was added and reacted at 80° C. for 6 hours to obtain a monomethyl maleate modified liquid polybutadiene (A-1).
[0117] Production of modified conjugated diene rubber having a monomer unit represented by the following formula (1b):
[0118] [ka]
[0119] Production Example 2: Production of modified conjugated diene rubber (A-2) A 5L autoclave that was thoroughly dried was replaced with nitrogen, and 1200g of hexane and 26.2g of n-butyllithium (17% by mass in hexane solution) were charged. The temperature was raised to 50°C, and then 1200g of isoprene was added successively under stirring conditions while controlling the polymerization temperature to 50°C, and polymerization was carried out for 1 hour. Methanol was then added to terminate the polymerization reaction, and a polymer solution was obtained. Water was added to the obtained polymer solution, and the mixture was stirred, and the polymer solution was washed with water. After stopping the stirring, it was confirmed that the polymer solution phase and the water phase were separated, and then the water was separated. The polymer solution after washing was vacuum dried at 70°C for 24 hours to obtain unmodified liquid polyisoprene (A'-2). Next, 500 g of the unmodified liquid polyisoprene (A'-2) obtained was charged into a 1 L autoclave that had been purged with nitrogen, and 25 g of maleic anhydride and 0.5 g of butylated hydroxytoluene (BHT) were added thereto, and the mixture was reacted at 170°C for 15 hours to obtain a maleic anhydride-modified liquid polyisoprene (A"-2). To 500 g of the resulting maleic anhydride modified liquid polyisoprene (A″-2), 8.1 g of methanol was added and reacted at 80° C. for 6 hours to obtain monomethyl maleate modified liquid polyisoprene (A-2).
[0120] Production of modified conjugated diene rubber having a monomer unit represented by the following formula (1c):
[0121] [ka]
[0122] Production Example 3: Production of modified conjugated diene rubber (A-3) A 5L autoclave that was thoroughly dried was purged with nitrogen, and 1500g of cyclohexane and 18.2g of sec-butyllithium (10.5% by mass solution in cyclohexane) were charged. The temperature was raised to 50°C, and then 1500g of a mixture of 900g of butadiene (a) and 600g of farnesene (b) (butadiene (a) and farnesene (b) were mixed in a cylinder) was added at 10ml / min and polymerized for 1 hour. Methanol was then added to terminate the polymerization reaction, and a polymer solution was obtained. Water was added to the obtained polymer solution and stirred, and the polymer solution was washed with water. After stopping the stirring and confirming that the polymer solution phase and the aqueous phase were separated, the water was separated. The polymer solution after washing was vacuum dried at 70°C for 12 hours to obtain an unmodified liquid polyfarnesene polybutadiene copolymer (A"-3). Next, 500 g of the obtained unmodified liquid polyfarnesene polybutadiene copolymer (A"-3) was charged into a 1 L capacity autoclave that had been purged with nitrogen, and 25 g of maleic anhydride and 0.5 g of N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine (trade name "Nocrac 6C", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) were added and reacted at 170°C for 24 hours to obtain a maleic anhydride-modified liquid polyfarnesene polybutadiene copolymer (A'-3). Further, 5.6 g of methanol was added to 300 g of the obtained maleic anhydride-modified liquid polyfarnesene polybutadiene copolymer (A'-3), and the mixture was reacted at 80°C for 6 hours to obtain a monomethyl maleate-modified liquid polyfarnesene polybutadiene copolymer (A-3).
[0123] Production of modified conjugated diene rubber (A-4) having a hydrogen-bonding functional group at the molecular end represented by the following formula (1d):
[0124] [ka]
[0125] Production Example 4: Production of modified conjugated diene rubber (A-4) A 5L autoclave was thoroughly dried and substituted with nitrogen, and 1200g of cyclohexane, 54g of sec-butyllithium (10.5% by mass solution in cyclohexane), and 2.06g of TMEDA were charged. The temperature was raised to 50°C, and then 1300g of butadiene was added successively at 10ml / min under stirring conditions while controlling the polymerization temperature to 50°C. After the addition of butadiene, the mixture was heated for 1 hour to complete the polymerization. 16.6g of triisopropyl borate was added to the obtained polymerization solution to introduce boronic acid to the polymerization terminal (terminal introduction rate 95%). Ion-exchanged water was added to the obtained polymer solution and stirred to wash the polymer solution. After confirming that the polymer solution phase and the water phase were separated, the polymer solution phase was collected and dried under reduced pressure at 90°C for 12 hours to obtain boronic acid-modified liquid polybutadiene (A-4).
