Dot-shaped hot melt ink printing on nonwoven fabrics using inkjet technology addresses printing accuracy and speed issues, ensuring excellent cosmetic properties and absorption performance in absorbent articles.
Patent Information
- Application Number
- JP2021152839
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-09-21
- Publication Date
- 2024-09-20
- Estimated Expiration
- 2037-05-31
AI Technical Summary
Existing methods for printing on nonwoven fabrics used in absorbent articles face challenges with printing accuracy due to surface irregularities, affecting aesthetics and operability, and aqueous inks are limited by drying processes, impacting speed and efficiency.
A method involving dot-shaped hot melt ink printing on the top sheet with specific dot configurations and inkjet technology is employed, allowing for high-speed printing with minimal surface interference and maintaining absorption performance.
The method achieves aesthetically pleasing, high-speed printing on nonwoven fabrics without impairing absorption performance, offering improved cosmetic properties and operational efficiency.
Smart Images

Figure 0007554725000006 
Figure 0007554725000005 
Figure 0007554725000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing absorbent articles such as printed light incontinence pads, pants-type disposable diapers, and tape-fastened disposable diapers. [Background technology]
[0002] Currently, absorbent articles such as disposable paper diapers for infants and adults are widely used. These absorbent articles are configured to include a liquid-permeable top sheet, a liquid-impermeable back sheet, and an absorbent body disposed between the top sheet and the back sheet. The liquid-permeable top sheet is mainly composed of a nonwoven fabric, and the liquid-impermeable back sheet is composed of a plastic film such as polyethylene.
[0003] In addition, absorbent articles are printed with patterns, letters, etc. for various purposes, and printing methods such as single-color printing or multi-color printing are appropriately selected depending on the printing area, purpose, etc. For example, absorbent articles for infants may have multi-colored patterns of animals or other characters printed on the back sheet. Also, absorbent articles for adults may have specifications such as the size, front and back, and absorption capacity of the absorbent article printed in a single color.
[0004] The printing method is appropriately selected depending on the surface properties of the material to be printed, but the printing accuracy may be limited depending on the printing method. For example, when the material to be printed is a plastic film or paper, flexographic printing or gravure printing can be used, and a certain degree of printing accuracy can be obtained. Here, flexographic printing and gravure printing are methods in which the printing plate roll and the material to be printed come into contact with each other to print.
[0005] In this regard, various nonwoven fabrics, which are commonly used for top sheets, three-dimensional gather sheets, individual packaging sheets, etc., do not have a smooth surface compared to plastic films, papers, etc. Therefore, when printing is performed on these using the above-mentioned contact printing method, there are problems such as poor printing accuracy and impaired aesthetics and visibility due to the presence of large and small irregularities on the surface. On the other hand, consumers' demands for aesthetics of printed parts have been increasing in recent years. Therefore, when printing on various nonwoven fabrics, etc., measures such as limiting the printing speed and enlarging the size of patterns and letters are required.
[0006] Patent Document 1 discloses a method for manufacturing absorbent articles in which a pattern visible from the outside is applied to a backsheet, with the aim of producing attractive-looking absorbent articles with high operational efficiency. The method includes an inkjet printer that uses oil-based ink and a cooling means that sprays a cooling spray liquid at a predetermined temperature or lower, and the ink is ejected from the outer surface side of the backsheet to form a pattern on the backsheet, and then the area where the pattern is formed is cooled by the cooling means.
[0007] Patent Document 2 discloses an aqueous composition containing an aqueous polyurethane, water and a colorant for the purpose of improving color transfer resistance properties with respect to aqueous printing inks for nonwoven fabric articles. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2011-206330 A [Patent Document 2] Special Publication No. 2010-509460 Summary of the Invention [Problem to be solved by the invention]
[0009] However, the manufacturing method of absorbent articles disclosed in Patent Document 1 assumes that a pattern is applied by inkjet printing to a back sheet having a relatively smooth surface as a printing substrate. Therefore, when a pattern is applied to a nonwoven fabric having an uneven surface as a printing substrate and being hydrophilic, problems arise in terms of efficiently manufacturing an absorbent article with good appearance.
[0010] Furthermore, when the aqueous composition disclosed in Patent Document 2 is printed, for example, on a top sheet by inkjet printing, since it is aqueous, the printing speed is limited by the time required for the drying process, which causes problems in operability.
[0011] Therefore, an object of the present invention is to provide a method for producing an absorbent article in which a nonwoven fabric used for a top sheet or the like is printed with printing that is decorative and does not impair the absorbent performance. [Means for solving the problem]
[0012] In view of the above problems, the inventors of the present invention have conducted intensive research and have found that the above problems can be solved by a method for manufacturing an absorbent article comprising a step of printing hot-melt ink dots on a surface of a top sheet that faces the body or a surface that faces clothing to form a pattern, lettering, or the like, and by forming the hot-melt ink dots printed on the top sheet in a predetermined configuration, thereby completing the present invention.
