Porous carbon structure, its manufacturing method and lithium secondary battery including same

A core-shell MOF-doped porous carbon structure addresses the insulating issues in lithium-sulfur batteries, enhancing conductivity and preventing polysulfide leakage to improve battery performance and efficiency.

JP7556134B2Active Publication Date: 2024-09-25LG ENERGY SOLUTION LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023513505
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-01-26
Filing Date
2022-01-27
Publication Date
2024-09-25
Estimated Expiration
2042-01-27

AI Technical Summary

Technical Problem

Existing lithium-sulfur secondary batteries face challenges with poor cycle characteristics and polysulfide seepage due to the insulating properties of sulfur, which limits their commercialization and energy efficiency.

Method used

A porous carbon structure with a core-shell MOF configuration is developed, where the core and shell have different MOF compositions, doped with elements like N and S, to enhance conductivity and physically/chemically prevent polysulfide leakage.

Benefits of technology

The core-shell structure effectively suppresses polysulfide seepage, improving the electrical conductivity and energy efficiency of lithium-sulfur secondary batteries by enhancing the adsorption of sulfur and supporting smooth electrochemical reactions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007556134000005
    Figure 0007556134000005
  • Figure 0007556134000006
    Figure 0007556134000006
  • Figure 0007556134000007
    Figure 0007556134000007
Patent Text Reader

Abstract

The present invention relates to a porous carbon structure and a manufacturing method thereof. More specifically, the porous carbon structure includes a core-shell MOF, and the first MOF included in the core and the second MOF included in the shell have different pore structures and constituent elements. Therefore, when the porous carbon structure is applied as a sulfur support to a lithium secondary battery containing sulfur as a positive electrode active material, the polysulfide generated in the positive electrode can be prevented from seeping into the electrolyte, thereby improving the performance and life characteristics of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of priority based on Korean Patent Application No. 2021-0011621 filed on January 27, 2021, and Korean Patent Application No. 2022-0011827 filed on January 26, 2022, and all contents disclosed in the documents of the relevant Korean patent applications are incorporated as part of this specification.

[0002] The present invention relates to a porous carbon structure applicable to a positive electrode material of a lithium secondary battery, a method for producing the same, and a lithium secondary battery including the same. [Background technology]

[0003] The lithium-sulfur (Li-S) secondary battery, which is an energy storage device, has a theoretical energy density of 2600Wh / kg and a theoretical capacity of 1672mAh / g, which is 3 to 5 times higher than that of existing lithium batteries, and is attracting attention as a next-generation energy storage device. However, since its cycle characteristics are not good enough for commercial use, research has been conducted to improve the cycle characteristics using various methods.

[0004] In particular, the carbon-based material graphene and activated carbon have been used as templates to prevent the volume expansion of sulfur while increasing its conductivity. However, this method also has many shortcomings for commercialization, and other methods must be presented for commercialization.

[0005] Metal organic frameworks (MOFs) are three-dimensional porous materials with a repeated arrangement of metal blocks and organic ligands, which are synthesized by a sequence synthesis method in which a metal precursor and an organic linker are placed in a specific solvent.

[0006] MOFs have micropores and mesopores of various sizes, and have a very large specific surface area, so they have been used as gas storage media. In addition, MOFs could not be used electrochemically due to the problem of low conductivity, but recently nano-sized MOFs have been synthesized and used for electrochemical purposes, and the use of metal organic frameworks is increasing.

[0007] In addition, MOFs have a wide variety of combinations of metal precursors and organic ligands, and can be embodied in thousands of crystal structures. They can also contain a variety of functional groups, making them highly useful in terms of their utility.

[0008] Such MOFs can be produced as porous carbon structures with high specific surface areas and large porosity through a carbonization process using heat treatment.

[0009] However, even porous carbon structures with high specific surface area and large porosity have limitations in improving energy efficiency when applied to energy devices. Thus, there is a need to develop porous carbon structures that can improve the reactivity of energy devices and thereby improve their energy efficiency. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] Korean Patent Publication No. 2020-0021214 [Patent Document 2] Korean Patent Publication No. 2012-0063925 Summary of the Invention [Problem to be solved by the invention]

[0011] Therefore, the present invention provides a porous carbon structure that is a support for sulfur contained in a positive electrode active material of a lithium-sulfur secondary battery, and can complement the insulating properties of sulfur to improve electrical conductivity and suppress the outflow of polysulfides from the positive electrode.

[0012] It is therefore an object of the present invention to provide a porous carbon structure comprising a core-shell MOF and a method for producing the same.

[0013] Another object of the present invention is to provide a lithium secondary battery including the porous carbon structure. [Means for solving the problem]

[0014] To achieve the above object, the present invention provides a core-shell porous carbon structure, in which the core comprises a first MOF (metal organic framework), the shell comprises a second MOF, and the second MOF is doped with a heteroelement including at least one of N and S.

[0015] The present invention also provides a method for producing a porous carbon structure, comprising: (S1) heating a mixed solution in which a metal precursor and a first organic ligand precursor are dissolved in an organic solvent to form an MOF; (S2) adding a second organic ligand containing at least one of N and S to the mixed solution and heating the mixture to form a core-shell MOF; and (S3) carbonizing the core-shell MOF formed in the step (S2). Effect of the Invention

[0016] The porous carbon structure according to the present invention has a core-shell structure in which the core and shell each contain MOFs having a different pore structure. When the porous carbon structure according to the present invention is used as a sulfur support in the positive electrode of a lithium-sulfur secondary battery, it can physically prevent polysulfides generated in the positive electrode from leaking into the electrolyte.

[0017] In addition, in the core-shell porous carbon structure, the shell contains heterogeneous elements such as N and S. Therefore, when the core-shell porous carbon structure is used as a sulfur support for the positive electrode of a lithium-sulfur secondary battery, polysulfides generated in the positive electrode are physically or chemically adsorbed by the heterogeneous elements, thereby preventing the polysulfides from leaking into the electrolyte. [Brief description of the drawings]

[0018] [Figure 1] FIG. 2 is a schematic diagram showing the process of forming a MOF having a core-shell structure in the MOF production method according to the present invention. [Diagram 2] 1 shows SEM (Scanning Electron Microscope) images of MOFs prepared in Example 1, Example 2, and Comparative Example 1, respectively. [Diagram 3] 1 is a graph (2-theta-scale) showing the results of XRD (X-ray Diffraction) analysis of the porous carbon structures prepared in Example 1 and Comparative Examples 1, 2, and 3, respectively. [Figure 4] 2 is an optical microscope photograph of the porous carbon structures prepared in Examples 1 and 2 and Comparative Examples 1, 2, and 3, respectively. [Diagram 5] 1 is a graph showing the results of FT-IR (Fourier-transform infrared spectroscopy) analysis of the MOFs prepared in Example 1 and Comparative Example 1 and their raw materials. [Figure 6] 1 shows the results of FIB-EDS (Focused Ion Beam-Energy Dispersive X-ray Spectrometer) measurement of the MOF produced in Example 1. [Figure 7] 1 shows the results of SEM-EDS (Scanning Electron Microscope-Energy Dispersive X-ray Spectrometer) measurement of the porous carbon structure produced in Example 2. [Figure 8a]1 shows the results of XPS (X-ray photoelectron spectroscopy) measurement of the porous carbon structure produced in Example 1. [Figure 8b] 1 shows the results of XPS (X-ray photoelectron spectroscopy) measurement of the porous carbon structure produced in Example 2. [Figure 9a] 1 is a graph showing the results of BET analysis of the porous carbon structures prepared in the examples and comparative examples. [Figure 9b] 1 is a graph showing the results of BET analysis of the porous carbon structures prepared in the examples and comparative examples. [Figure 9c] 1 is a graph showing the results of BET analysis of the porous carbon structures prepared in the examples and comparative examples. [Figure 10] 1 is a graph showing electrochemical performance of a lithium-sulfur secondary battery depending on a porous carbon structure material contained in a positive electrode. [Figure 11a] 1 is a graph showing the capacity after 1 cycle and 30 cycles of batteries including Example 1 and Comparative Example 1. [Figure 11b] 1 is a graph showing the capacity after 1 cycle and 30 cycles of batteries including Example 1 and Comparative Example 1. [Figure 12a] 1 is a graph showing the change in NMR peak depending on the synthesis time of the porous carbon structure in Example 1. [Figure 12b] 1 is a graph showing NMR peak changes in Example 1 and Comparative Examples 1, 2, and 3. [Figure 13] 3 is a photograph showing the results of measuring the contact angle of electrodes including the porous carbon structures of Example 1 and Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The present invention will now be described in more detail to facilitate understanding of the present invention.

