Silicon carbide cladding and brazing method thereof, fuel rod and fuel assembly

JP7556150B2Active Publication Date: 2024-09-25LINGDONG NUCLEAR POWER +3
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023528566
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-11-12
Filing Date
2021-09-17
Publication Date
2024-09-25
Estimated Expiration
2041-09-17

AI Technical Summary

Benefits of technology

【0020】 本発明における炭化ケイ素被覆のろう接接合方法では、ろう接接合方法に基づき、Al及びSiを接合材料として用い、被覆管と端栓との間にAl/Si/Alの3層構造を有する接合層を形成する。これにより、SiC被覆の高強度で確実な接合を実現し、良好な耐高温性能及び耐熱水腐食性能を持たせることで、原子核応用における要求を満たす。

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The brazing method for silicon carbide cladding includes the following steps: S1: Using Al and Si as joining materials, place the joining material between a compatible cladding tube and an end plug to form an intermediate joining material having an Al / Si / Al three-layer structure, and form a joining-ready assembly together with the cladding tube and the end plug. S2: Place the joining-ready assembly in a vacuum or inert atmosphere and perform brazing, whereby the intermediate joining material forms a joining layer, integrally joining the cladding tube and the end plug. The present invention also relates to silicon carbide cladding formed by the above method, and to fuel rods and fuel assemblies including the silicon carbide cladding. The brazing method uses Al and Si as joining materials to form a joining layer having an Al / Si / Al three-layer structure between the cladding tube and the end plug. This achieves a high-strength and reliable joining of the SiC cladding, and provides good high-temperature resistance and hot water corrosion resistance, meeting the requirements for nuclear applications.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the technical field of nuclear fuel, and in particular to silicon carbide cladding and brazing methods thereof, fuel rods and fuel assemblies. [Background technology]

[0002] Silicon carbide (SiC) is a structural ceramic material that not only has excellent mechanical properties, high temperature properties, wear resistance, etc., but also has good radiation resistance, hot water corrosion resistance, and small neutron absorption cross section in the field of nuclear applications, so it is particularly prominent for its application to cladding materials in nuclear reactors. However, in order to realize the application of SiC cladding materials in the nuclear industry, the problem of bonding between the SiC cladding and the end plug must be solved.

[0003] Since the melting point of SiC ceramics is extremely high (up to 2700°C), it is difficult to achieve direct fusion bonding like with metals, and therefore it is usually necessary to add an intermediate bonding material to bond them. Relatively common bonding methods include brazing bonding, nano-penetrated transient eutectoid (NITE) bonding, solid-state diffusion bonding, MAX phase bonding, glass ceramic bonding, and precursor bonding. However, due to the characteristics of the cladding tube itself being a thin-walled, long tube, and the prerequisite that nuclear fuel is loaded into the tube before bonding the SiC cladding, it is determined that large bonding pressures and bonding temperatures cannot be applied when bonding the SiC cladding tube and the end plug. Of the above-mentioned bonding methods, the three methods of NITE phase bonding, solid-state diffusion bonding, and MAX phase bonding usually require large bonding pressures, and in particular, NITE phase bonding must be performed under high temperatures (>1800°C) and high pressures (>10MPa). Therefore, these methods are not suitable for bonding the SiC cladding tube and the end plug. On the other hand, precursor bonding can be performed at low temperatures (<1500°C) and low pressures (<1MPa), but there is a large volume shrinkage during the bonding process. This causes many pores in the bonding layer, which is unfavorable to the airtightness of the SiC coating and reduces the bonding strength. Glass ceramic bonding can be performed at low temperatures and low pressures, and the bonding strength is also high. However, SiC coatingHowever, metal brazing is not suitable for bonding SiC coatings in nuclear reactors because of its poor resistance to hot water corrosion and radiation. In contrast, metal brazing not only enables bonding at low temperatures (up to 1200°C) and low pressures (up to 0.1MPa), but also has the advantage that the brazing process involves a liquid phase. bonding layer However, the by-products generated during the brazing process, especially the brazing joint, Covering High temperature resistance, radiation resistance and hot water corrosion resistance SiC coating This is likely to affect the overall performance of the system. Summary of the Invention [Problem to be solved by the invention]

