Novel compound, raw material for thin film formation containing said compound, and method for producing thin film

A β-diketiminate ligand with a fluorine-containing group addresses the vapor pressure issue in conventional complexes, allowing for the formation of high-quality metal-containing thin films through enhanced ALD methods.

JP7554763B2Active Publication Date: 2024-09-20ADEKA CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021553422
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-11-01
Filing Date
2020-10-19
Publication Date
2024-09-20
Estimated Expiration
2040-10-19

AI Technical Summary

Technical Problem

Conventional β-diketiminate metal complexes used in forming metal-containing thin films have insufficient vapor pressure, limiting their ability to form high-quality films, and existing compounds with fluorine-containing groups lack specific structural descriptions.

Method used

A compound with a β-diketiminate ligand containing a fluorine atom at a specific position, represented by formula (1), is developed to enhance vapor pressure and melting point, suitable for use in chemical vapor deposition methods like ALD.

Benefits of technology

The compound achieves high vapor pressure and low melting point, enabling the formation of high-quality metal-containing thin films with improved properties and processability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554763000014
    Figure 0007554763000014
  • Figure 0007554763000016
    Figure 0007554763000016
  • Figure 0007554763000017
    Figure 0007554763000017
Patent Text Reader

Abstract

This thin film-forming material contains a compound represented by formula (1). (In formula (1), R1-R5 are each independently a hydrogen atom, an alkyl group having 1-5 carbon atoms, or a group including a fluorine atom, M represents a metal atom, and n represents the valence of the metal atom represented by M. However, at least one of R2, R3, and R4 represents a group including a fluorine atom.)
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a novel compound, a thin film-forming raw material containing said compound, a method of using said compound as a precursor, a thin film produced by using said method, and a method of producing a thin film. [Background technology]

[0002] In the field of electronic devices such as semiconductors, photovoltaic cells, and display materials, compounds having β-diketiminate ligands are known as raw materials for conductive thin films. Methods for producing thin films include sputtering, ion plating, metal organic decomposition (MOD) methods such as coating pyrolysis and sol-gel methods, and chemical vapor deposition (CVD) methods. Among these, atomic layer deposition (ALD), a type of chemical vapor deposition method, is the optimal manufacturing process for thin films because it has many advantages such as excellent composition controllability, excellent step coverage, suitability for mass production, and the ability to perform hybrid integration.

[0003] For example, Patent Documents 1 to 3 propose a method of forming a metal-containing thin film by the ALD method using a compound having a β-diketiminate ligand. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 5181292 [Patent Document 2] Patent No. 5003978 [Patent Document 3] Special Publication No. 2009-503247 Summary of the Invention [Problem to be solved by the invention]

[0005] When forming a metal-containing thin film on a substrate surface by CVD, a thin film forming raw material is required that has a high vapor pressure, a low melting point, and can form a high-quality metal-containing thin film. In particular, a thin film forming raw material with a high vapor pressure is required to improve the productivity of thin films. Conventional β-diketiminate metal complexes still have insufficient vapor pressure, so further improvement is required. Patent Document 3 describes a compound having a β-diketiminate ligand with one or more fluorine-containing organic groups, but does not describe its specific structure. [Means for solving the problem]

[0006] As a result of extensive investigations, the present inventors have found that a compound having a β-diketiminate ligand having a group containing a fluorine atom at a specific position can solve the above-mentioned problems, and have thus completed the present invention.

[0007] The present invention relates to a compound represented by the following formula (1).

[0008] [ka]

[0009] In formula (1), R 1 ~R 5 each independently represents a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a group containing a fluorine atom, M represents a metal atom, and n represents the valence of the metal atom represented by M. 2 , R 3 and R 4 At least one of represents a group containing a fluorine atom.

[0010] R in formula (1) 1 ~R 5 The fluorine atom-containing group represented by the following formula (I) is preferably an alkyl group having 1 to 5 carbon atoms substituted with a fluorine atom.

[0011] R in formula (1) 1 and R 5is an alkyl group having 1 to 5 carbon atoms, and R 2 and R 4 At least one of R is an alkyl group having 1 to 5 carbon atoms substituted with a fluorine atom, 3 is preferably a hydrogen atom.

[0012] In formula (1), M is preferably a metal atom selected from copper, nickel, cobalt, tin, manganese and zinc.

[0013] The present invention is a thin film-forming material containing the above compound.

[0014] The present invention is a method for using the above compounds as precursors for producing metal-containing thin films by chemical vapor deposition.

[0015] The present invention is a thin film produced using the above method.

[0016] The present invention is a method for producing a thin film, which comprises introducing a raw material gas obtained by vaporizing the above-mentioned thin film-forming raw material into a processing atmosphere in which a substrate is placed, and decomposing and / or chemically reacting the above-mentioned compounds in the raw material gas to form a metal-containing thin film on the surface of the substrate. Effect of the Invention

[0017] According to the present invention, a compound (β-diketiminate metal complex) having a high vapor pressure and a low melting point can be provided. A thin film forming material containing the compound can be used to form a high-quality metal-containing thin film by a CVD method, particularly an ALD method. [Brief description of the drawings]

[0018] [Figure 1] FIG. 1 is a schematic diagram showing an example of an ALD apparatus used in a thin film manufacturing method according to the present invention. [Diagram 2] FIG. 1 is a schematic diagram showing another example of an ALD apparatus used in the thin film production method according to the present invention. [Diagram 3]FIG. 1 is a schematic diagram showing yet another example of an ALD apparatus used in the thin film manufacturing method according to the present invention. [Figure 4] FIG. 1 is a schematic diagram showing yet another example of an ALD apparatus used in the thin film manufacturing method according to the present invention. [Diagram 5] The molecular structure of compound No. 1 based on single crystal X-ray analysis is shown below. [Figure 6] The molecular structure of compound No. 19 based on single crystal X-ray analysis is shown below. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The compound of the present invention is represented by the following formula (1): The compound of the present invention is suitable as a precursor in a thin film manufacturing method having a vaporization step, such as the ALD method, which is a type of CVD method.