[0020] The terms and words used in this specification and claims should not be construed in a limited manner based on their ordinary or dictionary meaning, but should be interpreted in a meaning and concept that corresponds to the technical idea of ​​the present invention, based on the principle that the inventor can appropriately define the concept of the term in order to best describe his / her invention.

[0021] The term "hierarchical structure" as used herein means a core-shell porous carbon structure in which the shell is formed in the form of a separate layer on the core, where the shell is formed entirely or partially on the core.

[0022] Porous Carbon Structure The present invention relates to a core-shell porous carbon structure, in which the core comprises a first MOF (metal organic framework) and the shell comprises a second MOF, the second MOF being doped with a heteroelement, including at least one of N and S.

[0023] The first MOF and the second MOF have different pore structures and elemental compositions, and the second MOF forms a layer on the entire or partial surface of the first MOF, so that a core-shell porous carbon structure can be formed. Here, the pore structure refers to the volume and size of the pores.

[0024] Specifically, the shell differs from the core in that it is doped with foreign atoms and has developed micropores (micropore dominant).This structure makes it possible to chemically (foreign atom doping) and physically (micropores) suppress the outflow of LiPS when the battery is powered by a lithium secondary battery such as a lithium-sulfur secondary battery.

[0025] For example, the first MOF has a specific surface area of ​​1700 to 2000 m 2 / g, the pore volume is 1.9 to 2.5 cc / g, and the specific surface area of ​​the second MOF is 900 to 1300 m 2 / g and the pore volume is 0.8 to 1.0 cc / g.

[0026] In the present invention, the porous carbon structure may have different pore volumes and specific surface areas depending on the type of the foreign element doped into the second MOF of the shell. For example, if the foreign element is N, micropores may develop in the porous carbon structure, increasing the specific surface area and slightly decreasing the pore volume. On the other hand, if the foreign element is S, mesopores may develop in the porous carbon structure along with micropores, increasing both the specific surface area and the pore volume. The diameters of the micropores and mesopores are not particularly limited, but the diameter of the micropores is 1 nm or more and less than 5 nm, and the diameter of the mesopores is 5 nm to 10 nm.

[0027] In the present invention, the pore volume of the porous carbon structure is not particularly limited, but the larger the pore volume, the more suitable it is for use as a positive electrode material for lithium secondary batteries. For example, when the porous carbon structure is used as a positive electrode material for lithium secondary batteries, the larger the pore volume of the porous carbon structure, the more sulfur (S8) contained in the positive electrode active material can be impregnated, and damage to the positive electrode cell structure due to volume expansion that occurs during interconversion between sulfur (S8) and lithium polysulfide (LiPS) can be prevented.

[0028] Here, when the porous carbon structure is applied to a positive electrode material of a lithium secondary battery and functions as a sulfur carrier, the pore volume of the porous carbon structure is 1.5 cc / g to 4.5 cc / g, specifically, 1.5 cc / g or more, 2.0 cc / g or more, or 2.5 cc / g or more, and 3.5 cc / g or less, 4.0 cc / g or less, or 4.5 cc / g or less.

[0029] The pore volume of the porous carbon structure may vary depending on the type of the foreign element. For example, if the foreign element contained in the porous carbon structure is N, the porous carbon structure includes micropores.

[0030] In the present invention, the specific surface area of ​​the porous carbon structure is not particularly limited, but the larger the specific surface area, the more positions can be provided for the oxidation-reduction reaction between Li ions and sulfur, and therefore the smoother the electrochemical reaction can be performed during charging and discharging of the lithium secondary battery.

[0031] Here, the specific surface area of ​​the porous carbon structure is 1500 to 3000 m 2 / g, specifically, 1500m 2 / g or more or 1800m 2 / g or more, or 2500m 2 / g or less or 3000m 2 / g or less. The specific surface area of ​​the porous carbon structure is 1500 m 2 If the amount is less than 3000m / g, the active material cannot be sufficiently supported. 2 If it exceeds 1 / g, more process time and cost than necessary may be required to achieve the specific surface area.

[0032] In the present invention, the porous carbon structure may contain metal ions and organic ligands as components forming the framework of the first MOF and the second MOF.

[0033] The metal ion is one or more ions selected from the group consisting of metals of groups 1 to 16 of the periodic table. + , Na + , K + , Rb + , B.E. 2+ , Mg 2+ , Ca 2+ , Sr 2+ , B.A. 2+ , Sc 3+ , Y 3+ , Ti 4+ , Zr 4+ , Hf + , V 4+ , V 3+ , V 2+ , Nb 3+ , Ta 3+ , Cr 3+ , Mo 3+ , W 3+ , Mn3+ , Mn 2+ , Re 3+ , Re 2+ , Fe 3+ , Fe 2+ , Ru 3+ , Ru 2+ , Os 3+ , Os 2+ , Co 3+ , Co 2+ , Rh 2+ , Rh + , Ir 2+ , Ir + , Ni 2+ , Ni + , Pd 2+ , Pd + , Pt 2+ , Pt + , Cu 2+ , Cu + , Ag + , Au + , Zn 2+ , Cd 2+ , Hg 2+ , Al 3+ , Ga 3+ , In 3+ , Tl 3+ , Si 4+ , Si 2+ , Ge 4+ , Ge 2+ , Sn 4+ , Sn 2+ , Pb 4+ , Pb 2+ , As 5+ , As 3+ , As + , Sb 5+ , Sb 3+ , Sb + , Bi 5+ , Bi 3+ and Bi + The compound is one or more selected from the group consisting of:

[0034] The organic ligand is at least one selected from the group consisting of halides (fluorine, chlorine, bromine, iodine), carboxylates, cyano, isocyanate, isothiocyanate, nitrile, pyridyl, nitroso, nitro, and phosphate. Specific examples of the organic ligand include 4,4-bipyridin, benzene-1,4-dicarboxylate, or derivatives thereof.

[0035] In addition, the molar ratio of the metal ion to the organic ligand contained in the MOF is 1:0.2 to 5, preferably 1:0.3 to 4.5, and more preferably 1:0.5 to 4. If the molar ratio of the organic ligand to the metal ion is less than this range, the porosity may be reduced, and if it exceeds this range, the pore size may be reduced.

[0036] Method for producing porous carbon structure The present invention also relates to a method for producing a porous carbon structure, and provides a method for producing a porous carbon structure, comprising: (S1) heating a mixed solution in which a metal precursor and a first organic ligand precursor are dissolved in an organic solvent to form an MOF; (S2) adding a second organic ligand containing one or more of N and S to the mixed solution and heating the mixture to form a core-shell MOF; and (S3) carbonizing the core-shell MOF formed in the step (S2).

[0037] Hereinafter, each step of the method for producing a porous carbon structure according to the present invention will be described in more detail.

[0038] In the present invention, in step (S1), a mixed solution in which a metal precursor and a first organic ligand precursor are dissolved in an organic solvent may be heated to form a MOF.

[0039] The reaction conditions for forming the MOF are heating at a temperature of 100 to 150° C. for 6 to 40 hours.

[0040] If the reaction temperature is less than 100°C, the crystallization reaction is unlikely to start, and MOFs may not be formed, whereas if the reaction temperature is more than 150°C, MOFs can be formed.

[0041] In addition, if the reaction time is less than 6 hours, the reaction may end with the intermediate product remaining or with a mixture of MOF and the intermediate product, whereas if the reaction time is more than 40 hours, the process may take too long, resulting in reduced process efficiency.

