Method for producing polymer solid electrolyte and polymer solid electrolyte produced by the same

By employing a polymer and non-volatile liquid compound with immiscibility to form separate membranes, the method addresses conductivity and manufacturing issues in all-solid-state batteries, resulting in a stable and efficient solid polymer electrolyte.

JP7554957B2Active Publication Date: 2024-09-20LG ENERGY SOLUTION LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024503963
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-12-07
Filing Date
2022-12-08
Publication Date
2024-09-20
Estimated Expiration
2042-12-08

AI Technical Summary

Technical Problem

All-solid-state batteries face issues with ionic conductivity at the interface between the electrode and solid electrolyte due to voids, and thin film solid electrolytes are prone to damage during manufacturing.

Method used

A method involving the use of a polymer and a non-volatile liquid compound with poor miscibility, forming a liquid phase membrane and a polymer solid electrolyte membrane through phase separation, allowing for a uniform thin film electrolyte production without damage.

Benefits of technology

The method produces a solid polymer electrolyte in the form of a uniform thin film with high ionic conductivity, improving the stability and performance of all-solid-state batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554957000011
    Figure 0007554957000011
  • Figure 0007554957000009
    Figure 0007554957000009
  • Figure 0007554957000010
    Figure 0007554957000010
Patent Text Reader

Abstract

The present invention relates to a method for preparing a polymer solid electrolyte and a polymer solid electrolyte prepared by the same. More specifically, in preparing the polymer solid electrolyte, a polymer and a non-volatile liquid compound, which are poorly miscible with each other, are used as raw materials, and a liquid membrane and a polymer electrolyte membrane can be formed by a phase separation phenomenon that occurs when mixing and drying the raw materials, and the polymer electrolyte membrane can be obtained in the form of a uniform thin film.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of priority based on Korean Patent Application No. 2021-0175035 filed on December 8, 2021 and Korean Patent Application No. 2022-0169918 filed on December 7, 2022, and all contents disclosed in the documents of the relevant Korean patent applications are incorporated as part of this specification.

[0002] The present invention relates to a method for producing a polymer solid electrolyte and a polymer solid electrolyte produced thereby. [Background technology]

[0003] Currently, various batteries capable of overcoming the limitations of lithium secondary batteries are being researched from the standpoints of battery capacity, safety, output, large size, and ultra-compactness.

[0004] Representatively, ongoing research is being conducted on metal-air batteries, which have a much larger theoretical capacity than current lithium secondary batteries, all solid batteries, which are safe and have no risk of explosion, super capacitors, NaS batteries or RFBs (redox flow batteries), and thin film batteries, which are large-sized.

[0005] Among them, solid-state batteries are batteries that replace the liquid electrolyte used in existing lithium secondary batteries with a solid, and because they do not use flammable solvents in the battery, they can greatly improve safety by preventing fires and explosions caused by the decomposition reaction of conventional electrolytes.In addition, they have the advantage of being able to fundamentally improve the energy density relative to the mass and volume of the battery because they can use Li metal or Li alloy as the anode material.

[0006] As such, all-solid-state batteries are attracting attention as the next-generation lithium secondary batteries from the standpoints of safety, high energy density, high output, and simplified manufacturing processes.

[0007] However, in such an all-solid-state battery, since both the electrodes and the solid electrolyte are solid and there is no liquid electrolyte, there is a problem that dead space, i.e., a gap with no ionic conductivity, occurs at the interface between the electrodes and the solid electrolyte.

[0008] In addition, as batteries become thinner, the demand for thin-film solid electrolytes is increasing. However, as solid electrolytes become thinner, their strength weakens, making them difficult to separate from the release film attached during the manufacturing process, and there is also the problem of the thin film being damaged.

[0009] Therefore, there is a need for development of a technology capable of producing a uniform thin-film solid electrolyte. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] Patent No. 2020-526897 Summary of the Invention [Problem to be solved by the invention]

[0011] As a result of extensive research to solve the above problems, the present inventors have confirmed that when a polymer and a non-volatile liquid compound, which are poorly miscible with each other, are used as raw materials in the preparation of a polymer solid electrolyte, a liquid phase film and a polymer solid electrolyte film are formed due to a phase separation phenomenon that occurs when mixing and drying the raw materials, and the polymer solid electrolyte film has a uniform thin film shape.

[0012] SUMMARY OF THE PRESENT EMBODIMENT An object of the present invention is to provide a method for preparing a polymer solid electrolyte having a uniform thin film form and a polymer solid electrolyte prepared thereby. [Means for solving the problem]

[0013] The present invention relates to a method for producing a polymer solid electrolyte, the method for producing the polymer solid electrolyte includes: (S1) adding a polymer, a non-volatile liquid compound, and a lithium salt to a solvent to prepare a polymer solid electrolyte forming solution; (S2) applying the polymer solid electrolyte forming solution onto a substrate to form a coating layer; (S3) drying the coating layer to separate it into a liquid phase film and a polymer solid electrolyte film; and (S4) separating the polymer solid electrolyte film.

[0014] The liquid phase film may include the non-volatile liquid compound, the polymer solid electrolyte film may include the polymer and a lithium salt, the non-volatile liquid compound may be immiscible with the polymer, the liquid phase film may be formed on a substrate, and the polymer solid electrolyte film may be formed on the liquid film.

[0015] The weight ratio of the polymer to the non-volatile liquid compound may be 1:0.8 to 1:5.5.

[0016] The polymer may include one or more selected from the group consisting of polypropylene carbonate (PPC), polyacrylonitrile (PAN), and polyvinylpyrrolidone (PVP).

[0017] The non-volatile liquid compound may include at least one selected from the group consisting of polyhedral oligomeric silsesquioxane (POSS) and ionic liquid.

[0018] The POSS includes one or more functional groups (R), and the functional groups may be functional groups containing one or more elements selected from O, N, S, Si, and P, or functional groups capable of binding to lithium ions.

[0019] The functional group may be poly(ethylene glycol) (PEG), alcohol, amine, carboxylic acid, allyl, epoxide, thiol, silane, or silanol.

