Positive electrode active material for secondary battery, and secondary battery

The lithium transition metal composite oxide with specific F and Sb content addresses the stability and conductivity issues in Co-free lithium-excessive oxides, improving battery performance by stabilizing the crystal structure and enhancing electronic conductivity.

JP7555001B2Active Publication Date: 2024-09-24PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2021554305
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-10-30
Filing Date
2020-10-13
Publication Date
2024-09-24
Estimated Expiration
2040-10-13

AI Technical Summary

Technical Problem

Lithium-excessive lithium transition metal composite oxides without Co exhibit low crystal structure stability and low electronic conductivity, leading to deteriorated load characteristics in secondary batteries.

Method used

A lithium transition metal composite oxide with the formula Li x Mn y Ni z Sb a O b F c (x+y+z+a≦b+c=2, 1≦x≦1.2, 0.4≦y≦0.8, 0≦z≦0.4, 0

Benefits of technology

The proposed composite oxide suppresses the deterioration of load characteristics in secondary batteries by maintaining high stability and conductivity, enhancing battery capacity and charge/discharge cycle characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007555001000002
    Figure 0007555001000002
  • Figure 0007555001000001
    Figure 0007555001000001
Patent Text Reader

Abstract

This positive electrode active material is for a secondary battery and contains a lithium transition metal complex oxide. The lithium transition metal complex oxide is represented by general formula LixMnyNizSbaObFc (x+y+z+a≤b+c=2, 1≤x≤1.2, 0.4≤y≤0.8, 0≤z≤0.4, 0<a<0.01, and 1.8<b<2 are satisfied) and does not include Co.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a positive electrode active material for a secondary battery and a secondary battery using the positive electrode active material.

Background Art

[0002] Conventionally, lithium transition metal composite oxides have been widely used as positive electrode active materials for secondary batteries such as lithium ion batteries. For example, Patent Document 1 proposes a lithium-excess type lithium transition metal composite oxide that does not contain Co. In this specification, a lithium transition metal composite oxide in which the molar ratio of lithium (Li / Me) to a metal (Me) excluding lithium in the lithium transition metal composite oxide is 1 or more is described as a lithium-excess type lithium transition metal composite oxide.

Prior Art Documents

Patent Documents

[0003]

Patent Document 1

Summary of the Invention

[0004] A lithium-excess type lithium transition metal composite oxide that does not contain Co has a problem that the load characteristics of a secondary battery deteriorate.

[0005] The positive electrode active material for a secondary battery according to one aspect of the present disclosure includes a lithium transition metal composite oxide, and the lithium transition metal composite oxide has a general formula Li x Mn y Ni z Sb a O b F c (satisfying x + y + z + a ≤ b + c = 2, 1 ≤ x ≤ 1.2, 0.4 ≤ y ≤ 0.8, 0 ≤ z ≤ 0.4, 0 < a < 0.01, 1.8 < b < 2), and is a composite oxide that does not contain Co.

[0006] A secondary battery according to one aspect of the present disclosure includes a positive electrode containing the above positive electrode active material, a negative electrode, and an electrolyte.

[0007] According to the positive electrode active material for a secondary battery which is one aspect of the present disclosure, a decrease in the load characteristics of the secondary battery can be suppressed.

Brief Description of the Drawings

[0008] [Figure 1] FIG. 1 is a cross-sectional view of a secondary battery which is an example of an embodiment.

Embodiments for Carrying Out the Invention

[0009] The positive electrode active material for a secondary battery which is one aspect of the present disclosure contains a lithium transition metal composite oxide, and the lithium transition metal composite oxide has the general formula Li x Mn y Ni z Sb a O b F c (satisfying x + y + z + a ≤ b + c = 2, 1 ≤ x ≤ 1.2, 0.4 ≤ y ≤ 0.8, 0 ≤ z ≤ 0.4, 0 < a < 0.01, 1.8 < b < 2), and is a composite oxide containing no Co. Generally, a lithium-excess type lithium transition metal composite oxide containing no Co has low stability of the crystal structure and low electronic conductivity, so the load characteristics of the secondary battery tend to deteriorate. However, the lithium transition metal composite oxide represented by the above general formula is a lithium-excess type and contains no Co, but has high stability of the crystal structure and high electronic conductivity, so it is considered that a decrease in the load characteristics of the secondary battery is suppressed. In particular, it is presumed that the improvement in the stability of the crystal structure of the composite oxide is greatly affected by a predetermined amount of F atoms contained in the composite oxide, and the improvement in the electronic conductivity of the composite oxide is greatly affected by a predetermined amount of Sb atoms contained in the composite oxide.

