Microsphere-coated polyurethane articles and methods for making same - Patents.com
A multilayer article with a microsphere-coated polyurethane structure addresses durability and weather resistance issues, offering enhanced protection for automotive, marine, and aerospace applications.
Patent Information
- Application Number
- JP2021568504
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-05-17
- Filing Date
- 2020-05-13
- Publication Date
- 2024-09-24
- Estimated Expiration
- 2040-05-13
AI Technical Summary
Existing microsphere-coated articles lack sufficient durability and weather resistance, making them unsuitable for applications requiring mechanical protection and resistance to environmental factors in industries like automotive, marine, and aerospace.
A multilayer article comprising a microsphere layer embedded in a polyurethane layer, with a bead-binding layer of thermosetting polyurethane, a primer layer of polyurea-polyurethane copolymer, and an elastomeric layer of polyurethane thermoplastic elastomer, providing enhanced adhesion and durability.
The multilayer structure exhibits improved abrasion resistance, chip resistance, and weather resistance, suitable for protective coatings in harsh environments.
Smart Images

Figure 0007555358000011 
Figure 0007555358000013 
Figure 0007555358000008
Abstract
Description
[Technical field]
[0001] Multi-layer articles including a single layer of microspheres embedded in a polyurethane layer are discussed along with methods of making such articles. The articles of the present disclosure may be useful, for example, in applications requiring mechanical durability and weather resistance, such as paint protection or paint replacement applications for the automotive, marine, and aerospace industries. [Background technology]
[0002] Durable laminates and films composed of glass beads are widely known. These low gloss structures typically consist of an exposed glass bead surface that imparts high durability and decorativeness to the structure. Typically, the beads are cascade coated or applied such that the beads are randomly positioned in a closely packed monolayer to form a continuous monolayer across the article surface. See Ueda et al., U.S. Pat. No. 4,849,265 and LaPerre, U.S. Pat. No. 5,620,775. [Brief description of the drawings]
[0003] Embodiments of the present disclosure are illustrated by way of example, and not by way of limitation, in the accompanying figures.
[0004] [Figure 1] FIG. 1 is a schematic cross-sectional view of a microsphere coated polyurethane article according to one embodiment of the present disclosure.
[0005] [Figure 2A] 1 illustrates a method of making an article according to one embodiment of the present disclosure. [Figure 2B] 1 illustrates a method of making an article according to one embodiment of the present disclosure. [Figure 2C] 1 illustrates a method of making an article according to one embodiment of the present disclosure. [Figure 2D] 1 illustrates a method of making an article according to one embodiment of the present disclosure. [Figure 2E]1 illustrates a method of making an article according to one embodiment of the present disclosure.
[0006] [Diagram 3] 1 is a profilometry image of a portion of the surface of Comparative Example A.
[0007] [Figure 4] 1 is a profilometry image of a portion of the surface of Example 1. Summary of the Invention
[0008] It is desirable to identify microsphere coated articles that have good durability (such as abrasion and chip resistance) and weatherability. Such articles may find use as surface coatings in paint protection or paint replacement applications in the automotive, marine, and aerospace industries.
[0009] In one aspect, an article is provided. The article (also referred to herein as a multi-layer article) comprises: (a) a microsphere layer including a plurality of microspheres arranged in a monolayer; (b) a bead-bonded layer having a first major surface and an opposing second major surface, the plurality of microspheres being partially embedded in the first major surface of the bead-bonded layer, the bead-bonded layer comprising a thermosetting polyurethane having a glass transition temperature of at least 35° C.; (c) a primer layer disposed on the second major surface of the bead-attached layer, the primer layer comprising a copolymer of polyurea and polyurethane, the primer layer being covalently bonded to the bead-attached layer via a urea bond; and (d) an elastomer layer disposed on the primer layer opposite the bead-attaching layer, the elastomer layer comprising a polyurethane thermoplastic elastomer.
[0010] In another aspect, a method of making a bead-coated film is provided, the method comprising: providing a transfer sheet comprising a transfer polymer layer having a monolayer of microspheres partially embedded thereon; coating the monolayer of embedded microspheres with a bead binding reaction mixture; partially curing the bead bonding reaction mixture to form a bead bonding layer, the bead bonding layer comprising a thermosetting polyurethane and having a glass transition temperature of at least 35° C.; contacting a primer reaction mixture onto the bead-binding layer; curing the second reaction mixture to form a primer layer, the primer layer comprising a copolymer of polyurea and polyurethane, the primer layer being covalently bonded to the bead binding layer via a urea bond; disposing a polyurethane thermoplastic elastomer over the primer layer; and c. removing the transfer sheet to form the bead-coated film.
[0011] The above summary of the disclosure is not intended to describe every embodiment. The details of one or more embodiments of the invention are set forth in the following description. Other features, objects, and advantages will be apparent from the description and from the claims. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] As used herein, The terms "a," "an," and "the" are used interchangeably and mean one or more; The term "and / or" is used to indicate that either or both of the stated things may occur. For example, A and / or B includes (A and B) as well as (A or B); "ambient conditions" means a temperature of 25 degrees Celsius and a pressure of 1 atmosphere (approximately 100 kilopascals); "Ambient temperature" means a temperature of 25 degrees Celsius. "Catalyst" means a substance that can increase the rate of a chemical reaction; "Diol" means a compound having exactly two hydroxyl functional groups; "Diisocyanate" means a compound containing exactly two isocyanate functional groups; "Cure" means to change the physical and / or chemical state of a composition, such as from a fluid to a less flowable state, from a viscous to a non-viscous state, from a soluble to an insoluble state, to reduce the amount of polymerizable material by consumption in a chemical reaction, or from a particular molecular weight material to a higher molecular weight; "Curable" means capable of being cured; "Essentially free" means having only trace amounts of a given substance, e.g., having less than 0.5%, 0.4, 0.3, 0.2, 0.1, 0.05, 0.02, 0.01, 0.005, or 0.001% of that substance; "fully cured" means that the composition has cured to a condition suitable for use in its intended application; "Partially cured" means cured to a state less than completely cured; "Polyisocyanate" means a compound having two or more isocyanate functional groups; "Polyol" means a compound having two or more hydroxyl functional groups.
[0013] The term "substituted" as used herein in connection with a molecule refers to a state in which one or more hydrogen atoms contained therein are replaced with one or more non-hydrogen atoms. Examples of substituents or functional groups that can be substituted include, but are not limited to, halogens (e.g., F, Cl, Br, and I); oxygen atoms in groups such as hydroxyl groups, alkoxy groups, aryloxy groups, aralkyloxy groups, oxo(carbonyl) groups, carboxylic acids, carboxylates, and carboxylate esters; sulfur atoms in groups such as thiol groups, alkyl and aryl sulfide groups, sulfoxide groups, sulfone groups, sulfonyl groups, and sulfonamide groups; nitrogen atoms in groups such as amines, hydroxylamine, nitriles, nitro groups, N-oxides, hydrazides, azides, and enamines, as well as other heteroatoms in various other groups. Non-limiting examples of substituents that can be bonded to a substituted carbon (or other) atom include F, Cl, Br, I, OR, OC(O)N(R), CN, NO, NO, ONO, azido, CF, OCF, R, O(oxo), S(thiono), C(O), S(O), methylenedioxy, ethylenedioxy, N(R), SR, SOR, SO, SO, N(R), SO, R, C(O)R, C(O)C(O)R, C(O)CHC(O)R, C(S)R, C(O)OR, OC(O)R, C(O)N(R), OC(O)N(R), C(S)N(R), (CH) 0~2 N(R)C(O)R, (CH2) 0~2 N(R)N(R), N(R)N(R)C(O)R, N(R)N(R)C(O)OR, N(R)N(R)CON(R), N(R)SOR, N(R)SON(R), N(R)C(O)OR, N(R)C(O)R, N(R)C(S)R, N(R)C(O)N(R), N(R)C(S)N(R), N(COR)COR, N(OR)R, C(=NH)N(R), C(O)N(OR)R, and C(=NOR)R, where R can be hydrogen or a carbon-based moiety, e.g., R can be hydrogen, (C1-C 100) hydrocarbyl, alkyl, acyl, cycloalkyl, aryl, aralkyl, heterocyclyl, heteroaryl, or heteroarylalkyl, or wherein two R groups attached to the nitrogen atom or to adjacent nitrogen atoms together with said one or more nitrogen atoms may form a heterocyclyl.
[0014] The term "alkyl" as used herein refers to straight-chain and branched alkyl groups, as well as cycloalkyl groups, having 1 to 40 carbon atoms, 1 to about 20 carbon atoms, 1 to 12 carbon atoms, or in some embodiments, 1 to 8 carbon atoms. Examples of straight-chain alkyl groups include those having 1 to 8 carbon atoms, such as methyl, ethyl, n-propyl, n-butyl, n-pentyl, n-hexyl, n-heptyl, and n-octyl. Examples of branched alkyl groups include, but are not limited to, isopropyl, iso-butyl, sec-butyl, t-butyl, neopentyl, isopentyl, and 2,2-dimethylpropyl. As used herein, the term "alkyl" encompasses n-alkyl, isoalkyl, and anteisoalkyl groups, as well as other branched forms of alkyl. Representative substituted alkyl groups may be substituted one or more times with any of the groups enumerated herein, such as amino groups, hydroxy groups, cyano groups, carboxy groups, nitro groups, thio groups, alkoxy groups, and halogen groups.
[0015] The term "alkenyl" as used herein refers to straight and branched chain and cyclic alkyl groups as defined herein, except that there is at least one double bond between two carbon atoms. Thus, an alkenyl group has from 2 to 40 carbon atoms, or from 2 to about 20 carbon atoms, or from 2 to 12 carbon atoms, or in some embodiments, from 2 to 8 carbon atoms. Examples include, but are not limited to, vinyl, -CH=CH(CH3), -CH=C(CH3)2, -C(CH3)=CH2, -C(CH3)=CH(CH3), -C(CH2CH3)=CH2, cyclohexenyl, cyclopentenyl, cyclohexadienyl, butadienyl, pentadienyl, and hexadienyl, among others.
[0016] The term "acyl" as used herein refers to a group that contains a carbonyl moiety, which is bonded through a carbonyl carbon atom. The carbonyl carbon atom is either bonded to a hydrogen to form a "formyl" group or to another carbon atom, which may be part of an alkyl, aryl, aralkyl, cycloalkyl, cycloalkylalkyl, heterocyclyl, heterocyclylalkyl, heteroaryl, heteroarylalkyl group, and the like. The acyl group can further contain 0 to about 12, 0 to about 20, or 0 to about 40 carbon atoms bonded to the carbonyl group. The acyl group can contain a double bond or a triple bond within the meaning herein. An acryloyl group is an example of an acyl group. An acyl group can also contain a heteroatom within the meaning herein. A nicotinoyl group (pyridyl-3-carbonyl) is an example of an acyl group within the meaning herein. Other examples include acetyl, benzoyl, phenylacetyl, pyridylacetyl, cinnamoyl, and acryloyl groups. When the group containing the carbon atom bonded to the carbonyl carbon atom contains a halogen, the group is referred to as a "haloacyl" group. An example is the trifluoroacetyl group.
[0017] The term "cycloalkyl" as used herein refers to cyclic alkyl groups, such as, but not limited to, cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, and cyclooctyl groups. In some embodiments, cycloalkyl groups can have from 3 to about 8-12 ring members, while in other embodiments the number of ring carbon atoms ranges from 3 to 4, 5, 6, or 7. Cycloalkyl groups further include polycyclic cycloalkyl groups, such as, but not limited to, norbornyl, adamantyl, bornyl, camphenyl, isocamphenyl, and carenyl groups, as well as fused rings, such as, but not limited to, decarnyl. Cycloalkyl groups also include rings substituted with straight or branched chain alkyl groups, as defined herein. Representative substituted cycloalkyl groups can be mono- or more than twice substituted, such as, but not limited to, 2,2-, 2,3-, 2,4-, 2,5-, or 2,6-disubstituted cyclohexyl groups, or mono-, di-, or tri-substituted norbornyl or cycloheptyl groups, which can be substituted with, for example, amino, hydroxy, cyano, carboxy, nitro, thio, alkoxy, and halogen groups. The term "cycloalkenyl," alone or in combination, refers to a cyclic alkenyl group.
