Positive electrode active material for non-aqueous electrolyte secondary battery, and non-aqueous electrolyte secondary battery
The positive electrode active material with a spinel structure and surface-enriched Ge concentration addresses discharge capacity reduction, achieving higher voltage operation and improved performance in non-aqueous electrolyte secondary batteries.
Patent Information
- Application Number
- JP2021551285
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-09-30
- Filing Date
- 2020-09-29
- Publication Date
- 2024-09-24
- Estimated Expiration
- 2040-09-29
AI Technical Summary
Existing positive electrode active materials for non-aqueous electrolyte secondary batteries face issues such as reduced discharge capacity due to electrochemically inactive additives and surface coatings, limiting their performance at high voltages.
A positive electrode active material with a spinel structure, formulated as Li1+αNi0.5-xMn1.5-y-zGe y M x+zO4, where Ge is concentrated at the surface and less concentrated at the center, enhancing the discharge capacity while allowing operation at high voltages.
The proposed active material increases discharge capacity and enables operation at higher voltages by suppressing oxygen defects and maintaining electrochemical activity, outperforming conventional materials.
Smart Images

Figure 0007555000000002 
Figure 0007555000000001
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a positive electrode active material for a non-aqueous electrolyte secondary battery, and a non-aqueous electrolyte secondary battery using the positive electrode active material. [Background technology]
[0002] Lithium transition metal composite oxides containing Li, Ni, and Mn and having a spinel structure have been attracting attention as positive electrode active materials because they can be used at high voltages and Mn is abundantly available. Patent Document 1 discloses a positive electrode active material in which part of the Ni and Mn in lithium nickel manganese oxide is replaced with other metal elements and contains F in order to prevent deterioration of battery characteristics at high temperatures. Patent Document 2 discloses a positive electrode active material made of lithium manganese oxide having a spinel structure and a two-layer structure with different compositions on the surface and inside in order to prevent deterioration of battery characteristics. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2017-33817 A [Patent Document 2] Special Publication No. 2008-535173 Summary of the Invention
[0004] The positive electrode active material disclosed in Patent Document 1 may reduce the discharge capacity of the battery depending on the metal element substituted. Also, the positive electrode active material disclosed in Patent Document 2 has an electrochemically inactive surface coating layer, which may reduce the discharge capacity of the battery.
[0005] The positive electrode active material for a non-aqueous electrolyte secondary battery according to one embodiment of the present disclosure has a spinel structure and is represented by the general formula Li 1+α Ni 0.5-x Mn 1.5-y-z Ge y M x+zO4 (where 0 ≦ α < 0.2, 0 ≦ x < 0.2, 0 < y < 0.45, 0 ≦ z < 0.2, and M is at least one element selected from Mg, Al, Sc, Ti, Cr, V, Fe, and Co). The lithium transition metal composite oxide contains. In the secondary particles of the lithium transition metal composite oxide, when the total number of moles of metal elements other than Li in the surface portion is 2, the number of moles of Ge (Ge surf ) is higher than the number of moles of Ge (Ge bulk ) when the total number of moles of metal elements other than Li in the central portion is 2.
[0006] A non-aqueous electrolyte secondary battery according to one aspect of the present disclosure includes a positive electrode containing the positive electrode active material for the non-aqueous electrolyte secondary battery, a negative electrode, and a non-aqueous electrolyte.
[0007] According to one aspect of the present disclosure, it is possible to increase the voltage of the secondary battery while increasing the discharge capacity.
Brief Description of the Drawings
[0008] [Figure 1] FIG. 1 is a perspective view of a secondary battery as an example of an embodiment, showing the internal structure of a battery case with the front side of the exterior removed.
