Three-phase, three-legged wound core and three-phase, three-legged wound core transformer using the same
The three-phase tripod-wound core uses different magnetic flux density electrical steel sheets to suppress magnetic flux crossing, reducing transformer iron loss and noise, thereby enhancing transformer performance.
Patent Information
- Application Number
- JP2022053242
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-03-29
- Publication Date
- 2024-09-26
- Estimated Expiration
- 2042-03-29
AI Technical Summary
Three-phase wound core transformers experience increased transformer iron loss and noise due to magnetic flux concentration and interlayer magnetic flux crossing, which are not effectively addressed by existing materials and configurations.
A three-phase tripod-wound core is constructed using at least two types of grain-oriented electrical steel sheets with different magnetic flux densities, specifically higher density for the outer core and lower density for the inner core, to suppress magnetic flux crossing and reduce transformer iron loss and noise.
The solution effectively reduces transformer iron loss and noise by minimizing magnetic flux crossing, achieving improved transformer characteristics with optimized magnetic flux distribution.
Smart Images

Figure 0007556372000016 
Figure 0007556372000008 
Figure 0007556372000018
Abstract
Description
[Technical field]
[0001] The present invention relates to a three-phase, three-legged wound core, and more particularly to a three-phase, three-legged wound core for a transformer manufactured using grain-oriented electrical steel sheets. [Background technology]
[0002] The easy axis of magnetization of iron <001> Grain-oriented electrical steel sheets, which have a crystal structure with a highly aligned orientation in the rolling direction of the steel sheet, are used particularly as the core material for power transformers. Transformers are broadly classified into wound core transformers and stacked core transformers based on their core structure. Wound core transformers have a core formed by winding and stacking steel sheets. On the other hand, stacked core transformers have a core formed by stacking steel sheets cut to a specified shape. There are various requirements for transformer cores, but the most important are low iron loss and low noise.
[0003] It is generally believed that reducing the iron loss of a transformer can be achieved by reducing the iron loss (material iron loss) of the grain-oriented electromagnetic steel sheet, which is the core material. However, it is known that the iron loss in a transformer core, especially a wound-core transformer with three or five legs of electromagnetic steel sheet and three-phase excitation, is larger than the material iron loss. The value obtained by dividing the iron loss value (transformer iron loss) when electromagnetic steel sheet is used as the transformer core by the iron loss value of the core material obtained by the Epstein test is generally called the Building Factor (BF). In other words, in a wound-core transformer with three or five legs and three-phase excitation, the BF generally exceeds 1.
[0004] It is generally known that the concentration of magnetic flux on the inner core, which occurs mainly due to the difference in magnetic path length, is the reason why the transformer iron loss in a wound core transformer increases compared to the material iron loss. Figure 1 shows a schematic diagram of the magnetic flux flow at the moment when a three-phase three-legged wound core transformer is excited with three-phase excitation and only the left leg and the center leg are excited. As shown in Figure 1, a three-phase three-legged wound core transformer is constructed using a three-phase three-legged wound core consisting of an outer core 2 and two adjacent inner cores 1 arranged inside the outer core 2. As shown in Figure 1, when both the inner core 1 and the outer core 2 are excited, the magnetic path of the inner core 1 is shorter than that of the outer core 2, so that the magnetic flux is concentrated on the inner core 1. When the excitation magnetic flux density becomes relatively large, the inner core 1 alone cannot carry the excitation, and a lot of magnetic flux also passes through the outer core 2, so the magnetic flux concentration is alleviated. However, as shown in Fig. 2, the magnetic flux passing through outer core 2 flows toward the non-excited right leg, and when it tries to return to the excited center leg, the magnetic flux passes to inner core 1, and an interlayer magnetic flux crossover 3 occurs between inner core 1 and outer core 2. Magnetization occurring in the perpendicular direction causes an increase in in-plane eddy current loss, which increases the transformer iron loss.
