Metal organic structure

A novel MOF using triptycene and polyvalent metal ions enhances gas adsorption, particularly hydrogen and carbon dioxide, addressing the inefficiencies of existing frameworks.

JP7555914B2Active Publication Date: 2024-09-25RIKKYO EDUCATIONAL +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2021519424
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-09-24
Filing Date
2020-05-11
Publication Date
2024-09-25
Estimated Expiration
2040-05-11

AI Technical Summary

Technical Problem

Existing metal-organic frameworks (MOFs) are not effective in adsorbing gases such as hydrogen molecules, nitrogen molecules, and carbon dioxide at a practical level.

Method used

A novel MOF is developed using triptycene as a core and a polyvalent metal ion with a three-dimensional spatial expansion and a carboxylic acid ion, capable of adsorbing gases like hydrogen and carbon dioxide.

Benefits of technology

The novel MOF effectively adsorbs more hydrogen and carbon dioxide molecules compared to conventional methods, making it suitable for practical applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007555914000038
    Figure 0007555914000038
  • Figure 0007555914000039
    Figure 0007555914000039
  • Figure 0007555914000001
    Figure 0007555914000001
Patent Text Reader

Abstract

The present invention addresses the problem of providing a metal-organic structural body capable of adsorbing gases such as carbon dioxide and hydrogen molecules at a practical level for use. This metal-organic structural body is used for adsorbing gases such as carbon dioxide and hydrogen and includes a multivalent metal ion and a carboxylate ion represented by formula [I] [in formula [I], X1-X3 each independently represent a functional group represented by formula [II] (in formula [II], Z represents a single bond or a multivalent linkage group, k represents an integer of 1-4, * indicates the position at which a bond is formed with a benzene ring, Y1 and Y2 each independently represent a hydrogen atom, a halogeno group, a C1-6 alkyl group, or the like, but, when said multivalent metal ion is a trivalent metal ion, Y1 and Y2 each independently represent a halogeno group, a C1-6 alkyl group, or the like)], wherein the carboxylate ion and the multivalent metal ion are bound to each other.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a novel metal-organic framework and a gas adsorption method using the metal-organic framework. This application claims priority to Japanese Patent Application No. 2019-90662 filed on May 13, 2019, and Japanese Patent Application No. 2019-172510 filed on September 24, 2019, the contents of which are incorporated herein by reference. [Background technology]

[0002] Metal-organic frameworks (hereinafter sometimes referred to as "MOFs") are solid substances that have a polymer structure with internal spaces (i.e., pores) created by combining metal ions with bridging organic ligands that link them. They have attracted great interest over the past decade as porous materials with functions such as gas storage and separation. As the crosslinkable organic ligands, oxygen donor ligands and nitrogen donor ligands have been widely used.

[0003] It is known that an MOF obtained from triptycene-9,10-dicarboxylic acid having a triptycene skeleton as a crosslinkable organic ligand, zinc nitrate, and dipyridyl adsorbs low molecular weight compounds such as diacetylene and amyl acetate (see Patent Document 1).

[0004] In addition, hexakis(4-carboxyphenyl)triptycene, in which two 4-carboxyphenyl groups are symmetrically arranged on each benzene ring of triptycene, forms polymeric structures with intramolecular pores via hydrogen bonds between the carboxylic acid groups, and these are known to adsorb nitrogen molecules and carbon dioxide molecules (see Non-Patent Document 1).

[0005] In addition, hexakis(4-carboxyphenyl)triptycene, in which two 4-carboxyphenyl groups are symmetrically arranged on each benzene ring of triptycene, was used as an organic ligand, and the Fe 3+ , Cr 3+ and Sc 3+ The MOF with trivalent metal ions is 3580m2 / g~4280m 2 / g and is known to adsorb water molecules (see Non-Patent Document 2).

[0006] Meanwhile, with the advent of a hydrogen society, research into hydrogen adsorption by MOFs has been actively conducted. For example, it is known that a MOF consisting of a tricarboxylate ion and a zinc cluster ion having the following structure can adsorb 6% by mass of hydrogen at room temperature and 90 atm (see Patent Document 2).

[0007] [ka] [Prior art documents] [Patent documents]

[0008] [Patent Document 1] International Publication No. 2009 / 0098001 Brochure [Patent Document 2] JP 2018-058814 A [Non-patent literature]

[0009] [Non-Patent Document 1] JFStoddart, et al, Angew. Chem. Int. Ed., 2019, 58,1664-1669. [Non-Patent Document 2] JFStoddart, et al, J. Am. Chem. Soc., 2019, 141, 2900-2905. Summary of the Invention [Problem to be solved by the invention]

[0010] There are currently no known MOFs capable of adsorbing gases such as hydrogen molecules, nitrogen molecules, and carbon dioxide at practical levels. An objective of the present invention is to provide a novel MOF capable of adsorbing gases such as hydrogen molecules, nitrogen molecules, and carbon dioxide. [Means for solving the problem]

[0011] As a result of intensive research aimed at solving the above-mentioned problems, the inventors discovered that an MOF obtained using an organic ligand having a three-dimensional spatial extent with a triptycene core and a polyvalent metal ion has a high ability to adsorb gases such as hydrogen molecules, nitrogen molecules, and carbon dioxide, thereby completing the present invention.

[0012] That is, the present invention is as follows, which is specified by the items shown below. [1] A polyvalent metal ion and a compound represented by the formula [I] [ka] [In formula [I], X 1 ~X 3 Each independently represents the formula [II] [ka] (in formula [II], Z represents a single bond or a polyvalent linking group, k represents an integer of 1 to 4, and * means that the compound is bonded to a benzene ring at the position indicated, and the same applies hereinafter), R 1 ~R 3each independently represents a hydrogen atom, a C1-6 alkyl group, a C3-8 cycloalkyl group, a C6-10 aryl group, a 3- to 6-membered heterocyclyl group, a C1-6 alkoxy group, a C6-10 aryloxy group, a heteroaryloxy group, a halogeno group, a C1-6 haloalkyl group, a C6-10 haloaryl group, a C1-6 haloalkoxy group, a C1-6 alkylthio group, a C6-10 arylthio group, a heteroarylthio group, a C1-6 alkylsulfinyl group, a C6-10 arylsulfinyl group, a heteroarylsulfinyl group, a C1-6 alkylsulfonyl group, a C6-10 arylsulfonyl group, a heteroarylsulfonyl group, a cyano group, a nitro group, or a group represented by formula [III]. [ka] (In formula [III], R 11 and R 12 each independently represents a hydrogen atom, a C1-6 alkyl group, a C6-10 aryl group, a C1-6 alkylcarbonyl group, or a C6-10 arylcarbonyl group. a is X 1 and is 0, 1, 2, 3, or 4; when a is 2 or more, there are multiple X 1 may be the same or different from each other. a1 is R 1 and is 0, 1, 2, 3, or 4; when a1 is 2 or more, a plurality of R 1 may be the same or different from each other. b is X 2 and is 0, 1, 2, 3, or 4; when b is 2 or more, there are multiple X 2 may be the same or different from each other. b1 is R 2 and is 0, 1, 2, 3, or 4; when b1 is 2 or more, a plurality of R 2 may be the same or different from each other. c is X 3 and is 0, 1, 2, 3, or 4; when c is 2 or more, there are multiple X 3 may be the same or different from each other. c1 is R 3and is 0, 1, 2, 3, or 4; when c1 is 2 or more, multiple R 3 may be the same or different from each other. However, a+b+c is 2 or greater. Y 1 , Y 2 each independently represents a hydrogen atom, a halogeno group, a C1-6 alkyl group, or a C1-6 alkoxy group. However, when the polyvalent metal ion is a trivalent metal ion, Y 1 , Y 2 each independently represents a halogeno group, a C1-6 alkyl group, or a C1-6 alkoxy group.] The metal organic framework contains a carboxylate ion represented by the formula: [2] The metal organic structure according to [1], wherein the polyvalent metal ion is an ion of at least one metal selected from the group consisting of metals in groups 2 to 13 of the periodic table. [3] The metal organic structure according to [1] or [2], wherein the polyvalent metal ion is an ion of at least one metal selected from Zn, Fe, Co, Ni, Cu, Zr, and Mg. [4] The metal organic structure according to any one of [1] to [3], wherein the polyvalent linking group of Z in the formula [I] is a divalent or trivalent linking group. [5] The polyvalent linking group of Z in formula [I] is a linking group selected from linking group group A consisting of a di- to tetravalent linking group derived from an alkane having an unsubstituted or substituted group (excluding a carboxy group), a di- to tetravalent linking group derived from an ethene having an unsubstituted or substituted group (excluding a carboxy group), an ethynylene group, a di- to tetravalent linking group derived from an aryl having an unsubstituted or substituted group (excluding a carboxy group), a di- to tetravalent linking group derived from a heteroaryl having an unsubstituted or substituted group (excluding a carboxy group), and a combination thereof; -O-, -S-, -S(O)-, -SO2-, -C(═O)-, -O ... [ka] (In the formula, R 21 and R 22each independently represents a hydrogen atom, a C1-6 alkyl group, a C6-10 aryl group, a C1-6 alkylcarbonyl group, or a C6-10 arylcarbonyl group.) and a combination thereof, or a combination of a linking group selected from linking group group A and a linking group selected from linking group group B, provided that the carboxylate ion group (CO2 - The metal organic structure according to any one of [1] to [4], wherein the carbon atom in Z of the formula [II] is bonded to the metal organic structure. [6] In the formula [I], the formula [II] is the formula [V-1] or the formula [V-2], [ka] (In formula [V-2], Z 1 represents a single bond, -C≡C-, -O-, -S-, -S(O)-, -SO2- or -C(=O)-. R 31 represents a C1-6 alkyl group, a C3-8 cycloalkyl group, a C6-10 aryl group, a 3- to 6-membered heterocyclyl group, a C1-6 alkoxy group, a C6-10 aryloxy group, a heteroaryloxy group, a halogeno group, a C1-6 haloalkyl group, a C6-10 haloaryl group, a C1-6 haloalkoxy group, a C1-6 alkylthio group, a C6-10 arylthio group, a heteroarylthio group, a C1-6 alkylsulfinyl group, a C6-10 arylsulfinyl group, a heteroarylsulfinyl group, a C1-6 alkylsulfonyl group, a C6-10 arylsulfonyl group, a heteroarylsulfonyl group, a cyano group, a nitro group, or a group represented by formula [VI]. [ka] (In formula [VI], R 41 and R 42 each independently represents a hydrogen atom, a C1-6 alkyl group, a C6-10 aryl group, a C1-6 alkylcarbonyl group, or a C6-10 arylcarbonyl group. n is R 31 and is 0, 1, 2, 3, or 4; when n is 2 or more, there are multiple R 31 may be the same or different from each other. n1 is CO2 - and is 1 or 2. [7] The metal organic structure according to any one of [1] to [6], further comprising an organic ligand other than the carboxylate ion represented by the formula [I] as a constituent component. [8] A gas storage method comprising the steps of contacting a gas with the metal-organic framework according to any one of [1] to [7] and adsorbing the gas inside the metal-organic framework. Effect of the Invention

