Metal oxide thin film manufacturing method and apparatus

By employing plasma-excited humidified argon and UV irradiation, the method enhances the density and growth rate of metal oxide thin films, addressing the inefficiencies of existing deposition methods and reducing water vapor permeability in flexible electronic circuits.

JP7556540B2Active Publication Date: 2024-09-26YAMAGATA UNIVERSITY
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021002350
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-01-08
Publication Date
2024-09-26
Estimated Expiration
2041-01-08

AI Technical Summary

Technical Problem

Existing room-temperature atomic layer deposition methods for metal oxide thin films are slow and result in films with low density and high water vapor permeability due to hydrophilic properties and adsorption of water molecules, leading to poor durability of flexible electronic circuits.

Method used

A method involving the use of plasma-excited humidified argon and ultraviolet irradiation at 300-400 nm wavelength to enhance the adsorption of organometallic gas molecules, forming hydroxyl groups and desorbing water molecules, combined with alternating gas introduction and evacuation steps to increase film density and growth rate.

Benefits of technology

The method enables the formation of dense metal oxide thin films at low temperatures with reduced water vapor permeability, improving the durability of flexible electronic circuits by increasing film density and growth rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007556540000005
    Figure 0007556540000005
  • Figure 0007556540000004
    Figure 0007556540000004
  • Figure 0007556540000002
    Figure 0007556540000002
Patent Text Reader

Abstract

To provide a method and a device for producing a metal oxide thin film by increasing the amount of film deposition and improving the film compactness in RT atomic layer deposition.SOLUTION: A method for producing a metal oxide thin film includes a first step for holding an object for deposition at higher than 0°C to 150°C or lower, introducing an organometallic gas onto a deposition face of the object for deposition, and causing the deposition face to adsorb the organometallic gas molecules, and a second step for introducing the plasma-excited humidified argon onto the deposition face having adsorbed the organometallic gas molecules, oxidizing and decomposing the adsorbed organometallic gas molecules into metal oxides, and forming hydroxyl groups on the surface, the first step and the second step to be repeated, forming a metal oxide thin film. When the plasma-excited humidified argon is introduced in the second step, the object for deposition is irradiated with ultraviolet rays having a wavelength of 300-400 nm.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method and apparatus for producing a metal oxide thin film, which is capable of forming a dense metal oxide thin film on a film-forming target at a low temperature. [Background technology]

[0002] In organic electroluminescence (EL) and flexible electronics, electronic circuits are formed on more flexible films. For the flexible film, a resin, for example, a transparent resin such as polyethylene terephthalate (PET) or polyethylene naphthalate (PEN), is used. Then, for example, electronic components are attached to the flexible film and wired using a printing method to manufacture sensors or wireless tags that can be attached freely. It is also possible to form amorphous silicon or an organic semiconductor film, which are materials for solar cells, on the surface of the flexible film, and manufacture solar cells that can be flexibly attached to curved surfaces by attaching electrodes. For electronic components made of such flexible materials, it is necessary to form a thin film that prevents the penetration of oxygen, water, etc. into the electronic circuits on the surface, in order to prevent the deterioration of electrical performance due to oxidation of the semiconductors and electrical wires on the surface.

[0003] The water vapor transmission rate (WVTR) is an index that indicates the moisture permeability. For untreated PET and PEN films, the WVTR is usually 10 to 100 g m -2 day -1 However, depending on the application of electronic circuits, for example solar cells and organic electronic circuits, the WVTR is 10 -3 ~10 -4 g m -2 day -1 For organic electroluminescence applications, a WVTR of about 10 -6 g m -2 day -1 It is necessary to suppress WVTR to some extent.