[0010] Hereinafter, an example of a secondary battery which is one aspect of the present disclosure will be described.

[0011] FIG. 1 is a cross-sectional view of a secondary battery as an example of an embodiment. The secondary battery 10 shown in FIG. 1 includes a wound electrode body 14 formed by winding a positive electrode 11 and a negative electrode 12 with a separator 13 interposed therebetween, an electrolyte, insulating plates 18 and 19 respectively arranged above and below the electrode body 14, and a battery case 15 for accommodating the above-mentioned members. The battery case 15 is composed of a cylindrical case body 16 with a bottom and a sealing body 17 for closing an opening of the case body 16. Note that, instead of the wound electrode body 14, an electrode body of another form may be applied, such as a laminated electrode body formed by alternately stacking positive and negative electrodes with a separator interposed therebetween. In addition, examples of the battery case 15 include a metallic case having a cylindrical shape, a square shape, a coin shape, a button shape, etc., and a resin case formed by laminating a resin sheet (so-called laminate type).

[0012] The electrolyte may be an aqueous electrolyte, but is preferably a non-aqueous electrolyte containing a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. Examples of the non-aqueous solvent include esters, ethers, nitriles, amides, and mixed solvents of two or more of these. The non-aqueous solvent may contain a halogen-substituted product in which at least a portion of the hydrogen of these solvents is replaced with a halogen atom such as fluorine. Examples of the electrolyte salt include LiPF 6 The electrolyte is not limited to a liquid electrolyte, and may be a solid electrolyte using a gel polymer or the like.

[0013] The case body 16 is, for example, a cylindrical metal container with a bottom. A gasket 28 is provided between the case body 16 and the sealing body 17 to ensure airtightness inside the battery. The case body 16 has a protruding portion 22 that supports the sealing body 17, for example, a part of the side surface of the case body 16 protruding inward. The protruding portion 22 is preferably formed in an annular shape along the circumferential direction of the case body 16, and supports the sealing body 17 on its upper surface.

[0014] The sealing body 17 has a structure in which a filter 23, a lower valve body 24, an insulating member 25, an upper valve body 26, and a cap 27 are laminated in this order from the electrode body 14 side. Each member constituting the sealing body 17 has, for example, a disk shape or a ring shape, and each member except the insulating member 25 is electrically connected to each other. The lower valve body 24 and the upper valve body 26 are connected to each other at their respective centers, and the insulating member 25 is interposed between each of their peripheral edges. When the internal pressure of the secondary battery 10 increases due to heat generation caused by an internal short circuit or the like, for example, the lower valve body 24 deforms and breaks so as to push the upper valve body 26 toward the cap 27, and the current path between the lower valve body 24 and the upper valve body 26 is interrupted. When the internal pressure further increases, the upper valve body 26 breaks, and gas is discharged from the opening of the cap 27.

[0015] In the secondary battery 10 shown in Fig. 1, a positive electrode lead 20 attached to the positive electrode 11 passes through a through hole in an insulating plate 18 and extends toward the sealing body 17, and a negative electrode lead 21 attached to the negative electrode 12 passes outside an insulating plate 19 and extends toward the bottom side of the case body 16. The positive electrode lead 20 is connected to the underside of a filter 23, which is the bottom plate of the sealing body 17, by welding or the like, and a cap 27, which is the top plate of the sealing body 17 and is electrically connected to the filter 23, serves as a positive electrode terminal. The negative electrode lead 21 is connected to the inner bottom surface of the case body 16 by welding or the like, and the case body 16 serves as a negative electrode terminal.

[0016] The positive electrode 11, the negative electrode 12, and the separator 13 will be described in detail below.

[0017] [Positive electrode] The positive electrode 11 has a positive electrode core and a positive electrode composite layer provided on the surface of the positive electrode core. For the positive electrode core, a foil of a metal such as aluminum that is stable in the potential range of the positive electrode 11, a film with the metal disposed on the surface layer, or the like can be used. The positive electrode composite layer contains a positive electrode active material, a binder, and a conductive material, and is preferably provided on both sides of the positive electrode core except for the part to which the positive electrode lead 20 is connected. The positive electrode 11 can be produced, for example, by applying a positive electrode composite slurry containing a positive electrode active material, a binder, a conductive material, and the like to the surface of the positive electrode core, drying the coating, and then compressing it to form a positive electrode composite layer on both sides of the positive electrode core.