[0020] The ionic liquid comprises a cation and an anion, the cation being at least one selected from the group consisting of imidazolium, pyrazolium, triazolium, thiazolium, oxazolium, pyridazinium, pyrimidinium, pyrazinium, ammonium, phosphonium, pyridinium, and pyrrolidinium, which may be substituted or unsubstituted by an alkyl group having 1 to 15 carbon atoms; The anion is PF6 - , BF4 - , CF3SO3 - , N(CF3SO2)2 - , N(C2F5SO2)2 - , C(CF2SO2)3 - , AsF6 - , SbF6 - , AlCl4 - , NbF6 - , HSO4 - , ClO4 - , CH3SO3 - and CF3CO2 - The composition may include one or more selected from the group consisting of:

[0021] The lithium salts include lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(fluorosulfonyl)imide (LiFSI), LiNO3, LiOH, LiCl, LiBr, LiI, LiClO4, LiBF4, LiB 10 Cl 10 , LiPF6, LiCF3SO3, LiCF3CO2, LiAsF6, LiSbF6, LiAlCl4, CH3SO3Li, CF3SO3Li, LiSCN, LiC(CF3SO2)3, (CF3SO2)2NLi, and (FSO2)2NLi.

[0022] The substrate may include at least one selected from the group consisting of stainless steel, Cu foil, and Al foil.

[0023] The method for forming the coating layer may be bar coating, roll coating, spin coating, slit coating, die coating, blade coating, comma coating, slot die coating, lip coating, or solution casting.

[0024] The weight ratio of the polymer to the lithium salt may be 1:0.5 to 1:3.

[0025] The solvent may include one or more selected from the group consisting of propylene carbonate (PC), ethylene carbonate (EC), butylene carbonate (BC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propionate (MP), dimethyl sulfoxide, dimethoxyethane, diethoxyethane, tetrahydrofuran, N-methyl-2-pyrrolidone (NMP), ethyl methyl carbonate (EMC), vinylene carbonate (VC), gamma butyrolactone (GBL), fluoroethylene carbonate (FEC), methyl formate, ethyl formate, propyl formate, methyl acetate, ethyl acetate, propyl acetate, pentyl acetate, methyl propionate, ethyl propionate, ethyl propionate, and butyl propionate.

[0026] Drying of the coating layer may be accomplished at temperatures below 150°C.

[0027] The present invention also provides a polymer solid electrolyte comprising the above polymer and a lithium salt.

[0028] The polymer solid electrolyte may have a thickness of 23 μm to 35 μm.

[0029] The thickness deviation of the polymer solid electrolyte is 0.7 μm or less, and the thickness deviation is within 3×3 cm 2 The thickness was measured at nine positions in a solid polymer electrolyte sample punched out by , and the deviation between the thickest and thinnest thicknesses was calculated.

[0030] The polymer solid electrolyte may be in the form of a freestanding film.

[0031] The ionic conductivity of the polymer solid electrolyte is 1.2×10 -5 or 4.5 x 10 -5 The ionic conductivities, in S / cm, were measured at 80°C.

[0032] The present invention also provides an all-solid-state battery comprising the polymer solid electrolyte.

[0033] The present invention also provides a polymer solid electrolyte, the thickness of which is 23 μm to 35 μm, the thickness deviation of which is 0.7 μm or less, and the thickness deviation is within a range of 3×3 cm 2 The thickness was measured at nine positions in the solid polymer electrolyte sample punched out in step 1, and the deviation between the thickest and thinnest thicknesses was calculated. The solid polymer electrolyte was in the form of a freestanding film, and the ionic conductivity of the solid polymer electrolyte was 1.2×10 -5 or 4.5 x 10 -5 The present invention provides a polymer solid electrolyte having a specific surface area of ​​100 nm and a specific surface area of ​​100 nm. Effect of the Invention

[0034] According to the present invention, in the process of preparing the polymer solid electrolyte, a polymer and a non-volatile liquid compound, which are incompatible with each other, are used as raw materials, and the polymer and the non-volatile liquid compound are mixed together. In accordance with the principle that phase separation occurs during drying, a laminate in which a liquid phase membrane and a polymer solid electrolyte membrane are laminated is formed, and then the laminate is separated to prepare a uniform thin film of the polymer solid electrolyte.

[0035] In addition, in the process of preparing the polymer solid electrolyte, after a liquid phase membrane and a polymer solid electrolyte membrane are formed on the substrate, when the polymer solid electrolyte membrane is separated from the substrate, the polymer solid electrolyte membrane can be separated without additional resistance due to the liquid phase membrane in contact with the substrate. [Brief description of the drawings]

[0036] [Figure 1] 1 is a schematic diagram illustrating a process for preparing a polymer solid electrolyte according to an embodiment of the present invention; [Diagram 2] 1 is a schematic diagram showing a structure of a laminate including a liquid phase membrane and a polymer solid electrolyte membrane formed in a process for preparing a polymer solid electrolyte according to an embodiment of the present invention; FIG. [Diagram 3]FIG. 2 is a schematic diagram of a sample for measuring the uniformity of a polymer solid electrolyte prepared according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0037] The present invention will now be described in more detail to aid in understanding the present invention.

[0038] The terms and words used in this specification and claims should not be construed in a limited manner based on their ordinary or dictionary meaning, but should be construed in a meaning and concept that corresponds to the technical idea of ​​the present invention, based on the principle that the inventor can appropriately define the concept of the term in order to best describe his / her invention.

[0039] As used herein, the term "miscibility" refers to the property of not mixing.

[0040] The term "free-standing film" used herein means a film that can maintain its film form by itself without a separate support at room temperature and pressure.

[0041] Method for producing polymer solid electrolyte The present invention relates to a method for producing a polymer solid electrolyte, comprising the steps of: (S1) preparing a polymer solid electrolyte forming solution by adding a polymer, a non-volatile liquid compound, and a lithium salt to a solvent; (S2) applying the polymer solid electrolyte forming solution onto a substrate to form a coating layer; (S3) drying the coating layer to separate it into a liquid phase film and a polymer solid electrolyte film; and (S4) separating the polymer solid electrolyte film; wherein the non-volatile liquid compound is immiscible with the polymer, the liquid phase film comprises the non-volatile liquid compound, and the polymer solid electrolyte film comprises the polymer and a lithium salt.

