Sm-Fe-N based magnetic material and its manufacturing method

By optimizing the molar ratios and adjusting lattice volume and density in Sm-Fe-N magnetic materials with elements like La, Ce, Co, and Ni, the material achieves enhanced saturation magnetization, addressing the challenges of nitrogen presence and binder use in production.

JP7556248B2Active Publication Date: 2024-09-26TOYOTA JIDOSHA KK
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2020159901
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-24
Publication Date
2024-09-26
Estimated Expiration
2040-09-24

AI Technical Summary

Technical Problem

Sm-Fe-N magnetic materials face challenges in achieving high saturation magnetization due to the presence of nitrogen, which complicates handling during production and reduces the density of the compact when sintering without using binders, leading to decreased saturation magnetization.

Method used

The Sm-Fe-N magnetic material is formulated with specific molar ratios and adjusted lattice volume and density ranges, incorporating elements like La, Ce, Co, and Ni to enhance the saturation magnetization of the main phase, while maintaining the crystal structure integrity.

Benefits of technology

The solution results in improved saturation magnetization of the main phase, achieving higher lattice volume and density within predetermined ranges, enhancing the magnetic properties of the Sm-Fe-N magnetic material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007556248000003
    Figure 0007556248000003
  • Figure 0007556248000004
    Figure 0007556248000004
  • Figure 0007556248000002
    Figure 0007556248000002
Patent Text Reader

Abstract

To provide an Sm-Fe-N-based magnetic material and a method for manufacturing it, in which a magnetism-expressing main phase shows improved saturation magnetization of its own compared with a conventional one.SOLUTION: A magnetic material includes a main phase having a predetermined crystal structure. The main phase has a composition represented by (Sm(1-x-y-z)LaxCeyR1z)2(Fe(1-p-q-s)CopNiqMs)17 Nh (where, R1 is a predetermined rare earth element or the like, M is a predetermined element, and 0≤x+y<0.04, 0≤z≤0.10, 0<p+q≤0.10, 0≤s≤0.10, and 2.9≤h≤3.1 are satisfied). The main phase has a lattice volume of 0.830 to 0.840 nm3 and a density of 7.7 to 8.0 g / cm3. A method of manufacturing the magnetic material includes nitriding a magnetic material precursor including a crystal phase having a composition represented by (Sm(1-x-y-z)LaxCeyR1z)2(Fe(1-p-q-s)CopNiqMs)17.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to an Sm-Fe-N based magnetic material and a method for producing the same. 17 Type and Th2Ni 17 The present invention relates to an Sm-Fe-N based magnetic material having a main phase with at least one of the crystal structures of the above types, and a method for producing the same. [Background technology]

[0002] As high-performance magnetic materials, Sm-Co magnetic materials and Nd-Fe-B magnetic materials have been put to practical use, but in recent years, other magnetic materials have been under study. For example, Th2Zn 17 Type and Th2Ni 17 Sm-Fe-N based magnetic materials (hereinafter sometimes simply referred to as "Sm-Fe-N based magnetic materials") having a main phase with at least one of the above crystal structures have been investigated.

[0003] Sm-Fe-N magnetic materials are Th2Zn 17 Type and Th2Ni 17 The main phase has at least one of the following crystal structures: Sm-Fe-based crystal phase with nitrogen interstitially introduced therein.

[0004] Patent Document 1 discloses a method for producing an Sm-Fe-N based magnetic material, which comprises reducing an oxide containing Sm, Fe, La, and W, and nitriding the reduced product to obtain an Sm-Fe-N based magnetic material. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2017-117937 A Summary of the Invention [Problem to be solved by the invention]

[0006] Compared with Sm-Co magnetic materials and Nd-Fe-B magnetic materials, Sm-Fe-N magnetic materials have a very high coercive force. However, since Sm-Fe-N magnetic materials contain nitrogen (N), it is not possible to handle intermediate products, etc., during their production at a temperature at which nitrogen (N) is released. In particular, when obtaining a compact from a powdered Sm-Fe-N magnetic material (hereinafter sometimes referred to as "Sm-Fe-N magnetic material powder"), it is difficult to obtain a compact without using a binder.

[0007] One method for obtaining a compact from powder is the sintering method. The sintering method involves heating the powder at high temperature for a long period of time to bake and solidify the powder. If the powder does not decompose when heated to high temperature, it can be baked (sintered) without using a binder. By baking (sintering) the powder in this way, the density of the sintered body can be improved because no binder is used.

[0008] When obtaining a compact from magnetic material powder, if the magnetic material powder can be sintered without using a binder, the density of the compact (sintered body) can be improved, and the saturation magnetization of the compact can be improved. However, since the Sm-Fe-N magnetic material contains nitrogen (N), when obtaining a compact, the powder of the Sm-Fe-N magnetic material cannot be heated to a temperature higher than the temperature at which nitrogen (N) is released. For this reason, a resin binder or a low-melting metal or alloy binder is generally used to obtain a compact of the Sm-Fe-N magnetic material powder. Therefore, the saturation magnetization of the compact of the Sm-Fe-N magnetic material powder decreases by the amount of the binder content.

[0009] When obtaining a compact from Sm-Fe-N based magnetic material powder, attempts have been made to reduce the content of the binder to improve the saturation magnetization of the compact, and certain results have been achieved, but this alone is not necessarily sufficient. From this, the inventors have found the problem that an improvement in the saturation magnetization of the main phase itself that exhibits magnetism is desired in the Sm-Fe-N based magnetic material. In this specification, unless otherwise specified, "saturation magnetization" shall mean the saturation magnetization at room temperature.

[0010] The present disclosure has been made to solve the above problems. That is, an object of the present disclosure is to provide an Sm-Fe-N based magnetic material and a method for manufacturing the same in which the saturation magnetization of the main phase itself that exhibits magnetism is improved as compared with the prior art.

Means for Solving the Problems

[0011] The inventors have intensively studied to achieve the above object and completed the Sm-Fe-N based magnetic material and the method for manufacturing the same of the present disclosure. The Sm-Fe-N based magnetic material and the method for manufacturing the same of the present disclosure include the following aspects. 〈1〉An Sm-Fe-N based magnetic material including a main phase having at least one crystal structure of the Th2Zn 17 type and the Th2Ni 17 type, wherein the main phase has a composition represented by the molar ratio formula (Sm (1-x-y-z) La x Ce y R 1 z )2(Fe (1-p-q-s) Co p Ni q M s ) 17 N h (wherein R 1 is one or more rare earth elements other than Sm, La, and Ce and Zr, M is one or more elements other than Fe, Co, Ni, and rare earth elements and inevitable impurity elements, and 0 ≦ x + y < 0.04, 0 ≦ z ≦ 0.10, 0 < p + q ≦ 0.10, 0 ≦ s ≦ 0.10, and 2.9 ≦ h ≦ 3.2 is satisfied.). The lattice volume of the main phase is 0.830 to 0.840 nm 3 and the density of the main phase is 7.70 to 8.00 g / cm 3 Sm-Fe-N based magnetic material . 〈2〉The Sm-Fe-N based magnetic material according to item 〈1〉, wherein the volume fraction of the main phase is 95 to 100%. 〈3〉The Sm-Fe-N based magnetic material according to item 〈1〉 or 〈2〉, wherein the lattice volume of the main phase is 0.833 to 0.835 nm 3 . 〈4〉The Sm-Fe-N based magnetic material according to any one of items 〈1〉 to 〈3〉, wherein the density of the main phase is 7.70 to 7.90 g / cm 3 . 〈5〉A method for manufacturing the Sm-Fe-N based magnetic material according to item 〈1〉, comprising preparing a magnetic material precursor having a crystal phase represented by the molar ratio formula (Sm (1-x-y-z) La x Ce y R 1 z )2(Fe (1-p-q-s) Co p Ni q M s ) 17 (wherein R 1 is one or more rare earth elements other than Sm, La, and Ce and Zr, M is one or more elements other than Fe, Co, Ni, and rare earth elements and inevitable impurity elements, and 0 ≦ x + y < 0.04, 0 ≦ z ≦ 0.10, 0 < p + q ≦ 0.10, and 0 ≦ s ≦ 0.10 are satisfied), and nitriding the magnetic material precursor . 〈6〉The method according to item 〈5〉, wherein the volume fraction of the crystal phase is 95 to 100%. 〈7〉The method according to item 〈5〉 or 〈6〉, wherein after pulverizing the magnetic material precursor to obtain a magnetic material precursor powder, the magnetic material precursor powder is nitrided. <8> The method according to any one of <5> to <7>, further comprising melting and solidifying a raw material containing elements constituting the magnetic material precursor to obtain the magnetic material precursor. Effect of the Invention

[0012] According to the present disclosure, it is possible to provide an Sm-Fe-N based magnetic material in which the lattice volume and density of the main phase are each within a predetermined range, and the saturation magnetization of the main phase itself is improved compared to conventional materials.