[0004] To suppress the water vapor transmission rate, it is necessary to form a thin metal oxide film, such as aluminum oxide, silicon oxide, or zirconium oxide, on the resin film. These oxide thin films have a higher atomic density than resin films, and are effective in suppressing water vapor transmission. To form these oxide films, atomic layer deposition, which allows film formation at low temperatures, is used. Patent Document 1 discloses a thin film deposition method characterized by repeating a series of steps including the steps of placing a solid substrate in a reaction vessel, maintaining the temperature of the solid substrate higher than 0°C and not higher than 150°C, preferably not higher than 100°C, filling the reaction vessel with an organometallic gas such as trimethylaminosilane, bisdimethylaminosilane, methylethylaminohafnium, etc., evacuating the gas or filling the reaction vessel with an inert gas such as nitrogen gas, argon gas, helium, etc., introducing an oxidizing gas with a high activity, for example, water vapor or oxygen in the form of plasma, and evacuating the gas or filling the reaction vessel with an inert gas such as nitrogen gas, argon gas, helium, etc.

[0005] Furthermore, a room temperature atomic layer deposition method for aluminum oxide, which is effective in suppressing water vapor permeation, is reported in Non-Patent Document 1. Non-Patent Document 1 reports that this method makes it possible to form an aluminum oxide film at room temperature using trimethylaluminum as the source gas and humidified argon gas excited by plasma as the oxidizing gas. Furthermore, Non-Patent Document 2 shows an example of water vapor permeation suppression using aluminum oxide, in which 75 nm of aluminum oxide is laminated on a 100 μm PEN film, and the water vapor transmission rate (WVTR) is 2.6 × 10 -3 g m -2 day -1 has been reported.

[0006] However, the above-mentioned room temperature atomic layer deposition method has the following problems. First, the film formation process takes time, so there is a need to speed up the film formation process. 2 O 3The deposition amount of one cycle is 0.15 nm / cycle, and SiO 2 The deposition rate is 0.08 nm / cycle, one cycle takes about 1 to 2 minutes, and the amount of growth per cycle is very small, so a large number of cycles are required, and there is a need to improve the amount of film deposition. In addition, the metal oxide thin film formed is a hydrophilic material, and water molecules from the reaction product are adsorbed onto the surface, resulting in a film that is not very dense. As a result, there was an issue that the water vapor permeability was relatively high. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Patent No. 6484892 [Non-patent literature]

[0008] [Non-Patent Document 1] Journal of the Institute of Electronics, Information and Communication Engineers VOL.J98-C No.1 P.1~P.7 [Non-Patent Document 2] Applied Physics Vol. 86 No. 9, pp. 796-800, 2017 Summary of the Invention [Problem to be solved by the invention]

[0009] The present invention has been made in consideration of the above circumstances, and has an object to provide a method and apparatus for producing a metal oxide thin film, which improves the amount of metal oxide thin film formed and the density of the film in room temperature atomic layer deposition. [Means for solving the problem]

[0010] A first aspect of the present invention for achieving the above-mentioned object is a method for producing a metal oxide thin film, comprising a first step of maintaining a film-forming target at a temperature higher than 0°C and lower than 150°C, introducing an organometallic gas onto a film-forming surface of the target to adsorb organometallic gas molecules onto the film-forming surface, and a second step of introducing plasma-excited humidified argon onto the film-forming surface on which the organometallic gas molecules have been adsorbed, to oxidize and decompose the adsorbed organometallic gas molecules to form a metal oxide and form hydroxyl groups on the surface, and then repeating the first and second steps to form a metal oxide thin film, characterized in that when introducing the plasma-excited humidified argon in the second step, the target to be film-formed is irradiated with ultraviolet light having a wavelength of 300 to 400 nm, more preferably 350 to 400 nm. A second aspect of the present invention resides in the method for producing a metal oxide thin film according to the first aspect, characterized in that, prior to the first step, a preliminary step is carried out in which plasma-excited humidified argon is introduced onto the deposition surface of the deposition target to form hydroxyl groups on the deposition surface. A third aspect of the present invention resides in the method for producing a metal oxide thin film according to the first or second aspect, characterized in that a step of evacuating the introduced gas or introducing an inert gas is carried out between each step.