[0013] (1) A first aspect of the present invention is a method for producing an absorbent article having a liquid-permeable top sheet, a liquid-impermeable back sheet, and an absorbent body disposed between the top sheet and the back sheet, the method comprising the steps of printing dots of hot-melt ink on a surface of the top sheet that faces the body or a surface that faces clothing to form patterns, letters, and the like, and the average area of each dot of the hot-melt ink printed on the top sheet is 1000 μm 2 More than 2000μm 2the dot spacing between the dots of the hot melt ink printed on the top sheet is 50 μm or more and 300 μm or less, and the area ratio of the dots of the hot melt ink to the area of the top sheet where the hot melt ink is printed is 12% or less. (2) In the method for manufacturing an absorbent article described in (1), the hot melt ink is printed by inkjet printing, the printing line speed in the inkjet printing is 100 m / min or more, and the inkjet printing may be in-line printing incorporated into the manufacturing line of the absorbent article. (3) In the method for producing an absorbent article according to (1) or (2), the hot melt ink may have a melt viscosity of 0.1 Pa.s or less at 120°C. (4) In the method for producing an absorbent article according to any one of (1) to (3), the absorbent article further comprises a liquid-diffusing sheet disposed between the top sheet and the absorbent body, and a step of printing dots of hot-melt ink on a surface of the liquid-diffusing sheet that is to be a body side surface or a clothing side surface to form a pattern, letters, etc., the pattern, letters, etc. are visible through the top sheet, and the average area of the dots of the hot-melt ink on the liquid-diffusing sheet is 1000 μm or less. 2 More than 2000μm 2 the dot spacing of the hot melt ink on the liquid diffusion sheet is 50 μm or more and 300 μm or less, and the area ratio of the hot melt ink to the area where the hot melt ink is printed on the liquid diffusion sheet may be 12% or less. (5) In the method for manufacturing an absorbent article according to any one of (1) to (4), the top sheet is a thermal bonded nonwoven fabric or a spun bonded nonwoven fabric, and the basis weight of the top sheet is 15 g / m 2 More than 50g / m 2 It may be the following. Effect of the Invention
[0014] The method for producing an absorbent article of the present invention includes a step of printing dots of hot melt ink on the surface of a top sheet that faces the body or the surface that faces clothing to form patterns, letters, etc., and the average area of each dot of hot melt ink printed on the top sheet is 1000 μm 2 More than 2000μm 2 the dot spacing between the hot melt ink dots printed on the top sheet is 50 μm or more and 300 μm or less, and the area ratio of the hot melt ink dots to the area printed with the hot melt ink on the top sheet is 12% or less. This makes it possible to provide a method for manufacturing an absorbent article in which printing is applied to a nonwoven fabric used for a top sheet or the like that is excellent in aesthetic appearance and does not impair absorption performance. [Brief description of the drawings]
[0015] [Figure 1] 1A and 1B are plan views of an absorbent article as viewed from the body side surface in a manufacturing method for the absorbent article of the present invention, and FIG. 1C is a plan view of a packaging sheet for packaging the absorbent article of the present invention. [Diagram 2] 1(a) is a microscopic image of the area indicated by the dotted ellipse in FIG. 1(c), and (b) is a microscopic image of the darkest printed area in the comparative example. [Diagram 3] 2(a) is an image showing the dot spacing in the feed direction in the image in FIG. 2(a), and (b) is an image showing the dot spacing in the feed direction in the image in FIG. 2(b). [Figure 4] FIG. 2 is a graph showing the results of measuring the absorption rate of each of the nonwoven fabrics of the Examples, Comparative Examples, and Reference Examples. [Diagram 5] FIG. 2 is a graph showing the results of measuring the amount of wet-back for each of the nonwoven fabrics in the Examples, Comparative Examples, and Reference Examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Hereinafter, a method for manufacturing an absorbent article 1 according to an embodiment of the present invention will be described in detail, but these are presented for illustrative purposes and are not intended to limit the present invention. Note that the same elements are designated by the same numbers throughout the description of the embodiment.
[0017] <Absorbent articles> In the manufacturing method of the absorbent article 1 according to the embodiment of the present invention, the absorbent article 1 may be an absorbent article 1 such as a light incontinence pad, a light incontinence liner, a sanitary napkin, a pants-type paper diaper, or a tape-fastened paper diaper. The absorbent article 1 includes a liquid-permeable top sheet 10 arranged on the body-facing surface, a liquid-impermeable or liquid-permeable back sheet arranged on the clothing-facing surface facing the top sheet 10, and an absorbent body 11 arranged between the top sheet 10 and the back sheet, whereby the absorbent body 11 is sandwiched between the top sheet 10 and the back sheet. The top sheet 10, the back sheet, and the absorbent body 11 may be joined to each other by adhesives, heat fusion, or the like.
[0018] In the description of this specification, the longitudinal direction is the direction extending from the front to the back of the wearer when the absorbent article 1 is worn. The width direction is the direction horizontal to or perpendicular to the longitudinal direction. In addition, in this specification, the body-side surface refers to the surface that contacts the wearer's skin when the absorbent article 1 is worn or the surface that contacts the wearer's skin when the absorbent article 1 is worn, and the clothing-side surface refers to the surface opposite to the body-side surface, which contacts the wearer's clothing when the absorbent article 1 is worn or the surface that contacts the wearer's clothing when the absorbent article 1 is worn.