[0126] The methods for measuring and calculating the various properties of the modified conjugated diene rubber and the like are as follows. The results are shown in Table 1. <Methods for measuring weight average molecular weight, number average molecular weight and molecular weight distribution> The Mw, Mn and Mw / Mn of the modified conjugated diene rubber were determined as values converted into standard polystyrene by GPC (gel permeation chromatography) using the following measuring device and conditions: · Apparatus: Tosoh Corporation GPC device "GPC8020" Separation column: Tosoh Corporation's "TSKgelG4000HXL" Detector: Tosoh Corporation "RI-8020" Eluent: Tetrahydrofuran ·Eluent flow rate: 1.0ml / min Sample concentration: 5mg / 10ml Column temperature: 40℃
[0127] <Melt viscosity measurement method> The melt viscosity of the modified conjugated diene rubber at 38° C. was measured using a Brookfield viscometer (manufactured by BROOKFIELD ENGINEERING LABS. INC.).
[0128] <Method of measuring glass transition temperature> 10 mg of the modified conjugated diene rubber was placed in an aluminum pan, and a thermogram was measured by differential scanning calorimetry (DSC) at a heating rate of 10° C. / min. The DDSC peak top value was taken as the glass transition temperature.
[0129] <Average number of hydrogen-bonding functional groups per molecule> The average number of hydrogen-bonding functional groups per molecule of the modified conjugated diene rubber was calculated from the equivalent weight (g / eq) of the hydrogen-bonding functional groups of the modified conjugated diene rubber and the number average molecular weight Mn in terms of styrene by the following formula. Average number of hydrogen-bonding functional groups per molecule = [(number average molecular weight (Mn)) / (molecular weight of styrene unit) x (average molecular weight of conjugated diene and other monomer units other than conjugated diene contained as necessary)] / (equivalent weight of hydrogen-bonding functional group) The method for calculating the equivalent weight of the hydrogen-bonding functional group can be appropriately selected depending on the type of the hydrogen-bonding functional group.
[0130] The average number of hydrogen-bonding functional groups per molecule of the monomethyl maleate-modified conjugated diene rubber and the boronic acid-modified conjugated diene rubber was calculated by determining the acid value of the monomethyl maleate-modified conjugated diene rubber and the boronic acid-modified conjugated diene rubber and calculating the equivalent weight (g / eq) of the hydrogen-bonding functional group from the acid value. After the modification reaction, the sample was washed four times with methanol (5 mL per 1 g of sample) to remove impurities such as antioxidants, and then dried under reduced pressure at 80° C. for 12 hours. 180 mL of toluene and 20 mL of ethanol were added to 3 g of the sample after the modification reaction to dissolve it, and then neutralized with a 0.1 N ethanol solution of potassium hydroxide, and the acid value was calculated using the following formula. Acid value (mgKOH / g)=(AB)×F×5.611 / S A: Amount of 0.1N potassium hydroxide ethanol solution added for neutralization (mL) B: Amount of 0.1N potassium hydroxide ethanol solution dropped into a blank containing no sample (mL) F: Potency of 0.1N potassium hydroxide in ethanol S: mass of weighed sample (g)
[0131] From the acid value, the mass of the hydrogen-bonding functional group contained in 1 g of the monomethyl maleate-modified conjugated diene rubber and the boronic acid-modified conjugated diene rubber was calculated using the following formula, and the mass other than the functional group (polymer main chain mass) contained in 1 g of the monomethyl maleate-modified conjugated diene rubber and the boronic acid-modified conjugated diene rubber was calculated. Then, the equivalent weight (g / eq) of the hydrogen-bonding functional group was calculated using the following formula. [Hydrogen-bonding functional group mass per 1 g] = [acid value] / [56.11] x [hydrogen-bonding functional group molecular weight] / 1000 [Mass of polymer main chain per 1g] = 1 - [Mass of hydrogen-bonding functional group per 1g] [Equivalent weight of hydrogen-bonding functional group] = [mass of polymer main chain per 1 g] / ([mass of hydrogen-bonding functional group per 1 g] / [molecular weight of hydrogen-bonding functional group])
[0132] [Table 1]
[0133] <Preparation of emulsion> Preparation Example 1: Preparation of emulsion (E-1) of modified conjugated diene rubber (A-1) First, modified conjugated diene rubber (A-1) was used as a liquid conjugated diene rubber, and 2-ethylhexanoic acid triglyceride (hereinafter also referred to as "EHTG") (trade name "Excepearl TGO", manufactured by Kao Corporation, vapor pressure at 20°C: 1.7 × 10) was used as an oil. -7 The mixture was mixed in a mass ratio of 1:3 and stirred for 24 hours while heating to 50°C to prepare an oil dilution solution of modified conjugated diene rubber (A-1). Next, 9 g of primary alcohol ethoxylate (trade name "Adekator PC-8", manufactured by ADEKA Corporation, HLB value: 12.4) was added as a surfactant to 150 g of the oil dilution solution and stirred for 5 minutes. Next, 371 g of 0.09 mol / L sodium hydroxide aqueous solution was added little by little while stirring, and the mixture was stirred for 20 minutes to obtain an emulsion (E-1) of modified conjugated diene rubber (A-1).