[0020] [ka]

[0021] (In formula (1), R 1 ~R 5 each independently represents a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a group containing a fluorine atom, M represents a metal atom, and n represents the valence of the metal atom represented by M. 2 , R 3 and R 4 At least one of represents a group containing a fluorine atom.

[0022] In the above formula (1), R 1 ~R 5Examples of the alkyl group having 1 to 5 carbon atoms represented by the formula (1) include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, a sec-butyl group, a tert-butyl group, an isobutyl group, a pentyl group, an isopentyl group, a tert-pentyl group, etc. From the viewpoint of obtaining a compound with a high vapor pressure, an alkyl group having 1 to 4 carbon atoms is preferable, a methyl group, an ethyl group, an isopropyl group, or a sec-butyl group is more preferable, and a methyl group or an ethyl group is even more preferable.

[0023] In the above formula (1), R 1 ~R 5 The fluorine atom-containing group represented by the formula (I) may be any group containing a fluorine atom, and may be a fluorine atom. Among these, from the viewpoint of making the effects of the present invention more pronounced, an alkyl group having 1 to 5 carbon atoms substituted with a fluorine atom is preferred, a fluoroalkyl group such as fluoromethyl, difluoromethyl, trifluoromethyl, fluoroethyl, difluoroethyl, trifluoroethyl, fluoropropyl, difluoropropyl, or trifluoropropyl is more preferred, and trifluoromethyl is even more preferred.

[0024] In the above formula (1), the metal atom represented by M may be barium, titanium, zirconium, hafnium, vanadium, niobium, tantalum, chromium, molybdenum, tungsten, manganese, iron, osmium, ruthenium, cobalt, tin, rhodium, iridium, nickel, palladium, platinum, copper, silver, gold, zinc, aluminum, gallium, indium, germanium, lead, antimony, bismuth, radium, scandium, ruthenium, yttrium, lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, lutetium, etc. Among these, from the viewpoint of making the effects of the present invention more pronounced, M is preferably a metal atom selected from copper, nickel, cobalt, tin, manganese, and zinc.

[0025] In the above formula (1), R 1 and R 5 is an alkyl group having 1 to 5 carbon atoms, and R 2 and R 4 At least one of R is an alkyl group having 1 to 5 carbon atoms substituted with a fluorine atom, and R 3 However, compounds containing hydrogen atoms are preferred because they have a low melting point, are highly volatile, react with reactive gases at low temperatures, and can form metal-containing thin films with good productivity. 1 and R 5 is a methyl group or an ethyl group, R 2 is a trifluoromethyl group, and R 3 is a hydrogen atom and R 4 Compounds in which M is a methyl group are more preferable because these effects are more pronounced. Among these compounds, compounds in which M is cobalt are particularly preferable because they are liquid at room temperature.

[0026] Specific examples of preferred compounds of the present invention include the following compounds No. 1 to No. 48, but the present invention is not limited to these compounds. In the following compounds No. 1 to No. 48, "Me" represents a methyl group, "Et" represents an ethyl group, "iPr" represents an isopropyl group, "tBu" represents a tert-butyl group, "sBu" represents a sec-butyl group, and "CF3" represents a trifluoromethyl group.

[0027] [ka]

[0028] [ka]

[0029] [ka]

[0030] The method for producing the compound represented by the above formula (1) is not particularly limited, and the compound is produced by applying a known method. For example, a compound in which M is copper can be obtained by dissolving copper methoxide in ethanol, adding diketimine to react, removing the solvent, and purifying by distillation. Also, a compound in which M is cobalt can be obtained by dissolving cobalt bistrimethylsilylamide in toluene, adding diketimine to react, removing the solvent, and purifying by distillation.

[0031] In a film-forming apparatus for producing a thin film using the compound of the present invention, in order to ensure transportability in the piping of the film-forming apparatus, the melting point of the compound of the present invention is preferably less than 100°C, and it is more preferably liquid at room temperature.

[0032] Next, the thin film forming material of the present invention will be described. The thin film forming raw material of the present invention may contain a compound represented by the above formula (1) and serve as a precursor of a thin film, and the composition varies depending on the type of the target thin film. For example, when a thin film containing only a single metal is produced, the thin film forming raw material of the present invention does not contain metal compounds and metalloid compounds other than the metal. On the other hand, when a thin film containing multiple metals and / or metalloids is produced, the thin film forming raw material of the present invention can contain, in addition to the compound represented by the above formula (1), a compound containing the desired metal and / or a compound containing a metalloid (hereinafter referred to as "other precursors").

[0033] In the case of a multi-component CVD method using a plurality of precursors, other precursors that can be used together with the compound represented by the above formula (1) are not particularly limited, and any well-known precursors that are used as thin film forming materials for the CVD method can be used.

[0034] Examples of the other precursor include compounds of silicon or a metal with one or more compounds selected from the group consisting of compounds used as organic ligands, such as alcohol compounds, glycol compounds, β-diketone compounds, cyclopentadiene compounds, and organic amine compounds. Examples of the metal species of the precursor include lithium, sodium, potassium, magnesium, calcium, strontium, barium, titanium, zirconium, hafnium, vanadium, niobium, tantalum, chromium, molybdenum, tungsten, manganese, iron, osmium, ruthenium, cobalt, rhodium, iridium, nickel, palladium, platinum, copper, silver, gold, zinc, aluminum, gallium, indium, germanium, lead, antimony, bismuth, radium, scandium, ruthenium, yttrium, lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, and lutetium.