Modes for Carrying Out the Invention
[0009] Theoretically, lithium transition metal composite oxides containing Li, Ni, and Mn and having a spinel structure can be charged and discharged at about 4.7 V, but because oxygen deficiency is likely to occur during synthesis of the lithium transition metal composite oxide, the capacity that can be charged and discharged at a voltage of 4.5 V or more is actually limited. As disclosed in Patent Document 1, it is effective to add an additive element to the lithium transition metal composite oxide to suppress the occurrence of oxygen deficiencies during synthesis, but since many of the additive elements are electrochemically inactive, the actual capacity may decrease. In addition, the positive electrode active material disclosed in Patent Document 2 has a coating layer on the surface that is electrochemically inactive, and the discharge capacity of the battery may decrease. The inventors of the present application have found that a secondary battery that can be used at a high voltage of 4.5 V or more and has a large discharge capacity can be obtained by using a positive electrode active material that contains a lithium transition metal composite oxide containing Li, Ni, Mn, and Ge and having a spinel structure, and in which the mole fraction of Ge on the surface is greater than the mole fraction of Ge in the center. This is presumably because the occurrence of oxygen defects is suppressed by containing a large amount of Ge on the surface, while the decrease in battery capacity is suppressed by containing a small amount of Ge in the center.
[0010] An example of an embodiment of the present disclosure will be described in detail below. In this embodiment, a secondary battery 100 including a rectangular metal exterior body 1 is illustrated, but the exterior body is not limited to a rectangular shape and may be, for example, cylindrical. In addition, a wound electrode body 3 is illustrated, but a laminated electrode body in which multiple positive electrodes and multiple negative electrodes are alternately laminated one by one with separators interposed therebetween may also be used. In addition, in both the positive and negative electrodes, a case in which each composite layer is formed on both sides of each core body is illustrated, but each composite layer is not limited to being formed on both sides of each core body, and may be formed on at least one surface.
[0011] 1, the secondary battery 100 includes a wound electrode assembly 3 formed in a flat shape having a flat portion and a pair of curved portions by winding a positive electrode and a negative electrode with a separator interposed therebetween, an electrolyte, and an exterior body 1 that contains the electrode assembly 3 and the electrolyte. Both the exterior body 1 and the sealing plate 2 are made of metal, and are preferably made of aluminum or an aluminum alloy.
[0012] The exterior body 1 has a bottom part that is generally rectangular in bottom view, and side walls that stand on the periphery of the bottom part. The side walls are formed perpendicular to the bottom part. The dimensions of the exterior body 1 are not particularly limited, but an example is a lateral length of 60 to 160 mm, a height of 60 to 100 mm, and a thickness of 10 to 40 mm.
[0013] The positive electrode is a long body having a metallic positive electrode core and a positive electrode composite layer formed on both sides of the core, and a strip-shaped positive electrode core exposed portion 4 is formed at one end in the short direction, where the positive electrode core is exposed along the longitudinal direction. Similarly, the negative electrode is a long body having a metallic negative electrode core and a negative electrode composite layer formed on both sides of the core, and a strip-shaped negative electrode core exposed portion 5 is formed at one end in the short direction, where the negative electrode core is exposed along the longitudinal direction. The electrode body 3 has a structure in which the positive electrode and negative electrode are wound with a separator interposed between them, with the positive electrode core exposed portion 4 of the positive electrode arranged at one axial end and the negative electrode core exposed portion 5 of the negative electrode arranged at the other axial end.
[0014] A positive electrode current collector 6 is connected to the lamination portion of the positive electrode core exposed portion 4 of the positive electrode, and a negative electrode current collector 8 is connected to the lamination portion of the negative electrode core exposed portion 5 of the negative electrode. The positive electrode current collector 6 is preferably made of aluminum or an aluminum alloy. The negative electrode current collector 8 is preferably made of copper or a copper alloy. The positive electrode terminal 7 has a positive electrode external conductive portion 13 arranged on the battery exterior side of the sealing plate 2, a positive electrode bolt portion 14 connected to the positive electrode external conductive portion 13, and a positive electrode insertion portion 15 inserted into a through hole provided in the sealing plate 2, and is electrically connected to the positive electrode current collector 6. The negative electrode terminal 9 has a negative electrode external conductive portion 16 arranged on the battery exterior side of the sealing plate 2, a negative electrode bolt portion 17 connected to the negative electrode external conductive portion 16, and a negative electrode insertion portion 18 inserted into a through hole provided in the sealing plate 2, and is electrically connected to the negative electrode current collector 8.