[0018] Examples of the conductive material contained in the positive electrode composite layer include carbon materials such as carbon black, acetylene black, ketjen black, and graphite. Examples of the binder contained in the positive electrode composite layer include fluororesins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyimide, acrylic resin, and polyolefin. These resins may be used in combination with cellulose derivatives such as carboxymethyl cellulose (CMC) or its salts, polyethylene oxide (PEO), etc.

[0019] The positive electrode active material contains a lithium transition metal composite oxide. The lithium transition metal composite oxide has the general formula Li x Mn y Ni z Sb a O b F c (where x + y + z + a ≤ b + c = 2, 1 ≤ x ≤ 1.2, 0.4 ≤ y ≤ 0.8, 0 ≤ z ≤ 0.4, 0 < a < 0.01, 1.8 < b < 2, and it does not contain Co). In the general formula, since x + y + z + a is at most 2 and x is 1 or more and 1.2 or less, in the above lithium transition metal composite oxide, the molar ratio of Li to the metal (Me) excluding Li in the lithium transition metal composite oxide (Li / Me) is 1 or more, and it is a Li-excess type composite oxide.

[0020] The positive electrode active material preferably contains, as a main component, the above lithium transition metal composite oxide (hereinafter referred to as "composite oxide A"). The main component refers to the component with the highest content among the components in the positive electrode active material. The content of the composite oxide A in the positive electrode active material is preferably, for example, 50% by mass or more, more preferably 90% by mass or more, and still more preferably 100% by mass. Note that the positive electrode active material may contain a compound other than the composite oxide A as long as the effects of the present disclosure are not impaired.

[0021] Composite oxide A preferably has a crystal structure of the O2 structure. The O2 structure is preferably 50% by volume or more, more preferably 90% by volume or more, still more preferably 98% by volume or more, and even more preferably 100% by volume of the crystal structure of composite oxide A, from the viewpoints such as the stability of the crystal structure. Here, the O2 structure is a layered crystal structure in which lithium is present at the center of an oxygen octahedron and there are two types of ways of overlapping oxygen and transition metals per unit cell, and belongs to the space group P6 3 mc.

[0022] Composite oxide A may contain composite oxides of the T2 structure or O6 structure synthesized as by-products when synthesizing composite oxide A. Here, the T2 structure is a layered crystal structure in which lithium is present at the center of an oxygen tetrahedron and there are two types of ways of overlapping oxygen and transition metals per unit cell, and belongs to the space group Cmca. The O6 structure is a layered crystal structure in which lithium is present at the center of an oxygen octahedron and there are six types of ways of overlapping oxygen and transition metals per unit cell, and belongs to the space group R-3m.

[0023] In the above general formula of composite oxide A, a indicating the content of Sb only needs to satisfy 0 < a < 0.01, but preferably satisfies 0.002 ≤ a ≤ 0.005. By containing the predetermined amount of Sb in composite oxide A, for example, the electronic conductivity of composite oxide A is improved and the decrease in the load characteristics of the secondary battery is suppressed. When a is 0.01 or more, for example, the diffusivity of lithium ions in composite oxide A decreases and the decrease in the load characteristics of the secondary battery cannot be sufficiently suppressed.

[0024] Also, in the above general formula of composite oxide A, c indicating the content of F only needs to satisfy 0 < c ≤ 0.2, but preferably satisfies 0.02 ≤ c ≤ 0.1. By containing the predetermined amount of F in composite oxide A, for example, the stability of the crystal structure of composite oxide A is improved and the decrease in the load characteristics of the secondary battery is suppressed.

[0025] In addition, in the above general formula of the composite oxide A, y, which indicates the Mn content, may satisfy 0.4≦y≦0.8 in terms of suppressing the deterioration of the load characteristics of the secondary battery, but preferably satisfies 0.6≦y≦0.7 in terms of increasing the capacity of the secondary battery, for example. In addition, in the above general formula of the composite oxide A, z, which indicates the Ni content, may satisfy 0≦z≦0.4 in terms of suppressing the deterioration of the load characteristics of the secondary battery, but preferably satisfies 0.3≦z≦0.4 in terms of increasing the capacity of the secondary battery, for example. In addition, in the above general formula of the composite oxide A, x, which indicates the Li content, may satisfy 1≦x≦1.2 in terms of suppressing the deterioration of the load characteristics of the secondary battery, but preferably satisfies 1.1≦x≦1.15 in terms of suppressing the deterioration of the charge / discharge cycle characteristics of the secondary battery, for example.