[0011] A fourth aspect of the present invention is an apparatus for producing a metal oxide thin film, comprising: a reaction vessel having a mechanism for holding a film-forming target; a raw material gas introduction device for introducing an organic metal gas into the reaction vessel; a plasma-excited humidified argon introduction device for introducing plasma-excited humidified argon into the reaction vessel; an ultraviolet ray irradiation device for irradiating the film-forming target held in the reaction vessel with ultraviolet rays having a wavelength of 300 to 400 nm, more preferably 350 to 400 nm; and a control device for controlling these devices, wherein the control device controls a first step of introducing an organic metal gas onto a film-forming surface of the film-forming target to adsorb organic metal gas molecules onto the film-forming surface; a second step of introducing plasma-excited humidified argon onto the film-forming surface on which the organic metal gas molecules are adsorbed, and irradiating the film-forming target with ultraviolet rays via the ultraviolet ray irradiation device, to oxidize and decompose the adsorbed organic metal gas molecules to form metal oxide and form hydroxyl groups on the surface; and thereafter, the first step and the second step are controlled to be repeated.

[0012] In room temperature atomic layer deposition, the amount of film formed per cycle is determined by the density of organometallic gas molecules that are adsorbed onto the surface of the film during the process of filling the surface with organometallic gas. In order to increase the adsorption density of these molecules, it is important to make the surface of the film-forming target clean and free of adsorption of impurity molecules such as water. In addition, it is necessary to form a high density of hydroxyl groups, which serve as molecular adsorption points, on the surface of the film-forming target.

[0013] In order to increase the growth rate of one cycle, the amount of water molecules adsorbed on the surface of the hydroxyl group must be reduced as much as possible. These water molecules form hydrogen bonds with the surface on which the hydroxyl group is formed, and are highly likely to adhere to it. When the organometallic gas, which is the raw material for the metal oxide film, adheres to the surface of the film to be formed and is oxidized by OH radicals, water molecules are generated as reaction products and are adsorbed on the surface. In addition, water is also adsorbed on the inner surface of the reaction vessel as adsorbed water, which may be desorbed and adsorbed on the surface of the film to be formed, preventing the adsorption of the organometallic gas molecules and suppressing the amount of film formation in one cycle. In addition, if water is adsorbed, water may be contained in the film when the film is subsequently grown, resulting in a decrease in the density of the film.

[0014] In order to solve this problem, in the present invention, in the step of introducing plasma-excited humidified argon in the room temperature atomic layer deposition process, the surface of the film-forming target is irradiated with ultraviolet light having a wavelength of 300 to 400 nm, more preferably light having a wavelength of 350 to 400 nm, to cause photoinduced desorption of water adsorbed on the surface of the film-forming target. The above wavelengths are desirable because shorter wavelengths may cause chemical alteration in the case of a sample substrate made of a resin or other film. In typical films such as polyethylene and polypropylene, absorption of ultraviolet light occurs with light having a wavelength of 240 nm or less, and in addition, absorption occurs with light having a wavelength of 310 nm or less in polystyrene and 350 nm or less in polyethylene terephthalate. At that time, the absorption of ultraviolet light may cause oxidation or cleavage of molecules, which may lead to deterioration of the material. Specifically, it is known that trace amounts of catalytic metals, hydroperoxides, carbonyl groups, etc. introduced when the above resin is molded into a molded product undergo photochemical reactions, promoting the deterioration of the polymer of the resin. On the other hand, if the wavelength is longer than this, the photon energy of the light becomes smaller, and it is thought that the effect of photostimulated desorption weakens. When irradiating ultraviolet light of the above wavelength, it is desirable to use a light-emitting diode (LED) whose main component is GaN. GaN LEDs emit ultraviolet light with a wavelength of 380 nm. Conventionally, low-pressure mercury lamps and deuterium lamps have been used to irradiate ultraviolet light, but in this case, the above-mentioned short-wavelength ultraviolet light may cause deterioration of the resin film. However, with GaN LEDs, the wavelength is limited to 380 nm, making it possible to suppress the above-mentioned side effects. In addition, with conventional ultraviolet lamps, the light beam direction is isotropic, and when the lamp is stored in a reaction vessel and room temperature atomic layer deposition is performed, ultraviolet light hits the wall of the reaction vessel that is not the target of film formation, and there are problems such as the promotion of dirt on the wall due to accelerated film formation there. With LEDs, it is easy to make light into a beam, making it possible to prevent irradiation of unintended areas. Furthermore, GaN LEDs have the advantage of reducing costs compared to conventional ultraviolet lamps.