[0005] The noise of a transformer is generally caused by magnetostriction, which is the distortion that occurs when magnetic steel sheets are magnetized, the inherent vibration of the iron core, and electromagnetic vibration caused by magnetized steel sheets. Of these, electromagnetic vibration caused by magnetized steel sheets is a minute vibration that occurs when magnetization changes over time in the case of AC excitation, and the attractive force between laminated steel sheets also changes over time. In-plane magnetization, such as the interlayer magnetic flux transfer 3 between the inner iron core 1 and the outer iron core 2, also changes the attractive force between the steel sheets, causing electromagnetic vibration, which is one of the causes of transformer noise.
[0006] Based on a qualitative understanding of the factors that increase transformer iron loss and transformer noise, the following have been proposed as measures to reduce transformer iron loss and transformer noise:
[0007] Patent Document 1 discloses that transformer iron loss can be effectively reduced by arranging electromagnetic steel sheets with inferior magnetic properties to those on the outer periphery on the inner periphery, where the magnetic path length is short and the magnetic resistance is small, and electromagnetic steel sheets with superior magnetic properties to those on the inner periphery on the outer periphery, where the magnetic path length is long and the magnetic resistance is large. Patent Document 2 discloses that transformer noise can be effectively reduced by arranging a wound core wound with grain-oriented silicon steel sheets on the inner part and winding a magnetic material with lower magnetostriction than the grain-oriented silicon steel sheets around the outside of this wound core to form a combined core. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Patent No. 5286292 [Patent Document 2] Japanese Patent Application Publication No. 3-268311 [Patent Document 3] International Publication No. 2019 / 151399 [Patent Document 4] Patent No. 5750820 Summary of the Invention [Problem to be solved by the invention]
[0009] As disclosed in Patent Documents 1 and 2, by utilizing the concentration of magnetic flux on the inner core and applying different materials to the inner core and outer core, it is possible to efficiently improve the transformer characteristics. However, as disclosed in Patent Document 3, when the excitation magnetic flux density increases, magnetic flux also flows in the outer part of the core, and the concentration of magnetic flux is alleviated, so the effect of improving the transformer characteristics is reduced. In addition, at this time, the magnetic flux passing through the outer core passes to the inner core, which has a short magnetic path and low loss, and this magnetic flux passing between layers not only increases iron loss in the jumper part, but also increases noise due to electromagnetic vibration between the steel sheets, significantly deteriorating the transformer characteristics.
[0010] An object of the present invention is to provide a three-phase, three-legged wound core that is excellent in reducing transformer iron loss and noise. [Means for solving the problem]
[0011] In three-phase three-legged wound core transformers, it may be possible to reduce transformer iron loss and noise by suppressing magnetic flux transfer from the outer core to the inner core, and we investigated methods for doing so.
[0012] The inventors of the present invention thought that since magnetic flux transfer is a transfer of magnetic flux between the inner part of the outer core and the outer part of the inner core of a three-phase three-legged core transformer, magnetic flux transfer could be suppressed by reducing the amount of magnetic flux flowing through these parts. In other words, they tried to reduce the magnetic flux that can be transferred. For this purpose, the three-phase three-legged core was constructed from at least two types of grain-oriented electromagnetic steel sheets having different magnetic flux densities at 800 A / m. Specifically, a three-phase three-legged core was manufactured, which is composed of an outer core and two adjacent inner cores arranged inside the outer core, in which the inner (inner circumference side) part of the outer core and the outer (outer circumference side) parts of the two inner cores are constructed from grain-oriented electromagnetic steel sheets having a lower magnetic flux density at 800 A / m than the grain-oriented electromagnetic steel sheets constituting the outer (outer circumference side) part of the outer core and the inner (inner circumference side) parts of the two inner cores, and magnetic flux transfer, transformer iron loss, and transformer noise were investigated.