[0134] Preparation Example 2: Preparation of emulsion (E-2) of modified conjugated diene rubber (A-1) An emulsion (E-2) of the modified conjugated diene rubber (A-1) was prepared in the same manner as in Preparation Example 1, except that the mass ratio of the modified conjugated diene rubber (A-1) to EHTG in the oil dilution solution was 2:3.
[0135] Preparation Example 3: Preparation of emulsion (E-3) of modified conjugated diene rubber (A-1) An emulsion (E-3) of modified conjugated diene rubber (A-1) was prepared in the same manner as in Preparation Example 1, except that a special phenol ethoxylate (product name "Adetol PC-10", manufactured by ADEKA Corporation, HLB value: 13.5) was used instead of Adetol PC-8 as the surfactant.
[0136] Preparation Example 4: Preparation of emulsion (E-4) of modified conjugated diene rubber (A-2) An emulsion (E-4) of modified conjugated diene rubber (A-2) was prepared in the same manner as in Preparation Example 1, except that the modified conjugated diene rubber (A-2) was used as the liquid conjugated diene rubber.
[0137] Preparation Example 5: Preparation of emulsion (E-5) of modified conjugated diene rubber (A-3) An emulsion (E-5) of modified conjugated diene rubber (A-3) was prepared in the same manner as in Preparation Example 1, except that the modified conjugated diene rubber (A-3) was used as the liquid conjugated diene rubber.
[0138] Preparation Example 6: Preparation of emulsion (E-6) of modified conjugated diene rubber (A-4) The liquid conjugated diene rubber was modified conjugated diene rubber (A-4), and the oil was mineral oil (purity 99.9% or more, flash point 158°C, vapor pressure at 20°C: 1.1×10 -6 An emulsion (E-6) of a liquid conjugated diene rubber (A-4) was prepared in the same manner as in Preparation Example 1, except that a secondary alcohol ethoxylate (product name "Adetol SO-80", manufactured by ADEKA Corporation, HLB value: 8.0) was used as a surfactant.
[0139] The emulsions (E-1) to (E-6) obtained in Preparation Examples 1 to 6 are shown in Table 2.
[0140] [Table 2]
[0141] [Example 1] In Example 1, a reinforcing fiber was produced having an adhesive component containing a liquid conjugated diene rubber, an oil having a vapor pressure of 10 Pa or less at 20°C, and a surfactant on at least a portion of the surface of the fiber, and was evaluated as follows. An emulsion (E-1) of modified conjugated diene rubber (A-1) prepared by adding water so that the concentration of the adhesive component was 10% by mass was applied to vinylon fiber that had been subjected to a pretreatment described below using an oiling guide, and the fiber was dried for 1 second with a hot roller at 150° C. and then wound up. The vinylon fiber to which the adhesive component had been attached in this manner was twisted at a twist rate of 80 T / m to produce a fiber cord.
[0142] [Pretreatment of Vinylon Fiber] A polyvinyl alcohol fiber, Vinylon fiber ("Kuraray Co., Ltd." "Kuralon 1239", total fineness 1330 dtex, single yarn fineness 6.65 dtex) was immersed in an aqueous solution prepared to the following composition, and then the liquid was squeezed out with a roller. The obtained fiber was then dried at 130°C for 20 seconds, and further heat-treated at 240°C for 20 seconds and wound up to produce a pretreated Vinylon fiber.
