Surfactant composition for expanded sand
A surfactant composition with specific components enhances rapid foaming and mold strength in foamed sand applications, addressing the limitations of existing compositions by improving manufacturing efficiency and mold quality.
Patent Information
- Application Number
- JP2023538743
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-12-17
- Filing Date
- 2022-12-05
- Publication Date
- 2024-09-20
- Estimated Expiration
- 2042-12-05
AI Technical Summary
Existing surfactant compositions for foamed sand do not provide sufficient rapid foaming properties and mold strength, especially in mold manufacturing processes using foamed sand.
A surfactant composition comprising specific polyoxyethylene alkyl ether sulfate salt, acyl taurine salt, and polyalkylene glycol derivative in defined proportions, which enhances rapid foaming and mold strength.
The composition enables rapid foaming of the binder-sand mixture and results in high-strength molds, improving the efficiency and quality of mold manufacturing.
Smart Images

Figure 0007554939000006 
Figure 0007554939000007 
Figure 0007554939000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a surfactant composition for expanded sand, which is excellent in foaming speed of expanded sand and improves the strength of a mold when the expanded sand is used to manufacture a mold such as a sand core. [Background technology]
[0002] Patent Document 1 is known as a conventional technique related to a mold-making device. Patent Document 1 discloses a mold-making device that presses and fills a foamed mixture obtained by stirring particulate aggregate, a water-soluble binder, and water into the cavity of a heated mold to make a mold, and a mold device used therefor. This provides a mold-making device that can effectively use the foamed mixture and ensure sufficient filling of the mold cavity with fluid sand, as well as an apparatus that can significantly shorten the hardening time of the foamed mixture. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] WO 2005 / 089984 A1 Summary of the Invention [Problem to be solved by the invention]
[0004] In the method described in Patent Document 1, in order to improve the foaming and flow state of the foamed mixture, the water-soluble binder is required to have not only the inherent caking performance but also foaming properties, and a surfactant composition is added to the water-soluble binder. The surfactant is required to be a surfactant composition for foamed sand that is excellent in the foaming speed of the foamed sand and further improves the strength of the mold.
[0005] An object of the present invention is to provide a surfactant composition for expanded sand which, when used to manufacture molds such as sand cores using expanded sand, exhibits excellent foaming speed and improves the strength of the molds. [Means for solving the problem]
[0006] As a result of intensive research to solve the above problems, the present inventors have found that a surfactant composition for foamed sand containing a specific polyoxyethylene alkyl ether sulfate salt, a specific acyltaurine salt, and a specific polyalkylene glycol derivative in specific proportions has excellent foaming speed of foamed sand and also has the effect of improving the strength of the mold, thereby completing the present invention.
[0007] That is, the present invention is as follows. (1) A surfactant composition for foamed sand, comprising a compound (A) represented by the following formula (1) and a compound (B) represented by the following formula (2), characterized in that, when the total mass of the compound (A) and the compound (B) is taken as 100 mass%, the content of the compound (A) is 25 to 85 mass%, and the content of the compound (B) is 15 to 75 mass%. R 1 O-(EO) a -SO3M 1 (1) (In formula (1), R 1 represents a hydrocarbon group having 6 to 22 carbon atoms, EO is an oxyethylene group; a is the average number of moles of the oxyethylene group added, and a is 1 to 10. M 1 is an alkali metal, an alkaline earth metal, ammonium or an organic ammonium. R 2 CONR 3 C2H4SO3M 2 (2) (In formula (2), R 2 CO represents an aliphatic acyl group having 6 to 22 carbon atoms. R 3 is a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, M 2 is an alkali metal, an alkaline earth metal, ammonium or an organic ammonium. (2) The surfactant composition for foamed sand according to (1), further comprising a compound (C) represented by the following formula (3), wherein the content of the compound (C) is 1 to 20 parts by mass when the total mass of the compound (A) and the compound (B) is 100 parts by mass: R 4 O-(AO) b -H···(3) (In formula (3), R 4 represents a hydrogen atom or a hydrocarbon group having 1 to 5 carbon atoms, AO is an oxyalkylene group having 2 to 3 carbon atoms, b is the average number of moles of the oxyalkylene group added, and b is 2 to 100. Effect of the Invention
[0008] By using the surfactant composition for foamed sand of the present invention, it is possible to sufficiently foam the binder, sand, the surfactant composition, water and the like by simply kneading them for a short period of time, and further to produce a mold having high strength. [Brief description of the drawings]
[0009] [Figure 1] FIG. 2 is a schematic diagram showing a method for measuring a dynamic viscosity. [Diagram 2] FIG. 2 is a schematic diagram showing a state in which a test piece is set in a die flexural strength tester and the flexural strength of the test piece is measured. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The surfactant composition for foamed sand of the present invention contains component (A), component (B) and, if necessary, component (C). The total mass of the compound (A) and the compound (B) is taken as 100% by mass. Each component will be described below. It should be noted that numerical ranges such as "1 to 10" include the upper and lower limits, meaning 1 or more and 10 or less.