[0019] [Top sheet] In the manufacturing method of the absorbent article 1 according to the embodiment of the present invention, the top sheet 10 used in the absorbent article 1 allows bodily fluids to pass quickly toward the absorbent body 11, and is disposed opposite the back sheet with the absorbent body 11 sandwiched therebetween. Since the top sheet 10 is a sheet that comes into contact with the skin, it is preferable that the top sheet 10 is a hydrophilic nonwoven fabric that has a soft feel and does not irritate the skin. As the hydrophilic nonwoven fabric, a thermal bonded nonwoven fabric such as an air-through nonwoven fabric, a spunlace nonwoven fabric, a spunbonded nonwoven fabric, an open film such as an open polyethylene film, a foamed film such as a urethane foam, etc., using synthetic fibers such as polypropylene or polyethylene, regenerated fibers such as rayon, or natural fibers such as cotton, can be used. From the viewpoint of breathability and feel on the skin when worn, it is preferable to use a thermal bonded nonwoven fabric such as a hydrophilic air-through nonwoven fabric or a spunbonded nonwoven fabric.
[0020] The basis weight of the top sheet 10 is set to 15 g / m from the viewpoints of processability and strength. 2 More than 50g / m 2 It is preferable that the above conditions are satisfied. Furthermore, lotions, antioxidants, anti-inflammatory components, pH adjusters, antibacterial agents, moisturizers, and the like may be applied to the top sheet 10 in order to reduce irritation to the skin.
[0021] [Back seat] In the manufacturing method of the absorbent article 1 according to the embodiment of the present invention, the back sheet used in the absorbent article 1 is a liquid-impermeable sheet material, and is disposed opposite the top sheet 10 with the absorbent body 11 sandwiched therebetween. The back sheet can be a sheet material using a thin plastic sheet such as a polyethylene sheet or a polyethylene-laminated nonwoven fabric. The back sheet may be moisture-permeable to prevent stuffiness.
[0022] The basis weight of the back sheet is set to 15 g / m2 from the viewpoints of workability and strength. 2 More than 60g / m 2 It is preferable that:
[0023] [Absorbent] In the manufacturing method of the absorbent article 1 according to the embodiment of the present invention, the absorbent body 11 used in the absorbent article 1 contains absorbent fibers as a base material and a super absorbent polymer (hereinafter also referred to as SAP). The absorbent fibers are not particularly limited as long as they are generally used in the absorbent article 1 such as sanitary napkins, diapers, and urine pads, and examples thereof include fluff pulp, cotton, rayon, acetate, tissue, absorbent paper, and hydrophilic nonwoven fabric. Among these, fluff pulp is preferably used from the viewpoint of absorbency. Examples of fluff pulp include wood pulp (for example, coniferous bleached kraft pulp (N-BKP) such as southern pine and Douglas fir), synthetic fiber, polymer fiber, non-wood pulp, and the like that are defibrated into a cotton-like state. The absorbent fibers of the absorbent body 11 have a density of 400 g / m so as not to impair the absorption performance and the feel on the skin. 2 More than 800g / m 2 The following basis weight is preferred.
[0024] The SAP used in the absorbent body 11 is not particularly limited as long as it can absorb body fluids and prevent backflow, and can be made from materials such as sodium polyacrylate, polyaspartate, (starch-acrylic acid) graft copolymer, (acrylic acid-vinyl alcohol) copolymer, (isobutylene-maleic anhydride) copolymer, and saponified products thereof. Among these, sodium polyacrylate copolymers are preferred from the viewpoint of absorption capacity per mass. The amount of SAP in the absorbent body 11 is 50 g / m2 or less so as not to impair absorption performance and texture. 2 More than 700g / m 2 The content is preferably 15% by mass or more and 60% by mass or less.
[0025] In the absorbent body 11, the absorbent fibers and SAP are preferably in the form of a laminated mat formed by mixing SAP particles in the absorbent fibers. In addition, for the purpose of preventing leakage of the SAP particles and stabilizing the shape of the absorbent body 11, it is preferable to wrap the absorbent body 11 in a carrier sheet. The base material of the carrier sheet may be any material that has hydrophilicity, and examples of the base material include hydrophilic nonwoven fabrics such as tissue, absorbent paper, and air-laid nonwoven fabrics. When a plurality of carrier sheets are provided, the base materials of the carrier sheets may be the same or different, and the method of wrapping the absorbent body 11 in the carrier sheet is not particularly limited.
[0026] The basis weight of the absorbent body 11 is 400 g / m 2 More than 1500g / m 2 or less. By setting the basis weight of the absorbent body 11 in this range, it is possible to achieve excellent absorbency and effectively prevent leakage of bodily fluids. The absorbent body 11 may also be formed by laminating an upper-layer absorbent body and a lower-layer absorbent body. In this case, the longitudinal and width dimensions of the upper-layer absorbent body and the lower-layer absorbent body may be such that the upper-layer absorbent body is larger than the lower-layer absorbent body, the upper-layer absorbent body may be the same as the lower-layer absorbent body, or the upper-layer absorbent body may be smaller than the lower-layer absorbent body.
[0027] The absorbent body 11 may be a single layer or multiple layers, and may be provided with slit portions that are free of absorbent fibers and superabsorbent polymers.
[0028] [Liquid diffusion sheet] In the manufacturing method of the absorbent article 1 according to the embodiment of the present invention, a liquid-diffusing sheet may be provided between the top sheet 10 and the absorbent body 11 in the absorbent article 1 in order to promote diffusion of body fluids to the upper surface of the absorbent body 11. Examples of the liquid-diffusing sheet include nonwoven fabrics such as air-through nonwoven fabrics, point-bonded nonwoven fabrics, spunbonded nonwoven fabrics, and meltblown nonwoven fabrics, as well as composite nonwoven fabrics obtained by laminating spunbond / meltblown or spunbond / meltblown / spunbond.