[0013] Furthermore, according to the present disclosure, it is possible to provide a method for producing an Sm-Fe-N based magnetic material in which the lattice volume and density of the main phase are each set within a predetermined range by nitriding a magnetic material precursor, thereby improving the saturation magnetization of the main phase itself compared to conventional methods. [Brief description of the drawings]

[0014] [Figure 1] FIG. 1 is a graph showing the relationship between lattice volume and saturation magnetization Ms (300 K). [Diagram 2] FIG. 2 is a graph showing the relationship between lattice volume and density. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Hereinafter, embodiments of the Sm-Fe-N based magnetic material and the manufacturing method thereof according to the present disclosure will be described in detail. Note that the Sm-Fe-N based magnetic material and the manufacturing method thereof according to the present disclosure are not limited to the embodiments described below.

[0016] Without being bound by theory, the reason why the saturation magnetization of the main phase itself is improved in the Sm-Fe-N magnetic material of the present disclosure will be explained below.

[0017] Magnetic materials containing rare earth elements (hard magnetic materials) may exhibit strong magnetic force by combining mainly with Fe, or mainly with Co, depending on the type of rare earth element. As for Sm, there are cases where it exhibits strong magnetic force by combining mainly with Fe, and cases where it exhibits strong magnetic force by combining mainly with Co.

[0018] When Sm is mainly bonded with Co to exhibit a strong magnetic force, the main phase that exhibits a strong magnetic force has a CaCo5 type crystal structure. A main phase having a CaCo5 type crystal structure is typically the SmCo5 phase. The SmCo5 phase exhibits a strong magnetic force when magnetized. On the other hand, when Sm is mainly bonded with Fe to exhibit a strong magnetic force, the main phase that exhibits a strong magnetic force is the Th2Zn 17 Type and Th2Ni 17 It has at least one of the crystal structures of the Th2Zn type. 17 Type and Th2Ni 17 The main phase having at least one of the crystal structures of the type SmFe is typically 17 N3 phase. Sm2Fe 17 The N3 phase is Sm2Fe 17 N is interstitially introduced into the phase. Sm2Fe 17 Even if the phase is magnetized, it does not exhibit a strong magnetic force. 17 The phase is nitrided to Sm2Fe 17 When the N3 phase is formed, a strong magnetic force is generated by magnetization.

[0019] Conventionally, Sm2Fe 17It has been considered to replace a part of Sm in the N3 phase with inexpensive light rare earth elements such as La and Ce, and / or to replace a part of Fe with Co. However, in order to improve the economic efficiency by replacing a part of Sm with inexpensive light rare earth elements, it is necessary to make the substitution rate of the light rare earth elements at a certain level or higher, and it has been thought that it is inevitable that the saturation magnetization of the main phase will decrease. In addition, when a part of Fe is replaced with Co, the Curie temperature of the main phase increases, so that the decrease in saturation magnetization at high temperatures (403 to 473 K) can be suppressed, but it has been thought that the effect requires a substitution rate of Ce of about 0.1 to 0.4 moles.

[0020] Under these circumstances, the present inventors have developed SmFe 17 In order to improve the N3 phase and obtain a main phase with excellent saturation magnetization at room temperature, the inventors focused on the lattice volume and density of the main phase. Conventionally, it has been thought that the lattice volume and density of the main phase are inversely proportional to each other, but the inventors have found that the saturation magnetization of the main phase is improved when the density is higher than the inversely proportional relationship within a certain lattice volume range. The inventors have also found that in order to obtain a lattice volume and density that improves the saturation magnetization of the main phase, it is good to replace a part of Fe with a small amount of Co and / or Ni, and optionally replace a part of Sm with a small amount of La and / or Ce. Here, "a small amount" means a smaller amount than the amount of light rare earth element when a part of Sm is replaced with a light rare earth element for improving economy, and also means a smaller amount than the amount of Co when a part of Fe is replaced with Co for increasing the Curie temperature.

[0021] Next, the constituent elements of the Sm-Fe-N based magnetic material and the manufacturing method thereof according to the present disclosure, which have been completed based on the findings and the like described above, will be described.

[0022] 《Sm-Fe-N magnetic material》 The Sm-Fe-N magnetic material of the present disclosure is Th2Zn 17 Type and Th2Ni 17The Sm-Fe-N based magnetic material of the present disclosure exhibits magnetism due to the main phase. The main phase will be described below.

[0023] <Crystal structure of the main phase> The main phase is Th2Zn 17 Type and Th2Ni 17 The main phase has at least one of the crystal structures of the above-mentioned types. The crystal structure of the main phase may include a TbCu7 type crystal structure in addition to the above-mentioned structures. Here, Th is thorium, Zn is zinc, Ni is nickel, Tb is terbium, and Cu is copper. The crystal structure of the main phase can be identified by subjecting the Sm-Fe-N magnetic material to, for example, X-ray diffraction analysis.

[0024] A phase having the above-mentioned crystal structure can be achieved by various element combinations (compositions), but the main phase of the Sm-Fe-N magnetic material of the present disclosure is achieved by the following element combination (composition): The composition of the main phase of the Sm-Fe-N magnetic material of the present disclosure will be described below.

[0025] <Composition of the main phase> The main phase is represented by the molar ratio formula (Sm (1-x-y-z) La x Ce y R 1 z )2(Fe (1-p-q-s) Co p Ni q M s ) 17 N h In the above formula, Sm is samarium, La is lanthanum, Ce is cerium, Fe is iron, Co is cobalt, and Ni is nickel. 1 is one or more rare earth elements other than Sm, La, and Ce, and Zr, and M is one or more elements other than Fe, Co, Ni, and rare earth elements, and unavoidable impurity elements. Zr is zirconium. In the above formula, for the sake of convenience, Sm (1-x-y) La x Ce y R 1 z rare earth site, Fe(1-p-q-s) Co p Ni q M s are sometimes called iron group sites.

[0026] As can be seen from the above formula, the main phase contains 2 moles of one or more elements in the rare earth site, 17 moles of one or more elements in the iron group site, and h moles of nitrogen (N). In other words, a phase having the above-mentioned crystal structure is constituted by one or more elements in the rare earth site and one or more elements in the iron group site, and h moles of nitrogen (N) are introduced interstitially into the phase. The amount of introduced nitrogen (N) is h moles (where h is 2.9 to 4.0 moles). 3.2 ) can maintain the above-mentioned crystal structure. Details of nitrogen (N) in the main phase will be described later.

[0027] The rare earth sites are Sm, La, Ce, and R. 1 Sm, La, Ce, and R 1 Each of them exists in a molar ratio of (1-xyz):x:y:z. Since (1-xyz)+x+y+z=1, a part of Sm is present in La, Ce, and R. 1 It means that the group consisting of one or more elements is substituted.