[0011] [Component (A)] The component (A) used in the present invention is a polyoxyethylene alkyl ether sulfate represented by the following formula (1). R 1 O-(EO) a -SO3M 1 (1)
[0012] In the polyoxyethylene alkyl ether sulfate salt represented by formula (1), R 1 is a hydrocarbon group having 6 to 22 carbon atoms, preferably a hydrocarbon group having 6 to 20 carbon atoms. This hydrocarbon group may be a saturated hydrocarbon group, or a hydrocarbon group having a carbon-carbon double bond (particularly preferably an alkenyl group). When the hydrocarbon group is an unsaturated hydrocarbon group having a carbon-carbon double bond, the number of double bonds is preferably 3 or less, more preferably 2 or less. Examples of such hydrocarbon groups include a capryl group, a capric group, a lauryl group, a myristyl group, a palmityl group, a stearyl group, an oleyl group, and a behenyl group. In addition, a hydrocarbon group derived from a mixed fatty acid containing two or more kinds of hydrocarbon groups may also be used, such as a coconut oil hydrocarbon group or a palm kernel oil hydrocarbon group. Among these, a lauryl group, a myristyl group, a coconut oil hydrocarbon group, and a palm kernel oil hydrocarbon group are preferred, and a mixture of a lauryl group and a myristyl group is even more preferred.
[0013] In the formula (1), a represents the average number of moles of oxyethylene groups added, and a is 1 to 10, preferably 2 to 6, and more preferably 3 to 4.
[0014] In formula (1), M 1 is an alkali metal, an alkaline earth metal, ammonium or an organic ammonium. Examples of the alkali metal include lithium, sodium, potassium, etc., and preferably sodium. Examples of the alkaline earth metal include calcium, strontium, barium, etc., and preferably calcium. Ammonium is NH4 + It is.
[0015] Examples of the organic ammonium include alkanol ammonium derived from alkanolamines such as monoethanolamine, diethanolamine, and triethanolamine, and alkyl ammonium derived from alkylamines such as diethylamine and triethylamine.
[0016] In the present invention, the component (A) can be used in an appropriate combination of one or more types. When the total mass of the compound (A) and the compound (B) is taken as 100 mass%, the content of the component (A) is 25 to 85 mass%. If the content of the component (A) is less than 25 mass%, the foaming speed may decrease, so the content is set to 25 mass% or more, more preferably 30 mass% or more, and even more preferably 35 mass% or more. If the content of the component (A) exceeds 85 mass%, the strength of the mold may decrease, so the content is set to 85 mass% or less, more preferably 75 mass% or less, and even more preferably 70 mass% or less.
[0017] [(B) component] The component (B) used in the present invention is an acyltaurine salt represented by the following formula (2). R 2 CONR 3 C2H4SO3M 2 (2)
[0018] In the acyltaurine salt represented by formula (2), R 2 CO is an aliphatic acyl group having 6 to 22 carbon atoms, and preferably an aliphatic acyl group having 10 to 18 carbon atoms. Examples of such aliphatic acyl groups include a capryloyl group, a caprinoyl group, a lauroyl group, a myristoyl group, a palmitoyl group, a stearoyl group, a behenoyl group, and mixtures thereof such as coconut oil fatty acid residues, palm oil fatty acid residues, palm kernel oil fatty acid residues, beef tallow fatty acid residues, and hardened beef tallow fatty acid residues.
[0019] In formula (2), R 3is a hydrogen atom or an alkyl group having 1 to 3 carbon atoms. Examples of the alkyl group having 1 to 3 carbon atoms include a methyl group, an ethyl group, a propyl group, and an isopropyl group. A hydrogen atom, a methyl group, and an ethyl group are preferred. These can be obtained, for example, by the following method: Sodium methyl taurine is acylated with a fatty acid chloride in the presence of sodium hydroxide to obtain sodium acyl methyl taurine.
[0020] In formula (2), M 2 is an alkali metal, an alkaline earth metal, ammonium or an organic ammonium. Examples of the alkali metal include lithium, sodium, potassium, etc., and preferably sodium. Examples of the alkaline earth metal include magnesium, strontium, barium, etc., and preferably magnesium. Examples of the organic ammonium include alkanol ammonium derived from alkanolamines such as monoethanolamine, diethanolamine, and triethanolamine, and alkyl ammonium derived from alkylamines such as diethylamine and triethylamine.