[0143] [Pretreatment agent composition for vinylon fiber] Water: 96.96 parts by mass Meikanote DM-3031 CONC: 22 parts by weight Denacol EX-614B: 7 parts by weight The hydrophilic treatment agent was prepared using a blocked isocyanate and an epoxy resin. As the blocked isocyanate, "Meikanote DM-3031 CONC" manufactured by Meisei Chemical Industry Co., Ltd. was used, and as the epoxy resin, "Denacol EX-614B" manufactured by Nagase ChemteX Corporation was used.
[0144] [Examples 2 to 7] A fiber cord was produced in the same manner as in Example 1, except that the emulsion of the liquid conjugated diene rubber, the concentration of the adhesive component in the emulsion, and the amount of the adhesive component attached to the fiber were changed as shown in Table 3.
[0145] [Example 8] A fiber cord was produced in the same manner as in Example 1, except that PET fibers that had been pretreated as described below were used as the fibers, and an emulsion (E-1) of modified conjugated diene rubber (A-1) was used in which the concentration of the adhesive component was adjusted to 30 mass %.
[0146] [Pretreatment of PET fibers] A polyester-based PET fiber (Toray Industries, Inc., "702C", total fineness 1670 dtex, single yarn fineness 5.80 dtex) was immersed in an aqueous solution prepared to the following composition, and then the liquid was squeezed out with a roller. The resulting fiber was then dried at 130°C for 30 seconds, and further heat-treated at 240°C for 30 seconds and wound up to produce a pretreated PET fiber.
[0147] [Pretreatment agent composition for PET fibers] Water: 96.96 parts by mass Meikanote DM-3031 CONC: 22 parts by weight Denacol EX-614B: 7 parts by weight The hydrophilic treatment agent was prepared using a blocked isocyanate and an epoxy resin. As the blocked isocyanate, "Meikanote DM-3031 CONC" manufactured by Meisei Chemical Industry Co., Ltd. was used, and as the epoxy resin, "Denacol EX-614B" manufactured by Nagase ChemteX Corporation was used.
[0148] [Comparative Example 1] 15 g of polyoxyethylene alkyl (C=12-15) ether phosphate (manufactured by Toho Chemical Industry Co., Ltd., product name "Phosphanol RS-710") was added as a surfactant to 250 g of the modified conjugated diene rubber (A-1), and the mixture was stirred for 20 minutes. Then, 180 g of 0.7 mol / L aqueous sodium hydroxide solution was gradually added while stirring. After adding 2205 mL of water, the mixture was stirred for 20 minutes to obtain an emulsion of Comparative Example 1. A fiber cord was produced in the same manner as in Example 1, except that the obtained emulsion was used.
[0149] [Comparative Example 2] Without mixing the liquid conjugated diene rubber, 9 g of primary alcohol ethoxylate (PC-8) was added to 150 g of EHTG and stirred for 5 minutes. Then, 341 g of 0.05 mol / L aqueous sodium hydroxide solution was added little by little while stirring. Furthermore, 1090 mL of water was added, and the mixture was stirred for 20 minutes to obtain an emulsion of Comparative Example 2. A fiber cord was produced in the same manner as in Example 1, except that the obtained emulsion was used.
[0150] [Comparative Example 3] An attempt was made to prepare an emulsion of modified conjugated diene rubber (A-1) in the same manner as in Preparation Example 1, without adding any surfactant, but the emulsion was not stable enough to be applied to the fibers.
[0151] <Oil vapor pressure at 20℃> The vapor pressure of synthetic oils and mineral oils at 20°C was calculated based on the measured values measured by the gas flow method, after calculating constants A, B, and C of the Antoine equation: log10P=A-(B / (T+C)).
[0152] <Viscosity of emulsion containing adhesive component at 20°C> The viscosity at 20°C of the emulsions obtained in each of the Examples and Comparative Examples was measured using a rotary B-type viscometer (TVB-10, manufactured by Toki Sangyo Co., Ltd.) (rotation speed: 100 rpm) using the emulsions stored overnight in a room controlled at 20°C.
[0153] <Viscosity of adhesive components at 30℃> The viscosity of the adhesive component at 30°C was measured with a rotational B-type viscometer (TVB-10, manufactured by Toki Sangyo Co., Ltd.) (rotation speed 100 rpm) using a mixture of liquid conjugated diene rubber that had been preheated to 30°C using a thermostatic bath, an oil with a vapor pressure of 10 Pa or less at 20°C, and a surfactant in the mass ratio shown in Table 3.