[0013] A three-phase three-legged wound core was produced using electromagnetic steel sheets with a steel strip width of 150 mm in the shape of the wound core shown in Fig. 3. Specifically, in the three-phase three-legged wound core shown in Fig. 3, the outer and inner parts of the outer core 2 are made of grain-oriented electromagnetic steel sheets with different magnetic flux densities at 800 A / m (magnetic flux density B8 at magnetizing force of 800 A / m), and the outer and inner parts of the inner core 1 are made of grain-oriented electromagnetic steel sheets with different magnetic flux densities at 800 A / m. Here, the core material constituting the outer part of the outer core 2 and the inner part of the inner core 1 (the hatched area in the three-phase three-legged wound core shown in Fig. 3) is also referred to as the "outer core material," and the core material constituting the inner part of the outer core 2 and the outer part of the inner core 1 (the non-hatched area in the three-phase three-legged wound core shown in Fig. 3) is also referred to as the "inner core material." 3, the outer core material was a 0.23 mm-thick grain-oriented electromagnetic steel sheet with a relatively high magnetic flux density B8 at a magnetizing force of 800 A / m, and the inner core material was a 0.23 mm-thick grain-oriented electromagnetic steel sheet with a lower magnetic flux density B8 at a magnetizing force of 800 A / m than the outer core material. Furthermore, a three-phase three-legged core transformer was produced by changing the thickness t of region 4 (the outer part of the outer core and the inner part of the inner core) made up of the outer core material, and the thickness s of region 5 (the inner part of the outer core and the outer part of the inner core) made up of the inner core material, and three-phase excitation of 50 Hz and 1.7 T was performed to measure iron loss and noise.
[0014] The magnetic flux density B8 of the grain-oriented electromagnetic steel sheet, which is the core material, was obtained by cutting out the sheet before processing it into the core and measuring it by the Epstein test at an excitation frequency of 50 Hz based on JIS C 2550-1:2011. The thickness of region 4 (thickness in the lamination direction of the outer core material) composed of the outer core material, i.e., the thickness t of the outer part of the outer core and the inner part of the inner core when the three-phase three-legged wound core is viewed from the side, was obtained by measuring the length between the outermost and innermost grain-oriented electromagnetic steel sheets that compose the region with a vernier caliper. Similarly, the thickness of region 5 (thickness in the lamination direction of the inner core material) composed of the inner core material, i.e., the thickness s of the inner part of the outer core and the outer part of the inner core when the three-phase three-legged wound core is viewed from the side, was obtained by measuring the length between the outermost and innermost grain-oriented electromagnetic steel sheets that compose the region with a vernier caliper.
[0015] In addition, the region indicated by the reference numeral 6 in FIG. 3 indicates an interlayer jumper portion. The interlayer jumper portion 6 is defined as follows. In a side view, the center of the width of the inner core is set as the center line of the width of the interlayer jumper portion 6. The width (horizontal length) f of the interlayer jumper portion 6 is defined as 20% of the horizontal length c of the entire three-phase three-legged wound core. The thickness g of the interlayer jumper portion 6 is defined as a thickness extending from the line where the inner core and the outer core contact each other between the legs in the vertical direction by 75% of the thinner of the thicknesses of the region 4 of the outer core material and the region 5 of the inner core material. At the same time as the iron loss measurement, as disclosed in Patent Document 4, an infrared camera was used to measure the average temperature rise of the interlayer jumper portion 6 on the end face of the core during excitation, and the local iron loss of the interlayer jumper portion 6 was measured.
[0016] The transformer noise was measured during excitation for each of the wound core transformers at a position half the core height d, at a distance of 30 cm from the surface of the wound core transformer, and at eight points surrounding the wound core transformer, and the average value was taken as the transformer noise.
[0017] The transformer iron loss was calculated by winding 50 turns on both the primary and secondary sides of each leg of the three-phase, three-legged wound core that was fabricated, performing three-phase excitation under conditions of a maximum excitation magnetic flux density of 1.7 T and a frequency of 50 Hz, measuring the primary current and secondary voltage with a wattmeter, measuring the no-load loss, and dividing the result by the weight of the core. Table 1 shows the iron loss of the entire transformer (transformer iron loss) for each wound core transformer, the iron loss in the interlayer jumper where magnetic flux transfer occurs, and the transformer noise values.
