Positive electrode active material and method for producing same
By controlling the aspect ratio of crystal grains and void distribution in lithium transition metal oxides, the battery's initial capacity and stability are enhanced, addressing the limitations of existing materials.
Patent Information
- Application Number
- JP2023544137
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-02-05
- Filing Date
- 2022-02-03
- Publication Date
- 2024-09-26
- Estimated Expiration
- 2042-02-03
AI Technical Summary
Existing lithium transition metal oxides used in positive electrodes of lithium secondary batteries face challenges in controlling the size and position of voids in secondary particles, affecting the performance and stability of the active material, leading to issues such as poor thermal stability and potential battery explosions.
A lithium transition metal oxide with a specific composition and structure is developed, where the aspect ratio of crystal grains and the distribution of voids in secondary particles are controlled to enhance the initial capacity and stability of the battery.
The solution results in a positive electrode active material with improved initial discharge capacity and charge/discharge efficiency, ensuring uniform void distribution and increased contact area with the electrolyte, thereby enhancing the battery's performance and safety.
Smart Images

Figure 0007556616000012 
Figure 0007556616000009 
Figure 0007556616000008
Abstract
Description
[Technical field]
[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0017094 filed on February 5, 2021, the entire contents of which are incorporated herein by reference.
[0002] The present invention relates to a positive electrode active material and a manufacturing method thereof, and more specifically, to a positive electrode active material manufactured from a positive electrode active material precursor having a controlled aspect ratio of crystal grains, in which voids contained in secondary particles satisfy specific conditions, a manufacturing method thereof, and a positive electrode and a lithium secondary battery each including the positive electrode active material. [Background technology]
[0003] With the technological development and increasing demand for mobile devices, the demand for secondary batteries as an energy source is rapidly increasing. Among these secondary batteries, lithium secondary batteries, which have high energy density and voltage, long cycle life, and low self-discharge rate, have been commercialized and are widely used.
[0004] Lithium transition metal oxides are used as the positive electrode active material for lithium secondary batteries, and among them, lithium cobalt oxide LiCoO2, which has high working voltage and excellent capacity characteristics, is mainly used. However, LiCoO2 has very poor thermal properties due to the instability of its crystal structure caused by delithiation, and is expensive, so there are limitations to its mass use as a power source in fields such as electric vehicles.
[0005] As a material to be used in place of LiCoO2, lithium manganese composite metal oxides (LiMnO2 or LiMn2O4, etc.), lithium iron phosphate compounds (LiFePO4, etc.), lithium nickel composite metal oxides (LiNiO2, etc.), etc. have been developed. Among them, research and development of lithium nickel composite metal oxides, which have a high reversible capacity of about 200 mAh / g and therefore can easily be used to realize large-capacity batteries, has been actively carried out. However, LiNiO2 has inferior thermal stability compared to LiCoO2, and if an internal short circuit occurs due to external pressure in a charged state, the positive electrode active material itself decomposes, causing the battery to explode and catch fire. Therefore, as a method for maintaining the excellent reversible capacity of LiNiO2 and improving its low thermal stability, LiNiO2, which has a part of the nickel substituted with cobalt, has been developed. 1-α Co α Lithium nickel cobalt metal oxides in which O2 (α = 0.1-0.3) or nickel is partially replaced by Mn, Co or Al have been developed. a Co b Mn c ]O2, Li[Ni a Co b Al c ]O2, Li[Ni a Co b Mn c Al d Lithium composite transition metal oxides containing two or more transition metals, such as ]O2, have been developed and are widely used.
[0006] The lithium transition metal composite oxide containing two or more kinds of transition metals is usually manufactured in the form of spherical secondary particles formed by agglomeration of tens to hundreds of primary particles, and the secondary particles contain voids, but the physical properties of the positive electrode active material, such as reactivity due to changes in the contact area with the electrolyte and particle strength, change depending on the size, distribution, etc. of the voids in the secondary particles. Therefore, research is being attempted to analyze the voids contained in the secondary particles by BET analysis, mercury intrusion porosimetry, etc., and use the results to improve the performance of the positive electrode active material.
[0007] However, in the case of void analysis using BET analysis, mercury intrusion porosimetry, etc., it is possible to measure the size of the voids contained in the secondary particles, but it is not possible to know how the voids are located within the secondary particles, which makes it difficult to control the performance of the positive electrode active material.