[0004] The technical problem to be solved by the present invention is to provide a method for brazing and joining a silicon carbide cladding, a silicon carbide cladding formed by the method, and a fuel rod and a fuel assembly having the silicon carbide cladding, in response to the shortcomings of the prior art described above. [Means for solving the problem]

[0005] The technical solutions adopted in the present invention to solve the technical problems are as follows:

[0006] A method for brazing a silicon carbide coating is provided, the method comprising the steps of:

[0007] S1: Using Al and Si as joining materials, an intermediate joining material having a three-layer structure of Al / Si / Al is formed by placing the joining material between a cladding tube and an end plug that are compatible with each other, and a joining-ready assembly is formed together with the cladding tube and the end plug.

[0008] S2: The joining waiting assembly is placed in a vacuum or inert atmosphere to perform brazing joining, whereby the intermediate joining material forms a joining layer to integrally join the cladding tube and the end plug.

[0009] Preferably, in step S1, the mass percentage of Si in the intermediate bonding material is 20-30%.

[0010] Preferably, in step S1, the Al is aluminum powder or aluminum foil, and the Si is silicon powder or a silicon sheet.

[0011] Preferably, in step S1, the purity of each of the Al and Si is 95 to 99%.

[0012] Preferably, in step S2, the brazing and joining is performed by increasing the temperature to 1000 to 1400° C. at a heating rate of 5 to 20° C. / min and maintaining the temperature for 0.5 to 2 hours, and the joining pressure is 0.01 to 0.1 MPa.

[0013] Preferably, in step S2, Sealed SiC coating of Leak Rate is 10 -13 ~10 -9 Pa m3 / s.

[0014] Preferably, in step S1, first, Al and Si are laminated to form an intermediate bonding material having a three-layer structure of Al / Si / Al, and then the intermediate bonding material is disposed between the cladding tube and the end plug.

[0015] Preferably, in step S1, Al is placed on the cladding tube and the end plug, and an Al layer is formed on each of the cladding tube and the end plug. Then, Si is placed on one of the Al layers to form a Si layer, and the cladding tube and the end plug are combined to stack the Al layer and the Si layer, thereby forming an intermediate bonding material having a three-layer structure of Al / Si / Al.

[0016] Preferably, in step S1, first, Al and Si are laminated on the cladding tube or the end plug to form an intermediate bonding material having a three-layer structure of Al / Si / Al on the cladding tube or the end plug, and then the cladding tube and the end plug are combined to place the intermediate bonding material between the cladding tube and the end plug.

[0017] The present invention further provides a silicon carbide coating formed by brazing and joining the silicon carbide coating according to any of the methods described above.

[0018] The present invention further provides a fuel rod comprising the silicon carbide cladding described above.

[0019] The present invention further provides a fuel assembly including the fuel rod described above. Effect of the Invention

[0020] In the brazing method of silicon carbide cladding in the present invention, Al and Si are used as the bonding materials based on the brazing method, and a bonding layer having an Al / Si / Al three-layer structure is formed between the cladding tube and the end plug, which realizes a high-strength and reliable bonding of the SiC cladding and provides good high-temperature resistance and hot water corrosion resistance, thereby meeting the requirements for nuclear applications.

[0021] The brazing method for silicon carbide coating in the present invention realizes high-strength bonding at low temperatures (<1500°C) and low pressures (<0.1MPa). In addition, the bonding technology is simple, and the requirements for bonding technology for equipment are low, resulting in cost reduction. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] The brazing method for silicon carbide cladding in the present invention is a method for brazing a silicon carbide cladding tube and a brazing material suitable for the silicon carbide cladding tube. End Plug and (b) integrally bonding the silicon carbide coating to form an integral silicon carbide coating. The brazing method may include the following steps:

[0023] S1: Using Al and Si as joining materials, an intermediate joining material having a three-layer structure of Al / Si / Al is formed by placing the joining material between a cladding tube and an end plug that are compatible with each other, and a joining-ready assembly is formed together with the cladding tube and the end plug.