[0013] By using the MOF of the present invention, it is possible to adsorb more hydrogen molecules and carbon dioxide molecules than conventional methods. [Brief description of the drawings]

[0014] [Figure 1] 1 shows a nitrogen adsorption isotherm at 77 K for metal organic framework 1 obtained in Example 1. [Diagram 2] 1 shows a hydrogen adsorption isotherm at 77 K for metal organic framework 1 obtained in Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The metal organic framework of the present invention is a metal organic framework in which a polyvalent metal ion is bonded to a carboxylate ion group in an organic ligand represented by formula [I]. The polyvalent metal ion used in the present invention is preferably an ion of at least one metal selected from the group consisting of metals of Groups 2 to 13 of the periodic table, and is preferably an ion of at least one metal selected from Zn, Fe, Co, Ni, Cu, Zr, Sc, Cr, Al, and Mg. Among the polyvalent metal ions, a divalent or tetravalent metal ion is preferable, and is preferably an ion of at least one metal selected from Zn, Fe, Co, Ni, Cu, Zr, and Mg, and is further preferably an ion of at least one metal selected from Co, Ni, Cu, Zr, and Zn.

[0016] These polyvalent metal ions are supplied in the form of various salts, such as Zn(NO3)2·6H2O, Zn(NO3)2·4H2O, ZrCl4, ZrOCl2, Ni(NO3)2·6H2O, Mg(NO3)2·6H2O, Cu(NO3)2·xH2O, Cu(NO3)2·2.5H2O, Co(NO3)2·6H2O, Cr(NO3)3·9H2O, CrCl3·6H2O, and Al(NO3). e 9H e Examples include O.

[0017] The organic ligand used in the present invention contains a carboxylate ion represented by the formula [I]. In formula [I], X 1 ~X 3 each independently represents a functional group represented by formula [II]: In formula [II], Z represents a single bond or a polyvalent linking group. A single bond is a carboxylate ion group (CO2 - ) means a direct bond. There are no particular limitations on the polyvalent linking group, so long as it is a linking group that is divalent or higher and can link a benzene ring and a carboxylate ion group, among which divalent or trivalent linking groups are preferred.

[0018] In addition, the structure is not particularly limited as long as it is a structure capable of linking a benzene ring and a carboxylate ion group. Among them, a linking group selected from linking group group A consisting of a di- to tetravalent linking group derived from an alkane having an unsubstituted or substituted group (excluding a carboxy group), a di- to tetravalent linking group derived from an ethene having an unsubstituted or substituted group (excluding a carboxy group), an ethynylene group, a di- to tetravalent linking group derived from an aryl having an unsubstituted or substituted group (excluding a carboxy group), a di- to tetravalent linking group derived from a heteroaryl having an unsubstituted or substituted group (excluding a carboxy group), and a combination thereof, -O-, -S-, -S(O)-, -SO2-, -C(═O)-, -O ...

[0019] [ka]

[0020] (In the formula, R 21 and R 22 each independently represents a hydrogen atom, a C1-6 alkyl group, a C6-10 aryl group, a C1-6 alkylcarbonyl group or a C6-10 arylcarbonyl group.) and a combination thereof, selected from group B of linking groups, or a combination of a linking group selected from group A and a linking group selected from group B of linking groups, can be preferably exemplified. However, in the formula [II], the carboxylate ion group (CO2 - ) is bonded to a carbon atom in Z of formula [II].

[0021] Here, in the present invention, the term "unsubstituted" means that only the group that serves as the mother nucleus is present. When there is no description of "substituted" and only the name of the group that serves as the mother nucleus is described, it means "unsubstituted" unless otherwise specified. On the other hand, "having a substituent" is synonymous with "substituted" and means that any hydrogen atom of the group serving as the mother nucleus is substituted with a functional group (substituent) having the same or different structure as the mother nucleus. Therefore, a "substituent" is another functional group bonded to the functional group serving as the mother nucleus. The number of substituents may be one or more. The two or more substituents may be the same or different. Terms such as "C1-6" indicate that the number of carbon atoms in the parent group is 1 to 6. This number of carbon atoms does not include the number of carbon atoms in the substituent. For example, a butyl group having an ethoxy group as a substituent is classified as a C2 alkoxy C4 alkyl group.

[0022] The "substituent" is not particularly limited as long as it is chemically permissible and has the effect of the present invention. Examples of groups that can be the "substituent" are shown below. C1-6 alkyl groups such as methyl, ethyl, n-propyl, i-propyl, n-butyl, s-butyl, i-butyl, t-butyl, n-pentyl, and n-hexyl groups; C2-6 alkenyl groups such as vinyl group, 1-propenyl group, 2-propenyl group (allyl group), 1-butenyl group, 2-butenyl group, 3-butenyl group, 1-methyl-2-propenyl group, and 2-methyl-2-propenyl group; C2-6 alkynyl groups such as an ethynyl group, a 1-propynyl group, a 2-propynyl group (propargyl group), a 1-butynyl group, a 2-butynyl group, a 3-butynyl group, or a 1-methyl-2-propynyl group;

[0023] C3-8 cycloalkyl groups such as cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, and cubanyl; C6-10 aryl groups such as phenyl and naphthyl groups; C6-10 aryl C1-6 alkyl groups such as benzyl and phenethyl groups; 3- to 6-membered heterocyclyl groups; 3-6 membered heterocyclyl C1-6 alkyl group;

[0024] Hydroxyl; C1-6 alkoxy groups, such as a methoxy group, an ethoxy group, an n-propoxy group, an i-propoxy group, an n-butoxy group, an s-butoxy group, an i-butoxy group, or a t-butoxy group; C2-6 alkenyloxy groups such as a vinyloxy group, an allyloxy group, a propenyloxy group, or a butenyloxy group; C2-6 alkynyloxy groups such as ethynyloxy groups and propargyloxy groups; C6-10 aryloxy groups such as phenoxy and naphthoxy groups; C6-10 aryl C1-6 alkoxy groups such as benzyloxy groups and phenethyloxy groups; 5- to 6-membered heteroaryloxy groups such as thiazolyloxy groups and pyridyloxy groups; 5-6-membered heteroaryl C1-6 alkyloxy groups such as thiazolylmethyloxy groups and pyridylmethyloxy groups;

[0025] Formyl group; C1-6 alkylcarbonyl groups such as acetyl and propionyl groups; Formyloxy group; C1-6 alkylcarbonyloxy groups such as acetyloxy and propionyloxy; C6-10 arylcarbonyl groups such as benzoyl groups; C1-6 alkoxycarbonyl groups, such as a methoxycarbonyl group, an ethoxycarbonyl group, an n-propoxycarbonyl group, an i-propoxycarbonyl group, an n-butoxycarbonyl group, or a t-butoxycarbonyl group; C1-6 alkoxycarbonyloxy groups, such as a methoxycarbonyloxy group, an ethoxycarbonyloxy group, an n-propoxycarbonyloxy group, an i-propoxycarbonyloxy group, an n-butoxycarbonyloxy group, or a t-butoxycarbonyloxy group; Carboxy group;

[0026] halogeno groups such as fluoro, chloro, bromo, and iodo groups; C1-6 haloalkyl groups such as a fluoromethyl group, a difluoromethyl group, a trifluoromethyl group, a 2,2,2-trifluoroethyl group, a pentafluoroethyl group, a 3,3,3-trifluoropropyl group, a 2,2,3,3,3-pentafluoropropyl group, a perfluoropropyl group, a 2,2,2-trifluoro-1-trifluoromethylethyl group, a perfluoroisopropyl group, a 4-fluorobutyl group, a 2,2,3,3,4,4,4-heptafluorobutyl group, a perfluorobutyl group, a perfluoropentyl group, a perfluorohexyl group, a chloromethyl group, a bromomethyl group, a dichloromethyl group, a dibromomethyl group, a trichloromethyl group, a tribromomethyl group, a 1-chloroethyl group, a 2,2,2-trichloroethyl group, a 4-chlorobutyl group, a perchlorohexyl group, and a 2,4,6-trichlorohexyl group; C2-6 haloalkenyl groups, such as a 2-chloro-1-propenyl group and a 2-fluoro-1-butenyl group; C2-6 haloalkynyl groups such as a 4,4-dichloro-1-butynyl group, a 4-fluoro-1-pentynyl group, or a 5-bromo-2-pentynyl group; C1-6 haloalkoxy groups such as a trifluoromethoxy group, a 2-chloro-n-propoxy group, or a 2,3-dichlorobutoxy group; C2-6 haloalkenyloxy groups, such as a 2-chloropropenyloxy group or a 3-bromobutenyloxy group; C1-6 haloalkylcarbonyl groups such as a chloroacetyl group, a trifluoroacetyl group, or a trichloroacetyl group;