[0015] The irradiation of ultraviolet light is limited to the step of introducing plasma-excited humidified argon gas for the following reasons: The effect of photoinduced stimulated desorption can be obtained even if the step is not limited to this step, but if ultraviolet light is irradiated when the organometallic gas, which is the source gas, is introduced, a decomposition reaction of the organometallic gas molecules occurs in the gas phase, and a direct reaction occurs between the water molecules generated by photoinduced stimulated desorption and the organometallic gas, which may lead to the generation of particles, reduce the density of the film, and increase the water vapor transmission rate. Effect of the Invention

[0016] According to the present invention, it is possible to form a dense metal oxide thin film at a low temperature, for example, room temperature, and at a high film formation rate, and it is possible to reduce the water vapor permeability of the formed metal oxide thin film. That is, according to the present invention, the growth amount of a metal oxide thin film, particularly aluminum oxide, per cycle is increased in room temperature atomic layer deposition, the atomic density of the formed metal oxide thin film is increased, and the water vapor transmission rate of the metal oxide thin film can be suppressed, which makes it possible to suppress the deterioration of flexible electronic circuits due to water vapor transmission, and is effective in improving the durability of the electronic circuits. [Brief description of the drawings]

[0017] [Figure 1] 1 is a schematic explanatory diagram of a metal oxide thin film manufacturing apparatus according to an embodiment of the present invention. [Diagram 2] 1 is an explanatory diagram showing a schematic configuration of an ultraviolet irradiation device according to an embodiment of the present invention; [Diagram 3] FIG. 2 is an explanatory diagram illustrating the denseness of a metal oxide thin film formed by the apparatus according to the present invention. [Figure 4] 1 is a graph showing the results of measuring the gas barrier properties of the water vapor permeable barrier films according to Example 3 and Comparative Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] FIG. 1 is a schematic explanatory diagram of a metal oxide thin film manufacturing apparatus according to one embodiment. As shown in FIG. 1, the metal oxide thin film manufacturing apparatus 1 includes a reaction vessel 10, a raw material gas introduction device 20, a plasma excited humidified argon introduction device 30, an exhaust device 40, an ultraviolet ray irradiation device 50, and a control device 60. The source gas introduction device 20 includes a source gas tank 21 , an introduction pipe 22 connecting the source gas tank 21 with the reaction vessel 10 , and a variable valve 23 that is a flow rate controller provided midway along the introduction pipe 22 . The plasma-excited humidified argon introduction device 30 comprises an argon tank 31, a water bubbler 32 which humidifies the argon from the argon tank 31, a flow controller 33, and a plasma gas generator 34 which introduces the humidified argon gas from the water bubbler 32 via the flow controller 33 and introduces it into the reaction vessel 10 as plasma-excited humidified argon gas, and these are connected to the reaction vessel 10 via piping 35.

[0019] Here, the water bubbler 32 is for humidifying the argon gas by filling the water 32b in the tank 32a and introducing argon gas into the water 32b and passing the water through it. The plasma gas generator 34 includes a glass tube 34a, an induction coil 34b provided around the glass tube 34a, and a matching circuit 34c connected to the induction coil 34b, and generates plasma in the inner region of the glass tube 34a by applying a high-frequency current of, for example, 13.56 MHz to the induction coil 34b via the matching circuit 34c. The exhaust device 40 is for exhausting the inside of the reaction vessel 10, and is, for example, an exhaust pump. The ultraviolet irradiation device 50 includes an ultraviolet LED 51 that irradiates ultraviolet light of 350 to 400 nm. Specifically, the ultraviolet LED 51 is preferably an ultraviolet LED made of GaN that irradiates ultraviolet light of a wavelength of 365 nm. As will be described in detail later, the ultraviolet LED 51 includes a plurality of LEDs that are arranged at equal intervals in a plane parallel to the substrate S in an area facing the substrate S. By irradiating ultraviolet light with such an ultraviolet irradiation device 50, uniform irradiation over a large area is possible.

