Curable composition and synthetic leather

The curable composition addresses synthetic leather's durability and environmental impact by using a polyester polycarbonate polyol and polyisocyanate, enhancing flexibility and heat resistance while reducing solvent use.

JP7555473B2Active Publication Date: 2024-09-24ASAHI KASEI KOGYO KABUSHIKI KAISHA

Patent Information

Application Number
JP2023505526
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-03-08
Filing Date
2022-03-07
Publication Date
2024-09-24
Estimated Expiration
2042-03-07

AI Technical Summary

Technical Problem

Existing synthetic leathers face issues with insufficient sweat resistance and durability, requiring high solvent use during polyurethane polymerization, which impacts environmental sustainability and limits heat resistance.

Method used

A curable composition comprising a polyester polycarbonate polyol with specific hydroxyl values and a polyisocyanate with controlled functional groups, minimizing solvent use while enhancing flexibility, chemical resistance, and heat resistance.

Benefits of technology

The composition achieves an environmentally friendly synthetic leather with improved physical properties, including flexibility, chemical resistance, and heat resistance, suitable for applications requiring high durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007555473000042
    Figure 0007555473000042
  • Figure 0007555473000043
    Figure 0007555473000043
  • Figure 0007555473000037
    Figure 0007555473000037
Patent Text Reader

Abstract

The present invention provides a curable composition comprising component (a), which is a polyester polycarbonate polyol having a hydroxyl value of 40-75 mgKOH / g and having a specific structure, component (b), which is a polyol having a hydroxyl value of 100-280 mgKOH / g, and component (c), which is a polyisocyanate having two to six functional groups per molecule on average.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a curable composition and an artificial leather. [Background technology]

[0002] Conventionally, synthetic leathers with good flexibility have been obtained by applying a polyurethane resin solution polymerized using polyether polyols such as polypropylene glycol and polytetramethylene glycol to a fibrous substrate or a membrane plate and coagulating it in water. Although these synthetic leathers have excellent flexibility, they are susceptible to decomposition by components such as sweat and have problems with durability. There is also synthetic leather obtained by coagulating a polyurethane resin solution polymerized using polyester polyols obtained by reacting a hydroxy compound with a dibasic acid. This synthetic leather has problems with hydrolysis resistance.

[0003] As a synthetic leather for solving these problems, for example, Patent Document 1 discloses a synthetic leather obtained from a polyurethane resin polymerized using a polycarbonate diol. Specifically, Patent Document 1 discloses a porous sheet-like material in which a urethane composition consisting of a polyurethane consisting of a polycarbonate diol, an organic isocyanate, and a low molecular weight diol, and a polyurethane consisting of a polyester diol, an organic diisocyanate, and a low molecular weight diol is contained in or bonded to a fiber substrate and / or on the fiber substrate.

[0004] Patent Document 2 discloses a porous sheet material obtained by applying a solution of a polyurethane resin consisting of a polymer diol, an organic isocyanate, and optionally a chain extender to a substrate and carrying out a wet film-forming method. The porous sheet material is characterized in that the polymer diol is a mixed diol of a polycarbonate diol and a polyester diol, the polycarbonate diol is composed of 1,4-butanediol and one or more other alkanediols having 4 to 6 carbon atoms, the diol contains 50 to 90 mol % of 1,4-butanediol based on the total mole number of the diol, and is a copolymerized polycarbonate diol having a number average molecular weight of 500 to 5000, and the polyurethane resin has a coagulation value of 7 to 14.

[0005] Patent Document 3 discloses a surface coating layer for synthetic leather, which is made of a polyurethane resin composed of a polyester polycarbonate diol obtained by a transesterification reaction between an aliphatic oligocarbonate diol obtained by a transesterification reaction between an aliphatic diol and a dialkyl carbonate, and a polyester polyol obtained by ring-opening addition polymerization of a cyclic ester compound using a compound having an active hydrogen group as an initiator, a polyisocyanate, and a chain extender.

[0006] Patent Document 4 discloses a porous sheet material obtained by wet coagulation, which is composed of a polycarbonate diol (a1) made of an alkane diol having 4 to 6 carbon atoms and a polycarbonate diol (a2) made of an alkane diol having 7 to 12 carbon atoms, both of which are copolymerized polycarbonate diols, and which is obtained by reacting a polymer diol in which the percentage by weight of (a1) to the total weight of (a1) and (a2) is 10% to 80%, an organic isocyanate, and a chain extender.

[0007] Patent Document 5 discloses a synthetic leather comprising a surface layer formed from a composition for forming a surface material for a textile laminate, which is composed of a base agent and a curing agent, the base agent being a polycarbonate diol obtained from 1,6-hexanediol and a low molecular weight carbonate, the curing agent being a modified polyisocyanate (B1) of hexamethylene diisocyanate having a number average molecular weight of 350 to 500 and an average number of functional groups (f) of 2≦f<3, and an isocyanurate modified polyisocyanate (B2) of hexamethylene diisocyanate having f≧3, the ratio being (B1):(B2)=50:50 to 95:5 (weight ratio), and neither the base agent nor the curing agent containing an organic solvent.

[0008] Therefore, Patent Document 6 proposes a synthetic leather that uses a specific polycarbonate diol (a copolymer polycarbonate diol derived from 1,5-pentanediol and 1,6-hexanediol) in order to provide a synthetic leather that has an excellent balance of physical properties such as sweat resistance and flexibility and is also free from cracks and wrinkles during storage.

[0009] Patent Document 7 proposes a polyurethane for synthetic leather that has an excellent balance of physical properties including flexibility, chemical resistance, low-temperature characteristics, heat resistance, and touch. This polyurethane is obtained by reacting at least (a) a compound containing two or more isocyanate groups in one molecule, (b) a chain extender, and (c) a polycarbonate diol, characterized in that the polycarbonate diol (c) has a hydroxyl value of 20 mg-KOH / g or more and 45 mg-KOH / g or less, a glass transition temperature measured by a differential scanning calorimeter of -30°C or less, and the dihydroxy compound obtained by hydrolyzing the polycarbonate diol has an average carbon number of 3 or more and 5.5 or less.

[0010] In recent years, environmentally friendly polyurethanes have been proposed. For example, Patent Document 8 proposes a urethane prepolymer composition which is used by reacting a crosslinking agent with active hydrogen in the components to increase the molecular weight, the urethane prepolymer composition containing at least 20 to 80 mass% of a hydroxyl-terminated urethane prepolymer having a hydroxyl value of 10 to 100 mgKOH / g, and further containing 20 to 80 mass% of an oligomer having no urethane bonds and having a hydroxyl value of 20 to 400 mgKOH / g as a medium for the polymer, which can be crosslinked with the crosslinking agent, the urethane prepolymer composition being substantially 100% nonvolatile and being liquid at least at a temperature of 30°C, and a two-component, solvent-free polyurethane for synthetic leather which contains 90 to 150 equivalent % of a polyisocyanate crosslinking agent having an NCO content of 5 to 35 mass % relative to the average hydroxyl value of the urethane prepolymer composition. [Prior art documents] [Patent documents]

[0011] [Patent Document 1] Patent No. 3142102 [Patent Document 2] JP 2003-119314 A [Patent Document 3] JP 2004-346094 A [Patent Document 4] Patent No. 4177318 [Patent Document 5] JP 2009-185260 A [Patent Document 6] JP 2013-108196 A [Patent Document 7] JP 2016-8234 A [Patent Document 8] JP 2014-105250 A Summary of the Invention [Problem to be solved by the invention]

[0012] However, although the synthetic leathers disclosed in Patent Documents 1 to 5 have hydrolysis resistance, they do not have sufficient sweat resistance for applications requiring high durability, such as automobile seats.

[0013] Furthermore, the polycarbonate diol described in Patent Document 6 requires the use of a large amount of organic solvent during polyurethane polymerization, and further improvement is desired from the viewpoint of environmental load.

[0014] Furthermore, the polyurethane for synthetic leather disclosed in Patent Document 7 requires the use of a large amount of organic solvent during polyurethane polymerization, which is undesirable in terms of environmental impact.

[0015] In addition, the polyurethane prepolymer composition for synthetic leather disclosed in Patent Document 8 uses an ether polyol, such as poly-THF or THF-neopentyl glycol copolymer polyol, having a hydroxyl value of 20 to 400 mgKOH / g as an oligomer having no urethane bond in order to make the composition solvent-free, which results in reduced heat resistance and limited applications.

[0016] In view of the above problems, the present invention aims to provide an environmentally friendly curable composition that has an excellent balance of physical properties such as flexibility (touch), chemical resistance, low-temperature characteristics, and heat resistance, and uses a small amount of solvent. The curable composition is used for adhesives and coating agents that require flexibility, such as artificial leather. [Means for solving the problem]

[0017] Means for Solving the Problems The present inventors have conducted extensive research and have found that a curable composition containing a polyester polycarbonate polyol having a specified structure, a polyol having a specified hydroxyl value, and a specified polyisocyanate can provide an environmentally friendly synthetic leather that has an excellent balance of physical properties, including flexibility (touch), chemical resistance, low-temperature characteristics, and heat resistance, and can be produced using reduced amounts of solvents, thereby completing the present invention.

[0018] That is, the present invention includes the following aspects. [1] Component (a): A polyester polycarbonate polyol having a hydroxyl value of 40 to 75 mgKOH / g, which has a repeating unit represented by the following formula (1) and a repeating unit represented by the following formula (2) and / or the following formula (3) and has a hydroxyl group at the molecular end. [ka] (In formula (1), R1 is a divalent aliphatic or alicyclic hydrocarbon having 2 to 15 carbon atoms.) [ka] (In formula (2), R2 is a divalent hydrocarbon having 2 to 15 carbon atoms, and R3 is a divalent aliphatic or alicyclic hydrocarbon having 2 to 15 carbon atoms.) [ka] (In formula (3), R4 is a divalent hydrocarbon having 2 to 15 carbon atoms.) Component (b): polyol having a hydroxyl value of 100 to 280 mg KOH / g; A curable composition comprising: component (c): a polyisocyanate having an average number of functional groups per molecule of 2 to 6. [2] Component (d): an isocyanate-terminated prepolymer composition obtained by preliminarily reacting component (a) a polyester polycarbonate polyol having a hydroxyl value of 40 to 75 mgKOH / g with component (c) a polyisocyanate having an average number of functional groups per molecule of 2 to 6 at an equivalent ratio [isocyanate equivalent] / [hydroxyl equivalent] of 1.5 to 3.0; and Component (b) is a polyol having a hydroxyl value of 100 to 280 mgKOH / g; The curable composition according to [1], [3] Component (e): an isocyanate-terminated prepolymer composition obtained by preliminarily reacting a polyol having a hydroxyl value of 100 to 280 mgKOH / g (component (b)) with a polyisocyanate having an average functional group number per molecule of 2 to 6 (component (c)) at an equivalent ratio [isocyanate equivalent] / [hydroxyl equivalent] of 1.5 to 3.0; and Component (a) a polyester polycarbonate polyol having a hydroxyl value of 40 to 75 mgKOH / g; The curable composition according to [1], [4] The curable composition according to any one of [1] to [3], wherein a mass ratio of the polyester polycarbonate polyol as the component (a) to the polyol as the component (b) is 95 / 5 to 40 / 60. [5] The curable composition according to any one of [1] to [4], wherein a molar ratio of the structural unit represented by formula (1) to the structural units represented by formula (2) and / or formula (3) is 90 / 10 to 10 / 90. [6] The curable composition according to any one of [1] to [5], wherein 50 mol % or more of the repeating units represented by formula (1) include at least two kinds of repeating units selected from formulas (4), (5), and (6). [ka] [ka] [ka] [7] The curable composition according to any one of [1] to [6], wherein the polyol of the component (b) is a polycarbonate polyol having a repeating unit represented by formula (7) and a terminal hydroxyl group. [ka] (In formula (7), R5 is a divalent aliphatic or alicyclic hydrocarbon having 2 to 15 carbon atoms.) [8] The curable composition according to [7], wherein 50 mol % or more of the repeating units represented by formula (7) include at least two repeating units selected from formulas (8), (9), and (10). [ka] [ka] [ka] [9] The curable composition according to any one of [1] to [8], comprising an inert organic solvent in an amount of 40 mass % or less based on the total amount of the curable composition.

[10] The curable composition according to any one of [1] to [9], comprising 50 mass % or less of a polyester polyol based on the total amount of the curable composition.

[11] A synthetic leather obtained by using the curable composition according to any one of [1] to

[10] . Effect of the Invention

[0019] The curable composition of the present invention can provide an environmentally friendly cured product that has an excellent balance of physical properties including flexibility (touch), chemical resistance, low-temperature properties, and heat resistance, and uses a small amount of solvent. [Brief description of the drawings]

[0020] [Figure 1] FIG. 1 is a cross-sectional view of an example of synthetic leather using the curable composition of the present embodiment. [Diagram 2] FIG. 1 is a diagram showing an example of a process for producing synthetic leather using the curable composition of the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] Hereinafter, an embodiment for carrying out the present invention (hereinafter, abbreviated as "present embodiment") will be described in detail. Note that the present invention is not limited to the following embodiment, and can be carried out in various modifications within the scope of the gist of the present invention.