[0015] The positive electrode terminal 7 and the positive electrode current collector 6 are fixed to the sealing plate 2 via an internal insulating member and an external insulating member, respectively. The internal insulating member is disposed between the sealing plate 2 and the positive electrode current collector 6, and the external insulating member is disposed between the sealing plate 2 and the positive electrode terminal 7. Similarly, the negative electrode terminal 9 and the negative electrode current collector 8 are fixed to the sealing plate 2 via an internal insulating member and an external insulating member, respectively. The internal insulating member is disposed between the sealing plate 2 and the negative electrode current collector 8, and the external insulating member is disposed between the sealing plate 2 and the negative electrode terminal 9.
[0016] The electrode body 3 is housed in the exterior body 1. The sealing plate 2 is connected to the opening edge of the exterior body 1 by laser welding or the like. The sealing plate 2 has an electrolyte injection hole 10, which is sealed with a sealing plug after the electrolyte is injected into the exterior body 1. The sealing plate 2 is formed with a gas exhaust valve 11 for exhausting gas when the pressure inside the battery reaches or exceeds a predetermined value.
[0017] The electrolyte is a non-aqueous electrolyte containing a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. For example, carbonates, lactones, ethers, ketones, esters, etc. can be used as the non-aqueous solvent, and two or more of these solvents can be mixed and used. When two or more solvents are mixed and used, it is preferable to use a mixed solvent containing a cyclic carbonate and a chain carbonate. For example, ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), etc. can be used as the cyclic carbonate, and dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), etc. can be used as the chain carbonate. The non-aqueous solvent may contain a halogen-substituted product in which at least a part of the hydrogen of the above-mentioned solvent is replaced with a halogen atom such as fluorine. For the electrolyte salt, LiPF6, LiBF4, LiCF3SO3, etc., and mixtures thereof can be used. The amount of electrolyte salt dissolved in the non-aqueous solvent can be, for example, 0.5 to 2.0 mol / L. In addition, additives such as vinylene carbonate (VC) can be added as appropriate. The electrolyte is not limited to a liquid electrolyte, and may be a solid electrolyte using a gel polymer or the like.
[0018] The positive electrode, negative electrode, and separator that constitute the electrode assembly 3 will be described in detail below, in particular the positive electrode active material that constitutes the positive electrode.
[0019] [Positive electrode] The positive electrode has a positive electrode core and a positive electrode composite layer provided on the surface of the positive electrode core. For the positive electrode core, a foil of a metal such as aluminum that is stable in the potential range of the positive electrode, a film with the metal disposed on the surface layer, or the like can be used. The positive electrode composite layer contains a positive electrode active material, a binder, and a conductive material, and is preferably provided on both sides of the positive electrode core except for the positive electrode core exposed portion 4. The positive electrode can be produced, for example, by applying a positive electrode composite slurry containing a positive electrode active material, a binder, a conductive material, and the like to the surface of the positive electrode core, drying the coating, and then compressing it to form a positive electrode composite layer on both sides of the positive electrode core.
[0020] Examples of the conductive material contained in the positive electrode composite layer include carbon materials such as carbon black, acetylene black, ketjen black, and graphite. Examples of the binder contained in the positive electrode composite layer include fluororesins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyimide, acrylic resin, and polyolefin. These resins may be used in combination with cellulose derivatives such as carboxymethyl cellulose (CMC) or its salts, polyethylene oxide (PEO), and the like.
