High-strength and high-temperature-resistant powder core and preparation method and application thereof

Through vacuum impregnation and baking process of impregnating liquid containing components such as silicone resin and silicate, a mesh structure is formed, which solves the problem of insufficient strength and high temperature resistance of the powder core, and significantly improves the performance and service life of the magnetic core.

CN118983183APending Publication Date: 2024-11-19HENGDIAN GRP DMEGC MAGNETICS CO LTD +1
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411201133.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The impregnating liquid used in the prior art for magnetic cores cannot effectively improve the strength and high temperature resistance of the powder core, resulting in poor structural stability and failure of the magnetic core during long-term use.

Method used

Using modified silicone resin and silicate as the main components impregnation liquid, combined with epoxy resin, phenolic resin, polyvinyl alcohol, acrylate and curing accelerator, a mesh structure is formed to enhance the powder through vacuum impregnation and baking processes. The strength and heat resistance of the core.

Benefits of technology

It significantly improves the strength, heat resistance and chemical resistance of the powder core, extends the service life of the magnetic core, and ensures stability under high temperature conditions.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the technical field of magnetic material preparation, and particularly relates to a high-strength and high-temperature-resistant powder core and a preparation method and application thereof. The preparation method comprises the steps that a sintered powder core is placed in impregnation liquid to be subjected to vacuum impregnation and baking, and the high-strength and high-temperature-resistant powder core is obtained; the impregnation liquid comprises modified silicon resin and silicate; the impregnation liquid further comprises at least one of epoxy resin, phenolic resin, polyvinyl alcohol, acrylate and a curing accelerator; the baking temperature ranges from 180 DEG C to 220 DEG C. The preparation method can solve the problems of poor long-term high temperature resistance and strength of the existing powder core, and the powder core has the advantages of high strength, long-term high temperature resistance and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of magnetic material preparation, and in particular relates to a high-strength and high-temperature resistant powder core and a preparation method and application thereof. Background Art

[0002] Alloy magnetic powder cores are widely used in automotive, telecommunications, computers, control systems and other fields, including silicon-aluminum, iron-nickel, iron-silicon and other alloys. Because the magnetic core needs to be sintered at high temperature, the bonding between the powder particles uses a high-temperature resistant inorganic adhesive, but this type of adhesive has poor bonding effect and poor core strength, so the impregnation method is used after sintering to improve the core strength. The commonly used impregnation liquid is epoxy resin with high viscosity. This type of resin has poor permeability. Due to the poor temperature resistance of epoxy resin, the magnetic core will cause aging and decomposition of organic matter in long-term operation, which in turn affects the stability of the structure, such as the core strength, and causes the core to fail during application.

[0003] The prior art provides a soft magnetic powder core impregnation liquid, which includes methacrylate monomers, epoxy resins, curing agents and other ingredients. Since the basic components are methacrylate monomers and epoxy resins, the temperature resistance of the powder core deteriorates and cannot meet long-term temperature resistance requirements. Summary of the invention

[0004] Therefore, the technical problem to be solved by the present invention is to overcome the defects of the impregnation liquid used in the prior art that the strength and high temperature resistance of the powder core cannot be guaranteed, thereby providing a high-strength and high-temperature resistant powder core and a preparation method thereof.

[0005] To this end, the present invention provides the following technical solutions.

[0006] The first aspect of the present invention provides a method for preparing a high-strength and high-temperature resistant powder core, comprising: placing a sintered powder core in an impregnation liquid for vacuum impregnation, and baking to obtain the high-strength and high-temperature resistant powder core;

[0007] The impregnation liquid includes modified silicone resin and silicate;

[0008] The impregnation liquid further comprises at least one of epoxy resin, phenolic resin, polyvinyl alcohol, acrylate and curing accelerator;

[0009] The baking temperature is 180-220° C., wherein the baking temperature can be any value among 180° C., 185° C., 190° C., 195° C., 200° C., 205° C., 210° C., 215° C., and 220° C.