[0018] The term "aryl" as used herein refers to a cyclic aromatic hydrocarbon group that does not contain a heteroatom in the ring. Thus, aryl groups include, but are not limited to, phenyl, azulenyl, heptalenyl, biphenyl, indacenyl, fluorenyl, phenanthrenyl, triphenylenyl, pyrenyl, naphthacenyl, chrysenyl, biphenylenyl, anthracenyl, and naphthyl groups. In some embodiments, the aryl group contains about 6 to about 14 carbons in the ring portion of the group. The aryl group can be unsubstituted or substituted as defined herein. Representative substituted aryl groups may be mono-substituted or substituted two or more times, such as, but not limited to, phenyl groups substituted at any one or more of the 2-, 3-, 4-, 5-, or 6-positions of the phenyl ring, or naphthyl groups substituted at any one or more of the 2-8 positions.
[0019] The term "aralkyl" as used herein refers to an alkyl group, as defined herein, in which a hydrogen or carbon bond of the alkyl group is replaced with a bond to an aryl group, as defined herein. Representative aralkyl groups include benzyl and phenylethyl groups, as well as fused (cycloalkylaryl)alkyl groups, such as 4-ethyl-indanyl. An aralkenyl group is an alkenyl group, as defined herein, in which a hydrogen or carbon bond of the alkyl group is replaced with a bond to an aryl group, as defined herein.
[0020] The term "alkoxy" as used herein refers to an oxygen atom bonded to an alkyl group, including a cycloalkyl group, as defined herein. Examples of straight-chain alkoxy groups include, but are not limited to, methoxy, ethoxy, propoxy, butoxy, pentyloxy, hexyloxy, and the like. Examples of branched-chain alkoxy groups include, but are not limited to, isopropoxy, sec-butoxy, tert-butoxy, isopentyloxy, isohexyloxy, and the like. Examples of cyclic alkoxy groups include, but are not limited to, cyclopropyloxy, cyclobutyloxy, cyclopentyloxy, cyclohexyloxy, and the like. An alkoxy group can contain about 1 to about 12, about 1 to about 20, or about 1 to about 40 carbon atoms bonded to an oxygen atom, and can further contain double or triple bonds, and can also contain heteroatoms. For example, an allyloxy group or a methoxyethoxy group is also an alkoxy group within the meaning of this specification, as is a methylenedioxyoxy group in the situation where two adjacent atoms of the structure are replaced thereby.
[0021] Further herein, the recitation of ranges by endpoints includes all numbers subsumed within that range (eg, 1 to 10 includes 1.4, 1.9, 2.33, 5.75, 9.98, etc.).
[0022] Also, as used herein, the reference to a number preceded by "at least" includes the particular number and all numbers greater than the particular number. For example, "at least one" includes all numbers greater than or equal to 1 (e.g., at least 2, at least 4, at least 6, at least 8, at least 10, at least 25, at least 50, at least 100, etc.).
[0023] As used herein, "comprising at least one of A, B, and C" refers to a single element A, a single element B, a single element C, A and B, A and C, B and C, and combinations of all three.
[0024] The present disclosure identifies, inter alia, certain microsphere-coated multi-layer articles that have good mechanical durability (e.g., abrasion resistance, chip resistance, and / or pencil hardness) and weather durability (such as heat and / or UV resistance). These structures may be applied to surfaces to modify the properties of the surface.
[0025] Figure 1 depicts a cross-sectional view of one embodiment of a multi-layer article of the present disclosure. Multi-layer article 10 comprises a microsphere layer comprising a monolayer of microspheres 11. Bead-bonded layer 12 comprises a first major surface and a second major surface 13 opposite the first major surface. A plurality of microspheres are embedded in the first major surface of the bead-bonded layer, and second major surface 13 is in contact with a primer layer 14. Primer layer 14 is disposed on elastomeric layer 16. In one embodiment, the structure further comprises an adhesive layer 17, and optionally a liner 18, as shown in Figure 1.
[0026] Elastomer Layer
[0027] The elastomer layer is a thermoplastic elastomer layer, including polyurethane. This layer must have elastomeric properties that allow it to absorb impacts from small objects such as rocks while also allowing flexibility for the multi-layer article.
[0028] In one embodiment, the polyurethane has an elongation at break of at least 50, 100, 200, 400, 600, 800, or even 1000%, when tested, for example, by ASTM D-882-18, using, for example, an Instron model 5565 (Norwood, MA), at a pull speed of 12 inches / minute (30 cm / minute) with a 1 inch (30 cm) jaw gap.
[0029] In one embodiment, the elastomeric layer has a glass transition temperature of less than 30, 25, 20, 15, 10, 5, 0, -5, -10, -15, or even -20° C. Glass transition temperature can be determined using techniques known in the art, for example, using a dynamic mechanical analyzer such as a DMA Q800 from TA Instruments (New Castle, Del.) at a heating rate of 10° C. / min at 1 Hz.
[0030] The polyurethane in the elastomeric layer may have a weight average molecular weight in the range of at least about 80,000, 85,000, 90,000, 100,000, 150,000, or even 175,000 daltons, and up to 200,000, 300,000, or even 400,000 daltons.
[0031] The thickness of the elastomeric layer can be at least 25, 30, 40, 50, 60, 70, or even 100 micrometers. In one embodiment, the thickness of the elastomeric layer is at most 75, 100, 150, 200, 250, 300, 400, or even 500 micrometers.
[0032] In one embodiment, the polyurethane of the elastomeric layer is the reaction product of a reaction mixture including a diisocyanate, a polymeric diol, and a chain extender.
[0033] Diisocyanate refers to a molecule having two isocyanate (-N=C=O) functional groups. Examples of suitable diisocyanates include those according to Formula I: [ka] [Wherein R may be substituted or unsubstituted, (C1-C 40 ) alkylene, (C2-C 40 ) Alkenylene, (C4-C 20 )Arylene, (C4~C 20 )Arylene-(C1~C 40 )Alkylene-(C4~C 20 )Arylene, (C4~C20 ) cycloalkylene, or (C4-C 20 ) aralkylene. Exemplary diisocyanates include dicyclohexylmethane-4,4'-diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate, 1,4-phenylene diisocyanate, 1,3-phenylene diisocyanate, m-xylylene diisocyanate, tolylene-2,4-diisocyanate, toluene-2,4-diisocyanate, tolylene-2,6-diisocyanate, poly(hexamethylene diisocyanate), , 1,4-cyclohexylene diisocyanate, 4-chloro-6-methyl-1,3-phenylene diisocyanate, hexamethylene diisocyanate, toluylene diisocyanate, diphenylmethane 4,4'-diisocyanate, 1,4-diisocyanatobutane, 1,8-diisocyanatooctane, 2,6-toluene diisocyanate, 2,5-toluene diisocyanate, 2,4-toluene diisocyanate, m-phenylene diisocyanate Isocyanate, p-phenylene diisocyanate, methylene bis (o-chlorophenyl diisocyanate), methylene diphenylene-4,4'-diisocyanate, (4,4'-diisocyanato-3,3', 5,5'-tetraethyl) diphenylmethane, 4,4'-diisocyanato-3,3'-dimethoxybiphenyl (o-dianisidine diisocyanate), 5-chloro-2,4-toluene diisocyanate, 1-chloromethyl-2,4 -diisocyanatobenzene, tetramethyl-m-xylylene diisocyanate, 1,6-diisocyanatohexane 1,12-diisocyanatododecane, 2-methyl-1,5-diisocyanatopentane, methylenedicyclohexylene-4,4'-diisocyanate, 3-isocyanatomethyl-3,5,5-trimethylcyclohexyl isocyanate, 2,2,4-trimethylhexyl diisocyanate, or mixtures thereof.
[0034] The amount of diisocyanate used to form the elastomeric layer can range from at least 0.5, 1, 1.5, 2, 3, 5, 8, or even 10% by weight of the reaction mixture, and up to 15, 20, 25, 30, 35, 40, 45, or even 47% by weight. The amount of diisocyanate in the reaction mixture of the elastomeric layer can be expressed in terms of an isocyanate index. The isocyanate index can be understood to generally refer to the ratio of the equivalents of isocyanate functionality used to the theoretical equivalents of hydroxyl functionality. Theoretical equivalents equal one equivalent of isocyanate functionality per equivalent of hydroxyl group, which is an index of 1.00. In one embodiment, the isocyanate index of the reaction mixture used to form the elastomeric layer is at least 0.99, 1.00, 1.02, 1.03, 1.04, or even 1.05, and up to 1.10, 1.12, 1.14, 1.16, 1.18, or even 1.20.
[0035] The term polymeric diol as used herein includes both polymers and small molecules having two hydroxyl (-OH) groups. The diol can be selected from the group consisting of caprolactone diols, polycarbonate diols, polyester diols, acrylic diols, polyether diols, polyolefin diols, and mixtures thereof.
[0036] The amount of polymeric diol used to form the elastomeric layer can range from at least 43, 45, or even 50% by weight of the reaction mixture, and up to 55, 60, 65, or even 70% by weight.
[0037] In one embodiment, the polymeric diol is a polyester diol. In one embodiment, the polyester diol may be the reaction product of a condensation reaction, such as a polycondensation reaction. However, polyester polyols are not produced via a ring-opening polymerization reaction.
[0038] In instances where the polyester diol is produced by a condensation reaction, the reaction may be between one or more carboxylic acids and one or more polymeric diols. Examples of suitable carboxylic acids include carboxylic acids according to Formula II having the following structure: [ka] [In the formula, R 1 may be substituted or unsubstituted, (C1-C 40 ) alkylene, (C2-C 40 ) alkylene, (C2-C 40 ) Alkenylene, (C4-C 20 )Arylene, (C4~C 20 ) cycloalkylene, or (C4-C 20) aralkylene. Specific examples of suitable carboxylic acids include glycolic acid (2-hydroxyethanoic acid), lactic acid (2-hydroxypropanoic acid), succinic acid (butanedioic acid), 3-hydroxybutanoic acid, 3-hydroxypentanoic acid, terephthalic acid (benzene-1,4-dicarboxylic acid), naphthalene dicarboxylic acid, 4-hydroxybenzoic acid, 6-hydroxynaphthalene-2-carboxylic acid, oxalic acid, malonic acid (propanedioic acid), adipic acid (hexanedioic acid), pimelic acid (heptanedioic acid), ethanoic acid, Suberic acid (octanedioic acid), azelaic acid (nonanedioic acid), sebacic acid (decanedioic acid), glutaric acid (pentanedioic acid), dodecanedioic acid, brassylic acid, tapric acid, maleic acid ((2Z)-but-2-enedioic acid), fumaric acid ((2E)-but-2-enedioic acid), glutaconic acid (penta-2-enedioic acid), 2-decenedioic acid, traumatic acid ((2E)-dodec-2-enedioic acid), muconic acid ((2E,4E)-hexa-2,4-dienedioic acid), glutinic acid acid), citraconic acid ((2Z)-2-methylbut-2-enedioic acid), mesaconic acid ((2E)-2-methyl-2-butenedioic acid), itaconic acid (2-methylidenebutanedioic acid), malic acid (2-hydroxybutanedioic acid), aspartic acid (2-aminobutanedioic acid), glutamic acid (2-aminopentanedioic acid), tartonic acid, tartaric acid (2,3-dihydroxybutenedioic acid), diaminopimelic acid ((2R,6S)-2,6-diaminoheptanedioic acid), saccharic acid ((2S,3S,4S,5R)-2,3,4,5-tetrahydroxyhexanedioic acid), mexooxalic acid acid), oxaloacetic acid (oxobutanedioic acid), acetone dicarboxylic acid (3-oxopentanedioic acid), albinaric acid, phthalic acid (benzene-1,2-dicarboxylic acid), isophthalic acid, diphenic acid, 2,6-naphthalenedicarboxylic acid, or mixtures thereof.