[0026] The composite oxide A represented by the above general formula may contain metal elements other than Li, Mn, Ni, Sb, and Co. However, the molar ratio (Li / Me) of Li to the metal other than Li (Me) in the composite oxide A is 1 or more. The metal element other than Li, Mn, Ni, Sb, and Co is preferably at least one selected from, for example, Fe, Ti, Bi, and Nb. Among them, Ni and Fe are preferable.

[0027] The amount of each component constituting the composite oxide A is measured by inductively coupled plasma (ICP) emission spectrometry.

[0028] The composite oxide A is produced by adding and mixing raw materials such as Li compounds, Mn compounds, Ni compounds, Sb compounds, and F compounds to a predetermined molar ratio, pulverizing and mixing the resulting mixture by mechanochemical treatment, and firing the mixture after pulverization and mixing. The firing temperature of the mixture is preferably in the range of 700°C to 900°C. The firing atmosphere is preferably an oxygen atmosphere or air. The composite oxide A may be produced by firing the mixture to which the raw materials are added and mixed without mechanochemical treatment. In the synthesized composite oxide A, a part of Sb may not be solid-dissolved and may remain as an oxide on the particle surface of the composite oxide A, but this Sb is also an element that constitutes the composite oxide A. As a method for synthesizing the composite oxide A, it is preferable to carry out a mechanochemical treatment in that Sb is easily solid-dissolved.

[0029] The Li compound is not particularly limited, but examples thereof include Li oxide, Li carbonate, Li hydroxide, etc. The same applies to Mn compounds, Ni compounds, Sb compounds, and F compounds. In addition, each raw material may be a composite oxide, composite hydroxide, composite carbonate, etc. that contains at least two of Li, Mn, Ni, Sb, and F.

[0030] [Negative electrode] The negative electrode 12 has a negative electrode core and a negative electrode composite layer provided on the surface of the negative electrode core. For the negative electrode core, a foil of a metal such as copper that is stable in the potential range of the negative electrode 12, a film with the metal disposed on the surface layer, or the like can be used. The negative electrode composite layer contains a negative electrode active material and a binder, and is preferably provided on both sides of the negative electrode core except for the part to which the negative electrode lead 21 is connected. The negative electrode 12 can be produced, for example, by applying a negative electrode composite slurry containing a negative electrode active material and a binder to the surface of the negative electrode core, drying the coating, and then compressing it to form a negative electrode composite layer on both sides of the negative electrode core.

[0031] The negative electrode active material is not particularly limited as long as it can reversibly absorb and release lithium ions, but preferably contains a carbon-based active material. Suitable carbon-based active materials include natural graphite such as flake graphite, lump graphite, and earthy graphite, and artificial graphite such as lump artificial graphite (MAG) and graphitized mesophase carbon microbeads (MCMB). The negative electrode active material may also include a Si-based active material composed of at least one of Si and a Si-containing compound.

[0032] As in the case of the positive electrode 11, the binder may be a fluororesin, PAN, polyimide, acrylic resin, polyolefin, or the like, but it is preferable to use styrene-butadiene rubber (SBR). The negative electrode mixture layer preferably further contains CMC or a salt thereof, polyacrylic acid (PAA) or a salt thereof, polyvinyl alcohol (PVA), or the like. Among them, it is preferable to use SBR in combination with CMC or a salt thereof, or PAA or a salt thereof.

[0033] [Separator] For example, a porous sheet having ion permeability and insulating properties is used for the separator 13. Specific examples of the porous sheet include a microporous thin film, a woven fabric, and a nonwoven fabric. Suitable materials for the separator 13 include polyolefins such as polyethylene and polypropylene, and cellulose. The separator 13 may have either a single-layer structure or a laminated structure. A heat-resistant layer or the like may be formed on the surface of the separator.

[0034] <Example> The present disclosure will be further described below with reference to examples, but the present disclosure is not limited to these examples.