[0154] <Emulsion stability> The prepared emulsion was allowed to stand and visually evaluated according to the following criteria. ·standard G (good): No phase separation observed within 10 minutes, excellent stability B (bad): Phase separation was observed within 10 minutes, and the stability was poor.
[0155] <Measurement of adhesion amount of adhesive component> The amount of the adhesive component attached was measured by the following method. Approximately 10 g of reinforcing fiber was collected as a sample, and its mass X was measured. The adhesive component was extracted from the sample, and the extracted mass Y was measured. Toluene was used as the solvent for extraction, and extraction was performed for 3 hours using a Soxhlet extractor. The adhesion amount of the adhesive component was calculated using the following formula. Amount of adhesive component attached to reinforcing fiber (mass%) = (Y / X) x 100 The content (mass %) of the conjugated diene rubber in the adhesive component was calculated from the mass ratio of the conjugated diene rubber in the solid content of the adhesive component.
[0156] <Rubber adhesive strength measurement> For the fiber cords obtained in Examples 1 to 8 and Comparative Examples 1 and 2, evaluation sheets were prepared by the following method, and the force (N / 25.4 mm) required to T-separate the fiber cord from the rubber was measured and evaluated as the rubber adhesion. The results are shown in Table 3. In the evaluation results of the rubber adhesion, a larger value indicates a stronger adhesion between the reinforcing fiber and the rubber. The adhesive sheet was prepared as follows.
[0157] -Preparation of evaluation sheets The fiber cords produced in the above-mentioned Examples 1 to 5, 7, and 8 and Comparative Examples 1 and 2 were arranged and fixed on a masking tape in a curtain-like shape so that the fiber cords did not overlap each other, and then this was overlapped with an unvulcanized rubber composition (hereinafter also referred to as "EPDM unvulcanized rubber") (width 25.4 mm, length 240 mm) mainly composed of EPDM rubber ("Esprene 501A" manufactured by Sumitomo Chemical Co., Ltd.) prepared according to the following compounding composition using EPDM rubber (the length of the overlapping part of the fiber cord and the EPDM unvulcanized rubber was 190 mm). Next, the fiber cords were subjected to a pressure of 20 kg / cm at 150°C. 2 The mixture was press-vulcanized for 30 minutes under the above conditions to prepare a sheet for evaluation.
[0158] (EPDM unvulcanized rubber compounding composition) EPDM rubber: 100 parts by weight Filler (carbon black): 60 parts by weight Softener (paraffin-based process oil): 20 parts by weight Crosslinking agent (sulfur powder): 1.5 parts by weight Vulcanization aid (zinc oxide type 2, stearic acid): 6 parts by mass Vulcanization accelerator (thiazole type, thiuram type): 1.5 parts by mass
[0159] The fiber cords prepared in Example 6 were arranged and fixed on a masking tape in a curtain-like shape so that the fiber cords did not overlap each other, and then this was overlapped with an unvulcanized rubber composition (hereinafter also referred to as "NR / SBR unvulcanized rubber") (width 25.4 mm, length 240 mm) mainly composed of NR / SBR rubber prepared using NR ("RSS#3") and SBR (manufactured by Nippon Zeon Co., Ltd., "Nipol (registered trademark) 1502") according to the following compounding composition (the length of the overlapped portion of the fiber cord and the NR / SBR unvulcanized rubber was 190 mm). Next, it was subjected to a 150°C, 20 kg / cm pressure test. 2 The mixture was press-vulcanized for 30 minutes under the above conditions to prepare a sheet for evaluation.
[0160] (NR / SBR unvulcanized rubber compounding composition) NR: 50 parts by mass SBR: 50 parts by mass Filler (carbon black): 45 parts by weight Softener (paraffin-based process oil): 5 parts by weight Crosslinking agent (sulfur powder): 2.4 parts by weight Vulcanization aid (zinc oxide type 2, stearic acid): 7 parts by mass Vulcanization accelerator (thiazole type, thiuram type): 2.0 parts by mass
[0161] <Degree of process contamination> In Examples 1 to 8 and Comparative Examples 1 and 2, the emulsion was applied to each fiber as described in each example, and after 5 kg of reinforcing fiber was wound up, the degree of contamination (gum-up) of the holding roller through which the reinforcing fiber had passed was evaluated according to the following criteria. ·standard G (good): There is no roller contamination due to gum-up, or contamination is minimal, and there is no problem with silk reeling operability. P (poor): Roller contamination due to gum-up occurs, and spinning operability is poor. B (bad): Roller contamination due to gum-up is significant, single yarns are taken off during spinning, and there is a problem with spinning operability.