[0029] The basis weight of the liquid diffusion sheet is 15 g / m 2 The shape of the liquid-diffusing sheet is not particularly limited, but it is preferable that the liquid-diffusing sheet has a shape that can completely cover the surface of the absorbent body 11 so that body fluids such as urine are diffused throughout the absorbent body 11.
[0030] [3D gathers] In the manufacturing method of the absorbent article 1 according to the embodiment of the present invention, the body-facing surface of the absorbent article 1 may be provided with a pair of three-dimensional gathers 12 having a three-dimensional gather elastic member and a three-dimensional gather sheet along the longitudinal direction of the absorbent article 1 in order to prevent side leakage of bodily fluids excreted by the user. The three-dimensional gathers 12 are fixed to the back sheet at the widthwise end (fixed end) of the absorbent article 1, and the free end side is preferably folded in half at the end. The three-dimensional gather elastic member is preferably sandwiched between the three-dimensional gather sheet at the free end side folded in half. This allows the three-dimensional gathers 12 to have uprightness and to be deformable to fit the body shape of the wearer.
[0031] As the elastic member for the three-dimensional gathers, for example, polyurethane thread, belt-shaped polyurethane film, synthetic rubber, thread-shaped or belt-shaped natural rubber, etc. can be used, and thread-shaped, string-shaped, or flat-shaped ones can be used as appropriate. As the three-dimensional gather sheet, water-repellent or liquid-impermeable nonwoven fabric formed of hydrophobic fibers, for example, spunbond nonwoven fabric, meltblown nonwoven fabric, or composite nonwoven fabric of spunbond / meltblown / spunbond laminated, etc. is used. The thickness of the elastic member for the three-dimensional gathers is preferably 1240 dtex or less.
[0032] The basis weight of the three-dimensional gathered sheet is 10g / m 2 More than 40g / m 2 It is preferable that:
[0033] [Packaging sheet] In the manufacturing method of the absorbent article 1 according to the embodiment of the present invention, the absorbent article 1 may include a packaging sheet 13 that packages the absorbent article 1. As the packaging sheet 13, for example, paper, a resin film such as polyethylene, polypropylene, polyester, or polyvinyl alcohol, a spunbond nonwoven fabric, a meltblown nonwoven fabric, a composite nonwoven fabric in which spunbond / meltblown / spunbond are laminated, or a composite material of these can be used. In addition, the inside of the packaging sheet 13 that contacts the absorbent article 1 can be subjected to a release treatment using silicone or the like.
[0034] The basis weight of the packaging sheet 13 is not particularly limited, but from the viewpoints of strength and processability, it is preferably 15 g / m 2 More than 30g / m 2 It is preferable that the thickness is less than 20 g / m 2 More than 25g / m 2 It is preferable that:
[0035] [Hot melt ink printing] In the manufacturing method of the absorbent article 1 according to the embodiment of the present invention, it is preferable to include a step of printing dot-shaped hot melt ink on the surface of the top sheet 10 that will be the body side surface or the clothing side surface to form patterns, letters, etc., and a step of forming patterns, letters, etc. on the surface of the top sheet 10 that will be the body side surface. The hot melt ink may be printed to form patterns, letters, etc., and may be patterns, letters, etc. formed in non-printed areas by printing hot melt ink, so-called outline patterns, outline letters, etc., and may be numbers, symbols, figures, etc., which are usually printed on the absorbent article 1. In addition, a brand, product name, etc. may be printed, and a design or design may be printed for the purpose of improving the cosmetic appearance. In addition, specifications of the absorbent article 1, such as an approximate absorption amount, may be printed to prevent misidentification when different products are used for each user of the absorbent article 1 in nursing care facilities, hospital facilities, etc.
[0036] The average area of each dot of hot melt ink printed on the top sheet 10 is 1000 μm 2 More than 2000μm 2Less than or equal to 1100 μm 2 More than 1700μm 2 It is preferable that the dot interval between the dots of the hot melt ink printed on the top sheet 10 is 50 μm or more and 300 μm or less, and preferably 80 μm or more and 270 μm or less. It is preferable that the dot interval between the dots of the hot melt ink printed on the top sheet 10 is the dot interval in the feed direction. In addition, the area ratio of the dots of the hot melt ink in the region where the hot melt ink is printed on the top sheet 10 is 12% or less, and preferably 9% or less. In addition, the average dot interval between the dots of the hot melt ink printed on the top sheet 10 is preferably 90 μm or more and 280 μm or less, and more preferably 100 μm or more and 270 μm or less.
[0037] By printing dots of hot melt ink as described above, it is possible to provide an absorbent article 1 having a multicolored, highly variable, and fine print of fine dots on the surface of the top sheet 10, resulting in an absorbent article 1 with excellent aesthetic appeal. In addition, because the fine dots of hot melt ink are attached along the three-dimensional structure of the top sheet 10, the hot melt ink does not block the surface of the top sheet 10, and the effect on the absorption performance of the absorbent article 1 can be reduced, resulting in an absorbent article 1 with printing that does not inhibit the absorption performance of the absorbent article 1.