[0042] The metal precursor is a compound containing a metal ion as described above. For example, the metal precursor may include a zinc precursor, which may include one or more selected from the group consisting of zinc nitrate hexahydrate (Zn(NO3)2·6H2O), zinc acetate dihydrate (Zn(CH3CO2)2·2H2O), and zinc sulfate hexahydrate (ZnSO4·6H2O).

[0043] In addition, the first organic ligand precursor may be 1,4-benzenedicarboxylic acid, benzene-1,3,5-tricarboxylic acid, 2-methylimidazole, oxalic acid, malonic acid, butanedioic acid, glutaric acid, o-phthalic acid, m-phthalic acid, p-phthalic acid, 2-hydroxy-1,2,3-propanetricarboxylic acid, or the like. The dicarboxylic acid may include one or more selected from the group consisting of 1H-1,2,3-triazole, 1H-1,2,4-triazole, and 3,4-dihydroxy-3-cyclobutene-1,2-dione, and is preferably 1,4-benzenedicarboxylic acid.

[0044] The organic solvent is at least one selected from the group consisting of dimethyl carbonate, dimethylformamide (DMF), N-methylformamide, sulfolane (tetrahydrothiophene-1,1-dioxide), 3-methylsulfolane, N-butylsulfone, dimethylsulfoxide, pyrrolidinone (HEP), dimethylpiperidone (DMPD), N-methylpyrrolidinone (NMP), N-methylacetamide, dimethylacetamide (DMAc), dimethylformamide (DMF), diethylacetamide (DEAc), dipropylacetamide (DPAc), ethanol, propanol, butanol, hexanol, ethylene glycol, tetrachloroethylene, propylene glycol, toluene, turpentine, methyl acetate, ethyl acetate, petrol ether, acetone, cresol, and glycerol, and is preferably dimethylformamide (DMF).

[0045] In the present invention, in step (S2), a second organic ligand precursor containing at least one of N and S is added to the mixed solution in which the MOF is formed, and heated to form a core-shell MOF. At this time, the second organic ligand can be used in the form of a solution dissolved in an organic solvent. The organic solvent can be the same or different from the organic solvent used in step (S1) within the range of the type of organic solvent.

[0046] The reaction conditions for synthesizing the core-shell MOF are heating at 35°C to 100°C for 15 to 25 hours. If the reaction temperature or time is less than this range, the ligand exchange reaction rate is too slow, and if it is more than this range, the crystallinity may be destroyed by heat.

[0047] The synthesized MOF can be supported in a second organic ligand precursor solution to carry out the reaction. At this time, the synthesized MOF can be supported in the second organic ligand solution in a crystalline state after washing, activation, and drying. In the second organic ligand precursor solution in which the MOF is supported, a solvent-assisted ligand exchange reaction occurs, and one or more of the heteroelements N and S contained in the second organic ligand precursor are doped on the surface of the MOF.

[0048] In this case, the inside of the MOF that is not doped with the heteroelement may be called the first MOF, and the surface portion doped with the heteroelement may be called the second MOF. In addition, the first MOF may be called the core, and the second MOF may be called the shell, forming a core-shell structured MOF.

[0049] In general, a solvent-assisted ligand exchange reaction occurs when the parent and daughter ligands of a ligand solution and parent MOF exchange, resulting in the production of a daughter MOF that maintains the topology of the parent MOF. Depending on the reaction conditions (e.g., temperature, concentration, crystal size, etc.) and the characteristics of the daughter ligands, the parent MOF is either completely converted to a daughter MOF, or the surface of the parent MOF is converted to a daughter MOF in sequence, forming a core-shell structure. The ligand exchange is considered to be in equilibrium when ΔG, which is related to the linker exchange process, converges to 0.

[0050] According to one embodiment of the present invention, the parent ligand is terephthalic acid and the daughter ligand is 2-aminoterephthalic acid, and during the exchange process, the parent MOF does not completely convert to the daughter MOF due to the steric hindrance of the amine group present in 2-aminoterephthalic acid, forming a core-shell structure.

[0051] Ligand exchange can be confirmed by changes in crystal color, yellow frames on OM, FT-IR, FIB-EDS, NMR, etc., and the conversion rate can be determined through NMR analysis.

[0052] FIG. 1 is a schematic diagram showing the process of forming a core-shell MOF by the method for producing a porous carbon structure according to the present invention.

[0053] Referring to FIG. 1, circle 1 shows a schematic diagram of the MOF formed in step (S1). Circle 2 shows a schematic diagram of the initial MOF in step (S2) in which the surface of the MOF begins to be doped with N as the solvent-assisted ligand exchange reaction between the MOF and the second organic ligand precursor begins. Circle 3 shows a schematic diagram of a core-shell structured MOF in which the solvent-assisted ligand exchange reaction is completed, the surface of the MOF is doped with a foreign element, and the first MOF and the second MOF are separated. At this time, the second MOF forming the shell is doped with a foreign element.

[0054] The second organic ligand precursor contains one or more of N and S.

[0055] The N-containing second organic ligand precursor includes at least one selected from the group consisting of 2-aminoterephthalic acid, 4-aminophthalic acid, 4-aminoisophthalic acid, 5-aminoisophthalic acid, 2,5-diaminoterephthalic acid, 2,2'-diamino-4,4'-stilbenedicarboxylic acid, 5-cyano-1,3-benzenedicarboxylic acid, 2-methylimidazole, and 4,4',4"-s-triazine-2,4,6-triyl-tribenzoic acid. Hereinafter, the present invention will be described in more detail in order to facilitate understanding of the present invention.

[0056] The terms and words used in this specification and claims should not be construed in a limited manner based on their ordinary or dictionary meaning, but should be interpreted in a meaning and concept that corresponds to the technical idea of ​​the present invention, based on the principle that the inventor can appropriately define the concept of the term in order to best describe his / her invention.

[0057] The term "hierarchical structure" as used herein means a core-shell porous carbon structure in which the shell is formed in the form of a separate layer on the core, where the shell is formed entirely or partially on the core.

[0058] Porous Carbon Structure The present invention relates to a core-shell porous carbon structure, in which the core comprises a first MOF (metal organic framework) and the shell comprises a second MOF, the second MOF being doped with a heteroelement, including at least one of N and S.

[0059] The first MOF and the second MOF have different pore structures and elemental compositions, and the second MOF may form a layer on the entire or partial surface of the first MOF to form a core-shell porous carbon structure, where the pore structure refers to the volume and size of the pores.

[0060] Specifically, the shell differs from the core in that it is doped with foreign atoms and has developed micro-pores (micro-pore dominant).This structure makes it possible to chemically (foreign atom doping) and physically (micro-pores) suppress the outflow of LiPS when a lithium secondary battery such as a lithium-sulfur secondary battery is operated.

[0061] For example, the specific surface area of ​​the first MOF is 1700 to 2000 m 2 / g, the pore volume is 1.9 to 2.5 cc / g, and the specific surface area of ​​the second MOF is 900 to 1300 m 2 / g and the pore volume is 0.8 to 1.0 cc / g.

[0062] In the present invention, the porous carbon structure may have different pore volumes and specific surface areas depending on the type of the foreign element doped into the second MOF of the shell. For example, if the foreign element is N, micropores may develop in the porous carbon structure, increasing the specific surface area and slightly decreasing the pore volume. On the other hand, if the foreign element is S, mesopores may develop in the porous carbon structure along with micropores, increasing both the specific surface area and the pore volume. The diameters of the micropores and mesopores are not particularly limited, but the diameter of the micropores is 1 nm or more and less than 5 nm, and the diameter of the mesopores is 5 nm to 10 nm.

[0063] In the present invention, the pore volume of the porous carbon structure is not particularly limited, but the larger the pore volume, the more suitable it is for use as a positive electrode material for lithium secondary batteries. For example, when the porous carbon structure is used as a positive electrode material for lithium secondary batteries, the larger the pore volume of the porous carbon structure, the more sulfur (S8) contained in the positive electrode active material can be impregnated, and structural damage to the positive electrode cell due to volume expansion that occurs during interconversion between sulfur (S8) and lithium polysulfide (LiPS) can be prevented.

