Magnetic materials and magnetic elements

A magnetic material with an inorganic insulating layer and cured resin, containing Si and polyesterimide, addresses insulation and oxidation issues, providing long-term heat resistance and mechanical strength for automotive components.

JP7555803B2Active Publication Date: 2024-09-25TOKIN CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020197987
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-11-30
Publication Date
2024-09-25
Estimated Expiration
2040-11-30

AI Technical Summary

Technical Problem

Existing magnetic materials face challenges in maintaining long-term heat resistance and insulation in high-temperature environments, particularly around engines and motors, due to insulation deterioration and oxidation issues, and require processing at lower temperatures for manufacturing.

Method used

A magnetic material comprising iron alloy powder with an inorganic insulating layer and a cured resin, containing 4 to 10 parts by mass of Si and polyesterimide, which suppresses oxidation and thermal decomposition, ensuring excellent heat resistance up to 180°C.

Benefits of technology

The magnetic material maintains high insulation resistance and mechanical strength in high-temperature environments, enabling stable operation in automotive applications and allowing for lower processing temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007555803000006
    Figure 0007555803000006
  • Figure 0007555803000007
    Figure 0007555803000007
  • Figure 0007555803000008
    Figure 0007555803000008
Patent Text Reader

Abstract

To provide a magnetic body and a magnetic element which are usable under high temperature environment at 180°C and are excellent in heat resistance.SOLUTION: A magnetic body contains iron alloy powder having an inorganic insulating layer thereon, and a resin cured product, in which 4-10 pts.mass of Si is contained in 100 pts.mass of the iron alloy powder, and the resin cured product has polyester imide.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a magnetic body and a magnetic element. [Background technology]

[0002] In recent years, the demand for in-vehicle electronic components has increased with the electrification of automobiles. In addition, to secure space inside the vehicle, electronic components are placed near the engine and motor, so there is a demand for further improvement in heat resistance. Further heat resistance is also required for the magnetic elements used in electronic components. Furthermore, to ensure the functionality of inductors for a long period of time, there is a demand for long-term heat resistance in a high-temperature environment of 180°C and for the elements to maintain their strength against long-term vibration.

[0003] One of the magnetic bodies used in the magnetic element is a so-called plastic magnet. A plastic magnet is formed into a predetermined shape by injection molding or the like using a binder resin in which soft magnetic metal powder is dispersed. With a plastic magnet, it is relatively easy to obtain a magnetic body of a desired shape.

[0004] As one method for improving the heat resistance of a magnetic body, the selection of a binder resin with excellent heat resistance has been considered. For example, Patent Document 1 discloses a magnetic core using a composite fluororesin containing a perfluororesin with excellent heat resistance.

[0005] Also, the use of plastic magnets to manufacture integrated magnetic elements with coils embedded in magnetic bodies is being considered. For example, Patent Document 2 discloses a method for manufacturing an inductor in which a coil is placed in a cavity and then the cavity is filled with a composition containing a thermoplastic element and magnetic powder. An integrated molded inductor also has the advantage of being able to suppress leakage magnetic flux without the need for shielding. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2017-188680 A [Patent Document 2] JP 2019-102713 A Summary of the Invention [Problem to be solved by the invention]

[0007] The magnetic core using the magnetic material of Patent Document 1 is said to have a heat resistance of 260°C. On the other hand, when processing the magnetic material of Patent Document 1, it is necessary to process it at a temperature exceeding the melting point of the perfluoro fluororesin. In the magnetic material of Patent Document 1, in the form of an inductor containing a coil, the coil and terminal parts cannot withstand processing at a temperature exceeding the melting point of the perfluoro fluororesin, and there is a manufacturing problem in that insulation deterioration of the coil coating and oxidation of the terminal parts are unavoidable. In addition, in order to function as an inductor even when placed around the engine or motor, it is important to ensure not only insulation between the magnetic body and the coil but also insulation between the terminals. Furthermore, since electronic devices in automobiles are subjected to vibrations over the long term, it was necessary to ensure the strength of the element.