[0035] Examples of the alcohol compounds that can be used as organic ligands for the other precursors include alkyl alcohols such as methanol, ethanol, propanol, isopropyl alcohol, butanol, sec-butyl alcohol, isobutyl alcohol, tert-butyl alcohol, pentyl alcohol, isopentyl alcohol, and tert-pentyl alcohol; 2-methoxyethanol, 2-ethoxyethanol, 2-butoxyethanol, 2-(2-methoxyethoxy)ethanol, 2-methoxy-1-methylethanol, 2-methoxy-1,1-dimethylethanol, 2-ethoxy-1,1-dimethylethanol, and 2-isopropoxy-1,1-dimethylethanol. ether alcohols such as 2-butoxy-1,1-dimethylethanol, 2-(2-methoxyethoxy)-1,1-dimethylethanol, 2-propoxy-1,1-diethylethanol, 2-sec-butoxy-1,1-diethylethanol, and 3-methoxy-1,1-dimethylpropanol; and dialkylamino alcohols such as dimethylaminoethanol, ethylmethylaminoethanol, diethylaminoethanol, dimethylamino-2-pentanol, ethylmethylamino-2-pentanol, dimethylamino-2-methyl-2-pentanol, ethylmethylamino-2-methyl-2-pentanol, and diethylamino-2-methyl-2-pentanol.

[0036] Examples of glycol compounds used as organic ligands for the other precursors include 1,2-ethanediol, 1,2-propanediol, 1,3-propanediol, 2,4-hexanediol, 2,2-dimethyl-1,3-propanediol, 2,2-diethyl-1,3-propanediol, 1,3-butanediol, 2,4-butanediol, 2,2-diethyl-1,3-butanediol, 2-ethyl-2-butyl-1,3-propanediol, 2,4-pentanediol, 2-methyl-1,3-propanediol, 2-methyl-2,4-pentanediol, 2,4-hexanediol, and 2,4-dimethyl-2,4-pentanediol.

[0037] Examples of the β-diketone compound used as the organic ligand of the other precursors include acetylacetone, hexane-2,4-dione, 5-methylhexane-2,4-dione, heptane-2,4-dione, 2-methylheptane-3,5-dione, 5-methylheptane-2,4-dione, 6-methylheptane-2,4-dione, 2,2-dimethylheptane-3,5-dione, 2,6-dimethylheptane-3,5-dione, 2,2,6-trimethylheptane-3,5-dione, 2,2,6,6-tetramethylheptane-3,5-dione, octane-2,4-dione, 2,2,6-trimethyloctane-3,5-dione, 2,6-dimethyloctane-3,5-dione, 2,9-dimethylnonane-4,6-dione, 2-methyl- Examples of the alkyl-substituted β-diketones include 6-ethyldecane-3,5-dione and 2,2-dimethyl-6-ethyldecane-3,5-dione; fluorine-substituted alkyl β-diketones include 1,1,1-trifluoropentane-2,4-dione, 1,1,1-trifluoro-5,5-dimethylhexane-2,4-dione, 1,1,1,5,5,5-hexafluoropentane-2,4-dione and 1,3-diperfluorohexylpropane-1,3-dione; and ether-substituted β-diketones include 1,1,5,5-tetramethyl-1-methoxyhexane-2,4-dione, 2,2,6,6-tetramethyl-1-methoxyheptane-3,5-dione and 2,2,6,6-tetramethyl-1-(2-methoxyethoxy)heptane-3,5-dione.

[0038] Examples of the cyclopentadiene compound used as the organic ligand of the other precursors include cyclopentadiene, methylcyclopentadiene, ethylcyclopentadiene, propylcyclopentadiene, isopropylcyclopentadiene, butylcyclopentadiene, sec-butylcyclopentadiene, isobutylcyclopentadiene, tert-butylcyclopentadiene, dimethylcyclopentadiene, and tetramethylcyclopentadiene.

[0039] Examples of the organic amine compound used as the organic ligand of the other precursors include methylamine, ethylamine, propylamine, isopropylamine, butylamine, sec-butylamine, tert-butylamine, isobutylamine, dimethylamine, diethylamine, dipropylamine, diisopropylamine, ethylmethylamine, propylmethylamine, and isopropylmethylamine.

[0040] The above other precursors are known in the art, and their manufacturing methods are also known. For example, when an alcohol compound is used as an organic ligand, the precursor can be manufactured by reacting the inorganic salt of the metal or its hydrate described above with an alkali metal alkoxide of the alcohol compound. Here, examples of the inorganic salt of the metal or its hydrate include metal halides and nitrates. Examples of the alkali metal alkoxide include sodium alkoxide, lithium alkoxide, potassium alkoxide, etc.

[0041] In the multi-component CVD method as described above, there are a method in which each component of the thin film forming raw material is vaporized and supplied independently (hereinafter referred to as the "single source method"), and a method in which a mixed raw material in which multi-component raw materials are mixed in advance in a desired composition is vaporized and supplied (hereinafter referred to as the "cocktail source method"). In the single source method, the other precursor is preferably a compound whose thermal and / or oxidative decomposition behavior is similar to that of the compound represented by the above formula (1). In the cocktail source method, the other precursor is preferably one whose thermal and / or oxidative decomposition behavior is similar to that of the compound represented by the above formula (1) and which does not undergo deterioration due to chemical reaction or the like when mixed with the compound represented by the above formula (1).