[0064] Here, when the porous carbon structure is applied to a positive electrode material of a lithium secondary battery and functions as a sulfur carrier, the pore volume of the porous carbon structure is 1.5 cc / g to 4.5 cc / g, specifically, 1.5 cc / g or more, 2.0 cc / g or more, or 2.5 cc / g or more, and 3.5 cc / g or less, 4.0 cc / g or less, or 4.5 cc / g or less.

[0065] The pore volume of the porous carbon structure may vary depending on the type of the foreign element. For example, if the foreign element contained in the porous carbon structure is N, the porous carbon structure includes micropores.

[0066] In the present invention, the specific surface area of ​​the porous carbon structure is not particularly limited, but the larger the specific surface area, the more sufficient the sites for the oxidation-reduction reaction between Li ions and sulfur can be provided, and therefore the electrochemical reaction can be smoothly performed during charging and discharging of the lithium secondary battery.

[0067] Here, the specific surface area of ​​the porous carbon structure is 1500 to 3000 m 2 / g, specifically, 1500m 2 / g or more or 1800m 2 / g or more, or 2500m 2 / g or less or 3000m 2 / g or less. The specific surface area of ​​the porous carbon structure is 1500 m 2 If the carrier is less than 3000m / g, the active material cannot be sufficiently supported. 2 If it exceeds 1 / g, more process time and cost than necessary may be required to achieve the specific surface area.

[0068] In the present invention, the porous carbon structure may contain metal ions and organic ligands as components forming the framework of the first MOF and the second MOF.

[0069] The metal ion is one or more ions selected from the group consisting of metals of groups 1 to 16 of the periodic table. + , Na + , K + , Rb + , B.E. 2+ , Mg 2+ , Ca 2+ , Sr 2+ , B.A. 2+ , Sc 3+ , Y 3+ , Ti 4+ , Zr 4+ , Hf + , V 4+ , V 3+ , V 2+ , Nb 3+ , Ta 3+ , Cr 3+ , Mo 3+ , W 3+ , Mn 3+, Mn 2+ , Re 3+ , Re 2+ , Fe 3+ , Fe 2+ , Ru 3+ , Ru 2+ , Os 3+ , Os 2+ , Co 3+ , Co 2+ , Rh 2+ , Rh + , Ir 2+ , Ir + , Ni 2+ , Ni + , Pd 2+ , Pd + , Pt 2+ , Pt + , Cu 2+ , Cu + , Ag + , Au + , Zn 2+ , Cd 2+ , Hg 2+ , Al 3+ , Ga 3+ , In 3+ , Tl 3+ , Si 4+ , Si 2+ , Ge 4+ , Ge 2+ , Sn 4+ , Sn 2+ , Pb 4+ , Pb 2+ , As 5+ , As 3+ , As + , Sb 5+ , Sb 3+ , Sb + , Bi 5+ , Bi 3+ and Bi + The compound is one or more selected from the group consisting of:

[0070] The organic ligand is at least one selected from the group consisting of halides (fluorine, chlorine, bromine, iodine), carboxylates, cyano, isocyanate, isothiocyanate, nitrile, pyridyl, nitroso, nitro, and phosphate.Specific examples of the organic ligand include 4,4-bipyridin, benzene-1,4-dicarboxylate, or derivatives thereof.

[0071] In addition, the molar ratio of the metal ion to the organic ligand contained in the MOF is 1:0.2 to 5, preferably 1:0.3 to 4.5, and more preferably 1:0.5 to 4. If the molar ratio of the organic ligand to the metal ion is less than this range, the porosity may be reduced, and if it exceeds this range, the pore size may be reduced.

[0072] Method for producing porous carbon structures The present invention also relates to a method for producing a porous carbon structure, and provides a method for producing a porous carbon structure, comprising: (S1) heating a mixed solution in which a metal precursor and a first organic ligand precursor are dissolved in an organic solvent to form an MOF; (S2) adding a second organic ligand containing one or more of N and S to the mixed solution and heating the mixture to form a core-shell MOF; and (S3) carbonizing the core-shell MOF formed in the step (S2).

[0073] Hereinafter, each step of the method for producing a porous carbon structure according to the present invention will be described in more detail.

[0074] In the present invention, in step (S1), a mixed solution in which a metal precursor and a first organic ligand precursor are dissolved in an organic solvent may be heated to form a MOF.

[0075] The reaction conditions for forming the MOF are heating at a temperature of 100 to 150° C. for 6 to 40 hours.

[0076] If the reaction temperature is less than 100°C, the crystallization reaction is unlikely to start and MOFs may not be formed, whereas if the reaction temperature is more than 150°C, MOFs can be formed.

[0077] In addition, if the reaction time is less than 6 hours, the reaction may end with the intermediate product or a mixture of MOF and the intermediate product, whereas if the reaction time is more than 40 hours, the process may take too long, resulting in reduced process efficiency.

[0078] The metal precursor is a compound containing a metal ion as described above. For example, the metal precursor may include a zinc precursor, which may include one or more selected from the group consisting of zinc nitrate hexahydrate (Zn(NO3)2·6H2O), zinc acetate dihydrate (Zn(CH3CO2)2·2H2O), and zinc sulfate hexahydrate (ZnSO4·6H2O).

[0079] In addition, the first organic ligand precursor may be 1,4-benzenedicarboxylic acid, benzene-1,3,5-tricarboxylic acid, 2-methylimidazole, oxalic acid, malonic acid, butanedioic acid, glutaric acid, o-phthalic acid, m-phthalic acid, p-phthalic acid, 2-hydroxy-1,2,3-propanetricarboxylic acid, or the like. The dicarboxylic acid may include one or more selected from the group consisting of 1H-1,2,3-triazole, 1H-1,2,4-triazole and 3,4-dihydroxy-3-cyclobutene-1,2-dione, and is preferably 1,4-benzenedicarboxylic acid.

[0080] The organic solvent is at least one selected from the group consisting of dimethyl carbonate, dimethylformamide (DMF), N-methylformamide, sulfolane (tetrahydrothiophene-1,1-dioxide), 3-methylsulfolane, N-butylsulfone, dimethylsulfoxide, pyrrolidinone (HEP), dimethylpiperidone (DMPD), N-methylpyrrolidinone (NMP), N-methylacetamide, dimethylacetamide (DMAc), dimethylformamide (DMF), diethylacetamide (DEAc), dipropylacetamide (DPAc), ethanol, propanol, butanol, hexanol, ethylene glycol, tetrachloroethylene, propylene glycol, toluene, turpentine, methyl acetate, ethyl acetate, petrol ether, acetone, cresol, and glycerol, and is preferably dimethylformamide (DMF).

[0081] In the present invention, in step (S2), a second organic ligand precursor containing at least one of N and S is added to the mixed solution in which the MOF is formed, and heated to form a core-shell MOF. In this case, the second organic ligand can be used in the form of a solution dissolved in an organic solvent. The organic solvent can be the same or different from that used in step (S1) within the range of the organic solvent.

[0082] The reaction conditions for synthesizing the core-shell MOF are heating at 35°C to 100°C for 15 to 25 hours. If the reaction temperature or time is less than this range, the ligand exchange reaction rate is too slow, and if it is more than this range, the crystallinity may be destroyed by heat.

[0083] The synthesized MOF may be supported in a second organic ligand precursor solution to carry out the reaction. In this case, the synthesized MOF may be supported in the second organic ligand solution in a crystalline state after washing, activation, and drying. In the second organic ligand precursor solution in which the MOF is supported, a solvent-assisted ligand exchange reaction occurs, and one or more of the heteroelements N and S contained in the second organic ligand precursor are doped on the surface of the MOF.