[0020] To deposit a metal oxide film using such a manufacturing apparatus 1, a substrate S such as a film on which a film is to be formed is inserted into a reaction vessel 10, the inside of the reaction vessel 10 is evacuated to a vacuum via an exhaust device 40, and a process of introducing an organometallic gas as a raw material gas from a raw material gas introduction device 20 and a process of introducing plasma-excited humidified argon gas from a plasma-excited humidified argon introduction device 30 are alternately repeated. Here, the substrate S on which the film is to be formed in the reaction vessel 10 may be kept at room temperature without being heated, but the temperature must be 0° C. or higher. The upper limit depends on the heat resistance of the substrate S, but may be 150° C. or lower, preferably 100° C. or lower, and more preferably 70° C. or lower.

[0021] As the source gas, an organometallic gas that serves as a precursor of the metal oxide thin film to be formed is used. The organometallic gas that can be used in the present invention can be a compound in which carbon is directly bonded to a metal, a compound in which carbon is bonded via oxygen, a compound in which carbon is bonded via nitrogen, or any other various organometallic compounds that can be gasified, and all compounds that can be used in conventional atomic layer deposition methods can be applied. Examples of the organometallic gas include organosilicon compounds such as trimethylaminosilane and bisdimethylaminosilane; organohafnium compounds such as methylethylaminohafnium; organozirconium compounds such as trimethylamidozirconium, organoaluminum compounds such as trimethylaluminum; organotitanium compounds such as titanium isopropoxide and titanium dimethylethylaminotitanium; organogallium compounds such as trimethylgallium; organostrontium; organozinc compounds; organocuprate compounds; organosmium compounds; organoplatinum compounds; organotantalum compounds; organoniobium compounds; organotin compounds; organolanthanum compounds; organoyttrium compounds; organocerium compounds; organovanadium compounds; organoindium compounds; organomolybdenum compounds. Aluminum oxide (Al 2 O 3 For example, trimethylaluminum is used to form silicon oxide (SiO 2), for example, tridimethylaminosilane is preferably used.

[0022] The specific steps are as follows: (1) a first step of introducing a raw material gas into the reaction vessel 10 by the raw material gas introduction device 20; (2) a second step of introducing plasma-excited humidified argon gas into the reaction vessel 10 by the plasma-excited humidified argon introduction device 30 and irradiating ultraviolet rays onto the substrate S in the reaction vessel 10 by the ultraviolet irradiation device 50; By carrying out the above steps and repeating steps (1) and (2), a metal oxide thin film can be formed on the substrate S. Between each step, it is desirable to carry out a step of evacuating the introduced gas or introducing an inert gas.

[0023] In this method, when the source gas is introduced, the source gas is adsorbed to the hydroxyl groups on the surface of the substrate S, and then when plasma-excited humidified argon is introduced, the source gas molecules adsorbed on the surface of the substrate S are oxidized, a very thin metal oxide thin film is formed, and hydroxyl groups are generated on the surface. At this time, by irradiating ultraviolet light of 300 to 400 nm at the same time as introducing the plasma-excited humidified argon, water generated when the source gas is oxidized and adsorbed on the surface of the metal oxide thin film can be photoinduced stimulated desorption. To effectively induce such photoinduced desorption, it is preferable to irradiate with ultraviolet light having a wavelength in the range of 300 to 400 nm. If the wavelength is shorter than this, there is a possibility that chemical alteration will occur if the substrate S is a film such as a resin. Furthermore, if the wavelength is longer than this, the photon energy of the light will be smaller, and the effect of photoinduced desorption will be weakened.