[0027] Amino group; C1-6 alkyl-substituted amino groups such as methylamino, dimethylamino, and diethylamino groups; C6-10 arylamino groups such as anilino group and naphthylamino group; C6-10 aryl C1-6 alkylamino groups such as benzylamino groups and phenethylamino groups; Formylamino group; C1-6 alkylcarbonylamino groups, such as an acetylamino group, a propanoylamino group, a butyrylamino group, or an i-propylcarbonylamino group; C1-6 alkoxycarbonylamino groups, such as a methoxycarbonylamino group, an ethoxycarbonylamino group, an n-propoxycarbonylamino group, or an i-propoxycarbonylamino group; Unsubstituted or substituted aminocarbonyl groups, such as an aminocarbonyl group, a dimethylaminocarbonyl group, a phenylaminocarbonyl group, or an N-phenyl-N-methylaminocarbonyl group; imino C1-6 alkyl group such as an iminomethyl group, a (1-imino)ethyl group, or a (1-imino)-n-propyl group; substituted or unsubstituted N-hydroxyimino C1-6 alkyl groups such as an N-hydroxy-iminomethyl group, a (1-(N-hydroxy)-imino)ethyl group, a (1-(N-hydroxy)-imino)propyl group, an N-methoxy-iminomethyl group, or a (1-(N-methoxy)-imino)ethyl group; C1-6 alkoxyimino groups, such as a methoxyimino group, an ethoxyimino group, an n-propoxyimino group, an i-propoxyimino group, or an n-butoxyimino group; Aminocarbonyloxy group; C1-6 alkyl-substituted aminocarbonyloxy groups such as an ethylaminocarbonyloxy group and a dimethylaminocarbonyloxy group;

[0028] Mercapto group; C1-6 alkylthio groups, such as a methylthio group, an ethylthio group, an n-propylthio group, an i-propylthio group, an n-butylthio group, an i-butylthio group, an s-butylthio group, or a t-butylthio group; C1-6 haloalkylthio groups, such as a trifluoromethylthio group and a 2,2,2-trifluoroethylthio group; C6-10 arylthio groups, such as a phenylthio group and a naphthylthio group; 5- to 6-membered heteroarylthio groups, such as thiazolylthio groups and pyridylthio groups;

[0029] C1-6 alkylsulfinyl groups such as a methylsulfinyl group, an ethylsulfinyl group, or a t-butylsulfinyl group; C1-6 haloalkylsulfinyl groups such as a trifluoromethylsulfinyl group and a 2,2,2-trifluoroethylsulfinyl group; C6-10 arylsulfinyl groups, such as phenylsulfinyl groups; 5- to 6-membered heteroarylsulfinyl groups such as thiazolylsulfinyl groups and pyridylsulfinyl groups;

[0030] C1-6 alkylsulfonyl groups such as a methylsulfonyl group, an ethylsulfonyl group, or a t-butylsulfonyl group; C1-6 haloalkylsulfonyl groups such as a trifluoromethylsulfonyl group or a 2,2,2-trifluoroethylsulfonyl group; C6-10 arylsulfonyl groups, such as phenylsulfonyl groups; 5- to 6-membered heteroarylsulfonyl groups, such as thiazolylsulfonyl groups and pyridylsulfonyl groups; C1-6 alkylsulfonyloxy groups, such as a methylsulfonyloxy group, an ethylsulfonyloxy group, or a t-butylsulfonyloxy group; C1-6 haloalkylsulfonyloxy groups such as a trifluoromethylsulfonyloxy group or a 2,2,2-trifluoroethylsulfonyloxy group;

[0031] Tri-C1-6 alkyl-substituted silyl groups, such as trimethylsilyl group, triethylsilyl group, and t-butyldimethylsilyl group; Tri-C6-10 aryl-substituted silyl groups, such as triphenylsilyl groups; Cyano group; Nitro group.

[0032] In addition, any hydrogen atom in these "substituents" may be substituted with a substituent of a different structure. In this case, examples of the "substituents of a different structure" include a C1-6 alkyl group, a C1-6 haloalkyl group, a C1-6 alkoxy group, a C1-6 haloalkoxy group, a halogeno group, a cyano group, a nitro group, a hydroxy group, a carboxy group, and an amino group.

[0033] The above "3- to 6-membered heterocyclyl group" includes 1 to 4 heteroatoms selected from the group consisting of nitrogen, oxygen, and sulfur atoms as ring-constituting atoms. The heterocyclyl group may be either a monocyclic or polycyclic ring. As for the polycyclic heterocyclyl group, as long as at least one ring is a heterocyclic ring, the remaining rings may be any of a saturated alicyclic ring, an unsaturated alicyclic ring, or an aromatic hydrocarbon ring. Examples of the "3- to 6-membered heterocyclyl group" include a 3- to 6-membered saturated heterocyclyl group, a 5- to 6-membered heteroaryl group, and a 5- to 6-membered partially unsaturated heterocyclyl group.

[0034] Examples of the 3- to 6-membered saturated heterocyclyl group include an aziridinyl group, an epoxy group, a pyrrolidinyl group, a tetrahydrofuranyl group, a thiazolidinyl group, a piperidyl group, a piperazinyl group, a morpholinyl group, a dioxolanyl group, and a dioxanyl group.

[0035] Examples of the 5-membered heteroaryl group include a pyrrolyl group, a furyl group, a thienyl group, an imidazolyl group, a pyrazolyl group, an oxazolyl group, an isoxazolyl group, a thiazolyl group, an isothiazolyl group, a triazolyl group, an oxadiazolyl group, a thiadiazolyl group, and a tetrazolyl group. Examples of the 6-membered heteroaryl group include a pyridyl group, a pyrazinyl group, a pyrimidinyl group, a pyridazinyl group, and a triazinyl group. However, in the polyvalent linking group of Z, the substituent of the skeleton serving as the mother nucleus of the polyvalent linking group does not include a carboxy group.

[0036] In Z, the divalent to tetravalent linking group derived from an alkane is a group in which 2 to 4 arbitrary hydrogen atoms on a carbon constituting an alkane are converted into bonds, and specific examples of the linking groups are shown below. Note that a bond means a state in which an electron capable of forming a bond with another functional group is arranged, and "-" written on a carbon represents a bond. In addition, which bond is bonded to the carboxylate ion group and the benzene ring of triptycene can be arbitrarily determined. The same applies below.

[0037] [ka]

[0038] In Z, the divalent to tetravalent linking group derived from ethene is a group in which any 2 to 4 hydrogen atoms on a carbon constituting an alkane are converted into bonds with ethene as a mother nucleus. Specific examples of the linking groups include the following:

[0039] [ka]

[0040] In Z, the divalent to tetravalent linking group derived from an aryl is a group in which any 2 to 4 hydrogen atoms on a carbon constituting the aryl group are converted to bonds, and specific examples of the linking groups include the following:

[0041] [ka]

[0042] In Z, the di- to tetravalent linking group derived from a heteroaryl is a group in which 2 to 4 arbitrary hydrogen atoms on a heteroatom or carbon constituting the heteroaryl are converted to bonds with respect to the heteroaryl as a mother nucleus, and specific examples of the linking group include the following:

[0043] [ka]

[0044] The combination of those in the linking group group A in Z means a combination in which two or more are selected from the group consisting of divalent to tetravalent linking groups derived from alkanes, divalent to tetravalent linking groups derived from ethene, ethynylene groups, divalent to tetravalent linking groups derived from aryls, and divalent to tetravalent linking groups derived from heteroaryls within a chemically permissible range and are bonded via bonds to form a polyvalent linking group as a whole. In the above combinations, the valence of the linking group is not particularly limited, but is preferably 2 or 3. Specific examples of such combinations include the following linking groups.

[0045] [ka]

[0046] In formulas [IV-1] to [IV-3], R 21 and R 22 each independently represents a hydrogen atom, a C1-6 alkyl group, a C6-10 aryl group, a C1-6 alkylcarbonyl group, or a C6-10 arylcarbonyl group.

[0047] The "C1-6 alkyl group" may be a straight chain or a branched chain. Examples of the "C1-6 alkyl group" include a methyl group, an ethyl group, an n-propyl group, an n-butyl group, an n-pentyl group, an n-hexyl group, an i-propyl group, an i-butyl group, an s-butyl group, an t-butyl group, an i-pentyl group, a neopentyl group, a 2-methylbutyl group, and an i-hexyl group.

[0048] The "C6-10 aryl group" may be either a monocyclic or polycyclic group. As long as at least one ring of the polycyclic aryl group is an aromatic ring, the remaining rings may be any of a saturated alicyclic ring, an unsaturated alicyclic ring, or an aromatic ring. Examples of the "C6-10 aryl group" include a phenyl group, a naphthyl group, an azulenyl group, an indenyl group, an indanyl group, and a tetralinyl group.

[0049] Examples of the "C1-6 alkylcarbonyl group" include an acetyl group and a propionyl group. Examples of the "C6-10 arylcarbonyl group" include a benzoyl group and a 1-naphthylcarbonyl group.

[0050] Specific examples of the combinations in the linking group B include the linking groups shown below.

[0051] [ka]

[0052] Specific examples of combinations of a linking group selected from linking group group A and a linking group selected from linking group group B include the linking groups shown below.

[0053] [ka]

[0054] Among the functional groups represented by the formula [II], particularly preferred examples include functional groups represented by the formula [V-1] or [V-2]. In formula [V-2], R 31 represents a C1-6 alkyl group, a C3-8 cycloalkyl group, a C6-10 aryl group, a 3- to 6-membered heterocyclyl group, a C1-6 alkoxy group, a C6-10 aryloxy group, a heteroaryloxy group, a halogeno group, a C1-6 haloalkyl group, a C6-10 haloaryl group, a C1-6 haloalkoxy group, a C1-6 alkylthio group, a C6-10 arylthio group, a heteroarylthio group, a C1-6 alkylsulfinyl group, a C6-10 arylsulfinyl group, a heteroarylsulfinyl group, a C1-6 alkylsulfonyl group, a C6-10 arylsulfonyl group, a heteroarylsulfonyl group, a cyano group, a nitro group, or a group represented by formula [VI].

[0055] The "C1-6 alkyl group" and "C6-10 aryl group" are R 21 Examples of the specific examples are similar to those given in the above. Examples of the "C3-8 cycloalkyl group", "3- to 6-membered heterocyclyl group", "C1-6 alkoxy group", "C6-10 aryloxy group", "heteroaryloxy group", "halogeno group", "C1-6 haloalkyl group", "C1-6 haloalkoxy group", "C1-6 alkylthio group", "C6-10 arylthio group", "heteroarylthio group", "C1-6 alkylsulfinyl group", "C6-10 arylsulfinyl group", "heteroarylsulfinyl group", "C1-6 alkylsulfonyl group", "C6-10 arylsulfonyl group", and "heteroarylsulfonyl group" include the same as the specific examples given in "substituents". Examples of the "C6-10 haloaryl group" include a 4-chlorophenyl group, a 4-fluorophenyl group, and a 2,4-dichlorophenyl group.

