How neodymium iron boron magnets are manufactured

The described method for manufacturing neodymium iron boron magnets with controlled impurities and reduced grain size addresses the limitations of conventional methods, resulting in magnets with improved coercive force and uniformity.

JP7556038B2Active Publication Date: 2024-09-25YANTAI ZHENGHAI MAGNETIC MATERIAL CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2022547759
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-04-30
Filing Date
2021-04-29
Publication Date
2024-09-25
Estimated Expiration
2041-04-29

AI Technical Summary

Technical Problem

Conventional methods for improving the coercive force of neodymium iron boron magnets face limitations, particularly when grain sizes are reduced below 5 μm, as impurities such as C, O, and N adversely affect the magnet's structure and coercive force, and existing technologies do not effectively control these impurities.

Method used

A manufacturing method for neodymium iron boron sintered magnets involving a chemical composition of RFeBM, where R is a rare earth element, with controlled contents of C, O, and N, and a production process that includes stripping-hydrogen explosion, jet milling, low-temperature sintering with argon-hydrogen mixed gas, and tempering to achieve crystal grains of 5 μm or less.

Benefits of technology

The method results in neodymium iron boron magnets with enhanced coercive force and reduced impurity content, achieving high coercive force without heavy rare earths and maintaining uniform performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007556038000005
    Figure 0007556038000005
  • Figure 0007556038000006
    Figure 0007556038000006
  • Figure 0007556038000001
    Figure 0007556038000001
Patent Text Reader

Abstract

This article describes a neodymium-iron-boron-based sintered magnet with fine crystallinity and high coercivity, and a method for producing the same. The neodymium-iron-boron magnet has the chemical formula RFeBM, where R is a rare earth element, Fe is iron, and B is boron. The R content is 26-35 wt%, the B content is 0.8-1.3 wt%, and M is one of Co, Ga, Cu, Al, Zr, and Ti. The neodymium-iron-boron-based sintered magnet has a small grain size. As the grain size is reduced, the contents of the elements C, O, and N in the magnet are controlled, thereby significantly improving the magnet's coercivity. Magnets produced by this method have lower impurity contents of C, O, and N. Diffusion treatment of such products can provide better grain boundaries and diffusion paths. Therefore, re-diffusion of the fine-crystal product can produce magnets with higher performance.
Need to check novelty before this filing date? Find Prior Art

Description

Detailed Description of the Invention

[0001] This application claims priority to a prior application, bearing application number 202010367655.8, filed with the State Intellectual Property Office of China on April 30, 2020, for the invention entitled "Fine-crystal, high coercivity neodymium-iron-boron sintered magnet and its manufacturing method," the entire text of which is incorporated herein by reference.

[0002] [Technical field] The present invention relates to the field of neodymium-iron-boron based sintered magnets, and more particularly to fine crystal, high coercive force neodymium-iron-boron based sintered magnets and methods for producing the same.

[0003] [Background technology] Since its discovery, NdFeB permanent magnet material has been widely applied in the fields of communication, medicine, automobiles and electronics due to its excellent magnetic properties and high cost-effectiveness, but its relatively low coercive force and relatively poor temperature stability and corrosion resistance have seriously limited the expansion of its application range.

[0004] At present, the conventional technology generally uses the following four methods to improve the coercivity of NdFeB permanent magnet materials: (1) adding heavy rare earth to the raw alloy to improve the crystal magnetic anisotropy of the main phase; (2) a two-alloy method in which two types of alloy powder with different coercivity are mixed and sintered; (3) a method of refining crystal grains, in which as the crystal grain size becomes smaller, the effective scattering magnetic field factor of the crystal grains becomes smaller, and the coercivity of the magnet increases; and (4) a grain boundary diffusion method, in which the heavy rare earth diffuses along the grain boundary phase, significantly improving the anisotropy constant at the grain boundary, and achieving an obvious improvement in the magnet coercivity when a small amount of heavy rare earth is used. Among these methods, method (3) is relatively superior. Compared with methods (1) and (2), this method can greatly improve the magnet coercivity without using heavy rare earth or by using a small amount of heavy rare earth, while ensuring that the remanence remains unchanged. Compared to method (4), this improves magnet performance without being affected by product size, and ensures uniform performance both inside and outside the magnet.