[0042] In the case of a cocktail source method in a multi-component CVD method, a mixture of the compound represented by the above formula (1) and other precursors, or a mixed solution obtained by dissolving the mixture in an organic solvent, can be used as a thin film forming raw material.

[0043] The organic solvent is not particularly limited, and any well-known organic solvent can be used. Examples of the organic solvent include acetates such as ethyl acetate, butyl acetate, and methoxyethyl acetate; ethers such as tetrahydrofuran, tetrahydropyran, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, dibutyl ether, and dioxane; ketones such as methyl butyl ketone, methyl isobutyl ketone, ethyl butyl ketone, dipropyl ketone, diisobutyl ketone, methyl pentyl ketone, cyclohexanone, and methylcyclohexanone; hydrocarbons such as hexane, cyclohexane, methylcyclohexane, dimethylcyclohexane, ethylcyclohexane, heptane, octane, toluene, and xylene; hydrocarbons having a cyano group such as 1-cyanopropane, 1-cyanonobutane, 1-cyanohexane, cyanocyclohexane, cyanobenzene, 1,3-dicyanopropane, 1,4-dicyanobutane, 1,6-dicyanohexane, 1,4-dicyanocyclohexane, and 1,4-dicyanobenzene; pyridine, lutidine, and the like. These organic solvents may be used alone or in combination of two or more depending on the solubility of the solute, the relationship between the use temperature and the boiling point, the flash point, and the like.

[0044] When the thin film forming raw material of the present invention is a mixed solution with the above-mentioned organic solvent, the total amount of precursors in the thin film forming raw material is preferably 0.01 mol / L to 2.0 mol / L, and more preferably 0.05 mol / L to 1.0 mol / L.

[0045] Here, the total amount of precursors refers to the amount of the compound represented by the above formula (1) when the thin film forming raw material of the present invention does not contain any metal compounds and metalloid compounds other than the compound represented by the above formula (1), and refers to the total amount of the compound represented by the above formula (1) and other precursors when the thin film forming raw material of the present invention contains, in addition to the compound represented by the above formula (1), compounds containing other metals and / or compounds containing metalloids (other precursors).

[0046] In addition, the thin film forming material of the present invention may contain a nucleophilic reagent, if necessary, to improve the stability of the compound represented by the above formula (1) and other precursors. Examples of the nucleophilic reagent include ethylene glycol ethers such as glyme, diglyme, triglyme, and tetraglyme, crown ethers such as 18-crown-6, dicyclohexyl-18-crown-6, 24-crown-8, dicyclohexyl-24-crown-8, and dibenzo-24-crown-8, ethylenediamine, N,N'-tetramethylethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, 1,1,4,7,7-pentamethyldiethylenetriamine, 1,1,4,7,10,10-hexamethyltriethylenetetramine, Examples of the nucleophilic reagent include polyamines such as triethoxytriethyleneamine, cyclic polyamines such as cyclam and cyclen, heterocyclic compounds such as pyridine, pyrrolidine, piperidine, morpholine, N-methylpyrrolidine, N-methylpiperidine, N-methylmorpholine, tetrahydrofuran, tetrahydropyran, 1,4-dioxane, oxazole, thiazole, and oxathiolane, β-ketoesters such as methyl acetoacetate, ethyl acetoacetate, and 2-methoxyethyl acetoacetate, and β-diketones such as acetylacetone, 2,4-hexanedione, 2,4-heptanedione, 3,5-heptanedione, and dipivaloylmethane. The amount of these nucleophilic reagents used is preferably in the range of 0.1 mol to 10 mol, more preferably in the range of 1 mol to 4 mol, relative to 1 mol of the total amount of the precursor.

[0047] It is desirable that the thin film forming raw material of the present invention contains as little impurity metal elements, impurity halogens such as impurity chlorine, and impurity organic matter as possible other than the components constituting the thin film. The impurity metal elements are preferably 100 ppb or less per element, more preferably 10 ppb or less, and the total amount is preferably 1 ppm or less, more preferably 100 ppb or less. In particular, when used as a gate insulating film, gate film, or barrier layer of an LSI, it is necessary to reduce the content of alkali metal elements and alkaline earth metal elements that affect the electrical properties of the resulting thin film. The impurity halogens are preferably 100 ppm or less, more preferably 10 ppm or less, and even more preferably 1 ppm or less. The impurity organic matter is preferably 500 ppm or less in total, more preferably 50 ppm or less, and even more preferably 10 ppm or less. In addition, moisture is a cause of particle generation in the thin film forming raw material and particle generation during thin film formation, so it is better to remove as much moisture as possible from the precursor, organic solvent, and nucleophilic reagent before use in order to reduce the moisture of each. The moisture content of each of the precursor, the organic solvent and the nucleophilic reagent is preferably 10 ppm or less, more preferably 1 ppm or less.

[0048] In addition, in order to reduce or prevent particle contamination of the thin film to be formed, it is preferable that the thin film forming material of the present invention contains as few particles as possible. Specifically, in particle measurement in the liquid phase using a light scattering type liquid-borne particle detector, the number of particles larger than 0.3 μm is preferably 100 or less per 1 ml of liquid phase, and the number of particles larger than 0.2 μm is more preferably 100 or less per 1 ml of liquid phase.

[0049] Next, the method for producing a thin film of the present invention using the above-mentioned thin film-forming raw material will be described.