[0056] In formula [VI], R 41 and R 42 each independently represents a hydrogen atom, a C1-6 alkyl group, a C6-10 aryl group, a C1-6 alkylcarbonyl group, or a C6-10 arylcarbonyl group, and specifically, R 21Examples of the specific examples are similar to those given in . Specific examples of the formula [VI] include an amino group; C1-6 alkyl-substituted amino groups, such as a methylamino group, a dimethylamino group, and a diethylamino group; C6-10 arylamino groups, such as anilino group and naphthylamino group; C1-6 alkylcarbonylamino groups, such as an acetylamino group, a propanoylamino group, a butyrylamino group, and an i-propylcarbonylamino group; and a benzoylamino group.

[0057] Examples of the group represented by formula [V-2] include the following functional groups.

[0058] [ka]

[0059] In formula [I], R 1 ~R 3 each independently represents a hydrogen atom, a C1-6 alkyl group, a C3-8 cycloalkyl group, a C6-10 aryl group, a 3- to 6-membered heterocyclyl group, a C1-6 alkoxy group, a C6-10 aryloxy group, a heteroaryloxy group, a halogeno group, a C1-6 haloalkyl group, a C6-10 haloaryl group, a C1-6 haloalkoxy group, a C1-6 alkylthio group, a C6-10 arylthio group, a heteroarylthio group, a C1-6 alkylsulfinyl group, a C6-10 arylsulfinyl group, a heteroarylsulfinyl group, a C1-6 alkylsulfonyl group, a C6-10 arylsulfonyl group, a heteroarylsulfonyl group, a cyano group, a nitro group, or a group represented by formula [III]. In addition, in the formula [III], R 11 and R 12 Each independently represents a hydrogen atom, a C1-6 alkyl group, It represents an alkyl group, a C6-10 aryl group, a C1-6 alkylcarbonyl group or a C6-10 arylcarbonyl group. R 1 ~R 3 Specifically, R 31Examples of the specific examples include those exemplified in the above, those exemplified in the "Substituents" section, and those exemplified in formula [VI].

[0060] In formula [I], Y 1 , Y 2 each independently represents a hydrogen atom, a halogeno group, a C1-6 alkyl group, or a C1-6 alkoxy group, and specifically, R 21 However, when the polyvalent metal ion is a trivalent metal ion, Y 1 , Y 2 each independently represents a halogeno group, a C1 to 6 alkyl group, or a C1 to 6 alkoxy group.

[0061] Specific examples of the carboxylate ion represented by the formula [I] include structures such as those shown below.

[0062] [ka]

[0063] [ka]

[0064] [ka]

[0065] [ka]

[0066] The metal organic framework of the present invention can contain an organic ligand other than the organic ligand which is a carboxylate ion represented by formula [I] (hereinafter referred to as the organic ligand represented by formula [I]). Specific examples of such organic ligands include terephthalic acid, phthalic acid, isophthalic acid, 5-cyanoisophthalic acid, 1,3,5-trimesic acid, 1,3,5-tris(4-carboxyphenyl)benzene, 1,3,5-trimesic acid, 4,4'-dicarboxybiphenyl, 3,5-dicarboxypyridine, 2,4-dicarboxypyrazine, 1,3,5-tris(4-carboxyphenyl)benzene, 1,2,4,5-tetrakis(4-carboxyphenyl)benzene, 9,10-anthracenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, [1,1':4',1"]terphenyl-3,3",5,5"-tetracarboxylic acid, biphenyl-3,3",5,5"-tetracarboxylic acid, 3,3',5,5' -tetracarboxydiphenylmethane, 1,3,5-tris(4'-carboxy[1,1'-biphenyl]-4-yl)benzene, 1,3,5-tris(4-carboxyphenyl)triazine, 1,2-bis(4-carboxy-3-nitrophenyl)ethene, 1,2-bis(4-carboxy-3-aminophenyl)ethene, trans,trans-muconic acid, fumaric acid, benzimidazole, imidazole, 1,4-diazabicyclo[2.2.2]octane (DABCO), pyrazine, 4,4'-dipyridyl, 1,2-di(4-pyridyl)ethylene, 2,7-diazapyrene, 4,4'-azobispyridine, bis(3-(4-pyridyl)-2,4-pentanedionato)copper, and the like can be illustrated.

[0067] When an organic ligand represented by formula [I] and an organic ligand other than formula [I] are mixed and used, the molar ratio of the mixture is not particularly limited. For example, in the case of a pillar molecule for constructing a three-dimensional structure such as a pillared layer type structure by crosslinking with a pillar molecule, it is preferable to use an excess of the organic ligand other than formula [I] relative to the organic ligand represented by formula [I].

[0068] The method for producing the metal organic framework of the present invention is not particularly limited, and any of the following methods can be used: solution methods such as a solvent diffusion method, a solvent stirring method, and a hydrothermal method; a microwave method in which a reaction solution is irradiated with microwaves to uniformly heat the entire system in a short time; an ultrasonic method in which pressure changes repeatedly occur in a reaction vessel by irradiating a reaction vessel with ultrasound, and this pressure change causes a phenomenon called cavitation in which the solvent forms bubbles and collapses, and at that time, a high-energy field of about 5000 K and 10000 bar is locally formed as a reaction field for each generation of crystals; a solid-phase synthesis method in which a metal ion source and an organic ligand are mixed without using a solvent; and a LAG (liquid assisted grinding) method in which a metal ion source and an organic ligand are mixed by adding water of about the amount of water of crystallization.

[0069] For example, the method includes steps of preparing a first solution containing a metal compound and a solvent as a source of metal ions, a second solution containing a carboxylic acid and a solvent as raw materials of formula [I], and a third solution containing other organic ligands and a solvent as necessary, and a step of mixing the first solution, the second solution, and the third solution to prepare a reaction liquid, and heating the reaction liquid to obtain a metal organic framework. The first to third solutions do not need to be prepared separately, and for example, the metal compound, the carboxylic acid and the solvent as raw materials of formula [I], the other organic ligands, and the solvent may be mixed at once to prepare one solution.

[0070] The mixing molar ratio of the metal compound to the carboxylic acid serving as the raw material of formula [I] and, if necessary, other organic ligands can be arbitrarily selected depending on the pore size and surface properties of the resulting metal-organic framework. However, it is preferable to use 2 moles or more, and further 3 moles or more of the metal compound relative to the carboxylic acid serving as the raw material of formula [I] and, if necessary, other organic ligands. The concentration of the metal ions in the reaction solution is preferably in the range of 25 to 200 mol / L.

[0071] The concentration of the organic ligand represented by the formula [I] in the reaction solution is preferably in the range of 10 to 100 mol / L. The concentration of the organic ligand other than the formula [I] in the reaction solution is preferably 25 to 100 mol / L.

[0072] The solvent used may be one or more selected from the group consisting of N,N-dimethylformamide (hereinafter referred to as "DMF"), N,N-diethylformamide (hereinafter referred to as "DEF"), N,N-dimethylacetamide and water. Among these, it is preferable to use either DMF, DEF or dimethylacetamide alone, or a DMF / water mixed solvent, a DEF / water mixed solvent or an N,N-dimethylacetamide / water mixed solvent. If necessary, an acid component such as formic acid or acetic acid can be added.

[0073] The heating temperature of the reaction solution is preferably 80° C. or higher, and more preferably 100 to 140° C. When the reaction temperature is 100° C. or higher, the target metal organic framework tends to be easily produced. Also, when the reaction temperature is 140° C. or lower, the solvent such as DMF or DEF is difficult to decompose.

[0074] The method for storing gas using the metal organic framework of the present invention is not particularly limited, but a method having a step of contacting the metal organic framework of the present invention with a gas and adsorbing the gas inside the metal organic framework is preferred, and the contact method is not particularly limited. For example, a method of filling a tank with the gas-metal organic framework of the present invention to form a gas storage tank and flowing a gas into the tank, a method of supporting the metal organic framework of the present invention on the surface constituting the inner wall of a tank to form a gas storage tank and flowing a gas into the tank, a method of forming a tank from a material containing the metal organic framework of the present invention to form a gas storage tank and flowing a gas into the tank, etc. can be mentioned.

[0075] The present invention will be described in detail below using examples, but the scope of the present invention is not limited to the examples. EXAMPLES

[0076] (Production of Metal-Organic Frameworks)

[0077] [ka]

[0078] 4,4',4'',4''',4'''',4'''''-(9,10-dihydro-9,10-[1,2]benzenoanthracene-2,3,6,7,14,15-hexyl)hexabenzoic acid (hereinafter referred to as "organic ligand 1") (101 mg) and zinc nitrate hexahydrate (190 mg) were dissolved in DEF (2 mL). After stirring at room temperature for 10 minutes and filtering, the solution was placed in a screw-cap vial, sealed, and heated at 90°C for 24 hours. After cooling to room temperature, the generated crystals were filtered off, washed with DEF, and then washed with chloroform. The crystals were immersed in chloroform for 24 hours. After filtering, the solid was dried in vacuum to obtain metal-organic framework 1 (61.4 mg). EXAMPLES

[0079] The same procedure as in Example 1 was carried out except that the heating temperature was 120° C. instead of 90° C., to obtain metal organic structure 2 (92.0 mg). EXAMPLES

[0080] The same procedure as in Example 1 was carried out except that DMF was used instead of DEF, thereby obtaining metal organic structure 3 (75.3 mg). EXAMPLES

[0081] The same procedure as in Example 2 was carried out as in Example 1, except that DMF was used instead of DEF, to obtain metal organic structure 4 (97.9 mg). EXAMPLES