[0008] Therefore, in order to develop a positive electrode active material with better properties, it is necessary to develop a positive electrode active material in which not only the size of the voids contained in the secondary particles but also the position of the voids is controlled. Summary of the Invention [Problem to be solved by the invention]
[0009] An object of the present invention is to provide a positive electrode active material in which voids contained in secondary particles satisfy specific conditions and the initial capacity characteristics of a battery can be improved.
[0010] Another object of the present invention is to provide a method for producing a positive electrode active material by using a positive electrode active material precursor having a crystal grain aspect ratio that satisfies a specific condition. [Means for solving the problem]
[0011] The present invention includes a lithium transition metal oxide that contains 60 mol % or more of nickel relative to the total number of moles of transition metals other than lithium, and is in the form of secondary particles formed by aggregation of primary particles, The lithium transition metal oxide provides a positive electrode active material that satisfies the following formula 1. [Formula 1]
number
[0012] The present invention also provides a method for producing a positive electrode active material precursor comprising: (A) preparing a positive electrode active material precursor that contains 60 mol % or more of nickel relative to the total number of moles of transition metals, contains a transition metal hydroxide in the form of secondary particles formed by aggregation of primary particles, and has an aspect ratio of crystal grains of 4.0 to 10.0; (B) mixing the positive electrode active material precursor with a lithium-containing raw material, followed by calcining the mixture, to produce a lithium transition metal oxide.
[0013] The present invention also provides a positive electrode for a lithium secondary battery comprising the positive electrode active material, and a lithium secondary battery comprising the positive electrode. Effect of the Invention
[0014] The present invention provides a positive electrode active material having excellent initial capacity characteristics, specifically, excellent initial discharge capacity and initial charge / discharge efficiency, because the voids contained in the secondary particles satisfy specific conditions.
[0015] The present invention can use a positive electrode active material precursor in which the aspect ratio of the crystal grains satisfies specific conditions to produce a positive electrode active material in which the voids contained in the secondary particles satisfy specific conditions. [Brief description of the drawings]
[0016] [Figure 1] FIG. 2 is a diagram showing a cross-sectional SEM image of one secondary particle of the positive electrode active material prepared in Example 1 of the present invention, and a size and position distribution of voids. [Diagram 2] FIG. 2 is a diagram showing a cross-sectional SEM image of one secondary particle of the positive electrode active material prepared in Example 2 of the present invention, and a size and position distribution of voids. [Diagram 3] FIG. 2 is a diagram showing a cross-sectional SEM image of one secondary particle of the positive electrode active material prepared in Comparative Example 1 of the present invention, and a size and position distribution of voids. [Figure 4]FIG. 2 is a diagram showing a cross-sectional SEM image of one secondary particle of the positive electrode active material prepared in Comparative Example 2 of the present invention, and a size and position distribution of voids. [Diagram 5] FIG. 13 is a diagram showing a cross-sectional SEM image of one secondary particle of the positive electrode active material prepared in Comparative Example 3 of the present invention, and a size and position distribution of voids. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] The terms and words used in this specification and the claims should not be interpreted in a limited manner to their ordinary or dictionary meanings, but should be interpreted in a manner that is consistent with the technical idea of the present invention, based on the principle that the inventors can appropriately define the concepts of terms in order to best describe their invention.
[0018] In this specification, the terms "including," "comprising," or "having" are intended to indicate the presence of implemented features, numerals, steps, components, or combinations thereof, and should be understood as not precluding the presence or additional possibility of one or more other features, numerals, steps, components, or combinations thereof.
[0019] In the present invention, the term "crystal grain" refers to a unit of a single crystal particle having a regular atomic arrangement.
[0020] The crystal grain size is a value measured by analyzing XRD data obtained by X-ray diffraction analysis of a positive electrode active material precursor powder using a Rietveld refinement method, and the crystal grain aspect ratio is the ratio (a / c) of the major axis length (a) to the minor axis length (c) of the crystal grain calculated by applying the full width at half-maximum (FWHM) of all peaks shown in the XRD data to a modified Scherrer equation using ellipsoid modeling.
[0021] The size and aspect ratio of the crystal grains can be specifically determined by the following method.
[0022] First, perform X-ray diffraction analysis on the cathode active material precursor to obtain XRD data. At this time, the X-ray diffraction analysis can be performed under the following conditions using an Empyreon XRD apparatus manufactured by Malyer panalytical.