[0018] [Table 1]
[0019] The transformer iron loss of a three-phase three-limbed wound core transformer using high magnetic flux density B8 material (high magnetic flux density B8 grain-oriented electromagnetic steel sheet) and low magnetic flux density B8 material (low magnetic flux density B8 grain-oriented electromagnetic steel sheet) for the outer and inner core materials, respectively, was improved compared to a three-phase three-limbed wound core transformer made only of the same core material (conditions 11 and 12 in Table 1). Furthermore, by using low magnetic flux density B8 grain-oriented electromagnetic steel sheet with low B8 for the outer part of inner core 1 and the inner part of outer core 2, which are the interlayer jumpers, so that the thickness s of this area is related to the thickness t of the outer core material area, t / s ≧ 1.0, the transformer iron loss was significantly reduced compared to the three-phase three-limbed wound core transformers under conditions 11 and 12 made only of the same core material.
[0020] It is believed that the iron loss at the interlayer jumper is a reflection of the amount of magnetic flux passing at the interlayer jumper. In a three-phase three-legged core, in order to reduce energy loss, magnetic flux passes from the inner part of the outer core 2, which has a long magnetic path, to the outer part of the inner core 1, which has a short magnetic path. The amount of magnetic flux that can flow through a transformer core is determined by the magnetic permeability of the material, represented by the magnetic flux density B8 of the grain-oriented electrical steel sheet that is the core material. In the core region made of high-permeability material with a large B8, the amount of magnetic flux that can flow increases, and conversely, in the core region made of low-permeability material with a small B8, the amount of magnetic flux that can flow decreases. The amount of magnetic flux that can pass from the outer core 2 and the amount of magnetic flux that can pass to the inner core 1 are both determined by the magnetic permeability of the material in that part. FIG. 4(a) is a diagram showing the flow of magnetic flux in the inner part of the outer core and the outer part of the inner core in a conventional three-phase three-limbed core transformer, and FIG. 4(b) is a diagram showing the flow of magnetic flux in the inner part of the outer core and the outer part of the inner core in a three-phase three-limbed core transformer of the present invention. That is, as shown in FIG. 4(b), if the magnetic flux density B8 in the inner part of the outer core is small and the amount of magnetic flux flowing through the outer core is small, the amount of magnetic flux flowing into the inner core is reduced, and if the magnetic flux density B8 in the outer part of the inner core is small, the amount of magnetic flux transfer that the inner core can accept is reduced. Therefore, it is presumed that the reduction in transformer iron loss is due to the reduction in iron loss in the interlayer transfer section by suppressing magnetic flux transfer, which in turn reduces the transformer iron loss. In addition, under the condition that the thickness s of the region of the inner core material, which has low B8, is thicker than the thickness t of the region of the outer core material, the improvement in transformer iron loss is small. This is presumably because the use of a higher proportion of low B8 material (low magnetic flux density B8 grain-oriented electrical steel sheet) as the inner material of the core is affected by the increase in iron loss due to the low B8 content, which cancels out to some extent the decrease in iron loss due to magnetic flux transfer.
[0021] Compared to conditions 11 and 12, which consisted of only one type of core material, a reduction in transformer noise was observed under all conditions. In particular, the transformer noise was significantly reduced by using an inner core material with a thickness that satisfied t / s ≥ 1.0 relative to the outer core material. It is presumed that the magnetic flux transfer was suppressed by combining the outer and inner core materials, which suppressed electromagnetic vibration due to in-plane magnetization and reduced the transformer noise. In conditions 1, 2, 3, and 4, where magnetic flux transfer was suppressed but the transformer noise did not decrease significantly, this is thought to be due to a higher proportion of inner materials with low B8. It is generally known that transformer noise increases as the B8 of the electromagnetic steel sheet that is the material for three-phase three-limbed wound core transformers decreases. It is presumed that the noise of the transformer in conditions 1, 2, 3, and 4 was reduced by both the noise reduction due to the suppression of magnetic flux transfer and the increase in noise due to the lower B8, resulting in a smaller improvement in transformer noise.