[0010] The preparation method of the present invention can solve the defects of the prior art powder core in long-term high temperature resistance and poor strength, so that the powder core has high strength, high temperature resistance and other properties. The present invention places the sintered powder core in an impregnation liquid for vacuum impregnation, and the impregnation liquid includes modified silicone resin and silicate, and also includes at least one of epoxy resin, phenolic resin, polyvinyl alcohol, acrylate and curing accelerator. A mesh structure is formed inside the impregnation liquid to resist the stress of the powder core material, increase the strength and toughness of the powder core, and thus improve the strength, heat resistance and chemical resistance of the powder core. Then, baking at 180-220°C can keep the components in the impregnation liquid in the powder core, ensuring that the impregnation liquid can fully play its role, thereby improving the strength and high temperature resistance of the powder core.

[0011] It should be noted that the impregnation liquid is in a fluid state, the modified silicone resin is in a liquid state, the silicate is in a liquid state, and the epoxy resin, phenolic resin, polyvinyl alcohol, acrylate and curing accelerator are in a liquid state.

[0012] The impregnation liquid includes modified silicone resin and silicate, and also includes at least one of epoxy resin, phenolic resin, polyvinyl alcohol, acrylate and curing accelerator; after all the raw materials are mixed to form the impregnation liquid, a diluent can be added to the impregnation liquid according to the use requirements. The amount and type of the diluent added in the present invention are not specifically limited, and common diluents in the field, such as acetate, polyol, etc. are used. The viscosity of the impregnation liquid is generally 10000-18000mPa.s / 25℃. It should also be noted here that the diluent is not a necessary component of the impregnation liquid and is added according to the needs.

[0013] The curing accelerator is a common type of auxiliary agent in the art, such as a substituted urea curing agent.

[0014] The mass ratio of the modified silicone resin to the silicate is (50-65):(10-15); for example, the mass ratio of the modified silicone resin to the silicate can be any ratio of 65:15, 60:12, 55:13, 50:15, 55:10, 53:13, etc.

[0015] Preferably, the mass ratio of at least one of the epoxy resin, phenolic resin, polyvinyl alcohol, acrylate and curing accelerator to the modified silicone resin and the silicate is (50-65):(10-15):(20-40);

[0016] Preferably, the silicate is sodium silicate;

[0017] Preferably, the modified silicone resin is an epoxy resin modified silicone resin.

[0018] The impregnation liquid comprises modified silicone resin, sodium silicate and epoxy resin.

[0019] Preferably, the impregnation liquid comprises modified silicone resin, sodium silicate and epoxy resin in a mass ratio of (50-65):(10-15):(20-40); for example, the mass ratio of modified silicone resin, sodium silicate and epoxy resin can be any ratio of 50:10:40, 53:13:34, 55:15:30, 60:10:30, 60:12:28, 63:12:25, 65:15:20, etc.

[0020] Preferably, the impregnation liquid comprises epoxy resin-modified silicone resin, sodium silicate and epoxy resin in a mass ratio of (50-65):(10-15):(20-40).

[0021] Among them, modified silicone resin and silicate can improve the high temperature resistance of the powder core, epoxy resin, phenolic resin, etc. can ensure the strength of the powder core, and dispersing silicate in epoxy resin and other materials can form a network structure to resist stress and strain and increase material strength and toughness. By controlling the synergistic effect of the effective ingredients in the impregnation liquid, the strength, toughness and high temperature resistance of the powder core can be guaranteed. In particular, when the impregnation liquid includes epoxy resin modified silicone resin, sodium silicate and epoxy resin, the powder core effect is the best.

[0022] The baking time is 1-3 hours. For example, the baking time can be 1 hour, 2 hours, 3 hours, etc.

[0023] The vacuum impregnation conditions are as follows: the vacuum degree is not less than 1 atmosphere, and the impregnation time is 30-60 minutes.

[0024] The present invention adopts vacuum impregnation, which can make the impregnation liquid penetrate into the air gap inside the powder core and improve the strength compared with ordinary impregnation. And sintering before vacuum impregnation can further improve the density, mechanical strength and electrical properties of the powder core. The present invention can improve the performance of the alloy powder by the process of sintering first, vacuum impregnation and then baking.