[0005] The prior art further discloses a method for controlling the grain size of magnets by hot isostatic sintering using high pressure argon. First, a magnetic powder with an average grain size of 3 μm is produced, and a sintered magnet with a grain size of 5.2 μm and a density of 99.5% is finally produced by this method. The prior art further discloses that a sintered magnet is produced using magnetic powder with an average grain size of 2-5 μm, in which the heavy rare earth content is less than 0.2%, and the squareness of the product is 0.95 or more. The prior art further discloses that a 47H magnet with a grain size of about 5 μm is obtained by low-temperature sintering, and the coercive force of the magnet reaches 17 kOe in the absence of heavy rare earth.

[0006] As described above, various methods have been used to manufacture magnets with a crystal grain size of 5-6 μm, and it has been disclosed that the fineness of the crystal grains can improve the coercive force of the magnet. In the absence of heavy rare earths, the product performance can reach 47 H. In order to further improve the product performance under conditions without heavy rare earths, it is necessary to reduce the crystal grain size to 5 μm or less.

[0007] The prior literature further discloses a fine-crystal neodymium iron boron magnet with a median grain size of 4.5 μm or less in a cross section perpendicular to the c-axis. By reducing the grain size of the magnet, the coercive force of the magnet is improved. The prior literature further discloses that by refining the scale-like columnar crystals, a magnet with a grain size of 0.5 to 5.0 μm is produced, thereby reducing the amount of heavy rare earth used.

[0008] As mentioned above, the size of the scale-like columnar crystals is controlled to refine the grain size of the magnetic powder, and finally, a NdFeB magnet is produced with a magnet crystal grain smaller than 5 μm, thereby further improving the coercive force of the product. However, the performance improvement mentioned therein has a limit. This is mainly because as the crystal grain becomes smaller than 5 μm, the activity of the corresponding powder becomes stronger, and the contents of the elements C, O, and N in the final magnet gradually increase. The elements C, O, and N consume the rare earth elements in the grain boundary as impurities, and also act as nucleation sites for reverse magnetization domains, affecting the structure of the grain boundary and reducing the coercive force of the magnet.

[0009] Therefore, unless the impurity elements C, O, and N in magnets are controlled, as the particle size of the magnetic powder decreases, the magnet's crystal grains will become smaller and the magnet's coercivity will tend to rise and then fall. Prior literature does not mention the control or method of controlling the elements C, O, and N in products when the magnet's crystal grains become smaller, especially when they are smaller than 5 μm.

[0010] Summary of the Invention In order to remedy the shortcomings of the prior art, the present invention provides a fine-crystal, high-coercivity NdFeB-based sintered magnet and a manufacturing method thereof, in which the grain size of the NdFeB-based sintered magnet is 5 μm or less, and the contents of the elements C, O, and N in the NdFeB-based sintered magnet can be well controlled while reducing the grain size, thereby greatly improving the coercivity of the NdFeB-based sintered magnet.

[0011] The object of the present invention is achieved by the following technical solutions.

[0012] The neodymium iron boron magnet has the chemical formula RFeBM, in which R is a rare earth element, Fe is iron, B is boron, the R content is 26-35 wt%, the B content is 0.8-1.3 wt%, and M is multiple elements selected from Co, Ga, Cu, Al, Zr, and Ti, in which the Co content is 0.5-3.0 wt%, the Ga content is 0.05-0.4 wt%, the Cu content is 0.05-0.5 wt%, the Al content is 0-1.5 wt%, the Zr or Ti content is 0-0.3 wt%, and the remainder is iron and unavoidable impurities, and the contents of the elements C, O, and N in the magnet satisfy C+O+N(ppm)≦[1500+(5.0-crystal grain size(μm))×600](ppm).