[0023] <X-ray diffraction analysis conditions> Light source: Cu-target, 45 kV, 40 mA output Detector: GaliPIX3D Sample preparation: Fill a sample of about 5 g into a holder with a diameter of 2 cm and load it onto a rotation stage. Measurement time: About 30 minutes Measurement range: 2θ = 15° to 85°
[0024] The crystal grain size can be determined using Highscore, which is an XRD data refinement program manufactured by Malvern. Specifically, it can be determined by fitting the half-widths of all the peaks shown in the XRD data using the Caglioti equation.
[0025] The aspect ratio of the crystal grains can be determined from the length c of the minor axis and the length a of the major axis obtained by the least squares approximation method after applying the half-widths of all the peaks shown in the XRD data obtained by performing X-ray diffraction analysis on the cathode active material precursor to the following formula (2).
[0026] [Formula 2]
Number
[0027] In the above formula (2), d(hkl) is the half-width at the peak, and h, k, and l are the Miller indices of the crystal plane at the peak. Kis the Scherrer constant, θ is the Bragg angle, λ is the X-ray wavelength, a is the length of the major axis of the crystal grain, and c is the length of the minor axis of the crystal grain.
[0028] In the present invention, the term "primary particle" refers to the smallest particle unit that can be distinguished as a single mass when a cross section of a positive electrode active material precursor is observed with a scanning electron microscope (SEM), and may consist of one crystal grain or multiple crystal grains.
[0029] The present invention will now be described in more detail.
[0030] The present inventors have found that when the voids contained in the secondary particles satisfy certain conditions, the initial capacity characteristics of a battery containing the positive electrode active material according to the present invention can be improved, and have completed the present invention.
[0031] positive electrode active material The positive electrode active material according to the present invention contains 60 mol % or more of nickel relative to the total number of moles of transition metals other than lithium, and contains a lithium transition metal oxide in the form of secondary particles formed by aggregation of primary particles, The lithium transition metal oxide satisfies the following formula 1.
[0032] [Formula 1]
number
[0033] In the above formula 1, The values of x and y are obtained from a cross-sectional SEM image analysis of the secondary particle, and the value of x is the area of the closed voids distributed inside the secondary particle that is less than 0.002 μm 2 The minimum area of a rectangle that contains all voids exceeding 2 ) and the y is the area of the closed voids distributed inside the secondary particle that is 0.002 μm 2 The area of the void (unit: μm 2In this case, the x and y can be obtained by processing the positive electrode active material by ion milling, obtaining a SEM image of a cross section of secondary particles including voids using a SEM (Quanta FEG 250, manufactured by FEI), and analyzing the image using a commercial program, Image J, at an image threshold of 1 to 2%.
[0034] When the condition of the formula 1 is satisfied, the initial capacity characteristic of the battery including the positive electrode active material is excellent. Specifically, the initial discharge capacity and the initial charge / discharge efficiency of the battery including the positive electrode active material are excellent. This is because when the condition of the formula 1 is satisfied and the voids distributed inside the secondary particles are uniformly distributed inside the secondary particles, the contact area between the positive electrode active material and the electrolyte is expanded, and lithium insertion and desorption occurs actively.
[0035] Meanwhile, when a positive electrode active material is produced using a positive electrode active material precursor in which the aspect ratio of the crystal grains satisfies a specific condition, the lithium transition metal oxide can satisfy the condition of formula 1 above.
[0036] The lithium transition metal oxide has a shape of secondary particles formed by agglomeration of primary particles. When the lithium transition metal oxide is formed into a shape of secondary particles formed by agglomeration of primary particles, it has a high specific surface area and can realize a high rolling density, and when applied, it can increase the energy density per volume.
[0037] According to the present invention, in the formula 1, 20≦x≦400, specifically 40≦x≦225, and more specifically 100≦x≦225. When x is within the above range, there is an advantage that the voids in the secondary particles are uniformly distributed.
[0038] According to the present invention, in the formula 1, 0.01≦y≦5.0, specifically 0.05≦y≦3.0, and more specifically 0.1≦y≦1.5 can be satisfied. When y is within the above range, there is an advantage that the particle has an appropriate void, has electrochemical activity, and ensures particle strength.
[0039] According to the present invention, the area of the closed voids distributed inside the secondary particles is 0.002 μm 2 The average void area of voids exceeding 0.01 μm 2 / piece~0.1μm 2 The average void area can be specifically 0.015 μm 2 / piece~0.08μm 2 / piece, more specifically 0.018μm 2 / piece~0.05μm 2 When the average void area is within the above range, it is advantageous in that a suitable contact area between the positive electrode active material and the electrolyte can be secured. In this case, the average void area means a value obtained by dividing the total area of the voids by the number of voids.