[0008] From the viewpoints of processability during manufacturing, energy saving, etc., it is desirable to process magnetic materials at lower temperatures. Furthermore, when manufacturing an integrated magnetic element such as that in Patent Document 2, the coil, coil terminals, etc. are also required to have heat resistance to the temperature during magnetic material processing, so there is a demand for lowering the temperature at which magnetic materials are processed.

[0009] In view of the above problems, an object of the present invention is to provide a magnetic body and a magnetic element that are excellent in long-term heat resistance in a high-temperature environment of 180°C. [Means for solving the problem]

[0010] A magnetic body according to one embodiment of the present invention comprises: The present invention includes an iron alloy powder having an inorganic insulating layer on a surface thereof, and a cured resin material, The iron alloy powder contains 4 to 10 parts by mass of Si per 100 parts by mass of the iron alloy powder, The cured resin contains polyesterimide.

[0011] A magnetic element according to one aspect of the present invention includes a magnetic body and a coil embedded in the magnetic body. Effect of the Invention

[0012] According to the present invention, it is possible to provide a magnetic body and a magnetic element that are excellent in long-term heat resistance in a high-temperature environment of 180°C. [Brief description of the drawings]

[0013] [Figure 1] 1 is a schematic perspective view of a magnetic element according to an embodiment of the present invention; [Diagram 2] FIG. 2 is a schematic cross-sectional view showing the AA cross section of FIG. [Diagram 3] 1 is a graph showing the change over time in insulation resistance in a heat resistance evaluation of magnetic bodies of Examples and Comparative Examples. [Figure 4] 1 is a graph showing the change in weight over time in a heat resistance evaluation of magnetic materials of Examples and Comparative Examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The magnetic body and magnetic element according to the present invention will be described in detail below. In addition, unless otherwise specified, the symbol "~" indicating a numerical range includes the lower limit and the upper limit.

[0015] [Magnetic material] The magnetic body according to this embodiment (hereinafter also referred to as the present magnetic body) comprises an iron alloy powder having an inorganic insulating layer on its surface, and a cured resin, wherein 100 parts by mass of the iron alloy powder contains 4 to 10 parts by mass of Si, and the cured resin comprises polyesterimide.

[0016] The present magnetic material has excellent long-term heat resistance in a high-temperature environment of 180° C. due to the combination of an iron alloy powder containing a specific amount of Si, an inorganic insulating layer covering the iron alloy powder, and a cured resin containing polyesterimide. Although the reason for this is not entirely clear, the present inventors speculate as follows. It is presumed that the use of iron alloy powder containing 4 to 10 mass% Si suppresses the oxidation of the iron alloy powder itself in a high-temperature environment, and also suppresses the catalytic action of iron that occurs at the contact surface between iron and the cured resin, thereby suppressing the thermal oxidative decomposition of the cured resin. In addition, since the iron alloy powder has an inorganic insulating layer, contact between the iron alloy powders is suppressed, thereby maintaining insulation, and contact with the cured resin is further suppressed, thereby suppressing oxidation of the cured resin. In addition, it is presumed that the structure of the cured resin of the present magnetic material is stabilized by having multiple imide bonds in the molecule, and oxidation is suppressed even in a high-temperature environment. From these facts, it is presumed that the configuration of the present magnetic material described above suppresses thermal oxidation, particularly of the cured resin, and thus maintains high insulation resistance and mechanical strength even in a high-temperature environment of about 180°C. The magnetic material of the present invention contains at least an iron alloy powder having an inorganic insulating layer and a resin cured product, and may further contain other components within a range that does not impair the effects of the present invention. Each component of the magnetic material of the present invention will be described below.