[0042] In the method for producing the polymer solid electrolyte, a polymer and a non-volatile liquid compound, which are poorly miscible with each other, are used as raw materials. After the polymer and the non-volatile liquid compound are mixed, a phase separation phenomenon occurs during drying, so that a liquid phase film containing the non-volatile liquid compound and a polymer solid electrolyte film containing the polymer can be formed. After a laminate is formed in which the substrate, the liquid phase film, and the polymer solid electrolyte film are laminated in this order, the polymer solid electrolyte film is separated to obtain a polymer solid electrolyte. At this time, since a liquid phase film is formed between the substrate and the polymer solid electrolyte film, the polymer solid electrolyte film can be easily separated without resistance.

[0043] FIG. 1 is a schematic diagram showing a method for producing a polymer solid electrolyte according to an embodiment of the present invention, and FIG. 2 is a schematic diagram showing a structure of a laminate including a liquid phase membrane and a polymer solid electrolyte membrane formed during a process for producing a polymer solid electrolyte according to an embodiment of the present invention. Each step of the method for producing a polymer solid electrolyte according to the present invention will be described in more detail with reference to these drawings.

[0044] In the present invention, in the step (S1), a polymer, a non-volatile liquid compound, and a lithium salt may be added to a solvent to prepare a solution for forming a polymer solid electrolyte.

[0045] The polymer can form a uniform thin film of the polymer solid electrolyte without decreasing the electrical conductivity and ionic conductivity of the polymer solid electrolyte.

[0046] In addition, the polymer is not particularly limited as long as it is a polymer that exhibits immiscible properties with respect to the non-volatile liquid compound contained in the liquid phase film, and for example, the polymer may include one or more selected from the group consisting of polypropylene carbonate (PPC), polyacrylonitrile (PAN), and polyvinylpyrrolidone (PVP).

[0047] The non-volatile liquid compound exhibits immiscible properties with respect to the polymer, and may be phase-separated from the polymer during the preparation process of the polymer solid electrolyte to form a separate layer-type liquid membrane.

[0048] The non-volatile liquid compound may also include polyhedral oligomeric silsesquioxane (POSS) and / or ionic liquid.

[0049] The POSS is a polyhedral oligosilsesquioxane that includes one or more functional groups (R), and the functional group (R) is a functional group containing one or more elements selected from O, N, S, Si, and P, or includes a functional group capable of binding to a lithium ion. For example, the functional group (R) may be polyethylene glycol (PEG), alcohol, amine, carboxylic acid, allyl, epoxide, thiol, silane, silanol, glycidyl, octasilane, or methacryl.

[0050] In addition, the POSS may be PEG-POSS containing ethylene glycol (PEG) as a functional group (R), and when the PEG-POSS is used, the phase separation of the polymer is more smoothly performed. For example, when PPC and PEG-POSS are used, the phase separation is smoothly performed, and the process efficiency can be improved.

[0051] Furthermore, POSS is in a solid or liquid phase depending on the functional group (R). In order to smoothly separate the phase from the polymer, it is advantageous to use liquid POSS, and the liquid POSS may contain the functional group (R) as described above, and preferably, the liquid POSS may be PEG-POSS.

[0052] In the present invention, the liquid POSS may be represented by the following Chemical Formula 1: [Chemical formula 1] [ka] In the above Chemical Formula 1, R may be the same or different, and each R is independently selected from the group consisting of groups represented by the following formulas 1-1 to 1-4: [Chemical formula 1-1] [ka] [Chemical formula 1-2] [ka] [Chemical formula 1-3] [ka] [Chemical formula 1-4] [ka]

[0053] In the above Chemical Formulas 1-1 to 1-4, L1 to L5 are C1 to C30 alkylene groups, R1 to R4 are selected from the group consisting of hydrogen; a hydroxyl group; an amino group; a thiol group; a C1 to C30 alkyl group; a C2 to C30 alkenyl group; a C2 to C30 alkynyl group; a C1 to C30 alkoxy group; and a C1 to C30 carboxyl group; m and n may be the same or different, and each independently represents an integer from 0 to 10; * indicates the bond position.

[0054] In one embodiment of the present invention, in the formulas 1-1 to 1-4, L1 to L5 are C1 to C10 alkylene groups, R1 to R4 are hydrogen; a hydroxyl group; or a C1 to C30 alkyl group, and m and n may be the same or different and may each independently be an integer from 0 to 10.

[0055] In one embodiment of the present invention, the functional group R in Formula 1 is selected from the group consisting of a polyethylene glycol group, a glycidyl group, an octasilane group, and a methacryl group.

[0056] The ionic liquid includes a cation and an anion, the cation includes at least one selected from the group consisting of imidazolium, pyrazolium, triazolium, thiazolium, oxazolium, pyridazinium, pyrimidinium, pyrazinium, ammonium, phosphonium, pyridinium, and pyrrolidinium, which are substituted or unsubstituted with an alkyl group having 1 to 15 carbon atoms, and the anion is PF6. - , BF4 - , CF3SO3 - , N(CF3SO2)2 - , N(C2F5SO2)2 - , C(CF2SO2)3 - , AsF6 - , SbF6 - , AlCl4 - , NbF6 - , HSO4 - , ClO4 - , CH3SO3 - and CF3CO2 -For example, the ionic liquid may include one or more selected from the group consisting of 1-ethyl-3-methyl imidazolium, 1-butyl-3-methyl imidazolium, 1-butyl-1-methyl pyrrolidinium, 1-methyl-1-propyl piperidinium, bis(trifluoromethylsulfonyl)imide (TFSI), and trifluoromethanesulfonate.

[0057] The lithium salt can impart ionic conductivity to the polymer solid electrolyte, improving the ionic conductivity without decreasing the electrical conductivity of the electrically conductive polymer.