[0013] According to the present invention, the content of R is, for example, 26 wt%, 27 wt%, 28 wt%, 29 wt%, 30 wt%, 31 wt%, 32 wt%, 33 wt%, 34 wt%, or 35 wt%.

[0014] According to the present invention, the content of B is, for example, 0.8 wt%, 0.9 wt%, 1 wt%, 1.1 wt%, 1.2 wt%, or 1.3 wt%.

[0015] According to the present invention, the Co content is, for example, 0.5 wt%, 0.8 wt%, 1 wt%, 1.2 wt%, 1.5 wt%, 2 wt%, 2.5 wt%, or 3.0 wt%.

[0016] According to the present invention, the Ga content is, for example, 0.05 wt%, 0.1 wt%, 0.2 wt%, 0.3 wt%, or 0.4 wt%.

[0017] According to the present invention, the Cu content is, for example, 0.05 wt%, 0.1 wt%, 0.2 wt%, 0.3 wt%, 0.4 wt% or 0.5 wt%.

[0018] According to the present invention, the Al content is, for example, 0.01 wt%, 0.05 wt%, 0.1 wt%, 0.2 wt%, 0.5 wt%, 1 wt%, 1.2 wt%, or 1.5 wt%.

[0019] According to the present invention, the Zr or Ti content is, for example, 0.01 wt%, 0.05 wt%, 0.1 wt%, 0.2 wt% or 0.3 wt%.

[0020] According to the invention, the rare earth elements are selected from lanthanum (La), cerium (Ce), praseodymium (Pr), neodymium (Nd), promethium (Pm), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), lutetium (Lu), yttrium (Y) and scandium (Sc).

[0021] According to the present invention, the crystal grain size of the neodymium iron boron magnet is 5 μm or less, for example, 4.8 μm, 4.5 μm, 4.3 μm, 4 μm, 3.8 μm, 3 μm, 2 μm or 1 μm.

[0022] The present invention further provides a method for producing the neodymium-iron-boron based sintered magnet, the method comprising the steps of: 1) obtaining R-Fe-BM alloy fine powder by stripping-hydrogen explosion method; 2) grinding the alloy fine powder of step 1) with a jet mill to obtain a magnetic powder having a particle size D50 of 4.0 μm or less, mixing the magnetic powder with a lubricant, and then pressing the magnetic powder into a green compact; 3) low-temperature sintering the green compact of step 2) at 500-900°C, injecting a mixed gas of argon and hydrogen at 10 kPa or less during the low-temperature sintering, maintaining the temperature for 0.1-2 h, evacuating to 100 Pa or less, and performing a circulation treatment at least once, followed by high-temperature sintering at 980-1040°C, maintaining the temperature for 3-8 h, cooling, and then performing a tempering treatment to produce the neodymium-iron-boron sintered magnet.

[0023] According to the present invention, in step 1), the stripping-hydrogen explosion method includes, for example, the following steps: The R-Fe-BM alloy is melted under vacuum or inert gas atmosphere at a temperature of 1200-1600°C, and the melt is poured into a quench roll with a rotation speed of 0.3-4 m / s to produce an R-Fe-BM alloy strip. The alloy strip is then subjected to hydrogen explosion treatment in a HD hydrogen explosion furnace, and the vacuum is drawn to a pressure lower than 100 Pa before the treatment.

[0024] Wherein, the thickness of the alloy strip is 0.1-0.5 mm.

[0025] According to the present invention, step 2) specifically includes the following steps: The alloy fine powder of step 1) is ground by a jet mill, in which the oxygen content in the jet mill process is less than 50 ppm.

[0026] According to the present invention, in step 2), the amount of the lubricant added is 0.1 to 0.5 wt % of the mass of the magnetic powder.