[0084] In this case, the inside of the MOF that is not doped with the heteroelement may be called the first MOF, and the surface portion doped with the heteroelement may be called the second MOF. In addition, the first MOF may be called the core, and the second MOF may be called the shell, forming a core-shell structured MOF.

[0085] In general, a solvent-assisted ligand exchange reaction occurs when the parent and daughter ligands of a ligand solution and parent MOF exchange, resulting in the production of a daughter MOF that maintains the topology of the parent MOF. Depending on the reaction conditions (e.g., temperature, concentration, crystal size, etc.) and the characteristics of the daughter ligands, the parent MOF is either completely converted to a daughter MOF, or the surface of the parent MOF is converted to a daughter MOF in sequence to form a core-shell structure. The ligand exchange is considered to be in equilibrium when ΔG, which is related to the linker exchange process, converges to 0.

[0086] According to one embodiment of the present invention, the parent ligand is terephthalic acid and the daughter ligand is 2-aminoterephthalic acid, and during the exchange process, the parent MOF does not completely convert to the daughter MOF due to the steric hindrance of the amine group present in 2-aminoterephthalic acid, forming a core-shell structure.

[0087] Ligand exchange can be confirmed by changes in crystal color, yellow frames on OM, FT-IR, FIB-EDS, NMR, etc., and the conversion rate can be determined through NMR analysis.

[0088] FIG. 1 is a schematic diagram showing the process of forming a core-shell MOF by the method for producing a porous carbon structure according to the present invention.

[0089] Referring to FIG. 1, circle 1 shows a schematic diagram of the MOF formed in step (S1). Circle 2 shows a schematic diagram of the initial MOF in step (S2) where the surface of the MOF begins to be doped with N as the solvent-assisted ligand exchange reaction between the MOF and the second organic ligand precursor begins. Circle 3 shows a schematic diagram of a core-shell structured MOF in which the solvent-assisted ligand exchange reaction is completed, the surface of the MOF is doped with a foreign element, and the first MOF and the second MOF are separated. At this time, the second MOF forming the shell is doped with a foreign element.

[0090] The second organic ligand precursor contains at least one of N and S.

[0091] The N-containing second organic ligand precursor includes at least one selected from the group consisting of 2-aminoterephthalic acid, 4-aminophthalic acid, 4-aminoisophthalic acid, 5-aminoisophthalic acid, 2,5-diaminoterephthalic acid, 2,2'-diamino-4,4'-stilbenedicarboxylic acid, 5-cyano-1,3-benzenedicarboxylic acid, 2-methylimidazole, and 4,4',4"-s-triazine-2,4,6-triyl-tribenzoic acid.

[0092] The second organic ligand precursor containing S includes one or more selected from the group consisting of 2,5-disulfanylterephthalic acid (H4(C8H2O4S2)), 2-sulfanylterephthalic acid, and 2,5-thiophenedicarboxylic acid.

[0093] In the present invention, in step (S3), the core-shell MOF formed in step (S2) is heat-treated and carbonized to prepare a porous carbon structure.

[0094] The heat treatment is carried out in an inert atmosphere, which is formed by nitrogen gas, argon gas, helium gas, krypton gas or xenon gas, and is preferably formed by argon gas.

[0095] The heat treatment temperature is 900° C. to 1500° C., specifically, 900° C. or more, 950° C. or more, or 1000° C. or more, and 1100° C. or less, 1300° C. or less, or 1500° C. or less. If the heat treatment temperature is less than 900° C., the Zn metal in the MOF may not be sufficiently removed, and if it is more than 1500° C., the process may require a lot of time and energy, resulting in reduced process efficiency.

[0096] The heat treatment time is 6 to 24 hours, specifically 6 hours or more, 7 hours or more, or 8 hours or more, and 22 hours or less, 23 hours or less, or 24 hours or less. If the heat treatment time is less than 6 hours, carbonization may not be sufficient, and it may be difficult to secure a sufficient specific surface area and pore volume required for electrochemical reaction, and if it exceeds 24 hours, a lot of time and energy are required for the process, so the process efficiency may be reduced.

[0097] Lithium secondary battery The present invention also relates to a lithium secondary battery including a positive electrode, a negative electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte, and the porous carbon structure may be included as a positive electrode material.

[0098] Specifically, when a sulfur-containing material is used as a positive electrode active material, the porous carbon structure can be used as a sulfur carrier. A battery including a sulfur-containing material as a positive electrode active material can be called a lithium-sulfur secondary battery.

[0099] In the present invention, the positive electrode of the lithium secondary battery may include a positive electrode current collector and a positive electrode mixture layer formed on the positive electrode current collector and having a positive electrode active material.

[0100] The positive electrode active material may include elemental sulfur (S8), sulfur-based compounds, or mixtures thereof. Specifically, the sulfur-based compounds may include Li2Sn (n ≧ 1), organic sulfur compounds, or carbon-sulfur polymers ((C2Sx)n: x = 2.5 to 50, n ≧ 2). In the case of these sulfur substances, since they do not have electrical conductivity alone, they can also be used in the positive electrode of a lithium secondary battery in the form of a sulfur-carbon composite by being combined with a carbon material.

[0101] In addition, the positive electrode active material may further include a lithium-containing transition metal oxide. The lithium-containing transition metal oxides include LiCoO2, LiNiO2, LiMnO2, LiMn2O4, Li(Ni a Co b Mn c )O2 (0 < a < 1, 0 < b < 1, 0 < c < 1, a + b + c = 1), LiNi 1‐y Co y O2, LiCo 1‐y Mn y O2, LiNi 1‐y Mn y O2 (0 ≦ y < 1), Li(Ni a Co b Mn c )O4 (0 < a < 2, 0 < b < 2, 0 < c < 2, a + b + c = 2), LiMn 2‐z Ni z O4, LiMn 2‐z Co z O4 (0 < z < 2), LiCoPO4, and LiFePO4, and any one selected from the group consisting of these or a mixture of two or more thereof can be used. In addition to such oxides, sulfides, selenides, halides, etc. can also be used.

[0102] In addition, the positive electrode current collector is not particularly limited as long as it has high conductivity without causing a chemical change in the battery, and may be, for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. In this case, the positive electrode current collector may be in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc., having fine irregularities formed on the surface to enhance adhesion to the positive electrode active material.

[0103] In the present invention, the negative electrode of the lithium secondary battery may include a negative electrode current collector and a negative electrode mixture layer having a negative electrode active material formed on the negative electrode current collector.

[0104] The negative electrode active material may be a carbon material capable of absorbing and releasing lithium ions, lithium metal, silicon, or tin. A carbon material may be preferably used, and both low-crystalline carbon and high-crystalline carbon may be used as the carbon material. Representative low-crystalline carbons include soft carbon and hard carbon, and representative high-crystalline carbons include natural graphite, kish graphite, pyrolytic carbon, mesophase pitch based carbon fiber, carbon microbeads, mesophase pitches, and high-temperature fired carbons such as petroleum or coal tar pitch derived cokes. In this case, the negative electrode may contain a binder, and various types of binder polymers such as polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride, polyacrylonitrile, and polymethylmethacrylate may be used as the binder.

[0105] In addition, the negative electrode current collector is not particularly limited as long as it has conductivity without causing a chemical change in the battery, and may be, for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., aluminum-cadmium alloy, etc. In addition, the negative electrode current collector may be in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc., having fine irregularities formed on the surface, similar to the positive electrode current collector.

[0106] In this case, the positive electrode mixture layer or the negative electrode mixture layer may further include a binder resin, a conductive material, a filler, and other additives.

[0107] The binder resin is used to bind the electrode active material and the conductive material and to bind the electrode active material to the current collector. Examples of such binder resins include polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, fluororubber, and various copolymers thereof.

[0108] The conductive material is used to further improve the conductivity of the electrode active material. The conductive material is not particularly limited as long as it has conductivity without causing a chemical change in the battery, and examples of the conductive material that can be used include graphite such as natural graphite and artificial graphite, carbon black such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black, conductive fibers such as carbon fiber and metal fiber, metal powders such as carbon fluoride, aluminum, and nickel powder, conductive whiskers such as zinc oxide and potassium titanate, conductive metal oxides such as titanium oxide, and polyphenylene derivatives.