[0162] <Abrasion resistance (twisted abrasion)> After collecting the reinforcing fibers, they were stored at room temperature (20°C) for one month, and then their abrasion resistance was evaluated using the following method. The reinforcing fibers were twisted in the Z direction at 80t / m to create a loop, and then twisted in the S direction three times at the center of the loop. While applying a load of 3kg, the fibers were abraded against each other up and down at room temperature, and the number of times when they broke was recorded and judged according to the following evaluation criteria. G (good): Withstands abrasion more than 500 times and has excellent processability during processing. P (poor): The yarn breaks after 100 or more but less than 500 cycles of wear, and the processability during processing is poor. B (bad): The yarn breaks after less than 100 wears, and there is a problem with processability during processing.
[0163] [Table 3]
[0164] The reinforcing fiber of the present invention has excellent adhesion to rubber and abrasion resistance. Furthermore, according to the present invention, the reinforcing fiber can be efficiently produced while suppressing contamination of the production facility.
Claims
1. A reinforcing fiber having an adhesive component on at least a portion of a surface of the fiber, the adhesive component containing a liquid conjugated diene rubber, an oil having a vapor pressure of 10 Pa or less at 20° C., and a surfactant, The adhesive component does not contain resorcinol-formaldehyde resin, The liquid conjugated diene rubber contains, in its molecule, monomer units derived from one or more selected from butadiene, isoprene, and farnesene, A reinforcing fiber, characterized in that the rubber adhesive strength of the reinforcing fiber is 20 N / 25.4 mm or more and 61.1 N / 25.4 mm or less.
2. The reinforcing fiber according to claim 1 , wherein the fiber is at least one type selected from the group consisting of polyvinyl alcohol-based fibers, regenerated cellulose-based fibers, polyester-based fibers, and polyamide-based fibers.
3. 3. The reinforcing fiber according to claim 1, wherein the liquid conjugated diene rubber is a modified conjugated diene rubber having a hydrogen-bonding functional group in a portion of the conjugated diene rubber.
4. The reinforcing fiber according to claim 3, wherein the hydrogen-bonding functional group is at least one selected from a hydroxy group, an epoxy group, an aldehyde group, an acetalized product of an aldehyde group, a carboxy group, a salt of a carboxy group, an esterified product of a carboxy group, an acid anhydride of a carboxy group, a boronyl group, a salt of a boronyl group, an esterified product of a boronyl group, a silanol group, and an esterified product of a silanol group.
5. The reinforcing fiber according to any one of claims 1 to 4, wherein the surfactant is a nonionic surfactant.
6. The reinforcing fiber according to claim 5, wherein the HLB value of the nonionic surfactant is 6 to 17.
7. The reinforcing fiber according to any one of claims 1 to 6, wherein a content ratio of the surfactant to a total amount of the liquid conjugated diene rubber and the oil [surfactant / (liquid conjugated diene rubber+oil)] is 1 / 100 to 50 / 100 in mass ratio.
8. A reinforcing fiber described in any one of claims 1 to 7, characterized in that the rubber adhesion strength of the reinforcing fiber is 30 N / 25.4 mm or more and 61.1 N / 25.4 mm or less.
9. The method for producing the reinforcing fiber according to any one of claims 1 to 8, comprising the steps of mixing the liquid conjugated diene rubber, the oil and the surfactant to form an oil-in-water emulsion and attaching the emulsion to a fiber.
10. A woven or knitted fabric comprising at least a portion of the reinforcing fiber according to any one of claims 1 to 8.
11. A molded article using the reinforcing fiber according to any one of claims 1 to 8.
12. The molded article according to claim 11, further comprising a rubber component.
13. The molded article according to claim 11 or 12, which is a tire, a belt or a hose.
Citation Information
Patent Citations
Bonding of fibers for reinforcing rubbers
JP1979004976A
Production of liquid polyisoprene emulsion
JP1979093034A
Preparation of liquid polyisoprene emulsion
JP1979124040A
Adhesive between rubber and fiber
JP1983002370A
Treating agent for thermoplastic synthetic fiber
JP1984053779A