[0038] In the manufacturing method of the absorbent article 1 according to the embodiment of the present invention, the hot melt ink is preferably printed by inkjet printing. This allows the print design to be easily changed by changing the electronic data, making it unnecessary to change the plate. In addition, the printed patterns, letters, etc. may be printed in the same pattern at equal intervals in the feed direction in the manufacturing process of the absorbent article 1, and various electronic data such as patterns and letters can be appropriately selected depending on the purpose. In addition, unlike contact printing methods such as flexographic printing, this is a non-contact printing method, so printing can be performed without being affected by the surface properties such as the basis weight of the printing target.
[0039] Furthermore, the printing line speed in inkjet printing is 100 m / min or more, preferably 200 m / min or more, and may be 280 m / min or less.
[0040] In addition, the inkjet printing is preferably in-line printing incorporated into the manufacturing line of the absorbent article 1. This allows high-speed production of the absorbent article 1. For example, the nonwoven fabric sheet to be the top sheet 10 is conveyed to an inkjet printing device, and the inkjet head is serially scanned in a direction perpendicular to the feed direction (machine direction or MD direction) (cross machine direction or CD direction) based on the print image data transferred from a host computer, and the hot melt ink is heated to a predetermined temperature, and patterns, characters, etc. are printed with the hot melt ink on the surface of the nonwoven fabric sheet to be the top sheet 10 that is the body side surface that contacts the wearer's skin or the clothing side surface. The inkjet printing device may be installed on the line in which the absorbent article 1 having the top sheet 10, the back sheet, and the absorbent body 11 arranged between the top sheet 10 and the back sheet is manufactured. Although the hot melt ink can be cooled at room temperature, a cooling process may be provided in which the absorbent article 1 after inkjet printing is cooled by a cooling roll, a blower, or the like.
[0041] The method for ejecting hot melt ink is not particularly limited, and a thermal method, a piezoelectric method, or the like can be used.
[0042] The hot melt ink preferably has a melt viscosity of 0.1 Pa.s or less, and more preferably has a melt viscosity of 0.06 Pa.s or less at 120° C. This allows for the absorbent article 1 to be printed with excellent aesthetic appeal and without impairing the absorbency.
[0043] The hot melt ink is not particularly limited as long as it satisfies the above-mentioned melt viscosity, and examples of the thermoplastic resin that can be used include polyolefins such as polyethylene, mixtures thereof, polyamides, polyesters, polyesteramides, polyvinyl alcohols, cellulose esters, polyvinylpyridines, polyethers, polyethylenes, ethylene-vinyl acetate copolymers, copolyesters, olefin-based block copolymer rubbers, polystyrene-acrylic copolymers, terpene resins, rosin fluids, phenolic resins, and coumarone-indene resins. Examples of these hot melt inks include MDL5800 (manufacturer: EDM Co., Ltd.). The mass ratio of the binder in the hot melt ink is preferably 20% or more and 50% or less, and more preferably 30% or more and 40% or less.
[0044] These hot melt inks may contain additives such as waxes and oils to improve flow properties. For example, polyalkylene waxes (polyethylene wax, polypropylene wax, etc.), Fischer-Tropsch wax, linear primary alcohols, microcrystalline waxes, fatty acids, carnauba wax, candelilla wax, stearic acid amide, paraffin wax, montan wax, ethoxylated long-chain alcohols, etc. may be used. These waxes may be used alone or in combination. The mass ratio of the additives in the hot melt ink is preferably 40% or more and 70% or less, more preferably 50% or more and 60% or less.
[0045] These hot melt inks may contain inorganic pigments, organic pigments or dyes, and are not particularly limited as long as they are those that are commonly used in hot melt inks. For example, the inorganic pigments that can be used include titanium dioxide (white), carbon black (black), iron oxide (red, yellow, brown), chromium oxide (green), and ferric ammonium ferrocyanide (blue). For example, the organic pigments that can be used include diarylide yellow (pigment yellow), phthalocyanine blue (pigment blue), and red lake (pigment red). The mass ratio of the pigment or dye in the hot melt ink is preferably 0.1% or more and 20% or less, and more preferably 0.5% or more and 10% or less.
[0046] In addition to the binder, additives, and pigment or dye, these hot melt inks may also contain plasticizers, extenders, thickeners, defoamers, wetting agents or surfactants, antioxidants, and the like.
[0047] When these hot melt inks are used in inkjet printing, it is preferable to have a step in which the temperature of the hot melt ink is set to 60°C or higher and 150°C or lower, and more preferably 70°C or higher and 120°C or lower.
[0048] It is also preferable to have a step of printing dots of hot melt ink on the surface of the liquid-diffusing sheet that will be the body side surface or the clothing side surface to form a pattern, letters, etc., and it is more preferable to have a step of printing dots of hot melt ink on the surface of the liquid-diffusing sheet that will be the body side surface to form a pattern, letters, etc. It is preferable that the pattern, letters, etc. printed on the surface of the liquid-diffusing sheet are visible through the top sheet 10. The dots of the hot melt ink printed on the liquid-diffusing sheet are preferably the same as the dots of the hot melt ink printed on the above-mentioned top sheet 10, and it is preferable to use the printing method, etc., that is used for the above-mentioned top sheet 10. For example, the average area of the hot melt ink dots on the liquid-diffusing sheet is 1000 μm2 More than 2000μm 2 It is preferable that the dot spacing of the hot melt ink on the liquid diffusion sheet is 50 μm or more and 300 μm or less, and the area ratio of the hot melt ink in the region where the hot melt ink is printed on the liquid diffusion sheet is 12% or less.