[0058] The lithium salt may be lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(fluorosulfonyl)imide (LiFSI), LiNO3, LiOH, LiCl, LiBr, LiI, LiClO4, LiBF4, LiB 10 Cl 10 , LiPF6, LiCF3SO3, LiCF3CO2, LiAsF6, LiSbF6, LiAlCl4, CH3SO3Li, CF3SO3Li, LiSCN, LiC(CF3SO2)3, (CF3SO2)2NLi, (FSO2)2NLi, lithium chloroborane, lithium lower aliphatic carboxylate, and lithium 4-phenylborate.

[0059] The weight ratio of the polymer and the non-volatile liquid compound may be 1:0.8 to 1:5.5, specifically, 1:0.8 or less, 1:0.9 or less, or 1:1 or less, or 1:5 or more, 1:5.2 or more, or 1:5.5 or more. If the weight ratio exceeds 1:0.8, the content of the polymer is excessively high, and no phase separation occurs. A free-standing film-type polymer solid electrolyte is produced in a state where the polymer and the non-volatile liquid compound are simply mixed, and the uniformity and ion conductivity of the polymer solid electrolyte may be reduced. If the weight ratio is less than 1:5.5, the content of the non-volatile liquid compound is excessively high, and a liquid electrolyte may be produced instead of a solid polymer electrolyte.

[0060] In addition, the weight ratio of the polymer and the lithium salt may be 1:0.5 to 1:3, specifically, 1:0.5 or less, 1:0.6 or less, or 1:0.7 or less, or 1:1.5 or more, 1:2 or more, or 1:3 or more. If the weight ratio is more than 1:0.5, the content of the polymer may be too high, and the ion conductivity of the polymer solid electrolyte may be reduced, and if the weight ratio is less than 1:3, the content of the lithium salt may be too high, and the polymer electrolyte membrane may not be formed.

[0061] The solvent is not particularly limited as long as it is a solvent used in the art for preparing electrolytes. For example, the solvent may include at least one selected from the group consisting of propylene carbonate (PC), ethylene carbonate (EC), butylene carbonate (BC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propionate (MP), dimethyl sulfoxide, dimethoxyethane, diethoxyethane, tetrahydrofuran, N-methyl-2-pyrrolidone (NMP), ethyl methyl carbonate (EMC), vinylene carbonate (VC), gamma butyrolactone (GBL), fluoroethylene carbonate (FEC), methyl formate, ethyl formate, propyl formate, methyl acetate, ethyl acetate, propyl acetate, pentyl acetate, methyl propionate, ethyl propionate, ethyl propionate, and butyl propionate.

[0062] The concentration of the polymer solid electrolyte forming solution is not particularly limited, and is not particularly limited as long as it is a concentration that can perform a coating process. For example, the concentration of the polymer solid electrolyte forming solution may be 10 to 40 wt%, specifically, 10 wt% or more, 15 wt% or more, or 20 wt% or more, and 30 wt% or less, 35 wt% or less, or 40 wt% or less. It can be appropriately adjusted within the above range so as to be a concentration that can perform a coating process.

[0063] The polymer solid electrolyte forming solution is in a form in which a liquid moiety and a polymer chain are mixed.

[0064] The liquid moiety is derived from the non-volatile liquid compound, and the polymer chain is derived from the polymer. Since the non-volatile liquid compound and the polymer are immiscible with each other, the non-volatile liquid compound and the polymer exist separately in the solution.

[0065] In the present invention, in the step (S2), the solution for forming a polymer solid electrolyte may be applied onto a substrate to form a coating layer.

[0066] The substrate may be in the form of a foil, and the foil may be in the form of a thin metal film such as aluminum, copper, or stainless steel. The use of a foil in the form of a thin metal film as the substrate is advantageous for the preparation of a solid electrolyte in the form of a free-standing film.

[0067] In addition, the coating method may be bar coating, roll coating, spin coating, slit coating, die coating, blade coating, comma coating, slot die coating, lip coating, or solution casting, but is not limited thereto as long as it is a coating method capable of forming a coating layer on the substrate.

[0068] In the present invention, in the step (S3), the coating layer may be dried to separate the coating layer into a liquid phase membrane and a polymer electrolyte membrane.

[0069] The drying method is not particularly limited as long as it can induce phase separation between the liquid portion and the polymer chains contained in the coating layer, and for example, the drying may be performed at 150° C. or less, 130° C. or less, or 110° C. or less.

[0070] The phase separation occurs due to the immiscibility of the polymer and the non-volatile liquid compound, which are the raw materials.

[0071] As shown in FIG. 2, a liquid phase film 20 including the non-volatile liquid compound is formed on a substrate 10, and a polymer solid electrolyte film 30 including a polymer and a lithium salt is formed on the liquid phase film 20.

[0072] In the present invention, in the step (S4), the polymer solid electrolyte membrane may be separated.

[0073] Generally, as a polymer solid electrolyte membrane becomes thinner, its strength weakens, which makes it difficult to separate it from the substrate. However, since a liquid phase membrane is formed between the substrate and the polymer solid electrolyte membrane in the step (S3), the polymer solid electrolyte membrane can be separated from the substrate without any additional resistance.

[0074] In addition, after separating the polymer solid electrolyte membrane, a washing step may be further performed to remove non-volatile liquid compounds remaining on the polymer solid electrolyte membrane.

[0075] Polymer solid electrolyte The present invention also provides a polymer solid electrolyte produced by the above-mentioned method for producing a polymer solid electrolyte.

[0076] The polymer solid electrolyte includes a polymer and a lithium salt, and the types and weight ratios of the polymer and the lithium salt are the same as those described above.

[0077] In the present invention, the thickness of the polymer solid electrolyte may be 23 μm to 35 μm, and the thickness is reduced compared to a general polymer solid electrolyte, and the polymer solid electrolyte may have a thin solid electrolyte form. If the thickness is less than 23 μm, the durability of the polymer solid electrolyte may be reduced, and if the thickness is more than 35 μm, the polymer solid electrolyte may act as a resistor during battery operation.