[0028] The iron group site consists of Fe, Co, Ni, and M, and Fe, Co, Ni, and M are present in a molar ratio of (1-pqs):p:q:s. Since (1-pqs)+p+q+s=1, this means that a portion of Fe is substituted with one or more elements selected from the group consisting of Co, Ni, and M.

[0029] The elements constituting the above formula and their content ratios (molar ratios) will be explained below.

[0030] <Sm> Sm is a major element that constitutes the above-mentioned crystal structure together with Fe and N. A part of Sm is mixed with La, Ce, and R. 1 Hereinafter, La, Ce, and R are substituted with one or more elements selected from the group consisting of1 This article explains:

[0031] 〈La〉 La is substituted for a part of Sm, and contributes to the change in lattice volume and density of the main phase, especially the lattice volume. Since the ionic radius of La is much larger than that of Sm, when a part of Sm is substituted with La, the lattice volume of the main phase basically increases. However, due to the variation in the degree of penetration of nitrogen (N) introduced interstitially into the main phase during nitriding, when the amount of substitution by La is small, the lattice volume of the main phase may decrease.

[0032] As mentioned above, the ionic radius of La is much larger than that of Sm. Therefore, when a part of Sm is replaced with La, it has a large effect on the change in the lattice volume of the main phase. When the lattice volume of the main phase exceeds a certain range, the above-mentioned crystal structure cannot be maintained, or even if the above-mentioned crystal structure can be maintained, the magnetic properties, especially the saturation magnetization, deteriorate. In order to prevent this, when a part of Sm is replaced with La, it is essential not to make the substitution rate of La excessively high.

[0033] La belongs to the so-called light rare earth elements, and compared to Sm, it has large reserves (resources) and is inexpensive. Therefore, by substituting a portion of Sm with La, the amount of Sm used can be reduced, which is advantageous in improving economy.

[0034] <Ce> Ce is substituted for a part of Sm and contributes to the change in the lattice volume and density of the main phase, especially the lattice volume. Since the ionic radius of Ce is slightly larger than that of Sm, substituting a part of Sm with Ce basically increases the lattice volume of the main phase. However, because Ce ions can be trivalent or tetravalent, and there is variation in the degree of penetration of nitrogen (N) introduced interstitially into the main phase during nitriding, substituting a part of Sm with Ce may increase or decrease the lattice volume of the main phase.

[0035] As described above, the ionic radius of Ce is slightly larger than that of Sm. Therefore, even if a part of Sm is replaced with Ce, the effect on the change in the lattice volume of the main phase is small. Therefore, when changing the lattice volume of the main phase, the substitution rate of Ce is relatively high when a part of Sm is replaced with Ce compared to when a part of Sm is replaced with La.

[0036] Ce belongs to the so-called light rare earth elements, and compared to Sm, it has a large reserve (resource amount) and is inexpensive. Therefore, by substituting a part of Sm with Ce, the amount of Sm used can be reduced, which is economical.

[0037] <R 1 〉 R 1 R is one or more rare earth elements other than Sm, La, and Ce, and Zr. 1 R is one or more elements that may be contained within a range that does not impair the magnetic properties of the Sm-Fe-N magnetic material of the present disclosure. 1 Typically, R is one or more rare earth elements other than Sm, La, and Ce that are difficult to completely separate from Sm, La, and Ce when refining raw materials containing these elements, and remain in small amounts in the raw materials. 1 may contain Zr. Although Zr is not a rare earth element, a part of Sm may be substituted with Zr. Even if a part of Sm is substituted with Zr, as long as the amount of substitution is small, the magnetic properties of the Sm-Fe-N magnetic material are not significantly impaired.

[0038] In this specification, the rare earth elements consist of 17 elements: Sc (scandium), Y (yttrium), La (lanthanum), Ce (cerium), Pr (praseodymium), Nd (neodymium), Pm (promethium), Sm (samarium), Eu (eurobium), Gd (gadolinium), Tb (terbium), Dy (dysprosium), Ho (holmium), Er (erbium), Tm (thulium), Yb (ytterbium), and Lu (ruthenium).

[0039] <Fe> Fe is a main element that constitutes the above-mentioned crystal structure together with Sm and N. A part of Fe may be substituted with one or more elements selected from the group consisting of Co, Ni, and M. Co, Ni, and M will be described below.

[0040] <Co> Co is substituted for part of Fe and contributes to changes in the lattice volume and density of the main phase. Since the ionic radius of Co is smaller than that of Fe, substituting part of Fe with Co basically reduces the lattice volume of the main phase. However, due to variations in the degree of penetration of nitrogen (N) interstitially introduced into the main phase during nitriding, substituting part of Fe with Co may increase or decrease the lattice volume of the main phase.

[0041] Substituting a portion of Fe with Co is advantageous because it increases the Curie temperature of the main phase and makes it possible to suppress the decrease in saturation magnetization at high temperatures (403 to 473 K).

[0042] 〈Ni〉 Ni is substituted for part of Fe and contributes to changes in the lattice volume and density of the main phase. Since the ionic radius of Ni is smaller than that of Fe, substituting part of Fe with Ni basically reduces the lattice volume of the main phase. However, due to variations in the degree of penetration of nitrogen (N) interstitially introduced into the main phase during nitriding, substituting part of Fe with Ni may increase or decrease the lattice volume of the main phase.

[0043] Compared to Fe, Ni has a smaller contribution to magnetization. Therefore, it was previously thought that substituting part of the Fe in the main phase with Ni would result in a decrease in magnetic properties. However, since the ionic radius of Ni is smaller than that of Co, the lattice volume of the main phase is significantly reduced when part of the Fe is substituted with Ni, even if the Ni substitution rate is not so high, compared to when part of the Fe is substituted with Co. As a result, the magnetic properties, especially the saturation magnetization, are improved due to the significant change in the lattice volume of the main phase, rather than the decrease in magnetic properties due to the substitution of part of the Fe with Ni.

[0044] <M> M is one or more elements other than Fe, Co, Ni, and rare earth elements, and unavoidable impurity elements. M is one or more elements and unavoidable impurity elements that are permitted to be contained within a range that does not impair the magnetic properties of the Sm-Fe-N magnetic material of the present disclosure. The unavoidable impurity elements are elements whose inclusion must be avoided during the production, etc., of the Sm-Fe-N magnetic material of the present disclosure. Can Impurity elements that are not necessary or that would cause a significant increase in manufacturing costs to avoid are referred to as unavoidable impurity elements. Examples of such unavoidable impurity elements include impurity elements in raw materials, and elements such as Cu (copper), Zn (zinc), Ga (gallium), Al (aluminum), and B (boron) that diffuse and / or penetrate into the surface of the main phase when forming a bonded compact. Other examples include elements contained in a lubricant used during molding that diffuse and / or penetrate into the surface of the main phase. The bonded compact will be described later.

[0045] Examples of M excluding unavoidable impurity elements include one or more elements selected from the group consisting of Ti (titanium), Cr (chromium), Mn (manganese), V (vanadium), Mo (molybdenum), W (tungsten), and C (carbon). These elements form nuclei during the generation of the main phase, and contribute to promoting refinement of the main phase and / or suppressing grain growth of the main phase.

[0046] Also, Zr may be included as M. As mentioned above, Zr is not a rare earth element, but a part of Sm may be substituted with Zr, while a part of Fe may be substituted with Zr. In either case, if the amount of substitution is small, the magnetic properties of the Sm-Fe-N magnetic material are not significantly impaired.

[0047] <N> N is introduced interstitially into the main phase having the above-mentioned crystal structure. By introducing N to an extent that does not destroy the phase having the above-mentioned crystal structure, a magnetic moment appears in the main phase.

[0048] When the main phase of the Sm-Fe-N magnetic material of the present disclosure is composed of the elements described above and the lattice volume and density of the main phase are within predetermined ranges, a desired saturation magnetization can be obtained. The lattice volume and density will be described below.