[0050] A well-known ALD apparatus can be used in the thin film manufacturing method of the present invention. Specific examples of ALD apparatus include an apparatus capable of supplying a precursor by bubbling as shown in Figs. 1 and 3, and an apparatus having a vaporization chamber as shown in Figs. 2 and 4. In addition, an apparatus capable of performing plasma treatment on a reactive gas as shown in Figs. 3 and 4 can be used. Note that the present invention is not limited to single-wafer apparatuses equipped with a film-forming chamber (hereinafter referred to as a "deposition reaction section") as shown in Figs. 1 to 4, but an apparatus capable of simultaneously processing multiple wafers using a batch furnace can also be used. These can also be used as CVD apparatuses.

[0051] The method for producing a thin film of the present invention includes a step of introducing a source gas obtained by vaporizing the above-mentioned thin film-forming source material into a deposition reaction zone (treatment atmosphere) (source gas introduction step), a step of depositing a metal compound in the source gas on the surface of a substrate to form a precursor thin film (precursor thin film formation step), and a step of introducing a reactive gas into the deposition reaction zone (treatment atmosphere) and reacting the precursor thin film with the reactive gas to form a metal-containing thin film on the surface of the substrate (metal-containing thin film formation step). The method for producing a thin film of the present invention preferably further includes a step of exhausting gas from the deposition reaction zone (treatment atmosphere) between the precursor thin film formation step and the metal-containing thin film formation step and / or after the metal-containing thin film formation step (exhaust step).

[0052] In one embodiment of the method for producing a thin film of the present invention, a precursor thin film forming step, an evacuation step, a metal-containing thin film forming step, and an evacuation step are sequentially performed to form a series of operations, which constitute one cycle of deposition, and the thickness of the thin film of the present invention can be adjusted by repeating this cycle. Each step of the method for producing a thin film of the present invention will be described below.

[0053] (Raw material gas introduction process) The source gas introduction step refers to a step of vaporizing the above-mentioned thin film forming source material into vapor (hereinafter referred to as "source gas") and introducing the source gas into a film formation chamber in which a substrate is placed. As a method for transporting and supplying the thin film raw material, as shown in FIG. 1 and FIG. 3, there is a gas transport method in which the thin film raw material of the present invention is heated and / or depressurized in a container (hereinafter referred to as "raw material container") in which the thin film raw material is stored to be vaporized into a vapor, and the vapor is introduced into a deposition reaction section in which a substrate is placed together with a carrier gas such as argon, nitrogen, or helium as necessary, as shown in FIG. 2 and FIG. 4, and there is a liquid transport method in which the thin film raw material is transported in a liquid or solution state to a vaporization chamber, heated and / or depressurized in the vaporization chamber to be vaporized into a vapor, and the vapor is introduced into a deposition reaction section as a raw material gas. In the case of the gas transport method, the compound represented by the above formula (1) itself can be used as the thin film raw material. In the case of the liquid transport method, the compound represented by the above formula (1) or a solution in which the compound is dissolved in an organic solvent can be used as the thin film raw material. This mixture or mixed solution may further contain a nucleophilic reagent or the like.

[0054] In addition to the above gas transport method and liquid transport method, the method used in the raw material gas introduction step includes the single source method and cocktail source method described in the thin film forming raw material column as a multi-component ALD method containing a plurality of precursors, but whichever introduction method is used, the thin film forming raw material of the present invention is preferably vaporized at 0° C. to 200° C. In addition, when the thin film forming raw material is vaporized in the raw material container or vaporization chamber to form vapor, the pressure in the raw material container and the vaporization chamber are preferably within the range of 1 Pa to 10,000 Pa.

[0055] Here, examples of the material of the substrate placed in the deposition reaction section include silicon; ceramics such as silicon nitride, titanium nitride, tantalum nitride, titanium oxide, ruthenium oxide, zirconium oxide, hafnium oxide, and lanthanum oxide; glass; and metals such as metallic cobalt and metallic ruthenium. Examples of the shape of the substrate include plate-like, spherical, fibrous, and scale-like. The substrate surface may be flat or may have a three-dimensional structure such as a trench structure.

[0056] (Precursor thin film formation process) In the precursor thin film forming step, the compound represented by the above formula (1) in the raw material gas introduced into the deposition reaction section in which the substrate is placed is deposited on the substrate surface to form a precursor thin film on the substrate surface. At this time, the substrate may be heated or the deposition reaction section may be heated to apply heat. The manufacturing conditions for forming the precursor thin film are not particularly limited, and for example, the reaction temperature (substrate temperature), reaction pressure, deposition rate, etc. can be appropriately determined depending on the type of thin film forming raw material. The reaction temperature is preferably 100°C or higher, which is a temperature at which the thin film forming raw material of the present invention reacts sufficiently, and more preferably 100°C to 400°C. The reaction pressure is preferably 1 Pa to 10,000 Pa, and more preferably 10 Pa to 1,000 Pa.

[0057] The deposition rate can be controlled by the supply conditions of the thin film forming raw material (vaporization temperature, vaporization pressure), reaction temperature, and reaction pressure. If the deposition rate is high, the properties of the obtained thin film may deteriorate, and if it is low, problems may occur in productivity, so the deposition rate is preferably 0.01 nm / min to 100 nm / min, and more preferably 0.1 nm / min to 50 nm / min.

[0058] (Exhaust process) After the precursor thin film is formed, the source gas that has not been deposited on the surface of the substrate is exhausted from the deposition reaction section. At this time, it is ideal that the source gas is completely exhausted from the deposition reaction section, but it is not necessarily required to completely exhaust it. Examples of the exhaust method include a method of purging the inside of the deposition reaction section with an inert gas such as helium, nitrogen, or argon, a method of exhausting by reducing the pressure inside the system, and a combination of these methods. When reducing the pressure, the degree of reduction in pressure is preferably in the range of 0.01 Pa to 300 Pa, more preferably in the range of 0.01 Pa to 100 Pa.