[0078] In addition, the thickness deviation of the polymer solid electrolyte may be 0.7 μm or less. The smaller the thickness deviation within the range, the better the uniformity. If the thickness deviation exceeds 0.7 μm, the uniformity of the polymer solid electrolyte is poor. For example, the thickness deviation of the polymer solid electrolyte is 3*3 cm 2 The thickness was measured at a total of nine specified positions for the samples punched out to the size of 10 mm, and the deviation between the thickness at the thickest position and the thickness at the thinnest position was calculated. The smaller the deviation in the calculated thickness, the more uniform it was determined to be.

[0079] In the present invention, the polymer solid electrolyte may be in the form of a free-standing film.

[0080] The free-standing film-type polymer solid electrolyte maintains its film shape at room temperature and pressure and can be used in a variety of applications.

[0081] In the present invention, the ionic conductivity of the polymer solid electrolyte is 1.2×10 -5 or 4.5 x 10 -5 The ionic conductivity is measured in S / cm at 80° C. When applied to an all-solid-state battery, a polymer solid electrolyte having the above ionic conductivity can improve the stability and also the performance and life of the battery.

[0082] All solid state battery The present invention also relates to an all-solid-state battery including the above-mentioned polymer solid electrolyte, and the all-solid-state battery may include a positive electrode, a negative electrode, and the polymer solid electrolyte interposed therebetween.

[0083] In addition, the polymer solid electrolyte may be applied to an electrode and attached to one surface of a positive electrode or a negative electrode and included in the all-solid-state battery.

[0084] In the present invention, the positive electrode includes a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector.

[0085] The positive electrode active material layer includes a positive electrode active material, a binder, and a conductive material.

[0086] The positive electrode active material is not particularly limited as long as it is a material capable of reversibly absorbing and releasing lithium ions. For example, lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), Li[Ni x Co y Mn z M v ]O2 (wherein M is any one or more elements selected from the group consisting of Al, Ga, and In; 0.3≦x<1.0, 0≦y, z≦0.5, 0≦v≦0.1, and x+y+z+v=1), Li (Li a M b-a-b' M' b' )O 2-c A c (wherein, 0≦a≦0.2, 0.6≦b≦1, 0≦b'≦0.2, 0≦c≦0.2; M includes Mn and at least one selected from the group consisting of Ni, Co, Fe, Cr, V, Cu, Zn, and Ti; M' is at least one selected from the group consisting of Al, Mg, and B, and A is at least one selected from the group consisting of P, F, S, and N), and compounds substituted with one or more transition metals; 1+y Mn 2-y Lithium manganese oxides such as LiMnO4 (where y is 0-0.33), LiMnO3, LiMn2O3, LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, LiFe3O4, V2O5, Cu2V2O7; with the chemical formula LiNi 1-y Ni-site type lithium nickel oxide represented by MyO2 (where M=Co, Mn, Al, Cu, Fe, Mg, B or Ga, and y=0.01-0.3); chemical formula LiMn 2-y M yExamples of the lithium manganese composite oxides include, but are not limited to, lithium manganese oxides represented by Li2Mn3MO8 (where M=Co, Ni, Fe, Cr, Zn, or Ta, and y=0.01-0.1) or Li2Mn3MO8 (where M=Fe, Co, Ni, Cu, or Zn); LiMn2O4 in which part of the Li in the chemical formula is replaced with an alkaline earth metal ion; disulfide compounds; and Fe2(MoO4)3.

[0087] The positive electrode active material may be included in an amount of 40 to 80 wt % based on the total weight of the positive electrode active material layer. Specifically, the content of the positive electrode active material may be 40 wt % or more, or 50 wt % or more, or 70 wt % or less, or 80 wt % or less. If the content of the positive electrode active material is less than 40 wt %, the connectivity between the wet positive electrode active material layer and the dry positive electrode active material layer may be insufficient, and if it exceeds 80 wt %, the mass transfer resistance may be large.

[0088] The binder is a component that aids in binding the positive electrode active material to the conductive material and to the current collector, and may be any of the following: styrene-butadiene rubber, acrylated styrene-butadiene rubber, acrylonitrile copolymer, acrylonitrile-butadiene rubber, nitrile butadiene rubber, acrylonitrile-styrene-butadiene copolymer, acrylic rubber, butyl rubber, fluororubber, polytetrafluoroethylene, polyethylene, polypropylene, ethylene / propylene copolymer, polybutadiene, polyethylene oxide, chlorosulfonated polyethylene, polyvinylpyrrolidone, polyvinylpyridine, polyvinyl alcohol, polyvinyl acetate, polyepichlorohydrin, polyphosphagen, polyacrylonitrile, polystyrene- ... The binder may include at least one selected from the group consisting of styrene-butadiene rubber, polytetrafluoroethylene, carboxymethylcellulose, polystyrene, latex, acrylic resin, phenolic resin, epoxy resin, carboxymethylcellulose, hydroxypropylcellulose, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethylcellulose, cyanoethylsucrose, polyester, polyamide, polyether, polyimide, polycarboxylate, polycarboxylic acid, polyacrylic acid, polyacrylate, lithium polyacrylate, polymethacrylic acid, polymethacrylate, polyacrylamide, polyurethane, polyvinylidene fluoride, and poly(vinylidene fluoride)-hexafluoropropene. Preferably, the binder may include at least one selected from the group consisting of styrene-butadiene rubber, polytetrafluoroethylene, carboxymethylcellulose, polyacrylic acid, lithium polyacrylate, and polyvinylidene fluoride.

[0089] In addition, the binder may be included in an amount of 1 wt% to 30 wt% based on the total weight of the positive electrode active material layer, and more specifically, the binder content may be 1 wt% or more, or 3 wt% or more, or 15 wt% or less, or 30 wt% or less. If the binder content is less than 1 wt%, the adhesive strength between the positive electrode active material and the positive electrode current collector may be reduced, and if it exceeds 30 wt%, the adhesive strength is improved, but the content of the positive electrode active material may be reduced accordingly, resulting in a lower battery capacity.