[0021] The positive electrode active material has a spinel structure and has the general formula Li 1+α Ni 0.5-x Mn 1.5-y-z Ge y M x+z O4 (where 0 ≦ α < 0.2, 0 ≦ x < 0.2, 0 < y < 0.45, 0 ≦ z < 0.2, and M is at least one element selected from Mg, Al, Sc, Ti, Cr, V, Fe, and Co). In the lithium transition metal composite oxide, Li, Ni, Mn, and Ge are essential components, and M is an optional component. By satisfying 0 ≦ x < 0.2 and 0 < y < 0.45 for the contents of Ni and Mn, the lithium transition metal composite oxide can be used at high voltages. The fact that the lithium transition metal composite oxide has a spinel structure can be confirmed by X-ray diffraction (XRD). Further, the molar fractions of the respective elements constituting the lithium transition metal composite oxide are measured by inductively coupled plasma (ICP) optical emission spectrometry. Hereinafter, for convenience of explanation, the above lithium transition metal composite oxide is referred to as "composite oxide (Z)". The positive electrode active material may contain the composite oxide (Z) as a main component and may be substantially composed of only the composite oxide (Z). The positive electrode active material may contain a composite oxide other than the composite oxide (Z) or other compounds as long as the object of the present disclosure is not impaired.
[0022] The composite oxide (Z) is, for example, a secondary particle formed by agglomeration of a plurality of primary particles. The particle size of the primary particles constituting the secondary particles is, for example, 0.05 μm to 1 μm. The particle size of the primary particles is measured as the diameter of the circumscribed circle in a particle image observed by a scanning electron microscope (SEM).
[0023] The composite oxide (Z) is a particle having a volume-based median diameter (D50) of, for example, 3 μm to 30 μm, preferably 5 μm to 25 μm, and particularly preferably 7 μm to 15 μm. D50 means a particle diameter at which the cumulative frequency is 50% from the smallest particle diameter in the volume-based particle size distribution, and is also called the median diameter. The particle size distribution of the composite oxide (Z) can be measured using a laser diffraction type particle size distribution measuring device (e.g., MT3000II manufactured by Microtrack Bell Co., Ltd.) with water as a dispersion medium.
[0024] In the composite oxide (Z), the number of moles of Ge when the total number of moles of metal elements other than Li in the surface area is taken as 2 (Ge surf ) is the number of moles of Ge when the total number of moles of metal elements other than Li in the central part is 2 (Ge bulk ) is higher. This allows the discharge capacity to be increased while increasing the voltage of the secondary battery. Here, in the cross section of the composite oxide (Z), the part that is 1 / 3 the thickness of the radius from the center is referred to as the central part, and the part that is 1 / 3 the thickness of the radius from the surface is referred to as the surface part. The composite oxide (Z) may have a gradation structure in which the mole fraction of Ge relative to the total mole number of metal elements other than Li increases from the surface toward the inside. Ge surf and Ge bulk can be measured by an electron probe microanalyzer (EPMA).
[0025] Ge bulk For Ge surf Ratio of (Ge surf / Ge bulk ) is 1.5 <Ge surf / Ge bulk <5.0 relationship may be satisfied. surf / Ge bulkWhen the amount of Ge falls within this range, the discharge capacity can be increased. surf / Ge bulk If the surface area is smaller than this range, oxygen deficiency is likely to occur on the particle surface, resulting in a decrease in discharge capacity, whereas if the surface area is larger than this range, the particle surface becomes electrochemically inactive, resulting in an increase in resistance.
[0026] Ge bulk is 0.005 <Ge bulk <0.45 may be satisfied. bulk When the amount of the ion exchange material falls within this range, the voltage of the battery can be increased. bulk If it is smaller than this range, the voltage improvement effect cannot be obtained satisfactorily. bulk If the capacitance is greater than this range, the material becomes electrochemically inactive, causing an increase in resistance, etc.