[0039] Examples of suitable diols include diols according to Formula III having the following structure: [ka] [In the formula, R 2may be substituted or unsubstituted, (C1-C 40 ) alkylene, (C2-C 40 ) Alkenylene, (C4-C 20 )Arylene, (C1-C 40 ) Acylene, (C4~C 20 )Cycloalkylene, (C4-C 20 ) aralkylene, or (C1-C 40 ) alkoxyene, R 3 and R 4 may be -H, -OH, substituted or unsubstituted, (C1-C 40 ) Alkyl, (C2-C 40 ) Alkenyl, (C4-C 20 ) Aryl, (C1-C 20 )Acyl, (C4~C 20 )Cycloalkyl, (C4-C 20 ) aralkyl, and (C1-C 40 ) alkoxy.
[0040] Another example of a suitable polyol includes a compound according to formula IV having the following structure: [ka] [In the formula, R 5 and R 6 may be substituted or unsubstituted, (C1-C 40 ) alkylene, (C2-C 40 ) Alkenylene, (C4-C 20 )Arylene, (C1-C 40 ) Acylene, (C4~C 20 )Cycloalkylene, (C4-C 20 ) aralkylene, or (C1-C 40 ) alkoxyenes, where n is a positive integer greater than or equal to 1 (e.g., 2, 4, 5, or even greater than 10).
[0041] Another example of a suitable polyol includes a compound according to Formula V having the following structure: [ka] [In the formula, R 7 may be substituted or unsubstituted, (C1-C 40 ) alkylene, (C2-C 40 ) Alkenylene, (C4-C 20 )Arylene, (C1-C 40 ) Acylene, (C4~C 20 )Cycloalkylene, (C4-C 20 ) aralkylene, or (C1-C 40 )alkoxyenes, where n is a positive integer equal to or greater than 1 (e.g., 2, 4, 5, or even greater than 10). Specific examples of polyester polyols include polyglycolic acid (poly[oxy(1-oxo-1,2-ethanediyl)]), polybutylene succinate (poly(tetramethylene succinate)), poly(3-hydroxybutyrate-co-3-hydroxyvalerate), polyethylene terephthalate (poly(ethylbenzene-1,4-dicarboxylate)), polybutylene terephthalate (poly(oxy-1,4-butanediyloxycarbonyl-1,4-furan), poly(ethylene glycol) (poly(ethylene glycol-1,4-dimethylamino)phenyl)), poly(ethylene glycol-1,4-dimethylamino)phenyl ... Poly(1,7)-polyoxepan-2-one, polycaprolactone polyol, poly(1,7)-polyoxepan-2-one ...
[0042] An appropriate melting temperature can help increase the crystallinity of the elastomeric layer. Crystallinity can be determined by differential scanning calorimetry and is expressed as the crystallinity fraction in the polyurethane thermoplastic elastomer. The crystallinity can range from at least 30, 40, or even 50% up to 55, 60, 65, or even 70%. The crystallinity can make the elastomeric layer easier to roll as it requires a relatively high temperature to begin to liquefy the elastomeric layer.
[0043] A chain extender can be added to the reaction mixture used to form the elastomeric layer to increase the molecular weight of the resulting polyurethane and strengthen the elastomeric layer. The chain extender can range from at least 1, 1.5, 2, 2.5, 3, 4, or even 5% by weight of the reaction mixture, and up to 6, 7, 8, 10, 11, or even 13% by weight.
[0044] In one embodiment, the chain extender is a diol chain extender having two hydroxyl groups. The diol chain extender has a weight average molecular weight of at least 30, 40, 50, 60, or even 80 Daltons, and up to 100, 125, 150, 175, 200, 225, or even 250 Daltons. The diol chain extender may contain any suitable number of carbons. For example, the diol chain extender may contain from about 2 carbons to about 20 carbons, from about 3 carbons to about 10 carbons, or a number average number of carbons less than, equal to, or greater than about 2 carbons, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, or 20. Diol chain extenders containing relatively short chains may be stiffer than longer chain diols and may provide reinforcement to the elastomeric layer. Short chain diols may be more rigid, for example, because they are more restricted in terms of rotation about each bond along the chain. Examples of suitable diol chain extenders include ethylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, neopentyl glycol, 1,6-hexanediol, 1,4-cyclohexanedimethanol, or mixtures thereof.
[0045] In one embodiment, the polyurethane thermoplastic elastomer comprises hard segments. Hard segments generally refer to harder, less flexible polymer segments resulting from the polymerization of diisocyanates with diol chain extenders. The amount of hard segments can be determined by calculating the total amount (wt%) of isocyanates, chain extenders, and crosslinkers. Then, divide that total by the total weight of the polyurethane thermoplastic elastomer. The hard segments can range from at least 30, 32, 34, 36, 38, or even 40 wt% to up to 45, 48, 50, 53, or even 55 wt% of the polyurethane thermoplastic elastomer. The hard segments exist as domains that can interact with each other to effectively form crosslinks between them (e.g., via hydrogen bonds). When under stress, for example, through mechanical deformation, the hard segments can become aligned in the direction of the stress. This alignment coupled with hydrogen bonds can contribute to the stiffness, elastomeric elasticity, or tear resistance of the elastomeric layer.
[0046] In some examples, the reaction mixture used to form the elastomeric layer can include a crosslinking agent. Examples of crosslinking agents include polyhydroxy group compounds and polyisocyanate compounds. For example, a polyhydroxy compound can include three hydroxy groups or four hydroxy groups. A polyisocyanate can include three cyano groups or four cyano groups. Although many suitable crosslinking agents exist, the reaction mixture does not include an aziridine crosslinking agent. If present, the crosslinking agent can function to crosslink the polyurethane chains of the elastomeric layer.
[0047] The thickness of the elastomer layer is not particularly limited.Preferably, the elastomer layer is thin enough to allow the entire multilayer article to stretch as necessary to conform to a substrate having a curved or irregular three-dimensional contour, but thick enough to protect the substrate against abrasion and impact that may occur during use.The thickness of the elastomer layer may be at least 50, 60, 70, 80, 100, or even 150 micrometers, and up to 200, 250, 300, 250, 300, 350, 400, 450, 500, 550, or even 600 micrometers.
[0048] Bead-bound layer
[0049] The microspheres in the multi-layer article are held in place via a bead-tie layer. The bead-tie layer is a thermoset polyurethane (a thermoset is a polymer that does not have a bulk softening temperature and cannot be melted or molded after polymerization). In one embodiment, the thermoset polyurethane has a glass transition temperature of at least 35, 40, 45, 50, 60, 70, or even 80° C. In one embodiment, the thermoset polyurethane has a glass transition temperature of up to 90, 95, 100, 110, or even 120° C. The glass transition temperature can be determined using techniques known in the art, for example, using a dynamic mechanical analyzer such as a DMA Q800 from TA Instruments (New Castle, DE) at a heating rate of 10° C. / min at 1 Hz. The thermoset polyurethane should exhibit good adhesion to the microspheres. In one embodiment, an adhesion promoter is added to the bead-tie reaction mixture to improve adhesion between the microspheres and the bead-tie layer. The adhesion promoter must be compatible within the process window for disposing the bead attachment layer onto the surface of the microspheres.
[0050] In one embodiment, the bead-attached layer is obtained by curing a polyurethane composition. In some embodiments, the polyurethane composition is a curable composition whose components react with each other to provide a cured layer. The curable composition used to obtain the bead-attached layer can include a polyisocyanate and a polyol.
[0051] Suitable polyisocyanates include diisocyanates and polyisocyanates having an isocyanate functionality of more than 2 (e.g., more than 3, 4, 6, or even more). In an exemplary embodiment, the polyisocyanate is a primary polyisocyanate, such as a primary aliphatic polyisocyanate. Primary polyisocyanates having an isocyanate functionality of 3 or more can be made from primary diisocyanates, such as 1,6-hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, 1,4-tetramethylene diisoycanate, 1,3-xylylene diisocyanate, 1,4-xylylene diisocyanate, 1,12-dodecamethylene diisocyanate, 2-methylpentamethylene diisocyanate, or 1,4-cyclohexanedimethylene diisocyanate.
[0052] In the reaction mixture used to form the bead binding layer, the polyisocyanate can comprise at least 30, 35, 40, 45, or even 50% by weight and up to 60, 70, 75, 80, 85, or even 90% by weight, based on the total weight of the reaction mixture.
[0053] Suitable polyols include diols and polyols with a hydroxyl functionality greater than 2. The polyol may be selected from the group consisting of polycaprolactone polyols, polycarbonate polyols, polyester polyols, acrylic polyols, polyether polyols, polyolefin polyols, and mixtures thereof.
[0054] In total, the polyol components used in preparing the bead-attached layer can comprise at least 25, 30, or even 35% by weight and up to 60, 65, 70, 75, or even 80% by weight, based on the total weight of the reaction mixture used to form the bead-attached layer.
[0055] In one embodiment, the reaction mixture used to form the bead-attaching layer includes a hydroxy-functional silicone poly(meth)acrylate. The hydroxy-functional silicone poly(meth)acrylate is a copolymer consisting of siloxane side groups, such as polydimethylsiloxane side groups, covalently bonded to an acrylic or methacrylic backbone. The copolymer may have just one hydroxyl group, in which case it is a monohydroxyl silicone poly(meth)acrylate. Alternatively, the hydroxy-functional silicone poly(meth)acrylate can have two or more hydroxyl groups, in which case it is a silicone poly(meth)acrylate polyol. The backbone of the hydroxy-functional silicone poly(meth)acrylate can contain any of a variety of repeating units, including, for example, hydroxyethyl methacrylate, 2-ethylhexyl acrylate, 2-ethylhexanol, styrene, and combinations thereof. In one embodiment, the primer layer consists essentially of the hydroxy-functional silicone poly(meth)acrylate and contains less than 0.5, 0.2, 0.1, 0.05, 0.01, 0.005, or 0.001% of the hydroxy-functional silicone poly(meth)acrylate.
[0056] The addition of a hydroxy-functional silicone poly(meth)acrylate can improve the stain resistance of the bead-tie layer when fully cured. The hydroxy-functional silicone poly(meth)acrylate can be at least 0.1, 0.2, 0.5, 0.8, or even 1 weight percent up to 1.5, 2, 2.5, 3, 3.5, or even 4 weight percent based on the total weight of the reaction mixture used to form the bead-tie layer.
[0057] The curable composition used to form the bead-binding layer may further comprise a catalyst to promote the reaction between the polyisocyanate and the polyol component. Catalysts useful for the polymerization of polyurethane include aluminum, bismuth, tin, vanadium, zinc, mercury, and zirconium-based catalysts, amine catalysts, and mixtures thereof. Preferred catalysts include tin-based catalysts such as dibutyltin compounds. Particularly preferred are catalysts selected from the group consisting of dibutyltin diacetate, dibutyltin dilaurate, dibutyltin diacetylacetonate, dibutyltin dimercaptide, dibutyltin dioctoate, dibutyltin dimaleate, dibutyltin acetonylacetonate, and dibutyltin oxide.