[0017] <Iron alloy powder> In the magnetic body, the iron alloy powder contains 4 to 10 parts by mass of Si in 100 parts by mass of the iron alloy powder. By containing Si, the soft magnetic powder has a relatively high magnetic permeability. Furthermore, in this embodiment, by containing 4 parts by mass or more of Si, the oxidation of the iron alloy powder and the thermal decomposition of the resin cured product can be suppressed. From the viewpoint of the heat resistance of the magnetic body, the amount of Si in 100 parts by mass of the iron alloy powder is preferably 4.5 parts by mass or more, more preferably 5 parts by mass or more. On the other hand, the effect of suppressing thermal decomposition is sufficient if the amount of Si in 100 parts by mass of the iron alloy powder is 10 parts by mass or less, and by making the amount of Si 10 parts by mass or less, preferably 8 parts by mass or less, more preferably 7 parts by mass or less, the deterioration of the magnetic properties can be suppressed, and the hardness and brittleness of the iron alloy powder can be suppressed, and the handling during processing is also excellent.

[0018] The iron alloy powder may further contain other elements within the range in which the effects of the present invention are achieved. Examples of other elements include Cr, Al, Mn, Ni, C, O, N, S, P, B, and Cu. From the viewpoint of heat resistance, it is preferable that the iron alloy powder contains at least one element selected from Cr and Al. Cr and Al form a passive layer on the surface of the iron alloy powder, which suppresses oxidation of the iron alloy powder in a high-temperature environment, and also suppresses contact between the resin cured product and iron, thereby suppressing oxidation of the resin cured product. The proportion of Cr or Al in the iron alloy powder is preferably 0.5 to 10 mass%, more preferably 3 to 8 mass parts, based on 100 mass% of the iron alloy powder from the viewpoints of heat resistance and rust prevention. When both Cr and Al are contained, the total mass is preferably within the above range. The total content of elements other than Cr and Al is preferably 1% by mass or less, and more preferably 0.5% by mass or less, in 100% by mass of the iron alloy powder, from the viewpoints of heat resistance and magnetic properties.

[0019] The shape of the iron alloy powder may be spherical, elliptical, needle-like, rod-like, plate-like, etc., and a spherical shape is preferred from the viewpoints of filling the mold when molding the magnetic material and reducing the contact area with the resin cured product, etc. The average particle size of the iron alloy powder is preferably 1 to 100 μm, more preferably 3 to 60 μm, from the viewpoint of heat resistance, and further preferably 5 to 30 μm from the viewpoint of the skin effect in use in a frequency band of 1 MHz or more.

[0020] The method for producing the iron alloy powder is not particularly limited, and may be appropriately selected from known methods such as atomization, melt spinning, rotating electrode, mechanical alloying, and chemical precipitation by reduction. The atomization method is preferred because it can produce spherical particles. Examples of the atomization method include gas atomization, water atomization, centrifugal atomization, and plasma atomization. Gas atomization and water atomization are preferred from the viewpoint of mass production stability and productivity, and water atomization is preferred from the viewpoint of easy production of powder of 30 μm or less.

[0021] <Inorganic insulating layer> The iron alloy powder has an inorganic insulating layer on its surface. The inorganic insulating layer prevents contact between the iron alloy powder particles, ensuring insulation, and prevents contact between the iron alloy powder and the cured resin, thereby suppressing thermal decomposition of the cured resin. The use of the inorganic insulating layer also provides the insulating layer with excellent heat resistance.

[0022] The inorganic insulating layer may be, for example, SiO 2 (Silicate), Al 2 O 3 (Alumina), ZrO 2 Inorganic oxides such as Si 3 N 4 Examples of the insulating material in the inorganic insulating layer include nitrides such as BN, glass materials such as silicate glass, borate glass, borosilicate glass, phosphate glass, and bismuth glass, and minerals such as mica and clay, and among these, it is preferable to include phosphates and silicates. The insulating material in the inorganic insulating layer can be used alone or in combination of two or more kinds.