[0024] 1 is automatically operated by a control device 60. That is, the control device 60 comprehensively controls the variable valve 23 of the raw material gas introduction device 20, the flow rate controller 33 and matching circuit 34c of the plasma excited humidified argon introduction device 30, the exhaust device 40, and the control unit 52 of the ultraviolet ray irradiation device 50, and controls so that each of the above-mentioned steps is repeated a predetermined number of times.

[0025] Here, since there is a possibility that hydroxyl groups are not sufficiently present on the surface of the substrate S before the film is formed, it is preferable to carry out a preliminary step of introducing plasma-excited humidified argon onto the film formation surface of the substrate S, which is the target of film formation, before the initial first step (step (1) above), to form hydroxyl groups on the film formation surface of the substrate S. At this time, since there is no oxidation reaction of the raw material gas, it is not necessary to irradiate ultraviolet rays from the ultraviolet irradiation device 50, but there is no disadvantage if ultraviolet rays are irradiated. EXAMPLES

[0026] Example 1 The manufacturing apparatus 1 in FIG. 1 was used. In this example, a Si (100) substrate was used as the substrate S, and room temperature atomic layer deposition of aluminum oxide was attempted on the substrate S. Here, a 20 L reaction vessel 10 was placed with a 10×20 mm 2 The experiment was conducted by arranging four substrates S of the same size. In the room temperature atomic layer deposition, trimethylaluminum, an organometallic gas, was introduced into the reaction vessel 10 at an average pressure of 0.3 Pa for 50 seconds at 6 sccm, then evacuated for 60 seconds, and plasma-excited humidified argon was introduced at 10 sccm for another 120 seconds, and ultraviolet irradiation was performed at the same time. Then, evacuation was performed for 60 seconds. The substrate temperature at this time was 25°C. This series of steps was repeated 100 cycles. The plasma-excited humidified argon was generated by discharging with an energy of 200 W at 13.56 MHz using an induction coil. The humidified argon was generated by passing dry argon through water at 60°C using a water bubbler 32.

[0027] As shown in Fig. 2, the ultraviolet LEDs 51 of the ultraviolet irradiation device 50 for UV irradiation are configured by arranging four LEDs 51a with a wavelength of 380 nm and an output of 300 mW at intervals of 70 mm on a glass plate 51b of 100 x 100 mm, and each LED 51a is controlled by a control unit 52. N3535 manufactured by Intelligent LED Solutions is used as the LED 51a. The four substrates S are arranged at a distance of 55 mm from the glass plate 51b in parallel and facing each other. The current when the LEDs 51a are lit is 220 mA, and at this time, the irradiation energy intensity of the UV light on the substrate S as a sample is 1.56 to 1.58 mW / cm. 2 It was.

[0028] When four substrates S as samples were placed in the reaction vessel 10 and the reaction vessel 10 was evacuated, the pressure inside the reaction vessel 10 reached 2×10 -3 The vacuum level was 8×10 Pa, but when the UV light was irradiated onto the substrate S by the UV LED 51, the vacuum level dropped to 8×10 Pa in 180 seconds. -3 The pressure increased to 1 Pa, and this increase in pressure was due to an increase in water pressure. This is thought to indicate that water molecules that had naturally adsorbed on the substrate S were desorbed by photoinduced desorption due to UV irradiation. After 100 cycles of room temperature atomic layer deposition (ALD) processing, aluminum oxide films were formed on the four substrates S, with an average thickness of 25.95 nm, and the growth thickness of the aluminum oxide film per cycle was 0.26 nm / cycle.

[0029] Comparative Example 1 As a comparative example, a room temperature ALD process was performed in the same manner as in Example 1 except that UV irradiation by the ultraviolet LED 51 was not performed, and an aluminum oxide film having an average thickness of 16.46 nm was formed. The growth thickness of the aluminum oxide film per cycle was 0.16 nm / cycle.