[0058] A suitable amount of catalyst can be at least 0.001, 0.005, 0.01, 0.02, 0.05, or even 0.08 wt. % to up to 0.1, 0.12, 0.15, 0.17, or even 0.2 wt. % based on the total weight of the reaction mixture used to form the bead-bound layer.
[0059] The multi-layer structure of the present disclosure must be weather resistant.Therefore, ultraviolet absorbers and / or hindered amines (HALS) can be added to various layers, especially bead-binding layers, to help minimize ultraviolet damage to the article and / or the surface it protects, and to minimize defects caused by cracking and gloss reduction in these layers.Exemplary UV absorbers include benzotriazole compounds, 5-trifluoromethyl-2-(2-hydroxy-3-α-cumyl-5-tert-octylphenyl)-2H-benzotriazole, or combinations thereof. Other exemplary benzotriazoles include 2-(2-hydroxy-3,5-di-α-cumylphenyl)-2H-benzotriazole, 5-chloro-2-(2-hydroxy-3-tert-butyl-5-methylphenyl)-2H-benzothiazole, 5-chloro-2-(2-hydroxy-3,5-di-tert-butylphenyl)-2H-benzotriazole, 2-(2-hydroxy-3,5-di-tert-amylphenyl)-2H-benzotriazole, 2-(2-hydroxy-3-α-cumyl-5-tert-octylphenyl)-2H-benzotriazole, 2-(3-tert-butyl-2-hydroxy-5-methylphenyl)-5-chloro-2H-benzotriazole, or combinations thereof. Additional exemplary UV absorbers include 2(-4,6-diphenyl-1-3,5-triazin-2-yl)-5-hexyloxy-phenol and those sold under the trade names "TINUVIN 1577", "TINUVIN 405" and "TINUVIN 900" by BASF (Florham Park, NJ). In addition, the UV absorbers can be used in combination with stabilizers and / or antioxidants, such as hindered amine light stabilizers (HALS). The stabilizers can scavenge free radicals generated by photo-oxidation of the polymer. Exemplary HALS include those available under the trade names "CHIMASSORB 944", "TINUVIN-292" and "TINUVIN 123" by BASF.Typically, the UV absorbers and / or hindered amine light stabilizers are present in the reaction mixture and / or cured layer (such as the bead-bonded layer, primer layer, or elastomeric layer) in a total amount of at least 1, 1.5, 1.75, or even 2 wt. %, and up to 2.5, 3, 3.5, 4, 4.5, or even 5 wt. %.
[0060] If desired, other ingredients such as leveling agents, colorants, flame retardants, and pot life extenders can also be included in the reaction mixture to form the bead-bonded layer.
[0061] The bead-attached layer of the present disclosure is derived from a solvent-based solution. In other words, a solvent (such as an organic solvent or water) is used to dissolve the reactive components to create the bead-attached layer, but the solvent does not polymerize or harden when forming the bead-attached layer. Organic solvents can be used to adjust the viscosity of the reaction mixture used to create the bead-attached layer. Such organic solvents can include ether acetate, propylene glycol monomethyl ether acetate, ketones, benzene derivatives, and mixtures thereof. In one embodiment, the reaction mixture of the bead-attached layer is substantially free of water (e.g., 1, 0.5, 0.1, or even 0.05 wt. % in the reaction mixture). The amount of solvent can be selected to facilitate proper mixing and casting of the curable polyurethane composition. The organic solvents used are generally volatile so that they can be removed prior to or simultaneously with the curing of the bead-attached layer. Such evaporation can be facilitated by heat, vacuum, or both.
[0062] When the aforementioned reactive components of the bead-bonded layer are mixed and heated sufficiently, they polymerize into a crosslinked network. The crosslink density of the polyurethane in the bead-bonded layer is calculated by dividing the weight of reactive components having a functionality of 3 or more by the total weight of the polyurethane and multiplying by 100. High crosslink densities (e.g., greater than 30 percent) are generally associated with rigid polyurethane materials. However, the use of primary aliphatic polyisocyanates can enable polyurethanes that are both flexible and have a high crosslink density. Useful crosslink densities can be at least 25, 30, 35, 40, or even 45% up to 50, 55, 60, 70, 80, 90, or even 100%.
[0063] In one embodiment, the bulk bead binding layer is substantially free of polyurea, in other words, outside the interface with the adjacent layer, the bulk of the bead binding layer is less than 3, 2, 1, 0.5, 0.1 wt. % or even less of urea linkages.
[0064] Due to the high crosslink density in the bead-binding layer, the bead-binding layer is thin. Typically, the thickness of the cured bead-binding layer is less than the distance at which the microspheres are embedded in the bead-binding layer. For example, the thickness of the bead-binding layer is less than 50, 45, 40, 35, or even 30% of the average diameter of the microspheres. As shown in Figure 1 (not drawn to scale), the bead-binding layer extends between and covers the undersides of the microspheres that form part of the outermost surface of the multilayer article.
[0065] Primer layer
[0066] A second polyurethane layer is provided and is disposed between the bead-tie layer and the elastomeric layer, the purpose of this layer being to improve adhesion of the bead-tie layer to the elastomeric layer.
[0067] The primer layer extends along and contacts the second major surface 13 of the bead-attached layer. The primer layer is prepared by curing a second polyurethane composition. Use of a primer layer can be advantageous because it provides covalent bonds (through urea bonds) and optionally secondary bonds (such as hydrogen bonds) at the interface between the bead-attached layer and the primer layer, allowing for improved interlayer adhesion.
[0068] The primer layer composition can have similar properties to those of the bead-bonded composition described above. In one embodiment, the primer layer differs from the bead-bonded composition in that it contains not only polyurethane groups (-NH-C(=O)-O-), but also polyurea groups (-NH-C(=O)-NH-). The reaction mixture forming the primer layer contains amine groups or has the ability to form amine groups that can react with isocyanate groups of the bead-bonded layer and / or elastomeric layer, leading to covalent (urea) bonds (and possibly hydrogen bonds) between the primer layer and its adjacent layer (i.e., the second major surface 13 of the bead-bonded layer and the major surface 15 of the primer layer), resulting in improved interlayer adhesion.
[0069] In some embodiments, the primer layer composition is an aqueous polyurethane dispersion.Preferred aqueous polyurethane dispersions include aliphatic polycarbonate polyurethane dispersions.The dispersion can use a solvent system that includes water and one or more cosolvents.Certain cosolvents, such as diethylene glycol monomethyl ether, can be useful for improving coating quality by reducing the volatility of the dispersion.
[0070] The polyurethane dispersion used in the primer layer can include any of a number of suitable surfactants, such as anionic surfactants. Anionic surfactants include, for example, sulfates such as sodium dodecyl sulfate, ammonium dodecyl sulfate, and sodium lauryl ether sulfate, and sulfosuccinates such as sodium dioctyl sulfosuccinate and disodium lauryl sulfosuccinate. In water-based coatings, these surfactants can be used in combination with co-dispersants. Co-dispersants include amino alcohols. Amino alcohols such as 2-amino-2-methyl-1-propanol can help neutralize acid-functional resins and are suitable for use in water-based coatings.
[0071] The primer composition can include any suitable crosslinking agent, such as a polyfunctional aziridine liquid crosslinker. The amount of crosslinking agent is not critical and can be selected to provide the desired degree of crosslinking. The amount of crosslinking agent can be at least 0.5, 0.7, 1, 1.2, or even 1.5% by weight to up to 2, 2.5, 3, 3.5, 4.5, or even 5% by weight, based on the total weight of the reaction mixture used to form the primer layer.
[0072] When the aforementioned reactive components of the primer layer are mixed and heated sufficiently, they polymerize and become a crosslinked network. In one embodiment, the crosslink density of the primer layer is the same as or lower than the crosslink density of the bead-attached layer. Useful crosslink densities can be at least 25, 30, 35, 40, or even 45% up to 50, 55, 60, 70, 80, 90, or even 100%.
[0073] As mentioned above, other additives such as UV light absorbers and stabilizers may also be included in the primer layer.
[0074] In a preferred embodiment, the primer layer is formed from an aqueous polyurethane dispersion that is a polycarbonate polyurethane having a solids content of 30-40% by weight and a total solvent content of 5-15% by weight.
[0075] The primer layer has a chemical composition that allows it to permanently adhere to the bead-tie layer, and preferably the bead-tie layer and the primer layer do not delaminate from each other during the life of the multi-layer article, even in harsh environments.
[0076] The thickness of the primer layer does not need to be particularly limited. In some embodiments, this thickness can be similar to that of the bead-bonded layer. The film thickness of the primer layer when cured can be at least 12, 15, 20, 25, 30, 35, or even 40 micrometers, and up to 50, 60, 75, or even 85 micrometers. The primer layer is a continuous or discontinuous layer throughout the multilayer article, and typically has a less corrugated or flatter surface (compared to its opposite major surface that contacts the bead-bonded layer) on which the elastomeric layer is disposed.
[0077] The bead-attaching layer, primer layer, and / or elastomer layer may be transparent, translucent, or opaque. The bead-attaching layer, primer layer, and / or elastomer layer may be colored or colorless. The bead-attaching layer may be, for example, transparent and colorless, or colored with opaque, transparent, or translucent dyes and / or pigments. In some embodiments, it may be useful to include specialty pigments, such as, for example, metallic flake pigments.
[0078] microsphere layer
[0079] The microsphere layer comprises a plurality of microspheres. The plurality of microspheres are arranged in a monolayer (or single layer) across the bead-bound layer. Microspheres useful in the present disclosure include glasses, glass-ceramics, ceramics, polymers, metals, and combinations thereof. Glasses are amorphous materials, while ceramics refer to crystalline or partially crystalline materials. Glass-ceramics have an amorphous phase and one or more crystalline phases. Such materials are known in the art.
[0080] In some embodiments, the microspheres are glass beads. The glass beads are mostly spherical. Glass beads are typically produced from recycled sources such as glazing and / or glass products, typically by crushing regular soda-lime or borosilicate glasses. Regular industrial glasses can be of various refractive indices depending on their composition. Soda-lime silicates and borosilicates are common types of glasses. Borosilicate glasses typically contain boria and silica, along with other elemental oxides such as alkali metal oxides and alumina. Some glasses used in the industry that contain boria and silica, among other oxides, include E-glass and glasses available under the trade name "NEXTERION GLASS D" from Schott Industries, Kansas City, Missouri, and glasses available under the trade name "PYREX" from Corning Incorporated, New York, New York.
[0081] The milling process results in a wide distribution of glass particle sizes. The glass particles are spheronized by processing in a heated column that melts the glass into spherical droplets that are subsequently cooled. Not all particles are perfectly spherical; some are oblate, some are fused together, and some contain small gas bubbles.
[0082] In one embodiment, the microspheres are plastic particles. The selected plastic particles should have a higher hardness than the underlying substrate surface to protect the substrate surface. Exemplary plastic particles include polyurethane, polystyrene, acrylic and methacrylic acid ester polymers and copolymers (e.g., poly(methyl methacrylate)), and polyurea spheres.
[0083] In one embodiment, the microspheres include a surface modification to improve adhesion of the microspheres to the bead-attached layer, as known in the art. Such treatments include those selected from the group consisting of silane coupling agents, titanates, organochromium complexes, and the like, to maximize adhesion of the microspheres to the first polymer layer. Preferably, the coupling agent includes nucleophilic groups present on the surface of the microspheres that can react with isocyanates in the bead-attached layer reaction mixture. Exemplary coupling agents may include amino groups, such as aminosilanes. Having nucleophilic groups present on the surface of the microspheres allows isocyanates from the bead-attached reaction mixture to form covalent bonds, thereby improving adhesion between the bead-attached layer and the plurality of microspheres.