[0040] According to the present invention, the lithium transition metal oxide may have a composition represented by the following Chemical Formula 1.
[0041] [Chemical formula 1] Li a Ni x1 Co y1 M1 z1 M2 w1 O2
[0042] In Chemical Formula 1, M1 is one or more selected from Mn and Al, M2 is one or more selected from B, Zr, Y, Mo, Cr, V, W, Ta, and Nb, 0.9≦a≦1.2, 0.6≦x1≦1.0, 0≦y1≦0.4, 0≦z1≦0.4, 0≦w1≦0.2, and x1+y1+z1+w1=1.
[0043] Specifically, M1 can be Mn or a combination of Mn and Al.
[0044] The a represents the ratio of the number of moles of Li to the total number of moles of transition metals, and can be 0.9≦a≦1.2, specifically 1.0≦a≦1.2, and more specifically 1.0≦a≦1.1.
[0045] The above-mentioned x1 represents the ratio of the number of moles of Ni to the total number of moles of transition metals, and 0.6 ≦ x1 < 1, specifically 0.8 ≦ x1 < 1, and more specifically 0.85 ≦ x1 < 1.
[0046] The above-mentioned y1 represents the ratio of the number of moles of Co to the total number of moles of transition metals, and 0 ≦ y1 ≦ 0.4, specifically 0 < y1 < 0.2, and more specifically 0 < y1 < 0.15.
[0047] The above-mentioned z1 represents the ratio of the number of moles of M1 to the total number of moles of transition metals, and 0 ≦ z1 ≦ 0.4, specifically 0 < z1 < 0.2, and more specifically 0 < z1 < 0.15.
[0048] The above-mentioned w1 represents the ratio of the number of moles of M2 to the total number of moles of transition metals, and 0 ≦ w1 ≦ 0.2, specifically 0 ≦ w1 ≦ 0.05.
[0049] When the lithium transition metal oxide has the composition represented by the above chemical formula 1, it can exhibit high capacity characteristics.
[0050] On the other hand, the positive electrode active material according to the present invention can further include a coating layer on the surface of the above-mentioned lithium transition metal oxide. When a coating layer is further included on the surface of the lithium transition metal oxide, the coating layer can block the contact between the lithium transition metal oxide and the electrolyte, and reduce the elution of transition metals and the generation of gas due to side reactions with the electrolyte.
[0051] The coating layer can include one or more coating elements selected from the group consisting of Li, B, W, Al, Zr, Na, S, P, and Co.
[0052] Manufacturing method of positive electrode active material The method for producing a positive electrode active material according to the present invention includes the steps of: (A) preparing a positive electrode active material precursor, which contains a transition metal hydroxide that contains 60 mol % or more of nickel relative to the total moles of transition metals, has a shape of secondary particles formed by aggregation of primary particles, and has an aspect ratio of crystal grains of 4.0 to 10.0; (B) mixing the positive electrode active material precursor with a lithium-containing raw material and baking the mixture to produce a lithium transition metal oxide.
[0053] When a cathode active material precursor having a crystal grain aspect ratio that satisfies a specific condition is used as in the method for producing a cathode active material according to the present invention, a cathode active material can be produced in which the voids contained in the secondary particles satisfy a specific condition. Specifically, when the aspect ratio of the crystal grains of the cathode active material precursor is 4.0 to 10.0, specifically 4.0 to 9.0, and more specifically 4.0 to 8.0, the voids contained in the secondary particles of the produced cathode active material can satisfy the above formula 1. This is because, when the cathode active material precursor having a large crystal grain aspect ratio and the lithium-containing raw material are fired together, the primary particles present inside and on the surface of the secondary particles of the cathode active material precursor are uniformly crystallized and crystal-grown.
[0054] If the aspect ratio of the crystal grains of the positive electrode active material precursor is less than 4.0, there is a problem that the voids in the secondary particles of the positive electrode active material are not uniformly distributed, and if it exceeds 10.0, there is a problem that the positive electrode active material contains excessive voids.
[0055] Meanwhile, the aspect ratio of the crystal grains of the positive electrode active material precursor can be controlled according to the molar ratio of ammonia / transition metal input, the temperature during the co-precipitation reaction, the molar ratio of nickel to the total number of moles of the transition metal contained in the transition metal-containing solution, the pH condition during the co-precipitation reaction, and the like during the preparation of the positive electrode active material precursor.