[0049] <Lattice volume> The lattice volume of the main phase of the Sm-Fe-N magnetic material of the present disclosure is 0.830 to 0.840 nm 3 When the lattice volume of the main phase is in the above-mentioned range and, in addition, the density of the main phase is in the range described below, a desired saturation magnetization can be obtained.

[0050] Without being bound by theory, the reason why the lattice volume of the main phase needs to be within the above-mentioned range in order to obtain a desired saturation magnetization is believed to be as follows.

[0051] As mentioned above, the saturation magnetization of Sm-Fe-N magnetic materials is derived from the magnetic moment that appears in the main phase due to the introduction of N in an interstitial manner into the main phase. For this reason, the saturation magnetization is significantly affected by the Fe-N distance in the lattice of the main phase (hereinafter, sometimes simply referred to as the "Fe-N distance"). Since Fe and N are arranged three-dimensionally in the lattice of the main phase, the lattice volume of the main phase is convenient for grasping the Fe-N distance.

[0052] In the Sm-Fe-N magnetic material of the present disclosure, a portion of Fe is substituted with Co and / or Ni, and optionally a portion of Sm is substituted with La and / or Ce, thereby forming SmFe 17 The lattice volume of the N3 phase is changed. At this time, the Fe-N distance in the lattice of the main phase is changed to Sm2Fe 17 It is considered best to approximate the Fe-N distance in the lattice of the N3 phase. 17 The lattice volume of the N3 phase is approximately 0.838 nm 3 Therefore, the lattice volume of the main phase of the Sm-Fe-N magnetic material of the present disclosure is set to 0.838 nm 3 From this viewpoint, it is considered that the lattice volume of the main phase of the Sm-Fe-N based magnetic material of the present disclosure is close to 0.830 nm 3 Above, 0.831nm 3 Above, 0.832nm 3 Above, 0.833nm 3 or more than 0.834 nm 3 or more, 0.840 nm 3 Below, 0.839nm 3 Below, 0.838nm 3 Below, 0.837nm 3 Below, 0.836nm 3 Less than or equal to 0.835 nm 3 It may be the following:

[0053] The lattice volume of the main phase can be obtained as follows. The Sm-Fe-N magnetic material is subjected to X-ray diffraction analysis, and the a-axis length and the c-axis length are obtained from the X-ray diffraction pattern based on the relationship between the plane index and the lattice spacing value (d value). When obtaining the a-axis length and the c-axis length, since the main phase of the Sm-Fe-N magnetic material of the present disclosure has the above-mentioned crystal structure, it may be assumed that the main phase is a rhombohedron. Therefore, the plane indexes that can be used are the (202) plane, the (113) plane, the (104) plane, the (211) plane, the (122) plane, and the (300) plane. Then, the lattice volume is calculated according to the following formula. (Lattice volume) = {(a-axis length) / 2} 2 x6x3 0.5 ×{(c-axis length) / 3}

[0054] <Density of the main phase> Usually, the lattice volume and density of the crystal phase are inversely proportional to each other. However, in the Sm-Fe-N magnetic material of the present disclosure, the density is higher than the inversely proportional relationship between the lattice volume and density of the main phase. At such a density, the saturation magnetization of the main phase is Sm2Fe 17 The saturation magnetization is higher than that of the N3 phase. It has been experimentally confirmed that such a density is obtained when the lattice volume of the main phase is within the above-mentioned range and a part of Fe is substituted with a small amount of Co and / or Ni. It has also been confirmed that a part of Sm may be substituted with La and / or Ce, if desired. The "small amount" is as already explained. Specifically, x+y is 0 or more, 0.01 or more, or 0.02 or more, and less than 0.04 or 0.03 or less. The value of p+q is 0.01 or more, 0.02 or more, or 0.03 or more, and 0.05 or less, or 0.04 or less.

[0055] The density of the main phase is 7.70 g / cm 3 More than 7.71g / cm 3 Above, 7.73g / cm 3 More than 7.75g / cm 3 More than 7.77g / cm 3 Above, 7.79g / cm 3 More than 7.80g / cm 3 More than 7.81g / cm 3 Above, 7.83g / cm 3 More than 7.85g / cm 3 or more than 7.87 g / cm 3 or more, and 3 Below, 7.98g / cm 3 Below, 7.96g / cm 3 Below, 7.94g / cm 3 Below, 7.92g / cm 3 or less than 7.90 g / cm 3 It may be the following:

[0056] The density of the main phase is obtained by pulverizing the Sm-Fe-N magnetic material to obtain a powder, and measuring the density of the powder by a pycnometer method. As described above, in the Sm-Fe-N magnetic material of the present disclosure, the volume fraction of the main phase is preferably 95%. 17 The densities of the N3 and SmFe3 phases are 7.65 g / cm 3 and 8.25 g / cm 3 Therefore, the density of the main phase can be approximated by the value obtained by the above-mentioned measurement method.

[0057] In the Sm-Fe-N magnetic material of the present disclosure, a portion of Fe is substituted with Co and / or Ni, and optionally a portion of Sm is substituted with La and / or Ce, so that the lattice volume and density of the main phase are within the above-mentioned ranges. (1-x-y-z) La x Ce y R 1 z )2(Fe (1-p-q-s) Co p Ni q M s ) 17 N h The following will be explained using the following.

[0058] 〈x+y〉 In the above formula representing the composition of the main phase, the value of x indicates the proportion (molar ratio) of a portion of Sm substituted with La, and the value of y indicates the proportion (molar ratio) of a portion of Sm substituted with Ce.

[0059] The lattice volume of the main phase is changed by substituting part of Fe with Co and / or Ni, and optionally, part of Sm may be substituted with La and / or Ce to change the lattice volume of the main phase. For this reason, the value of x+y may be 0 or more, 0.01 or more, or 0.02 or more. On the other hand, if the value of x+y is less than 0.04 or 0.03 or less, the lattice volume of the main phase does not change excessively, in particular does not increase excessively.

[0060] Also, while the value of x+y satisfies the above-mentioned range, the value of x may be 0 or more, 0.01 or more, or 0.02 or more, and may be less than 0.04 or 0.03 or less. Similarly, while the value of x+y satisfies the above-mentioned range, the value of y may be 0 or more, 0.01 or more, or 0.02 or more, and may be less than 0.04 or 0.03 or less.

[0061] <z> In the above formula that represents the composition of the main phase, z is a part of Sm that is R. 1 As mentioned above, R 1 is one or more rare earth elements and Zr that are permitted to be contained within a range that does not impair the magnetic properties of the Sm-Fe-N magnetic material of the present disclosure. For this reason, z may be 0.10 or less, 0.08 or less, 0.06 or less, 0.04 or less, or 0.02 or less. On the other hand, when the Sm-Fe-N magnetic material of the present disclosure has R 1 In other words, z may be 0. However, when producing the Sm-Fe-N based magnetic material of the present disclosure, the raw material may contain R. 1 From this viewpoint, z may be 0.01 or more.

[0062] <p+q> In the above formula representing the composition of the main phase, the value of p indicates the proportion (molar ratio) of part of Fe substituted with Co, and the value of q indicates the proportion (molar ratio) of part of Fe substituted with Ni.

[0063] As described above, a part of Fe is substituted with Co and / or Ni to change the lattice volume of the main phase. If the value of p+q exceeds 0, the lattice volume of the main phase changes. From this viewpoint, the value of p+q may be 0.01 or more, 0.02 or more, or 0.03 or more. On the other hand, if the value of p+q is 0.10 or less, the lattice volume of the main phase does not change excessively. From this viewpoint, the value of p+q may be 0.09 or less, 0.08 or less, 0.07 or less, 0.06 or less, 0.05 or less, or 0.04 or less.