[0049] It is also preferable to have a step of printing hot melt ink dots on one side or the other side of the three-dimensional gathers 12 to form patterns, letters, etc. In the case of the three-dimensional gathers 12 in which the free end side of the three-dimensional gather sheet is folded in half at the end and has an inner surface that is folded back to form the inner surface and an outer surface that is folded back to form the outer surface, a step of printing hot melt ink dots on the inner surface or the outer surface of the three-dimensional gathers 12 to form patterns, letters, etc. may be included. The hot melt ink dots printed on the three-dimensional gathers 12 are preferably the same as the hot melt ink dots printed on the above-mentioned top sheet 10, and the printing method, etc. used in the above-mentioned top sheet 10 is also preferably used. For example, the average area of the hot melt ink dots on the three-dimensional gathers 12 is 1000 μm 2 More than 2000μm 2 It is preferable that the dot spacing of the hot melt ink in the three-dimensional gathers 12 is 50 μm or more and 300 μm or less, and the area ratio of the hot melt ink in the area where the hot melt ink is printed on the three-dimensional gathers 12 is 12% or less.
[0050] It is also preferable to have a process of printing hot melt ink dots on one side or the other side of the packaging sheet 13 to form patterns, characters, etc. The hot melt ink dots printed on the packaging sheet 13 are preferably the same as the hot melt ink dots printed on the above-mentioned top sheet 10, and the printing method, etc. used for the above-mentioned top sheet 10 is also preferably used. For example, the average area of the hot melt ink dots on the packaging sheet 13 is 1000 μm 2 More than 2000μm 2 It is preferable that the dot spacing of the hot melt ink on the packaging sheet 13 is 50 μm or more and 300 μm or less, and the area ratio of the hot melt ink to the area printed with the hot melt ink on the packaging sheet 13 is 12% or less.
[0051] [Method of manufacturing absorbent articles] The manufacturing method of the absorbent article 1 is not particularly limited except for the manufacturing method described above, and a conventionally known method can be adopted. For example, as in the manufacturing method of the absorbent article 1 according to the embodiment of the present invention, the absorbent article can be manufactured by providing a step of printing a hot melt ink on the surface of the top sheet 10 that will be the body side surface or the clothing side surface, and further providing a step of placing a liquid diffusive sheet and three-dimensional gathers 12 on the top sheet 10, sandwiching an absorbent body 11 between the top sheet 10 and the back sheet, and fixing the top sheet 10 and the back sheet partially or entirely around the periphery using a hot melt adhesive, heat embossing, ultrasonic embossing, high frequency embossing, or the like. Also, for example, the absorbent article can be manufactured by first arranging the liquid-diffusing sheet and the three-dimensional gathers 12 on the top sheet 10, sandwiching the absorbent body 11 between the top sheet 10 and the back sheet, and fixing the top sheet 10 and the back sheet partially or entirely using a hot melt adhesive, heat embossing, ultrasonic embossing, high frequency embossing, or the like, and then applying a hot melt ink to the top sheet 10 as in the manufacturing method of the absorbent article 1 according to an embodiment of the present invention.
[0052] Although the present invention has been described above using the embodiments, it goes without saying that the technical scope of the present invention is not limited to the scope of the invention described in the above embodiments, and it is clear to those skilled in the art that various modifications and improvements can be made to the above embodiments. Furthermore, it is clear from the description of the claims that forms including such modifications or improvements can also be included in the technical scope of the present invention. EXAMPLES
[0053] The present invention will be described in more detail with reference to the following examples. However, the present invention is not limited to the description of the following examples as long as it does not depart from the gist of the present invention.
[0054] [Example 1] In Example 1, a hot melt ink was printed by inkjet printing on an air-through nonwoven fabric that can be used for a top sheet, a liquid-diffusing sheet, a packaging sheet, etc. of an absorbent article. The basis weight of the air-through nonwoven fabric was 20 g / m 2 The fineness was 2.0 dtex. The inkjet printer head used was a commercially available product, and the printing line speed of the inkjet printing was 200 m / min. The hot melt ink used contained 40% by mass of binder, 55% by mass of wax, and 5% by mass of pigment.
[0055] With the nonwoven fabric of Example 1, it was possible to print beautiful designs, characters, and the like on the nonwoven fabric using hot melt ink, as shown in FIGS. 1(a) to (c).
[0056] In addition, in FIG. 1(c), the darkest printed area (area surrounded by a dotted ellipse in FIG. 1(c)) was measured at a magnification of 120x using a 3D shape measuring microscope One Shot VR-3000 (product name, manufacturer: Keyence Corporation). The measurement area was W: 2521.81 μm, H: 1890.74 μm. An image of the measurement area is shown in FIG. 2(a). In FIG. 2, the direction extending from left to right on the image is the feed direction (machine direction or MD), and the direction extending from top to bottom is the direction perpendicular to the feed direction (cross machine direction or CD).
[0057] From Figure 2(a), the average area of each dot of hot melt ink is 1400 μm 2 The area ratio of the hot melt ink dots to the area printed with the hot melt ink was 7%. Figure 3(a) shows the dot spacing of each dot of the hot melt ink in Figure 2(a). Figure 3(a) shows that the dot spacing of each dot of the hot melt ink in the feed direction was 70 μm or more and 290 μm or less, and the average dot spacing was 200 μm.