[0056] The transition metal hydroxide has a shape of secondary particles formed by aggregation of primary particles. When the transition metal hydroxide is formed into the shape of secondary particles in which primary particles are aggregated, the produced transition metal oxide can have a high specific surface area and can achieve a high rolling density.
[0057] According to the present invention, the transition metal hydroxide can have a composition represented by the following Chemical Formula 2.
[0058] [Chemical Formula 2] Ni x2 Co y2 M1’ z2 M2’ w2 (OH)2
[0059] In Chemical Formula 2, M1' is one or more selected from Mn and Al, M2' is one or more selected from B, Zr, Y, Mo, Cr, V, W, Ta, and Nb, 0.6 ≦ x2 ≦ 1.0, 0 ≦ y2 ≦ 0.4, 0 ≦ z2 ≦ 0.4, 0 ≦ w2 ≦ 0.2, and x2 + y2 + z2 + w2 = 1.
[0060] Specifically, M1 can be Mn or a combination of Mn and Al.
[0061] X2 represents the ratio of the number of moles of Ni to the total number of moles of transition metals, and 0.6 ≦ x2 < 1, specifically 0.8 ≦ x2 < 1, and more specifically 0.85 ≦ x2 < 1.
[0062] Y2 represents the ratio of the number of moles of Co to the total number of moles of transition metals, and 0 ≦ y2 ≦ 0.4, specifically 0 < y2 < 0.2, and more specifically 0 < y2 < 0.15.
[0063] Z2 represents the ratio of the number of moles of M1 to the total number of moles of transition metals, and 0 ≦ z2 ≦ 0.4, specifically 0 < z2 < 0.2, and more specifically 0 < z2 < 0.15.
[0064] The w2 indicates the ratio of the number of moles of M2 to the total number of moles of the transition metals, and can be 0≦w2≦0.2, specifically 0≦w2≦0.05.
[0065] When the transition metal hydroxide has the composition represented by Chemical Formula 1, the positive electrode active material produced can exhibit high capacity characteristics.
[0066] The lithium-containing raw material may be, for example, at least one selected from the group consisting of lithium carbonate (Li2CO3), lithium hydroxide (LiOH), LiNO3, CH3COOLi, and Li2(COO)2, and may be preferably lithium carbonate (Li2CO3), lithium hydroxide (LiOH), or a combination thereof.
[0067] When preparing the positive electrode active material, the positive electrode active material precursor and the lithium-containing raw material may be mixed in a molar ratio of 1:1 to 1:1.2 or 1:1 to 1:1.1. When the lithium-containing raw material is within the above range, the capacity of the positive electrode active material may be improved and the by-product of unreacted Li may be minimized.
[0068] The calcination can be carried out at a temperature of 700° C. to 1000° C. When the calcination temperature is within the above range, the reaction between the raw materials can be sufficiently carried out and the particles can grow uniformly.
[0069] The calcination can be carried out for 5 to 35 hours. When the calcination time is within the above range, a highly crystalline positive electrode active material can be obtained, the particle size is appropriate, and production efficiency can be improved.
[0070] The method for preparing a positive electrode active material according to the present invention may further include washing the lithium transition metal oxide prepared in step (B) with a washing solution and drying the washed lithium transition metal oxide. The washing step is a step for removing by-products such as residual lithium present in the lithium transition metal oxide prepared in step (B), and the drying step is a step for removing moisture from the positive electrode active material that contains moisture after the washing step.
[0071] In addition, the method for manufacturing a positive electrode active material according to the present invention may further include a step of mixing a coating element-containing raw material with a dried lithium transition metal oxide and heat-treating the mixture to form a coating layer, thereby manufacturing a positive electrode active material having a coating layer formed on a surface of the lithium transition metal oxide.
[0072] The metal element contained in the coating element-containing raw material may be Zr, B, W, Mo, Cr, Nb, Mg, Hf, Ta, La, Ti, Sr, Ba, Ce, F, P, S, and Y. The coating element-containing raw material may be acetate, nitrate, sulfate, halide, sulfide, hydroxide, oxide, or oxyhydroxide containing the metal element. For example, when the metal element is B, boric acid (H3BO3) may be used.
[0073] The coating element-containing raw material may be included in the dried lithium transition metal oxide in an amount of 200 ppm to 2000 ppm by weight. When the content of the coating element-containing raw material is within the above range, the capacity of the battery may be improved, and the resulting coating layer may suppress a direct reaction between the electrolyte and the lithium transition metal oxide, thereby improving the long-term performance characteristics of the battery.