[0064] Also, while the value of p+q satisfies the above-mentioned range, the value of p may be greater than 0, 0.01 or more, 0.02 or more, or 0.03 or more, and may be 0.10 or less, 0.09 or less, 0.08 or less, 0.07 or less, 0.06 or less, 0.05 or less, or 0.04 or less. Similarly, while the value of p+q satisfies the above-mentioned range, the value of q may be greater than 0, 0.01 or more, 0.02 or more, or 0.03 or more, and may be 0.10 or less, 0.09 or less, 0.08 or less, 0.07 or less, 0.06 or less, 0.05 or less, or 0.04 or less.

[0065] 〈s〉 In the above formula representing the composition of the main phase, s indicates the ratio (molar ratio) of Fe partially substituted with M. As described above, M is one or more elements and inevitable impurity elements that are permitted to be contained within a range that does not impair the magnetic properties of the Sm-Fe-N magnetic material of the present disclosure. For this reason, s may be 0.10 or less, 0.08 or less, 0.06 or less, 0.04 or less, or 0.02 or less. On the other hand, the Sm-Fe-N magnetic material of the present disclosure may not contain M at all, that is, s may be 0, but it is difficult to completely prevent M from containing inevitable impurity elements. From this viewpoint, s may be 0.01 or more.

[0066] 〈Relationship between x, y, z, p, q, and s〉 x, y, z, p, q, and s are appropriately determined so that the lattice volume and density of the main phase are within the above-mentioned ranges while satisfying the conditions for x, y, z, p, q, and s described above. In this case, x, y, p, and q preferably satisfy the relationship of the following formula (1). 830≦16.267x+3.927y-26.279p-56.5327q+836≦840...Formula (1)

[0067] The reason why it is preferable that x, y, p, and q satisfy the formula (1) will be explained below.

[0068] In formula (1), the relational expression between the inequality signs, "16.267x+3.927y-26.279p-56.5327q+836", represents the lattice volume of the main phase with x, y, p, and q. This relational expression was derived by machine learning from Sm2Fe 17 This shows the results of calculating the lattice volume of the main phase when part of Sm is replaced with La and / or Ce and part of Fe is replaced with Co and / or Ni for the N3 phase. Hereinafter, the part between the inequality signs in formula (1), "16.267x+3.927y-26.279p-56.5327q+836", may be referred to as the "relationship representing the lattice volume of the main phase".

[0069] Then, formula (1) indicates that the "relationship that expresses the lattice volume of the main phase" is 830 to 840 cubic angstroms (0.830 to 0.840 nm 3 As described above, the lattice volume of the main phase of the Sm-Fe-N magnetic material of the present disclosure is in the range of 0.830 to 0.840 nm 3 This means that it is preferable that the composition of the main phase of the Sm—Fe—N based magnetic material of the present disclosure is such that s, y, p, and q satisfy formula (1).

[0070] In the "relationship that expresses the lattice volume of the main phase", R 1 The reason for not including z with respect to and s with respect to M is as follows.

[0071] R 1 and M are one or more elements that are permitted to be contained within a range that does not impair the magnetic properties of the Sm-Fe-N magnetic material of the present disclosure. Since there is a close relationship between the magnetic properties and the lattice volume of the main phase, the influence on the lattice volume of the main phase is small within a range that does not impair the magnetic properties of the Sm-Fe-N magnetic material of the present disclosure, and there is little need to consider z and s. Therefore, z and s are not taken into consideration in the "relationship expression representing the lattice volume of the main phase."

[0072] As described above, the "relational equation expressing the lattice volume of the main phase" was obtained by machine learning, and it has the following technical significance and is considered to be highly reliable.

[0073] First, when x=y=p=q=0, it means that a part of Sm is not substituted with La and / or Ce, and a part of Fe is not substituted with Co and / or Ni. That is, SmFe 17 The lattice volume of the N3 phase is 836 cubic angstroms (0.836 nm 3 ) in the actual Sm2Fe 17 The lattice volume of the N3 phase is approximately 0.838 nm 3 Therefore, the relational expression expressing the lattice volume of the main phase, SmFe 17 It can be seen that the lattice volume values ​​of the N3 phase are very close to the actual values.

[0074] The ratio of the coefficients x and y (16.267:3.927) is close to the ratio of the ionic radius of La to that of Ce, and the ratio of the absolute values ​​of the coefficients p and q (26.279:56.5327) is close to the ratio of the ionic radius of Co to that of Ni.

[0075] Each of the above coefficients indicates the magnitude of the effect on the change in the lattice volume of the main phase when a portion of Sm is substituted with La or Ce, or when a portion of Fe is substituted with Co or Ni.

[0076] The fact that the coefficients of x and y are positive indicates that the lattice volume of the main phase basically increases when part of Sm is replaced with La and / or Ce. The fact that the coefficient of x is larger than the coefficient of y indicates that the ionic radius of La is larger than that of Ce, and therefore replacement of part of Sm with La has a larger effect on the change in the lattice volume of the main phase than replacement of part of Sm with Ce.

[0077] The fact that the coefficients of p and q are negative indicates that the lattice volume of the main phase is basically decreased when part of Fe is substituted with Co and / or Ni. The fact that the absolute value of the coefficient of q is larger than the absolute value of the coefficient of p indicates that the ionic radius of Ni is larger than that of Co, and therefore substituting part of Fe with Ni has a larger effect on the change in the lattice volume of the main phase than substituting part of Fe with Co.

[0078] In the above description of the coefficients of the "relationship formula expressing the lattice volume of the main phase", the reason for the word "basically" will be explained below.

[0079] In formula (1), the "relationship formula expressing the lattice volume of the main phase" is Sm2Fe 17 The model is obtained using machine learning, assuming that part of Sm is replaced with La and / or Ce, and part of Fe is replaced with Co and / or Ni, for the N3 phase. 17 When the phase is nitrided, Sm2Fe 17 Not only N3 phase, but also Sm2Fe 17 N h (however, h is 2.9~ 3.2 ) is obtained. Details of h will be explained later.

[0080] The coefficients x, y, p, and q change depending on the degree of nitridation. The smaller the absolute value of the coefficient, the more susceptible it is to the degree of nitridation. For example, the absolute value of the coefficient of y is the smallest among the coefficients of x, y, p, and q, so y is more susceptible to the degree of nitridation. Specifically, when a part of Sm is substituted with Ce, the lattice volume of the main phase basically increases. Therefore, basically, the coefficient of y is positive. However, depending on the degree of nitridation, the coefficient of y may decrease. In that case, since the absolute value of the coefficient of y is small, the coefficient of y may decrease and become negative. The coefficient of y becoming negative means that the lattice volume of the main phase decreases even when a part of Sm is substituted with Ce. This is due to the fact that the ionic radius of Ce is large compared to the ionic radius of Sm, but the difference is small, so the absolute value of the coefficient of y is small. In addition, Ce ions are available in trivalent and tetravalent forms, and the coefficient of y is easily changed.

[0081] On the other hand, since the ionic radius of La is very large compared to the ionic radius of Sm, it is less affected by the degree of nitriding. Specifically, when a part of Sm is substituted with La, the lattice volume of the main phase basically increases. Therefore, basically, the coefficient of x is positive. However, depending on the degree of nitriding, the coefficient of x may decrease. Even in such a case, since the absolute value of the coefficient of x is relatively large, even if the coefficient of x decreases, it is difficult for the coefficient of x to become negative. An example of a case in which the coefficient of x decreases to the point where it becomes negative depending on the degree of nitriding is when the amount of substitution by La is small.

[0082] When a part of Fe is replaced with Co and / or Ni, the lattice volume of the main phase is basically reduced. Therefore, the coefficients of p and q are basically negative. However, depending on the degree of nitriding, the coefficients of p and q may increase. Even in that case, the absolute values ​​of the coefficients of p and q are large compared to the absolute values ​​of the coefficients of x and y, so even if the coefficients of p and q increase, it is difficult for the coefficients of p and q to become positive.

[0083] As explained above, even if the "relational expression expressing the lattice volume of the main phase" in formula (1) is obtained by machine learning, it still has the above-mentioned technical significance. 3 and the density of the main phase is 7.7 to 8.0 g / cm 3 It has been experimentally confirmed that a desired saturation magnetization can be obtained if x, y, p, and q satisfy formula (1).