[0022] Based on the above experimental facts and assumptions, it was found that in order to reduce the transformer iron loss and transformer noise in a three-phase three-legged wound core transformer using a three-phase three-legged wound core, it is essential to reduce the magnetic flux transfer at the interlayer jumper. Furthermore, it was also found that in order to reduce the magnetic flux transfer at the interlayer jumper, it is effective to use a material with a magnetic flux density B8 at 800 A / m lower than that of the other parts in the inner part of the outer core and the outer part of the inner core, where the magnetic flux transfer occurs. On the other hand, if the proportion of the material with a low B8 is increased too much, the improvement in the transformer iron loss and transformer noise will be reduced due to the influence of the low B8 material, so it was found that it is particularly preferable to use the material in an amount less than half the thickness of the inner core and the outer core when the wound core is viewed from the side.
[0023] Based on the above findings, the present invention has been completed. That is, the present invention has the following features. [1] A three-phase three-legged core comprising an outer core and two adjacent inner cores disposed inside the outer core, the outer core and the two inner cores are each made of at least two types of grain-oriented electrical steel sheets having different magnetic flux densities at 800 A / m; A three-phase three-legged wound core, in which the inner portion of the outer core and the outer portions of the two inner cores are made of grain-oriented electromagnetic steel sheets having a lower magnetic flux density at 800 A / m than the grain-oriented electromagnetic steel sheets constituting the outer portion of the outer core and the inner portions of the two inner cores. [2] The grain-oriented electromagnetic steel sheet constituting the inner part of the outer core and the outer parts of the two inner cores is called grain-oriented electromagnetic steel sheet B. When the grain-oriented electromagnetic steel sheet constituting the outer portion of the outer core and the inner portions of the two inner cores is referred to as grain-oriented electromagnetic steel sheet A, The magnetic flux density of the grain-oriented electrical steel sheet A at 800 A / m is 1.88 T or more, The three-phase three-legged wound core according to [1], wherein the magnetic flux density of the grain-oriented electrical steel sheet B at 800 A / m is 1.83 T or more and is lower than the magnetic flux density of the grain-oriented electrical steel sheet A. [3] In side view, The thickness of the outer part of the outer core and the inner parts of the two inner cores is t, When the thickness of the inner part of the outer core and the outer parts of the two inner cores is s, A three-phase, three-legged wound core according to [1] or [2], satisfying t / s ≧ 1.0. [4] A three-phase three-legged wound core transformer using the three-phase three-legged wound core according to any one of [1] to [3] above. Effect of the Invention
[0024] According to the present invention, it is possible to provide a three-phase three-legged wound core that is excellent in the effects of reducing transformer iron loss and reducing noise.
[0025] According to the present invention, by using grain-oriented electrical steel sheets having a lower magnetic flux density at 800 A / m in the inner part of the outer core and the outer part of the inner core of a three-phase three-legged wound core than in the other parts, it is possible to reduce transformer iron loss and transformer noise. According to the present invention, it is possible to suppress magnetic flux transfer between layers even when the excitation magnetic flux density is relatively high, thereby reducing transformer iron loss and transformer noise. [Brief description of the drawings]
[0026] [Figure 1] FIG. 1 is a diagram (side view) that illustrates the shape of a three-phase, three-legged wound core and the concentration of magnetic flux on the inner core. [Diagram 2] FIG. 2 is a diagram (side view) that typically shows magnetic flux transfer from the outer core to the inner core when the excitation magnetic flux density increases. [Diagram 3] FIG. 3 is a side view showing the configuration of a three-phase, three-legged wound core of the present invention. [Figure 4] FIG. 4 is a diagram (side view) that illustrates a schematic diagram of the flow of magnetic flux in the inner part of the outer core and the outer part of the inner core in a three-phase three-legged wound core. [Diagram 5] FIG. 5 is a diagram showing the relationship between the magnetic flux density B8 of the iron core material and the iron loss of the transformer. [Figure 6] FIG. 6 is a diagram showing the relationship between the magnetic flux density B8 of the iron core material and the transformer noise. [Figure 7] FIG. 7 is a diagram showing the relationship between magnetic flux density B8 in the inner core material and transformer iron loss. [Figure 8] FIG. 8 is a diagram showing the relationship between magnetic flux density B8 of the inner core material and transformer noise. [Figure 9] FIG. 9 is a diagram showing the relationship between the ratio (t / s) of thickness of the region of the outer core material to the region of the inner core material and the transformer iron loss. [Figure 10] FIG. 10 is a diagram showing the relationship between the ratio (t / s) of thickness of the region of the outer core material to the region of the inner core material and transformer noise. [Figure 11] FIG. 11 is a side view showing the configuration of a three-phase, three-legged wound core produced in an example. [Figure 12] FIG. 12 is a side view showing the configuration of a three-phase, three-legged wound core produced in an example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0027] The present invention will be specifically described below.