[0022] The composition of the present embodiment is Component (a): A polyester polycarbonate polyol having a hydroxyl value of 40 to 75 mgKOH / g, which has a repeating unit represented by the following formula (1) and a repeating unit represented by the following formula (2) and / or the following formula (3) and has a hydroxyl group at the molecular end. [ka] (In formula (1), R1 is a divalent aliphatic or alicyclic hydrocarbon having 2 to 15 carbon atoms.) [ka] (In formula (2), R2 is a divalent hydrocarbon having 2 to 15 carbon atoms, and R3 is a divalent aliphatic or alicyclic hydrocarbon having 2 to 15 carbon atoms.) [ka] (In formula (3), R4 is a divalent hydrocarbon having 2 to 15 carbon atoms.) Component (b): a polyol having a hydroxyl value of 100 to 280 mg KOH / g, and A curable composition containing component (c): a polyisocyanate having an average of 2 to 6 functional groups per molecule. The curable composition of the present embodiment forms a polyurethane by curing, that is, by reacting components (a) and (b) with component (c). The polyurethane obtained by this reaction can be used as an adhesive or coating agent for synthetic leather or other materials that require flexibility.

[0023] The curable composition of the present embodiment contains components (a), (b), and (c). The curable composition of this embodiment may be a mixture of components (a), (b) and (c), which can be obtained by the one-shot method described later. Alternatively, the curable composition of this embodiment may be a mixture of an isocyanate-terminated prepolymer composition obtained by reacting component (a) or component (b) with component (c) in advance, and the isocyanate-terminated prepolymer composition and component (b) or component (a) are blended to obtain the curable composition. Therefore, the composition of this embodiment also includes the following two aspects of the curable composition. The following two aspects can be obtained by the prepolymer method described later.

[0024] That is, in one aspect, the composition of the present embodiment is Ingredient (d): An isocyanate-terminated prepolymer composition in which component (a) a polyester polycarbonate polyol having a hydroxyl value of 40 to 75 mgKOH / g is reacted in advance with component (c) a polyisocyanate having an average number of functional groups per molecule of 2 to 6 at an equivalent ratio [isocyanate equivalent] / [hydroxyl equivalent] of 1.5 to 3.0; and Component (b) is a polyol having a hydroxyl value of 100 to 280 mg KOH / g. The curable composition comprises:

[0025] The composition of the present embodiment, in one aspect, comprises: Ingredient (e): An isocyanate-terminated prepolymer composition in which a polyol having a hydroxyl value of 100 to 280 mgKOH / g (component (b)) is reacted in advance with a polyisocyanate having an average functional group number per molecule of 2 to 6 (component (c)) at an equivalent ratio [isocyanate equivalent] / [hydroxyl equivalent] of 1.5 to 3.0; and Component (a) is a polyester polycarbonate polyol having a hydroxyl value of 40 to 75 mg KOH / g. The curable composition comprises:

[0026] The isocyanate-terminated prepolymer compositions of components (d) and (e) may contain unreacted component (c) and / or unreacted component (a) or component (b).

[0027] The synthetic leather obtained from the curable composition of the present embodiment has an excellent balance of physical properties such as flexibility (touch), chemical resistance, low-temperature characteristics, and heat resistance. In addition, the synthetic leather obtained from the curable composition of the present embodiment is an environmentally friendly synthetic leather that can be produced using a reduced amount of solvent.

[0028] In the curable composition of the present embodiment, at least two kinds of polyols (a) and (b) having different hydroxyl values ​​are used. By using two kinds of polyols having different hydroxyl values, the solubility in the solvent is increased, so that the amount of solvent used can be reduced compared to the use of one kind of polyol alone. In addition, without being bound by theory, it is considered that the advantages of a polyester polycarbonate polyol having a low hydroxyl value (high molecular weight) (contributing to the main physical properties such as flexibility) and a polyol having a high hydroxyl value (low molecular weight) (contributing to the reduction of the amount of solvent as a reactive diluent) are well balanced, and the physical properties of flexibility (touch), chemical resistance, low temperature properties, and heat resistance are excellent.

[0029] <Component (a)> The polyester polycarbonate polyol used in the curable composition of the present embodiment is a polyester polycarbonate polyol (component (a)) having a hydroxyl value of 40 to 75 mgKOH / g. The hydroxyl value of component (a) is preferably 45 to 70 mgKOH / g, and more preferably 50 to 65 mgKOH / g. By making the hydroxyl value of component (a) 40 mgKOH / g or more, the viscosity of the resulting curable composition can be kept low, and the amount of organic solvent used can be reduced. Also, by making the hydroxyl value of component (a) 75 mgKOH / g or less, the flexibility (touch) and low-temperature properties of the resulting synthetic leather tend to be improved.

[0030] The melt viscosity of the component (a) polyester polycarbonate polyol at 50°C is preferably 1000 to 6000 mPa·s, more preferably 1500 to 5000 mPa·s, even more preferably 1800 to 4500 mPa·s, and particularly preferably 2000 to 4500 mPa·s. When the melt viscosity of the component (a) at 50°C is 1000 mPa·s or more, the flexibility and low-temperature properties of the obtained cured product tend to be improved. When the melt viscosity of the component (a) at 50°C is 6000 mPa·s or less, the viscosity of the obtained curable composition can be kept low, and the amount of organic solvent used can be reduced.

[0031] The average number of hydroxyl groups in one molecule of the component (a) polyester polycarbonate polyol is preferably 1.7 to 3.5, more preferably 1.8 to 3.0, and even more preferably 2.0 to 2.5. When the average number of hydroxyl groups is 1.7 or more, the strength, chemical resistance, heat resistance, and hydrolysis resistance of the obtained cured product tend to be increased. In addition, when the average number of hydroxyl groups is 3.0 or less, not only an appropriate curing time is obtained, but also flexibility of the cured product is obtained.

[0032] In this embodiment, the polyester polycarbonate polyol (a) has a repeating unit represented by the following formula (1) and a repeating unit represented by the following formula (2) and / or the following formula (3), and has a hydroxyl group at the molecular end. The polyester polycarbonate polyol (a) is not particularly limited, but can be synthesized, for example, by using a bifunctional diol compound (and optionally a trifunctional or higher polyhydric alcohol), a dibasic acid and / or a cyclic ester compound, and a carbonate ester as raw materials, for example, by the transesterification reaction described in "Polymer Reviews, Vol. 9, pages 9-20" or the like. [ka] (In formula (1), R1 is a divalent aliphatic or alicyclic hydrocarbon having 2 to 15 carbon atoms.) [ka] (In formula (2), R2 is a divalent hydrocarbon having 2 to 15 carbon atoms, and R3 is a divalent aliphatic or alicyclic hydrocarbon having 2 to 15 carbon atoms.) [ka] (In formula (3), R4 is a divalent hydrocarbon having 2 to 15 carbon atoms.)

[0033] From the viewpoint of flexibility, R2 in formula (2) is preferably a divalent hydrocarbon having 2 to 15 carbon atoms and not containing an alicyclic structure.

[0034] The bifunctional diol compound used in the transesterification reaction is not particularly limited, and examples thereof include diols having a divalent aliphatic or alicyclic hydrocarbon skeleton having 2 to 15 carbon atoms. Specific examples of the bifunctional diol compound include ethylene glycol, 1,3-propanediol, 2-methyl-1,3-propanediol, 1,4-butanediol, neopentyl glycol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 2-methyl-1,8-octanediol, 1,11-undecanediol, and 1,12-dodecanediol. Examples of such hexanediol include 1,13-tridecanediol, 1,14-tetradecanediol, 1,15-pentadecanediol, 2-isopropyl-1,4-butanediol, 2-ethyl-1,6-hexanediol, 3-methyl-1,5-pentanediol, 2,4-dimethyl-1,5-pentanediol, 2,4-diethyl-1,5-pentanediol, 1,3-cyclohexanediol, 1,4-cyclohexanediol, and 1,4-cyclohexanedimethanol. These difunctional diol compounds may be used alone or in combination of two or more. Among these, from the viewpoint of obtaining a curable composition excellent in flexibility (touch), chemical resistance, low-temperature properties, and heat resistance, alkylene diols having 3 to 9 carbon atoms are preferred, and alkylene diols having 4 to 6 carbon atoms are more preferred. It is also preferred to use two or more alkylene diols in combination.

[0035] When the carbon number of the bifunctional diol compound is 2 or more, the viscosity of the curable composition can be kept low, the amount of organic solvent used can be reduced, and the flexibility and low-temperature properties of the obtained cured product tend to be improved.When the carbon number of the bifunctional diol compound is 15 or less, the chemical resistance of the obtained cured product tends to be excellent.

[0036] By using two or more bifunctional diol compounds in combination, the regularity of the structural unit of the polyester polycarbonate polyol obtained is decreased, and the crystallinity is decreased, so that not only is a polyester polycarbonate polyol liquid at room temperature (25°C) obtained, but the flexibility of the curable composition tends to be increased. Also, the amount of organic solvent used tends to be reduced. In this embodiment, in addition to the bifunctional diol, a trifunctional or higher polyhydric alcohol compound can be used as necessary as a raw material for the component (a) polyester polycarbonate polyol. The polyhydric alcohol compound is not particularly limited, but examples thereof include trimethylolethane, trimethylolpropane, hexanetriol, pentaerythritol, glycerin, etc. By using a polyhydric alcohol, the average number of hydroxyl groups in one molecule of component (a) can be easily adjusted to the range of 1.7 to 3.5.

[0037] In this embodiment, it is preferable that 50 mol % or more of the repeating units represented by formula (1) contain at least two repeating units selected from formulas (4), (5), and (6). The content of the repeating units of formulas (4), (5), and (6) is preferably 70 mol % or more, and more preferably 80 mol % or more.

[0038] [ka] [ka] [ka]

[0039] In one embodiment, among the repeating units represented by formula (1), at least two repeating units selected from formulas (4), (5), and (6) account for 50 mol % or more, preferably 65 mol % or more, and more preferably 80 mol % or more. By having these repeating units account for 50 mol % or more, the resulting synthetic leather is excellent in flexibility (feel), chemical resistance, low-temperature properties, and heat resistance, and the amount of inert organic solvent used tends to be reduced.

[0040] In this embodiment, when two kinds of repeating units are selected from formula (4), formula (5), and formula (6), the ratio of the two kinds of repeating units is 90:10 to 10:90, preferably 70:30 to 30:70, more preferably 60:40 to 40:60 in molar ratio. By the copolymerization ratio being within the above range, the crystallinity of the polyester polycarbonate polyol tends to be reduced, and a cured product having high flexibility, good low-temperature properties, and good touch tends to be obtained. Furthermore, if the copolymerization ratio is within this range, the amount of the inert organic solvent used tends to be reduced.

[0041] In this embodiment, when the three repeating units of formula (4), formula (5), and formula (6) are selected, the ratio of the structural units of formula (4), formula (5), and formula (6) is preferably 5 mol% or more, more preferably 10 mol% or more, and even more preferably 20 mol% or more, when the total of the three repeating units of formula (4), formula (5), and formula (6) is 100 mol%. When the ratio of each of the three repeating units of formula (4), formula (5), and formula (6) in the total of the three repeating units of formula (4), formula (5), and formula (6) is within the above range, the crystallinity of the polycarbonate diol is reduced, and synthetic leather having high flexibility, good low-temperature properties, and feel tends to be obtained. Furthermore, when the ratio of each of the three repeating units of formula (4), formula (5), and formula (6) is within the above range, the amount of inert organic solvent used tends to be reduced.

[0042] Dibasic acids that can be used in the synthesis of component (a) polyester polycarbonate polyol include aliphatic and / or aromatic dicarboxylic acids. Examples of aliphatic dicarboxylic acids include oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, and sebacic acid. Examples of aromatic dicarboxylic acids include phthalic acid, isophthalic acid, and terephthalic acid. In order to obtain a cured product with excellent flexibility, aliphatic dicarboxylic acids are particularly preferred, and among them, succinic acid, glutaric acid, and adipic acid are preferred. In addition, these dicarboxylic acids can also be used as esters of alcohols, and can be used as methyl esters such as dimethyl succinate, dimethyl glutarate, and dimethyl adipate. These dicarboxylic acids may be used alone or in combination.

[0043] Examples of cyclic esters that can be used in the synthesis of component (a) polyester polycarbonate polyol include α-acetolactone, β-propiolactone, γ-butyrolactone, σ-valerolactone, ε-caprolactone, cyclopentadecanolide, cyclohexadecanolide, etc. γ-butyrolactone, σ-valerolactone, and ε-caprolactone are particularly preferred, as they provide an excellent balance between the flexibility and chemical resistance of the curable composition.

[0044] The molar ratio of the polycarbonate structural unit represented by formula (1) to the polyester structural unit represented by formula (2) and / or formula (3) in the component (a) polyester polycarbonate polyol is preferably 90 / 10 to 10 / 90, more preferably 70 / 30 to 30 / 70, and even more preferably 60 / 40 to 40 / 60. By setting the molar ratio of the polycarbonate structural unit represented by formula (1) to the polyester structural unit represented by formula (2) and / or formula (3) in the above range, a cured product excellent in flexibility, chemical resistance, adhesiveness, and hydrolysis resistance can be obtained. Furthermore, by setting the molar ratio of the polycarbonate structural unit represented by formula (1) to the polyester structural unit represented by formula (2) and / or formula (3) in the above range, the amount of solvent used can be reduced.