[0084] In addition, the density of the main phase is 7.7 to 8.0 g / cm 3 The following formula (2) can be used as a reference for x, y, p, and q, which are determined by machine learning. 0.0619≦-0.817x-0.5669y+0.499p+2.606q≦0.16194...Equation (2)

[0085] <h> Next, we will explain h, which indicates the degree of nitriding. 17 The nitridation of the phase basically results in Sm2Fe 17 N h phase (where h=3). Nitriding is typically performed using the SmFe 17 This is done by exposing a precursor of a Sm-Fe-N magnetic material having a nitriding phase (hereinafter, simply referred to as the "precursor") to a nitrogen gas atmosphere at high temperature. Therefore, since the degree of nitridation differs between the surface and the inside of the precursor, the nitridation is performed when h is 2.9 to 1.5 mm. 3.2 The same applies when a portion of Sm in the precursor is replaced with La and / or Ce, and a portion of Fe is replaced with Co and / or Ni. That is, (Sm, La, Ce)2(Fe, Co, Ni) 17 When the phase is nitrided, (Sm, La, Ce)2(Fe, Co, Ni) 17 N h Phase (where h is 2.9~ 3.2 ) is formed.

[0086] <Volume ratio of main phase> The Sm-Fe-N magnetic material of the present disclosure has a main phase represented by the above composition formula. The magnetic properties of the Sm-Fe-N magnetic material of the present disclosure are expressed by the main phase. Therefore, it is preferable that the volume ratio of the main phase is high relative to the entire Sm-Fe-N magnetic material of the present disclosure. Specifically, the volume ratio of the main phase may be 95% or more, 96% or more, or 97% or more relative to the entire Sm-Fe-N magnetic material of the present disclosure. On the other hand, when manufacturing the Sm-Fe-N magnetic material of the present disclosure, there may be a process in which a phase other than the main phase represented by the above composition formula is in a stable temperature range. In addition, it may be difficult to completely eliminate the inclusion of unavoidable impurity elements that do not constitute the main phase. For these reasons, the volume ratio of the main phase is ideally 100%, but as long as the volume ratio of the main phase is secured, there is no practical problem even if the volume ratio of the main phase is 99% or less or 98% or less.

[0087] Phases other than the main phase typically exist at grain boundaries between the main phases, particularly at triple points. Typical examples of phases other than the main phase include the SmFe3 phase and its nitride phase. In the SmFe3 phase and its nitride phase, part of Sm is replaced by La, Ce, and R. 1 a phase in which a part of Fe is substituted with one or more elements selected from the group consisting of Co, Ni, and M, and a nitride phase thereof; and a phase in which a part of Sm is substituted with La, Ce, and R. 1 and a phase in which a portion of Fe is substituted with one or more elements selected from the group consisting of Co, Ni, and M, and a nitride phase thereof.

[0088] The volume fraction of the main phase was determined by measuring the overall composition of the precursor before nitriding using inductively coupled plasma atomic emission spectroscopy (ICP-AES). From the measured value, it was found that the precursor before nitriding contained the following elements: (Sm, La, Ce, R 1 )2(Fe, Co, Ni, M) 17 Phase and (Sm, La, Ce, R 1) (Fe, Co, M) and calculate the volume fraction of the main phase. Specifically, after obtaining the mass concentration (mass fraction) of each element from the ICP measurement results, SmFe 17 The mass ratio of the SmFe3 phase and the SmFe3 phase is first calculated, and the volume ratio is calculated from the density of each phase. 1 )2(Fe, Co, Ni, M) 17 The phase is SmFe 17 phase, Sm2Fe 17 Part of the Sm in the phase is Sm, La, Ce, and R. 1 A phase substituted with one or more elements selected from the group consisting of Sm2Fe 17 A phase in which part of the Fe in the phase is replaced with one or more elements selected from the group consisting of Co, Ni, and M, and SmFe 17 Part of the Sm in the phase is Sm, La, Ce, and R. 1 and is substituted with one or more elements selected from the group consisting of Sm2Fe 17 It represents a phase in which a part of the Fe in the phase is replaced with one or more elements selected from the group consisting of Co, Ni, and M. Also, (Sm, La, Ce, R 1 )(Fe,Co,Ni,M)3 phase is SmFe3 phase, part of Sm in SmFe3 phase is Sm, La, Ce, and R 1 a phase in which part of the Fe in the SmFe3 phase is replaced by one or more elements selected from the group consisting of Co, Ni, and M; and a phase in which part of the Sm in the SmFe3 phase is replaced by one or more elements selected from the group consisting of Sm, La, Ce, and R. 1 and is substituted with one or more elements selected from the group consisting of Sm2Fe 17 The Fe in the phase is partially substituted with one or more elements selected from the group consisting of Co, Ni, and M.

[0089] The overall composition (total of the main phase and phases other than the main phase) of the Sm-Fe-N magnetic material of the present disclosure is such that, from the viewpoint of suppressing the appearance of the α-(Fe, Co, Ni, M) phase and its nitride phase during the production of the Sm-Fe-N magnetic material of the present disclosure, the main phase contains Sm, La, Ce, and R. 1That is, the overall composition of the Sm-Fe-N magnetic material of the present disclosure can be set to be equal to or greater than the total mole number of (Sm (1-x-y-z) La x Ce y R 1 z ) w (Fe (1-p-q-s) Co p Ni q M s ) 17 N h (wherein w is 2.00 to 3.00). In this case, x, y, z, p, q, s, and h may be the same as x, y, z, p, q, s, and h in the formula expressing the composition of the main phase described above. From the viewpoint of suppressing the appearance of the α-(Fe, Co, Ni, M) phase, w is more preferably 2.02 or more, 2.04 or more, 2.06 or more, 2.08 or more, 2.10 or more, 2.20 or more, 2.30 or more, 2.40 or more, or 2.50 or more. On the other hand, in the case of the above-mentioned (Sm, La, Ce, R 1 From the viewpoint of reducing the volume fraction of the (Fe, Co, Ni, M) 3 phase, w is more preferably 2.90 or less, 2.80 or less, 2.70 or less, or 2.60 or less.

[0090] 《Manufacturing method》 Next, a method for producing the Sm-Fe-N based magnetic material of the present disclosure (hereinafter sometimes referred to as the "production method of the present disclosure") will be described.

[0091] The manufacturing method of the present disclosure includes a magnetic material precursor preparation step and a nitriding step. Each step will be described below.

[0092] <Magnetic material precursor preparation process> In the manufacturing method of the present disclosure, the molar ratio formula (Sm (1-x-y-z) La x Ce y R 1 z )2(Fe (1-p-q-s) Co p Ni q M s ) 17 A magnetic material precursor having a crystalline phase with a composition represented by the following formula is prepared.

[0093] In the formula that represents the composition of the crystal phase, Sm, La, Ce, R 1 , Fe, Co, Ni, and M, as well as x, y, z, p, q, and s are as explained in “Sm—Fe—N based magnetic material.”

[0094] The crystal phase of the magnetic material precursor is Th2Zn 17 Type and Th2Ni 17 The magnetic material precursor has at least one of the crystal structures of the above types. When the magnetic material precursor is nitrided, the crystal phase in the magnetic material precursor is nitrided, and the main phase of the Sm-Fe-N magnetic material of the present disclosure is formed. The main phase of the Sm-Fe-N magnetic material of the present disclosure is Th2Zn 17 Type and Th2Ni 17 The nitridation has at least one of the following crystal structures: Th2Zn 17 Type and Th2Ni 17 This is done to the extent that the crystal structure of at least one of the types is maintained.