[0084] In one embodiment, treatment levels of such coupling agents are on the order of 50-700 parts by weight per million parts by weight of microspheres. Smaller diameter microspheres have a larger surface area and can typically be treated at higher levels. Treatment is typically accomplished by spray drying or wet mixing a dilute solution of the coupling agent, such as an alcohol solution (e.g., ethyl alcohol or isopropyl alcohol, etc.) with the microspheres, followed by drying in a rotary drier or auger-fed dryer to prevent the microspheres from sticking together. One of ordinary skill in the art will be able to determine how to optimally treat the microspheres with the coupling agent.
[0085] In one embodiment, the microspheres of the present disclosure have a Knoop hardness of at least 1,300 kg / mm 2 or further 1,800kg / mm 2As used herein, "Knoop hardness" is the microhardness indentation measured using a Knoop indenter, and is calculated by dividing the load applied to form a diamond-shaped indentation on the surface of a sample by the projected area of the indentation calculated from the long diagonal of the permanent indentation. The method for measuring Knoop hardness is described in ASTM C849-88(2011) "Standard Test Method for Knoop Indentation Hardness of Ceramic Whitewares".
[0086] Microspheres for use in this disclosure are substantially spherical, e.g., having a sphericity of at least 80%, 85%, or even 90%, where sphericity is defined as the surface area of a sphere (of the same volume as a given particle) divided by the surface area of the particle, and is reported as a percentage.
[0087] Preferred examples of spherical particles include fused alumina, alumina produced by the Bayer process, zirconia, and eutectic mixtures thereof.
[0088] As a method for forming inorganic particles into spherical ones, it is possible to apply a method in which the above-mentioned inorganic materials having an indefinite shape are crushed and melted in a high-temperature oven at a temperature higher than the melting point of these materials, thereby obtaining spherical particles by utilizing surface tension, or a method in which the above-mentioned inorganic materials are melted at a temperature higher than the melting point of these materials, and the molten material is sprayed to obtain spherical particles.
[0089] Microspheres useful in the present disclosure may be transparent, translucent, or opaque, depending on the desired properties of the resulting article.
[0090] In another embodiment, the microspheres have a refractive index less than 1.30, less than 1.40, less than 1.49, less than 1.50, less than 1.55, less than 1.60, less than 1.70, less than 1.80, or even less than 1.90. The refractive index can be measured by the standard Becke line method.
[0091] The microspheres are preferably defect-free. As used herein, "defect-free" means that the microspheres have a low amount of air bubbles, a low amount of irregularly shaped particles, low surface roughness, low amount of inhomogeneities, low amount of undesirable colors or tints, or low amount of other scattering centers. In one embodiment, the microspheres are not glass bubbles, but rather are hollow cores encapsulated in glass spheres.
[0092] In some embodiments, useful ranges of average microsphere diameters are at least 10, 20, 25, 40, 50, 75, 100, or even 150 μm (micrometers) and up to 200, 400, 500, 600, 800, 900, or even 1000 μm. The microspheres can have a unimodal or multimodal (e.g., bimodal) size distribution depending on the application.
[0093] Microspheres are typically sized by sieving to provide a useful particle size distribution. Sieving is also used to characterize the size of microspheres. Sieving uses a series of sieves with controlled size openings, and microspheres that pass through an opening are considered to be equal to or smaller than the size of that opening. This is true for microspheres because the cross-sectional diameter of the microsphere is almost always the same, no matter how the microsphere is oriented relative to the sieve openings.
[0094] In some embodiments, to calculate the "average diameter" of a mixture of microspheres, a given weight of particles, e.g., a 100 gram sample, may be sieved through a stack of standard sieves, with the top sieve having the largest size opening and the bottom sieve having the smallest size opening.
[0095] Alternatively, the average diameter can be measured using any well-known microscopic method for sizing particles, such as optical or scanning electron microscopy, in combination with any image analysis software, such as the software commercially available as freeware from the NIH, Bethesda, Maryland, under the trademark "IMAGE J."
[0096] In one embodiment, the plurality of microspheres has a size distribution that differs by no more than 40% (30% or even 20%) based on the average microsphere diameter.
[0097] adhesive layer
[0098] In some embodiments, multi-layer articles of the present disclosure include an adhesive layer that extends across the primer layer and directly contacts a major surface of the elastomeric layer that faces away from the primer layer.
[0099] In one embodiment, the adhesive layer is a pressure-sensitive adhesive, and is usually tacky under ambient conditions.Suitable pressure-sensitive adhesives can be based on polyacrylates, polymethacrylates, synthetic and natural rubbers, polybutadienes and copolymers, or polyisoprenes and copolymers.Silicone adhesives such as polydimethylsiloxanes and polymethylphenylsiloxanes can also be used.
[0100] Particularly preferred pressure-sensitive adhesives include poly(meth)acrylate adhesives, which can exhibit advantageous properties such as high transparency, UV stability and aging resistance.The poly(meth)acrylate adhesives that can be used for surface treatment film applications are described in, for example, U.S. Patent No. 4,418,120 (Kealy et al.), U.S. Patent No. RE24,906 (Ulrich), U.S. Patent No. 4,619,867 (Charbonneau et al.), U.S. Patent No. 4,835,217 (Haskett et al.) and International Patent Publication WO87 / 00189 (Bonk et al.).
[0101] Preferably, the poly(meth)acrylate pressure sensitive adhesive is a C4 to C12 The adhesive comprises a crosslinkable copolymer of alkyl acrylate and (meth)acrylic acid. The adhesive can be used with or without a crosslinker. Useful crosslinking reactions include chemical and ionic crosslinking. Chemical crosslinkers can include polyaziridines and / or bisamides, and ionic crosslinkers can include metal ions of aluminum, zinc, zirconium, or mixtures thereof. Mixtures of chemical and ionic crosslinkers can also be used. In some embodiments, the poly(meth)acrylate pressure sensitive adhesive includes a tackifier such as a rosin ester. The adhesives useful in the present disclosure may also contain additives such as ground glass, titanium dioxide, silica, glass beads, waxes, tackifiers, low molecular weight thermoplastics, oligomeric species, plasticizers, pigments, metal flakes, and metal powders, so long as they are provided in amounts that do not unduly degrade the quality of the adhesive's bond to the surface.
[0102] As an alternative to a pressure sensitive adhesive, the adhesive layer may be a hot melt adhesive that is not tacky at room temperature but becomes tacky when heated. Such adhesives include acrylic, ethylene vinyl acetate, and polyurethane materials.
[0103] Generally, the adhesive layer has a thickness of at least 15, 20, 25, 30, or even 40 micrometers, and up to 50, 60, 75, or even 90 micrometers.
[0104] In certain applications, it may be desirable to be at least initially repositionable so that the sheet can be adjusted to fit a desired location before a permanent bond is formed. Such repositionability can be achieved, for example, by providing a layer of microscopic glass bubbles on the adhesive surface, as disclosed in U.S. Patent No. 3,331,729 (Danielson et al.).
[0105] Optional liner
[0106] When a pressure sensitive adhesive is used, a liner may be placed on the pressure sensitive adhesive opposite the elastomeric layer. The liner is not intended for the end use of the adhesive article, but is a temporary support used to support and / or protect the adhesive layer during manufacturing or storage. The liner is removed from the adhesive layer prior to use. Such liners are known in the art.
[0107] Typically, the liner comprises a support such as a polymer film (such as polyolefin or polyester) or paper (such as crepe or kraft paper) coated with a release agent. Such release agents are known in the art and are described, for example, in "Handbook of Pressure Sensitive Adhesive Technology", D. Satas, editor, Van Nostrand Reinhold, New York, NY, 1989, pp. 585-600. Examples of release agents include carbamates, silicones, and fluorocarbons. In one embodiment, the liner comprises a silicone-coated polyester or a silicone-coated paper.
[0108] In one embodiment, the 180 degree peel force to separate the adhesive layer (e.g., (meth)acrylic pressure sensitive adhesive) from the liner is at least 0.1, 0.2, 0.3, 0.4, 0.5, or even 0.6 N / mm, and up to 0.7, 0.8, 0.9, or even 1.0 N / mm at a speed of 12 inches / min (30 cm / min).
[0109] How to make it
[0110] In one embodiment, the articles disclosed herein can be made by a transfer process, where a monolayer of microspheres is held in a transfer polymer, which is then used to transfer the monolayer of microspheres onto a bead-binding layer. Such a transfer process is illustrated in Figures 2A-2E. Figure 2A shows a transfer carrier comprising a monolayer of microspheres 21 partially embedded in a transfer polymer 29. Typically, the transfer polymer is supported on a transfer support (not shown) to provide handling capabilities for the transfer carrier. Such transfer supports include, for example, a polyester layer. Such transfer carriers are described, for example, in U.S. Patent Application Publication No. 2015 / 0010723 (Krishnan et al.), paragraphs
[0021] -
[0029] , and in WO 2017 / 172888(A1), paragraphs
[0130] -
[0139] . In one embodiment, the transfer polymer is disposed on a transfer support layer and coated with microspheres, as discussed in the Examples section below. In another embodiment, the polymer disposed on the substrate can be obtained commercially (eg, from Felix Schoeller Group, Pulaski, NY) and the microspheres are then coated onto the commercial product.
[0111] In one embodiment, the multiple microspheres are randomly distributed on the transfer carrier and are densely packed (ie, there is generally not enough space between adjacent microspheres to place another microsphere).
[0112] In one embodiment, a plurality of microspheres are patterned on the surface of a transfer carrier and thus on the resulting finished article. WO 2017 / 106239 (Clark et al.), incorporated herein by reference, discloses a monolayer of microspheres arranged in a microperiodic pattern, where the microspheres are arranged in a pattern (i.e., in relation to other microspheres) at a microscopic level, and the pattern is periodic (i.e., not random, but has order). The repeating units, i.e., the areas consuming the repeating pattern, may have triangles, quadrilaterals (e.g., squares, diamonds, rectangles, parallelograms), hexagons, or other repeating pattern shapes, which may be symmetric or asymmetric in nature. WO 2017 / 024711 (Walker et al.), incorporated herein by reference, discloses a monolayer of randomly distributed microspheres arranged in a predetermined pattern on a surface. The predetermined pattern includes at least one of: (i) a plurality of first regions; (ii) a plurality of second regions; and (iii) a combination thereof. In one embodiment, the plurality of microspheres in the second regions are closely packed. Exemplary shapes of the first and second regions include lines (or stripes), triangles, hexagons, rectangles, or ellipses. The pattern may be pseudorandom, i.e., the pattern may appear random but may not actually be random. Pseudorandom patterns are typically less noticeable to the naked eye than regular patterns.
[0113] As shown in Figure 2B, the bead-binding layer 22 is applied to the transfer carrier such that the microspheres are located between the bead-binding layer 22 and the transfer polymer 29. The bead-binding layer is made from a liquid reaction mixture and therefore can be coated using any known technique, such as coating or extrusion.
[0114] In an exemplary extrusion process, the reaction mixture components of the bead-tie layer are first mixed into two separate parts to prevent premature reaction. One part can be prepared by first mixing the polyol component with the hydroxy-functional silicone poly(meth)acrylate, a suitable solvent, and any optional additives. The other part contains the isocyanate component along with any solvent or optional additives. The first and second parts are then mixed in appropriate amounts to obtain the desired NCO:OH ratio. In these embodiments, the NCO:OH ratio can be selected to be between 0.75 and 1.25.
[0115] Once mixed, the bead-bound reaction mixture can be coated onto the transfer carrier containing the microspheres. The coating can be made using conventional equipment such as a knife coater, roll coater, reverse roll coater, notched bar coater, curtain coater, rotogravure coater, or rotary printer. The coating can be spread by hand or automated and may be performed according to either a batch or continuous process. The viscosity of the bead-bound reaction mixture can be adjusted as needed to suit the type of coater used.