[0023] The inorganic insulating layer is preferably 0.1 parts by mass or more, more preferably 0.3 parts by mass or more, and even more preferably 0.5 parts by mass or more, per 100 parts by mass of the iron alloy powder in terms of ensuring insulation resistance and suppressing oxidation of the resin cured product. The inorganic insulating layer may be 3 parts by mass or less, per 100 parts by mass of the iron alloy powder, and is preferably 2.5 parts by mass or less, more preferably 2.0 parts by mass or less, in terms of magnetic properties.

[0024] The average thickness of the inorganic insulating layer is preferably from 10 to 100 nm, and more preferably from 10 to 60 nm, from the viewpoints of ensuring insulation resistance and suppressing oxidation of the cured resin. The thickness of the inorganic insulating layer can be determined by observing the surface of the metal powder with a transmission electron microscope (TEM). In addition, the average thickness of the inorganic insulating layer can be calculated simply by assuming that the metal powder is a spherical particle of a uniform particle size, using the specific surface area of ​​the metal powder and the specific gravity of the insulating material, using the following formulas (1) and (2). Equation (1): Specific surface area of ​​metal powder (m 2 / g) = 6 / [specific gravity of metal powder (g / m 3 ) × particle size of metal powder (m)] Equation (2): Inorganic insulating layer thickness (m) = mass of insulating material (g) / [mass of metal powder (g) × specific surface area of ​​metal powder (m 2 / g) × specific gravity of coating powder (g / m 3 )]

[0025] The method for providing the iron alloy powder with an inorganic insulating layer can be appropriately selected from, for example, a powder mixing method, a dipping method, a sol-gel method, a CVD method, a PVD method, or various other known methods.

[0026] <Cured resin> The magnetic material includes a cured resin having a polyesterimide in the molecule. In the present invention, polyesterimide refers to a material having two or more ester bonds and two or more imide bonds in the molecule. The magnetic material has a three-dimensional structure in which a plurality of polymer chains are cross-linked, and the cured resin has a plurality of ester bonds and a plurality of imide bonds, which stabilizes the structure and suppresses thermal decomposition in a high-temperature environment of 180°C.

[0027] The resin cured product in the magnetic body is preferably a cured product of a thermosetting resin from the viewpoint of achieving both processability during heat molding and heat resistance after production. In the present invention, the resin cured product refers to a thermosetting resin in which at least a part of the resin has undergone a crosslinking reaction. The thermosetting resin, which is a precursor of the resin cured product, will be described below.

[0028] The thermosetting resin may be any resin that forms a cured product containing a polyesterimide structure after curing. Among them, a thermosetting resin composition containing a polyester resin, an epoxy resin, and a polyimide resin is preferred because the magnetic body can be easily molded at a low temperature. By using the thermosetting resin composition, the heating temperature during molding can be set to, for example, about 180°C.

[0029] The polyester resin can be appropriately selected from polymers of polycarboxylic acid and polyol, and among them, polyester resins having a carboxyl group are preferred from the viewpoint of reactivity with epoxy resins. The polycarboxylic acid can be appropriately selected from compounds having two or more carboxylic acids in one molecule, and among them, a dicarboxylic acid having two carboxylic acids in one molecule or an anhydride thereof is preferable. Specific examples of the dicarboxylic acid include terephthalic acid, isophthalic acid, naphthalenedicarboxylic acid, succinic acid, adipic acid, and maleic acid, and may be used alone or in combination of two or more. In the present invention, it is preferable that the polycarboxylic acid contains one or more selected from isophthalic acid and maleic acid. The polyol can be appropriately selected from compounds having two or more hydroxyl groups in one molecule.Specific examples of the polyol include ethylene glycol, propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 2-methyl-1,3-propanediol, 3-methyl-1,5-pentanediol, diethylene glycol, dipropylene glycol, neopentyl glycol, 1,3-butanediol, trimethylolpropane, glycerin, 1,4-cyclohexanediol, cyclohexanedimethanol, bisphenol A, bisphenol F, etc., and can be used alone or in combination of two or more.

[0030] The polyester resin can be obtained by subjecting the polycarboxylic acid and the polyol to a dehydration condensation reaction by a known method. Alternatively, a commercially available product having a desired structure may be used.