[0059] (Metal-containing thin film formation process) In the metal-containing thin film formation process, after the exhaust process, a reactive gas is introduced into the deposition reaction section, and the reactive gas is reacted with the precursor thin film, i.e., the compound represented by formula (1) deposited on the surface of the substrate, by the action of the reactive gas or the action of the reactive gas and the action of heat, to form a metal-containing thin film.

[0060] Examples of the reactive gas include oxidizing gases such as oxygen, ozone, nitrogen dioxide, nitric oxide, water vapor, hydrogen peroxide, formic acid, acetic acid, acetic anhydride, etc., reducing gases such as hydrogen, organic amine compounds such as monoalkylamine, dialkylamine, trialkylamine, alkylenediamine, etc., nitriding gases such as hydrazine, ammonia, etc. These reactive gases may be used alone or in combination of two or more.

[0061] When heat is used in the reaction between the precursor thin film and the reactive gas, the temperature is preferably 50° C. to 200° C., and more preferably 100° C. to 200° C. The pressure in the deposition reaction zone during this step is preferably 1 Pa to 10,000 Pa, and more preferably 10 Pa to 1,000 Pa.

[0062] (Exhaust process) After the metal-containing thin film is formed, the unreacted reactive gas and by-product gas are exhausted from the deposition reaction zone. Ideally, the reactive gas and by-product gas are completely exhausted from the deposition reaction zone, but it is not necessary to exhaust them completely. The exhaust method and the degree of pressure reduction are the same as those in the exhaust step after the precursor thin film formation step described above.

[0063] As described above, the source gas introduction step, precursor thin film formation step, exhaust step, metal-containing thin film formation step, and exhaust step are performed in order, and deposition by a series of operations is regarded as one cycle. This cycle is repeated several times until a thin film of the required thickness is obtained, thereby producing a metal-containing thin film having a desired thickness. In the thin film production method using the ALD method, the thickness of the formed metal-containing thin film can be controlled by the number of cycles.

[0064] In the thin film manufacturing method of the present invention, energy such as plasma, light, voltage, etc. may be applied to the deposition reaction section, and a catalyst may be used, as shown in Figures 3 and 4. The timing of applying the energy and the timing of using the catalyst are not particularly limited, and may be, for example, when introducing a raw material gas of a raw material for forming the thin film in a raw material gas introduction step, during a heating step in forming a precursor thin film, when introducing a reactive gas or reacting a reactive gas with a precursor thin film in a metal-containing thin film formation step, when exhausting the system in an exhaust step, or between the above steps.

[0065] In the method for producing a thin film of the present invention, after the formation of the thin film, an annealing treatment may be performed in an inert atmosphere, an oxidizing atmosphere, or a reducing atmosphere in order to obtain better electrical properties, and a reflow step may be performed if step filling is required. The temperature in this case is preferably 200°C to 1,000°C, more preferably 250°C to 500°C.

[0066] The thin film produced using the thin film-forming material of the present invention can be coated on a substrate such as a metal, an oxide ceramic, a nitride ceramic, or a glass to produce a desired type of thin film by appropriately selecting other precursors, reactive gases, and production conditions. The thin film of the present invention has excellent electrical and optical properties, and can be widely used in the production of, for example, electrode materials for memory elements such as DRAM elements, resistive films, diamagnetic films used in the recording layers of hard disks, and catalyst materials for polymer electrolyte fuel cells. EXAMPLES

[0067] The present invention will be described in more detail below using examples, etc. However, the present invention is not limited to the following examples, etc.

[0068] [Example 1] Synthesis of Compound No. 1 In a 100ml four-neck flask, 0.60g (4.7mmol) of copper(II) methoxide complex and 20ml of dehydrated ethanol were added at room temperature, and 1.69g (9.4mmol) of the corresponding diketimine ligand was added dropwise under ice cooling, and the mixture was stirred at room temperature for 20 hours. The ethanol was distilled off at a slight reduced pressure in an oil bath of 75°C. The purple solid remaining in the flask was then distilled under reduced pressure (50Pa), and 0.92g (2.2mmol, 46% yield) of purple solid was obtained as the effluent. Analysis of this solid by single crystal X-ray analysis confirmed that it was the target compound, Compound No. 1. The molecular structure of the obtained purple solid by single crystal X-ray analysis is shown in Figure 5.

[0069] Single crystal X-ray analysis results of compound No. 1 Crystal lattice size: 0.11mm x 0.11mm x 0.10mm Crystal system: triclinic system (2 molecules in asymmetric unit, R1=0.0820, wR2=0.1807) Lattice parameters: a=8.859Å b=9.349Å c=12.58Å α=74.69° β=71.28° γ=63.91° V=877Å 3

[0070] [Example 2] Synthesis of Compound No. 19 In a 100 ml four-neck flask, 8.4 g (22.2 mmol) of cobalt bistrimethylsilylamide complex and 50 ml of dehydrated toluene were added at room temperature, and 6.8 g (44.4 mmol) of the corresponding diketimine ligand was added dropwise at room temperature and reacted for 2 hours. The toluene solvent was distilled off at a slight reduced pressure in an oil bath at 100°C. The dark brown viscous liquid remaining in the flask was then distilled under reduced pressure (20-30 Pa), and 7.5 g (20.5 mmol, 92.4% yield) of dark reddish brown liquid was obtained as the distillate. The obtained dark reddish brown liquid slowly solidified at room temperature and became a dark reddish brown solid with a melting point of 38°C. The solid was analyzed by single crystal X-ray analysis and confirmed to be the target compound, Compound No. 19. The molecular structure of the obtained dark reddish brown solid by single crystal X-ray analysis is shown in Figure 6.