[0090] In addition, the conductive material is not particularly limited as long as it prevents side reactions in the internal environment of the all-solid-state battery, does not cause chemical changes in the battery, and has excellent electrical conductivity. Representative examples of the conductive material include graphite and conductive carbon. For example, graphite such as natural graphite and artificial graphite; carbon black such as carbon black, acetylene black, ketjen black, denka black, thermal black, channel black, furnace black, lamp black, and thermal black; carbon-based materials having a graphene or graphite crystal structure; conductive fibers such as carbon fibers and metal fibers; carbon fluoride; metal powders such as aluminum powder and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive oxides such as titanium oxide; and conductive polymers such as polyphenylene derivatives. These may be used alone or in combination, but are not necessarily limited thereto.

[0091] The conductive material may be typically included in an amount of 0.5 wt % to 30 wt % based on the total weight of the positive electrode active material layer, and specifically, the conductive material may be included in an amount of 0.5 wt % or more, or 1 wt % or more, or 20 wt % or less, or 30 wt % or less. If the conductive material is included in an amount of less than 0.5 wt %, the electrical conductivity improvement effect may be difficult to achieve, or the electrochemical properties of the battery may be reduced, and if the conductive material is included in an amount of more than 30 wt %, the amount of the positive electrode active material may be relatively reduced, and the capacity and energy density may be reduced. The method of including the conductive material in the positive electrode is not particularly limited, and a conventional method known in the art, such as coating the positive electrode active material, may be used.

[0092] The positive electrode current collector supports the positive electrode active material layer and serves to transfer electrons between an external conductor and the positive electrode active material layer.

[0093] The positive electrode current collector is not particularly limited as long as it has high electronic conductivity without causing chemical changes in the all-solid-state battery. For example, the positive electrode current collector may be made of copper, stainless steel, aluminum, nickel, titanium, palladium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, silver, or the like, or an aluminum-cadmium alloy.

[0094] The positive electrode current collector may have a fine uneven structure or a three-dimensional porous structure on the surface thereof in order to strengthen the bonding force with the positive electrode active material layer, and thus may include various forms such as a film, a sheet, a foil, a mesh, a net, a porous body, a foam, a nonwoven fabric, etc.

[0095] The positive electrode may be manufactured by a conventional method, specifically, by mixing a positive electrode active material, a conductive material, and a binder in a solvent to prepare a composition for forming a positive electrode active material layer, coating the composition on a positive electrode current collector, drying the composition, and optionally compressing the composition into a current collector to improve the electrode density. At this time, it is preferable to use a solvent that can uniformly disperse the positive electrode active material, the binder, and the conductive material and that can be easily evaporated. Specifically, acetonitrile, methanol, ethanol, tetrahydrofuran, water, isopropyl alcohol, etc. may be used.

[0096] In the present invention, the negative electrode includes a negative electrode current collector and a negative electrode active material layer formed on the negative electrode current collector. The negative electrode active material layer includes a negative electrode active material, a binder, and a conductive material.

[0097] The negative electrode active material is lithium (Li + The lithium-containing compound may include a material capable of reversibly intercalating or deintercalating lithium ions, a material capable of reversibly reacting with lithium ions to form a lithium-containing compound, lithium metal, or a lithium alloy.

[0098] The lithium ion (Li +The material capable of reversibly inserting or de-inserting lithium ions (Li) may be, for example, crystalline carbon, amorphous carbon, or a mixture thereof. + The material capable of reacting with lithium (Li) to reversibly form a lithium-containing compound may be, for example, tin oxide, titanium nitride, or silicon. The lithium alloy may be, for example, an alloy of lithium (Li) and a metal selected from the group consisting of sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), francium (Fr), beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), radium (Ra), aluminum (Al), and tin (Sn).

[0099] Preferably, the negative electrode active material is lithium metal, and specifically, may be in the form of a lithium metal thin film or lithium metal powder.

[0100] The negative active material may be included in an amount of 40 to 80 wt % based on the total weight of the negative active material layer. Specifically, the content of the negative active material may be 40 wt % or more, or 50 wt % or more, or 70 wt % or less, or 80 wt % or less. If the content of the negative active material is less than 40 wt %, the connectivity between the wet negative active material layer and the dry negative active material layer may be insufficient, and if it exceeds 80 wt %, the mass transfer resistance may be large.

[0101] The binder is as described above in the positive electrode active material layer.

[0102] The conductive material is as described above in the positive electrode active material layer.

[0103] In addition, the negative electrode current collector is not particularly limited as long as it has conductivity without causing a chemical change in the battery, and for example, the negative electrode current collector may be made of copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., aluminum-cadmium alloy, etc. In addition, the negative electrode current collector may be in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc., having fine irregularities formed on the surface, similar to the positive electrode current collector.

[0104] The method for manufacturing the negative electrode is not particularly limited, and the negative electrode may be manufactured by forming a negative electrode active material layer on a negative electrode current collector using a method for forming a layer or film commonly used in the art, such as squeezing, coating, deposition, etc. In addition, the negative electrode of the present invention also includes a case where a thin lithium film is formed on a metal plate by initial charging after assembling a battery without a thin lithium film on the negative electrode current collector.

[0105] The method for producing the all-solid-state battery having the above-mentioned configuration is not particularly limited in the present invention, and any known method can be used.

[0106] When manufacturing the all-solid-state battery of the present invention, electrodes including a positive electrode and a negative electrode are arranged, and then the resulting structure is pressure-molded to assemble a cell.

[0107] The assembled cell is placed in an exterior material and then sealed by heating and squeezing, etc. As the exterior material, a laminate pack of aluminum, stainless steel, etc., or a cylindrical or rectangular metal container is very suitable.

[0108] Below, preferred examples are presented to aid in understanding the present invention. However, the following examples are merely illustrative of the present invention, and it will be obvious to those skilled in the art that various changes and modifications are possible within the scope of the scope and technical ideas of the present invention, and it is natural that such changes and modifications fall within the scope of the appended claims.