[0024] The cladding tube is a silicon carbide cladding tube and the end plugs are silicon carbide end plugs.

[0025] When metal Al (aluminum) and Si (silicon) are used as the bonding material, their application form may be powder or sheet. That is, Al is aluminum powder or aluminum foil, and Si is silicon powder or silicon sheet. For example, when using powder raw materials such as Si powder and Al powder, they are first mixed in an organic solvent to form a slurry during installation, and then a corresponding layer is formed by coating or pressed to form a powder sheet.

[0026] In addition, when the purity of both Al and Si is 95 to 99%, the bonding effect is reliably guaranteed.

[0027] The Al / Si / Al three-layer structure (sandwich-like structure) of the intermediate bonding material is a laminated structure of an Al layer, a Si layer, and an Al layer, i.e., a Si layer is laminated between two Al layers.

[0028] In the intermediate bonding material, the mass percentage of Si is 20 to 30% (mass percentage of the entire intermediate bonding material), and is preferably 27%.

[0029] There are several embodiments for placing the intermediate joint material between the cladding tube and the end plug:

[0030] In the first embodiment, first, Al and Si are laminated on the outside of the cladding tube and the end plug to form an intermediate bonding material having a three-layer structure of Al / Si / Al, and then the intermediate bonding material is placed between the cladding tube and the end plug.

[0031] In the second embodiment, Al is placed on the cladding tube and the end plug, and an Al layer is formed on each of the cladding tube and the end plug. Then, Si is placed on one of the Al layers to form a Si layer, and then the cladding tube and the end plug are joined together. This forms an intermediate bonding material with a three-layer structure of Al / Si / Al by stacking the Al layer and the Si layer.

[0032] In the third embodiment, first, Al and Si are laminated on the cladding tube or the end plug to form an intermediate bonding material having a three-layer structure of Al / Si / Al on the cladding tube or the end plug, and then the cladding tube and the end plug are combined to place the intermediate bonding material between the cladding tube and the end plug.

[0033] S2: The joining-ready assembly formed in step S1 is placed in a vacuum or inert atmosphere to perform brazing and joining, whereby the intermediate joining material forms a joining layer to integrally join the cladding tube and the end plug.

[0034] The Al layer or Si layer in the intermediate bonding material is formed by mixing powder and an organic solvent to form a slurry, and then coating the slurry. Therefore, before performing brazing, the bonding-ready assembly is first dried to remove the organic solvent in the slurry.

[0035] Specifically, the assembly waiting to be joined is placed in a tube furnace, and brazing is performed under vacuum or an inert atmosphere (such as nitrogen gas or argon gas).

[0036] In brazing, the temperature is raised to 1000-1400°C at a heating rate of 5-20°C / min and kept at that temperature for 0.5-2 hours. The brazing pressure is 0.01-0.1 MPa.

[0037] After brazing, the intermediate bonding material forms a dense bonding layer that is firmly bonded between the cladding tube and the end plug. In the bonding layer, Al and Si are mixed together after being melted at high temperature during the brazing process. Therefore, the bonding layer does not show a separated layer structure of Al and Si on the cross section in the thickness direction.

[0038] In the silicon carbide cladding formed by the brazing and joining method for the silicon carbide cladding described above, the end plug is firmly joined to the cladding tube via a joining layer, thereby sealing the end opening of the cladding tube.

[0039] Sealed SiC coating of Leak Rate is 10 -13 ~10 -9The shear strength is 40-100MPa, and the high temperature shear strength at 1200℃ is 40-80MPa. Sealed SiC coating The corrosion rate of the cladding and end plugs is less than 10%.

[0040] The silicon carbide cladding of the present invention is used in a fuel assembly as a structural component of a fuel rod, specifically, the fuel rod includes the silicon carbide cladding described above and further includes fuel pellets disposed within the silicon carbide cladding.