[0025] The sintering temperature is 680-750° C. and the sintering time is 4-5 hours.

[0026] Before sintering, the alloy powder and the coating agent are mixed for insulation coating, annealing, and pressing;

[0027] Preferably, the alloy powder is at least one of iron silicon, iron silicon aluminum, and iron nickel;

[0028] Preferably, the coating agent is at least one of chromic acid, phosphoric acid, kaolin, silica sol, and liquid aluminum phosphate; wherein the liquid aluminum phosphate is an aluminum phosphate solution with a solid content of 50%;

[0029] Preferably, the coating agent is used in an amount of 0.1-1.0wt% of the alloy powder. For example, the coating agent is used in an amount of any value among 0.1wt%, 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt%, 1.0wt% and the like of the alloy powder.

[0030] It should be noted that: when performing insulation coating, some coating agents need to be mixed with alloy powders and water needs to be added, and the purpose of adding water is to improve the uniformity of coating; for example, phosphoric acid needs to be mixed with alloy powders and water needs to be added, and there is no specific limit on the amount of water added, such as 10wt% of the alloy powder. Some coating agents can be directly mixed with alloy powders, such as kaolin. Whether to add water during insulation coating is well known in the art and will not be repeated here.

[0031] The present invention has no requirement on the particle size of the alloy powder, and conventional powder is used, for example, the mesh size of the alloy powder can be 200 mesh, 500 mesh, 600 mesh, etc.

[0032] The step of adding a binder and granulating is included before the compression molding;

[0033] Preferably, the adhesive is a silicone resin;

[0034] Preferably, the amount of the adhesive is 1.0-2.0wt% of the alloy powder;

[0035] Preferably, the annealing temperature is 800-820°C and the time is 4-6h;

[0036] Preferably, the compression molding pressure is 17-21T / cm 2 .

[0037] The second aspect of the present invention provides a powder core obtained by the above preparation method.

[0038] A third aspect of the present invention provides an inductor device, comprising the powder core obtained by the above preparation method.

[0039] The technical solution of the present invention has the following advantages:

[0040] 1. The preparation method of the high-strength and high-temperature resistant powder core provided by the present invention comprises placing the sintered powder core in an impregnation liquid for vacuum impregnation and baking to obtain the high-strength and high-temperature resistant powder core; the impregnation liquid comprises modified silicone resin and silicate; the impregnation liquid also comprises at least one of epoxy resin, phenolic resin, polyvinyl alcohol, acrylate and curing accelerator; the baking temperature is 180-220°C. The preparation method can solve the problems of long-term high temperature resistance and poor strength of the existing powder core, and make the powder core have the advantages of high strength and long-term high temperature resistance. The impregnation liquid of the present invention comprises modified silicone resin, silicate, and at least one of epoxy resin, phenolic resin, polyvinyl alcohol, acrylate and curing accelerator. A mesh structure is formed inside the impregnation liquid to resist the stress of the powder core material, increase the strength and toughness of the powder core, and further improve the strength, heat resistance, chemical resistance and other properties of the powder core. After sintering, vacuum impregnation is performed and baking is performed at 180-220°C, so that the components in the impregnation liquid can remain in the powder core, ensuring that the impregnation liquid can fully play its role and improving the strength and high temperature resistance of the powder core. Modified silicone resin and silicate in the impregnation liquid can improve the high temperature resistance of the powder core, at least one of epoxy resin, phenolic resin, polyvinyl alcohol, acrylate and curing accelerator can ensure that the powder core has sufficient strength, and silicate can be evenly dispersed in epoxy resin and other substances to form a network structure, which can resist stress and strain and increase the strength and toughness of the material; modified silicone resin can be used as a reinforcing agent for epoxy resin and other substances to overcome the defects of epoxy resin such as poor toughness, poor heat resistance and poor chemical resistance, and improve the formability and handling of epoxy resin and other substances. Using these substances as impregnation liquid can ensure that the powder core has high strength, high toughness and high temperature resistance.