[0027] The composite oxide (Z) can be prepared, for example, by the following procedure. (1) A Li source such as lithium hydroxide (LiOH) is added to a composite compound (X) that does not contain Li, and the resulting mixture is fired to synthesize a lithium composite oxide (Y). An example of the composite compound (X) is a composite oxide or hydroxide that contains Ni and Mn. (2) Lithium composite oxide (Y) containing GeO2, GeCl4, tetramethoxygermanium, tetraethoxygermanium, and LiNi 0.5 Ge 1.5 O4, LiCo 0.5 Ge 1.5 O4, LiZn 0.5 Ge 1.5 A Ge source such as O4, GeMnO3, GeCoO3, GeMn2O4, or GeCo2O4 is added, mixed, and then fired to dissolve Ge in the lithium composite oxide (Y) to synthesize the composite oxide (Z). At this time, a Li source such as LiOH may be added together with the Ge source.
[0028] In the above step (2), the firing temperature is, for example, 700° C. to 1200° C., and the firing time is, for example, 10 minutes to 10 hours. By adjusting the firing temperature and firing time, the distribution state of Ge dissolved in the composite oxide (Z) can be changed. surf and Ge bulk The lower the firing temperature and the shorter the firing time, the more Ge remains near the surface and does not penetrate into the interior, so the Ge surf / Ge bulk The value of becomes larger.
[0029] [Negative electrode] The negative electrode has a negative electrode core and a negative electrode composite layer provided on the surface of the negative electrode core. For the negative electrode core, a foil of a metal such as copper that is stable in the potential range of the negative electrode, a film with the metal disposed on the surface layer, or the like can be used. The negative electrode composite layer contains a negative electrode active material and a binder, and is preferably provided on both sides of the negative electrode core except for the negative electrode core exposed portion 5. The negative electrode can be produced, for example, by applying a negative electrode composite slurry containing a negative electrode active material and a binder to the surface of the negative electrode core, drying the coating, and then compressing it to form a negative electrode composite layer on both sides of the negative electrode core.
[0030] The negative electrode mixture layer contains, as the negative electrode active material, for example, a carbon-based active material that reversibly absorbs and releases lithium ions. Suitable carbon-based active materials are graphites such as natural graphite, such as flake graphite, lump graphite, and earthy graphite, and artificial graphite, such as lump artificial graphite (MAG) and graphitized mesophase carbon microbeads (MCMB). In addition, the negative electrode active material may be a Si-based active material composed of at least one of Si and a Si-containing compound, or a carbon-based active material and a Si-based active material may be used in combination.
[0031] The binder contained in the negative electrode mixture layer may be fluororesin, PAN, polyimide, acrylic resin, polyolefin, etc., as in the case of the positive electrode, but it is preferable to use styrene-butadiene rubber (SBR). In addition, it is preferable that the negative electrode mixture layer further contains CMC or a salt thereof, polyacrylic acid (PAA) or a salt thereof, polyvinyl alcohol (PVA), etc. Among them, it is preferable to use SBR in combination with CMC or a salt thereof, and PAA or a salt thereof.
[0032] [Separator] The separator is a porous sheet having ion permeability and insulation. Specific examples of the porous sheet include a microporous thin film, a woven fabric, and a nonwoven fabric. The separator is preferably made of a polyolefin such as polyethylene or polypropylene, or cellulose. The separator may have either a single-layer structure or a laminated structure. A heat-resistant layer or the like may be formed on the surface of the separator.
[0033] <Example> The present disclosure will be further described below with reference to examples, but the present disclosure is not limited to these examples.
[0034] <Example 1> [Synthesis of positive electrode active material] Obtained by coprecipitation, D50 is 12μm and composition is Ni 0.5 Mn 1.5 Nickel manganese composite hydroxide (OH)4 was calcined at 500°C to obtain nickel manganese composite oxide (X).