[0031] The epoxy resin can be appropriately selected from compounds having one or more epoxy groups in one molecule. Specific examples of suitable epoxy resins include epibis-based epoxy resins obtained by condensation reaction of epichlorohydrin with bisphenol A, bisphenol F, and alkylene oxide modified products thereof; novolac-based epoxy resins obtained by condensation reaction of epichlorohydrin with phenolic resin; alkyl glycidyl ethers such as methyl glycidyl ether and butyl glycidyl ether, and the like, and can be used alone or in combination of two or more.

[0032] The polyimide resin may be appropriately selected from compounds having two or more imide bonds in one molecule. Among them, from the viewpoint of crosslinking with other resins, those having an ethylenic double bond are preferred, and N,N'-(4,4'-diphenylmethane)diallylnadiimide and N,N'-(m-xylylene)diallylnadiimide are preferred. The polyimide resin may be used alone or in combination of two or more.

[0033] The blending ratio of the above thermosetting resin composition is preferably 20 to 50 parts by mass of polyester resin, 1 to 25 parts by mass of epoxy resin, and 1 to 15 parts by mass of polyimide resin, from the viewpoint of heat resistance and mechanical strength of the obtained resin cured product.

[0034] The thermosetting resin composition may further contain other components, such as a vinyl monomer, an epoxy acrylate, a curing agent, and a catalyst. Examples of the vinyl monomer include monomers having a vinyl group, a (meth)acryloyl group, etc., such as vinyl monomers such as vinyl acetate and styrene, and acrylic monomers such as methyl (meth)acrylate, etc. The (meth)acryloyl group refers to an acryloyl group or a methacryloyl group, and the same applies to (meth)acrylate. Examples of epoxy acrylates include compounds obtained by reacting the epoxy group of various epoxy resins with the carboxyl group of (meth)acrylic acid. As a curing agent for promoting the curing reaction of the thermosetting resin composition, a peroxide is preferable.Specific examples of the peroxide include dicumyl peroxide, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, 2,2-bis(tert-butyldioxy)octane, t-butylperoxatate, dicumyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, α,α'-bis(t-butylperoxy-m-isopropyl)benzene, t-butyl-cumyl-peroxide, di-t-butyl-peroxide, 2,5-dimethyl,2,5-di(t-butylperoxy)hexane-3, etc. Furthermore, examples of reaction catalysts for the carboxyl group and the epoxy group include imidazole and tertiary amines.

[0035] When a vinyl monomer or epoxy acrylate is blended into the thermosetting resin composition, the blending ratio is preferably such that the ratio of the total of the polyester resin, the epoxy resin, and the polyimide resin to the total of the vinyl monomer and the epoxy acrylate is 1:3 to 3:1 by mass.

[0036] The magnetic material can be obtained, for example, by dispersing the iron alloy powder having the insulating layer in the thermosetting resin composition, filling it into a mold of a desired shape, and heating it. The heating conditions vary depending on the reactivity of the thermosetting resin composition, but for example, heating at 150 to 200°C for about 0.5 to 12 hours will allow the crosslinking reaction to proceed sufficiently. In the cured resin obtained by curing the thermosetting resin composition, ester bonds, imide bonds, and hydroxyl groups resulting from the reaction between epoxy groups and carboxyl groups are detected.

[0037] The blending ratio of the thermosetting resin composition and the iron alloy powder may be appropriately adjusted depending on the application, but for example, it is preferably 1 to 10 parts by mass, more preferably 2 to 6 parts by mass, per 100 parts by mass of the iron alloy powder. If it is equal to or more than the lower limit, the mechanical strength of the magnetic material is improved. On the other hand, if it is equal to or less than the upper limit, the magnetic properties are excellent.