[0071] Single crystal X-ray analysis results of compound No. 19 Crystal lattice size: 0.26mm x 0.24mm x 0.07mm Crystal system: Monoclinic (8 molecules in the asymmetric unit, R1=0.0598, wR2=0.1310) Lattice parameters: a=28.047Å b=9.9896Å c=18.954Å β=125.704° V=4312Å 3

[0072] [Example 3] Synthesis of Compound No. 27 In a 100 ml four-neck flask, 1.65 g (3.8 mmol) of tin bis(trimethylsilylamide) complex and 25 ml of dehydrated hexane were added at room temperature, and 1.58 g (7.6 mmol) of the corresponding diketimine ligand was added dropwise under ice cooling, and the reaction was allowed to proceed for 16 hours. The hexane solvent was distilled off under slight reduced pressure in an oil bath at 60°C. The orange liquid remaining in the flask was then distilled under reduced pressure (20-30 Pa), and 0.05 g (0.1 mmol, 2.5% yield) of a yellow solid was obtained as the distillate. 1 The results of H-NMR and ICP-AES analyses confirmed that the compound was the target compound, Compound No. 27.1 The results of analysis by H-NMR and ICP-AES are shown below.

[0073] ( 1 H-NMR (heavy benzene) 0.868-0.904ppm(3H,triplet), 1.147-1.183ppm(3H,triplet), 1.563ppm(3H,singlet), 3.049-3.067ppm(2H,doublet), 3.585ppm(2H,singlet), 5.166ppm(1H,singlet)

[0074] (ICP-AES analysis results) Tin content: 22.1% by mass (theoretical value: 22.27% by mass)

[0075] [Example 4] Synthesis of Compound No. 43 0.57g (4.2mmol) of zinc chloride complex and 40ml of ether were added to a 100ml four-neck flask at room temperature, and 1.93g (8.4mmol) of the corresponding lithium-modified diketimine ligand was added dropwise under ice cooling, and the reaction was allowed to proceed for 16 hours. The ether solution was distilled off at normal pressure in an oil bath at 50°C. Hexane was added to the resulting yellow solid, and the mixture was filtered. The filtrate was subjected to slight desolvation in an oil bath at 60°C. The orange liquid remaining in the flask was then distilled under reduced pressure (20-30Pa), and 1.18g (2.5mmol, 59% yield) of a pale yellow liquid was obtained as the distillate. The pale yellow liquid 1 The results of H-NMR and ICP-AES analyses confirmed that the compound was the target compound, Compound No. 43. 1 The results of analysis by H-NMR and ICP-AES are shown below.

[0076] ( 1 H-NMR (heavy benzene) 0.889-0.925ppm(3H,triplet), 1.079-1.115ppm(3H,triplet), 1.547ppm(3H,singlet), 2.977-3.043ppm(2H,multiplet), 3.502-3.557ppm(2H,multiplet), 5.008ppm(1H,singlet)

[0077] (ICP-AES analysis results) Zinc content: 13.8% by mass (theoretical value: 13.63% by mass)

[0078] [Comparative Example 1] Synthesis of Comparative Compound 1 In formula (1), R 1 and R 5 is CH2CF3, R 2 and R 4 is Me and R 3 The synthesis of the following comparative compound 1 in which is H and M is Cu was attempted. In a 100 ml four-neck flask, 1.07 g (8.5 mmol) of copper (II) methoxide complex and 50 ml of dehydrated ethanol were added at room temperature, and 4.46 g (17 mmol) of a diketimine ligand corresponding to the comparative compound 1 below was added dropwise under ice cooling, and the mixture was stirred at room temperature for 18 hours. The ethanol was distilled off at a slight reduced pressure in an oil bath of 75°C. The black solid remaining in the flask was then distilled under reduced pressure (50 Pa), but the target product could not be isolated.

[0079] [ka]

[0080] [Evaluation example] The following evaluations were carried out using Compound No. 1, Compound No. 19, Compound No. 27, and Compound No. 43 obtained by synthesis in Examples 1 to 4 above, and Comparative Compounds 2 to 5 shown in Tables 1 to 4 below.

[0081] (1) Melting point evaluation The state of the compound was visually observed at normal pressure and 25° C., and the melting point of the solid compound was measured using a micro melting point measuring device. The results are shown in Tables 1 to 4.

[0082] (2) Temperature at 50% mass loss in reduced pressure TG-DTA (℃) Using TG-DTA, measurements were performed at 10 Torr, Ar flow rate: 50 mL / min, heating rate 10°C / min, and scanning temperature range 30°C to 600°C. The temperature (°C) at which the weight of the test compound was reduced by 50% by mass was evaluated as the "temperature (°C) at reduced pressure TG-DTA 50% mass reduction." The lower the temperature (°C) at reduced pressure TG-DTA 50% mass reduction, the lower the temperature at which vapor can be obtained. These results are shown in Tables 1 to 4.

[0083] [Table 1]

[0084] [Table 2]

[0085] [Table 3]

[0086] [Table 4]

[0087] Example 5 Using the above-mentioned compound No. 1 as a thin film forming raw material, and using the ALD apparatus of FIG. 1, a thin film was produced on the surface of a ruthenium wafer as a substrate under the following conditions. When the composition of the thin film was analyzed using X-ray electron spectroscopy, it was confirmed that the thin film contained copper and that the residual carbon content was less than the detection limit of 0.1 atom%. In addition, when the thickness of the thin film was measured using a scanning electron microscope, the thin film formed on the surface of the ruthenium wafer was a smooth film of 2 nm, and the film thickness obtained per cycle was about 0.02 nm.