[0045] Examples of carbonate esters that can be used in the synthesis of component (a) polyester polycarbonate polyol include dialkyl carbonates such as dimethyl carbonate, diethyl carbonate, dipropyl carbonate, and dibutyl carbonate; diaryl carbonates such as diphenyl carbonate; alkylene carbonates such as ethylene carbonate, trimethylene carbonate, 1,2-propylene carbonate, 1,2-butylene carbonate, 1,3-butylene carbonate, and 1,2-pentylene carbonate; etc. From the viewpoints of ease of availability and ease of setting polymerization reaction conditions, it is preferable to use dimethyl carbonate, diethyl carbonate, diphenyl carbonate, or ethylene carbonate as the carbonate ester.

[0046] In the production of component (a) polyester polycarbonate polyol, a catalyst may or may not be added. When a catalyst is added, it can be freely selected from catalysts used in normal transesterification reactions. As the catalyst, for example, a catalyst selected from metals such as lithium, sodium, potassium, rubidium, cesium, magnesium, calcium, strontium, barium, zinc, aluminum, titanium, cobalt, germanium, tin, lead, antimony, arsenic, and cerium, as well as metal salts, metal alkoxides, and organic compounds containing the metals can be used. Among the above catalysts, organic compounds containing titanium, tin, or lead are preferred. The amount of the catalyst used is usually 0.00001 to 0.1% of the mass of the bifunctional diol compound and the trifunctional or higher polyhydric alcohol that may be contained as necessary, which are raw materials.

[0047] In the present embodiment, as described above, the method for producing component (a) can be carried out by synthesizing the component (a) by an ester exchange reaction using a bifunctional diol compound (and optionally a trifunctional or higher polyhydric alcohol), a dibasic acid and / or a cyclic ester compound, and a carbonate ester as raw materials. More specifically, the transesterification reaction is carried out according to the following procedure. First, one or more bifunctional diol compounds in a predetermined ratio, one or more dibasic acids and / or cyclic ester compounds in a predetermined ratio, one or more carbonate esters in a predetermined ratio, and one or more trifunctional or higher polyhydric alcohols in a predetermined ratio as required are mixed together, and an ester exchange reaction is carried out at normal or reduced pressure in the absence or presence of an ester exchange catalyst at a temperature of 100 to 200°C, preferably 140 to 180°C.

[0048] Next, the alcohol derived from the carbonate ester and the water derived from the dibasic acid (when a dibasic acid ester is used, the monoalcohol derived from the dibasic acid ester) produced during the reaction are distilled off to obtain a polyester polycarbonate polyol having a molecular weight of about 300 to 500 g / mol.

[0049] Next, under reduced pressure at 130 to 230°C, preferably 150 to 200°C, the unreacted carbonate ester and bifunctional diol, and any optionally contained trifunctional or higher polyhydric alcohol, and water produced by the condensation reaction of the dibasic acid (when a dibasic acid ester is used, the monoalcohol derived from the dibasic acid ester) are distilled off, and a condensation reaction is carried out to obtain component (a), a polyester polycarbonate polyol, having the desired hydroxyl value. The average number of hydroxyl groups in the component (a), the polyester polycarbonate polyol, can be adjusted by controlling the initial charging ratio of each component, the amount of each raw material distilled during production, and the amount of the reaction product. When a polyester polycarbonate polyol is produced using a cyclic ester, it is possible to synthesize it by the above-mentioned transesterification reaction, but it is also possible to synthesize it by first synthesizing a polycarbonate polyol, then modifying the terminal hydroxyl groups of the polycarbonate polyol with an alkali metal or the like, and using the modified polycarbonate polyol as a polymerization initiation point to carry out ring-opening polymerization.

[0050] In the present embodiment, the component (a) polyester polycarbonate polyol can also be produced by first producing a polycarbonate polyol and a polyester polyol, mixing these polycarbonate polyol and polyester polyol, and carrying out a transesterification reaction at a temperature of 100 to 200°C under stirring in the presence or absence of the transesterification catalyst.

[0051] <Component (b)> Examples of the component (b) polyol used in the curable composition of this embodiment include polyether polyols, polyester polyols, polycarbonate polyols, polyolefin polyols, polybutadiene polyols, polyacrylic polyols, oil-modified polyols, etc. Among these, polycarbonate polyols are more preferred because the resulting cured product is excellent in heat resistance, chemical resistance, and hydrolysis resistance.

[0052] The component (b) polyol used in the curable composition of the present embodiment has a hydroxyl value of 100 to 280 mgKOH / g. The hydroxyl value of the component (b) polyol is preferably 130 to 250 mgKOH / g, more preferably 160 to 240 mgKOH / g. By using the component (b) polyol having a hydroxyl value of 100 mgKOH / g or more, the viscosity of the resulting curable composition can be kept low, and the amount of organic solvent used can be reduced. Also, by using the component (b) polyol having a hydroxyl value of 280 mgKOH / g or less, the resulting synthetic leather has excellent flexibility (touch) and low-temperature properties.

[0053] The melt viscosity of component (b) at 50°C is preferably 150 to 2000 mPa·s, more preferably 200 to 1500 mPa·s, further preferably 300 to 1300 mPa·s, and particularly preferably 300 to 1000 mPa·s. When the melt viscosity of component (b) polyol at 50°C is 150 mPa·s or more, the flexibility (touch) and low-temperature properties of the resulting synthetic leather tend to be excellent. In addition, when the melt viscosity of component (b) at 50°C is 2000 mPa·s or less, the viscosity of the resulting curable composition can be kept low, and the amount of organic solvent used can be reduced.

[0054] The average number of hydroxyl groups in one molecule of the component (b) polyol is preferably from 1.7 to 3.5, more preferably from 1.8 to 3.0, and even more preferably from 2.0 to 2.5.

[0055] The component (b) polyol is preferably a polycarbonate polyol having a repeating unit represented by formula (7) and a terminal hydroxyl group. [ka] (In formula (7), R5 is a divalent aliphatic or alicyclic hydrocarbon having 2 to 15 carbon atoms.)

[0056] When the polyol of component (b) is a polycarbonate polyol, it is not particularly limited, but for example, it can be synthesized by using a bifunctional diol compound (and, if necessary, a trifunctional or higher polyhydric alcohol) and a carbonate ester as raw materials, for example, by an ester exchange reaction as described in "Polymer Reviews, Vol. 9, pages 9 to 20" or the like.

[0057] The bifunctional diol compound used in the transesterification reaction is not particularly limited, and examples thereof include diols having a divalent aliphatic or alicyclic hydrocarbon skeleton having 2 to 15 carbon atoms. Specific examples of the bifunctional diol compound include ethylene glycol, 1,3-propanediol, 2-methyl-1,3-propanediol, 1,4-butanediol, neopentyl glycol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 2-methyl-1,8-octanediol, 1,11-undecanediol, and 1,12-dodecanediol. Examples of such hexanediol include 1,13-tridecanediol, 1,14-tetradecanediol, 1,15-pentadecanediol, 2-isopropyl-1,4-butanediol, 2-ethyl-1,6-hexanediol, 3-methyl-1,5-pentanediol, 2,4-dimethyl-1,5-pentanediol, 2,4-diethyl-1,5-pentanediol, 1,3-cyclohexanediol, 1,4-cyclohexanediol, and 1,4-cyclohexanedimethanol. These difunctional diol compounds may be used alone or in combination of two or more. Among these, from the viewpoint of obtaining a curable composition excellent in flexibility (touch), chemical resistance, low-temperature properties, and heat resistance, alkylene diols having 3 to 9 carbon atoms are preferred, and alkylene diols having 4 to 6 carbon atoms are more preferred. It is also preferred to use two or more alkylene diols in combination.

[0058] When the carbon number of the bifunctional diol compound is 2 or more, the viscosity of the curable composition can be kept low, the amount of organic solvent used can be reduced, and the flexibility and low-temperature properties of the obtained cured product tend to be improved.When the carbon number of the bifunctional diol compound is 15 or less, the chemical resistance of the obtained cured product tends to be excellent.

[0059] By using two or more kinds of bifunctional diol compounds in combination, the regularity of the structural unit of the obtained polycarbonate polyol is decreased, and the crystallinity is decreased, so that not only does it tend to give a liquid polycarbonate polyol at room temperature (25°C), but it also tends to increase the flexibility of the curable composition. Also, it tends to reduce the amount of organic solvent used. In the present embodiment, in addition to the bifunctional diol, a trifunctional or higher polyhydric alcohol compound can be used as the raw material of the polycarbonate polyol, if necessary. The polyhydric alcohol compound is not particularly limited, but examples thereof include trimethylolethane, trimethylolpropane, hexanetriol, pentaerythritol, glycerin, etc. By using a polyhydric alcohol, the average number of hydroxyl groups in one molecule of component (b) can be easily adjusted to the range of 1.7 to 3.5.

[0060] When the component (b) polyol in this embodiment is a polycarbonate polyol represented by formula (7), it is preferable that 50 mol % or more of the repeating units represented by formula (7) contain at least two types of repeating units selected from formulas (8), (9), and (10). [ka] [ka] [ka]

[0061] In this embodiment, the preferred mass ratio of the polyester polycarbonate polyol (a) and the polyol (b) is preferably 40 to 95 mass%, more preferably 60 to 85 weight%, and even more preferably 75 to 80 weight%, of the component (a) contained therein, when the total of the components (a) and (b) is taken as 100 mass%. When the proportion of the component (a) is 40 mass% or more, the flexibility (touch) and low-temperature properties of the obtained cured product tend to be more excellent. When the proportion of the component (a) is 95 mass% or less, the viscosity of the obtained curable composition is kept low, and the amount of organic solvent used tends to be reduced.

[0062] In the curable composition of the present embodiment, the components (a) and (b) are used, but polyols other than the components (a) and (b) may be used in combination as necessary. Here, the polyols other than the components (a) and (b) are not particularly limited as long as they are used in the normal production of polyurethane, and examples of such polyols include polyether polyols other than the components (a) and (b), polyester polyols, polycarbonate polyols, polyolefin polyols, polybutadiene polyols, polyacrylic polyols, and oil-modified polyols. The mass ratio of components (a) and (b) to the combined mass of components (a) and (b) and other polyols is preferably 50 mass% or more, more preferably 70 mass% or more, and even more preferably 80 mass% or more. When the mass ratio of components (a) and (b) is 50 mass% or more, the cured product tends to have an excellent balance of flexibility (touch), chemical resistance, low temperature properties, and heat resistance.

[0063] <Ingredient (c)> In the curable composition of the present embodiment, a polyisocyanate (component (c)) having an average of 2 to 6 functional groups per molecule is used. Examples of the component (c) in this embodiment include aromatic diisocyanates such as 2,4-tolysin diisocyanate, 2,6-tolysin diisocyanate and mixtures thereof, diphenylmethane-4,4'-diisocyanate (MDI), naphthalene-1,5-diisocyanate (NDI), 3,3'-dimethyl-4,4'biphenylene diisocyanate (TODI), and polymethylene polyphenylene polyisocyanate (PMDI); aromatic aliphatic diisocyanates such as xylylene diisocyanate (XDI) and phenylene diisocyanate; and aliphatic diisocyanates such as 4,4'-methylenebiscyclohexyl diisocyanate (hydrogenated (also called hydrogenated) MDI), hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI), and cyclohexane diisocyanate (hydrogenated XDI).

[0064] As the component (c) used in this embodiment, a polyisocyanate having an average of 2.1 or more isocyanate groups per molecule can also be used. Examples of polyisocyanates having an average of 2.1 or more isocyanate groups per molecule include aromatic polyisocyanates such as crude MDI and crude TDI; derivatives of aliphatic isocyanates such as HDI and IPDI, specifically diisocyanate derivatives such as biuret, allophanate, uretdione, and isocyanurate; and polyhydric alcohol adducts. The polyisocyanate having 2.1 or more isocyanate groups per molecule is not particularly limited, but examples thereof include Sumidur 44S, 44V70 (both manufactured by Sumika Bayer Urethane), Dismodur HL (manufactured by Sumika Bayer Urethane), which is a copolymer of TDI and HDI, and various Duranates manufactured by Asahi Kasei Corporation, namely, Duranate 24A-100, Duranate 22A-75PX, Duranate 18H-70B, Duranate 21S-75E, Duranate THA-100, Duranate TPA-100, Duranate-TKA100, Duranate MFA-75X, Duranate TSA-100, Duranate-TKA200, Duranate MFA-75X, Duranate TSA ... TKA200, Duranate TKA200, Duranate TKA200, Duranate TKA200, Duranate TKA200, Duranate TKA200, Duranate TKA200, Duranate TKA200 Available as Duranate TSS-100, Duranate TSE-100, Duranate D-101, Duranate D-201, Duranate P-301-75E, Duranate E-402-90T, Duranate E-402-90T, Duranate E-405-80T, Duranate ME20-100, Duranate 17B-60PX, Duranate TPA-B80X, Duranate MF-B60X, Duranate E-402-B80T, Duranate ME20-B80S, Duranate WB40-100, Duranate WB40-80D, Duranate WT20-100, Duranate WT30-100, etc.