[0028] First, the reasons for restricting the constituent elements of the present invention will be described.
[0029] It was revealed that in the transformer iron loss of a three-phase three-limbed wound core transformer using a three-phase three-limbed wound core, a flow of magnetic flux occurs from the non-excited leg to the excited leg, which results in magnetic flux transfer from the outer core 2 to the inner core 1, and that magnetic flux transfer is one of the factors that increases the transformer iron loss.
[0030] Since magnetic flux transfer is a phenomenon that occurs through the part where outer core 2 and inner core 1 are in contact, it is expected that the iron loss of the transformer will be reduced by using grain-oriented electrical steel sheet with a low magnetic flux density B8 at 800 A / m to limit the amount of magnetic flux possible for magnetic flux transfer to the inner part of outer core 2 and the outer part of inner core 1, which are close to the contact points.
[0031] Generally, in a three-phase three-legged wound core, if the magnetic flux density B8 at 800A / m of the grain-oriented electromagnetic steel sheet that is the core material is low, the core material's core loss will be poor, and so will the transformer's core loss. Also, with regard to transformer noise, it is known that with a core material that has a low magnetic flux density B8 at 800A / m, magnetostriction, which is the elongation of the steel sheet when the core material is excited, becomes large, and the increased magnetostrictive vibrations also increase the transformer noise.
[0032] A three-phase three-legged wound core with the shape shown in Figure 1 was made using materials with different magnetic flux densities B8 of the core material shown in Table 2, and the results of measuring the transformer iron loss and transformer noise are shown in Figures 5 and 6, respectively. As the magnetic flux density B8 of the grain-oriented electrical steel sheet, which is the core material, increases, there is a tendency for both the transformer iron loss and the transformer noise to improve. The amount of improvement is saturated at a magnetic flux density B8 of 1.88T or more, so the preferred range for the magnetic flux density B8 of the core material is set to 1.88T or more.
[0033] [Table 2]
[0034] In order to find the optimum range of magnetic flux density of the inner core material applied to the inner part of the outer core and the outer part of the inner core, a material with magnetic flux density B8 of 1.92T (grain-oriented electromagnetic steel sheet) was used as the outer core material applied to the outer part of the outer core and the inner part of the inner core, the magnetic flux density of the inner core material was changed, and the transformer iron loss and transformer noise were measured when the thickness ratio of the thickness t of the outer core material area to the thickness s of the inner core material was set to t / s = 0.25. The magnetic flux density B8 of the inner core material is shown in Table 3, and the measurement results of the transformer iron loss and transformer noise are shown in Figures 7 and 8, respectively.
[0035] [Table 3]
[0036] When the magnetic flux density B8 of the inner core material is lower than the magnetic flux density B8 of the reference outer core material, both characteristics (transformer iron loss and transformer noise) were found to improve. However, when the magnetic flux density B8 of the inner core material is less than 1.83 T, both characteristics tend to deteriorate, and the improvement rate decreases. This deterioration is presumably because the improvement of both characteristics due to the suppression of magnetic flux crossing between layers is suppressed by the deterioration of both characteristics due to the use of an iron core material with a lower magnetic flux density B8.