[0088] (Manufacturing conditions) Manufacturing method: ALD method Reaction temperature (substrate temperature): 200℃ Reactive gas: Hydrogen

[0089] (Process) A series of steps consisting of the following steps (1) to (4) was defined as one cycle, and 100 cycles were repeated. (1) The vapor of the thin film forming raw material (raw material gas) evaporated under conditions of a raw material container temperature of 120°C and a raw material container internal pressure of 100 Pa is introduced into the deposition reaction section, and the raw material gas is deposited on the substrate surface at a system pressure of 100 Pa for 20 seconds to form a precursor thin film. (2) Undeposited source gas is purged from the system by argon purging for 15 seconds. (3) A reactive gas is introduced into the deposition reaction zone, and the precursor thin film is reacted with the reactive gas at a system pressure of 100 Pa for 20 seconds. (4) Unreacted reactive gases and by-product gases are purged from the system by argon purging for 15 seconds.

[0090] Example 6 A thin film was produced on the surface of a ruthenium wafer in the same manner as in Example 5, except that the compound No. 19 was used as a thin film forming raw material, the reaction temperature was changed to 300°C, and the process was changed to 300 cycles. The composition of the thin film was analyzed using X-ray electron spectroscopy, and it was confirmed that the thin film was a thin film containing cobalt and that the residual carbon content was less than the detection limit of 0.1 atom%. In addition, the thickness of the thin film was measured using a scanning electron microscope, and the thin film formed on the surface of the ruthenium wafer was a smooth film of 6 nm, and the film thickness obtained per cycle was about 0.02 nm.

[0091] Example 7 A thin film was produced on the surface of a copper wafer in the same manner as in Example 6, except that the ruthenium wafer was replaced with a copper wafer. The composition of the thin film was analyzed using X-ray photoelectron spectroscopy, and it was confirmed that the thin film contained cobalt and had a residual carbon content less than the detection limit of 0.1 atom%. The thickness of the thin film was measured using a scanning electron microscope, and it was found that the thin film formed on the copper wafer surface was a smooth film of 3 nm, and the film thickness obtained per cycle was about 0.01 nm.

[0092] Comparative Example 6 A copper-containing thin film was produced on the surface of a ruthenium wafer in the same manner as in Example 5, except that Compound No. 1 was changed to Comparative Compound 2 and the temperature of the raw material container was changed from 120° C. to 140° C. However, a smooth film could not be formed. In addition, residual carbon was detected in the obtained film.

[0093] Comparative Example 7 A thin film containing cobalt was produced on the surface of a ruthenium wafer in the same manner as in Example 6, except that Compound No. 19 was changed to Comparative Compound 3 and the temperature of the raw material container was changed from 120° C. to 140° C. However, a smooth film could not be formed. Furthermore, residual carbon was detected in the obtained film.

[0094] Comparative Example 8 A thin film containing cobalt was produced on the surface of a copper wafer in the same manner as in Comparative Example 7, except that the ruthenium wafer was replaced with a copper wafer, but a smooth film could not be formed. In addition, residual carbon was detected in the obtained film.

[0095] From the results of Comparative Example 1, R 2 , R 3 and R 4 It has been difficult to produce compounds in which R other than the above is a group containing a fluorine atom. The reason why good thin films could not be produced in Comparative Examples 6, 7, and 8 is believed to be that the vapor pressure of Comparative Compounds 2 and 3 was low, which required the temperature of the source container to be high, but when the source container temperature was 140°C, thermal decomposition occurred in Comparative Compounds 2 and 3.

[0096] From the above, in the compound represented by formula (1), R 2 , R 3 and R 4 It was confirmed that at least one of the above points enables the production of highly volatile and high-quality thin films by using a compound substituted with a group containing a fluorine atom as a thin-film-forming raw material.

Claims

1. A compound represented by the following formula (1): [Formula 1] (In formula (1), R 1 and R 5 are each independently an alkyl group having 1 to 5 carbon atoms, R 2 and R 4 are each independently a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or an alkyl group having 1 to 5 carbon atoms substituted with a fluorine atom, but at least one of R 2 and R 4 is an alkyl group having 1 to 5 carbon atoms substituted with a fluorine atom, R 3 is a hydrogen atom, M represents a metal atom, and n represents the valence of the metal atom represented by M.

2. 2. The compound according to claim 1, wherein M in formula (1) is a metal atom selected from copper, nickel, cobalt, tin, manganese and zinc.

3. A thin film-forming material comprising the compound according to claim 1 or 2.

4. 3. Use of a compound according to claim 1 or 2 as a precursor for producing metal-containing thin films by chemical vapor deposition.

5. A thin film produced using the method of claim 4.

6. A method for producing a thin film, comprising: introducing a raw material gas obtained by vaporizing the thin film-forming raw material according to claim 3 into a processing atmosphere in which a substrate is placed; and decomposing and / or chemically reacting the compounds in the raw material gas to form a metal-containing thin film on the surface of the substrate.

Citation Information

Patent Citations

  • Novel beta-diketiminato zirconium compound, preparation thereof and application thereof

    CN101274939A

  • JP1975003978A

  • Taishinyo roshinsentaaguritsudo

    JP1976081292A

  • β-Diketiminate Ligand Sources and Metal-Containing Compounds Thereof, and Systems and Methods Containing Them

    JP2009503247A

  • Methods for deposition of alkaline earth metal fluoride films

    US20120308739A1