[0095] As described above, the crystalline phase in the magnetic material precursor is nitrided to form the main phase of the Sm-Fe-N magnetic material of the present disclosure, so the volume fraction of the crystalline phase in the magnetic material precursor may be considered to be equivalent to the volume fraction of the main phase in the Sm-Fe-N magnetic material of the present disclosure. For this reason, the volume fraction of the crystalline phase in the magnetic material precursor may be 95% or more, 96% or more, or 97% or more with respect to the entire magnetic material precursor. When manufacturing the magnetic material precursor, there may be a process in which a phase other than the crystalline phase represented by the above-mentioned composition formula is in a stable temperature range. In addition, it may be difficult to completely eliminate the inclusion of unavoidable impurity elements that do not constitute the crystalline phase. Although the volume fraction of the crystalline phase is ideally 100%, as long as the volume fraction of the above-mentioned crystalline phase is secured, there is no practical problem even if the volume fraction of the main phase is 99% or less or 98% or less.

[0096] Phases other than the crystalline phase are typically present at grain boundaries between crystalline phases, particularly triple junctions. Typical examples of phases other than the crystalline phase include the SmFe3 phase. In the SmFe3 phase, part of Sm is replaced by La, Ce, and R. 1a phase in which a portion of Fe is replaced by one or more elements selected from the group consisting of Co, Ni, and M; and a phase in which a portion of Sm is replaced by La, Ce, and R. 1 and a phase in which a portion of Fe is substituted with one or more elements selected from the group consisting of Co, Ni, and M.

[0097] The volume fraction of the crystalline phase was determined by measuring the overall composition of the precursor before nitridation using inductively coupled plasma atomic emission spectroscopy (ICP-AES). From the measured value, it was determined that the precursor before nitridation contained the following elements: (Sm, La, Ce, R 1 )2(Fe, Co, Ni, M) 17 Phase and (Sm, La, Ce, R 1 ) (Fe, Co, M) and calculate the main phase ratio. Specifically, after obtaining the weight concentration (weight ratio) of each element from the ICP measurement results, Sm2Fe 17 The weight ratio of the SmFe3 phase and the SmFe3 phase is first calculated, and the volume ratio is calculated from the density of each phase. 1 )2(Fe, Co, Ni, M) 17 The phase is SmFe 17 phase, Sm2Fe 17 Part of the Sm in the phase is Sm, La, Ce, and R. 1 A phase substituted with one or more elements selected from the group consisting of Sm2Fe 17 A phase in which part of the Fe in the phase is replaced with one or more elements selected from the group consisting of Co, Ni, and M, and SmFe 17 Part of the Sm in the phase is Sm, La, Ce, and R. 1 and is substituted with one or more elements selected from the group consisting of Sm2Fe 17 It represents a phase in which a part of the Fe in the phase is replaced with one or more elements selected from the group consisting of Co, Ni, and M. Also, (Sm, La, Ce, R 1 )(Fe,Co,Ni,M)3 phase is SmFe3 phase, part of Sm in SmFe3 phase is Sm, La, Ce, and R1 a phase in which part of the Fe in the SmFe3 phase is replaced by one or more elements selected from the group consisting of Co, Ni, and M; and a phase in which part of the Sm in the SmFe3 phase is replaced by one or more elements selected from the group consisting of Sm, La, Ce, and R. 1 and a portion of the Fe in the SmFe3 phase is substituted with one or more elements selected from the group consisting of Co, Ni, and M.

[0098] The overall composition of the magnetic material precursor (the sum of the crystalline phase and the phases other than the crystalline phase) is, from the viewpoint of suppressing the appearance of the α-(Fe, Co, Ni, M) phase during the production of the magnetic material precursor, Sm, La, Ce, and R in the crystalline phase. 1 That is, the overall composition of the magnetic material precursor can be set to be equal to or greater than the total mole number of (Sm (1-x-y-z) La x Ce y R 1 z ) w (Fe (1-p-q-s) Co p Ni q M s ) 17 (wherein w is 2.00 to 3.00). In this case, x, y, z, p, q, and s may be the same as x, y, z, p, q, and s in the formula expressing the composition of the above-mentioned crystal phase. From the viewpoint of suppressing the appearance of the α-(Fe, Co, Ni, M) phase, w is more preferably 2.02 or more, 2.04 or more, 2.06 or more, 2.08 or more, 2.10 or more, 2.20 or more, 2.30 or more, 2.40 or more, or 2.50 or more. On the other hand, when (Sm, La, Ce, R 1 From the viewpoint of reducing the volume fraction of the (Fe, Co, Ni, M) 3 phase, w is more preferably 2.90 or less, 2.80 or less, 2.70 or less, or 2.60 or less.

[0099] The magnetic material precursor can be obtained by using a well-known manufacturing method. For example, a method for obtaining the magnetic material precursor includes melting and solidifying raw materials containing elements constituting the magnetic material precursor. For example, a method for melting the raw materials includes charging the raw materials into a container such as a crucible, and melting the raw materials in the container by arc melting or high frequency melting to obtain a molten metal, and then pouring the molten metal into a mold such as a book mold, or solidifying the molten metal in a crucible. From the viewpoint of suppressing the coarsening of the crystalline phase in the magnetic material precursor and homogenizing the crystalline phase, it is preferable to increase the cooling rate of the molten metal. From this viewpoint, it is preferable to pour the molten metal into a mold such as a book mold. Furthermore, from the viewpoint of suppressing the coarsening of the crystalline phase in the magnetic material precursor and enhancing the homogenization of the crystalline phase, for example, the following method may be adopted. That is, the raw materials are melted by high frequency or arc in a container, solidified, and the resulting ingot is melted again by high frequency melting or the like, and the resulting molten liquid is quenched using a strip casting method, a liquid quenching method, or the like to obtain a flake, which may be used as the magnetic material precursor.

[0100] Prior to nitriding, which will be described later, the magnetic material precursor may be heat-treated (hereinafter, such heat treatment may be referred to as "homogenization heat treatment") in order to homogenize the crystal grains in the magnetic material precursor. The temperature of the homogenization heat treatment may be, for example, 1273K or more, 1323K or more, or 1373K or more, and may be 1523K or less, 1473K or less, or 1423K or less. The homogenization heat treatment time may be, for example, 6 hours or more, 12 hours or more, 18 hours or more, or 24 hours or more, and may be 48 hours or less, 42 hours or less, 36 hours or less, or 30 hours or less.

[0101] In order to suppress oxidation of the magnetic material precursor, the homogenization heat treatment is preferably performed in a vacuum or in an inert gas atmosphere. The inert gas atmosphere does not include a nitrogen gas atmosphere. When the homogenization heat treatment is performed in a nitrogen gas atmosphere, Th2Zn 17 Type and / or Th2Ni 17 This is because the phase having the crystal structure of this type is easily decomposed.

[0102] <Nitriding process> The above-mentioned magnetic material precursor is nitrided, whereby the crystal phase in the magnetic material precursor is nitrided to form the main phase of the Sm—Fe—N based magnetic material of the present disclosure.

[0103] As long as the desired main phase can be obtained, the nitriding method is not particularly limited, but typically includes, for example, exposing the magnetic material precursor to an atmosphere containing nitrogen gas while heating, or exposing it to a gas atmosphere containing nitrogen (N). Examples of the atmosphere containing nitrogen gas include a nitrogen gas atmosphere, a mixed gas atmosphere of nitrogen gas and an inert gas, and a mixed gas atmosphere of nitrogen gas and hydrogen gas. Examples of the gas atmosphere containing nitrogen (N) include an ammonia gas atmosphere, or a mixed gas atmosphere of ammonia gas and hydrogen gas. The atmospheres exemplified above may be combined. From the viewpoint of nitriding efficiency, an ammonia gas atmosphere, a mixed gas atmosphere of ammonia gas and hydrogen gas, and a mixed gas atmosphere of nitrogen gas and hydrogen gas are preferred.