[0082] A mixed solution of organic ligand 1 (61.6 mg), DMF (0.8 mL), and triethylamine (0.05 mL) was added to a 10 mL centrifuge tube, and stirred at room temperature for 15 minutes to obtain solution 1. In another 10 mL centrifuge tube, zinc acetate dihydrate (104.5 mg) was added to DMF (1.0 mL), and stirred at room temperature for 15 minutes to obtain solution 2. Solution 2 was added to solution 1, and stirred at room temperature for 2.5 hours. DMF (5.0 mL) was added, and centrifuged. After decantation, the mixture was immersed in DMF. The next day, the mixture was centrifuged and decanted, and then washed with chloroform. After centrifugation and decantation, the mixture was immersed in chloroform for 48 hours. After centrifugation and decantation, the mixture was immersed in chloroform for 48 hours. After centrifugation and decantation, the mixture was immersed in chloroform for 72 hours. After centrifugation and decantation, the mixture was dried under reduced pressure at 150°C for 6 hours to obtain metal-organic structure 5 (78.3 mg). EXAMPLES

[0083] Organic ligand 1 (100.9 mg) and zirconium oxychloride octahydrate (102.2 mg) were dissolved in DMF (5.2 mL) in a 20 mL vial. Formic acid (0.7 mL) was then added. The mixture was heated in an oven at 120°C for 24 hours. After cooling to room temperature, the mixture was washed with DMF, centrifuged, and decanted three times. The mixture was immersed in DMF for 24 hours, centrifuged, and decanted three times. The mixture was immersed in methanol for 24 hours, centrifuged, and decanted three times, and then dried under reduced pressure at 150°C for 6 hours to obtain metal-organic framework 6 (127.9 mg). EXAMPLES

[0084] 2.1 mL of DMF was added to organic ligand 1 (101.6 mg), zinc nitrate hexahydrate (93.3 mg), and 1,4-diazabicyclo[2,2,2]octane (DABCO) (17.0 mg), and the mixture was stirred at room temperature for 10 minutes. After filtration, the mixture was transferred to an autoclave and heated in an oven at 120 ° C for 48 hours. The mixture was cooled to room temperature and decanted. 10 mL of DMF was added, the mixture was stirred at room temperature for 30 minutes, and the mixture was immersed in DMF for 24 hours. After decantation, 10 mL of chloroform was added, and the mixture was stirred at room temperature for 30 minutes. After decantation, the mixture was immersed in chloroform for 48 hours. After centrifugation and decantation, the mixture was dried under reduced pressure at 150 ° C for 6 hours to obtain metal organic framework 7 (73.6 mg). EXAMPLES

[0085] Organic ligand 1 (100.3 mg) and ethanol (0.34 mL) were added to a 50 mL eggplant flask to prepare solution 3. Copper nitrate hemipentahydrate (142.5 mg) was dissolved in water (4.1 mL) in another 50 mL eggplant flask to prepare solution 4. Solution 4 was added to solution 3, and the resulting solution was transferred to an autoclave and heated in an oven at 140°C for 24 hours. After cooling to room temperature, the solution was centrifuged and decanted. The operation of washing with water, centrifugation, and decantation was performed three times. The operation of washing with ethanol, centrifugation, and decantation was performed three times, and then the solution was dried under reduced pressure at 150°C for 6 hours to obtain metal organic framework 8 (62.1 mg). EXAMPLES

[0086] Organic ligand 1 (100.4 mg, 0.103 mmol), magnesium nitrate hexahydrate (79.4 mg, 0.310 mmol) and a mixed solvent (2.5 mL) of tetrahydrofuran (hereinafter referred to as "THF"):water:1M sodium hydroxide aqueous solution = 7:3:2 were added to an autoclave. The mixture was heated in an oven at 100°C for 24 hours. After cooling to room temperature, the mixture was centrifuged and decanted. The operation of washing with DMF, centrifugation, and decantation was repeated three times. The mixture was washed with chloroform and pressure filtered. The mixture was immersed in chloroform for 24 hours, pressure filtered, and then dried under reduced pressure at 150°C for 6 hours to obtain metal organic framework 9 (40.2 mg). EXAMPLES

[0087] Copper nitrate trihydrate (73.4 mg) and organic ligand 1 (101.7 mg) were dissolved in DMF (2.1 mL). After stirring at room temperature for 10 minutes and filtration, the solution was placed in a screw-cap vial, sealed, and heated at 90°C for 36 hours. After cooling to room temperature, DMF was added, centrifuged, and decanted. Chloroform was added, centrifuged, decanted, and then immersed in chloroform for 24 hours. After centrifugation and decantation, the solid was vacuum dried to obtain metal-organic framework 10 (97.2 mg). EXAMPLES

[0088] The same procedure as in Example 10 was carried out except that the heating temperature was 120° C. instead of 90° C., to obtain metal organic framework 11 (72.6 mg). EXAMPLES

[0089] The same procedure as in Example 10 was performed except that DEF was used instead of DMF, to obtain metal organic structure 12 (78.3 mg). EXAMPLES

[0090] The same procedure as in Example 11 was performed except that DEF was used instead of DMF, to obtain metal organic structure 13 (92.8 mg).

[0091] [Reference example 1] Preparation of 4,4',4'',4''',4'''',4'''''-(9,10-dibromo-9,10-dihydro-9,10-[1,2]benzenoanthracene-2,3,6,7,14,15-hexyl)hexabenzoic acid (hereinafter referred to as "organic ligand 2").

[0092] (Step 1) Synthesis of 2,3,6,7,9,10,14,15-octabromo-9,10-dihydro-9,10[1',2']-benzenoanthracene 9,10-Dibromo-9,10-dihydro-9,10[1',2']-benzenoanthracene (0.504g), iron powder (80.6mg), and 1,2-dichloroethane (6mL) were added to a two-neck flask, and a mixed solution of bromine (0.37mL) and 1,2-dichloroethane (6mL) was slowly added dropwise thereto. After stirring at 80°C for 1 hour, the mixture was returned to room temperature, quenched with an aqueous solution of sodium thiosulfate, and then filtered with suction to obtain 2,3,6,7,9,10,14,15-octabromo-9,10-dihydro-9,10[1',2']-benzenoanthracene (0.574g) as an off-white solid.

[0093] (Step 2) Synthesis of organic ligand 2 2,3,6,7,9,10,14,15-Octabromo-9,10-dihydro-9,10[1',2']-benzenoanthracene (0.502 g) obtained in step 1, cesium carbonate (3.91 g), 4-methoxycarbonylphenylboronic acid (2.13 g), and tetrakis(triphenylphosphine)palladium (0.233 g) were added to a Schlenk, followed by THF (50 mL). After heating and refluxing with stirring for 2 days, the mixture was returned to room temperature and the solvent was distilled off under reduced pressure. After extraction with dichloromethane, the mixture was dehydrated with anhydrous magnesium sulfate, naturally filtered, and the solvent was distilled off under reduced pressure using a rotary evaporator. The mixture was purified by silica gel column chromatography to obtain a solid. The obtained solid was dissolved in ethyl acetate, and then hexane was added to precipitate the solid. The obtained solid was transferred to a recovery flask, potassium hydroxide (0.933 g) was added thereto, and a mixed solvent of methanol / THF / water (1:1:1, total 150 mL) was added, and the mixture was heated under reflux while stirring overnight. After returning the mixture to room temperature, concentrated hydrochloric acid was added, and the organic solvent was distilled off under reduced pressure. The precipitated solid was filtered by suction to obtain organic ligand 2 (0.168 g) as a colorless solid. EXAMPLES

[0094] Zinc nitrate hexahydrate (66.7 mg) and the organic ligand 2 (41.3 mg) obtained in Reference Example 1 were dissolved in DMF (0.71 mL). After stirring at room temperature for 10 minutes and filtration, the solution was placed in a screw-cap vial, sealed, and heated at 90°C for 48 hours. The solution was cooled to room temperature, DMF was added, centrifuged, and decanted. Chloroform was added, centrifuged, decanted, and then immersed in chloroform for 24 hours. After centrifugation and decantation, the solid was vacuum-dried to obtain metal-organic framework 14 (26.0 mg). EXAMPLES

[0095] The same procedure as in Example 14 was carried out except that the heating temperature was 120° C. instead of 90° C. and the heating time was 24 hours, to obtain metal organic framework 15 (30.9 mg). EXAMPLES

[0096] The same procedure as in Example 14 was carried out except that DEF was used instead of DMF, thereby obtaining metal organic structure 16 (29.9 mg). EXAMPLES

[0097] The same procedure as in Example 15 was performed except that DEF was used instead of DMF, to obtain metal organic structure 17 (24.0 mg). EXAMPLES

[0098] Organic ligand 2 (90.6 mg, 0.080 mmol), zirconium tetrachloride (111.9 mg, 0.48 mmol), DMF (6.3 mL), water (0.1 ml, 72 eq.), and acetic acid (0.87 g, 180 eq.) were placed in a screw-cap vial and subjected to ultrasonic treatment. The vial was then sealed and heated at 120°C for 24 hours. The vial was cooled to room temperature, centrifuged, and decanted to obtain a solid. The operation of adding DMF to the solid, centrifuging, and decanting was repeated three times. The solvent was changed to acetone, and the same operation was repeated three times. After washing the solid, it was immersed in acetone for 24 hours. After centrifugation and decantation, the solid was vacuum-dried at 150°C for about 6 hours to obtain metal-organic framework 18 (131.3 mg).

[0099] (Reference example 2) Synthesis of 4,4',4'',4''',4'''',4'''''-((9,10-dihydro-9,10-[1,2]benzenoanthracene-2,3,6,7,14,15-hexyl)hexakis(ethyne-2,1-diyl))hexabenzoic acid (hereinafter referred to as "organic ligand 3").