[0116] After coating, the bead-attached layer can be subjected to heat and / or vacuum to remove the organic solvent and any other volatile components, heat activate the curing reaction between the polyol and the isocyanate, and partially cure the bead-attached layer. In one embodiment, the reaction mixture used to form the bead-attached layer is substantially free (i.e., less than 1, 0.5, 0.1, or even 0.05 wt %, or even no) of photoactive curing agent. In some embodiments, the bead-attached layer is 30% to 90% cured.
[0117] Partial curing of the bead-tie layer has been found to improve adhesion of the primer layer to the bead-tie layer, particularly when the primer layer is disposed over the partially cured bead-tie layer and both layers are cured together, whereas full curing of the bead-tie layer has been observed to reduce adhesion between the bead-tie layer and the primer layer.
[0118] An oven can be used to first evaporate the solvent and partially cure the bead-bound layer. Generally, the drying / curing steps are performed in air. If continuous processes are used, these processes can operate on a moving web. In an exemplary continuous process, a wet coating 0.0076 centimeters (0.003 inches) thick can have a solids content of about 45% and can be dried and cured using a temperature profile with a dwell time of 2 minutes at 80°C, followed by a dwell time of 10 minutes at 125°C.
[0119] In general, the bead-bonded layer is preferably dried and / or cured at a predetermined temperature of at least 25, 20, 35, 40, 50, or even 60° C. up to 80, 90, 100, 110, 120, 130, 140, or even 150° C. The residence time at a given temperature is highly temperature dependent, but can be at least 5, 10, 20, 30, 45, or even 60 seconds up to 120, 150, or even 180 seconds. The bead-bonded layer is preferably subjected to a residence time and temperature or temperature range that balances solvent removal and curing effectiveness with overall throughput and energy efficiency.
[0120] As shown in FIG. 1, the bead bonding layer 22 conforms to the plurality of microspheres such that its second major surface 13 (the surface opposite the monolayer of microspheres) is wavy. Depending on the bead bonding reaction mixture and curing conditions, the cured bead bonding layer may not have a uniform thickness throughout the layer. For simplicity, reference will be made to the effective thickness of the bead bonding layer. The effective thickness of the bead bonding layer is the average theoretical thickness of the bead bonding layer assuming a linear profile. In one embodiment, the effective thickness of the bead bonding layer is at least 12, 15, 20, 25, 30, 35, or even 40 micrometers, and up to 50, 60, 75, or even 85 micrometers. In one embodiment, the bead bonding layer needs to be thick enough to strongly attach the microspheres, but not so thick that it may crack when bent (e.g., rolling the finished article or bending the finished article around a curved object).
[0121] As shown in Figure 2C, primer layer 24 is applied directly onto bead-attaching layer 22. Any known method can be used to place the primer layer onto the underlying bead-attaching layer, including any of those described above for coating the bead-attaching layer.
[0122] Typically, heat is applied to evaporate water and / or any other volatile species and then cure the primer layer and the bead-bonded layer. The oven temperature profile may be similar to that described above for partially curing the bead-bonded layer. However, the degree of cure need not be limited to this second cure cycle, so it may be advantageous to use a higher temperature or increase the duration of the curing step if the temperature does not increase significantly.
[0123] In some embodiments, the bead-attaching layer and the primer layer can continue to cool and cure after the heating step and before any further coating or lamination steps. This can be accomplished by aging the multilayer article including these layers at ambient conditions. Aging is performed for at least 1 week, at least 2 weeks, at least 3 weeks, or at least 4 weeks to allow the bead-attaching layer and the primer layer to reach a generally stable and consistent degree of crosslinking.
[0124] The primer layer contains excess unreacted amine (e.g., at least 3, 4, or even 5% and up to 6, 7, 8, 9, or even 10% by weight amine), allowing the primer layer to covalently bond with the bead attachment layer 22 and the subsequently added elastomer layer 26, as shown in FIG. 2D.
[0125] An elastomeric layer 26 is disposed on the exposed major surface of the primer layer 24. In one embodiment, both the bead-bonded layer and the primer layer are fully cured. In some embodiments, the elastomeric layer may be melt processed and coated onto the primer layer from the melt. In an alternative embodiment, the elastomeric layer may be melt processed and separately formed into a uniform sheet and then subsequently hot laminated to the exposed primer layer.
[0126] In one embodiment, the elastomeric layer 26 can be formed by extruding the reactive polyurethane mixture through a die directly onto the primer layer 24 (e.g., using a twin screw or planetary extruder). The components of the reactive mixture (e.g., diisocyanate, diol chain extender, and polyester polyol) can be fed into the extruder individually or simultaneously. An example of a suitable die includes a coat hanger die. The uniform film can be further pressed by a cold roller that thermally quenches the reactive formation of the polyurethane, thereby solidifying the polyurethane thermoplastic elastomer. The extrusion can be performed at any suitable temperature. For example, the temperature can range from 40, 50, 60, 70, 80, 90, or even 100° C. up to 175, 200, 210, 220, or even 230° C. The extrusion can occur for any suitable amount of time. For example, the extrusion process (eg, in making a continuous web) can occur for a time ranging from at least 0.5, 1, 2, 4, or even 6 hours up to 10, 12, 15, or even 17 hours.
[0127] Additional layers can be applied to the multilayer article including the adhesive layer and the liner, not shown in FIG. 2D. For example, the adhesive layer may be coated directly onto the remaining layers of the article, or formed into an adhesive film and then laminated to the bulk layers in a subsequent step. In the latter case, a sacrificial release liner is typically placed in contact with the adhesive layer to facilitate handling and storage of the web. To apply a pressure-sensitive adhesive layer to the elastomeric layer, it may be desirable to corona treat (e.g., air or N2 corona treat) and thermally laminate the major surface of the extruded elastomeric layer, for example, to be bonded to the pressure-sensitive adhesive layer. To achieve this, the major surface of the elastomeric layer that is not in contact with the primer layer is exposed and then corona treated. If a hot laminating process is used (e.g., the elastomeric layer is extruded onto a releasable carrier web or liner), the carrier web or liner may first be peeled away from the elastomeric layer.
[0128] The primer layer and the elastomeric layer can be bonded together, for example, by laminating the layers at elevated temperature and pressure. For example, one major surface of the primer layer can be cold laminated under pressure to one major surface of the extruded elastomeric layer, while at least one major surface of the elastomeric layer, or of both the elastomeric layer and the primer layer, is at an elevated temperature high enough to facilitate proper bonding between the primer layer and the elastomeric layer. As used herein, cold laminating refers to layers that are laminated together between two nip surfaces at about room temperature or in an ambient temperature environment (e.g., the layers are not intentionally kept in a heated environment during the laminating process). The nip surfaces can be two nip rollers, a fixed nip surface (e.g., a low friction surface of a flat or curved plate) and one nip roller, or two stationary nip surfaces. The laminating process can also be carried out in an environment below ambient temperature (i.e., the layers are purposely cooled during the laminating process). For example, one or both of the nip surfaces can be cooled to a temperature below ambient temperature to cool the exposed major surfaces of the polyurethane layers (i.e., the major surfaces that the nip surfaces contact). The use of such cooled surfaces can help eliminate, or at least reduce, warping of the layers resulting from the laminating process. At the same time, the major surfaces that contact at the interface between the polyurethane layers are maintained at a high enough temperature to be adequately bonded by the laminating pressure applied by the nip surfaces. Such cold laminating can be accomplished by laminating a freshly extruded elastomeric layer directly onto a preformed primer layer, while the material of the elastomeric layer still retains significant heat from the extrusion process.The multi-layer article including the primer layer may still be releasably bonded to a carrier web or liner to provide additional structural strength.
[0129] Alternatively, one major surface of the primer layer can also be bonded to one major surface of the extruded polymer layer by using a hot laminating process. In this process, the initial temperatures of both the primer layer and the elastomeric layer are about room temperature, or at least too low to facilitate proper bonding between the primer layer and the elastomeric layer. Then, at least one major surface of the elastomeric layer, at least one major surface of the primer layer, or one major surface of both the primer layer and the elastomeric layer are heated to an elevated temperature sufficiently higher than room temperature to facilitate proper bonding between the primer layer and the elastomeric layer under laminating pressure. In a hot laminating process, the layers are heated before or during the application of laminating pressure. When a hot laminating process is used, the major surface of the elastomeric layer can be peelably laminated to an easily peelable carrier web or liner (e.g., a polyester carrier web) immediately after the elastomeric layer is extruded to provide additional structural support for the new polymer layer.
[0130] The minimum acceptable temperatures and pressures for bonding the layers together using either the cold or hot lamination process include temperatures of at least about 200°F (93°C) and pressures of at least about 15 lb / in 2 (pounds / inch 2 or psi) (10.3 N / cm 2 (Newtons / centimeter 2 )) pressure is included.
[0131] In one embodiment, the transfer polymer layer 29 is removed from the bead-binding layer 22, resulting in a plurality of microspheres being transferred to the bead-binding layer, ultimately resulting in a microsphere-coated polyurethane article 20, as shown in FIG. 2E. The transfer polymer layer (and transfer carrier) is typically removed after the adhesive layer and liner are assembled onto the multilayer article. Typically, at least one stiff layer needs to be part of the multilayer article to allow handling of the article during further processing. Typically, this stiff layer is either a release liner attached to the adhesive layer of the article or is part of the transfer carrier. The transfer carrier (including the transfer polymer and corresponding transfer support layer) may be removed during manufacturing or by the end user immediately prior to application of the multilayer article onto the surface to be protected.
[0132] Additional Layers
[0133] In addition to the aforementioned elastomeric, primer, bead bonding, and microsphere layers, as well as optional adhesives and release liners, the resulting articles of the present disclosure may also include additional layers that impart desirable properties to the article.
[0134] In one embodiment, an undercoat containing nanoparticles can be applied between the microsphere layer and the bead binding layer to provide stain resistance, as taught in U.S. Patent Application Publication No. 2015-0343502 (Clark et al.), which is incorporated herein by reference.
[0135] In one embodiment, the multilayer article may include pigments so that it also has graphic capabilities. Typically, if a graphic image is desired, the bead-binding layer is provided with at least one separate colored polymer layer on the surface opposite the microsphere layer. The optional colored polymer layer may include, for example, an ink. Examples of inks suitable for use in the present disclosure include, but are not limited to, pigmented vinyl polymers and copolymers, acrylic and methacrylic copolymers, urethane polymers and copolymers, copolymers of ethylene and acrylic acid, methacrylic acid and their metal salts, and blends thereof. The colored polymer layer may be an ink and may be printed by a range of methods, including, but not limited to, screen printing, flexography, offset printing, lithography, transfer electrophotography, transfer foil, and direct or transfer xerography. The colored polymer layer may be transparent, opaque, or translucent.
[0136] In one embodiment, the multi-layer article includes a thin coating of metal (eg, silver or aluminum) on the underside of the microspheres to act as a retroreflective mirror.
[0137] Goods
[0138] The multilayer articles of the present disclosure include a plurality of microspheres arranged in a monolayer (i.e., a single layer) on a surface of a bead-binding layer. The plurality of microspheres are partially embedded in the bead-binding layer, meaning that the microspheres are embedded (on average) at least 50, 55, 60, 65, or even 70% and no more than 80% of the average microsphere diameter into the bead-binding layer, while a portion of each microsphere (e.g., at least 10, 20, or even 25%) protrudes outward from the surface of the bead-binding layer.
[0139] Depending on the arrangement of the microspheres on the surface of the bead-binding layer (random vs. patterned), the microspheres cover more than 10, 15, 20, 25, or even 30% and less than 35, 40, 45, 50, 55, 60, 65, 70, or even 75% of the surface of the bead-binding layer. In one embodiment, the microspheres are randomly distributed and closely packed (i.e., generally there is not enough space between adjacent microspheres to place another microsphere) and the microspheres cover at least 65% and up to 80% of the first surface. Generally, it is preferred to have less than one average microsphere diameter between adjacent microspheres to achieve adequate wear resistance and minimize visual defects.