[0027] According to the present invention, in step 2), the mixing time is 0.1 to 3 hours, and the mixing temperature is room temperature.

[0028] According to the present invention, in step 2), the magnetic powder is pressed into a green compact with an oxygen content of less than 500 ppm in a magnetic orientation molding device with an orientation magnetic field strength of 1-2 T. The size and dimensions of the green compact are not particularly defined and can be adjusted according to the required amount of the final product.

[0029] According to the present invention, in step 3), the low-temperature sintering is carried out in a mixed atmosphere of argon and hydrogen, in which argon occupies 95-99 vol% of the total volume of the mixed atmosphere and hydrogen occupies 1-5 vol% of the total volume of the mixed atmosphere. By injecting the mixed atmosphere of argon and hydrogen into the low-temperature sintering process and performing a heat retention treatment within a specific temperature range, hydrogen is reacted with the lubricant in the magnet and the oxygen and nitrogen adsorbed on the surface of the magnetic powder through the gaps in the magnet, and the final reactant is discharged, reducing the contents of carbon, oxygen and nitrogen impurities in the magnet and improving product performance.

[0030] According to the present invention, in step 3), the temperature of the low-temperature sintering is 500°C, 600°C, 700°C, 800°C or 900°C. The temperature of the high-temperature sintering is 980°C, 990°C, 1000°C, 1010°C, 1020°C, 1030°C or 1040°C.

[0031] According to the present invention, the tempering treatment includes a primary tempering treatment and a secondary tempering treatment.

[0032] The temperature of the primary tempering treatment is 700 to 900°C (e.g., 700°C, 750°C, 800°C, 850°C, 900°C), and the time of the primary tempering treatment is 3 to 7 hours. The temperature of the secondary tempering treatment is 450 to 600°C (e.g., 450°C, 480°C, 500°C, 520°C, 550°C, 580°C, 600°C), and the time of the secondary tempering treatment is 3 to 7 hours.

[0033] According to the present invention, by employing the above-mentioned method, it is possible to obtain a NdFeB based sintered magnet having a crystal grain size of 5.0 μm or less, and the C+O+N content (ppm) in the NdFeB magnet satisfies the following relationship: ≦[1500+(5.0-crystal grain size (μm))×600](ppm).

[0034] BRIEF DESCRIPTION OF THE DRAWINGS FIG. 1 shows the particle size measurement results of the magnetic powder in Example 1.

[0035] [Figure 2] A photograph of a fracture surface of the magnet in Example 1 scanned by a scanning electron microscope.

[0036] [Mode for carrying out the invention] The present invention will be described in more detail with reference to the following specific examples. It should be understood that the following examples are merely illustrative and explanatory of the present invention and do not limit the scope of the claims of the present invention. Any technology realized based on the above content of the present invention is included in the scope of the claims of the present invention.

[0037] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods, and the reagents, materials, etc. used in the following examples are all commercially available, unless otherwise specified.

[0038] Instruments and Equipment The method for calculating the grain size in the present invention is as follows: using the fracture surface diagram of the green compact scanned by a scanning electron microscope, the number of grains in the fracture surface diagram is calculated, and then the average equivalent area of ​​the number of grains under the area of ​​the metal structure diagram is calculated, and the grain size is calculated according to the equivalent area.

[0039] The particle size D50 of the magnetic powder in the present invention is measured by a laser diffraction particle size distribution analyzer.

[0040] Example 1 (1) NdPr, Co, Al, Fe, Cu, Ga, Zr and ferroboron with a purity of at least 99% by weight are high-frequency melted in an argon atmosphere, and the melt is poured into a quench roll to produce an alloy with a mass percentage of 31% NdPr, 0.8% Co, 0.5% Al, 0.2% Cu, 0.15% Ga, 0.10% Zr, 0.96% B, and the rest being iron and unavoidable impurities. The alloy is hydrogenated and crushed into coarse powder, which is then polished by a jet mill, and the particle size D50 of the obtained magnetic powder is 3.5 μm. After adding 0.2 wt% lubricant to the jet mill powder, the material is mixed for 2 h and molded under the environment of room temperature and an orientation field with a magnetic field strength of 2 T.