[0100] [ka]

[0101] (Step 1) Synthesis of hexamethyl 4,4',4'',4''',4'''',4''''-((9,10-dihydro-9,10-[1,2]benzenoanthracene-2,3,6,7,14,15-hexyl)hexakis(ethyne-2,1-diyl))hexabenzoate 2,3,6,7,14,15-Hexabromo-9,10-dihydro-9,10-[1,2]benzenoanthracene (0.737g, 1.01mmol), CuI (43.0mg, 0.226mmol), PdCl2(PPh3)2 (98.6mg, 0.104mmol), PPh3 (53.5mg, 0.204mmol), methyl 4-ethynylbenzoate (1.30g, 8.14mmol) were added to a 100mL Schlenk, and 22mL of degassed triethylamine was added. After heating and refluxing for 2 days with stirring, the solvent was distilled off under reduced pressure. The mixture was dissolved in dichloromethane and washed with a saturated aqueous sodium chloride solution, and the organic layer was dehydrated with magnesium sulfate, filtered, and the solvent was distilled off under reduced pressure using a rotary evaporator. After purification using silica gel column chromatography (dichloromethane to ethyl acetate), the solvent was removed under reduced pressure using a rotary evaporator to obtain a solid. The solid was reprecipitated with ethyl acetate and hexane, and suction filtered to obtain 4,4',4'',4'',4'',4'',4'''',4'''''-((9,10-dihydro-9,10-[1,2]benzenoanthracene-2,3,6,7,14,15-hexyl)hexakis(ethyne-2,1-diyl))hexamethyl hexabenzoate as a brown solid (0.504 g, 0.419 mmol) (yield 41.5%).

[0102] (Step 2) Synthesis of organic ligand 3 In a 300 mL recovery flask, hexamethyl 4,4',4'',4''',4'',4'''',4'''''-((9,10-dihydro-9,10-[1,2]benzenoanthracene-2,3,6,7,14,15-hexyl)hexakis(ethyne-2,1-diyl))hexabenzoate (0.413 g, 0.343 mmol) and potassium hydroxide (1.58 g, 28.1 mmol) were added, and a mixed solvent of MeOH, THF, and HO (1:1:1; total 150 mL) was added and the mixture was heated to reflux overnight with stirring. After returning to room temperature, concentrated hydrochloric acid was added, and the organic solvent was distilled off under reduced pressure. The precipitated solid was filtered by suction to obtain organic ligand 3 as a brown solid (0.291 g, 0.260 mmol) (yield 75.8%).

[0103] (Reference example 3) Synthesis of 4,4',4'',4''',4'''',4'''''-((9,10-dibromo-9,10-dihydro-9,10-[1,2]benzenoanthracene-2,3,6,7,14,15-hexyl)hexakis(ethyne-2,1-diyl))hexabenzoic acid (hereinafter referred to as "organic ligand 4").

[0104] [ka]

[0105] (Step 1) Synthesis of hexamethyl 4,4',4'',4''',4'''',4''''-((9,10-dibromo-9,10-dihydro-9,10-[1,2]benzenoanthracene-2,3,6,7,14,15-hexyl)hexakis(ethyne-2,1-diyl))hexabenzoate 2,3,6,7,9,10,14,15-Octabromo-9,10-dihydro-9,10-[1,2]benzenoanthracene (0.917g, 1.04mmol), CuI (41.5mg, 0.278mmol), PdCl2(PPh3)2 (74.5mg, 0.106mmol), PPh3 (57.3mg, 0.204mmol), methyl 4-ethynylbenzoate (1.30g, 8.10mmol) were added to a 100mL Schlenk, and 22mL of degassed triethylamine was added. After heating and refluxing with stirring for 2 days, the solvent was distilled off under reduced pressure. The mixture was dissolved in dichloromethane and washed with a saturated aqueous sodium chloride solution, and the organic layer was dehydrated with magnesium sulfate, filtered, and the solvent was distilled off under reduced pressure using a rotary evaporator. After purification using silica gel column chromatography (dichloromethane to ethyl acetate), the solvent was removed under reduced pressure using a rotary evaporator to obtain a solid. The resulting solid was reprecipitated with ethyl acetate and hexane, and suction filtered to obtain 4,4',4'',4'',4'',4'',4'''',4'''''-((9,10-dibromo-9,10-dihydro-9,10-[1,2]benzenoanthracene-2,3,6,7,14,15-hexyl)hexakis(ethyne-2,1-diyl))hexamethyl hexabenzoate as a brown solid (1.19 g, 0.847 mmol) (yield 84.0%).

[0106] (Step 2) Synthesis of organic ligand 4 In a 300 mL recovery flask, hexamethyl 4,4',4'',4''',4'',4'''',4'''''-((9,10-dibromo-9,10-dihydro-9,10-[1,2]benzenoanthracene-2,3,6,7,14,15-hexyl)hexakis(ethyne-2,1-diyl))hexabenzoate (0.899 g, 0.660 mmol) and potassium hydroxide (0.767 g, 11.7 mmol) were added, and a mixed solvent of MeOH, THF, and HO (1:1:1; total 150 mL) was added and the mixture was heated to reflux overnight with stirring. After returning to room temperature, concentrated hydrochloric acid was added, and the organic solvent was distilled off under reduced pressure. The precipitated solid was filtered by suction to obtain organic ligand 4 as a brown solid (0.767 g, 0.600 mmol) (yield 90.9%).

[0107] (Reference example 4) 9,10-Dibromo-9,10-dihydro-9,10-[1,2]benzenoanthracene-2,3,6,7,14,15-hexa Synthesis of aryl carboxylic acid (hereinafter referred to as "organic ligand 5")

[0108] [ka]

[0109] (Step 1) Synthesis of 9,10-dibromo-2,3,6,7,14,15-hexamethyl-9,10-dihydro-9,10-[1,2]benzenoanthracene 2,3,6,7,9,10,14,15-Octabromo-9,10-dihydro-9,10-[1,2]benzenoanthracene (114 mg, 0.128 mmol), PdCl2(PPh3)2 (42.6 mg, 0.0608 mmol) were added to a 100 mL Schlenk, and 15 mL of dehydrated THF was added. After stirring at 60 ° C for 30 minutes, 1.09 M trimethylaluminum hexane solution (1.8 mL, 2.0 mmol) was added and heated to reflux for 18 hours while stirring. After cooling to 0 ° C, the reaction was stopped with 1 M aqueous hydrogen chloride solution. After extraction with chloroform and washing with saturated aqueous sodium chloride solution, the organic layer was dehydrated with magnesium sulfate, filtered, and the solvent was distilled under reduced pressure using a rotary evaporator. After purification using silica gel column chromatography (dichloromethane), the solvent was removed under reduced pressure using a rotary evaporator to obtain a solid. The solid was washed with methanol and suction filtered to obtain 9,10-dibromo-2,3,6,7,14,15-hexamethyl-9,10-dihydro-9,10-[1,2]benzenoanthracene as a colorless solid (42.4 mg, 0.0854) (yield 66.7%).

[0110] (Step 2) Synthesis of organic ligand 5 9,10-Dibromo-2,3,6,7,14,15-hexamethyl-9,10-dihydro-9,10-[1,2]benzenoanthracene (1.12 g, 2.26 mmol), potassium permanganate (19.0 g, 120 mmol), pyridine 5 mL, and water 5 mL were added to a 50 mL two-neck flask, and the mixture was heated to reflux for 24 hours while stirring. The mixture was returned to room temperature, filtered through Celite, and the residue was washed with hot water, and concentrated hydrochloric acid was added to the filtrate until it became acidic. After extraction with ethyl acetate and washing with a saturated aqueous sodium chloride solution, the organic layer was dehydrated with magnesium sulfate, filtered, and the solvent was distilled off under reduced pressure using a rotary evaporator to obtain organic ligand 5 as a colorless solid (575 mg, 0.851 mmol) (yield 37.7%). EXAMPLES

[0111] Zinc nitrate hexahydrate (98.8 mg) and organic ligand 3 (60.9 mg) were dissolved in DMF (1.11 mL). After stirring at room temperature for 10 minutes and filtration, the solution was placed in a screw-cap vial, sealed, and heated at 90°C for 48 hours. After cooling to room temperature, DMF was added, centrifuged, and decanted. Chloroform was added, centrifuged, decanted, and then immersed in chloroform for 24 hours. After centrifugation and decantation, the solid was vacuum dried to obtain metal-organic framework 19 (36.0 mg). EXAMPLES

[0112] The same procedure as in Example 19 was carried out except that the heating temperature was 120° C. instead of 90° C. and the heating time was 24 hours, to obtain metal organic structure 20 (38.7 mg). EXAMPLES

[0113] The same procedure as in Example 19 was carried out except that DEF was used instead of DMF, to obtain metal organic structure 21 (46.1 mg). EXAMPLES

[0114] The same procedure as in Example 20 was performed except that DEF was used instead of DMF, to obtain metal organic structure 22 (66.1 mg). EXAMPLES

[0115] Zinc nitrate hexahydrate (143 mg) and organic ligand 4 (100 mg) were dissolved in DMF (1.6 mL). After stirring at room temperature for 10 minutes and filtration, the solution was placed in a screw-cap vial, sealed, and heated at 90°C for 24 hours. After cooling to room temperature, DMF was added, centrifuged, and decanted. Chloroform was added, centrifuged, decanted, and then immersed in chloroform for 24 hours. After centrifugation and decantation, the solid was vacuum-dried to obtain metal-organic framework 23 (101 mg). EXAMPLES

[0116] The same procedure as in Example 23 was carried out except that the heating temperature was 120° C. instead of 90° C., to obtain metal organic structure 24 (103 mg). EXAMPLES

[0117] The same procedure as in Example 23 was performed except that DEF was used instead of DMF, to obtain metal organic structure 25 (79.4 mg). EXAMPLES

[0118] The same procedure as in Example 24 was carried out except that DEF was used instead of DMF, to obtain metal organic structure 26 (125 mg). EXAMPLES

[0119] Zinc nitrate hexahydrate (266 mg) and organic ligand 5 (100 mg) were dissolved in DMF (3.0 mL). After stirring at room temperature for 10 minutes and filtration, the solution was placed in a screw-cap vial, sealed, and heated at 90°C for 24 hours. After cooling to room temperature, DMF was added, centrifuged, and decanted. Chloroform was added, centrifuged, decanted, and then immersed in chloroform for 24 hours. After centrifugation and decantation, the solid was vacuum dried to obtain metal-organic framework 27 (59.2 mg). EXAMPLES

[0120] The same procedure as in Example 27 was carried out except that the heating temperature was 120° C. instead of 90° C., to obtain metal organic structure 28 (82.6 mg). EXAMPLES

[0121] The same procedure as in Example 27 was carried out except that DEF was used instead of DMF, to obtain metal organic structure 29 (73.1 mg). EXAMPLES