[0038] This magnetic material can be used in known applications where magnetic materials are used. Because this magnetic material has excellent long-term heat resistance in a high-temperature environment of 180°C, it can be suitably used for in-vehicle applications that require heat resistance, particularly as a core material for inductors that are placed near the engine. Furthermore, since the heat treatment temperature during molding of this magnetic material can be a relatively low temperature of about 180° C., it can be suitably used for coil-embedded magnetic elements, which will be described later.

[0039] [Magnetic elements] An example of the magnetic element according to the present invention (also referred to as the present magnetic element) will be described with reference to Figs. 1 and 2. Fig. 1 is a schematic top view of the magnetic element 1, and Fig. 2 is a schematic AA cross-sectional view of Fig. 1. The terminal portion 12 in Fig. 1 is attached to the magnetic body 10 using an adhesive member 13 in Fig. 2. The present magnetic element has a magnetic body 10 and a coil 11 embedded in the magnetic body 10, and the magnetic body 10 is the magnetic body according to the present invention. In the present magnetic element, at least the winding portion of the coil 11 may be embedded in the magnetic body 10, and a part of the coil 11 may be exposed from the magnetic body 10. For example, the terminal portion may be copper plated with Sn or the like in terms of wettability of lead-free solder or the like. The copper of the terminal portion may be joined to the coil 11 or may be integral with it.

[0040] The shape of the coil 11 is appropriately selected from among known coils used in magnetic elements, and usually has a winding portion and a terminal portion for connecting to a circuit, etc. The material of the coil 11 is not particularly limited, and may be, for example, a copper wire, etc., and the copper wire preferably has an insulating coating. As the insulating coating, a polyamideimide film, a polyimide film, etc. are preferable from the viewpoint of heat resistance.

[0041] When manufacturing a coil-embedded magnetic element, in the method for manufacturing a magnetic body, a coil may be disposed in a mold before or during filling of the magnetic body in the mold. Although not shown, a magnetic element manufactured by winding a coil around the magnetic body also has excellent long-term heat resistance in a high-temperature environment of 180°C. The magnetic element can be suitably used as an inductor for use in a power inductor, a choke coil, a transformer, and the like. EXAMPLES

[0042] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to these descriptions.

[0043] Example 1 First, an iron alloy powder containing 4.5 to 7 mass % of Si, 3 to 8 mass % of Cr and having an average particle size of 10 μm per 100 parts by mass was prepared. The iron alloy powder was coated with a phosphoric acid-based inorganic insulating material in an amount of 0.5 parts by mass per 100 parts by mass of the iron alloy powder to form an insulating layer (the insulating layer had a thickness of about 10 nm). A thermosetting resin composition in an amount of 5 parts by mass per 100 parts by mass of the iron alloy powder was added to the iron alloy powder with the insulating layer and kneaded to obtain an iron alloy powder coated with the resin composition. The obtained iron alloy powder was passed through a 500 μm metal mesh, and the particle size was adjusted so that it would be easy to fill into a die, and then granulated. The granulated powder was filled into a ring-shaped die with an outer diameter of 13 mm and an inner diameter of 8 mm, and the powder was compressed at 5 ton / cm. 2 The resulting ring-shaped sample was thermally cured in a thermostatic chamber at a temperature of 180° C. for 2 hours or more to obtain the composite magnetic element of Example 1.

[0044] Example 2 A magnetic body of Example 2 was obtained in the same manner as in Example 1, except that the amount of the phosphate-based inorganic insulating material in Example 1 was changed to 1.5 parts by mass (the thickness of the insulating layer was about 50 nm).

[0045] Example 3 An insulator of Example 3 was obtained in the same manner as in Example 1, except that the amount of the phosphoric acid-based inorganic insulating material was changed to 1.5 parts by mass and the amount of the thermosetting resin composition was changed to 2 parts by mass.

[0046] Comparative Example 1 A magnetic body of Comparative Example 1 was obtained in the same manner as in Example 1, except that the insulating coating treatment was not carried out.

[0047] Comparative Example 2 A magnetic body of Comparative Example 2 was obtained in the same manner as in Comparative Example 1, except that the thermosetting resin in Comparative Example 1 was changed to a thermosetting phenolic resin.