[0037] Furthermore, we investigated the thickness ratio between the outer core material and the inner core material that improves transformer iron loss and transformer noise. A material with a B8 of 1.92T (grain-oriented electromagnetic steel sheet) was used for the outer part of the outer core and the inner part of the inner core, and a material with a B8 of 1.88T was used for the inner part of the outer core and the outer part of the inner core, respectively, and a three-phase three-legged wound core was manufactured by changing the ratio (t / s) of the thickness t of the outer core material region to the thickness s of the inner core material region as shown in Table 4, and the transformer iron loss and transformer noise were measured. Figures 9 and 10 show the measurement results of the transformer iron loss and transformer noise, respectively.
[0038] [Table 4]
[0039] A significant improvement was seen in both transformer iron loss and transformer noise when the thickness ratio (t / s) between the area of the outer core material and the area of the inner core material was greater than or equal to 1. This is thought to be because the reduction in the amount of magnetic flux passing between layers by using an inner core material that exhibits a low magnetic flux density of B8 within the above ratio range was able to greatly exceed the deterioration in transformer iron loss and transformer noise caused by using a material with a low magnetic flux density of B8.
[0040] From the above experimental results, it can be said that as a characteristic of the core material used for a three-phase three-legged wound core, a higher magnetic flux density B8 at 800 A / m is preferable, with grain-oriented electrical steel sheets of 1.88 T or more being preferable as high B8 materials, and grain-oriented electrical steel sheets of 1.83 T or more being preferable as low B8 materials. That is, in the present invention, when a high B8 material with a high magnetic flux density at 800 A / m is designated as grain-oriented electrical steel sheet A, and a low B8 material with a lower magnetic flux density at 800 A / m than that of grain-oriented electrical steel sheet A is designated as grain-oriented electrical steel sheet B, the magnetic flux density at 800 A / m of the grain-oriented electrical steel sheet A is preferably 1.88 T or more, and the magnetic flux density at 800 A / m of the grain-oriented electrical steel sheet B is preferably 1.83 T or more.
[0041] Furthermore, when using a combination of high B8 material (grain-oriented electrical steel sheet A) and low B8 material (grain-oriented electrical steel sheet B), if the proportion of low B8 material increases, the B8 of the entire transformer decreases, and the improvement in transformer iron loss and transformer noise decreases. A particularly suitable range where this improvement is large is when, when viewed from the side of the wound core, the thickness s of the region made up of the inner core material (grain-oriented electrical steel sheet B) is equal to or less than the thickness t of the region made up of the outer core material (grain-oriented electrical steel sheet A), i.e., t / s ≧ 1.0.
[0042] The properties, components, manufacturing method, etc. of the grain-oriented electrical steel sheet other than those described above are not particularly limited. Furthermore, the height, width, depth, shape such as curvature of corners, and manufacturing method of the three-phase three-legged wound core are also not particularly limited.
[0043] However, when a magnetic domain refined material in which the core material has been subjected to a magnetic domain refinement process in which grooves are formed on the surface to reduce the core material's iron loss is used as the core material (grain-oriented electromagnetic steel sheet) used in a three-phase three-legged wound core, the magnetic flux density B8 at 800 A / m decreases due to a reduction in the amount of base iron when the grooves are formed, but since the magnetic permeability does not decrease, the magnetic flux density B8 of the base material (grain-oriented electromagnetic steel sheet after groove formation) plus 0.04 T is usually used as the effective magnetic flux density B8 equivalent to the magnetic permeability. Therefore, when such a magnetic domain refined material is applied to the present invention, the value obtained by adding 0.04 T to the magnetic flux density B8 of the base material (grain-oriented electromagnetic steel sheet after groove formation) can be applied to the constituent elements of the present invention.