[0109] In the following Examples and Comparative Examples, solid electrolytes were prepared using the types and weight ratios of the base material, polymer, lithium salt, and solvent as shown in Table 1 below.

[0110] [Table 1]

[0111] Example 1 As raw materials for manufacturing a polymer solid electrolyte, a polymer polypropylene carbonate (PPC), a non-volatile liquid compound poly(ethylene glycol)-polyhedral oligomeric silsesquioxane (PEG-POSS), a lithium salt LiTFSI, and a solvent NMP were prepared. The weight ratio of the polymer PPC, the non-volatile liquid compound PEG-POSS, and the lithium salt LiTFSI was 1:1:1.

[0112] The polymer, the non-volatile liquid compound, and the lithium salt were added to a solvent and mixed to prepare a 20% solution for forming a polymer solid electrolyte.

[0113] The polymer solid electrolyte forming solution was bar coated on a stainless steel (SS) foil substrate to form a coating layer.

[0114] The coating layer was then vacuum dried at 100° C. During drying, phase separation occurred, and a laminate was produced in which a liquid phase film containing the non-volatile liquid compound and a polymer solid electrolyte film containing the polymer and lithium salt were sequentially formed on the SS foil. The SS foil was separated from the laminate to obtain a polymer solid electrolyte including a liquid phase film and a polymer solid electrolyte film formed on the liquid phase film.

[0115] Example 2 A polymer solid electrolyte was prepared in the same manner as in Example 1, except that the weight ratio of PPC and PEG-POSS used in the polymer and non-volatile liquid compound was 1:2.

[0116] Example 3 A polymer solid electrolyte was prepared in the same manner as in Example 1, except that the weight ratio of PPC and PEG-POSS used in the polymer and non-volatile liquid compound was 1:5.

[0117] Comparative Example 1 A polymer solid electrolyte was prepared in the same manner as in Example 1, except that the non-volatile liquid compound was not used.

[0118] Comparative Example 2 A polymer solid electrolyte was prepared in the same manner as in Example 1, except that a non-volatile liquid compound was not used and a polyethylene terephthalate (PET) release film was used instead of SS foil as a substrate.

[0119] Comparative Example 3 A polymer solid electrolyte was prepared in the same manner as in Example 1, except that the weight ratio of PPC and PEG-POSS used in the polymer and non-volatile liquid compound was 1:6.

[0120] Comparative Example 4 A polymer solid electrolyte was prepared in the same manner as in Example 1, except that the weight ratio of PPC and PEG-POSS used in the polymer and non-volatile liquid compound was 1:0.5.

[0121] Experimental Example 1: Evaluation of polymer solid electrolyte The polymer solid electrolytes prepared in the examples and comparative examples were measured for free-standing film form, thickness, uniformity, and ionic conductivity by the following methods, and the results are shown in Table 2 below.

[0122] (1) Possibility of free-standing film It was confirmed whether the polymer solid electrolyte membrane could be separated from the substrate and obtained as a membrane, and whether the polymer solid electrolyte could be formed into a free-standing film was evaluated.

[0123] (2) Thickness As shown in Figure 3, the prepared polymer solid electrolyte was placed on a 3 x 3 cm 2 The thickness of the samples punched out to the size of 100 mm was measured at a total of 9 specified positions, and the average thickness was calculated.

[0124] (3) Uniformity The deviation between the thicknesses was calculated for the total thickness measurements at the nine specified positions obtained in (2). The smaller the deviation in the calculated thickness, the more uniform it was determined to be.

[0125] (4) Ionic conductivity The polymer solid electrolyte sample obtained in (3) was contacted with a SS metal electrode having the same surface area as the sample, and an AC voltage was applied through the electrodes on both sides of the sample at room temperature. At this time, the applied condition was set to a measurement frequency in the amplitude range of 0.01 Hz to 1 MHz, and the impedance was measured using BioLogic's VMP3. The resistance of the polymer solid electrolyte was calculated from the intersection (Rb) where the semicircle or straight line of the measured impedance locus meets the real axis, and the ionic conductivity of the polymer solid electrolyte at 80°C was calculated from the area and thickness of the sample.

[0126] [Formula 1]

number

[0127] [Table 2]

[0128] As shown in Table 2, it was confirmed that the polymer solid electrolytes of Examples 1 to 3, which were prepared using the polymer PPC and the non-volatile liquid compound PEG-POSS in an appropriate weight ratio, were prepared in the form of a free-standing film. In addition, it was confirmed that the polymer solid electrolytes of Examples 1 to 3 were prepared uniformly with little deviation in thickness and had excellent ion conductivity. In addition, the polymer solid electrolyte of Comparative Example 1 was prepared without using a non-volatile liquid compound, and was not prepared in the form of a free-standing film, so the thickness and ion conductivity could not be measured.

[0129] In addition, in Comparative Example 2, a polymer solid electrolyte was prepared in the form of a free-standing film using a PET release film instead of a SS foil as a substrate without using a non-volatile liquid compound, but it was confirmed that the thickness deviation was large and the uniformity was poor, and the ion conductivity was relatively lower than in Examples 1 to 3. In general, compared to metal foils such as SS, Cu, or Al, a PET release film has a low adhesive strength with an electrolyte membrane prepared on a metal foil, making it relatively easy to separate the electrolyte membrane after drying, but if the strength of the electrolyte membrane is weak, it may break or become deformed, making it difficult to use.

[0130] On the other hand, in Comparative Example 3, the non-volatile liquid compound PEG-POSS was used in an excessive amount compared to the polymer PPC, and the film was not produced in the form of a membrane but existed in a liquid state, which made it impossible to measure the thickness, uniformity and ionic conductivity.

[0131] In addition, in Comparative Example 4, the amount of the non-volatile liquid compound PEG-POSS was very small compared to the amount of the polymer PPC, and it was confirmed that a film containing the polymer and the non-volatile liquid compound in a mixed state was formed without phase separation between the polymer and the non-volatile liquid compound, resulting in a large thickness deviation and poor uniformity.