[0041] The fuel assembly includes several of the above-mentioned fuel rods arranged in parallel at intervals, and further includes several positioning grids and the like distributed at intervals along the axial direction of the fuel rods, but the specific structural configuration and combination method are referred to in the prior art fuel assemblies.

[0042] Next, the present invention will be further described with reference to specific examples. EXAMPLES

[0043] The bonding materials were a 15μm thick metal Al foil and 1μm (grain size) Si powder. The purity of both the Al foil and the Si powder was 99%. The Si powder was dispersed in anhydrous ethanol in advance, ultrasonically dispersed for 5 minutes, and then uniformly applied onto the Al foil to form an intermediate bonding material with a layer distribution of Al / Si / Al. The ratio of Si in the intermediate bonding material was controlled to be 27wt%.

[0044] The intermediate bonding material was placed between the SiC cladding tube and the end plug to form a ready-to-bond assembly. Then, anhydrous ethanol was removed by first drying in a vacuum oven at 60°C. After drying, the ready-to-bond assembly was placed in a tube furnace and bonded under vacuum. The temperature was increased to 1200°C at 10°C / min and held for 1 h, and the pressure was applied at 0.01 MPa to produce the SiC cladding upon completion.

[0045] When measured, the sealed typeThe room temperature shear strength of the SiC coating was 100 MPa, and the high temperature shear strength at 1200°C was 80 MPa. Leak Rate is 10 -13 After hot water corrosion (400℃), Sealed SiC coating The corrosion rate of the cladding and end plugs was 5% higher. EXAMPLES

[0046] The bonding materials were 15 μm thick metal Al foil and 1 μm Si powder. The purity of both the Al foil and the Si powder was 99%. The Si powder was dispersed in anhydrous ethanol in advance, ultrasonically dispersed for 5 minutes, and then uniformly applied onto the Al foil to form an intermediate bonding material with a layer distribution of Al / Si / Al. The ratio of Si in the intermediate bonding material was controlled to be 30 wt%.

[0047] The intermediate bonding material was placed between the SiC cladding tube and the end plug to form a ready-to-bond assembly. Then, anhydrous ethanol was removed by first drying in a vacuum oven at 60°C. After drying, the ready-to-bond assembly was placed in a tube furnace and bonded under vacuum. The temperature was increased to 1200°C at 10°C / min and held for 1 h, and the pressure was applied at 0.01 MPa to produce the SiC cladding upon completion.

[0048] When measured, the sealed type The room temperature shear strength of the SiC coating was 60 MPa, and the high temperature shear strength at 1200°C was 40 MPa. Leak Rate is 10 -10 After hot water corrosion (400℃), Sealed SiC coating The corrosion rate of the cladding and end plugs was 8% higher. EXAMPLES

[0049] The bonding materials were 15 μm thick metal Al foil and 1 μm Si powder. The purity of both the Al foil and the Si powder was 99%. The Si powder was dispersed in anhydrous ethanol in advance, ultrasonically dispersed for 5 minutes, and then uniformly applied onto the Al foil to form an intermediate bonding material with a layer distribution of Al / Si / Al. The ratio of Si in the intermediate bonding material was controlled to be 25 wt%.

[0050] The intermediate bonding material was placed between the SiC cladding tube and the end plug to form a ready-to-bond assembly. Then, anhydrous ethanol was removed by first drying in a vacuum oven at 60°C. After drying, the ready-to-bond assembly was placed in a tube furnace and bonded under vacuum. The temperature was increased to 1200°C at 10°C / min and held for 1 h, and the pressure was applied at 0.01 MPa to produce the SiC cladding upon completion.

[0051] When measured, the sealed type The room temperature shear strength of the SiC coating was 80 MPa, and the high temperature shear strength at 1200°C was 60 MPa. Leak Rate is 10 -10 After hot water corrosion (400℃), Sealed SiC coating The corrosion rate of the cladding and end plugs was 6% higher. EXAMPLES

[0052] The bonding materials were a 10 μm thick metal Al foil and a 5 μm thick Si sheet. The purity of both the Al foil and the Si sheet was 99%. The Al foil and the Si sheet were laminated to form an Al / Si / Al intermediate bonding material. The ratio of Si in the intermediate bonding material was controlled to be 20 wt%.