[0109] The filler is selectively used as a component for suppressing the expansion of the electrode, and is not particularly limited as long as it is a fibrous material that does not cause a chemical change in the battery, and examples of the filler include olefin polymers such as polyethylene and polypropylene; glass fiber, carbon fiber, and other fibrous materials.

[0110] In the present invention, the separator is a physical separator having a function of physically separating electrodes, and may be any separator generally used in lithium secondary batteries, and is preferably one having low resistance to ion migration of the electrolyte and excellent moisture absorption ability of the electrolyte. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, or an ethylene / methacrylate copolymer, may be used alone or in a laminated state, or a conventional porous nonwoven fabric, for example, a nonwoven fabric made of a high melting point glass fiber, a polyethylene terephthalate fiber, or the like, may be used, but is not limited thereto.

[0111] In the present invention, the electrolyte may be a non-aqueous electrolyte, and the electrolyte salt contained in the non-aqueous electrolyte is a lithium salt. The lithium salt may be any of those commonly used in electrolytes for lithium secondary batteries. For example, the lithium salt may be LiFSI, LiPF6, LiCl, LiBr, LiI, LiClO4, LiBF4, LiB 10 Cl 10 , LiPF6, LiCF3SO3, LiCF3CO2, LiAsF6, LiSbF6, LiPF6, LiAlCl4, CH3SO3Li, CF3SO3Li, (CF3SO2)2NLi, lithium chloroborane, and lithium 4-phenylborate.

[0112] The organic solvent contained in the non-aqueous electrolyte may be any organic solvent commonly used in electrolytes for lithium secondary batteries, and may be used alone or in combination of two or more of ethers, esters, amides, linear carbonates, cyclic carbonates, etc. Representative examples of the organic solvent include cyclic carbonates, linear carbonates, and carbonate compounds that are slurries thereof.

[0113] Specific examples of the cyclic carbonate compound include ethylene carbonate (EC), propylene carbonate (PC), 1,2-butylene carbonate, 2,3-butylene carbonate, 1,2-pentylene carbonate, 2,3-pentylene carbonate, vinylene carbonate, vinylethylene carbonate, and halides thereof, or a mixture of two or more of these. Examples of these halides include, but are not limited to, fluoroethylene carbonate (FEC).

[0114] In addition, specific examples of the linear carbonate compound include, but are not limited to, any one selected from the group consisting of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate, ethyl methyl carbonate (EMC), methyl propyl carbonate, and ethyl propyl carbonate, or a slurry of two or more of these. In particular, among the carbonate-based organic solvents, ethylene carbonate and propylene carbonate, which are cyclic carbonates, are high-viscosity organic solvents with high dielectric constants, and can dissociate lithium salts in the electrolyte better. If such cyclic carbonates are mixed with linear carbonates with low viscosity and low dielectric constants, such as dimethyl carbonate and diethyl carbonate, in an appropriate ratio, an electrolyte with higher electrical conductivity can be prepared.

[0115] In addition, the organic solvent may be, but is not limited to, any one or more of ethers selected from the group consisting of dimethyl ether, diethyl ether, dipropyl ether, methyl ethyl ether, methyl propyl ether, and ethyl propyl ether.

[0116] In addition, the ester in the organic solvent may be any one or two or more selected from the group consisting of methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, γ-valerolactone, γ-caprolactone, σ-valerolactone, and ε-caprolactone, but is not limited thereto.

[0117] The injection of the non-aqueous electrolyte may be performed at an appropriate stage during the manufacturing process of the electrochemical device depending on the manufacturing process and required properties of the final product, i.e., before assembly of the electrochemical device or at the final stage of assembly of the electrochemical device.

[0118] The lithium secondary battery according to the present invention can be manufactured by a lamination (stack) and folding process of the separator and the electrode in addition to a general winding process.

[0119] The shape of the battery case is not particularly limited, and may be various shapes such as a cylindrical shape, a laminated shape, a square shape, a pouch shape, a coin shape, etc. The structure and manufacturing method of these batteries are widely known in this field, so a detailed description will be omitted.

[0120] In addition, the lithium secondary battery can be classified into various types of batteries such as lithium-sulfur secondary battery, lithium-air battery, lithium-oxide battery, and lithium solid-state battery depending on the cathode / anode materials used.

[0121] The present invention also provides a battery module including the lithium secondary battery as a unit cell.

[0122] The battery module can be used as a power source for medium to large devices that require high temperature stability, long cycle characteristics, and high capacity characteristics.

[0123] Examples of the medium- to large-sized devices include, but are not limited to, power tools that are powered by battery-powered motors; electric vehicles, including electric vehicles (EVs), hybrid electric vehicles (HEVs), and plug-in hybrid electric vehicles (PHEVs); electric two-wheeled vehicles, including electric bicycles (E-bikes) and electric scooters (E-scooters); electric golf carts; and power storage systems.

[0124] In the following, preferred examples are presented to facilitate understanding of the present invention. However, the following examples are merely illustrative of the present invention, and it will be obvious to those skilled in the art that various changes and modifications are possible within the scope of the scope and technical idea of ​​the present invention, and it is natural that such changes and modifications fall within the scope of the attached claims.

[0125] Example 1 (1) MOF manufacturing 0.8g (4.2mmol) of Zn(NO3)2·6H2O and 0.149g (0.89mmol) of 1,4-benzenedicarboxylic acid (H2BDC) were placed in a 50mL container together with 30mL of N,N'-dimethylformamide (DMF). The reaction solution was heated at 120℃ in a box-type electric furnace for one day. The crystalline product was collected through a vacuum device and filter paper, and washed several times with N,N'-dimethylformamide (DMF) and chloroform (Chloroform). The product was dried in a vacuum desiccator at room temperature.

[0126] The MOF produced was MOF-5 (Zn4O(BDC)3, BDC: 1,4-benzenedicarboxylate).

[0127] (2) Core-shell structure formation (MOF-5@N-MOF-5) 2-aminoterephthalic acid, which is an organic ligand precursor containing an N element, was dissolved in DMF (N,N'-dimethylformamide), an organic solvent, to prepare a 0.01M organic ligand precursor solution.

[0128] After the organic ligand precursor solution was heated at 100 °C for 30 min, the resulting core-shell structured MOF was collected and dried (MOF-5@N-MOF-5).

[0129] (3) Carbonization The core-shell structured MOF was heat-treated in an Ar atmosphere at 1000°C for 6 h to prepare a porous carbon structure (MOF-5@N-MOF-5).

[0130] Example 2 A porous carbon structure (MOF-5@S-MOF-5) was prepared in the same manner as in Example 1, except that 2,5-dimercaptoterephthalic acid, an organic ligand precursor containing an S element, was used instead of 2-aminoterephthalic acid, an organic ligand precursor containing an N element.

[0131] Comparative Example 1 MOF-5 was carbonized in the same manner as in Example 1 to produce porous carbon (MOF-5), except that the core-shell structure was not formed.

[0132] Comparative Example 2 N-MOF-5 was carbonized in the same manner as in Example 1 to produce porous carbon (N-MOF-5), except that the core-shell structure was not formed.

[0133] Comparative Example 3 Porous carbon was prepared in the same manner as in Example 1, except that the core and shell materials were reversed (N-MOF-5@MOF-5).

[0134] Experimental Example 1 The shapes of the porous carbon structures produced in Example 1, Example 2 and Comparative Example 1 were confirmed.

[0135] FIG. 2 is a SEM (Scanning Electron Microscope, FE-SEM; JEOL, JSM-7100F) photograph of the MOFs produced in Example 1, Example 2, and Comparative Example 1, respectively.

[0136] 2, it can be seen that the porous carbon structures of Example 1, Example 2, and Comparative Example 1 are all regular hexahedrons. In addition, it can be seen that an additional layer is formed on the surface of the cubic shape in Example 1 and Example 2, which indicates that a core-shell structure is formed.