[0122] The same procedure as in Example 28 was carried out except that DEF was used instead of DMF, to obtain metal organic structure 30 (80.9 mg). EXAMPLES

[0123] The same procedure as in Example 18 was carried out except that the organic ligand 5 was used instead of the organic ligand 2, to obtain metal organic structure 31 (78.3 mg). EXAMPLES

[0124] Zinc nitrate hexahydrate (105 mg) and 9,10-dihydro-9,10-[1,2]benzenoanthracene-2,3,6,7,14,15-hexacarboxylic acid (hereinafter referred to as "organic ligand 6") (93.1 mg) were dissolved in DMF (1.2 mL). After stirring at room temperature for 10 minutes and filtration, the solution was placed in a screw-cap vial, sealed, and heated at 90°C for 24 hours. After cooling to room temperature, DMF was added, centrifuged, and decanted. Chloroform was added, centrifuged, decanted, and then immersed in chloroform for 24 hours. After centrifugation and decantation, the solid was vacuum dried to obtain metal-organic framework 32 (27.6 mg). EXAMPLES

[0125] The same procedure as in Example 32 was carried out except that the heating temperature was 120° C. instead of 90° C., to obtain metal organic structure 33 (35.0 mg). EXAMPLES

[0126] The same procedure as in Example 32 was carried out except that DEF was used instead of DMF, to obtain metal organic structure 34 (30.7 mg). EXAMPLES

[0127] The same procedure as in Example 33 was carried out except that DEF was used instead of DMF, to obtain metal organic structure 35 (33.2 mg). EXAMPLES

[0128] The same procedure as in Example 18 was carried out except that the organic ligand 2 was replaced with the organic ligand 6, thereby obtaining metal organic structure 36 (94.1 mg).

[0129] (Reference example 5) Synthesis of 4,4',4'',4''',4'''',4'''''-(9,10-dimethyl-9,10-dihydro-9,10-[1,2]benzenoanthracene-2,3,6,7,14,15-hexayl)hexabenzoic acid (hereinafter referred to as "organic ligand 7").

[0130] [ka] TIFF0007555914000026.tif32133

[0131] (Step 1) Synthesis of 9,10-dimethyl-2,3,6,7,14,15-hexabromo-9,10-dihydro-9,10[1',2']-benzenoanthracene Bromine (8.3mL, 25.6g, 160mmol) was added dropwise to a 1,2-dichloroethane solution (270mL) of 9,10-dimethyltriptycene (7.48g, 26.6mmol) and iron powder (608mg). After heating and stirring for 10 hours, the mixture was returned to room temperature and the reaction was quenched with an aqueous solution of sodium thiosulfate. The mixture was extracted with dichloromethane, the organic layer was dried over anhydrous magnesium sulfate, filtered and the solvent was distilled off under reduced pressure. The resulting solid was washed with dichloromethane and filtered to obtain the target product (20.1g, 26.6mmol, quant.) as an off-white solid.

[0132] (Step 2) Synthesis of organic ligand 7 In a nitrogen atmosphere, 9,10-dimethyl-2,3,6,7,14,15-hexabromo-9,10-dihydro-9,10-[1',2']-benzenoanthracene (0.502g, 0.566mmol), cesium carbonate (3.91g, 12.0mmol), tetrakistriphenylphosphinepalladium (0.233g, 0.201mmol), 4-methoxycarbonylphenylboronic acid (2.13g, 11.8mmol), and dehydrated THF (50mL) were added to a 100mL Schlenk tube, and the mixture was stirred for 2 days while being heated under reflux. After the solvent was removed under reduced pressure, dichloromethane was added and the organic layer was washed with water. After washing the organic layer with salt water, it was dehydrated with anhydrous magnesium sulfate and filtered. The solvent was removed under reduced pressure, and the mixture was purified by silica gel column chromatography (CH2Cl2→AcOEt), and the solvent was removed under reduced pressure. The obtained solid was mixed with KOH (0.933 g, 16.6 mmol), THF, MeOH, and HO (50 / 50 / 50, 150 mL) were added, and the mixture was heated under reflux with stirring for 18 hours. The mixture was returned to room temperature, concentrated hydrochloric acid was added, and the precipitated solid was filtered by suction to obtain the target product (0.168 g, 0.148 mmol, 26.1%) as a colorless solid.

[0133] (Reference Example 6) Synthesis of 9,10-dimethyl-9,10-dihydro-9,10-[1,2]benzenoanthracene-2,3,6,7,14,15-hexacarboxylic acid (hereinafter referred to as "organic ligand 8")

[0134] [ka] TIFF0007555914000028.tif27131

[0135] (Step 1) Synthesis of 2,3,6,7,9,10,14,15-octamethyl-9,10-dihydro-9,10-[1,2]benzenoanthracene A solution of 2,3,6,7,14,15-hexabromo-9,10-dimethyl-9,10-dihydro-9,10-[1,2]benzenoanthracene (0.854g, 1.13mmol) and PdCl2(PPh3)2 (333mg, 0.452mmol) in THF (50mL) was stirred at 60℃ for 30 minutes. 1.8M trimethylaluminum toluene solution (10.1mL, 18.1mmol) was added thereto, and the mixture was heated and refluxed for 18 hours while stirring. The temperature was lowered to 0℃, and the reaction was stopped with 1M hydrochloric acid. The organic layer was extracted with chloroform, and washed with salt water. The organic layer was dried over anhydrous magnesium sulfate, filtered, and the solvent was removed under reduced pressure. The solid obtained was purified by silica gel chromatography (CH2Cl2:Hexane=1:3), and the solvent was removed under reduced pressure. The mixture was washed with methanol and filtered under suction to obtain the desired product (0.190 g, 0.518 mmol, 45.8%) as a colorless solid.

[0136] (Step 2) Synthesis of organic ligand 8 2,3,6,7,9,10,14,15-Octamethyl-9,10-dihydro-9,10-[1,2]benzenoanthracene (0.154g, 0.420mmol) and potassium permanganate (1.17g, 7.40mmol) were mixed, and a mixed solvent of t-BuOH (2mL) and H2O (2mL) was added. The mixture was heated with stirring for one day. The mixture was filtered through Celite, and the residue was washed with hot water. The filtrate was mixed, and concentrated hydrochloric acid was added to the filtrate to precipitate a solid. The mixture was filtered by suction to obtain the target product (59.6mg, 0.109mmol, 26.6%) as a colorless solid. EXAMPLES

[0137] Organic ligand 7 (104 mg, 0.103 mmol) and zinc nitrate hexahydrate (176 mg, 0.592 mmol) were dissolved in DMF (2.0 mL). After stirring at room temperature for 10 minutes and filtration, the solution was placed in a screw-cap vial, sealed, and heated at 90°C for 24 hours. After cooling to room temperature, DMF was added, centrifuged, and decanted. Chloroform was added, centrifuged, decanted, and then immersed in chloroform for 24 hours. After centrifugation and decantation, the solid was vacuum-dried to obtain metal-organic framework 37 (76.2 mg). EXAMPLES

[0138] The same procedure as in Example 37 was carried out except that the heating temperature was 120° C. instead of 90° C., to obtain metal-organic structure 38 (78.6 mg) as white crystals. EXAMPLES

[0139] The same procedure as in Example 37 was performed except that DEF was used instead of DMF, to obtain metal-organic structure 39 (48.5 mg) as white crystals. EXAMPLES

[0140] The same procedure as in Example 38 was carried out except that DEF was used instead of DMF, to obtain metal organic structure 40 (64.1 mg). EXAMPLES

[0141] The same procedure as in Example 18 was carried out except that the organic ligand 7 was used instead of the organic ligand 2, and 70.5 mg (0.303 mmol, 3.7 eq.) of zirconium tetrachloride was used, to obtain a metal organic structure 41 (85.7 mg). EXAMPLES

[0142] Organic ligand 8 (52.7 mg, 0.0964 mmol) and zinc nitrate hexahydrate (165 mg, 0.554 mmol) were dissolved in DMF (1.8 mL). After stirring at room temperature for 10 minutes and filtration, the solution was placed in a screw-cap vial, sealed, and heated at 90°C for 24 hours. After cooling to room temperature, DMF was added, centrifuged, and decanted. Chloroform was added, centrifuged, decanted, and then immersed in chloroform for 24 hours. After centrifugation and decantation, the solid was vacuum-dried to obtain metal-organic framework 42 (8.0 mg) as a colorless solid. EXAMPLES

[0143] The same procedure as in Example 42 was carried out except that the heating temperature was 120° C. instead of 90° C., to obtain metal-organic structure 43 (13.2 mg) as a colorless solid. EXAMPLES

[0144] The same procedure as in Example 42 was carried out except that DEF was used instead of DMF, to obtain metal-organic structure 44 (2.8 mg) as a colorless solid. EXAMPLES

[0145] The same procedure as in Example 43 was carried out except that DEF was used instead of DMF, to obtain metal organic structure 45 (58.5 mg). EXAMPLES

[0146] The same procedure as in Example 18 was carried out except that organic ligand 8 was used instead of organic ligand 2, to obtain metal organic structure 46 (104.1 mg). EXAMPLES

[0147] Organic ligand 2 (113 mg, 0.10 mmol), chromium nitrate nonahydrate (131 mg, 0.33 mmol), and water (5 ml) were placed in an autoclave, sealed, and heated at 220°C for 24 hours. The mixture was cooled to room temperature, centrifuged, and decanted to obtain a solid. The procedure of adding water to the solid, centrifuging, and decanting was repeated three times. 20 mL of ethanol was added to the solid, and the mixture was heated to reflux for 4 hours. After returning to room temperature, the mixture was centrifuged and decanted to obtain a solid. The solid was vacuum-dried at 150°C for about 6 hours to obtain metal-organic framework 47 (41.1 mg). EXAMPLES

[0148] The same procedure as in Example 47 was carried out except that organic ligand 7 was used instead of organic ligand 2, to obtain metal organic structure 48 (72.9 mg). EXAMPLES

[0149] The same procedure as in Example 47 was carried out except that organic ligand 8 was used instead of organic ligand 2, to obtain metal organic structure 49 (27.6 mg). EXAMPLES