[0035] Next, LiOH and nickel manganese composite oxide (X) were mixed so that the total molar ratio of Li, Ni, and Mn was 1.02:1. This mixture was fired at 700°C in an oxygen atmosphere for 8 hours and then pulverized to obtain lithium composite oxide (Y). XRD confirmed that the lithium composite oxide (Y) had a spinel structure. In addition, the composition of the lithium composite oxide (Y) was analyzed by ICP, and the results were LiNi 0.5 Mn 1.5 He was O4.
[0036] Next, the lithium composite oxide (Y) and GeO2 were dry mixed so that the molar ratio of the total amount of Ni and Mn in the lithium composite oxide (Y) to the amount of Ge in GeO2 was 2:0.136. This mixture was baked at 1000°C for 30 minutes in air and then pulverized to obtain a positive electrode active material in which Ge was dissolved in the lithium composite oxide (Y). Measurement by EPMA showed that Ge bulk The value of is 0.082, and Ge surf / Ge bulk The value of was 2.1. In addition, the composition of the positive electrode active material was analyzed by ICP, and it was found to be LiNi 0.5 Mn 1.5 Ge 0.136 It was confirmed by XRD that the obtained positive electrode active material had a spinel structure.
[0037] [Preparation of positive electrode] The positive electrode active material, acetylene black, and polyvinylidene fluoride (PVdF) were mixed in a solid content mass ratio of 96.3:2.5:1.2, and an appropriate amount of N-methyl-2-pyrrolidone (NMP) was added, followed by kneading to prepare a positive electrode composite slurry. The positive electrode composite slurry was applied to both sides of a positive electrode core made of aluminum foil, and the coating was dried. The coating was then rolled using a roller and cut to a predetermined electrode size to obtain a positive electrode in which a positive electrode composite layer was formed on both sides of the positive electrode core. An exposed portion was provided in part of the positive electrode, exposing the surface of the positive electrode core.
[0038] [Preparation of negative electrode] Natural graphite was used as the negative electrode active material. The negative electrode active material, sodium carboxymethylcellulose (CMC-Na), and styrene-butadiene rubber (SBR) were mixed in an aqueous solution at a solid content mass ratio of 100:1:1 to prepare a negative electrode composite slurry. The negative electrode composite slurry was applied to both sides of a negative electrode core made of copper foil, and the coating film was dried. The coating film was then rolled using a roller and cut to a predetermined electrode size to obtain a negative electrode in which a negative electrode composite layer was formed on both sides of the negative electrode core. An exposed portion was provided in part of the negative electrode, where the surface of the negative electrode core was exposed.
[0039] [Preparation of non-aqueous electrolyte] Lithium hexafluorophosphate (LiPF6) was dissolved at a concentration of 1.0 mol / L in a mixed solvent of fluoroethylene carbonate (FEC) and methyl 3,3,3-trifluoropropionate (FMP) in a volume ratio of 2:8. Furthermore, vinylene carbonate (VC) was dissolved at a concentration of 2.0 mass% in the mixed solvent to prepare a non-aqueous electrolyte.
[0040] [Battery construction] An aluminum lead was attached to the exposed part of the positive electrode, and a nickel lead was attached to the exposed part of the negative electrode, and the positive and negative electrodes were spirally wound with a polyolefin separator interposed therebetween, and then pressed in the radial direction to produce a flat wound electrode body. This electrode body was housed in an exterior body made of an aluminum laminate sheet, and the nonaqueous electrolyte was injected, and the opening of the exterior body was sealed to obtain a nonaqueous electrolyte secondary battery with a design capacity of 650 mAh.
[0041] <Example 2> A non-aqueous electrolyte secondary battery was fabricated in the same manner as in Example 1, except that the lithium composite oxide (Y) and GeO2 were dry mixed so that the molar ratio of the total amount of Ni and Mn in the lithium composite oxide (Y) to the molar ratio of Ge in the GeO2 was 2:0.015, and the mixture was baked in air at 1000°C for 30 minutes and then pulverized to obtain a positive electrode active material in which Ge was dissolved in the lithium composite oxide (Y). bulk The value of is 0.0076, and Ge surf / Ge bulk The value of was 2.5. In addition, the composition of the positive electrode active material was analyzed by ICP, and it was found to be LiNi 0.5 Mn 1.5 Ge 0.015 It was confirmed by XRD that the obtained positive electrode active material had a spinel structure.