[0021] In the present invention, the component (B) can be used singly or in combination of two or more. When the total mass of the compound (A) and the compound (B) is taken as 100 mass%, the content of the component (B) is 15 to 75 mass%. If the content of the component (B) is less than 15 mass%, the foaming speed decreases, so the content is set to 15 mass% or more, and more preferably 20 mass% or more. If the content of the component (B) exceeds 75 mass%, the strength of the mold may decrease, so the content is set to 75 mass% or less, and more preferably 65 mass% or less, and more preferably 60 mass% or less.
[0022] [(C) component] The component (C) used in the present invention is a polyalkylene glycol derivative represented by the following formula (3). R 4 O-(AO) b -H···(3)
[0023] In formula (3), R 4 is a hydrogen atom or an alkyl group having 1 to 5 carbon atoms. Examples of the alkyl group having 1 to 5 carbon atoms include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a hexyl group, and an isohexyl group. A hydrogen atom, a methyl group, or a butyl group is preferred.
[0024] In formula (3), AO is an oxyalkylene group having 2 to 3 carbon atoms. Examples of the oxyalkylene group having 2 to 3 carbon atoms include an oxyethylene group and an oxypropylene group. Note that AO may be only an oxyethylene group, may be only an oxypropylene group, or may contain both an oxyethylene group and an oxypropylene group. When both are contained, it is more preferable that the ratio of the oxyethylene group and the oxypropylene group is 40 mol % or more, and the addition form may be block or random.
[0025] In the formula (3), b is the number of moles of oxyalkylene having 2 to 3 carbon atoms added, which is 2 to 100, preferably 10 to 80, and more preferably 30 to 60.
[0026] In the present invention, the component (C) can be used in an appropriate combination of one or more types. In addition, when the total mass of the compound (A) and the compound (B) is 100 parts by mass, the content of the (C) component is preferably 1 to 20 parts by mass. If the content of the (C) component is less than 1 part by mass, the strength of the mold decreases, so the content is set to 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more. If the content of the (C) component exceeds 20 parts by mass, the foaming speed may decrease, so the content is set to 20 parts by mass or less, preferably 18 parts by mass or less, and even more preferably 15 parts by mass or less.
[0027] The weight average molecular weight of component (C) is preferably 100 to 5000, more preferably 500 to 4500, and even more preferably 1000 to 4000. If the molecular weight is less than 100, the strength of the mold may decrease. If the molecular weight exceeds 5000, the foaming speed may decrease.
[0028] The surfactant composition for foamed sand of the present invention may contain additives other than the above components within the range that does not impair the effects of the present invention. For example, surfactants other than components (A), (B), and (C), organic or inorganic salts, pH adjusters, bactericides, thickeners, chelating agents, colorants, fragrances, etc. may be included. EXAMPLES
[0029] [Examples 1 to 11 and Comparative Examples 1 to 6] The present invention will now be described in detail with reference to examples and comparative examples. The raw materials of Examples 1 to 11 and Comparative Examples 1 to 6 shown in Tables 4 and 5 were all placed in a beaker and stirred for 1 hour at 50°C using a magnetic stirrer to prepare surfactant compositions for foamed sand. "-" in the table means that no material was used.
[0030] In addition, explanations of the symbols etc. in formula (1) for each component A1 and A2 shown in Tables 4 and 5 are given in Table 1, explanations of the symbols etc. in formula (2) for each component B1 and B2 shown in Tables 4 and 5 are given in Table 2, and physical properties etc. of each component C1 and C2 shown in Tables 4 and 5 are given in Table 3.
[0031] The following tests were carried out on each of the obtained surfactant compositions for foamed sand. In each test, those rated as "A" and "B" were deemed to have passed the tests.
[0032] (1) Fast foaming Step 1 Prepare artificial sand as particulate aggregate, water glass and a surfactant for evaluation as water-soluble binders, and water. These materials are put into a kneading machine in a weight ratio of 100 parts artificial sand, 0.5 to 2.5 parts water glass solids, 0.01 to 0.05 parts active ingredient of surfactant, and 2 to 4 parts water. Step 2 The above ingredients are mixed for 90 seconds using a mixer to produce a foamed mixture. Step 3 The foamed kneaded product is placed in a kinematic viscosity measuring device as shown in FIG. Step 4 As shown in Figure 1, a 1 kg weight is placed on the foamed kneaded material, and the foamed kneaded material is discharged from the φ6 mm hole at the bottom while the weight is lowered. The time it takes for the weight to pass through the reference lines spaced 50 mm apart is measured as the kinetic viscosity.