[0041] 2. The preparation method of the high-strength and high-temperature resistant powder core provided by the present invention, when the impregnation liquid of the present invention especially includes epoxy resin-modified silicone resin, sodium silicate and epoxy resin, the epoxy resin-modified silicone resin cooperates with the sodium silicate and epoxy resin to exert synergistic effects, and the obtained powder core has the best effect.

[0042] Compared with ordinary impregnation, vacuum impregnation allows the impregnation liquid to penetrate into the air gap inside the powder core, thereby improving the strength. Sintering before vacuum impregnation can improve the density, mechanical strength and electrical properties of the powder core; during the sintering process, the alloy powder forms a dense material, thereby improving the performance of the powder core. DETAILED DESCRIPTION

[0043] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0044] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.

[0045] The raw materials used in the following examples and comparative examples, such as iron-nickel powder, phosphoric acid, silicone resin, epoxy resin, epoxy resin-modified silicone resin, can be obtained commercially. Among them, silicone resin, epoxy resin, epoxy resin-modified silicone resin can also be prepared by conventional methods provided by the prior art.

[0046] For example, the manufacturer and model of epoxy resin modified silicone resin is: Jinwangxing JWX-175; the manufacturer and model of silicone resin is: Shenzhen Dypu DM7470. Here, one manufacturer and model of the raw materials are listed respectively, but the raw materials of the present invention are not limited to these two manufacturers.

[0047] Example 1

[0048] This embodiment provides a method for preparing a high-strength and high-temperature resistant powder core, comprising the following steps:

[0049] (1) Take an iron-nickel powder with a particle size of -500 mesh, weigh phosphoric acid (analytical grade) according to 0.2% of the weight of the iron-nickel powder, mix the phosphoric acid with water to obtain a phosphoric acid aqueous solution, the amount of water used is 10wt% of the iron-nickel powder, then add the iron-nickel powder to the phosphoric acid aqueous solution for insulation coating, anneal at 810° C. for 5 h, add 1.0wt% of organic silicon resin, and granulate; at a pressure of 20T / cm 2 Press down to form.

[0050] (2) The powder core obtained by compression molding is sintered at 700°C for 4.5 hours; then, the sintered powder core is placed in an impregnation liquid for vacuum impregnation at room temperature, and after the impregnation, it is baked at 200°C for 1 hour to obtain a powder core.

[0051] The impregnation liquid includes epoxy resin modified silicone resin, sodium silicate and epoxy resin in a mass ratio of 65:15:20, and the viscosity of the impregnation liquid satisfies 10000-18000 mPa.s / 25° C. The vacuum impregnation is carried out under one atmosphere, and the impregnation time is 0.5 h.

[0052] Example 2

[0053] This embodiment provides a method for preparing a high-strength and high-temperature resistant powder core, comprising the following steps:

[0054] (1) Take an iron-nickel powder with a particle size of -500 mesh, weigh phosphoric acid (analytical grade) according to 0.5wt% of the iron-nickel powder, mix it with water to obtain a phosphoric acid aqueous solution, the amount of water added is 10wt% of the iron-nickel powder, then add the iron-nickel powder into the phosphoric acid aqueous solution for insulation coating, then anneal at 810°C for 5h, then add 1.2wt% of organic silicon resin, granulate; then at a pressure of 20T / cm 2 Press down to form.

[0055] (2) The powder core obtained by compression molding is sintered at 700° C. for 5 h. Then, the sintered powder core is placed in an impregnation liquid for vacuum impregnation at room temperature. After the impregnation, the powder core is baked at 200° C. for 1 h to obtain a powder core.

[0056] The impregnation liquid includes epoxy resin modified silicone resin, sodium silicate and epoxy resin in a mass ratio of 60:12:28, and the viscosity of the impregnation liquid satisfies 10000-18000 mPa.s / 25° C. The vacuum impregnation is carried out under one atmosphere, and the impregnation time is 0.5 h.