[0048] Comparative Example 3 A magnetic body of Comparative Example 3 was obtained in the same manner as in Comparative Example 1, except that the thermosetting resin in Comparative Example 1 was changed to an epoxy resin having a glass transition temperature of 250° C. or higher.

[0049] Comparative Example 4 A magnetic body of Comparative Example 4 was obtained in the same manner as in Comparative Example 1, except that the thermosetting resin in Comparative Example 1 was changed to a silicone resin.

[0050] Comparative Example 5 A magnetic body of Comparative Example 5 was obtained in the same manner as in Comparative Example 1, except that the thermosetting resin composition in Example 1 was changed to a thermosetting phenolic resin.

[0051] Comparative Example 6 As the iron alloy powder, an iron alloy powder containing 0.5 mass % of Si and 1 mass % of Cr per 100 parts by mass and having an average particle size of 10 μm was prepared. The iron alloy powder was coated with a silicate-based inorganic insulating material in an amount of 1 part by mass per 100 parts by mass of the iron alloy powder to form an insulating layer (the insulating layer had a thickness of about 30 nm). A thermosetting resin composition in an amount of 5 parts by mass per 100 parts by mass of the iron alloy powder was added to the iron alloy powder with the insulating layer and kneaded to obtain an iron alloy powder coated with the resin composition. The subsequent steps were the same as in Example 1, except that the thermosetting resin composition in Example 1 was changed to a thermosetting phenolic resin, to obtain a magnetic body of Comparative Example 6.

[0052] Comparative Example 7 The magnetic body of Comparative Example 7 was obtained in the same manner as Comparative Example 1, except that in Example 1, 0.5 parts by mass of the phosphate-based inorganic insulating material was changed to 1 part by mass of a silicate-based insulating material, and the thermosetting resin composition was changed to a thermosetting phenolic resin.

[0053] Comparative Example 8 A magnetic body of Comparative Example 7 was obtained in the same manner as in Comparative Example 7, except that the iron alloy powder was changed to iron alloy powder containing 6.5 mass % Si per 100 parts by mass and having an average particle size of 10 μm.

[0054] <Evaluation of magnetic materials> The magnetic materials of the examples and comparative examples were evaluated by the following methods. The outer diameter, inner diameter and height of the ring-shaped magnetic body obtained above were measured with a vernier caliper, and the apparent density was calculated from the volume and weight. The initial magnetic permeability was measured at a frequency of 1 MHz using an impedance analyzer after winding 10 turns of copper wire around a ring-shaped magnetic body having an outer diameter of 13 mm and an inner diameter of 8 mm. The insulation resistance of the magnetic material was measured with an insulation resistance meter by placing electrodes with a diameter of 1 mm on the top and bottom surfaces of the magnetic material. The strength of the magnetic material was evaluated by carrying out a compression test in accordance with the radial crushing strength test method of JIS Z2507 and calculating the radial crushing strength from Equation 1. K = [F × (De)] / (L × e 2 ) :Formula (1) K: Radial crushing strength (MPa) F: Maximum load at break (N) L: Length of hollow cylinder (mm) D: Outer diameter of hollow cylinder (mm) e: wall thickness of hollow cylinder (mm)

[0055] (Heat resistance evaluation) Heat resistance was evaluated by storing the magnetic materials of the examples and comparative examples in an air environment at 180°C, and after 1000 hours, the insulation resistance and radial crushing strength were measured in the same manner as above. Note that for comparative examples 5 to 8, only the insulation resistance was measured. The results are shown in Tables 1 to 5. The strength retention rate was calculated by (radial crushing strength after standing for 1000 hours) / (radial crushing strength immediately after production)×100(%). For the magnetic bodies of Examples 1 and 2 and Comparative Examples 5 to 8, the insulation resistance was repeatedly measured up to 1000 hours to confirm the change over time during the heat resistance evaluation period. For the magnetic bodies of Examples 1 and 2 and Comparative Example 1, the weight of the magnetic body was repeatedly measured up to 1000 hours to confirm the change in weight during the heat resistance evaluation period. Figure 3 shows a graph showing the change in insulation resistance over time. Figure 4 shows a graph showing the change in weight over time.