[0035] <Example 1> [Synthesis of positive electrode active material] LiMnO 2 , Li 2 MnO 3 , LiNiO 2 , LiF, Sb 2 O 3The above were mixed to a stoichiometric ratio of 0.033:0.3:0.3:0.05:0.001, and the mixture was placed in a 45cc zirconia pot containing zirconia balls with a diameter of 5 mm. The mixture was then placed in a planetary ball mill (FRITSCH, product name "PLP-7") and ground and mixed for 35 hours at a revolution speed of 600 rpm. The mixture was placed in a firing furnace and fired in air at 800°C for 1 hour to obtain a positive electrode active material.

[0036] The composition of the obtained positive electrode active material was analyzed using an inductively coupled plasma (ICP) emission spectrometer (manufactured by Thermo Fisher Scientific, product name "iCAP6300"), and the results showed that Li 1.167 Mn 0.554 Ni 0.277 Sb 0.002 O 1.95 F 0.05 It was.

[0037] [Preparation of positive electrode] The positive electrode active material, acetylene black, and polyvinylidene fluoride (PVdF) were mixed in a mass ratio of 92:5:3, and N-methyl-2-pyrrolidone (NMP) was used as a dispersion medium to prepare a positive electrode composite slurry. Next, this positive electrode composite slurry was applied to the surface of a positive electrode core made of aluminum foil, and the coating was dried and compressed, and then cut into a predetermined electrode size to produce a positive electrode in which a positive electrode composite layer was formed on the positive electrode core.

[0038] [Preparation of non-aqueous electrolyte] LiPF was added to a mixed solvent of fluoroethylene carbonate (FEC) and methyl 3,3,3-trifluoropropionate (FMP) in a mass ratio of 1:3. 6 was dissolved at a concentration of 1 mol / L to prepare a non-aqueous electrolyte solution.

[0039] [Preparation of test cell] An electrode assembly was prepared by attaching lead wires to the positive electrode and the Li metal counter electrode, and arranging the positive electrode and the counter electrode facing each other via a polyolefin separator. The electrode assembly and the nonaqueous electrolyte were enclosed in an exterior body made of an aluminum laminate film to prepare a test cell.

[0040] <Example 2> LiMnO 2 , Li 2 MnO 3 , LiNiO 2 , LiF, Sb 2 O 3 A positive electrode active material was synthesized in the same manner as in Example 1, except that the above was mixed in a stoichiometric ratio of 0.033:0.3:0.3:0.05:0.0025. Analysis of the composition of the obtained positive electrode active material revealed that Li 1.167 Mn 0.553 Ni 0.276 Sb 0.005 O 1.95 F 0.05 Moreover, a test cell was produced in the same manner as in Example 1 using the positive electrode active material.

[0041] <Comparative Example 1> LiMnO 2 , Li 2 MnO 3 , LiNiO 2 , LiF, Sb 2 O 3 A positive electrode active material was synthesized in the same manner as in Example 1, except that the above was mixed in a stoichiometric ratio of 0.033:0.3:0.3:0.05:0.005. Analysis of the composition of the obtained positive electrode active material revealed that Li 1.167 Mn 0.55 Ni 0.274 Sb 0.01 O 1.95 F 0.05 Moreover, a test cell was produced in the same manner as in Example 1 using the positive electrode active material.

[0042] <Comparative Example 2> LiMnO 2 , Li 2 MnO 3, LiNiO 2 A positive electrode active material was synthesized in the same manner as in Example 1, except that LiF was mixed in a stoichiometric ratio of 0.033:0.3:0.3:0.05. The composition of the obtained positive electrode active material was analyzed, and it was found that Li 1.167 Mn 0.555 Ni 0.278 O 1.95 F 0.05 Moreover, a test cell was produced in the same manner as in Example 1 using the positive electrode active material.

[0043] <Comparative Example 3> LiMnO 2 , Li 2 MnO 3 , LiNiO 2 , LiF, TiO 2 A positive electrode active material was synthesized in the same manner as in Example 1, except that the above was mixed in a stoichiometric ratio of 0.033:0.3:0.3:0.05:0.005. Analysis of the composition of the obtained positive electrode active material revealed that Li 1.167 Mn 0.553 Ni 0.276 Ti 0.005 O 1.95 F 0.05 Moreover, a test cell was produced in the same manner as in Example 1 using the positive electrode active material.