[0057] Example 3

[0058] This embodiment provides a method for preparing a high-strength and high-temperature resistant powder core, comprising the following steps:

[0059] (1) Take a Fe-Si-Al powder with a particle size of -500 mesh, weigh phosphoric acid (analytical grade) according to 0.5wt% of Fe-Ni powder, mix it with water to obtain a phosphoric acid aqueous solution, the amount of water added is 10wt% of Fe-Ni powder, then add Fe-Ni powder into the phosphoric acid aqueous solution for insulation coating, then anneal at 810°C for 5h, then add 1.2wt% of organic silicon resin, granulate; then at a pressure of 20T / cm 2 Press down to form.

[0060] (2) The powder core obtained by compression molding is sintered at 700° C. for 5 h. Then, the sintered powder core is placed in an impregnation liquid for vacuum impregnation at room temperature. After the impregnation, the powder core is baked at 200° C. for 1 h to obtain a powder core.

[0061] The impregnation liquid includes epoxy resin modified silicone resin, sodium silicate and epoxy resin in a mass ratio of 65:15:20, and the viscosity of the impregnation liquid satisfies 10000-18000 mPa.s / 25° C. The vacuum impregnation is carried out under one atmosphere, and the impregnation time is 0.5 h.

[0062] Example 4

[0063] This embodiment provides a method for preparing a high-strength and high-temperature resistant powder core, comprising the following steps:

[0064] (1) Take iron-nickel powder with a particle size of -500 mesh, weigh kaolin according to 0.2wt% of the iron-nickel powder and add it to the iron-nickel powder for insulation coating, then anneal at 810°C for 5h, then add 1.2wt% of organic silicon resin and granulate; then 2 Press down to form.

[0065] (2) The powder core obtained by compression molding is sintered at 710° C. for 4 h. Then, the sintered powder core is placed in an impregnation liquid for vacuum impregnation at room temperature. After the impregnation, the powder core is baked at 190° C. for 2 h to obtain a powder core.

[0066] The impregnation liquid includes epoxy resin modified silicone resin, sodium silicate and epoxy resin in a mass ratio of 65:15:20, and the viscosity of the impregnation liquid satisfies 10000-18000 mPa.s / 25° C. The vacuum impregnation is carried out under one atmosphere, and the impregnation time is 0.5 h.

[0067] Comparative Example 1

[0068] This comparative example provides a method for preparing a powder core, comprising the following steps:

[0069] (1) Take an iron-nickel powder with a particle size of -500 mesh, weigh phosphoric acid (analytical grade) according to 0.2% of the weight of the iron-nickel powder, mix the phosphoric acid with water to obtain a phosphoric acid aqueous solution, the amount of water used is 10wt% of the iron-nickel powder, then add the iron-nickel powder to the phosphoric acid aqueous solution for insulation coating, anneal at 810° C. for 5 h, add 1.0wt% of organic silicon resin, and granulate; at a pressure of 20T / cm 2 Press down to form.

[0070] (2) The powder core obtained by compression molding is sintered at 700°C for 4.5 hours; then, the sintered powder core is placed in an impregnation liquid for vacuum impregnation at room temperature, and after the impregnation, it is baked at 200°C for 1 hour to obtain a powder core.

[0071] The impregnation liquid is epoxy resin, and the viscosity of the impregnation liquid satisfies 10000-18000 mPa.s / 25° C. The vacuum impregnation is carried out under one atmosphere, and the impregnation time is 0.5 h.

[0072] Comparative Example 2

[0073] This comparative example provides a method for preparing a powder core, comprising the following steps:

[0074] (1) Take an iron-nickel powder with a particle size of -500 mesh, weigh phosphoric acid (analytical grade) according to 0.5wt% of the iron-nickel powder, mix it with water to obtain a phosphoric acid aqueous solution, the amount of water added is 10wt% of the iron-nickel powder, then add the iron-nickel powder into the phosphoric acid aqueous solution for insulation coating, then anneal at 810°C for 5h, then add 1.2wt% of organic silicon resin, granulate; then at a pressure of 20T / cm 2 Press down to form.

[0075] (2) The powder core obtained by compression molding is sintered at 700° C. for 5 h. Then, the sintered powder core is placed in an impregnation liquid for vacuum impregnation at room temperature. After the impregnation, the powder core is baked at 200° C. for 1 h to obtain a powder core.