[0033] The evaluation of the quick foaming property was carried out according to the following evaluation criteria. ◎: Measurement time is less than 1.80 seconds ○: Measurement time is 2.20 seconds or less, 1.80 seconds or more ×: Measurement time is more than 2.20 seconds
[0034] (2) Mold strength The flexural strength of a mold made of foamed sand is measured. Step 1 Prepare artificial sand as particulate aggregate, water glass and a surfactant for evaluation as water-soluble binders, and water. These materials are put into a kneading machine in a weight ratio of 100 parts artificial sand, 0.5 to 2.5 parts water glass solids, 0.01 to 0.05 parts active ingredient of surfactant, and 2 to 4 parts water. Step 2 These materials are mixed for 120 seconds using a mixer to produce a foamed mixture. Step 3 The foamed mixture prepared above is poured into a mold using a strength measurement test piece molding device. The mold test piece (10 mm x 30 mm x 85 mm) is molded by baking in a molding die at 200 to 300°C for 30 to 120 seconds. Step 4 The molded and removed mold specimen is cooled to room temperature. Step 5 As shown in Figure 2, a test piece was set in a die-bending strength tester, and the die-bending strength of the test piece was measured to determine the die strength. The die strength is measured in kg / cm. 2 It is.
[0035] The mold strength was evaluated according to the following evaluation criteria. ◎: Mold strength is 25kg / cm 2 End ○: Mold strength is 20kg / cm 2 More than 25kg / cm 2 less than ×: Mold strength is 20kg / cm 2 less than
[0036] [Table 1]
[0037] [Table 2]
[0038] [Table 3]
[0039] [Table 4] D1: "Persoft SK" (manufactured by NOF Corp.) D2: "Nissan Anon BDL-SF" (NOF Corporation) D3: "NAA-43" (NOF Corporation) D4: "Non-Sal LK-2" (NOF Corporation)
[0040] [Table 5]
[0041] The surfactant compositions for foamed sand of Examples 1 to 11 according to the present invention contain components (A), (B) and (C) in specific ratios, and therefore exhibit excellent foaming speed of the foamed sand and also good mold strength.
[0042] In Comparative Example 1, the components (B) and (C) were not contained, and therefore the foaming speed was low. In Comparative Example 2, since components (A) and (C) were not contained, the mold strength was low. In Comparative Example 3, the content of component (A) was low and the content of component (B) was high, so the mold strength was low. In Comparative Example 4, the content of the component (A) was high and the content of the component (B) was low, so that the foaming speed was low. In Comparative Example 5, since component (B) was not contained, the foaming speed and mold strength were low. In Comparative Example 6, the content of component (A) was low and the content of component (B) was high, so the mold strength was low.
Claims
1. A surfactant composition for foamed sand, comprising a compound (A) represented by the following formula (1) and a compound (B) represented by the following formula (2), wherein the content of the compound (A) is 25 to 85% by mass and the content of the compound (B) is 15 to 75% by mass when the total mass of the compound (A) and the compound (B) is taken as 100% by mass. 2 1 9-(59) a -39 3 7. 1 ・・・(1) (In formula (1), R 1 represents a hydrocarbon group having 6 to 22 carbon atoms, EO is an oxyethylene group; a is the average number of moles of the oxyethylene group added, and a is 1 to 10; M 1 is an alkali metal, an alkaline earth metal, ammonium or an organic ammonium. R 2 CONR 3 C 2 H 4 SO 3 M 2 ・・・(2) (In formula (2), R 2 CO represents an aliphatic acyl group having 6 to 22 carbon atoms; R 3 is a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, M 2 is an alkali metal, an alkaline earth metal, ammonium or an organic ammonium.
2. The foamed sand surfactant composition according to claim 1, further comprising a compound (C) represented by the following formula (3), wherein the content of the compound (C) is 1 to 20 parts by mass when the total mass of the compound (A) and the compound (B) is 100 parts by mass. R 4 O-(AO) b -H・・・(3) (In formula (3), R 4 represents a hydrogen atom or a hydrocarbon group having 1 to 5 carbon atoms, AO is an oxyalkylene group having 2 to 3 carbon atoms, b is the average number of moles of the oxyalkylene group added, and b is 2 to 100.
Citation Information
Patent Citations
Hoosuseizosochi
JP1976016364A
Refractory coating composition
JP1992295075A
Component of binding agent for gas hardening mold
JP2001314939A
Surface active agent composition for foam sand
JP2020089909A
Casting mold forming apparatus and metal mold unit for use therein
WO2005089984A1