[0137] FIG. 3 is a graph (2-theta-scale) showing the results of XRD (X-ray Diffraction) analysis of the porous carbon structures prepared in Example 1 and Comparative Examples 1, 2, and 3, respectively.

[0138] Referring to FIG. 3, the main peaks (6.8°, 9.7°, 13.7°, 15.4°) of Comparative Example 1 (MOF-5) and Comparative Example 2 (N-MOF-5) are the same, and the main peaks of Example 1 (MOF-5@N-MOF-5) and Comparative Example 2 (N-MOF-5@MOF-5) are also the same, which shows that the crystal structure of the existing MOF is preserved even after the ligand exchange reaction.

[0139] FIG. 4 is an optical microscope photograph of the porous carbon structures prepared in Examples 1 and 2 and Comparative Examples 1, 2, and 3, respectively.

[0140] Referring to FIG. 4, it can be seen that the core-shell structured MOF forms after the ligand exchange reaction, Example 1 (MOF-5@N-MOF-5), Example 2 (MOF-5@S-MOF-5) and Comparative Example 3 (N-MOF-5@MOF-5), maintain the hexahedral pattern of the existing MOF forms, Comparative Example 1 (MOF-5) and Comparative Example 2 (N-MOF-5).

[0141] FIG. 5 is a graph showing the results of Fourier-transform infrared spectroscopy (FT-IR) analysis of the MOFs prepared in Example 1 and Comparative Example 1 and their raw materials.

[0142] Referring to FIG. 5, it can be seen that a core-shell structure was formed through the amide group of 2-aminoterephthalic acid, which is the organic ligand precursor of N-MOF-5 (IRMOF-3) present in Example 1 (MOF-5@N-MOF-5).

[0143] Experimental Example 2 FIG. 6 shows the results of FIB-EDS (Focused Ion Beam-Energy Dispersive X-ray Spectrometer, ZEISS, crossbeam 540) measurement of the MOF produced in Example 1.

[0144] Referring to FIG. 6, it can be seen that the inside and the surface of the MOF of Example 1 are separated, and thus a core-shell structure is formed.

[0145] In addition, the following Table 1 shows the results of elemental analysis of the core surface (Surface) and the inside of the shell (Inside) of the MOF of Example 1.

[0146] [Table 1]

[0147] As shown in Table 1, N element was detected only on the surface of the MOF, i.e., the shell. This indicates that the porous carbon structure has a core-shell structure in which the core and shell are made of different components.

[0148] Figure 7 shows the results of SEM-EDS (Scanning Electron Microscope-Energy Dispersive X-ray Spectrometer, FE-SEM; JEOL, JSM-7100F) measurement of the MOF produced in Example 2.

[0149] 7, it can be seen that the porous carbon structure of Example 2 has a core-shell structure in which a shell is formed on the surface of a cubic core. In addition, S is observed only in the shell, which indicates that the core and shell have different components, and therefore a MOF with a core-shell structure was formed. The shell is observed in a crushed form, and it can be seen that a shell made of a different component from the core was formed by distributing S elements along the crushed parts.

[0150] 8a and 8b show the results of XPS (X-ray photoelectron spectroscopy, Thermo UK, K-alpha) measurements on the porous carbon structures prepared in Examples 1 and 2, respectively.

[0151] Referring to FIG. 8a and FIG. 8b, the binding energies of the hetero elements N and S can be seen, and it can be seen that they are well doped.

[0152] Table 2 below shows the results of component analysis of the porous carbon structures produced in Example 1, Example 2 and Comparative Example 1.

[0153] [Table 2]

[0154] As shown in Table 2, in Example 1 and Example 2, 2-aminoterephthalic acid containing N and 2,5-dimercaptoterephthalic acid containing S were used as organic ligand precursors, respectively, and the composition analysis results confirmed that the contents of N and S were high, respectively.

[0155] Experimental Example 3 9a to 9c are graphs showing the results of BET analysis of the porous carbon structures prepared in the examples and comparative examples, respectively.

[0156] 9a to 9c, in Examples 1 and 2, the shell, which is the exterior of the hierarchical porous carbon structure, is doped with foreign atoms to develop micropores, and the specific surface area and pore volume of the porous carbon structure are increased compared to Comparative Example 1 due to the development of the micropores.

[0157] On the other hand, in Comparative Example 3, in which the core and shell materials were formed in the opposite manner compared to Comparative Example 2 and Example 1 rather than a hierarchical porous carbon structure, the pore volume and specific surface area were significantly reduced compared to Comparative Example 1.

[0158] The pore volumes and specific surface areas of the porous carbon structures of Examples 1 and 2 and Comparative Examples 1 to 3 are as shown in Table 3 below.

[0159] [Table 3]

[0160] Experimental Example 4 The electrochemical performance of lithium-sulfur secondary batteries was evaluated according to the morphology of the porous carbon structures used in the cathode material.

[0161] A lithium-sulfur secondary battery for evaluating electrochemical performance was fabricated as follows.

[0162] A separator was placed between the positive and negative electrodes and placed inside the case, and then an electrolyte was injected into the case to fabricate a lithium-sulfur secondary battery in the form of a CR-2032 coin cell. The positive electrode was fabricated by coating, drying, and rolling a positive electrode slurry made by mixing a positive electrode active material, a conductive material (Super P), and a binder (styrene-butadiene rubber, SBR) in a weight ratio of 80:10:10 on an Al foil, and the positive electrode active material was a sulfur-carbon composite (S loading: 70%) obtained by mixing sulfur (Sigma-Aldrich product) with a porous carbon structure using a ball mill and then heat-treating it at 155°C.

[0163] The negative electrode was made of lithium foil.

[0164] The electrolyte was prepared by dissolving 0.3M LiNO3 and 1M LiTFSi in a mixed solvent of DOL and DME (DOL:DME=1:1 (v / v)) (DOL: dioxolane, DME: dimethoxyethane).

[0165] At this time, the porous carbon structures used were those of Example 1, Comparative Example 1, Comparative Example 2, and Comparative Example 3, respectively.

[0166] Experimental Example 4-1 The fabricated lithium-sulfur secondary battery was charged and discharged at 0.1C, and the initial capacity and the discharge capacity at 14 cycles were measured, and the performance retention rate was calculated. The results are shown in Table 4 and FIG. 10.

[0167] [Table 4]

[0168] As a result, the electrochemical performance of the lithium-sulfur secondary battery including the porous carbon structure of Example 1 was found to be the best, and this was due to the fact that the porous carbon structure of Example 1 has a hierarchical core-shell structure, in particular, fine pores are developed in the shell, and the shell is doped with a different element.

[0169] Experimental Example 4-2 The manufactured lithium-sulfur secondary battery was charged and discharged at 0.1C, and the capacity after 1 cycle and 30 cycles was compared.

[0170] 11a and 11b are graphs showing the capacities of the batteries including Example 1 and Comparative Example 1 after 1 cycle and 30 cycles.

[0171] Referring to FIG. 11a and FIG. 11b, Example 1 (MOF-5@N-MOF-5) exhibits an improved initial discharge capacity compared to Comparative Example 1 (MOF-5) (initial capacity, Example 1: 939.96 mAh g ‐1 , Comparative example 1: 810.66mAh g ‐1 ).

[0172] In addition, the discharge capacity of Example 1 was higher even after 30 cycles, indicating an improved performance maintenance rate (discharge capacity after 30 cycles, Example 1: 705.62 mAh g ‐1 (75% performance maintained), Comparative Example 1: 810.66 mAh g ‐1 (73% performance maintained).

[0173] It was confirmed that the degree of electrode polarization was lower than that in Example 1.

[0174] Experimental Example 5 The NMR peaks of the porous carbon structures synthesized in the examples and comparative examples were confirmed.

[0175] The synthesized porous carbon structure crystals were dissolved in 1M NaOD (sodium deuteroxide) solution and NMR of the organic ligand was measured.