[0074] The heat treatment can be carried out at a temperature of 200°C to 400°C. When the heat treatment temperature is within the above range, a coating layer can be formed while maintaining the structural stability of the transition metal oxide. The heat treatment can be carried out for 1 hour to 10 hours. When the heat treatment time is within the above range, an appropriate coating layer can be formed and production efficiency can be improved.
[0075] positive electrode The present invention can also provide a positive electrode for a lithium secondary battery, which contains the positive electrode active material according to the present invention.
[0076] Specifically, the positive electrode includes a positive electrode current collector and a positive electrode active material layer located on at least one surface of the positive electrode current collector and including the above-mentioned positive electrode active material.
[0077] The positive electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity, and for example, stainless steel, aluminum, nickel, titanium, baked carbon, or aluminum or stainless steel surface treated with carbon, nickel, titanium, silver, etc. can be used. In addition, the positive electrode current collector can usually have a thickness of 3 μm to 500 μm, and fine irregularities can be formed on the surface of the current collector to increase the adhesive force of the positive electrode active material. For example, it can be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.
[0078] The positive electrode active material layer may contain a conductive material and a binder in addition to the positive electrode active material.
[0079] In this case, the positive electrode active material may be included in an amount of 80 wt% to 99 wt%, more specifically, 85 wt% to 98 wt%, based on the total weight of the positive electrode active material layer. When included in the above content range, excellent capacity characteristics can be exhibited.
[0080] In this case, the conductive material is used to impart conductivity to the electrode, and can be used without any particular limitation as long as it does not cause a chemical change in the battery to be constructed and has electronic conductivity. Specific examples include graphite such as natural graphite and artificial graphite; carbon-based materials such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fibers; metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive polymers such as polyphenylene derivatives, and one or more of these can be used alone or in combination. The conductive material can be included in an amount of 1% by weight to 30% by weight based on the total weight of the positive electrode active material layer.
[0081] The binder serves to improve adhesion between the positive electrode active material particles and adhesion between the positive electrode active material and the current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene-butadiene rubber (SBR), fluororubber, and various copolymers thereof, and one or more of these may be used alone or in combination. The binder may be included in an amount of 1 wt% to 30 wt% based on the total weight of the positive electrode active material layer.
[0082] The positive electrode may be manufactured by a typical positive electrode manufacturing method, except for using the positive electrode active material. Specifically, the positive electrode active material and, optionally, a binder and a conductive material may be dissolved or dispersed in a solvent to prepare a positive electrode active material slurry, which may be coated on a positive electrode current collector, followed by drying and rolling. In this case, the types and contents of the positive electrode active material, binder, and conductive material are as described above.
[0083] The solvent may be a solvent commonly used in the art, such as dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, or water, and may be used alone or in combination of two or more of these. The amount of the solvent used is sufficient to dissolve or disperse the positive electrode active material, conductive material, and binder, and to provide a viscosity that allows excellent thickness uniformity during subsequent coating for the manufacture of a positive electrode, taking into consideration the coating thickness of the slurry and the manufacturing yield.
[0084] As another method, the positive electrode can also be produced by casting the positive electrode active material layer forming slurry on another support, peeling the slurry from the support, and laminating the resulting film on a positive electrode current collector.
[0085] Lithium secondary battery In addition, the present invention can provide an electrochemical device including the positive electrode of the present invention. The electrochemical device can be, specifically, a battery, a capacitor, or the like, and more specifically, a lithium secondary battery.
[0086] Specifically, the lithium secondary battery includes a positive electrode, a negative electrode facing the positive electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte. Since the positive electrode is as described above, a detailed description thereof will be omitted, and only the remaining components will be described in detail below.
[0087] Also, the lithium secondary battery may optionally further include a battery container that houses an electrode assembly of the positive electrode, the negative electrode, and the separator, and a sealing member that seals the battery container.
[0088] In the lithium secondary battery, the negative electrode includes a negative electrode current collector and a negative electrode active material layer located on the negative electrode current collector.
[0089] The negative electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has high conductivity, and may be, for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface treated with carbon, nickel, titanium, silver, or aluminum-cadmium alloy. The negative electrode current collector may have a thickness of usually 3 μm to 500 μm, and like the positive electrode current collector, the surface of the current collector may be formed with fine irregularities to strengthen the binding force of the negative electrode active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.