[0053] The intermediate bonding material was placed between the SiC cladding tube and the end plug to form a bond-ready assembly. Then, anhydrous ethanol was removed by first drying in a vacuum oven at 60°C. After drying, the bond-ready assembly was placed in a tube furnace and bonded under vacuum. The temperature was increased to 1400°C at 10°C / min and held for 2 h, and the pressure was applied at 0.1 MPa to produce the SiC cladding upon completion.

[0054] When measured, the sealed type The room temperature shear strength of the SiC coating was 40 MPa, and the high temperature shear strength at 1200°C was 40 MPa. Leak Rate is 10 -9 Pa·m3 / s. After hot water corrosion, Sealed SiC coating The corrosion rate of the cladding and end plugs was 10% higher. EXAMPLES

[0055] The bonding materials were 5 μm metallic Al powder and 1 μm Si powder. The purity of both Al powder and Si powder was 99%. First, Al powder and Si powder were uniformly dispersed in anhydrous ethanol, respectively, and then coated to laminate the intermediate bonding material formed between the SiC cladding tube and the end plug. The ratio of Si was controlled to be 20 wt%.

[0056] First, the prepared bond-ready assembly was dried in a vacuum oven at 60°C to remove the anhydrous ethanol. After drying, the bond-ready assembly was placed in a tube furnace and bonded under an argon gas environment. The temperature was increased to 1000°C at 10°C / min and kept at that temperature for 1 h, and the pressure was applied at 0.1 MPa to produce a SiC coating after completion.

[0057] When measured, the sealed type The room temperature shear strength of the SiC coating was 70 MPa, and the high temperature shear strength at 1200°C was 50 MPa. Leak Rate is 10 -9 Pa·m3 / s. After hot water corrosion, Sealed SiC coating The corrosion rate of the cladding and end plugs was 10% higher. EXAMPLES

[0058] 10μmThe bonding materials were a metal Al powder of 100 μm and a Si sheet of 5 μm. The purity of both the Al powder and the Si sheet was 99%. Referring to the method of Example 5, the Al powder was uniformly mixed with anhydrous ethanol, coated, and laminated with the Si sheet to form an intermediate bonding material located between the SiC cladding tube and the end plug. The ratio of Si was controlled to be 30 wt%.

[0059] First, the prepared bond-ready assembly was dried in a vacuum oven at 60°C to remove the anhydrous ethanol. After drying, the bond-ready assembly was placed in a tube furnace and bonded under an argon gas environment. The temperature was increased to 1200°C at 10°C / min and kept at that temperature for 2 h, and the pressure was applied at 0.1 MPa, after which the SiC coating was produced.

[0060] When measured, the sealed type The room temperature shear strength of the SiC coating was 70 MPa, and the high temperature shear strength at 1200°C was 60 MPa. Leak Rate is 10 -9 Pa·m3 / s. After hot water corrosion, Sealed SiC coating The corrosion rate of the cladding and end plugs was 9% higher.

[0061] [Comparative Example 1] The bonding materials were 15 μm thick metal Al foil and 1 μm Si powder. The purity of both the Al foil and the Si powder was 99%. The Si powder was dispersed in anhydrous ethanol in advance, ultrasonically dispersed for 5 minutes, and then uniformly applied onto the Al foil to form an intermediate bonding material with a layer distribution of Al / Si / Al. The ratio of Si in the intermediate bonding material was controlled to be 10 wt%. The intermediate bonding material was placed between the SiC cladding tube and the end plug to form a ready-to-bond assembly. Then, anhydrous ethanol was removed by first drying in a vacuum oven at 60°C. After drying, the ready-to-bond assembly was placed in a tube furnace and bonded under vacuum. The temperature was increased to 1200°C at 10°C / min and held for 1 h, and the pressure was applied at 0.01 MPa to produce the SiC cladding upon completion. Created sealed typeThe room temperature shear strength of the SiC coating was 30 MPa, and the high temperature shear strength at 1200°C was 10 MPa. Leak Rate is 10 -5 The thermal conductivity was 1.0 Pa m3 / s. After hot water corrosion, the joint between the cladding tube and the end plug cracked, indicating that pores were generated in the joint layer after hot water corrosion.