[0056] [Table 1]

[0057] [Table 2]

[0058] [Table 3]

[0059] [Table 4]

[0060] [Table 5]

[0061] For stable use in an environment of 180°C, the insulation resistance after 1000 hours must be 10 7 Ω or more, and the radial crushing strength is preferably 50 MPa or more. Comparative Examples 1 to 4 have lower insulation resistance than the Examples because there is no insulating coating. Comparative Example 4 has relatively high insulation resistance, but low radial crushing strength. Comparative Example 6 has high initial insulation resistance because there is an insulating coating, but since Si is less than 4, the insulation resistance drops significantly. Comparative Examples 7 and 8, which used a silicate-based insulating material, are excellent in terms of insulation resistance after 1000 hours, but the radial crushing strength is equivalent to that of Comparative Example 5 and is insufficient. In addition, Comparative Example 1 has no insulating coating, so there is a large weight change due to thermal decomposition of the resin cured product. It was revealed that the magnetic bodies of Examples 1 to 4, which comprise an iron alloy powder having an inorganic insulating layer on its surface and a cured resin, in which 100 parts by mass of the iron alloy powder contains 4 to 10 parts by mass of Si, and in which the cured resin contains polyesterimide, have high initial radial crushing strength, excellent insulating properties after being left standing for 1,000 hours, and also maintain their strength. [Explanation of symbols]

[0062] 10 Magnetic material 11 Coil 12 Terminal section 13 Adhesive materials

Claims

1. The present invention includes an iron alloy powder having an inorganic insulating layer on a surface thereof, and a cured resin material, The iron alloy powder contains 4 to 10 parts by mass of Si per 100 parts by mass of the iron alloy powder, The magnetic material, wherein the cured resin comprises polyesterimide.

2. The magnetic body according to claim 1 , wherein the inorganic insulating layer contains at least one selected from the group consisting of phosphates and silicates.

3. 3. The magnetic body according to claim 1, wherein the inorganic insulating layer has a content of 0.1 to 3 parts by mass with respect to 100 parts by mass of the iron alloy powder.

4. The magnetic body according to any one of claims 1 to 3, wherein the iron alloy powder further contains one or more selected from Cr and Al.

5. The magnetic body according to any one of claims 1 to 4, wherein the iron alloy powder has an average particle size of 5 to 30 µm.

6. The magnetic body according to any one of claims 1 to 5, wherein the inorganic insulating layer has an average thickness of 10 to 100 nm.

7. The magnetic body according to any one of claims 1 to 6, wherein the ratio of the cured resin is 2 to 6 parts by mass with respect to 100 parts by mass of the iron alloy powder.

8. The magnetic body according to any one of claims 1 to 7, wherein the resin cured product comprises a cured product of a thermosetting resin composition containing a polyester-based resin, an epoxy-based resin, and a polyimide-based resin.

9. The magnetic body according to claim 8 , wherein the polyester resin has a carboxy group.

10. The magnetic material according to claim 8 or 9, wherein the polyimide resin has an ethylenic double bond.

11. The magnetic body according to any one of claims 8 to 10, wherein the thermosetting resin composition contains a peroxide.

12. A magnetic body according to any one of claims 1 to 11, A magnetic element comprising: a coil embedded in the magnetic body.

Citation Information

Patent Citations

  • Composite slice type inductive element and preparation method thereof

    CN101325126A

  • Magnetic material, magnetic core, and method for manufacturing the same

    JP2017188680A

  • Coil component

    JP2018056524A

  • Inductor and method of manufacturing the same

    JP2019102713A

  • Soft magnetic metal powder, powder magnetic core and magnetic component

    JP2019160944A