[0041] (2) The green compact is placed in a vacuum sintering furnace, filled with 10 kPa of a mixed gas of argon and hydrogen with a volume ratio of 98:2 at 600°C, and kept at that temperature for 0.5 h. After the temperature is kept at 600°C, the vacuum is drawn to 0.1 kPa, the temperature is continued to rise, and the compact is sintered at 1030°C for 6 h. After the temperature is kept at 600°C, the compact is cooled and the first tempering process is performed at 900°C for 3 h. The second tempering process is performed at 520°C for 5 h. After cooling and removing from the furnace, a fine-crystalline neodymium iron boron magnet is obtained. This magnet is called A1, and a sample column (diameter 10 mm, length 10 mm) with a diameter of D10~10 mm is processed into the A1 magnet and a performance test is performed.

[0042] Comparative Example 1 The other steps are the same as in Example 1, except for step (2): The green compact is placed in a vacuum sintering furnace and sintered at 1030℃ for 6 h. After the heat retention, it is cooled and then the first tempering treatment is performed at 900℃ for 3 h. The second tempering treatment is performed at 520℃ for 5 h. After cooling and removing from the furnace, a fine-crystalline neodymium iron boron magnet is obtained. This magnet is called B1, and a sample column with a diameter of D10~10 mm is processed into the B1 magnet and a performance test is performed.

[0043] [Table 1]

[0044] As can be seen from Table 1, by using the method of the present invention, magnet A1 of Example 1 reaches a high coercivity level of 46H under the conditions of no heavy rare earths and a grain size of 4.5 μm. Example 1 has a comparable Br and a higher Hcj compared to Comparative Example 1, which is mainly due to the relatively good control of the impurity content (C+O+N) by the method of Example 1. Comparing the impurity contents of Example 1 and Comparative Example 1, Example 1<1500+(5.0-grain size)×600<Comparative Example 1.

[0045] Example 2 (1) NdPr, Dy, Co, Al, Fe, Cu, Ga, Ti and ferroboron with a purity of at least 99% by weight are high-frequency melted in an argon atmosphere, and the melt is poured into a quench roll to produce an alloy with a mass percentage of 32% NdPr, 0.3% Dy, 1.0% Co, 0.8% Al, 0.15% Cu, 0.15% Ga, 0.15% Ti, 0.98% B, and the rest being iron and unavoidable impurities. The alloy is hydrogenated and crushed into coarse powder, which is then polished by a jet mill, and the particle size D50 of the obtained magnetic powder is 3.2 μm. After adding 0.3 wt% lubricant to the jet mill powder, the material is mixed for 2 h and molded under the environment of room temperature and an orientation field with a magnetic field strength of 2 T.

[0046] (2) The compact is placed in a vacuum sintering furnace, filled with 8 kPa of argon and hydrogen mixed gas with a volume ratio of 99:1 at 650 ° C, and kept warm for 1 h. After the end of the warming, the vacuum is drawn to be lower than 100 Pa, the temperature is continued to be raised to 700 ° C, and the mixed gas of argon and hydrogen with a volume ratio of 99:1 is filled with 5 kPa of argon and hydrogen mixed gas with a volume ratio of 99:1, and kept warm for 0.5 h. After the end of the warming, the vacuum is drawn to 0.1 kPa, the temperature is continued to be raised, and sintered at 1020 ° C for 5.5 h. After the end of the warming, the compact is cooled and subjected to a primary tempering treatment at 850 ° C for 4 h. After the secondary tempering treatment at 550 ° C for 5 h. After cooling and removing from the furnace, a fine-crystalline neodymium iron boron magnet is obtained. This magnet is called A2, and a sample column with D10 ~ 10 mm is processed into the A2 magnet and a performance test is performed.