[0044] <Comparative Example 4> LiMnO 2 , Li 2 MnO 3 , LiNiO 2 , LiF, Sr(OH) 2 8H 2 A positive electrode active material was synthesized in the same manner as in Example 1, except that Li, LiO, and O were mixed in a stoichiometric ratio of 0.033:0.3:0.3:0.05:0.005. Analysis of the composition of the obtained positive electrode active material revealed that the 1.167 Mn 0.553 Ni 0.276 Sr 0.005 O 1.95 F 0.05 Moreover, a test cell was produced in the same manner as in Example 1 using the positive electrode active material.

[0045] <Comparative Example 5> LiMnO 2 , Li 2 MnO 3 , LiNiO 2 , LiF, Al(OH) 3 A positive electrode active material was synthesized in the same manner as in Example 1, except that the above was mixed in a stoichiometric ratio of 0.033:0.3:0.3:0.05:0.002. Analysis of the composition of the obtained positive electrode active material revealed that Li 1.167 Mn 0.554 Ni 0.277 Al 0.002 O 1.95 F 0.05 Moreover, a test cell was produced in the same manner as in Example 1 using the positive electrode active material.

[0046] <Comparative Example 6> LiMnO 2 , Li 2 MnO 3 , LiNiO 2 , LiF, (NH 4 ) 2 HPO 4 A positive electrode active material was synthesized in the same manner as in Example 1, except that the above was mixed in a stoichiometric ratio of 0.033:0.3:0.3:0.05:0.01. Analysis of the composition of the obtained positive electrode active material revealed that Li 1.167 Mn 0.55 Ni 0.274 P 0.01 O 1.95 F 0.05 Moreover, a test cell was produced in the same manner as in Example 1 using the positive electrode active material.

[0047] [Charge / discharge test] The test cells of each Example and Comparative Example were charged to 4.7V at a constant current of 0.05C in a temperature environment of 25°C, and then discharged to 2.5V at a constant current of 0.05C. The discharge capacity at this time is summarized in Table 1 as the battery capacity at 0.05C. In addition, the test cells of each Example and Comparative Example were charged to 4.7V at a constant current of 0.2C in a temperature environment of 25°C, and then discharged to 2.5V at a constant current of 0.2C. The discharge capacity at this time is summarized in Table 1 as the battery capacity at 0.2C. The smaller the difference between the battery capacity at 0.05C and the battery capacity at 0.2C, the more the deterioration of the load characteristics of the secondary battery is suppressed.

[0048] [Table 1]

[0049] In the test cells of Examples 1 and 2, the difference between the battery capacity at 0.05 C and the battery capacity at 0.2 C was kept small compared to the test cells of Comparative Examples 1 to 6. Therefore, it can be said that the deterioration of the load characteristics of the secondary battery was suppressed more in Examples 1 and 2 than in Comparative Examples 1 to 6. [Explanation of symbols]

[0050] 10 Secondary battery 11 Positive electrode 12 Negative electrode 13 Separator 14 Electrode body 15 Battery case 16 Case body 17 Sealing body 18,19 Insulating plate 20 Positive lead 21 Negative lead 22 Overhang 23 Filters 24 Lower valve body 25 Insulating materials 26 Upper valve 27 Cap 28 Gasket

Claims

1. A positive electrode active material for a secondary battery containing a lithium transition metal composite oxide, The lithium transition metal composite oxide has the general formula Li x Mn y Ni z Sb a O b F c (satisfying x+y+z+a≦b+c=2, 1≦x≦1.2, 0.4≦y≦0.8, 0≦z≦0.4, 0<a<0.01, 1.8<b<2), and which is a composite oxide containing no Co.

2. The positive electrode active material for a secondary battery according to claim 1 , wherein the general formula satisfies 0.002≦a≦0.

005.

3. A secondary battery comprising a positive electrode containing the positive electrode active material for a secondary battery according to claim 1 or 2, a negative electrode, and an electrolyte.

Citation Information

Patent Citations

  • Cordless telephone system

    JP1988087054A

  • Positive electrode mixture with improved conductivity, positive electrode comprising the same, and electrochemical device

    JP2016524275A

  • Cationic disordered oxides for rechargeable lithium batteries and other applications

    JP2018535904A

  • Fluorine substituted cation-disordered lithium metal oxides and methods of making same

    WO2018187531A1