[0150] Organic ligand 2 (114 mg, 0.10 mmol), chromium chloride hexahydrate (80 mg, 0.30 mmol), and DMF (10 ml) were stirred for 10 minutes and then completely dissolved by ultrasonic irradiation. The solution was filtered, sealed in an autoclave, and heated at 190 ° C for 3 days. The solution was cooled to room temperature, centrifuged, and decanted to obtain a solid. The operation of adding DMF to the solid, centrifuging, and decanting was repeated three times. After adding DMF and immersing overnight, the solvent was replaced with chloroform, and the same operation of centrifugation and decantation was repeated three times. The obtained solid was immersed in chloroform for two days, centrifuged, and decanted to obtain a solid. The solid was vacuum dried at 150 ° C for about 6 hours to obtain metal organic framework 50 (49.5 mg). EXAMPLES

[0151] Organic ligand 2 (113 mg, 0.10 mmol), aluminum nitrate nonahydrate (113 mg, 0.30 mmol), and water (10 ml) were stirred for 10 minutes, then placed in an autoclave, sealed, and heated at 220 ° C. for 42 hours. The mixture was cooled to room temperature, centrifuged, and decanted to obtain a solid. The operation of adding water to the solid, centrifuging, and decanting was repeated three times. After washing with acetone, DMF was added and the mixture was immersed for three days. Then, the mixture was placed in a 100 ° C. oven and heated for three days. The mixture was returned to room temperature, centrifuged, and decanted to obtain a solid. The operation of adding DMF to the solid, centrifuging, and decanting was repeated twice, and the solvent was replaced with acetone, and centrifuged and decanted. The obtained solid was vacuum dried at 100 ° C. for about 6 hours to obtain metal-organic framework 51 (87.1 mg). EXAMPLES

[0152] The same procedure as in Example 50 was performed except that organic ligand 7 was used instead of organic ligand 2, to obtain metal-organic framework 52 (67.4 mg) as a green solid. EXAMPLES

[0153] The same procedure as in Example 50 was performed except that organic ligand 8 was used instead of organic ligand 2, to obtain metal-organic structure 53 (60.2 mg) as a pale green solid.

[0154] (Elemental analysis test) The metal organic frameworks obtained in Examples 1 and 5 to 9 were subjected to elemental analysis. The results are shown in Table 1.

[0155] [Table 1]

[0156] (IR spectrum measurement) The IR spectra were measured for organometallic structures 1 to 9, 14 to 17, 19 to 30, 32 to 35, 37, 40, and 45 obtained in Examples 1 to 9 and 14 to 33. Table 2 shows the peaks indicating the stretching vibration of the carbonyl group of each organometallic structure.

[0157] [Table 2]

[0158] (X-ray structural analysis) The metal organic framework 1 obtained in Example 1 was subjected to X-ray structural analysis under the measurement conditions shown below. [Measurement conditions] A single grain of colorless and transparent crystal of the metal-organic framework 1 obtained in Example 1, measuring 0.03×0.03×0.03 mm, was placed on a micromount and a diffraction experiment was performed using a single crystal X-ray analyzer (D8 VENTURE, manufactured by Bruker). The diffraction data obtained by irradiating the single crystal with X-rays having a wavelength of 0.78192 Å was analyzed to determine the structure. The results are shown in Table 3.

[0159] [Table 3]

[0160] (BET specific surface area measurement and hydrogen storage capacity measurement) The BET specific surface area and the hydrogen storage capacity at 77 K and atmospheric pressure were measured for the metal organic frameworks 1 to 37, 40, 41, 45 and 46 obtained in Examples 1 to 37, 40, 41, 45 and 46. In addition, the hydrogen storage capacity of the metal organic framework 1 was also measured at 298 K and 10 MPa. The BET specific surface area and hydrogen storage capacity at 77 K and atmospheric pressure were measured using a gas adsorption measurement device Tristar-II (Micromeritics), and the hydrogen storage capacity at 298 K and 10 MPa was measured using a gas adsorption measurement device PTC characteristic evaluation device (Suzuki Shokan Co., Ltd.).

[0161] The BET specific surface area was calculated by the following method. Approximately 50 mg of each of the metal organic frameworks 1 to 33 obtained in Examples 1 to 33 was placed in a glass cell. The inside of the glass cell was depressurized to a vacuum at a temperature of 135° C. and dried for 6 hours. The glass cell was attached to a gas adsorption measurement device and immersed in a thermostatic bath containing liquid nitrogen. The pressure of nitrogen injected into the glass cell was gradually increased. When the pressure of nitrogen introduced into the glass cell reached 1.0×10 5 The measurement was continued until the pressure reached 1 Pa. The amount of hydrogen stored at 77K and normal pressure was calculated as follows. After measuring nitrogen, the gas type was changed to hydrogen and measurements were performed. The pressure of hydrogen injected into the glass cell was gradually increased. When the pressure of hydrogen introduced into the glass cell reached 1.0×10 5 The measurement was continued until the pressure reached 1 Pa.

[0162] The hydrogen storage amount at 298K and 10MPa was calculated by the following method. 220mg of the metal organic framework 1 obtained in Example 1 was placed inside a stainless steel sample cell. Next, the temperature inside the cell was set to 135°C, the pressure was reduced to vacuum, and the state was maintained for 65 hours. In this way, the gas and solvent contained inside the metal organic framework 1 were removed. The cell was immersed in a thermostatic bath at 298K, and in this state, the pressure of hydrogen injected into the cell was gradually increased using a gas adsorption amount measuring device. After the internal hydrogen pressure reached 10MPa, the pressure of hydrogen contained in the cell was gradually reduced. The results of the measurements performed as described above are shown in Table 4.

[0163] [Table 4]

[0164] [Table 5]

[0165] Regarding the metal organic framework 1 obtained in Example 1, the nitrogen adsorption isotherm (77 K) is shown in FIG. 1, and the hydrogen adsorption isotherm (77 K) is shown in FIG.

[0166] For the metal organic frameworks 1, 14 to 16, 37, 40 and 45 obtained in Examples 1, 14 to 16, 37, 40 and 45, the adsorption amounts of carbon dioxide and the heats of carbon dioxide adsorption were measured at 273 K and 298 K under atmospheric pressure. The carbon dioxide adsorption amount was measured using a gas adsorption amount measuring device Tristar-II (manufactured by Micromeritics) as follows. Approximately 50 mg of the metal organic frameworks 1, 14 to 16, 37, 40 and 45 obtained in Examples 1, 14 to 16, 37, 40 and 45 were placed in a glass cell. The inside of the glass cell was depressurized to a vacuum at a temperature of 135°C and dried for 6 hours. The glass cell was attached to a gas adsorption measurement device and immersed in a thermostatic bath at 273K or 298K. The pressure of carbon dioxide injected into the glass cell was gradually increased. When the pressure of carbon dioxide introduced into the glass cell reached 1.0×10 5 The measurement was continued until the pressure reached 1 Pa. The results are shown in Table 5.

[0167] [Table 6] [Industrial Applicability]

[0168] The metal organic framework of the present invention can adsorb hydrogen and carbon dioxide at a practical level, which will facilitate the use of hydrogen toward the advent of a hydrogen society and reduce carbon dioxide in the atmosphere.

Claims

1. A polyvalent metal ion and a compound represented by the formula [I] 【Chemistry 1】 [In formula [I], X 1 ~X 3 represents the formula [V-1] or the formula [V-2′], 【Chemistry 2】 (In formula [V-2'], Z 1 represents a single bond, -C≡C-, -O-, -S-, -S(O)-, -SO 2 - or -C(═O)-. R 31 represents a C1-6 alkyl group, a C3-8 cycloalkyl group, a C6-10 aryl group, a 3- to 6-membered heterocyclyl group, a C1-6 alkoxy group, a C6-10 aryloxy group, a heteroaryloxy group, a halogeno group, a C1-6 haloalkyl group, a C6-10 haloaryl group, a C1-6 haloalkoxy group, a C1-6 alkylthio group, a C6-10 arylthio group, a heteroarylthio group, a C1-6 alkylsulfinyl group, a C6-10 arylsulfinyl group, a heteroarylsulfinyl group, a C1-6 alkylsulfonyl group, a C6-10 arylsulfonyl group, a heteroarylsulfonyl group, a cyano group, a nitro group, or a group represented by formula [VI].) 【Chemistry 3】 (In formula [VI], R 41 and R 42 each independently represent a hydrogen atom, a C1-6 alkyl group, a C6-10 aryl group, a C1-6 alkylcarbonyl group, or a C6-10 arylcarbonyl group.) n represents the number of R 31 and is 0, 1, 2, 3 or 4, and when n is 2 or more, a plurality of R 31 may be the same or different from each other; a is X 1 and is 2, a1 represents the number of R 1 and is 0, b is X 2 and is 2; b1 represents the number of R 2 and is 0, c is X 3 and is 2, c1 represents the number of R 3 and is 0. Y1, Y 2 each independently represents a hydrogen atom, a halogeno group, a C1-6 alkyl group, or a C1-6 alkoxy group. However, when the polyvalent metal ion is a trivalent metal ion, Y 1 , Y 2 each independently represents a halogeno group, a C1-6 alkyl group, or a C1-6 alkoxy group. The metal organic framework contains a carboxylate ion represented by the formula:

2. The metal organic framework according to claim 1, wherein the polyvalent metal ion is an ion of at least one metal selected from the group consisting of metals of groups 2 to 13 of the periodic table of the elements.

3. 3. The metal organic structure according to claim 1, wherein the polyvalent metal ion is an ion of at least one metal selected from the group consisting of Zn, Fe, Co, Ni, Cu, Zr, and Mg.

4. The metal organic structure according to any one of claims 1 to 3, further comprising an organic ligand other than the carboxylate ion represented by formula [I] as a constituent component.

5. A gas storage method comprising the steps of contacting a gas with the metal-organic framework according to any one of claims 1 to 4 and adsorbing the gas inside the metal-organic framework.

Citation Information

Patent Citations

  • Porous coordination polymer, and gas occlusion method and gas occlusion device using the same

    JP2018058814A

  • Organometallic skeleton compounds on the basis of triptycene

    WO2009098001A1