[0065] Furthermore, it is also possible to use so-called blocked isocyanates in which component (c) is blocked with a known blocking agent, such as butanol, 2-ethylhexanol or other lower alcohols, methyl ethyl ketone oxime, lactams, phenols, imidazoles, active methylene compounds, etc.

[0066] The amount of component (c) used, expressed as [isocyanate equivalent of component (c)] / [total hydroxyl equivalent of both components (a) and (b)], is adjusted to be preferably 0.7 to 1.3, more preferably 0.8 to 1.2, and even more preferably 0.9 to 1.1. By making the [isocyanate equivalent of component (c)] / [total hydroxyl equivalent of both components (a) and (b)] 0.7 to 1.3, the molecular weight of the obtained polyurethane can be appropriately controlled, and the polyurethane tends to have excellent mechanical properties such as strength, elongation, and abrasion resistance.

[0067] It is preferable to use aromatic polyisocyanate such as MDI as component (c). By using aromatic polyisocyanate, it is likely to obtain a cured product with excellent mechanical properties. When aromatic polyisocyanate such as MDI is used as component (c) in the curable composition, the curable composition can be suitably used as an adhesive between the base fabric and the surface layer of synthetic leather. In addition, when an aliphatic polyisocyanate such as hydrogenated MDI is used as the component (c) in the curable composition, the curable composition can give synthetic leather having excellent weather resistance, and therefore the curable composition is suitably used as a curable composition for synthetic leather for a skin layer, etc.

[0068] <Chain extender> A chain extender can be used in the curable composition of the present embodiment as necessary. The chain extender is used to increase the abrasion resistance and strength of the resulting polyurethane, but on the other hand, it may reduce the flexibility of the resulting polyurethane, so it is used appropriately and as necessary. The chain extender is not particularly limited, but examples thereof include short-chain diols such as ethylene glycol and 1,4-butanediol; polyhydric alcohols such as trimethylolethane, trimethylolpropane, hexanetriol, pentaerythritol, and glycerin; and the like. The chain extender is not particularly limited, but examples thereof include diamines such as ethylenediamine, propylenediamine, hexamethylenediamine, tolylenediamine, xylylenediamine, diphenyldiamine, diaminodiphenylmethane, diaminocyclohexylmethane, piperazine, 2-methylpiperazine, and isophoronediamine, and water.

[0069] The amount of the chain extender added is preferably 30% by mass or less, more preferably 3% by mass to 20% by mass, and even more preferably 5% by mass to 10% by mass, based on the total amount of the components (a) and (b). It is desirable to adjust the amount of the isocyanate according to the amount of the chain extender added. For example, the isocyanate equivalent of the component (c) used is preferably adjusted to 0.7 to 1.3 equivalents, more preferably 0.8 to 1.2 equivalents, and even more preferably 0.9 to 1.1 equivalents, based on the total of the hydroxyl group equivalents of both the components (a) and (b) plus the equivalent of the functional group of the chain extender.

[0070] The chain extender can be used to adjust the physical properties of the cured polyurethane, such as strength, abrasion resistance, flexibility, etc. In addition, by using a polyhydric alcohol as a chain extender, the crosslink density of the resulting polyurethane can be increased, and the strength, abrasion resistance, and chemical resistance can be improved, and the resulting curable composition can be suitably used, particularly as a skin material for synthetic leather.

[0071] <Inert organic solvent> The curable composition of the present embodiment may contain an inert organic solvent as necessary to adjust the workability during urethane production. The content of the inert organic solvent is preferably 40% by mass or less, more preferably 3% by mass or more and 35% by mass or less, even more preferably 3% by mass or more and 30% by mass or less, and particularly preferably 5% by mass or more and 20% by mass or less, based on the total amount of the curable composition. Addition of an inert organic solvent is effective in lowering the viscosity of the curable composition, improving its workability, and further improving the appearance of the obtained cured product. On the other hand, it is preferable to suppress the content of the inert organic solvent to a small amount from the viewpoint of reducing the environmental load.

[0072] The inert organic solvent is not particularly limited as long as it is an organic solvent that is substantially inert to polyisocyanate, and is preferably one that does not have active hydrogen. The inert organic solvent is not particularly limited, but examples thereof include hydrocarbons such as pentane, hexane, heptane, octane, decane, petroleum ether, petroleum benzine, ligroin, petroleum spirit, cyclohexane, and methylcyclohexane; fluorine-based inert liquids such as trichlorofluoroethane, tetrachlorodifluoroethane, and perfluoroether fluorinated oils; perfluorocyclohexane, perfluorobutyltetrahydrofuran, perfluorodecalin, perfluoro-n-butylamine, perfluoropolyether, and dimethylpolysiloxane. These may be used alone or as a mixture. The inert organic solvent may further include methyl ethyl ketone (also referred to as MEK), acetone, ethyl acetate, butyl acetate, toluene, xylene, and other single or mixed solvents.

[0073] <Polyester polyol> In order to improve workability and adhesiveness during production, the curable composition of the present embodiment may contain polyester polyol, if necessary, in an amount of usually 50% by mass or less, preferably 5% by mass or more and 40% by mass or less, more preferably 10% by mass or more and 30% by mass or less, based on the total amount of the curable composition. When the content of polyester polyol is 50% by mass or less, the moist heat resistance (hydrolysis resistance) tends to be increased.

[0074] The polyester polyol is not particularly limited, but examples thereof include ethylene glycol adipate, propanediol adipate, butanediol adipate, 3-methyl-1,5-pentanediol adipate, polycaprolactone polyol, etc. The hydroxyl value of the polyester polyol is preferably 25 to 200 mgKOH / g, more preferably 30 to 130 mgKOH / g, and further preferably 40 to 70 mgKOH / g.

[0075] <Other additives> To the curable composition of the present embodiment, a curing accelerator (catalyst), a filler, a flame retardant, a dye, an organic or inorganic pigment, a release agent, a flowability adjusting agent, a plasticizer, an antioxidant, an ultraviolet absorber, a light stabilizer, an antifoaming agent, a leveling agent, a colorant, a foaming agent, and the like can be added depending on various applications.

[0076] The curing accelerator includes, but is not limited to, amines and metal catalysts. Examples of the amine effect accelerator include, but are not limited to, monoamines such as triethylamine and N,N-dimethylcyclohexylamine, diamines such as tetramethylethylenediamine, other triamines, cyclic amines, alcohol amines such as dimethylethanolamine, and ether amines. The metal catalyst is not particularly limited, but examples thereof include potassium acetate, potassium 2-ethylhexanoate, calcium acetate, lead octoate, dibutyltin dilaurate, tin octoate, bismuth neodecanoate, bismuth oxycarbonate, bismuth 2-ethylhexanoate, zinc octoate, zinc neodecanoate, phosphine, and phospholine.

[0077] The fillers and pigments are not particularly limited, but examples thereof include woven fabric, glass fiber, carbon fiber, polyamide fiber, mica, kaolin, bentonite, metal powder, azo pigments, carbon black, clay, silica, talc, gypsum, alumina white, barium carbonate, and the like.

[0078] The release agent, flow control agent, and leveling agent are not particularly limited, but examples thereof include silicone, aerosil, wax, stearates, and polysiloxanes such as BYK-331 (manufactured by BYK Chemicals).

[0079] The additives used in this embodiment are preferably an antioxidant, a light stabilizer, and a heat stabilizer. The antioxidant is not particularly limited, but examples thereof include phosphorus compounds such as aliphatic, aromatic, or alkyl group-substituted aromatic esters of phosphoric acid, phosphorous acid, hypophosphorous acid derivatives, phenylphosphonic acid, phenylphosphinic acid, diphenylphosphonic acid, polyphosphonates, dialkyl pentaerythritol diphosphites, and dialkyl bisphenol A diphosphites; phenol derivatives, particularly hindered phenol compounds; sulfur-containing compounds such as thioethers, dithioacid salts, mercaptobenzimidazoles, thiocarbanilides, and thiodipropionates; and tin compounds such as tin maleates and dibutyltin monoxide. These may be used alone or in combination of two or more.

[0080] <Method of manufacturing the cured product> A cured product using the curable composition of the present embodiment can be produced by a production method generally used industrially.

[0081] The curable composition of the present embodiment can be produced, for example, by a method in which components (a), (b), and (c) are mixed together and reacted (hereinafter referred to as the "one-shot method"). The curable composition of the present embodiment can be produced, for example, by a method in which components (a) and (c) are first reacted in advance to prepare a prepolymer composition (component (d)) having isocyanate groups at the terminals, and then component (b) is blended therein (hereinafter referred to as the "prepolymer method"), or by a method in which components (b) and (c) are first reacted in advance to prepare a prepolymer composition (component (e)) having isocyanate groups at the terminals, and then component (a) is blended therein (this method is also classified as the "prepolymer method").

[0082] (One-shot method) When the curable composition is obtained by the one-shot method, the amount of component (c) used is usually, in terms of isocyanate equivalent, preferably 0.7 to 1.3 equivalents, more preferably 0.8 to 1.2 equivalents, and even more preferably 0.9 to 1.1 equivalents, relative to the total hydroxyl group equivalents of both components (a) and (b). By using an amount of component (c) of 0.7 equivalents or more and 1.3 equivalents or less, the molecular weight of the obtained polyurethane can be appropriately controlled, and the mechanical properties such as strength, elongation, and abrasion resistance tend to be excellent. When the curable composition is obtained by the one-shot method, an inert organic solvent can be used for the purpose of improving the workability during production. In general, when a polyol (corresponding to components (a) and (b)) and a polyisocyanate (corresponding to component (c)) are mixed, the viscosity of the curable mixture increases over time. By adding an inert organic solvent to the curable composition, the viscosity of the composition can be reduced, and the application time tends to be extended.

[0083] When other additives are used, the other additives may be added at the same time when components (a), (b), and (c) are mixed together, or may be mixed in advance with component (a) and / or component (b).

[0084] (Prepolymer method) An example of the prepolymer method is a method in which component (a) and component (c) are reacted in advance to prepare an isocyanate-terminated prepolymer composition (also simply referred to as a prepolymer composition), and then component (b) is added. As an example of the prepolymer method, component (b) and component (c) are reacted in advance to prepare an isocyanate-terminated prepolymer composition, and then component (a) is added.

[0085] The ratio of component (a) or component (b) to component (c) during prepolymer synthesis is adjusted so that the equivalent ratio [isocyanate equivalent] / [hydroxyl equivalent] of the isocyanate group contained in component (c) to the hydroxyl group contained in component (a) or component (b) is 1.5 to 3.0, preferably 1.8 to 2.7, more preferably 1.9 to 2.3. When the [isocyanate equivalent] / [hydroxyl equivalent] during prepolymer synthesis is 1.5 or more, the molecular weight of the obtained prepolymer is appropriately controlled, the viscosity of the prepolymer is suppressed, and the use of organic solvents can be reduced. When the [isocyanate equivalent] / [hydroxyl equivalent] during prepolymer synthesis is 3.0 or less, the amount of unreacted component (c) is suppressed, and the obtained polyurethane tends to be prevented from becoming hard.

[0086] The ratio of the isocyanate-terminated prepolymer composition obtained by reacting the components (a) and (c) in advance to the component (b), or the ratio of the isocyanate-terminated prepolymer composition obtained by reacting the components (b) and (c) in advance to the component (a), expressed as [isocyanate equivalent of the prepolymer composition] / [hydroxyl value equivalent of the component (a) or component (b)], is preferably 0.7 to 1.3, more preferably 0.8 to 1.2, and even more preferably 0.9 to 1.1. By making the [isocyanate equivalent of the prepolymer composition] / [hydroxyl value equivalent of the component (a) or component (b)] 0.7 equivalents or more and 1.3 equivalents or less, the molecular weight of the polyurethane obtained can be appropriately controlled, and the polyurethane tends to have excellent mechanical properties such as strength, elongation, and abrasion resistance.

[0087] When the curable composition is obtained by the prepolymer method, an inert organic solvent can be used for the purpose of improving the workability during production. The amount of the inert organic solvent used is preferably 40% by mass or less. When the isocyanate-terminated prepolymer composition is mixed with the polycarbonate polyol, the viscosity of the curable composition increases over time. By adding an inert organic solvent to the curable composition, the viscosity of the composition can be reduced, and the application time tends to be extended.

[0088] When an inert organic solvent is used, the viscosity increases during the synthesis of the prepolymer, so it is preferable to add the inert organic solvent to component (a) or component (b) before the synthesis of the prepolymer and then carry out the prepolymer reaction. In addition, by using an inert organic solvent during the synthesis of the prepolymer, the reaction tends to proceed uniformly.

[0089] When other additives are used, the viscosity of the polycarbonate polyol tends to increase due to prepolymerization. Therefore, when other additives are mixed, it is preferable to add them to the polycarbonate polyol that has not been prepolymerized (component (a) or component (b) to be added later).