[0047] Comparative Example 2 The other steps are the same as in Example 2, except for step (2): The compact is placed in a vacuum sintering furnace and sintered at 1020℃ for 5.5 h. After the warming is completed, it is cooled and the first tempering is performed at 850℃ for 4 h. The second tempering is performed at 550℃ for 5 h. After cooling and removing from the furnace, a fine-crystalline neodymium iron boron magnet is obtained. This magnet is called B2, and a sample column with a diameter of D10~10 mm is processed into the B2 magnet for performance testing.

[0048] [Table 2]

[0049] As can be seen from Table 2, magnet A2 of Example 2 reaches a high coercivity of 42 SH level under low heavy rare earth conditions according to the method of the present invention. Example 2 has comparable Br and higher Hcj compared to Comparative Example 2, mainly due to the better control of the impurity content (C+O+N) by the method of Example 2. Comparing the impurity contents of Example 2 and Comparative Example 2, Example 2<1500+(5.0-grain size)×600<Comparative Example 2.

[0050] Example 3 (1) NdPr, Dy, Co, Al, Fe, Cu, Ga, Ti and ferroboron with a purity of at least 99% by weight are melted in an argon atmosphere by high frequency induction, and the melt is poured into a quench roll to produce an alloy with a mass percentage of 31.5% NdPr, 0.5% Dy, 1.0% Co, 0.6% Al, 0.2% Cu, 0.10% Ga, 0.2% Ti, 0.98% B, and the rest being iron and unavoidable impurities. The alloy is hydrogenated and pulverized into coarse powder, which is then polished by a jet mill, and the particle size D50 of the resulting magnetic powder is 2.6 μm. After adding 0.15 wt% lubricant to the jet mill powder, the material is mixed for 2 h and molded under the environment of room temperature and an orientation field with a magnetic field strength of 2 T.

[0051] (2) The compact is placed in a vacuum sintering furnace, filled with a mixed gas of argon and hydrogen with a volume ratio of 96:4 at 800 ° C, and kept at 6 kPa for 1 h. After the end of the heat retention, the furnace is evacuated to less than 100 Pa, and then filled with a mixed gas of argon and hydrogen with a volume ratio of 96:4 at 800 ° C, and kept at 6 kPa for 1 h. After the heat retention, the furnace is evacuated to 0.1 kPa and the temperature is increased, and the furnace is sintered at 1000 ° C for 7 h. After the heat retention, the furnace is cooled and the first tempering process is performed at 850 ° C, the time is 4 h. After the second tempering process is performed at 500 ° C, the time is 6 h. After cooling and removing from the furnace, a fine-crystalline neodymium iron boron magnet is obtained. This magnet is called A3, and a sample column with D10 to 10 mm is processed into the A3 magnet and a performance test is performed.

[0052] Comparative Example 3 The other steps are the same as in Example 3, except for step (2): The compact is placed in a vacuum sintering furnace and sintered at 1000°C for 7 h. After the heat retention is completed, it is cooled and the first tempering treatment is performed at 850°C for 4 h. The second tempering treatment is performed at 500°C for 6 h. After cooling and removing from the furnace, a fine-crystalline neodymium iron boron magnet is obtained. This magnet is called B3, and a sample column with a diameter of D10~10 mm is processed into the B3 magnet for performance testing.

[0053] [Table 3]

[0054] As can be seen from Table 3, Example 3 has comparable Br and higher Hcj compared to Comparative Example 3, which is mainly due to the impurity content (C+O+N) being better controlled by the method of Example 3. As the particle size of the magnetic powder becomes smaller, theoretically, the coercive force of the magnet in Comparative Example 3 increases, but the impurity content also increases rapidly, resulting in poor performance of the final product. Comparing the impurity content of Example 3 and Comparative Example 3, Example 3<1500+(5.0-crystal grain size)×600<Comparative Example 3.