[0140] In one embodiment, the surface of the finished article can be polished to trim the exposed top surfaces of the microspheres in the microsphere monolayer. Such techniques are described in WO 2019 / 046407 (Clark et al.), which is incorporated herein by reference.
[0141] In one embodiment, the multi-layer article may be molded.
[0142] Uses and characteristics
[0143] The multi-layer articles provided can be useful in paint protection and paint replacement applications. These films can be applied to any of a wide variety of substrates. Such substrates can be flat or curved. When it is desired to adhere these articles to such curved surfaces, the articles preferably have sufficient flexibility to conform to the surface of the substrate without delaminating or wrinkling at the edges.
[0144] In one embodiment, the provided article is applied to a vehicle, aircraft, or watercraft. In some embodiments, the provided article is applied for protection to the exterior surfaces of automobiles (such as bumper fascias, pillar posts, rocker panels, wheel covers, headlights, door panels, trunk and hood lids, mirror housings, dashboards, floor mats, and door jambs), trucks, motorcycles, trains, airplanes (such as propeller blades, wings, or fuselages), rotorcraft, watercraft (such as hulls, transoms, bulwarks, and the like), and snowmobiles. In alternative embodiments, the articles of the present disclosure can be applied to surfaces of structures other than vehicles, such as fixtures, buildings, and architectural surfaces. Applications of these films can be either indoor or outdoor in nature.
[0145] In an exemplary method of application, the multilayer articles disclosed herein can be attached to a suitable substrate by simultaneously peeling the release liner from the adhesive layer while applying the film onto the substrate in a single continuous motion.
[0146] Advantageously, the bead-bonded layer provides a combination of desirable optical and mechanical properties that make it particularly suitable as an outermost layer in protective film applications.
[0147] In one embodiment, the article of the present disclosure is durable, i.e., the article of the present disclosure is abrasion and / or scratch resistant. Abrasion resistance can be measured by visually inspecting the sample for damage using a rotary Taber polisher. In one embodiment, the decorative article of the present disclosure is abrasion resistant with little or no visible abrasion. Scratch resistance can be measured by pencil hardness. In other words, the hardness at which a pencil scratches the surface. In one embodiment, the decorative article of the present disclosure has a pencil hardness value of at least 6H, 8H, or even 10H at a force of 2.5 Newtons. In one embodiment, the article of the present disclosure has a pencil hardness value of at least 3H, 5H, 6H, 8H, 9H, or even 10H at a force of 7.5 Newtons.
[0148] In one embodiment, the article of the present disclosure does not exhibit fingerprints.
[0149] The articles of the present disclosure may or may not be retroreflective. Typically, to be retroreflective, a thin layer of metal is used in the structure behind the embedded portion of the microspheres to achieve retroreflection. The retroreflectivity of an article is measured by its coefficient of retroreflectivity (R a ) R a =E r * d 2 / E s * A [In the formula, E r = Illuminance on the receiver E s = Illuminance on the plane perpendicular to the incident light at the position of the test specimen (E r (measured in the same units as d = distance from specimen to projector A = area of test surface] It can be expressed as: Coefficient of retroreflection (R a ) is further described in U.S. Patent No. 3,700,305 (Bingham). In one embodiment, the article of the present disclosure has a coefficient of retroreflection of 10 candela / lux / square meter or less, 5 candela / lux / square meter or less, 1 candela / lux / square meter or less, 0.5 candela / lux / square meter or less, or even 0.3 candela / lux / square meter or less, measured at an observation angle of 0.2° and an entrance angle of 5° according to ASTM E810-03(2013) "Standard Test Method for Coefficient of Retroreflection of Retroreflective Sheeting Utilizing the Coplanar Geometry".
[0150] In one embodiment, the multi-layer article is weather resistant. For example, the article is impermeable to water (such as rain and moisture), stable under exposure to ultraviolet light, and / or durable. For example, weather testing may include placing a panel of the multi-layer article in an exterior environment, e.g., at an angle of 45 degrees to the ground in Arizona and 5 degrees to the ground in Florida. The multi-layer article with a single layer of microspheres facing outward is exposed to the elements (e.g., rain, sun, wind, etc.) for 1 to 4 years.
[0151] In one embodiment, the multilayer article is stable to ultraviolet radiation and / or heat. In one embodiment, the multilayer article of the present disclosure is heat stable. Heat stability can be determined by adhesively attaching the multilayer article to a white painted panel and heating in an oven at 80° C. for 7 days. The CIELAB color space is used to monitor color change. In the CIELAB color space, L * is the brightness, a is * represents red / green, b represents * defines blue / yellow. In optical applications, b * The parameter is the blue-yellow scale defined by the CIE (International Commission on Illumination 1976 Color Space), so b * Lower values are selected as more desirable. In one embodiment, the article of the present disclosure has a b * is less than 2, 1, or even 0.5.
[0152] In one embodiment, the multi-layer article of the present disclosure is ultraviolet (UV) resistant. UV resistance can be determined in a similar manner as described above for thermal stability, except that the sample is exposed to ultraviolet radiation for a given period of time. In one embodiment, the article of the present disclosure exhibits a thermal stability of about 100% when exposed to ultraviolet radiation. * is less than 2, 1, or even 0.5. EXAMPLES
[0153] Unless otherwise noted, all parts, percentages, ratios, etc. in the examples and the rest of the specification are by weight, and all reagents used in the examples were obtained or available from general chemical suppliers, such as Sigma-Aldrich Company (Saint Louis, Missouri), or can be synthesized by conventional methods. [Table 1]
[0154] Transfer Carrier
[0155] A transfer carrier containing a monolayer of microspheres can be obtained as follows: borosilicate glass powder was flame treated by passing it twice through a hydrogen / oxygen flame at a rate of 3 grams / min, then collected in a stainless steel container, where a magnet was used to remove metallic impurities. The resulting glass microspheres were treated with 600 ppm of A1100 by the following method: Silane was dissolved in water, then added to the microsphere beads with mixing, air-dried overnight, and then dried at 110°C for 20 minutes. The dried silane-treated microsphere beads were then sieved to remove any agglomerates to obtain free-flowing beads with a size of 75 μm or less. The resulting transparent silane-treated microspheres were cascade coated using a mechanical sifter onto a transfer carrier film with a polyethylene-coated polyester (PET) film liner, preheated to about 140°C (284°F), to form a bead carrier with a uniform layer of transparent microspheres embedded in the polyethylene layer to a depth corresponding to about 30-40% of the diameter as determined by a magnification imaging system.
[0156] Test Method
[0157] Heat aging
[0158] This example was adhesively attached to the front side of a clearcoat whitecoat painted panel (available from ACT Painted Panels LLC, Hillsdale, MI) using an acrylic pressure sensitive adhesive layer. A Hunterlab UltraScan Pro Spectrophotometer (Hunter Associates Laboratory Inc., Reston, VA) was placed in front of a single layer of microspheres in the structure and used to determine the CIELAB color space. The sample (still adhered to the painted panel) was placed in an oven held at 80° C. for 7 days. The sample was removed from the oven, cooled, and the CIELAB color space was determined.
[0159] Taber abrasion test
[0160] Abrasion testing was performed according to standard procedures described in ASTM 1044-13. Testing was performed using a 5130 Abraser obtained from Taber Industry (North Tonawanda, NY). A coarse abrasive wheel CS17 (from the same company) with a load of 500 grams was used. The test was run for 200 cycles. After testing, the haze was visually inspected.
[0161] Gravel resistance
[0162] The fatigue test was performed at -20°C according to the standard procedure described in SAE (Society of Automotive Society) J400. A Gravel-O-Meter machine from Q-Lab Corporation (Westlake, OH) was used. The beaded films were applied onto ACT clearcoat white coat painted panels and conditioned at -20°C for 24 hours. The panels were then gravel tested with 1 pint of gravel at 70 psi. After the gravel test, the panels were visually inspected.
[0163] Profilometry
[0164] Profilometry images were generated with a DektakXT profilometer available from the Bruker Nano Surfaces Division of Bruker Corporation, Tucson, AZ. Images were generated using the MapScan feature of the instrument over a 1 mm x 1 mm surface area with a Z-axis range of 524 micrometers using a 2 micrometer radius stylus tip and 3 milligrams of stylus pressure. Scan resolution was 0.3 microns per data point in the scan, and 250 scans were stitched together with 4 microns between scans to create the image.
[0165] Comparative example A
[0166] A bead-binding composition was prepared by mixing 11 grams of propylene glycol methyl ether acetate, 18 grams of butyl acetate, 19 grams of methyl isobutyl ketone, 2.2 grams of cellulose acetate butyrate-381.01, 0.7 grams of TINUVIN-405, 0.35 grams of TINUVIN-292, 6.8 grams of CAPA-2054, 27.2 grams of JONCRYL-587AC, and 14.75 grams of xylene. The mixture was mixed for 30 minutes. After 30 minutes, 0.579 grams of 2,4-pentanedione, 0.021 grams of dibutyltin dilaurate, and 11.72 grams of DESMODUR N3900 were added to the mixture, and the clear and colorless solution was thoroughly stirred for 15 minutes.
[0167] The solution was then coated onto a monolayer on the microsphere side of the transfer carrier at a wet thickness of approximately 127 micrometers using a notch bar coater. The bead-bonded layer was dried and partially cured in an air oven at 195°F (90.6°C) for 5 minutes. The bead-bonded layer was allowed to stand at ambient conditions for 1 week. The bead-bonded layer had a glass transition temperature of 90°C as measured at 1 Hertz with a heating rate of 10°C / min using a dynamic mechanical analyzer (such as a DMA Q800).
[0168] The exposed surface of the bead-bound layer was primed by plasma treatment (Atto, Diener electronic GmbH+Co. KG, Ebhausen, Germany) using air as the process gas and set at a maximum power of 200 watts at 40 kilohertz for 5 minutes.
[0169] After allowing the primed bead-coated structure to sit overnight, an elastomeric layer was extruded onto the plasma-treated bead-bonded surface: 504.7 grams of pre-melted FOMREZ-44-111 (having a melt temperature of 60° C.) at 100° C., 5 grams of IRGANOX-1076, 0.3 grams of T12, 88.6 grams of 1,4 butanediol, 401.9 grams of DESMODUR W, 3 grams of TINUVIN-292, and 4.5 grams of TINUVIN-571 were fed separately into a twin-screw extruder. The extruder settings, conditions, and temperature profile were similar to those described in Example 1 and Table 1 of U.S. Pat. No. 8,551,285 (Ho et al.). The isocyanate index was NCO / OH=1.03 and the hard segment was 48.25 wt.%. The resulting aliphatic thermoplastic polyurethane was extruded onto the plasma-treated bead-tie layer as a 4 mil (100 micrometer) thick layer. The extruded elastomeric layer was heat laminated with the bead-tie layer to achieve good interfacial adhesion. The elastomeric layer had an elongation of about 600% as measured by ASTM D-882-18, e.g., using an Instron model 5565 (Norwood, MA), at a pull rate of 12 inches / minute (30 cm / minute) with a jaw gap of 1 inch (30 cm).
[0170] An acrylic pressure sensitive adhesive (isooctyl acrylate / acrylic acid copolymer) disposed on a 2 mil silicone coated polyethylene terephthalate release liner was heat laminated to the elastomeric layer at 190°F (88°C) under 35 psi (0.24 MPa) nip roll pressure. After one week, the polyethylene coated polyester film liner was removed from the transfer carrier. Visual inspection of the removed polyethylene coated polyester film liner showed that the microspheres had not transferred. Figure 3 shows a profilometry image of an approximately 1 mm x 1 mm section of the exposed surface of the sample after the polyethylene coated polyester film liner was removed.