[0058] <Absorption speed> The time it took for the nonwoven fabric of Example 1 to absorb water was measured. The measurement method was as follows. The nonwoven fabric of Example 1 was used as a sample of 100 mm length and 200 mm width including the area printed most darkly. Ten sheets of impregnation filter paper (product name: Advantech #26-WA, 200 mm x 200 mm) were placed in a tray, and the nonwoven fabric sample of Example 1 was placed on top of the filter paper. A cylindrical weight (load 46 g / cm) with a circular water injection hole and an inner diameter of 30 mm was then placed on top of the filter paper. 2 ) was used to inject 10 mL of water, and the time it took for the nonwoven fabric sample to absorb it was measured (first injection). 10 mL of water was injected at 3 minute intervals from the first injection until the third injection, and the time it took for the nonwoven fabric sample to absorb it was measured. Figure 4 shows the measurement results of the absorption rate of the nonwoven fabric of Example 1. Note that the absorption rate of the nonwoven fabric of Example 1, which was not printed with hot melt ink, was also measured in the same manner as above, and is shown in the figure as a reference example.
[0059] <Wet back amount> The amount of wet-back, which is the amount of liquid returning, was measured for the nonwoven fabric of Example 1. The measurement method is as follows. The nonwoven fabric of Example 1 was used as a sample of 100 mm length and 200 mm width including the area printed most darkly. The mass (W A ) was measured. Five sheets of impregnating filter paper (product name: Advantech #26-WA, 200 mm x 200 mm) were placed in a tray. 200 mL of physiological saline was measured using a measuring cylinder, poured onto the impregnating filter paper, and left to stand for about 1 minute. The edges of each impregnating filter paper were held vertically and drained for 1 minute. The nonwoven fabric sample of Example 1 was placed on top of the five sheets of impregnating filter paper after draining, the measurement filter paper whose mass had been measured was placed on the nonwoven fabric sample, and two cylindrical weights (diameter 55 mm, mass 688 g) were placed on top of each other on the measurement filter paper, and the weights were left to stand for 30 seconds. After 30 seconds, the weights, measurement filter paper, and nonwoven fabric sample were removed, and the mass (W B ) was measured. B -W A The value calculated from the above was taken as the wet-back amount. Fig. 5 shows the measurement results of the wet-back amount of the nonwoven fabric of Example 1. Note that, for the nonwoven fabric of Example 1, the wet-back amount was also measured in the same manner as described above for a nonwoven fabric not printed with hot melt ink, and is shown as a reference example.
[0060] <Running costs> The nonwoven fabric of Example 1 was evaluated for productivity and switchability when the patterns, characters, etc. printed on the nonwoven fabric were switched multiple times and operated for one week in the same manner as in a normal manufacturing line for absorbent articles 1. The evaluation results of the running costs of the nonwoven fabric of Example 1 are shown in Table 1.
[0061] [Table 1]
[0062] <Print clarity> The nonwoven fabric of Example 1 was subjected to a sensory evaluation by 20 monitors for the clarity of printed patterns, characters, etc. The results of the sensory evaluation of the clarity of the print on the nonwoven fabric of Example 1 are shown in Table 1. ◎: When 16 to 20 people "see clearly" or "see clearly" 〇: When 11 to 15 people answered "clearly" or "distinctly" △: When 6 to 10 people answered "clearly" or "distinctly" ×: When there are no people who can see clearly or clearly, or when there are 1 to 5 people who can see clearly
[0063] <Texture> For the nonwoven fabric of Example 1, a sensory evaluation was carried out by 20 monitors on the softness and feel of the printed areas of the printed patterns, characters, etc. The results of the sensory evaluation of the feel of the nonwoven fabric of Example 1 are shown in Table 1. ◎: When 16 to 20 people answered "soft" or "comfortable to the touch" 〇: When 11 to 15 people answered "soft" or "comfortable" △: When 6 to 10 people answered "soft" or "comfortable" ×: No one said "soft" or "comfortable" or 1 to 5 people said "soft"
[0064] [Comparative Example 1] In Comparative Example 1, an aqueous ink was printed by flexographic printing on an air-through nonwoven fabric that can be used for a top sheet, a liquid-diffusing sheet, a packaging sheet, etc. of an absorbent article. The basis weight of the air-through nonwoven fabric was 20 g / m 2 The yarn thickness was 2.0 dtex. The printing line speed of the flexographic printing was 200 m / min. The water-based ink used was one that is typically used for nonwoven fabrics and is composed of polyurethane resin, water, colorants, etc.
[0065] The area printed most darkly was measured at a magnification of 120x using a 3D shape measuring microscope One Shot VR-3000 (product name, manufactured by Keyence Corporation). The measured area was W: 2521.81μm, H: 1890.74μm. An image of the measured area is shown in Figure 2(b). Figure 2(b) shows that the average area of each dot of the water-based ink is 5500μm. 2 The area ratio of the water-based ink dots to the area printed with the water-based ink was 20%. Figure 3(b) shows the dot spacing of each dot of the water-based ink in Figure 2(b). Figure 3(b) shows that the dot spacing of each dot in the feed direction of the water-based ink was 100 μm or more and 250 μm or less, and the average dot spacing was 190 μm.