[0042] <Comparative Example 1> A nonaqueous electrolyte secondary battery was fabricated in the same manner as in Example 1, except that GeO2 was not dissolved and the lithium composite oxide (Y) was used as it was as the positive electrode active material.
[0043] The discharge capacity and the voltage at SOC 50% were evaluated for each battery in the examples and comparative examples. The evaluation results are shown in Table 1. Table 1 also shows the results of the evaluation of Ge bulk , and Ge surf / Ge bulk Also shown.
[0044] [Discharge capacity measurement] The test cell was charged at a constant current of 0.2 C at a temperature of 25° C. until the cell voltage reached 4.9 V, and then discharged at a constant current of 0.2 C until the cell voltage reached 3.0 V to determine the discharge capacity.
[0045] [Evaluation of voltage at SOC 50%] The above test cell was charged at a constant current of 0.2 C to 50% of the battery's design capacity under a temperature condition of 25° C., and then the initial voltage when the cell was discharged at a constant current of 1 C was taken as the voltage at SOC 50%.
[0046] [Table 1]
[0047] As shown in Table 1, all of the batteries of the examples had a larger discharge capacity and a higher voltage at SOC 50% than the batteries of the comparative examples. bulk In Example 1, where the value was set to 0.082, the characteristics were greatly improved. [Explanation of symbols]
[0048] 1 Exterior body 2 Sealing plate 3 Electrode body 4 Positive electrode core exposed part 5 Negative electrode core exposed part 6 Positive electrode current collector 7 Positive terminal 8 Negative electrode current collector 9 Negative terminal 10 Electrolyte injection hole 11 Gas exhaust valve 13 Positive electrode outer conductive part 14 Positive Bolt Part 15 Positive electrode insertion part 16 Negative electrode outer conductive part 17 Negative Bolt Part 18 Negative electrode insertion part 100 Secondary battery
Claims
1. It has a spinel structure and has the general formula Li 1+α Ni 0.5-x Mn 1.5-y-z Ge y M x+z O 4 (wherein 0≦α<0.2, 0≦x<0.2, 0<y<0.45, 0≦z<0.2, and M is at least one element selected from Mg, Al, Sc, Ti, Cr, V, Fe, and Co), In the secondary particles of the lithium transition metal composite oxide, the number of moles of Ge when the total number of moles of metal elements other than Li in the surface portion is taken as 2 (Ge surf ) is the number of moles of Ge when the total number of moles of metal elements other than Li in the central part is 2 (Ge bulk ) A positive electrode active material for a non-aqueous electrolyte secondary battery.
2. The Ge bulk The Ge surf Ratio (Ge surf / Ge bulk ) is 1.5<Ge surf / Ge bulk The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1 , which satisfies the relationship:
3. The Ge bulk is 0.005<Ge bulk The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1 or 2, which satisfies the above-mentioned formula (1).
4. A positive electrode comprising the positive electrode active material for a non-aqueous electrolyte secondary battery according to any one of claims 1 to 3; A negative electrode; An electrolyte.
Citation Information
Patent Citations
Positive electrode active material for lithium secondary battery
JP1999191416A
Anode active material for lithium secondary batteries having a core-shell layer structure, method for manufacturing the same, and lithium secondary battery using the same
JP2008535173A
Electrode member, all-solid-state battery and manufacturing method of electrode member
JP2013149433A
Positive electrode active material for lithium ion secondary battery, positive electrode material for lithium ion secondary battery, and lithium ion secondary battery
JP2017033817A
Positive electrode active material for all-solid type secondary battery, positive electrode active material layer for all-solid type secondary battery, and all-solid type secondary battery
JP2018120705A