[0090] Comparing the one-shot method and the prepolymer method, the molecular weight of the soft segment portion can be adjusted more easily in the prepolymer method, and as a result, phase separation between the soft segment and the hard segment occurs more easily, and the flexibility and low-temperature properties of the obtained polyurethane tend to be excellent. Therefore, in one embodiment, the prepolymer method is preferred.

[0091] In the prepolymer method, when comparing the method of prepolymerizing component (a) with the method of prepolymerizing component (b), the method of prepolymerizing component (b) tends to lower the viscosity of the prepolymer obtained and reduce the amount of the inert organic solvent used.Therefore, in one embodiment, the method of prepolymerizing component (b) is preferred.

[0092] <Manufacturing method of synthetic leather> Synthetic leather can be produced from the curable composition of this embodiment. Examples of methods for producing synthetic leather from the curable composition of this embodiment include a wet method in which the curable composition of this embodiment is applied to or impregnated into a substrate (base fabric) and wet-solidified, and a dry method in which the curable composition of this embodiment is applied to release paper or a substrate (base fabric) and dried. Furthermore, as a method for producing synthetic leather, a transfer coating method (a type of dry method) can also be used in which the curable composition of the present embodiment is applied to release paper to form a skin material, and then the curable composition of the present embodiment is used as an adhesive layer on top of the skin material, and the release paper is removed after bonding to a substrate (base fabric). Since the curable composition of the present embodiment can reduce the amount of inert organic solvent used, a dry method (transfer coating method) is preferably used.

[0093] The method for producing synthetic leather will be explained below using the dry method as an example. Various substrates (base fabrics) can be used, and examples thereof include fibrous substrates. Examples of fibrous substrates include fiber assemblies in which fibers are shaped into nonwoven fabrics, woven fabrics, net fabrics, etc., or fiber assemblies in which each fiber is bonded with an elastic polymer. Examples of fibers used in the fiber assemblies include natural fibers such as cotton, hemp, and wool, regenerated or semi-synthetic fibers such as rayon and acetate, and synthetic fibers such as polyamide, polyester, polyacrylonitrile, polyvinyl alcohol, and polyolefin. These fibers may be either single spun fibers or mixed spun fibers. Other substrates include paper, release paper, plastic films of polyester or polyolefin, metal plates such as aluminum, and glass plates.

[0094] The curable composition of the present embodiment can be applied by a commonly used method, such as a floating knife coater, a knife over roll coater, a reverse roll coater, a roll doctor coater, a gravure roll coater, or a kiss roll coater.

[0095] The synthetic leather obtained can be used as it is. Alternatively, the synthetic leather can be obtained in a form in which a polymer solution or emulsion of polyurethane resin, vinyl chloride, cellulose resin, or the like is applied to the synthetic leather for the purpose of imparting various properties. The synthetic leather can also be obtained in a form of a laminate obtained by laminating a coating film obtained by drying the above-mentioned polymer solution or emulsion that has been applied separately to a release paper, and then peeling off the release paper.

[0096] Hereinafter, the present embodiment will be described with reference to the drawings. The drawings and manufacturing conditions described below are one embodiment of the present embodiment, and the present embodiment is not limited thereto.

[0097] Fig. 1 is a schematic cross-sectional view of a synthetic leather laminate produced by the dry method shown in Fig. 2. The structure of this laminate has a surface layer 2 on a substrate (nonwoven fabric) 4 with an adhesive layer 3 interposed therebetween. Release paper 1 used during production is attached to the outermost layer, but is peeled off before use.

[0098] 2 is a schematic diagram showing one of the methods for producing a dry synthetic leather laminate sheet using the curable composition of the present invention of this embodiment. In this production method, first, the raw materials of the curable composition of this embodiment, which have been adjusted to a predetermined temperature in advance, are mixed in a mixing head 5, and the resulting curable composition is allowed to flow down onto a release paper 1 (usually having a leather-like pattern). When the one-shot method is applied, components (a), (b), and (c), as well as an inert organic solvent, a chain extender, and additives as necessary, are fed separately, or component (c) and other raw materials (a mixture of components (a), (b), and an inert organic solvent, a chain extender, and additives as necessary) are continuously fed into a mixing head 5, mixed, and allowed to flow down onto the release paper 1. When the prepolymer method is applied, the prepolymer composition and the non-prepolymerized polycarbonate polyol or polyol (component (a) or component (b)), if necessary, an inert organic solvent, a chain extender, and additives are fed separately, or the prepolymer composition and the other raw materials (a mixture of non-prepolymerized polycarbonate polyol or polyol (component (a) or component (b)), if necessary, an inert organic solvent, a chain extender, and additives) are continuously fed into a mixing head 5, mixed, and allowed to flow down onto the release paper 1.

[0099] Each component before mixing is adjusted to a temperature of usually 20 to 80°C, preferably 30 to 70°C, more preferably 40 to 60°C. The temperature of the mixing head 5 is also adjusted to a temperature of usually 20 to 80°C, preferably 30 to 70°C, more preferably 40 to 60°C. When the temperature of each component before mixing and the temperature of the mixing head 5 are 20°C or higher, the viscosity of the raw materials used, particularly the polycarbonate polyol or polyol, tends to be suppressed and the flow rate tends to be stable. When the temperature of each component before mixing and the temperature of the mixing head 5 are 80°C or lower, the curing speed of the curable composition of this embodiment is appropriately controlled, a sudden increase in the viscosity of the curable composition is suppressed, and a uniform thickness of the synthetic leather tends to be obtained.

[0100] Thereafter, the mixture is passed through coating roll 8 to form a sheet of a certain thickness, and then passed through dryer 11 for hardening and drying of the inert organic solvent to form the synthetic leather skin layer 2. The temperature of the dryer is usually set to 60 to 150° C., preferably 70 to 130° C., and more preferably 80 to 120° C. The drying time is usually 2 to 15 minutes, preferably 3 to 10 minutes, and more preferably 4 to 7 minutes.

[0101] Next, the raw materials of the curable composition of this embodiment, which have been adjusted to a predetermined temperature in advance, are mixed in a mixing head 6, and the curable composition of this embodiment obtained is allowed to flow down to form an adhesive layer 3. When the one-shot method is applied to the production of the adhesive layer, components (a), (b), and (c), as well as an inert organic solvent, a chain extender, and additives, if necessary, are fed separately into a mixing head 6, or component (c) and other raw materials (a mixture of components (a), (b), and an inert organic solvent, a chain extender, and additives, if necessary) are fed continuously into the mixing head 6, mixed, and allowed to flow down onto the skin layer. When the prepolymer method is applied to the production of the adhesive layer, the prepolymer composition and the non-prepolymerized polyol (component (a) or component (b)), optionally an inert organic solvent, a chain extender, and additives, separately, or the prepolymer composition and a mixture of other raw materials (non-prepolymerized polyol (component (a) or component (b)), optionally an inert organic solvent, a chain extender, and additives), are continuously fed into a mixing head 6, mixed, and allowed to flow down onto the skin layer.

[0102] Each component before mixing is adjusted to a temperature of usually 20 to 60°C, preferably 30 to 50°C, more preferably 35 to 45°C. The temperature of the mixing head 6 is also adjusted to a temperature of usually 20 to 60°C, preferably 30 to 50°C, more preferably 35 to 45°C. When the temperature of each component before mixing and the temperature of the mixing head 6 are 20°C or higher, the viscosity of the raw materials used, particularly the polyester polycarbonate polyol, tends to be suppressed and the flow rate tends to be stable. When the temperature of each component before mixing and the temperature of the mixing head 6 are 60°C or lower, the curing speed of the curable composition of this embodiment is appropriately controlled, a sudden increase in the viscosity of the curable composition is suppressed, and a uniform thickness of the synthetic leather tends to be obtained.

[0103] Thereafter, the sheet is passed through a coating roll 8 to form a sheet of a certain thickness, and then passed through a dryer 11 for hardening and drying the inert organic solvent to form an adhesive layer 3 of synthetic leather. Next, the substrate 4 and the adhesive layer 3 are superimposed and pressed with a pressure roll 9 to obtain a post-sheet structure 7, which is then taken up by a take-up roll 10 to obtain a desired synthetic leather laminate. The temperature of the dryer 11 is usually set to 60 to 150°C, preferably 70 to 130°C, and more preferably 80 to 120°C. The drying time is usually 2 to 15 minutes, preferably 3 to 10 minutes, and more preferably 4 to 7 minutes.

[0104] FIG. 2 shows an example of the production of synthetic leather including three layers of a skin layer / an adhesive layer / a substrate, but a synthetic leather laminate including two layers of a skin layer / a substrate, omitting the adhesive layer, can also be produced in the same equipment. The adhesion between the skin layer and the substrate is controlled by adjusting the curing state of the curable composition. Specifically, the curable composition of the present embodiment can be obtained by pressing the substrate in a state where it is not completely cured. Therefore, the curing temperature of the dryer 11 is set to 60 to 150°C, preferably 70 to 130°C, and more preferably 80 to 120°C. The drying time is usually set to 2 to 15 minutes, preferably 3 to 10 minutes, and more preferably 4 to 7 minutes.

[0105] <Application> The synthetic leather obtained by using the curable composition of the present embodiment can be used for automobile interior materials such as automobile seats, furniture such as sofas, clothing, shoes, bags, other miscellaneous products, etc. It can also be used as a laminating adhesive for various films, a surface protective agent, etc. EXAMPLES

[0106] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples as long as it does not depart from the gist of the invention. In the following examples and comparative examples, the methods for analyzing and evaluating the physical properties of each component are as follows.

[0107] [Analysis and evaluation of polyester polycarbonate polyols and polyols] <Hydroxyl value of polyester polycarbonate polyol and polyol> Measurements were performed in accordance with JIS K1557-1.

[0108] <Polyester polycarbonate polyol and polyol composition (copolymerization ratio)> 1g of polycarbonate polyol or polyol sample was taken in a 100mL eggplant flask, 30g of methanol, and 8g of 28% sodium methoxide methanol solution were added, and the reaction was carried out at 100°C for 1 hour. After cooling the reaction solution to room temperature, 2-3 drops of phenolphthalein were added as an indicator, and the solution was neutralized with hydrochloric acid. After cooling in a refrigerator for 1 hour, the solution was filtered and analyzed using gas chromatography (GC). GC analysis was carried out using a gas chromatograph GC-14B (Shimadzu Corporation, Japan) equipped with DB-WAX (J&W, USA) as a column, diethylene glycol diethyl ester was used as an internal standard, and a hydrogen flame ionization detector (FID) was used as a detector, and quantitative analysis of each component was performed. The temperature rise profile of the column was held at 60°C for 5 minutes, and then raised to 250°C at 10°C / min. The composition (copolymerization ratio) of the polyester polycarbonate polyol or polyol was determined from the molar ratio of each alcohol component and the methyl ester component derived from a dibasic acid and / or the methyl ester component derived from a cyclic ester detected from the above analysis results. For the composition of polyester polycarbonate polyols containing dibasic acids, the number of moles of diols constituting the carbonate skeleton can be determined by subtracting the same number of moles of diol from the number of moles of methyl ester derived from the dibasic acid (when multiple diols are used, the ratio of diols determined by gas chromatography is subtracted as the same).

[0109] <Polycarbonate polyol and average number of functional groups of polyol> The average functionality of polycarbonate polyol synthesized using only diol monomer as raw material was 2. When polyfunctional monomer was included as raw material, the average functionality was calculated as follows. The number average molecular weight (Mn) of polycarbonate polyol was calculated by gel permeation chromatography (GPC) analysis (see below for GPC device and analysis conditions) in which a calibration curve was created using standard polystyrene of known molecular weight. The average functionality (n) per molecule was calculated by the following formula (11) using the hydroxyl value analyzed separately and the number average molecular weight (Mn) calculated by GPC. The same method was used for polyol.

[0110] Average number of functional groups (n) = [Mn] × ([OH value] × 10-3 / 56.1) (11)

[0111] GPC equipment: Tosoh HLC-8320 Column: TSKgel G4000H 1 piece G3000H 1pc G2000H 2pcs Eluent: THF (tetrahydrofuran) Flow rate: 1.0mL / min Column temperature: 40℃ RI detector: RI (built into the device HLC-8320)

[0112] <Melt Viscosity Measurement> The polyester polycarbonate polyol or polyol was preheated to 50° C., and then the melt viscosity was measured at 50° C. using an E-type viscometer (manufactured by Toki Sangyo Co., Ltd., TVE-22HT, cone: No. 6).

[0113] [Analysis and Evaluation of Prepolymer Compositions] <Melt Viscosity Measurement> The prepolymer composition was preheated to 50° C., and then the melt viscosity was measured at 50° C. under a nitrogen atmosphere using an E-type viscometer (manufactured by Toki Sangyo Co., Ltd., TVE-22HT, cone: No. 6).