[0062] [Comparative Example 2] A 15 μm thick metal Al foil and 1 μm Si powder were used as the bonding materials. The purity of both the Al foil and the Si powder was 99%. The ratio of Si in the intermediate bonding material was controlled to be 40 wt%. Then, a SiC coating was produced according to the above Comparative Example 1. Created sealed type The room temperature shear strength of the SiC coating was 20 MPa, and the high temperature shear strength at 1200°C was 20 MPa. Leak Rate is 10 -6 The thermal conductivity was 1.0 Pa m3 / s. After hot water corrosion, the joint between the cladding tube and the end plug cracked, indicating that pores were generated in the joint layer after hot water corrosion.

[0063] The above description is merely an embodiment of the present invention, and does not limit the scope of the patent of the present invention. Any equivalent structure or equivalent flow modification made by utilizing the contents of the specification of the present invention, or direct or indirect application to other related technical fields, are all included in the scope of patent protection of the present invention for the same reasons.

Claims

1. S1: Using Al and Si as a joining material, by placing the joining material between a cladding tube and an end plug that are compatible with each other, an intermediate joining material having an Al / Si / Al three-layer structure is formed, and a joining waiting assembly is formed together with the cladding tube and the end plug; S2: The joining waiting assembly is placed in a vacuum or an inert atmosphere to perform brazing and joining, so that the intermediate joining material forms a joining layer and the cladding tube and the end plug are joined together.

2. A method for brazing a silicon carbide coating comprising the steps of:

2. The method for brazing and joining silicon carbide coatings according to claim 1, characterized in that in step S1, the mass percentage of Si in the intermediate joining material is 20-30%.

3. 2. The method for brazing and joining a silicon carbide coating according to claim 1, wherein in step S1, the Al is aluminum powder or aluminum foil, and the Si is silicon powder or a silicon sheet.

4. 2. The method for brazing and joining a silicon carbide coating according to claim 1, wherein in step S1, the purity of each of the Al and Si is 95 to 99%.

5. The brazing method for silicon carbide coating according to claim 1, characterized in that in step S2, the temperature is increased to 1000 to 1400 ° C. at a heating rate of 5 to 20 ° C. / min and kept at that temperature for 0.5 to 2 h, and the bonding pressure is 0.01 to 0.1 MPa.

6. In step S2, the airtightness of the bonding layer is 10- 13 ~10- 9 2. The method of claim 1, wherein the brazing rate is Pa·m3 / s.

7. 7. The method for brazing and joining a silicon carbide coating according to claim 1, wherein in step S1, first, Al and Si are laminated to form an intermediate joining material having a three-layer structure of Al / Si / Al, and then the intermediate joining material is disposed between the coating tube and the end plug.

8. 7. The method for brazing and joining a silicon carbide coating according to claim 1, wherein in step S1, Al is placed on the cladding tube and on the end plug, and an Al layer is formed on each of the cladding tube and the end plug. Then, Si is placed on one of the Al layers to form a Si layer, and the cladding tube and the end plug are combined to overlap the Al layer and the Si layer, thereby forming an intermediate joining material having a three-layer structure of Al / Si / Al.

9. 7. The method for brazing and joining a silicon carbide coating according to claim 1, wherein in step S1, first, Al and Si are laminated on the cladding tube or the end plug, to form an intermediate joining material having a three-layer structure of Al / Si / Al on the cladding tube or the end plug, and then the cladding tube and the end plug are combined to place the intermediate joining material between the cladding tube and the end plug.

Citation Information

Patent Citations

  • A fuel cladding tube in which end plugs are sintered by discharge plasma on a SiC substrate

    JP2016531080A

  • Ceramic joined body

    JP2018104227A