[0055] Example 4 (1) Nd, Co, Al, Fe, Cu, Ga and ferroboron with a purity of at least 99% by weight are high-frequency melted in an argon atmosphere, and the melt is poured into a quench roll to produce an alloy with a mass percentage of 31% Nd, 0.8% Co, 0.3% Al, 0.2% Cu, 0.1% Ga, 1% B, and the rest being iron and unavoidable impurities. The alloy is hydrogenated and crushed into coarse powder, which is then polished by a jet mill, and the particle size D50 of the resulting magnetic powder is 3.5 μm. After adding 0.1 wt% lubricant to the jet mill powder, the materials are mixed for 2 h and molded under room temperature and an orientation field environment with a magnetic field strength of 2 T.

[0056] (2) The green compact is placed in a vacuum sintering furnace, filled with 10 kPa of a mixed gas of argon and hydrogen with a volume ratio of 99:1 at 600°C, and kept at this temperature for 0.5 h. After the temperature is kept at this temperature, the vacuum is pulled to 0 Pa, the temperature is continued to increase, and the compact is sintered at 1030°C for 6 h. After the temperature is kept at this temperature, the compact is cooled and then subjected to a primary tempering treatment at 900°C for 3 h. After the secondary tempering treatment at 510°C for 5 h, the compact is cooled and removed from the furnace to obtain a fine-grained neodymium iron boron magnet marked as substrate A4.

[0057] The magnet is processed into a square piece with a size of 20-10-5 mm. After degreasing and pickling, the square piece is subjected to Tb grain boundary diffusion treatment, and the diffusion amount of Tb is 0.4 wt%. The grain boundary diffusion in this embodiment is performed by selecting the thermal spraying method. The product after the diffusion treatment is called A5.

[0058] Comparative Example 4 The other steps are the same as in Example 4, except for step (2): The green compact is placed in a vacuum sintering furnace and sintered at 1030℃ for 6 h. After the heat is released, it is cooled and then subjected to the first tempering treatment at 900℃ for 3 h. The second tempering treatment is performed at 510℃ for 5 h. After cooling and removing from the furnace, a fine-grained NdFeB magnet is obtained, which is marked as Base material B4.

[0059] The magnet was processed into a square piece with a size of 20 - 10 - 5 mm. After degreasing and pickling, the square piece was subjected to a Tb grain boundary diffusion treatment, and the diffusion amount of Tb was 0.4 wt%. The grain boundary diffusion of this comparative example was processed by selecting the spraying method, and the product after the diffusion treatment was called B5.

[0060]

Table 4

[0061] As can be seen from Table 4, compared with B4, A4 has a comparable Br and a higher Hcj. This is mainly because the impurity content (C + O + N) is relatively well controlled by the method of Example 4. When comparing the impurity contents of A4 and B4, A4 < 1500 + (5.0 - crystal grain size) × 600 < B4. Furthermore, from the coercive forces of A4 and A5, the coercive force of A5 increases by 798 kA / m. From the coercive forces of B4 and B5, the coercive force of B5 increases by 721 kA / m. The magnet of A4 has a lower content of impurities C, O, and N, which is more favorable for the diffusion of heavy rare earths, but the magnet of A5 has a higher coercive force.

[0062] As described above, the embodiments of the present invention have been explained. However, the present invention is not limited to the above embodiments. Modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should all be included in the claims of the present invention.

Brief Description of the Drawings

[0063] [Figure 1] It is the measurement result of the particle size of the magnetic powder in Example 1. [Diagram 2] It is a fracture surface photograph scanned by a scanning electron microscope of the magnet in Example 1.