[0044] In addition, although the present specification describes the characteristics of a three-phase, three-leg wound core transformer, the present invention is also suitable for application to other three-phase wound core transformers, for example, a three-phase, five-leg wound core transformer. EXAMPLES
[0045] [Example 1] A three-phase, three-legged wound core was fabricated using the core shapes (wound core A, wound core B) shown in Figure 11 and the core materials shown in Table 5, and then stress relief annealed at 800°C for 2 hours. A 50-turn winding coil was attached to fabricate a three-phase, three-legged wound core transformer. Excitation was performed under conditions of an excitation flux density of 1.7T and a frequency of 50Hz, and the transformer iron loss, interlayer crossover iron loss, and transformer noise were measured using the methods described above.
[0046] The results are shown in Table 5. The compatible examples of the present invention were found to have excellent transformer characteristics, with better transformer iron loss and transformer noise, compared to the comparative example (a three-phase three-legged wound core using high B8 material with a high magnetic flux density at 800 A / m as the inner core material and low B8 material with a low magnetic flux density at 800 A / m as the outer core material).
[0047] [Table 5]
[0048] [Example 2] A three-phase, three-legged wound core was fabricated using the core shape (wound core A) shown in Figure 12 and the core material shown in Table 6, which was then subjected to stress relief annealing at 800°C for two hours, and a 50-turn winding coil was attached to fabricate a three-phase, three-legged wound core transformer. Excitation was performed under conditions of an excitation flux density of 1.7T and a frequency of 50Hz, and the transformer iron loss, interlayer iron loss, and transformer noise were measured using the methods described above. Note that the outer core material used was a magnetic domain refined material in which grooves were formed on the surface of the steel sheet by laser etching.
[0049] The results are shown in Table 6. The B8 value of the outer core material was calculated by adding 0.04T to the B8 value of the base material (grain-oriented electrical steel sheet after groove formation). When the B8 value of the outer core material was 1.84T or more, improvements in the transformer iron loss and transformer noise were observed, and when the B8 value of the outer core material was 1.88T or more, significant improvements in the transformer iron loss and transformer noise were observed. In this way, it was found that the magnetic domain refinement material produced by groove formation can be applied to the present invention by adding 0.04T to the magnetic flux density B8 value of the base material (grain-oriented electrical steel sheet after groove formation), and exhibits excellent transformer characteristics.
[0050] [Table 6]
Claims
1. A three-phase three-legged wound core including an outer core and two inner cores adjacent to each other and disposed inside the outer core, the outer core and the two inner cores are each made of at least two types of grain-oriented electrical steel sheets having different magnetic flux densities at 800 A / m, A three-phase three-legged wound core, in which the inner portion of the outer core and the outer portions of the two inner cores are made of grain-oriented electromagnetic steel sheets having a lower magnetic flux density at 800 A / m than the grain-oriented electromagnetic steel sheets constituting the outer portion of the outer core and the inner portions of the two inner cores.
2. The grain-oriented electromagnetic steel sheet constituting the inner part of the outer core and the outer parts of the two inner cores is called grain-oriented electromagnetic steel sheet B. When the grain-oriented electromagnetic steel sheet constituting the outer portion of the outer core and the inner portions of the two inner cores is referred to as grain-oriented electromagnetic steel sheet A, The grain-oriented electrical steel sheet A has a magnetic flux density of 1.88 T or more at 800 A / m, 2. The three-phase, three-legged wound core according to claim 1, wherein the magnetic flux density of the grain-oriented electrical steel sheet B at 800 A / m is 1.83 T or more and is lower than the magnetic flux density of the grain-oriented electrical steel sheet A.
3. In side view, The thickness of the outer portion of the outer core and the inner portions of the two inner cores is t, When the thickness of the inner part of the outer core and the outer parts of the two inner cores is s, 3. The three-phase, three-legged wound core according to claim 1, wherein t / s≧1.0 is satisfied.
4. A three-phase, three-legged wound core transformer using the three-phase, three-legged wound core according to any one of claims 1 to 3.
Citation Information
Patent Citations
Method of joining dental adding device to tooth
JP1977086292A
Coiled steel core for transformer
JP1980052207A
Waste straw transfer apparatus of waste straw cutter
JP1982050820A
Iron core of transformer
JP1991268311A
Grain oriented silicon steel containing super high