[0090] The negative electrode active material layer includes a negative electrode active material, and optionally a binder and a conductive material.
[0091] The negative electrode active material may be a compound capable of reversible intercalation and deintercalation of lithium. Specific examples of the negative electrode active material include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloys, Sn alloys, and Al alloys; SiO β(0<β<2), metal oxides capable of doping and dedoping lithium, such as SnO2, vanadium oxide, and lithium vanadium oxide; or composites containing the metallic compounds and carbonaceous materials, such as Si-C composites or Sn-C composites, and any one or a mixture of two or more of these may be used. In addition, a thin film of metallic lithium may be used as the negative electrode active material. In addition, the carbon material may be either low-crystalline carbon or high-crystalline carbon. Representative examples of low crystalline carbon include soft carbon and hard carbon, and representative examples of high crystalline carbon include amorphous, plate-like, flake-like, spherical or fibrous natural or artificial graphite, kish graphite, pyrolytic carbon, mesophase pitch based carbon fiber, meso-carbon microbeads, mesophase pitches, and high-temperature fired carbon such as petroleum or coal tar pitch derived cokes.
[0092] The negative electrode active material may be included in an amount of 80% by weight to 99% by weight based on the total weight of the negative electrode active material layer.
[0093] The binder is a component that facilitates bonding between the conductive material, the active material, and the current collector, and can be added in an amount of 0.1% by weight to 10% by weight based on the total weight of the negative electrode active material layer. Examples of such binders include polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, nitrile-butadiene rubber, fluororubber, and various copolymers thereof.
[0094] The conductive material is a component for further improving the conductivity of the negative electrode active material, and may be added in an amount of 10% by weight or less, specifically 5% by weight or less, based on the total weight of the negative electrode active material layer. Such a conductive material is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity, and examples of such conductive materials include graphite such as natural graphite and artificial graphite; carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fibers and metal fibers; metal powders such as carbon fluoride, aluminum, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.
[0095] The negative electrode active material layer can be produced by applying a negative electrode active material layer forming slurry, which is prepared by dissolving or dispersing a negative electrode active material, and optionally a binder and a conductive material, in a solvent, onto a negative electrode current collector and drying the slurry. Alternatively, the negative electrode active material layer forming slurry can be cast onto a separate support, and then peeled off from the support to obtain a film, which can be laminated onto the negative electrode current collector.
[0096] Meanwhile, in the lithium secondary battery, the separator separates the negative electrode and the positive electrode and provides a path for lithium ions to move. Any separator that is generally used as a separator in a lithium secondary battery can be used without any particular limitation. In particular, a separator that has low resistance to ion movement of the electrolyte and has excellent humidification ability of the electrolyte solution is preferable. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin-based polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminate structure of two or more layers thereof can be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of a high-melting point glass fiber, a polyethylene terephthalate fiber, etc., can be used. In addition, a coated separator containing a ceramic component or a polymeric material can be used to ensure heat resistance or mechanical strength, and can be selectively used as a single layer or a multilayer structure.
[0097] In addition, examples of the electrolyte used in the present invention include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the production of lithium secondary batteries, but are not limited to these.
[0098] Specifically, the electrolyte may include an organic solvent and a lithium salt.
[0099] The organic solvent can be used without any particular limitation as long as it serves as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the organic solvent can be an ester solvent such as methyl acetate, ethyl acetate, γ-butyrolactone, or ε-caprolactone; an ether solvent such as dibutyl ether or tetrahydrofuran; a ketone solvent such as cyclohexanone; an aromatic hydrocarbon solvent such as benzene or fluorobenzene; dimethylcarbonate (DMC), diethylcarbonate (DEC), ethylmethylcarbonate (EMC), ethylene carbonate (EC), or propylene carbonate (propylene carbonate). Carbonate-based solvents such as ethylene carbonate (PC); alcohol-based solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (R is a straight-chain, branched or cyclic hydrocarbon group having 2 to 20 carbon atoms, which may contain a double bond aromatic ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes may be used. Among them, carbonate-based solvents are preferred, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate) having high ionic conductivity and high dielectric constant that can improve the charge / discharge performance of a battery and a low-viscosity linear carbonate compound (e.g., ethyl methyl carbonate, dimethyl carbonate or diethyl carbonate) is more preferred. In this case, the cyclic carbonate and the linear carbonate are mixed in a volume ratio of about 1:1 to about 1:9, so that the electrolyte can exhibit excellent performance.