[0076] The impregnation liquid includes epoxy resin, and the viscosity of the impregnation liquid satisfies 10000-18000 mPa.s / 25° C. The vacuum impregnation is performed under an atmospheric pressure, and the impregnation time is 0.5 h.

[0077] Comparative Example 3

[0078] This comparative example provides a method for preparing a powder core, comprising the following steps:

[0079] (1) Take a Fe-Si-Al powder with a particle size of -500 mesh, weigh phosphoric acid (analytical grade) according to 0.5wt% of Fe-Ni powder, mix it with water to obtain a phosphoric acid aqueous solution, the amount of water added is 10wt% of Fe-Ni powder, then add Fe-Ni powder into the phosphoric acid aqueous solution for insulation coating, then anneal at 810°C for 5h, then add 1.2wt% of organic silicon resin, granulate; then at a pressure of 20T / cm 2 Press down to form.

[0080] (2) The powder core obtained by compression molding is sintered at 700° C. for 5 h. Then, the sintered powder core is placed in an impregnation liquid for vacuum impregnation at room temperature. After the impregnation, the powder core is baked at 200° C. for 1 h to obtain a powder core.

[0081] The impregnation liquid includes epoxy resin, and the viscosity of the impregnation liquid satisfies 10000-18000 mPa.s / 25° C. The vacuum impregnation is performed under an atmospheric pressure, and the impregnation time is 0.5 h.

[0082] Comparative Example 4

[0083] This comparative example provides a method for preparing a powder core, comprising the following steps:

[0084] (1) Take an iron-nickel powder with a particle size of -500 mesh, weigh phosphoric acid (analytical grade) according to 0.2% of the weight of the iron-nickel powder, mix the phosphoric acid with water to obtain a phosphoric acid aqueous solution, the amount of water used is 10wt% of the iron-nickel powder, then add the iron-nickel powder to the phosphoric acid aqueous solution for insulation coating, anneal at 810° C. for 5 h, add 1.0wt% of organic silicon resin, and granulate; at a pressure of 20T / cm 2 Press down to form.

[0085] (2) The powder core obtained by compression molding is sintered at 700°C for 4.5 hours; then, the sintered powder core is placed in an impregnation liquid for vacuum impregnation at room temperature, and after the impregnation, it is baked at 200°C for 1 hour to obtain a powder core.

[0086] The impregnation liquid includes epoxy resin modified silicone resin and epoxy resin in a mass ratio of 65:20, and the viscosity of the impregnation liquid satisfies 10000-18000 mPa.s / 25° C. The vacuum impregnation is performed under one atmosphere, and the impregnation time is 0.5 h.

[0087] Test Case

[0088] This test example provides the properties of the powder cores prepared in each embodiment and comparative example, as follows:

[0089] Magnetic permeability test method: Take the standard ring to measure the size and wind it 20 turns of copper wire, test conditions 100kHz, 1V, test instrument HP4284 inductance tester, the measured inductance value can be converted into magnetic permeability, the results are shown in Table 1.

[0090] Strength test method: Place the powder core on the strength tester, move the test probe downward at a speed of 20mm / min until the core breaks, and read the strength test value.

[0091] Testing method for magnetic loss Pv: Two wire groups are wound with copper wire, N1=20Ts, N2=5Ts, test conditions are shown in Table 1, test equipment is SY8218 tester, and results are shown in Table 1.

[0092] Test method for high temperature resistance: Test the inductance of the powder core after it works at 200±10℃ for 1000h, and calculate whether the change rate of inductance before and after work exceeds ±10%.

[0093] Table 1 Test results of the powder cores of the embodiments and comparative examples

[0094] Example Magnetic Permeability Strength N Loss @50kHz / 100mT High temperature resistance Example 1 127 647 166 OK Example 2 95.2 665 186 OK Example 3 85.8 544 95 OK Example 4 93 612 190 OK Comparative Example 1 125.4 576 281 NG Comparative Example 2 93.4 588 193 NG Comparative Example 3 83.1 489 105 NG Comparative Example 4 132 590 212 OK

[0095] Note: OK means the change rate of inductance before and after operation does not exceed ±10%; NG means the change rate of inductance before and after operation exceeds ±10%.