[0171] Example 1
[0172] The bead binding composition was applied to a transfer carrier and dried in an oven as described in Comparative Example A.
[0173] The primer layer was prepared as follows: 89.30 grams of ALBERDINGK U933 was added with 0.35 grams of TINUVIN-123, 0.05 grams of AMP-95, 0.20 grams of TRITON GR-7M, 8.5 grams of butyl carbitol, 1.16 grams of UVINUL N3039, and 2 grams of NEOCRYL CX-100 and mixed homogeneously. The solution mixture was diluted with 10 grams of deionized water to maintain a viscosity of 100-200 centipoise.
[0174] A primer layer was coated onto the dried beaded bond layer at 100 micrometer wet thickness and cured in a 195°F (91°C) air oven for 10 minutes.
[0175] The elastomer layer was prepared and extruded as described in Comparative Example A. The elastomer layer was extruded onto the primer layer of the construction at a thickness of 4 mil (0.1 mm), and the elastomer layer was heat laminated with the primer layer to achieve good interfacial adhesion.
[0176] An acrylic pressure sensitive adhesive (isooctyl acrylate / acrylic acid copolymer) disposed on a 2 mil (0.05 mm) silicone coated polyethylene terephthalate release liner was heat laminated to the elastomeric layer at 190°F (88°C) under 35 psi (0.24 MPa) nip roll pressure. After one week, the polyethylene coated polyester film liner was removed from the transfer carrier. Visual inspection of the removed polyethylene coated polyester film liner showed little or no microspheres thereon. FIG. 4 is a profilometry image of an approximately 1 mm x 1 mm section of the exposed surface of the sample after removal of the polyethylene coated polyester film liner. A single layer on the microsphere side of the construction was then tested for Taber abrasion and gravel resistance, and the abraded construction showed no haze or chipped paint. The examples were also tested for heat aging with the following results: Delta L * =-0.15, delta a * =-0.05, delta b * = 0.45, and Delta E * =0.48.
[0177] Foreseeable modifications and variations of the present invention will be apparent to those skilled in the art without departing from the scope and spirit of the present invention. The present invention is not limited to the embodiments described in this application for illustrative purposes. In the event of any discrepancy or inconsistency between the description of this specification and the disclosure in any document mentioned in this specification or incorporated by reference, the description of this specification shall prevail. The present invention includes the following aspects. (1) (a) a microsphere layer including a plurality of microspheres arranged in a monolayer; (b) a bead-bonded layer having a first major surface and an opposing second major surface, the plurality of microspheres being partially embedded in the first major surface of the bead-bonded layer, the bead-bonded layer comprising a thermosetting polyurethane having a glass transition temperature of at least 35° C.; (c) a primer layer disposed on the second major surface of the bead-attached layer, the primer layer comprising a copolymer of polyurea and polyurethane, the primer layer being covalently bonded to the bead-attached layer via a urea bond; and (d) an elastomer layer disposed on the primer layer opposite the bead-attaching layer, the elastomer layer comprising a polyurethane thermoplastic elastomer; and Including, articles. (2) The article according to item 1, wherein the article is stable to ultraviolet radiation, heat, or a combination thereof. (3) The article according to item 1 or 2, wherein the elastomeric layer has an elongation at break of at least 200%. (4) The elastomer layer is Diisocyanate, A polymer diol; A diol chain extender; and a reaction product of the reaction mixture comprising Optionally, the diol chain extender has a weight average molecular weight of less than about 250 Daltons. (5) The article according to any one of items 1 to 4, wherein the weight average molecular weight of the polyurethane thermoplastic elastomer is within the range of 80,000 daltons to 400,000 daltons. (6) The article according to item 4 or 5, wherein the diisocyanate is selected from dicyclohexylmethane-4,4'-diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate, 1,4-phenylene diisocyanate, 1,3-phenylene diisocyanate, m-xylylene diisocyanate, tolylene-2,4-diisocyanate, toluene 2,4-diisocyanate, tolylene-2,6-diisocyanate, poly(hexamethylene diisocyanate), 1,4-cyclohexylene diisocyanate, 4-chloro-6-methyl-1,3-phenylene diisocyanate, hexamethylene diisocyanate, toluylene diisocyanate, diphenylmethane 4,4'-diisocyanate, 1,4-diisocyanatobutane, 1,8-diisocyanatooctane, or a mixture thereof. (7) The article according to any one of items 4 to 6, wherein the polymer diol is selected from at least one of polyester diols, polycaprolactone diols, polyether diols, polycarbonate diols, and polyolefin diols. (8) The article according to any one of items 4 to 7, wherein the diol chain extender is selected from ethylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, neopentyl glycol, 1,6-hexanediol, 1,4-cyclohexanedimethanol, or a mixture thereof. (9) The article according to any one of items 1 to 8, wherein the polyurethane thermoplastic elastomer contains a hard segment in the range of about 30% by weight to about 55% by weight. (10) The thermosetting polyurethane is A polyisocyanate, a polyol selected from the group consisting of polycaprolactone polyols, polycarbonate polyols, polyester polyols, acrylic polyols, polyether polyols, polyolefin polyols, and mixtures thereof; 10. The article according to any one of items 1 to 9, which is a reaction product of: (11) The article according to any one of items 1 to 10, wherein the thermosetting polyurethane is an organic solvent-based polyurethane. (12) The article according to item 10 or 11, wherein the polyisocyanate is a primary aliphatic polyisocyanate. (13) The article according to any one of items 1 to 12, wherein the primer layer is a water-based polyurethane. (14) The article according to any one of items 1 to 13, wherein the primer layer is essentially free of a hydroxy-functional silicone poly(meth)acrylate. (15) The article according to any one of items 1 to 14, wherein the refractive index of the plurality of microspheres is less than 1.9. (16) The article according to any one of items 1 to 15, wherein a surface of the plurality of microspheres comprises nucleophilic groups, and optionally the nucleophilic groups are amino groups. (17) The article according to any one of items 1 to 16, further comprising an adhesive layer disposed on the elastomer layer opposite the primer layer, optionally wherein the adhesive is a (meth)acrylic pressure-sensitive adhesive. 18. The article of claim 17, further comprising a disposable liner disposed on the pressure-sensitive adhesive layer opposite the elastomeric layer, optionally the disposable liner having a 180° peel force from the adhesive of 0.1 to 1.0 N / mm. (19) A method for making a bead-coated film, comprising the steps of: providing a transfer sheet comprising a transfer polymer layer having a monolayer of microspheres partially embedded thereon; coating the monolayer of embedded microspheres with a bead binding reaction mixture; partially curing the bead bonding reaction mixture to form a bead bonding layer, the bead bonding layer comprising a thermosetting polyurethane and having a glass transition temperature of at least 35° C.; contacting a primer reaction mixture onto the bead-bound layer; curing the second reaction mixture to form a primer layer, the primer layer comprising a copolymer of polyurea and polyurethane, the primer layer being covalently bonded to the bead binding layer via a urea bond; disposing a polyurethane thermoplastic elastomer on the primer layer; removing the transfer sheet to form the bead-coated film; A method comprising: 20. The method of claim 19, wherein the polyurethane thermoplastic elastomer is extruded onto the primer. (21) Use of an article according to any of items 1 to 18 in a vehicle, aircraft, or ship.
Claims
1. (a) a microsphere layer including a plurality of microspheres arranged in a monolayer; (b) a bead-bonded layer including a first major surface and an opposing second major surface, the plurality of microspheres being partially embedded in the first major surface of the bead-bonded layer, the bead-bonded layer comprising a thermosetting polyurethane having a glass transition temperature of at least 35° C.; (c) a primer layer disposed on the second major surface of the bead-attached layer, the primer layer comprising a copolymer of polyurea and polyurethane, the primer layer being covalently bonded to the bead-attached layer via a urea bond; and (d) an elastomer layer disposed on the primer layer opposite the bead-attaching layer, the elastomer layer comprising a polyurethane thermoplastic elastomer; and Including, articles.
2. The article of claim 1 , wherein the article is stable to ultraviolet radiation, heat, or a combination thereof.
3. The article of claim 1 or 2, wherein the elastomeric layer has an elongation at break of at least 200%.
4. The elastomer layer comprises: Diisocyanate, A polymer diol; A diol chain extender; and a reaction product of the reaction mixture comprising Optionally, the diol chain extender has a weight average molecular weight of less than about 250 Daltons.
5. The article of any one of claims 1 to 4, wherein the polyurethane thermoplastic elastomer has a weight average molecular weight in the range of 80,000 Daltons to 400,000 Daltons.
6. 5. The article of claim 4, wherein the diisocyanate is selected from dicyclohexylmethane-4,4'-diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate, 1,4-phenylene diisocyanate, 1,3-phenylene diisocyanate, m-xylylene diisocyanate, tolylene-2,4-diisocyanate, toluene 2,4-diisocyanate, tolylene-2,6-diisocyanate, poly(hexamethylene diisocyanate), 1,4-cyclohexylene diisocyanate, 4-chloro-6-methyl-1,3-phenylene diisocyanate, hexamethylene diisocyanate, toluylene diisocyanate, diphenylmethane 4,4'-diisocyanate, 1,4-diisocyanatobutane, 1,8-diisocyanatooctane, or mixtures thereof.
7. 7. The article of claim 4 or 6, wherein the polymeric diol is selected from at least one of polyester diols, polycaprolactone diols, polyether diols, polycarbonate diols, and polyolefin diols.
8. 8. The article of any one of claims 4, 6 and 7, wherein the diol chain extender is selected from ethylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, neopentyl glycol, 1,6-hexanediol, 1,4-cyclohexanedimethanol, or mixtures thereof.
9. The article of any one of claims 1 to 8, wherein the polyurethane thermoplastic elastomer comprises a hard segment in the range of about 30% to about 55% by weight.
10. The thermosetting polyurethane is A polyisocyanate, a polyol selected from the group consisting of polycaprolactone polyols, polycarbonate polyols, polyester polyols, acrylic polyols, polyether polyols, polyolefin polyols, and mixtures thereof; The article of any one of claims 1 to 9, which is the reaction product of:
11. The article of any one of claims 1 to 10, wherein the primer layer is a water-based polyurethane.
12. The article of any one of claims 1 to 11, wherein the primer layer is essentially free of hydroxy-functional silicone poly(meth)acrylates.
13. The article of any one of claims 1 to 12, wherein a surface of said plurality of microspheres comprises nucleophilic groups, optionally said nucleophilic groups being amino groups.
14. The article of any one of claims 1 to 13, further comprising an adhesive layer disposed on the elastomeric layer opposite the primer layer, optionally wherein the adhesive is a (meth)acrylic pressure sensitive adhesive.
15. 1. A method of making a bead coated film, comprising: providing a transfer sheet comprising a transfer polymer layer having a monolayer of microspheres partially embedded thereon; coating the monolayer of embedded microspheres with a bead binding reaction mixture; partially curing the bead bonding reaction mixture to form a bead bonding layer, the bead bonding layer comprising a thermosetting polyurethane and having a glass transition temperature of at least 35° C.; contacting a primer reaction mixture onto the bead-bound layer; curing the second reaction mixture to form a primer layer, the primer layer comprising a copolymer of polyurea and polyurethane, the primer layer being covalently bonded to the bead-attached layer via a urea bond; and disposing a polyurethane thermoplastic elastomer on the primer layer; removing the transfer sheet to form the bead-coated film; and optionally wherein the polyurethane thermoplastic elastomer is extruded onto the primer.
16. Use of an article according to any one of claims 1 to 14 in a vehicle, aircraft or ship.
Citation Information
Patent Citations
Abrasion resistant microsphere article
JP2017512683A