[0104] The magnetic material precursor may be pulverized before nitriding to obtain a magnetic material precursor powder, which may then be nitrided. By pulverizing the magnetic material precursor and then nitriding it, the crystal phase present inside the magnetic material precursor can be sufficiently nitrided. The magnetic material precursor is preferably pulverized in an inert gas atmosphere. The inert gas atmosphere may include a nitrogen gas atmosphere. This makes it possible to suppress oxidation of the magnetic material precursor during pulverization. The particle size of the magnetic material precursor powder is D 50 and may be 5 μm or more, 10 μm or more, or 15 μm or more, and may be 50 μm or less, 40 μm or less, 30 μm or less, 25 μm or less, or 20 μm or less.

[0105] The nitriding temperature may be, for example, 673 K or more, 698 K or more, 723 K or more, or 748 K or more, and may be 823 K or less, 798 K or less, or 773 K or less. In addition, the nitriding time may be, for example, 4 hours or more, 8 hours or more, 12 hours or more, or 16 hours or more, and may be 48 hours or less, 36 hours or less, 24 hours or less, 20 hours or less, or 18 hours or less.

[0106] 《Transform》 The Sm-Fe-N magnetic material and its manufacturing method of the present disclosure are not limited to the embodiments described above, and may be modified as appropriate within the scope of the claims. For example, the Sm-Fe-N magnetic material of the present disclosure may be a powder or a compact of the powder. The compact may be a bonded compact or a sintered compact. In the case of a compact, a bonded compact is preferred from the viewpoint of easily avoiding a temperature at which nitrogen (N) in the main phase is separated (decomposed) during the molding process. Examples of the bond include resin and low-melting-point metal bond. Examples of the low-melting-point metal bond include metal zinc or zinc alloy, and combinations thereof. EXAMPLES

[0107] The Sm-Fe-N magnetic material and the manufacturing method thereof according to the present disclosure will be described in more detail below with reference to examples and comparative examples. Note that the Sm-Fe-N magnetic material and the manufacturing method thereof according to the present disclosure are not limited to the conditions used in the following examples.

[0108] <Sample preparation> A sample of the Sm-Fe-N magnetic material was prepared in the following manner.

[0109] Metal Sm, metal La, Ce-Fe alloy, metal Fe, metal Co, and metal Ni were mixed so that the main phase had the composition shown in Table 1, and this was melted by high-frequency at 1673K (1400°C) and solidified to obtain a magnetic material precursor. During mixing, the total number of moles of Sm, La, and Ce mixed was made larger than the total number of moles of Sm, La, and Ce in the main phase so that the volume fraction of the main phase was 95 to 100%. In this specification, for example, "metal Sm" means unalloyed Sm. Of course, metal Sm may contain unavoidable impurities.

[0110] The magnetic material precursor was homogeneously heat-treated in an argon gas atmosphere at 1373 K for 24 hours.

[0111] The magnetic material precursor after the homogeneous heat treatment was placed in a glove box and pulverized in a nitrogen gas atmosphere using a cutter mill. The particle size of the pulverized magnetic material precursor powder was D 50 The average particle size was less than 20 μm.

[0112] The magnetic material precursor powder was heated to 748 K in a nitrogen gas atmosphere and nitrided for 16 hours. The amount of nitridation was determined by the change in mass of the magnetic material precursor powder before and after nitriding.

[0113] "evaluation" The composition, volume fraction, density, and lattice volume of the main phase of each sample were determined by the above-mentioned measurement method. In addition, the magnetic properties of each sample were measured by applying a maximum magnetic field of 9 T using a physical property processing system PPMS (registered trademark)-VSM. Regarding the measurement of magnetic properties, each sample powder after nitriding was solidified while being magnetically oriented in an epoxy resin, and the magnetic properties of each sample after solidification were measured in the easy axis direction and the hard axis direction at 300 to 453 K. From the measured value for the easy axis direction, the saturation magnetization Ms was calculated using the saturation asymptotic law. In addition, the anisotropic magnetic field Ha was obtained from the intersection of the hysteresis curve in the easy axis direction and the hysteresis curve in the hard axis direction.

[0114] The results are shown in Table 1. Figure 1 is a graph showing the relationship between lattice volume and saturation magnetization Ms (300K), and Figure 2 is a graph showing the relationship between lattice volume and density.

[0115] [Table 1-1]

[0116] [Table 1-2]

[0117] From Table 1 and Figs. 1 and 2, for the samples of Examples 1 to 5, the lattice volume of the main phase is 0.830 to 0.840 nm 3and the density of the main phase is 7.70 to 8.00 g / cm 3 2, it can be seen that the saturation magnetization is improved. Also, from Fig. 2, it can be seen that the samples of Comparative Examples 1 to 14 have an inversely proportional relationship between the lattice volume and the density, and that the samples of Examples 1 to 5 have a higher density than that relationship.

[0118] These results confirm the effects of the Sm-Fe-N based magnetic material and the manufacturing method thereof according to the present disclosure.

Claims

1. Th 2 Zinc 17 Type and Th 2 Ni 17 A Sm-Fe-N based magnetic material having a main phase having at least one of the following crystal structures: The overall composition is represented by the molar ratio formula (Sm(1-xyz)LaxCeyR1z)w(Fe(1-pqs)CopNiqMs)17Nh, The main phase is represented by the molar ratio formula (Sm (1-x-y-z) La x C y R 1 z ) 2 (Fe (1-p-q-s) Co p Ni q M s ) 17 It has a composition represented by N h , R 1 represents one or more rare earth elements other than Sm, La, and Ce, and Zr; M is one or more elements other than Fe, Co, Ni, and rare earth elements, and unavoidable impurity elements; 0≦x+y<0.04, 0≦z≦0.10, 2.00≦w≦3.00, 0<p+q≦0.10, 0≦s≦0.10, and 2.9≦h≦3.2 is satisfied, The volume fraction of the main phase is 95 to 100%, The lattice volume of the main phase is 0.830 to 0.840 nm 3 and The density of the main phase is 7.70 to 8.00 g / cm 3 That is, Sm-Fe-N magnetic material.

2. The lattice volume of the main phase is 0.833 to 0.835 nm 3 2. The Sm-Fe-N based magnetic material according to claim 1,

3. The density of the main phase is 7.70 to 7.90 g / cm 3 3. The Sm-Fe-N based magnetic material according to claim 1, wherein

4. A method for producing the Sm-Fe-N based magnetic material according to claim 1, The overall composition is represented by the molar ratio formula (Sm (1-x-y-z) La x Ce y R 1 z ) w (Fe (1-p-q-s) Co p Ni q M s ) 17 and the molar ratio formula (Sm (1-x-y-z) La x C y R 1 z ) 2 (Fe (1-p-q-s) Co p Ni q M s providing a magnetic material precursor having a crystalline phase having a composition represented by the formula: nitriding the magnetic material precursor; Including, In the above molar ratio formula: R 1 represents one or more rare earth elements other than Sm, La, and Ce, and Zr; M is one or more elements other than Fe, Co, Ni, and rare earth elements, and unavoidable impurity elements; 0≦x+y<0.04, 0≦z≦0.10, 2.00≦w≦3.00, 0<p+q≦0.10, and 0≦s≦0.10 Satisfying the above, and The volume fraction of the crystalline phase is 95 to 100%. A method for producing an Sm-Fe-N based magnetic material.

5. The method according to claim 4 , further comprising nitriding the magnetic material precursor powder after pulverizing the magnetic material precursor to obtain the magnetic material precursor powder.

6. The method according to claim 4 or 5, wherein the magnetic material precursor is obtained by melting and solidifying raw materials containing elements constituting the magnetic material precursor.

Citation Information

Patent Citations

  • Manufacture of rare earth bond magnet and injection molded object

    JP2000340442A

  • Production method of magnetic powder, production method of dust magnet member, and dust magnet member

    JP2016100519A

  • Anisotropic magnetic powder and production method therefor

    JP2017117937A

  • Samarium-iron-nitrogen alloy powder and method for producing same

    WO2017150557A1