Claims

1. A method for producing a neodymium iron boron magnet having a chemical formula of RFeBM, in which R is a rare earth element, Fe is iron, and B is boron, the R content is 26-35 wt%, the B content is 0.8-1.3 wt%, and M is a plurality of elements selected from Co, Ga, Cu, Al, Zr, and Ti, in which the Co content is 0.5-3.0 wt%, the Ga content is 0.05-0.4 wt%, the Cu content is 0.05-0.5 wt%, the Al content is 0-1.5 wt%, the Zr or Ti content is 0-0.3 wt%, and the remainder is iron and unavoidable impurities, and the contents of the elements C, O, and N in the magnet satisfy C + O + N (ppm) ≦ [1500 + (5.0 - crystal grain size (μm)) × 600] (ppm), 1) melting an R-Fe-B-M alloy in a vacuum or inert gas atmosphere at a temperature of 1200-1600°C, pouring the melt into a quench roll rotating at a speed of 0.3-4 m / s to produce an R-Fe-B-M alloy strip, and then subjecting the alloy strip to hydrogen explosion treatment in a HD hydrogen explosion furnace, followed by evacuation to a pressure of less than 100 Pa before treatment, to obtain an R-Fe-B-M alloy fine powder by a stripping-hydrogen explosion method; 2) grinding the alloy fine powder of step 1) with a jet mill to obtain a magnetic powder having a particle size D50 of 4.0 μm or less, mixing the magnetic powder with a lubricant, and then pressing the magnetic powder into a green compact; 3) low-temperature sintering the powder compact of step 2) at 500-900°C, injecting a mixed gas of argon and hydrogen of 10kPa or less during the low-temperature sintering, keeping the temperature for 0.1-2 hours, and then evacuating the powder compact to 100Pa or less at least once, and then high-temperature sintering at 980-1040°C, keeping the temperature for 3-8 hours, cooling, and then tempering the powder compact to produce the neodymium iron boron magnet. Including, The rare earth elements are selected from lanthanum (La), cerium (Ce), praseodymium (Pr), neodymium (Nd), promethium (Pm), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), lutetium (Lu), yttrium (Y), and scandium (Sc); How to manufacture neodymium iron boron magnets.

2. In step 2), specifically, Step 1) grinding the alloy fine powder with a jet mill, in which the oxygen content in the jet mill process is less than 50ppm; The method for producing the neodymium iron boron magnet according to claim 1 .

3. 3. The method for producing a neodymium iron boron magnet according to claim 1, wherein in step 2), the amount of the lubricant added is 0.1 to 0.5 wt% of the mass of the magnetic powder.

4. The method for producing a neodymium iron boron magnet according to any one of claims 1 to 3, wherein in step 2), the magnetic powder is pressure-molded into a green compact using a magnetic orientation molding device having an oxygen content of less than 500 ppm and an orientation magnetic field strength of 1 to 2 T.

5. The method for producing a neodymium iron boron magnet according to any one of claims 1 to 4, wherein in step 3), the low-temperature sintering is carried out in a mixed atmosphere of argon and hydrogen, in which argon occupies 95-99 vol% of the total volume of the mixed atmosphere and hydrogen occupies 1-5 vol% of the total volume of the mixed atmosphere.

6. The method for producing a neodymium iron boron magnet according to any one of claims 1 to 5, wherein the tempering treatment includes a primary tempering treatment and a secondary tempering treatment.

7. The method for producing a neodymium iron boron magnet according to claim 6, wherein the temperature of the first tempering treatment is 700-900°C, the time of the first tempering treatment is 3-7h, the temperature of the second tempering treatment is 450-600°C, and the time of the second tempering treatment is 3-7h.

Citation Information

Patent Citations

  • R-fe-b sintered permanent magnet

    JP1999097223A

  • Sintered permanent magnet

    JP1999273922A

  • Rare earth magnet

    JP2009260338A

  • Method for producing rare earth sintered magnet

    JP2010150604A

  • MANUFACTURING METHOD OF SINTERED Nd-Fe-B MAGNETIC SUBSTRATE CONTAINING NO HEAVY RARE EARTH ELEMENT

    JP2017128793A