[0176] FIG. 12a is a graph showing the change in NMR peak depending on the synthesis time of the porous carbon structure of Example 1, and FIG. 12b is a graph showing the change in NMR peak in Example 1 and Comparative Examples 1, 2, and 3.

[0177] Referring to FIG. 12a, the H1 peak (*) in the BDC benzene ring of MOF-5 was maintained in the porous carbon structure (MOF-5@N-MOF-5) of Example 1, but was not found in N-MOF-5 with BDC-NH2 as the organic ligand.

[0178] In addition, it was confirmed that with the increase in the ligand exchange reaction time of MOF-5@N-MOF-5, the main H1 peaks (A, B, C) of the BDC-NH2 organic ligand of MOF-5@N-MOF-5 appeared and their magnitudes increased.

[0179] Referring to FIG. 12b, Example 1 (MOF-5@N-MOF-5) and Comparative Example 3 (N-MOF-5@MOF-5) all exhibited the main peaks (*, A, B, C) of Comparative Example 1 (MOF-5) and Comparative Example 2 (N-MOF-5), which means that ligand exchange occurred in the precursor MOF.

[0180] Experimental Example 6 The contact angles of the electrodes including the porous carbon structures of Example 1 and Comparative Example 1 were measured to determine the wetting of the electrodes with the electrolyte.

[0181] FIG. 13 is a photograph showing the contact angle measurement results of the cathodes including the porous carbon structures of Example 1 and Comparative Example 1.

[0182] Referring to FIG. 13, the negative electrode including MOF-5, which is the porous carbon structure of Comparative Example 1, is pure carbon without heteroatoms and is hydrophobic, with a water contact angle of 57.9°.

[0183] In addition, the negative electrode containing the porous carbon structure MOF-5@N-MOF-5 of Example 1 is N-doped carbon, which has improved electronegativity and hydrophilicity, and the contact angle of water was shown to be 33.3°.

[0184] The contact angle measurement results of water showed that the negative electrode containing MOF-5@N-MOF-5 in Example 1 had a low contact angle and improved polarity, which improved the wettability of the electrolyte and the binding force with lithium ions, thereby improving the battery performance.

[0185] Although the present invention has been described above based on limited examples and drawings, the present invention is not limited thereto, and it is of course possible for a person having ordinary knowledge in the technical field to which the present invention pertains to make various modifications and variations within the technical spirit of the present invention and the equivalent scope of the following claims.

Claims

1. A core-shell porous carbon structure comprising: The core comprises first MOFs (metal organic frameworks), The shell comprises a second MOF, the second MOF being doped with a different element including S.

2. 2. The porous carbon structure of claim 1, wherein the porous carbon structure has a pore volume of 1.5 cc / g to 4.5 cc / g.

3. The porous carbon structure has a specific surface area of ​​1500 m 2 / g to 3000m 2 3. The porous carbon structure according to claim 1, wherein the molecular weight of the porous carbon structure is 1 / g.

4. The porous carbon structure according to any one of claims 1 to 3, wherein the first MOF and the second MOF each contain a metal ion and an organic ligand.

5. The metal ion is Li + , Na + , K + , Rb + , Be 2+ , Mg 2+ , Ca 2+ , Sr 2+ , Ba 2+ , Sc 3+ , Y 3+ , Ti 4+ , Zr 4+ , Hf + , V 4+ , V 3+ , V 2+ , Nb 3+ , Ta 3+ , Cr 3+ , Mo 3+ , W 3+ , Mn 3+ , Mn 2+ , Re 3+ , Re 2+ , Fe 3+ , Fe 2+ , Ru 3+ , Ru 2+ , Os 3+ , Os 2+ , Co 3+ , Co 2+ , Rh 2+ , Rh + , Ir 2+ , Ir + , Ni 2+ , Ni + , Pd 2+ , Pd + , Pt 2+ , Pt + , Cu 2+ , Cu + , Ag + , Au + , Zn 2+ , Cd 2+ , Hg 2+ , Al 3+ , Ga 3+ , In 3+ , Tl 3+ , Si 4+ , Si 2+ , Ge 4+ , Ge 2+ , Sn 4+ , Sn 2+ , Pb 4+ , Pb 2+ , As 5+ , As 3+ , As + , Sb 5+ , Sb 3+ , Sb + , Bi 5+ , Bi 3+ and Bi + The porous carbon structure according to claim 4, wherein the porous carbon structure is one or more selected from the group consisting of:

6. 6. The porous carbon structure according to claim 4 or 5, wherein the organic ligand comprises at least one selected from the group consisting of halide, carboxylate, cyano, isocyanate, isothiocyanate, nitrile, pyridyl, nitroso, nitro and phosphate.

7. (S1) forming a MOF by heating a mixed solution in which a metal precursor and a first organic ligand precursor are dissolved in an organic solvent; (S2) adding a second organic ligand containing at least one of N and S to the mixed solution without adding an additional metal precursor, and heating the mixture to form a core-shell MOF; and (S3) carbonizing the core-shell MOF formed in the (S2) step.

8. The metal precursor is zinc nitrate hexahydrate (Zn(NO 3 ) 2 ・6H 2 O), zinc acetate dihydrate (Zn(CH 3 CO 2 ) 2 ・2H 2 O) and zinc sulfate hexahydrate (ZnSO 4 ・6H 2 8. The method for producing a porous carbon structure according to claim 7, wherein the porous carbon structure comprises at least one selected from the group consisting of:

9. The first organic ligand precursor may be 1,4-benzenedicarboxylic acid, benzene-1,3,5-tricarboxylic acid, 2-methylimidazole, oxalic acid, malonic acid, succinic acid, glutaric acid, o-phthalic acid, m-phthalic acid, p-phthalic acid, or the like.

9. The method for producing a porous carbon structure according to claim 7 or 8, wherein the compound contains one or more selected from the group consisting of 2-hydroxy-1,2,3-propanetricarboxylic acid, 1H-1,2,3-triazole, 1H-1,2,4-triazole and 3,4-dihydroxy-3-cyclobutene-1,2-dione.

10. The second organic ligand precursor in the step (S2) is selected from a second organic ligand precursor containing N and a second organic ligand precursor containing S, The N-containing second organic ligand precursor includes at least one selected from the group consisting of 2-aminoterephthalic acid, 4-aminophthalic acid, 4-aminoisophthalic acid, 5-aminoisophthalic acid, 2,5-diaminoterephthalic acid, 2,2'-diamino-4,4'-stilbenedicarboxylic acid, 5-cyano-1,3-benzenedicarboxylic acid, 2-methylimidazole, and 4,4',4"-s-triazine-2,4,6-triyl-tribenzoic acid; The second organic ligand precursor containing S is 2,5-disulfanylterephthalic acid (H 4 (C 8 H 2 O 4 S 2 10. The method for producing a porous carbon structure according to claim 7, wherein the porous carbon structure contains one or more compounds selected from the group consisting of 2-sulfanylterephthalic acid, 2-sulfanylterephthalic acid, and 2,5-thiophenedicarboxylic acid.

11. The method for producing a porous carbon structure according to any one of claims 7 to 10, wherein the step (S2) is performed at 35°C to 100°C for 15 minutes to 25 hours.

12. The method for producing a porous carbon structure according to any one of claims 7 to 11, wherein in the step (S3), the carbonization is performed at a temperature of 900°C to 1500°C in an inert atmosphere.

13. A positive electrode for a lithium secondary battery comprising the porous carbon structure according to any one of claims 1 to 6.

14. The positive electrode includes a positive electrode active material, The positive electrode for a lithium secondary battery according to claim 13 , wherein the positive electrode active material comprises: a sulfur-containing material; and the porous carbon structure as a sulfur carrier.

15. A lithium secondary battery comprising the positive electrode according to claim 13 or 14, a negative electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte.

Citation Information

Patent Citations

  • Method for Preparing Porous Carbon Structure

    KR1020200021214A

  • Metal organic framework, porous carbon structure comprising the same and method for preparing the same

    KR1020210001662A

  • KR2012‐0063925

  • KR2020‐0021214