[0114] <Measurement of isocyanate group concentration> 10 mL of di-n-butylamine / toluene (weight ratio: 25.85 / 865) mixed solution was diluted with 10 mL of dimethylformamide (DMF), and then titrated with 0.1 N hydrochloric acid propanol solution to measure the amount of hydrochloric acid propanol required for neutralization, which was used as the blank value. Then, 2 g of the prepolymer liquid was extracted, 10 mL of di-n-butylamine / toluene mixed solution was added, and the mixture was stirred at room temperature for 30 minutes, after which it was diluted with 10 mL of DMF in the same manner as in the blank measurement, and titrated with 0.1 N hydrochloric acid propanol solution to measure the amount of hydrochloric acid propanol solution required for neutralization, and the amount of remaining amine was quantified. The concentration of isocyanate groups was calculated from the volume of hydrochloric acid propanol solution required for neutralization using the following formula (12).

[0115] Isocyanate group concentration (mass%) =(V1-V2)×f×42×100 / (W×1000) (12)

[0116] V1: Amount of 0.1 N hydrochloric acid propanol solution required for blank measurement (mL) V2: Amount of 0.1 N hydrochloric acid propanol solution required for this measurement (mL) W: Sample used in this measurement (g) f: Factor of hydrochloric acid propanol solution

[0117] <Isocyanate equivalent> The isocyanate equivalent was calculated from the number of functional groups according to the type of polyisocyanate or prepolymer by the following formula (13). Isocyanate equivalent (mol) = charge weight (g) / molecular weight of isocyanate (g / mol) × number of functional groups (13)

[0118] <Hydroxyl equivalent> Similarly, the hydroxyl group equivalent was calculated from the number of functional groups according to the type of polyester polycarbonate polyol or polyol, according to the following formula (14). Hydroxyl equivalent (mol) = weight (g) / molecular weight of polyester polycarbonate polyol or polyol (g / mol) × number of functional groups (14)

[0119] [Analysis and evaluation of polyurethane films] <Preparation of polyurethane film> Each component of the curable composition, which had been preheated to 40°C, was added to a 200mL separable four-neck flask with stirring blades (four paddles inclined at 45°C) in an amount of 80g of the curable composition under a nitrogen atmosphere, and after stirring for 5 minutes at 40°C, the mixture was applied to a polypropylene resin sheet (width 100mm, length 1200mm, thickness 1mm) with an applicator to a width of 80mm, length 100mm, and thickness of 0.6mm, and dried for 2 hours on a hot plate with a surface temperature of 60°C, and then for 12 hours in an oven at 100°C. The mixture was then left to stand at a constant temperature and humidity of 23°C and 55%RH for 12 hours or more to obtain a polyurethane film. The obtained polyurethane film was subjected to evaluation of various physical properties.

[0120] <Flexibility of polyurethane film> The flexibility of the polyurethane film was evaluated by five examiners who evaluated the feel of the film when touched with their hands. The evaluation criteria were as follows: ○ indicates flexibility, and the evaluation results of the five inspectors were consistent. △ indicates that the sample was slightly hard, and the evaluation results of the five inspectors were consistent. × indicates that the sample was hard, and the evaluation results of the five inspectors were consistent.

[0121] <Appearance of polyurethane film> The surface appearance of the polyurethane film prepared above was visually evaluated according to the following criteria. A mark "◯" indicates that the surface was smooth. △ indicates that a few streaks were observed on the surface in the direction of applicator movement. × indicates that many streaks were observed on the surface in the direction of applicator movement.

[0122] <Molecular weight measurement> A part of the polyurethane film was cut out, and a solution in N,N-dimethylacetamide was prepared so that the polyurethane concentration was 0.1% by mass. The number average molecular weight (Mn) and weight average molecular weight (Mw) were measured in terms of standard polystyrene using a GPC apparatus (Tosoh Corporation, product name "HLC-8320" (column: Tskgel SuperHM-H x 4), using a solution of 2.6 g of lithium bromide dissolved in 1 L of dimethylacetamide as the eluent).

[0123] <Evaluation of resistance to oleic acid> A 3cm x 3cm test piece was cut out from the polyurethane film. After measuring the weight of the test piece with a precision balance, it was placed in a 250mL glass bottle containing 50mL of oleic acid as a test solvent, and left to stand in a constant temperature bath at 80°C under a nitrogen atmosphere for 16 hours. After the test, the test piece was removed and lightly wiped on both sides with a paper wiper, after which the weight was measured with a precision balance and the weight change rate (increase rate) from before the test was calculated. A weight change rate closer to 0% indicates better resistance to oleic acid.

[0124] <Evaluation of ethanol resistance> After preparing a urethane film in the same manner as in <Evaluation of oleic acid resistance> above, a urethane film test piece was cut out to 3 cm x 3 cm. The weight of the test piece was measured using a precision balance, and then it was placed in a glass petri dish with an inner diameter of 10 cm and containing 50 mL of ethanol as the test solvent, and immersed for 1 hour at room temperature of about 23°C. After the test, the test piece was removed and lightly wiped with a paper wiper, and then the weight was measured using a precision balance, and the weight change rate (rate of increase) from before the test was calculated. A weight change rate closer to 0% indicates better ethanol resistance.

[0125] <Measurement of glass transition temperature (Tg)> A test piece measuring 10 mm in width, 40 mm in length, and 0.4 mm in thickness was cut out from the polyurethane film. Using a viscoelasticity measuring device (Hitachi High-Tech Science Corporation, [TA7000 series, DMA7100]), the test piece was set at a chuck distance of 20 mm, and the viscoelasticity was measured while increasing the temperature from -100°C to 100°C at a rate of 5°C / min. The glass transition temperature (Tg) was calculated by reading the peak of tan δ.

[0126] <Room temperature tensile test> In accordance with JIS K6301 (2010), a tensile test was carried out on rectangular polyurethane test pieces measuring 10 mm in width, 100 mm in length, and approximately 0.5 mm in thickness using a tensile testing machine (manufactured by Orientec Co., Ltd., product name "Tensilon, Model RTE-1210") at a chuck distance of 20 mm, a tensile speed of 100 mm / min, and a temperature of 23°C (relative humidity of 55%). The stress at the point when the test pieces were elongated to 100%, as well as the strength at break and elongation at break were measured.

[0127] <Low temperature tensile test> In accordance with JIS K6301 (2010), a rectangular polyurethane test piece 10 mm wide, 100 mm long, and approximately 0.5 mm thick was placed on a tensile testing machine (manufactured by Orientec Co., Ltd., product name "Tensilon, Model RTE-1210") equipped with a thermostatic bath (manufactured by Orientec Co., Ltd., "Model TLF-R3T-EW") with a chuck distance of 20 mm. The test piece was then left to stand at -20°C for 5 minutes, after which a tensile test was carried out at a tensile speed of 100 mm / min, and the stress at the point when the test piece was elongated by 100% was measured.

[0128] <Evaluation of heat resistance> The polyurethane film was cut into a strip of 10 mm width, 100 mm length, and approximately 50 μm thickness, and heated in a gear oven at 120° C. for 1000 hours. The breaking strength of the heated sample was measured in the same manner as in the above <Room temperature tensile test>, and its retention rate (%) was calculated.

[0129] <Evaluation of hydrolysis resistance> The polyurethane film was cut into a strip of 10 mm width, 100 mm length, and approximately 50 μm thickness, and heated in a thermo-hygrostat at a temperature of 70° C. and a relative humidity of 95% for 400 hours. The samples after heating were measured for breaking strength in the same manner as in the above <Room temperature tensile test>, and the retention rate (%) was calculated.

[0130] [Analysis and evaluation of synthetic leather] <Flexibility of synthetic leather> The softness of the synthetic leather was evaluated by five panelists who evaluated the feel of the synthetic leather when touched with their hands. The evaluation criteria were as follows: ○ indicates flexibility, and the evaluation results of the five inspectors were consistent. △ indicates that the sample was slightly hard, and the evaluation results of the five inspectors were consistent. × indicates that the sample was hard, and the evaluation results of the five inspectors were consistent.

[0131] <Abrasion resistance of synthetic leather> A load of 9.8N was applied to a friction element covered with cotton cloth to abrade the surface of the synthetic leather. The friction element was abraded 10,000 times at a speed of 60 back and forth strokes per minute over a distance of 140 mm on the surface of the synthetic leather. The synthetic leather was observed after abrasion and rated according to the following criteria. A mark "◯" indicates that the resin layer had no cracks or tears. △ indicates that a crack occurred in the resin layer. × indicates that the resin layer was torn.

[0132] <Low temperature storage stability of synthetic leather> The synthetic leather was wrapped around a paper tube with a diameter of 10 cm and stored in a thermostatic chamber at -20°C for one month. The synthetic leather was removed from the paper tube and left in a thermostatic chamber at a temperature of 23°C and a humidity of 50% for one day, after which the surface was visually observed. The evaluation was performed as follows: no cracks or wrinkles at all was marked as ◯, minute cracks or wrinkles of 1 mm or less were observed was marked as △, and cracks or wrinkles exceeding 1 mm were observed was marked as ×.

[0133] <Method for evaluating adhesion> An incision was made in advance at the interface between the polyester base fabric and the polyurethane resin layer of the synthetic leather, and the peeled urethane resin layer and base fabric were each fixed with a chuck. The peel strength between the polyurethane layer and base fabric was measured using a tensile tester (Tensilon model RTE-1210, manufactured by Orientec Co., Ltd.) in accordance with JIS K6854-2 at a temperature of 23°C and a speed of 200 mm / min to evaluate the adhesion.

[0134] [Polymerization Example 1 of Polyester Polycarbonate Polyol] A 2L glass flask equipped with a rectification column filled with structured packing and a stirrer was charged with 221g (2.51mol) of ethylene carbonate, 148g (1.64mol) of 1,4-butanediol, 195g (1.65mol) of 1,6-hexanediol, and 202g (1.38mol) of adipic acid. 0.10g of titanium tetrabutoxide was added as a catalyst, and the reaction was carried out for 12 hours while distilling off the mixture of water, ethylene glycol, and ethylene carbonate produced at a reaction temperature of 150-170°C and a pressure of 10kPa to 3kPa. Thereafter, the reaction was switched to simple distillation, and the pressure was gradually reduced to 0.1 kPa while the reaction was carried out at 170° C. for 5 hours to distill off the monomer. The analysis results of the obtained polyester polycarbonate polyol (also referred to as PEC1) are shown in Table 1.

[0135] [Polymerization Example 2 of Polyester Polycarbonate Polyol] Polymerization was carried out in the same manner as in Polymerization Example 1, except that the amounts of ethylene carbonate, 221 g (2.51 mol), 1,4-butanediol, 148 g (1.64 mol), 1,5-pentanediol, 172 g (1.65 mol), adipic acid, 202 g (1.38 mol), and titanium tetrabutoxide as a catalyst were used and 0.10 g were used as the catalyst. The analysis results of the obtained polyester polycarbonate polyol (also referred to as PEC2) are shown in Table 1.

[0136] [Polymerization Example 3 of Polyester Polycarbonate Polyol] Polymerization was carried out in the same manner as in Polymerization Example 1, except that the amounts of ethylene carbonate, 198 g (2.25 mol), 1,6-hexanediol, 413 g (3.49 mol), adipic acid, 188 g (1.28 mol), and titanium tetrabutoxide as a catalyst were changed to 198 g (2.25 mol), 1,6-hexanediol, 413 g (3.49 mol), and 188 g (1.28 mol), respectively, and 0.10 g of titanium tetrabutoxide was used as a catalyst. The analysis results of the obtained polyester polycarbonate polyol (also referred to as PEC3) are shown in Table 1.

[0137] [Polymerization Example 4 of Polyester Polycarbonate Polyol] Polymerization was carried out in the same manner as in Polymerization Example 1, except that the amounts of ethylene carbonate (250 g, 2.84 mol), 1,4-butanediol (377 g, 4.18 mol), adipic acid (215 g, 1.47 mol), and titanium tetrabutoxide (0.10 g) used as a catalyst were changed to 250 g (2.84 mol) using the same apparatus as in Polymerization Example 1. The analysis results of the obtained polyester polycarbonate polyol (also referred to as PEC4) are shown in Table 1.

[0138] [Polymerization Example 5 of Polyester Polycarbonate Polyol] Except for changing the polymerization time after switching to simple distillation to 4 hours, polymerization was carried out in the same manner as in Polymerization Example 1. The analysis results of the obtained polyester polycarbonate polyol (also referred to as PEC5) are shown in Table 1.

[0139] [Polymerization Example 6 of Polyester Polycarbonate Polyol] Except for changing the polymerization time after switching to simple distillation to 7 hours, polymerization was carried out in the same manner as in Polymerization Example 1. The analysis results of the obtained polyester polycarbonate polyol (also referred to as PEC6) are shown in Table 1.

[0140] [Polymerization Example 7 of Polyester Polycarbonate Polyol] Polymerization was carried out in the same manner as in Polymerization Example 1, except that the amounts of ethylene carbonate, 221 g (2.51 mol), 1,4-butanediol, 207 g (2.30 mol), 1,6-hexanediol, 117 g (0.99 mol), adipic acid, 202 g (1.38 mol), and titanium tetrabutoxide as a catalyst were used and 0.10 g were used as the catalyst. The analysis results of the obtained polyester polycarbonate polyol (also referred to as PEC7) are shown in Table 1.