[0096] It can be seen from the above results that by adopting the method of the present invention to vacuum impregnate the sintered powder core in the impregnation liquid and then bake it, a powder core with high strength and high temperature resistance can be obtained.

[0097] From comparative examples 1 to 3, the loss of the powder core obtained by using epoxy resin as the impregnation liquid is higher than that of the powder core obtained by using the specific impregnation liquid of the present invention, the strength is reduced, and the high temperature resistance is poor. Comparison between Example 1 and Comparative example 4 shows that the introduction of sodium silicate into the impregnation liquid of the present invention helps to improve the strength and reduce the loss.

[0098] From Examples 1-4, the impregnation liquid of the present invention includes modified silicone resin, silicate, and at least one of epoxy resin, phenolic resin, polyvinyl alcohol, acrylate and curing accelerator. The powder core after sintering is impregnated under vacuum conditions and baked to obtain a powder core with high strength and high temperature resistance. The powder core also has the advantage of low loss.

[0099] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.

Claims

1. A method for preparing a high-strength and high-temperature resistant powder core, characterized in that: include: The sintered powder core is placed in an impregnation liquid for vacuum impregnation, and then baked to obtain the high-strength and high-temperature resistant powder core; The impregnation liquid includes modified silicone resin and silicate; The impregnation liquid further comprises at least one of epoxy resin, phenolic resin, polyvinyl alcohol, acrylate and curing accelerator; The baking temperature is 180-220°C.

2. The preparation method according to claim 1, characterized in that: The mass ratio of the modified silicone resin to the silicate is (50-65):(10-15); Preferably, the mass ratio of at least one of the epoxy resin, phenolic resin, polyvinyl alcohol, acrylate and curing accelerator to the modified silicone resin and the silicate is (50-65):(10-15):(20-40); Preferably, the silicate is sodium silicate; Preferably, the modified silicone resin is an epoxy resin modified silicone resin.

3. The preparation method according to claim 1 or 2, characterized in that: The impregnation liquid comprises modified silicone resin, sodium silicate and epoxy resin.

4. The preparation method according to any one of claims 1 to 3, characterized in that The baking time is 1-3h.

5. The preparation method according to any one of claims 1 to 4, characterized in that: The vacuum impregnation conditions are as follows: the vacuum degree is not less than 1 atmosphere, and the impregnation time is 30-60 minutes.

6. The preparation method according to any one of claims 1 to 5, characterized in that: The sintering temperature is 680-750° C. and the sintering time is 4-5 hours.

7. The preparation method according to any one of claims 1 to 6, characterized in that: Before sintering, the alloy powder and the coating agent are mixed for insulation coating, annealing, and pressing; Preferably, the alloy powder is at least one of iron silicon, iron silicon aluminum, and iron nickel; Preferably, the coating agent is at least one of chromic acid, phosphoric acid, kaolin, silica sol, and liquid aluminum phosphate; Preferably, the coating agent is used in an amount of 0.1-1.0 wt % of the alloy powder.

8. The preparation method according to claim 7, characterized in that: The step of adding a binder and granulating is included before the compression molding; Preferably, the adhesive is a silicone resin; Preferably, the amount of the adhesive is 1.0-2.0wt% of the alloy powder; Preferably, the annealing temperature is 800-820°C and the time is 4-6h; Preferably, the compression molding pressure is 17-21T / cm 2 .

9. The powder core obtained by the preparation method according to any one of claims 1 to 8.

10. An inductor device, characterized in that: The invention comprises a powder core prepared by the preparation method according to any one of claims 1 to 8.

Citation Information

Cited By

  • Inductance composite material and preparation method thereof

    CN120261130A

  • Iron-nickel metal magnetic powder core with high stable magnetic conductivity and low loss and preparation method of iron-nickel metal magnetic powder core