[0066] The nonwoven fabric of Comparative Example 1 was also evaluated in the same manner as in Example 1 with respect to absorption speed, wet-back amount, running cost, print clarity, and texture, and the results are shown in Table 1, FIG.
[0067] As described above, according to the nonwoven fabric of Example 1, the printing was clear without being affected by the surface properties of the nonwoven fabric, there was no load on the nonwoven fabric due to printing, and the texture of the nonwoven fabric was also good, so the sensory evaluation of the clarity of the printing and the sensory evaluation of the texture were "good". In addition, since the hot melt ink was printed in a predetermined dot shape, the absorption speed and the wet back amount were good compared to the nonwoven fabric of the reference example that was not printed. Therefore, according to the nonwoven fabric of Example 1, it is possible to provide an absorbent article with excellent cosmetic properties and printed without impairing the absorption performance. In terms of running costs, it is possible to provide an absorbent article with excellent running costs because high-speed printing is possible, the printed image can be easily switched depending on the printed image data, and the switching ability is good, and a large-scale drying process is not required.
[0068] Therefore, by inkjet printing with the hot melt ink in Example 1, it was possible to print beautiful designs, characters, etc. on the nonwoven fabric, as shown in FIG.
[0069] In the nonwoven fabric of Comparative Example 1, the printing line speed during production was the same as in Example 1, but it was contact-type flexographic printing, not noncontact-type inkjet printing. Therefore, unevenness due to the basis weight of the nonwoven fabric caused problems with the clarity of the print, resulting in low printing accuracy and a sensory evaluation of the clarity of the print being "x". In addition, the problem of the texture of the nonwoven fabric being reduced by the pressure applied during ink adhesion and ink application also occurred, so the sensory evaluation of the texture was also "x". In addition, the amount of wetback was worse than that of the nonwoven fabric of the reference example that was not printed due to the influence of ink adhesion and ink pressure. Therefore, compared with the nonwoven fabric of Example 1, the nonwoven fabric was inferior in aesthetics and had impaired absorption performance. In addition, since water-based ink was used, a drying process using heat and wind was required, and since it was flexographic printing, the work time for switching the printed image was longer than in Example 1, so the running cost was also inferior. [Explanation of symbols]
[0070] 1. Absorbent articles 10 Top sheet 11 Absorbent 12 Three-dimensional gathers 13 Packaging Sheet
Claims
1. A method for manufacturing an absorbent article having a liquid-permeable top sheet, a liquid-impermeable back sheet, and an absorbent body disposed between the top sheet and the back sheet, comprising: The top sheet is a hydrophilic air-through nonwoven fabric, a step of printing dots of hot melt ink by inkjet printing on a surface of the top sheet that will be the body side surface or the clothing side surface to form patterns, letters, etc.; The average area of each dot of the hot melt ink printed on the top sheet is 1000 μm 2 2000 μm or more 2 is as follows: an area ratio of the hot melt ink dots to the area of the top sheet where the hot melt ink is printed is 7% or more and 12% or less; the mass ratio of the binder in the hot melt ink is 30% or more and 40% or less, the mass ratio of the additive containing the wax or oil is 50% or more and 60% or less, and the mass ratio of the pigment or dye is 0.5% or more and 10% or less, The printing line speed in the inkjet printing is 100 m / min or more, The absorbent article has a pair of three-dimensional gathers on the body-facing surface along the longitudinal direction of the absorbent article, A step of printing dots of hot melt ink on one surface or the other surface of the three-dimensional gathers to form a pattern, letters, etc., the average area of the dots of the hot melt ink in the three-dimensional gathers is 1000 μm 2 or more and 2000 μm 2 or less; A method for manufacturing an absorbent article, characterized in that the area ratio of the hot melt ink to the area of the three-dimensional gathers where the hot melt ink is printed is 7% or more and 12% or less.
2. The method for manufacturing an absorbent article according to claim 1 , wherein the inkjet printing is in-line printing incorporated into a manufacturing line for the absorbent article.
3. The method for manufacturing an absorbent article according to claim 1 or 2, wherein the hot melt ink has a melt viscosity of 0.1 Pa.s or less at 120°C.
4. The absorbent article further comprises a liquid-diffusing sheet disposed between the top sheet and the absorbent body, a step of printing dots of hot melt ink on a surface of the liquid-diffusing sheet that will be the body side surface or the clothing side surface to form a pattern, letters, or the like, The pattern, lettering, etc. are visible through the top sheet, The average area of each dot of the hot melt ink on the liquid diffusion sheet is 1000 μm 2 2000 μm or more 2 is as follows:
4. The method for manufacturing an absorbent article according to claim 1, wherein an area ratio of the hot melt ink dots in the region where the hot melt ink is printed on the liquid diffusion sheet is 7% or more and 12% or less.
5. The top sheet is a thermal bonded nonwoven fabric or a spun bonded nonwoven fabric, The basis weight of the top sheet is 15 g / m 2 50g / m or more 2 A method for producing an absorbent article according to any one of claims 1 to 4, characterized in that:
Citation Information
Patent Citations
Absorptive article with front-rear expression
JP2002360620A
Disposable paper diaper having color design
JP2003070838A
Absorptive article
JP2006136582A
Absorbent products with enhanced rewetting, uptake and soil masking performance
JP2006512159A
Water-based printing ink for nonwoven fabric substrates
JP2010509460A