[0141] [Polymerization Example 8 of Polyester Polycarbonate Polyol] Polymerization was carried out in the same manner as in Polymerization Example 1, except that the amounts of ethylene carbonate, 221 g (2.51 mol), 1,4-butanediol, 89 g (0.99 mol), 1,6-hexanediol, 272 g (2.30 mol), adipic acid, 202 g (1.38 mol), and titanium tetrabutoxide as a catalyst were used and 0.10 g were used as the catalyst. The analysis results of the obtained polyester polycarbonate polyol (also referred to as PEC8) are shown in Table 1.

[0142] [Polymerization Example 9 of Polyester Polycarbonate Polyol] Polymerization was carried out in the same manner as in Polymerization Example 1, except that the amounts of ethylene carbonate, 221 g (2.51 mol), 1,4-butanediol, 207 g (2.30 mol), 1,6-hexanediol, 271 g (2.30 mol), adipic acid, and 0.10 g of titanium tetrabutoxide as a catalyst were used and polymerization was carried out in the same manner as in Polymerization Example 1. The analysis results of the obtained polyester polycarbonate polyol (also referred to as PEC9) are shown in Table 1.

[0143] [Polymerization Example 10 of Polyester Polycarbonate Polyol] Polymerization was carried out in the same manner as in Polymerization Example 1, except that the amounts of ethylene carbonate, 221 g (2.51 mol), 1,4-butanediol, 79.3 g (0.88 mol), 1,6-hexanediol, 104.0 g (0.88 mol), adipic acid, 282 g (1.93 mol), and titanium tetrabutoxide as a catalyst were used and 0.10 g were used as the catalyst. The analysis results of the obtained polyester polycarbonate polyol (also referred to as PEC10) are shown in Table 1.

[0144] [Polymerization Example 11 of Polyester Polycarbonate Polyol] A 2L glass flask equipped with a rectification column filled with structured packing and a stirrer was charged with 226g (2.51mol) of dimethyl carbonate, 148g (1.64mol) of 1,4-butanediol, 195g (1.65mol) of 1,6-hexanediol, and 240g (1.38mol) of dimethyl adipate. 0.10g of titanium tetrabutoxide was added as a catalyst, and the reaction was carried out for 12 hours while distilling off the mixture of methanol and dimethyl carbonate produced at a reaction temperature of 130-190°C and a pressure of 3kPa from normal pressure. Thereafter, the reaction was switched to simple distillation, and the pressure was gradually reduced to 0.1 kPa while the reaction was carried out at 180° C. for 5 hours to distill off the monomer. The analysis results of the obtained polyester polycarbonate polyol (also referred to as PEC11) are shown in Table 1.

[0145] [Polymerization Example 12 of Polyester Polycarbonate Polyol] Except for using 229 g (1.38 mol) of phthalic acid instead of adipic acid, polymerization was carried out in the same manner as in Polyester Polycarbonate Polyol Polymerization Example 1. The analysis results of the obtained polyester polycarbonate polyol (also referred to as PEC12) are shown in Table 1.

[0146] [Polymerization Example 13 of Polyester Polycarbonate Polyol] A 2L glass flask equipped with a rectification column filled with structured packing and a stirrer was charged with 221g (2.51mol) of ethylene carbonate, 148g (1.64mol) of 1,4-butanediol, 195g (1.65mol) of 1,6-hexanediol, and 158g (1.38mol) of ε-caprolactone. 0.10g of titanium tetrabutoxide was added as a catalyst, and the reaction was carried out for 12 hours while distilling off the resulting water, ethylene glycol, and ethylene carbonate mixture at a reaction temperature of 150-170°C and a pressure of 10kPa to 3kPa. Thereafter, the reaction was switched to simple distillation, and the pressure was gradually reduced to 0.1 kPa while the reaction was carried out at 170° C. for 5 hours to distill off the monomer. The analysis results of the obtained polyester polycarbonate polyol (also referred to as PEC13) are shown in Table 1.

[0147] [Polymerization Example 14 of Polyester Polycarbonate Polyol] Except for changing the polymerization time after switching to simple distillation to 10 hours, polymerization was carried out in the same manner as in Polymerization Example 1. The analysis results of the obtained polyester polycarbonate polyol (also referred to as PEC14) are shown in Table 1.

[0148] [Polymerization Example 15 of Polyester Polycarbonate Polyol] Except for changing the polymerization time after switching to simple distillation to 2.5 hours, polymerization was carried out in the same manner as in Polymerization Example 1. The analysis results of the obtained polyester polycarbonate polyol (also referred to as PEC15) are shown in Table 1.

[0149] [Polycarbonate polyol polymerization example 1 (also called polymerization example 16)] In a 2L glass flask equipped with a rectification column filled with structured packing and a stirrer, 423g (4.8mol) of ethylene carbonate, 216g (2.4mol) of 1,4-butanediol, and 284g (2.4mol) of 1,6-hexanediol were charged. 0.09g of titanium tetrabutoxide was added as a catalyst, and the reaction was carried out for 12 hours while the reaction temperature was set to 140-160°C, the pressure was reduced from 10kPa to 2kPa, and the mixture of ethylene glycol and ethylene carbonate produced was distilled off. Thereafter, the reaction was switched to simple distillation, and the pressure was gradually reduced to 0.5 kPa while the reaction was carried out at 180° C. for 1 hour to distill off the monomer. The analysis results of the obtained polycarbonate diol (also referred to as PC1) are shown in Table 1.

[0150] [Polycarbonate polyol polymerization example 2 (also called polymerization example 17)] Using the same apparatus as in the above-mentioned Polycarbonate Polyol Polymerization Example 1, polymerization was carried out in the same manner as in Polycarbonate Polyol Polymerization Example 1, except that 423 g (4.8 mol) of ethylene carbonate, 250 g (2.4 mol) of 1,5-pentanediol, 284 g (2.4 mol) of 1,6-hexanediol, and 0.09 g of titanium tetrabutoxide as a catalyst were used. The analysis results of the obtained polycarbonate polyol (also referred to as PC2) are shown in Table 1.

[0151] [Polycarbonate polyol polymerization example 3 (also called polymerization example 18)] Except for changing the polymerization time after switching to simple distillation to 1.5 hours, polymerization was carried out in the same manner as in Polycarbonate Polyol Polymerization Example 1. The results of analysis of the obtained polycarbonate polyol (also referred to as PC3) are shown in Table 1.

[0152] [Polycarbonate polyol polymerization example 4 (also called polymerization example 19)] Except for changing the polymerization time after switching to simple distillation to 2.0 hours, polymerization was carried out in the same manner as in Polycarbonate Polyol Polymerization Example 1. The results of analysis of the obtained polycarbonate polyol (also referred to as PC4) are shown in Table 1.

[0153] [Polycarbonate polyol polymerization example 5 (also called polymerization example 20)] Except for changing the polymerization time after switching to simple distillation to 3.0 hours, polymerization was carried out in the same manner as in Polycarbonate Polyol Polymerization Example 1. The results of analysis of the obtained polycarbonate polyol (also referred to as PC5) are shown in Table 1.

[0154] [Polycarbonate polyol polymerization example 6 (also called polymerization example 21)] In a 2L glass flask equipped with a rectification column filled with structured packing and a stirrer, 423g (4.8mol) of ethylene carbonate, 250g (2.4mol) of 1,5-pentanediol, and 284g (2.4mol) of 1,6-hexanediol were charged. 0.09g of titanium tetrabutoxide was added as a catalyst, and the reaction was carried out for 12 hours at a reaction temperature of 140-160°C, while the pressure was reduced from 10kPa to 2kPa, and the mixture of ethylene glycol and ethylene carbonate produced was distilled off. Thereafter, the reaction was switched to simple distillation, and the pressure was gradually reduced to 0.5 kPa while the reaction was carried out at 180° C. for 5 hours to distill off the monomer. The analysis results of the obtained polycarbonate diol (also referred to as PC6) are shown in Table 1.

[0155] [Polymerization Example 22 of Polyester Polycarbonate Polyol] A 2L glass flask equipped with a rectification column filled with structured packing and a stirrer was charged with 221g (2.51mol) of ethylene carbonate, 236.5g (1.64mol) of 1,4-cyclohexanedimethanol, 195g (1.65mol) of 1,6-hexanediol, and 202g (1.38mol) of adipic acid. 0.10g of titanium tetrabutoxide was added as a catalyst, and the reaction was carried out for 12 hours while distilling off the mixture of water, ethylene glycol, and ethylene carbonate produced at a reaction temperature of 150-170°C and a pressure of 10kPa to 3kPa. The reaction was then switched to simple distillation, and the pressure was gradually reduced to 0.1 kPa while the reaction was continued at 170°C for 5 hours to distill off the monomer, yielding polyester polycarbonate polyol (PEC16). The hydroxyl value of the resulting polyester polycarbonate polyol was 56.6 mgKOH / g, the average molecular weight was 1982, and the melt viscosity at 50°C was 6800 mPa s.

[0156] [Table 1]

[0157] [Synthesis Example 1 of Prepolymer Composition] A 500 mL separable flask sealed with nitrogen gas was charged with 30 g (0.12 mol) of MDI and heated to 50°C. 100 g of methyl ethyl ketone (MEK) heated to 50°C and 121 g (0.06 mol) of polyester polycarbonate polyol PEC1 to which 0.007 g of dibutyltin dilaurate was added as a catalyst were added dropwise over 30 minutes under stirring. The reaction was carried out at 50°C under stirring for 2 hours to obtain a prepolymer composition with isocyanates at both ends. The analysis results of the obtained prepolymer composition (also referred to as PCP1) are shown in Table 2.

[0158] [Synthesis Examples 2 to 28 of Prepolymer Compositions] Prepolymer compositions were synthesized in the same manner as in Synthesis Example 1 of Prepolymer Composition, except that the amounts of polycarbonate polyol, MDI, and MEK used were shown in Table 2. The results of analysis of the obtained prepolymer compositions (also referred to as PCP2 to PCP28, respectively) are shown in Table 2.

[0159] [Table 2]

[0160] [Synthesis Example 29 of Prepolymer Composition] A 500 mL separable flask sealed with nitrogen gas was charged with 31.5 g (0.12 mol) of hydrogenated MDI and heated to 50°C. 120 g of methyl ethyl ketone (MEK) heated to 50°C and 120 g (0.06 mol) of polyester polycarbonate polyol PEC1 to which 0.028 g of dibutyltin dilaurate was added as a catalyst were added dropwise over 30 minutes under stirring. The reaction was carried out at 50°C under stirring for 2 hours to obtain a prepolymer composition with isocyanates at both ends. The analysis results of the obtained prepolymer composition (also referred to as PCP29) are shown in Table 3.

[0161] [Synthesis Examples 30 to 33 of Prepolymer Compositions] Prepolymer compositions were synthesized in the same manner as in Synthesis Example 29 of Prepolymer Composition, except that the amounts of polyester polycarbonate polyol, hydrogenated MDI, and MEK used were shown in Table 3. The results of analysis of the obtained prepolymer compositions (also referred to as PCP30 to PCP33, respectively) are shown in Table 3.

[0162] [Table 3]

[0163] [Example 1] 40g of polyester polycarbonate polyol PEC1, 10g of polyol PC1, 10g of MDI pre-dissolved at 80°C, 10g of methyl ethyl ketone (MEK), and 0.003g of dibutyltin dilaurate as a catalyst were charged into a nitrogen-sealed 200mL separable flask with stirring blade. After stirring for 5 minutes at 40°C, the mixture was applied to a polypropylene resin sheet (width 100mm, length 1200mm, thickness 1mm) with an applicator to a width of 80mm, length 100mm, and thickness of 0.6mm, and dried on a hot plate with a surface temperature of 60°C for 2 hours and then in an oven at 100°C for 12 hours. The polyurethane film was then left to stand at a constant temperature and humidity of 23°C and 55%RH for 12 hours or more to obtain a polyurethane film. The obtained polyurethane film was subjected to evaluation of various physical properties. The evaluation results are shown in Table 4.

[0164] [Examples 2 to 22] A polyurethane film was obtained in the same manner as in Example 1, except that the types and amounts of the polyester polycarbonate polyol, polyol, and commercially available polyester polyol (POLYLITE OD-X2420, manufactured by DIC Corporation; liquid at room temperature, hydroxyl value 56 mgKOH / g) were as shown in Table 4. The evaluation results of the obtained polyurethane film are shown in Table 4.

[0165] [Example 69] 40g of polyester polycarbonate polyol PEC16, 10g of polyol PC1, 10g of MDI pre-dissolved at 80°C, 10g of methyl ethyl ketone (MEK), and 0.003g of dibutyltin dilaurate as a catalyst were charged into a nitrogen-sealed 200mL separable flask with stirring blade. After stirring for 5 minutes at 40°C, the mixture was applied to a polypropylene resin sheet (width 100mm, length 1200mm, thickness 1mm) with an applicator to a width of 80mm, length 100mm, and thickness of 0.6mm, and dried for 2 hours on a hot plate with a surface temperature of 60°C, and then for 12 hours in an oven at 100°C. The polyurethane film was then left to stand at a constant temperature and humidity of 23°C and 55%RH for 12 hours or more to obtain a polyurethane film. The obtained polyurethane film was subjected to evaluation of various physical properties. The evaluation results are shown in Table 4.