[0030] (Test result 1) Comparing the deposition amounts of Example 1 and Comparative Example 1, it was found that adding UV irradiation by the ultraviolet LED 51 to the room temperature ALD process increased the deposition amount per cycle by 1.63 times. In other words, it was found that the deposition amount of Example 1 was 1.63 times that of Comparative Example 1. In addition, when the refractive index of the aluminum oxide films formed in Example 1 and Comparative Example 1 was measured, it was 1.53 for light with a wavelength of 633 nm in Example 1, while it was 1.48 for light with a wavelength of 633 nm in Comparative Example 1. Therefore, for aluminum oxide, it was found that by adding UV irradiation from an ultraviolet LED51 to room temperature ALD processing, i.e., when UV irradiation is present, the refractive index of the film increases from 1.48 to 1.53 for light with a wavelength of 633 nm. This indicates that the dielectric constant of the film has increased, and since the dielectric constant of a film is correlated with the molecular density, it is believed that the density of the film has increased due to UV irradiation.

[0031] Example 2 In this example, room temperature atomic layer deposition of titanium oxide was carried out on a substrate S, which is a Si (100) substrate. 2 Four substrates S having the same size were placed and film formation was performed. In the room temperature atomic layer deposition, tetrakisdimethylaminotitanium, an organometallic gas, was introduced into the reaction vessel 10 at a pressure of 0.7 Pa for 200 seconds, then the vessel was evacuated for 180 seconds, and plasma-excited humidified argon was introduced at 10 sccm for another 120 seconds, while UV irradiation was performed at the same time. The vessel was then evacuated for 60 seconds. The substrate temperature at this time was 25°C. This series of steps was repeated 100 cycles. The plasma-excited humidified argon was generated by discharging with an energy of 200 W at 13.56 MHz using the induction coil 34b. The humidified argon was generated by passing dry argon through water at 60°C using the water bubbler 32. The ultraviolet irradiating device and the irradiation method for UV irradiation are the same as those in the first embodiment. After 100 cycles of room temperature ALD processing, titanium oxide films were formed on the four substrates S, the average film thickness was 12.79 nm, and the titanium oxide film growth thickness per cycle was 0.13 nm / cycle.

[0032] Comparative Example 2 As a comparative example, the same procedure as in Example 2 was performed except that UV irradiation was not performed. 60 cycles of room temperature ALD were performed. The average film thickness was 5.51 nm, and the growth thickness of the titanium oxide film per cycle was 0.09 nm / cycle.

[0033] (Test result 2) Comparing the deposition amounts of Example 2 and Comparative Example 2, it was found that adding UV irradiation to the room temperature ALD process increased the deposition amount per cycle by 1.44 times. In other words, it was found that the deposition amount of Example 2 was 1.44 times that of Comparative Example 2. In addition, when the refractive index of the titanium oxide films formed in Example 2 and Comparative Example 2 was measured, it was 1.95 for light with a wavelength of 633 nm in Example 2, while it was 1.78 for light with a wavelength of 633 nm in Comparative Example 2. Therefore, it was found that for titanium dioxide, the refractive index of the film increased from 1.78 to 1.95 when exposed to UV light at a wavelength of 633 nm. This indicates that the dielectric constant of the film increased, and because the dielectric constant of a film correlates with molecular density, it is believed that the film's density increased due to UV light.

[0034] Example 3 Under the same manufacturing conditions as in Example 1, a water vapor permeation barrier film was formed by laminating two layers of aluminum oxide films and two layers of zinc oxide films alternately on both surfaces of a 100 μm-thick PEN film. The structure is shown in FIG. 3. That is, aluminum oxide (Al 2 O 3 A water vapor permeation barrier film was formed by alternately laminating two layers of a fluorine-containing polysilicon (FGP) film S11 and two layers of a zinc oxide (ZnO) film S12. In this example, the number of film formation cycles for the aluminum oxide film S11 was 150 cycles per layer, and the number of film formation cycles for the zinc oxide film S12 was 200 cycles per layer. The temperature of the substrate S on which the film was formed was 25° C. The zinc oxide film S12 was formed by room temperature atomic layer deposition under the conditions shown in Table 1 below. The raw material gas was dimethyl zinc (DMZ). In this film formation, UV light with a wavelength of 360 nm was irradiated only in the process of oxidizing the plasma-excited humidified argon (second process). The surface energy during irradiation, i.e., the irradiation energy intensity of the UV light on the substrate S, was 1.56 to 1.58 mW / cm. 2 It was.