[0132] From these results, it was confirmed that when a polymer and a non-volatile liquid compound that are not well miscible are used in an appropriate weight ratio and a polymer solid electrolyte is prepared by phase separation between the polymer and the non-volatile liquid compound, a free-standing film-type polymer solid electrolyte including a liquid phase membrane and a polymer solid electrolyte membrane formed by phase separation between the polymer and the non-volatile liquid compound is prepared, and the polymer solid electrolyte has excellent uniformity and ionic conductivity.

[0133] Although the present invention has been described above with reference to limited embodiments and drawings, the present invention is not limited thereto, and it is of course possible for a person having ordinary skill in the art to which the present invention pertains to make various modifications and variations within the technical spirit of the present invention and the equivalent scope of the following claims. [Explanation of symbols]

[0134] 1:Polymer solid electrolyte 10: Base material 20: Liquid membrane 30:Polymer solid electrolyte membrane

Claims

1. (S1) preparing a solution for forming a polymer solid electrolyte by adding a polymer, a non-volatile liquid compound, and a lithium salt to a solvent; (S2) applying the polymer solid electrolyte forming solution onto a substrate to form a coating layer; (S3) drying the coating layer to separate it into a liquid phase membrane and a polymer solid electrolyte membrane; (S4) separating the polymer solid electrolyte membrane; the liquid phase membrane is formed on a substrate, and the polymer solid electrolyte membrane is formed on the liquid phase membrane, In the solution for forming a polymer solid electrolyte, the weight ratio of the polymer to the non-volatile liquid compound is 1:0.8 to 1:5.

5.

2. the liquid phase film contains the non-volatile liquid compound, the polymer solid electrolyte film contains the polymer and a lithium salt, The method for producing a polymer solid electrolyte according to claim 1 , wherein the non-volatile liquid compound is immiscible with the polymer.

3. 2. The method of claim 1, wherein the polymer comprises at least one selected from the group consisting of polypropylene carbonate (PPC), polyacrylonitrile (PAN), and polyvinylpyrrolidone (PVP).

4. 2. The method for producing a polymer solid electrolyte according to claim 1, wherein the non-volatile liquid compound comprises at least one selected from the group consisting of polyhedral oligomeric silsesquioxane (POSS) and an ionic liquid.

5. 5. The method for producing a polymer solid electrolyte according to claim 4, wherein the POSS comprises one or more functional groups (R), the functional groups being functional groups containing one or more elements selected from the group consisting of O, N, S, Si, and P, or functional groups capable of bonding with lithium ions.

6. 6. The method of claim 5, wherein the functional group is poly(ethylene glycol) (PEG), alcohol, amine, carboxylic acid, allyl, epoxide, thiol, silane, or silanol.

7. The ionic liquid includes a cation and an anion, and the cation includes at least one selected from the group consisting of imidazolium, pyrazolium, triazolium, thiazolium, oxazolium, pyridazinium, pyrimidinium, pyrazinium, ammonium, phosphonium, pyridinium, and pyrrolidinium, which are substituted or unsubstituted by an alkyl group having 1 to 15 carbon atoms; The anion is PF 6 - , B.F. 4 - , C.F. 3 SO 3 - , N(CF 3 SO 2 ) 2 - , N(C 2 F 5 SO 2 ) 2 - , C(CF 2 SO 2 ) 3 - , AsF 6 - , SbF 6 - , AlCl 4 - , NbF 6 - , H.S.O. 4 - , ClO 4 - , C.H. 3 SO 3 - and C.F. 3 CO 2 - The method for producing a polymer solid electrolyte according to claim 4, wherein the polymer solid electrolyte contains one or more selected from the group consisting of:

8. The lithium salt includes lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(fluorosulfonyl)imide (LiFSI), and LiNO 3 , LiOH, LiCl, LiBr, LiI, LiClO 4 , LiBF 4 , LiB 10 C 10 , LiPF 6 , LiCF 3 SO 3 , LiCF 3 CO 2 , LiAsF 6 , LiSbF 6 , LiAlCl 4 , C.H. 3 SO 3 Li, C.F. 3 SO 3 Li, LiSCN, LiC(CF 3 SO 2 ) 3 , (CF 3 SO 2 ) 2 NLi and (FSO 2 ) 2 2. The method for producing a polymer solid electrolyte according to claim 1, wherein the polymer solid electrolyte comprises one or more selected from the group consisting of NLi,

9. 2. The method for producing a polymer solid electrolyte according to claim 1, wherein the substrate comprises at least one selected from the group consisting of stainless steel, Cu foil, and Al foil.

10. 2. The method of claim 1, wherein the coating layer is formed by bar coating, roll coating, spin coating, slit coating, die coating, blade coating, comma coating, slot die coating, lip coating, or solution casting.

11. 2. The method of claim 1, wherein the weight ratio of the polymer to the lithium salt is 1:0.5 to 1:

3.

12. The method for producing a polymer solid electrolyte according to claim 1, wherein the solvent is at least one selected from the group consisting of propylene carbonate (PC), ethylene carbonate (EC), butylene carbonate (BC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propionate (MP), dimethyl sulfoxide, dimethoxyethane, diethoxyethane, tetrahydrofuran, N-methyl-2-pyrrolidone (NMP), ethyl methyl carbonate (EMC), vinylene carbonate (VC), gamma butyrolactone (GBL), fluoroethylene carbonate (FEC), methyl formate, ethyl formate, propyl formate, methyl acetate, ethyl acetate, propyl acetate, pentyl acetate, methyl propionate, ethyl propionate, ethyl propionate, and butyl propionate.

13. The method for preparing a polymer solid electrolyte according to claim 1, wherein the coating layer is dried at a temperature of 150° C. or less.

Citation Information

Patent Citations

  • Electrolyte, method of preparing the same, and lithium secondary battery comprising the same

    JP2016062895A

  • Polymer solid electrolyte and lithium secondary battery containing the same

    JP2019526908A

  • Composite solid electrolyte membrane for all-solid-state battery and all-solid-state battery including the same

    JP2020526897A

  • Lithium ion secondary battery

    JP2021157983A