[0166] [Comparative Examples 1 to 4] A polyurethane film was obtained in the same manner as in Example 1, except that the types and amounts of the polycarbonate polyol and polyol were changed to those shown in Table 4. The evaluation results of the obtained polyurethane film are shown in Table 4.

[0167] [Table 4]

[0168] [Example 23] 40g of polyester polycarbonate polyol PEC1, 10g of polyol PC1, 10.5g of hydrogenated MDI, 10g of methyl ethyl ketone (MEK), and 0.009g of dibutyltin dilaurate as a catalyst, which had been preheated to 40°C, were charged into a 200mL separable flask with a stirring blade sealed with nitrogen. After stirring for 5 minutes at 40°C, the mixture was applied to a polypropylene resin sheet (width 100mm, length 1200mm, thickness 1mm) with an applicator to a width of 80mm, length 100mm, and thickness of 0.6mm, and dried for 2 hours on a hot plate with a surface temperature of 60°C, and then for 12 hours in an oven at 110°C. The polyurethane film was then left to stand at a constant temperature and humidity of 23°C and 55%RH for 12 hours or more to obtain a polyurethane film. The obtained polyurethane film was subjected to evaluation of various physical properties. The evaluation results are shown in Table 5.

[0169] [Examples 24 to 30] A polyurethane film was obtained in the same manner as in Example 23, except that the types and amounts of the polyester polycarbonate polyol and polyol were changed to those shown in Table 5. The evaluation results of the obtained polyurethane film are shown in Table 5.

[0170] [Comparative Examples 5 to 8] A polyurethane film was obtained in the same manner as in Example 23, except that the types and amounts of the polyester polycarbonate polyol and polyol were changed to those shown in Table 5. The evaluation results of the obtained polyurethane film are shown in Table 5.

[0171] [Example 31] 40g of polyester polycarbonate polyol PEC1, 10g of polyol PC1, 7.7g of Duranate TKA-100 (Asahi Kasei Corporation: hexamethylene diisocyanate-based isocyanurate type curing agent, NCO content = 21.8wt%, isocyanate groups in one molecule: 3), 10g of methyl ethyl ketone (MEK), and 0.003g of dibutyltin dilaurate as a catalyst were charged into a 200mL separable flask with a stirring blade sealed with nitrogen, which had been preheated to 40°C. After stirring for 5 minutes at 40°C, the mixture was applied to a polypropylene resin sheet (width 100mm, length 1200mm, thickness 1mm) with an applicator to a width of 80mm, length 100mm, and thickness of 0.6mm, and then dried on a hot plate with a surface temperature of 60°C for 2 hours and then in an oven at 110°C for 12 hours. The polyurethane film was then left to stand at a constant temperature and humidity of 23° C. and 55% RH for 12 hours or more to obtain a polyurethane film. The polyurethane film thus obtained was subjected to evaluation of various physical properties. The evaluation results are shown in Table 5.

[0172] [Table 5]

[0173] [Example 32] 80 g of prepolymer composition PCP1 and 13 g of polyol PC1, which had been preheated to 50°C, were charged into a 200 mL separable flask with stirring blades and sealed with nitrogen. After stirring for 5 minutes at 50°C, the mixture was applied to a polypropylene resin sheet (width 100 mm, length 1200 mm, thickness 1 mm) with an applicator to a width of 80 mm, length of 100 mm, and thickness of 0.6 mm, and dried for 2 hours on a hot plate with a surface temperature of 60°C, and then for 12 hours in an oven at 100°C. The polyurethane film was then left to stand at a constant temperature and humidity of 23°C and 55%RH for 12 hours or more to obtain a polyurethane film. The obtained polyurethane film was subjected to evaluation of various physical properties. The evaluation results are shown in Table 6.

[0174] [Examples 33 to 50] A polyurethane film was obtained in the same manner as in Example 32, except that the types and amounts of the prepolymer composition and polyol were changed to those shown in Table 6. The evaluation results of the obtained polyurethane film are shown in Table 6.

[0175] [Comparative Examples 9 to 12] A polyurethane film was obtained in the same manner as in Example 32, except that the types and amounts of the prepolymer composition and polyol were changed to those shown in Table 6. The evaluation results of the obtained polyurethane film are shown in Table 6.

[0176] [Table 6]

[0177] [Example 51] 80g of polyester polycarbonate polyol PEC1 and 61.5g of prepolymer composition PCP16, which had been preheated to 50°C, were charged into a 200mL separable flask with stirring blades sealed with nitrogen. After stirring for 5 minutes at 50°C, the mixture was applied to a polypropylene resin sheet (width 100mm, length 1200mm, thickness 1mm) with an applicator to a width of 80mm, length 100mm, and thickness of 0.6mm, and dried for 2 hours on a hot plate with a surface temperature of 60°C, followed by 12 hours in an oven at 100°C. The polyurethane film was then left to stand at a constant temperature and humidity of 23°C and 55%RH for 12 hours or more to obtain a polyurethane film. The obtained polyurethane film was subjected to evaluation of various physical properties. The evaluation results are shown in Table 7.

[0178] [Examples 52 to 54] A polyurethane film was obtained in the same manner as in Example 51, except that the type and amount of the polyester polycarbonate polyol and the type and amount of the prepolymer composition were the types and amounts shown in Table 7. The evaluation results of the obtained polyurethane film are shown in Table 7.

[0179] [Comparative Example 13] A polyurethane film was obtained in the same manner as in Example 51, except that the type and amount of the polyester polycarbonate polyol and the type and amount of the prepolymer composition were the types and amounts shown in Table 7. The evaluation results of the obtained polyurethane film are shown in Table 7.

[0180] [Table 7]

[0181] [Example 55] 80g of prepolymer composition PCP26 and 10g of polyol PC1, which had been preheated to 50°C, were charged into a 200mL separable flask with stirring blades sealed with nitrogen. After stirring for 5 minutes at 50°C, the mixture was applied to a polypropylene resin sheet (width 100mm, length 1200mm, thickness 1mm) with an applicator to a width of 80mm, length 100mm, and thickness of 0.6mm, and dried for 2 hours on a hot plate with a surface temperature of 60°C, and then for 12 hours in an oven at 100°C. The polyurethane film was then left to stand at a constant temperature and humidity of 23°C and 55%RH for 12 hours or more to obtain a polyurethane film. The obtained polyurethane film was subjected to evaluation of various physical properties. The evaluation results are shown in Table 8.

[0182] [Examples 56 to 60] A polyurethane film was obtained in the same manner as in Example 55, except that the types and amounts of the prepolymer composition and polyol were changed to those shown in Table 8. The evaluation results of the obtained polyurethane film are shown in Table 8.

[0183] [Comparative Example 14] A polyurethane film was obtained in the same manner as in Example 55, except that the types and amounts of the prepolymer composition and polyol were changed to those shown in Table 8. The evaluation results of the obtained polyurethane film are shown in Table 8.

[0184] [Table 8]

[0185] [Example 61] Using the same apparatus as shown in Fig. 2 and release paper having a grain pattern (R-8, manufactured by Lintec Corporation), a composition having the same composition ratio as in Example 23 was continuously mixed with a mixing head at a temperature of 40°C, continuously flowed down onto the release paper, and adjusted to a thickness of 50 μm with a coating roll. The mixture was passed through a dryer at 120°C to form a urethane layer that would become a surface layer. Next, the composition having the same composition ratio as in Example 1 was continuously mixed in a mixing head at a temperature of 40°C, continuously flowed down onto a release paper, and adjusted to a thickness of 250 μm with a coating roll. The mixture was passed through a dryer at 120°C to form a urethane layer that would become an adhesive layer. Next, a 500 μm thick base fabric (nonwoven fabric made of polyester fiber) was laminated using a pressure roller, and then wound up using a winding roller to obtain synthetic leather made of a polyurethane laminate. The synthetic leather obtained was evaluated, and the results are shown in Table 9.

[0186] [Examples 62 to 68] Synthetic leather made of a polyurethane laminate was obtained in the same manner as in Example 61, except that the types of curable compositions for the surface layer and the adhesive layer were changed to those shown in Table 9. The obtained synthetic leather was evaluated, and the results are shown in Table 9.

[0187] [Comparative Examples 15 to 19] Synthetic leather made of a polyurethane laminate was obtained in the same manner as in Example 61, except that the types of curable compositions for the surface layer and the adhesive layer were changed to those shown in Table 9. The obtained synthetic leather was evaluated, and the results are shown in Table 9.

[0188] [Table 9] [Industrial Applicability]

[0189] The curable composition of the present invention has an excellent balance of physical properties including flexibility, chemical resistance, low-temperature properties, heat resistance, and touch, and can be used for environmentally friendly synthetic leather that uses a small amount of solvent. The curable composition of the present embodiment is also used as a lamination adhesive for various films, a surface protective agent, and the like.

[0190] The disclosure of Japanese Patent Application No. 2021-036424, filed on March 8, 2021, is incorporated by reference in its entirety into this specification. In addition, all publications, patent applications, and technical standards mentioned in the specification are herein incorporated by reference to the same extent as if each individual publication, patent application, and technical standard was specifically and individually indicated to be incorporated by reference. [Explanation of symbols]

[0191] 1 Release paper 2 Epidermal layer 3 Adhesive layer 4 Base material (nonwoven fabric) 5 Mixing head (skin layer) 6 Mixing head (adhesive layer) 7 Seat structure (dry synthetic leather product) 8 Coating roll 9. Pressure Roll 10 Winding roll 11 Dryer

Claims

1. Component (a): A polyester polycarbonate polyol having a hydroxyl value of 40 to 75 mgKOH / g, which has a repeating unit represented by the following formula (1) and a repeating unit represented by the following formula (2) and has a hydroxyl group at the molecular end. 【Chemistry 1】 (In formula (1), R 1 is a divalent aliphatic or alicyclic hydrocarbon having 2 to 15 carbon atoms. 【Chemistry 2】 (In formula (2), R 2 is a divalent hydrocarbon having 2 to 15 carbon atoms, R 3 is a divalent aliphatic or alicyclic hydrocarbon having 2 to 15 carbon atoms. Component (b): a polyol having a hydroxyl value of 100 to 280 mg KOH / g, A curable composition comprising: component (c): a polyisocyanate having an average functionality of 2 to 6 per molecule.

2. Component (d): an isocyanate-terminated prepolymer composition in which component (a) is a polyester polycarbonate polyol having a hydroxyl value of 40 to 75 mgKOH / g and component (c) is a polyisocyanate having an average functionality of 2 to 6 per molecule, the equivalent ratio of which isocyanate equivalent / hydroxyl equivalent is 1.5 to 3.0; and Component (b) is a polyol having a hydroxyl value of 100 to 280 mgKOH / g; The curable composition of claim 1 comprising:

3. Component (e): an isocyanate-terminated prepolymer composition in which component (b) is a polyol having a hydroxyl value of 100 to 280 mgKOH / g and component (c) is a polyisocyanate having an average functionality of 2 to 6 per molecule, the equivalent ratio [isocyanate equivalent] / [hydroxyl equivalent] being 1.5 to 3.0; and Component (a) a polyester polycarbonate polyol having a hydroxyl value of 40 to 75 mgKOH / g; The curable composition of claim 1 comprising:

4. The curable composition according to any one of claims 1 to 3, wherein the mass ratio of the polyester polycarbonate polyol of component (a) to the polyol of component (b) is 95 / 5 to 40 / 60.

5. The curable composition according to any one of claims 1 to 4, wherein a molar ratio of the structural unit represented by formula (1) to the structural unit represented by formula (2) is from 90 / 10 to 10 / 90.

6. At least 50 mol % of the repeating units represented by formula (1) include at least two repeating units selected from formulas (4), (5), and (6). The curable composition according to any one of claims 1 to 5. 【Chemistry 3】 【Chemistry 4】 【Chemistry 5】

7. The curable composition according to any one of claims 1 to 6, wherein the polyol of the component (b) is a polycarbonate polyol having a repeating unit represented by formula (7) and a terminal hydroxyl group. 【Chemistry 6】 (In formula (7), R 5 is a divalent aliphatic or alicyclic hydrocarbon having 2 to 15 carbon atoms.

8. At least 50 mol % of the repeating units represented by formula (7) are selected from at least two repeating units represented by formulas (8), (9), and (10). The curable composition according to claim 7. 【Chemistry 7】 【Chemistry 8】 【Chemistry 9】

9. The curable composition according to any one of claims 1 to 8, comprising 40 mass% or less of an inert organic solvent based on the total amount of the curable composition.

10. The curable composition according to any one of claims 1 to 9, comprising 50 mass% or less of a polyester polyol based on the total amount of the curable composition.

11. A synthetic leather produced using the curable composition according to any one of claims 1 to 10.

Citation Information

Patent Citations

  • Polyurethane and polyester polycarbonate diel used therefor

    JP1996239442A

  • Porous sheet material and method for producing the same

    JP2003119314A

  • Polyurethane resin and surface film layer of synthetic leather obtained using the same

    JP2004346094A

  • Surface layer material-forming composition for fiber laminate, synthetic / artificial leather using the same, and method for producing synthetic / artificial leather

    JP2009185260A

  • Synthetic leather

    JP2013108196A

Cited By

  • Polyester polycarbonate polyol, and synthetic leather