[0035] [Table 1]

[0036] Comparative Example 3 The same procedure as in Example 3 was carried out, except that UV irradiation was not performed.

[0037] (Test result 3) The gas barrier properties of the water vapor permeable barrier films formed on the substrates S were measured for each of Example 3 and Comparative Example 3. The results are shown in FIG. The gas barrier property is measured by the water vapor transmission rate (WVTR). In Example 3 in which UV light was irradiated, the WVTR was 6.6×10 -3 g / m 2 / day to 3.0 x 10 -3 g / m 2 / day. This is presumably due to the fact that the thickness of the aluminum oxide film S11 is increased by UV light irradiation, and furthermore, the density of the aluminum oxide film S11 and the zinc oxide film S12 is improved. [Industrial Applicability]

[0038] It is used in the manufacturing process of flexible electronic circuits that use organic electronics, etc., and is utilized as a coating technology to prevent deterioration due to moisture penetration of electronic circuits formed on flexible substrates. [Explanation of symbols]

[0039] 1...Manufacturing equipment 10...Reaction vessel 20...Source gas introduction device 30...Plasma excited humidified argon introduction device 40…Exhaust system 50...UV irradiation device 60...Control device

Claims

1. A method for manufacturing a metal oxide thin film, comprising: a first step of maintaining a film-forming target at a temperature higher than 0° C. and lower than 150° C., introducing an organometallic gas onto a film-forming surface of the film-forming target to adsorb organometallic gas molecules onto the film-forming surface; a second step of introducing plasma-excited humidified argon onto the film-forming surface on which the organometallic gas molecules have been adsorbed, to oxidize and decompose the adsorbed organometallic gas molecules to form metal oxide and to form hydroxyl groups on the surface; and then repeating the first step and the second step to form a metal oxide thin film, When the plasma-excited humidified argon is introduced in the second step, the target to be film-formed is irradiated with ultraviolet light having a wavelength of 300 to 400 nm.

2. A method for producing a metal oxide thin film comprising the steps of:

2. Prior to the first step, a preliminary step is carried out in which plasma-excited humidified argon is introduced onto the film-forming surface of the film-forming target to form hydroxyl groups on the film-forming surface.

2. The method for producing a metal oxide thin film according to claim 1.

3. Between each step, a step of exhausting the introduced gas or introducing an inert gas is carried out.

3. The method for producing a metal oxide thin film according to claim 1 or 2.

4. A reaction vessel having a mechanism for holding a film-forming target; a source gas introduction device for introducing an organometallic gas into the reaction vessel; a plasma excited humidified argon introduction device for introducing plasma excited humidified argon into the reaction vessel; an ultraviolet irradiation device that irradiates the film-forming target held in the reaction vessel with ultraviolet light having a wavelength of 300 to 400 nm; A control device for controlling these devices, The control device controls a first process of introducing an organic metal gas onto the film-forming surface of the film-forming target to adsorb organic metal gas molecules onto the film-forming surface, a second process of introducing plasma-excited humidified argon onto the film-forming surface on which the organic metal gas molecules are adsorbed and irradiating the film-forming target with ultraviolet light via the ultraviolet irradiation device to oxidize and decompose the adsorbed organic metal gas molecules to form metal oxides and form hydroxyl groups on the surface, and then repeats the first process and the second process.

2. A metal oxide thin film manufacturing apparatus comprising:

Citation Information

Patent Citations

  • Water storage tank equipped with waterproof sheet

    JP1989084892A

  • Method and apparatus for thin film formation by atomic layer growth

    JP2001220287A

  • Sealing film for organic electronic device and its manufacturing method

    JP2003347042A

  • Atomic layer growth method for depositing layer

    JP2007027723A

  • Thin film formation method and apparatus

    JP2013175720A