[0100] The lithium salt can be used without any particular limitation as long as it is a compound capable of providing lithium ions used in a lithium secondary battery. Specifically, the lithium salt may be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2. The concentration of the lithium salt is preferably within the range of 0.1M to 2.0M. When the concentration of the lithium salt is within the above range, the electrolyte has appropriate conductivity and viscosity, so that it can exhibit excellent electrolyte performance and lithium ions can move effectively.
[0101] In addition to the electrolyte components, the electrolyte may further contain one or more additives such as haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ethers, ethylenediamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinoneimine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride, in order to improve the life characteristics of the battery, suppress the decrease in the capacity of the battery, and improve the discharge capacity of the battery. In this case, the additives may be contained in an amount of 0.1% by weight to 5% by weight based on the total weight of the electrolyte.
[0102] As described above, the lithium secondary battery including the positive electrode active material according to the present invention stably exhibits excellent discharge capacity, output characteristics and life characteristics, and is therefore useful in portable devices such as mobile phones, notebook computers and digital cameras, and electric vehicles such as hybrid electric vehicles (HEVs).
[0103] Therefore, according to another embodiment of the present invention, there is provided a battery module including the lithium secondary battery as a unit cell, and a battery pack including the same.
[0104] The battery module or battery pack may be used as a power source for one or more medium- to large-sized devices, such as a power tool; an electric vehicle (EV), a hybrid electric vehicle, and a plug-in hybrid electric vehicle (PHEV); or a power storage system.
[0105] The shape of the lithium secondary battery is not particularly limited, but may be a cylindrical type using a can, a square type, a pouch type, a coin type, or the like.
[0106] The lithium secondary battery can be used not only as a battery cell used as a power source for a small device, but also as a unit battery in a medium- to large-sized battery module including a large number of battery cells.
[0107] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention may, however, be embodied in many different forms and should not be construed as limited to the embodiments set forth herein.
[0108] Manufacturing Example 1 NiSO4, CoSO4, and MnSO4 were mixed in distilled water in amounts such that the molar ratio of nickel:cobalt:manganese was 88:5:7 to prepare an aqueous transition metal solution with a concentration of 2.4 M.
[0109] Next, deionized water was added to the reactor, and nitrogen gas was purged into the reactor to remove dissolved oxygen in the water and create a non-oxidizing atmosphere in the reactor. Next, 7.96M NaOH was added to maintain the pH in the reactor at 11.9.
[0110] Next, the transition metal aqueous solution was added to the reactor at a rate of 510 mL / hr, and a 7.96 M NaOH aqueous solution was added at a rate of 306 mL / hr, and a 5.08 M NH4OH aqueous solution was added at a rate of 96 mL / hr. The coprecipitation reaction was carried out for 40 hours under the conditions of a reaction temperature of 45° C., pH 11.4, and a stirring speed of 300 rpm to obtain Ni with an average particle size of 10 μm. 0.88 Co 0.05 Mn 0.07 A positive electrode active material precursor A represented by (OH)2 was prepared.
[0111] Manufacturing Example 2 NiSO4, CoSO4, and MnSO4 were mixed in distilled water in amounts such that the molar ratio of nickel:cobalt:manganese was 88:5:7 to prepare an aqueous transition metal solution with a concentration of 2.4 M.
[0112] Next, deionized water was added to the reactor, and nitrogen gas was purged into the reactor to remove dissolved oxygen in the water and create a non-oxidizing atmosphere in the reactor. Next, 7.96M NaOH was added to maintain the pH in the reactor at 11.4.
[0113] Next, the transition metal aqueous solution was added to the reactor at a rate of 510 mL / hr, and a 7.96 M NaOH aqueous solution was added at a rate of 306 mL / hr, and a 5.08 M NH4OH aqueous solution was added at a rate of 72 mL / hr. The coprecipitation reaction was carried out for 40 hours under the conditions of a reaction temperature of 45° C., pH 11.4, and a stirring speed of 300 rpm to obtain Ni with an average particle size of 10 μm. 0.88 Co 0.05 Mn 0.07 A positive electrode active material precursor B represented by (OH)2 was prepared.
[0114] Production Example 3 NiSO4, CoSO4, and MnSO4 were mixed in distilled water in amounts such that the molar ratio of nickel:cobalt:manganese was 88:5:7 to prepare an aqueous transition metal solution with a concentration of 2.4 M.
[0115] Next, deionized water was added to the reactor, and nitrogen gas was purged into the reactor to remove dissolved oxygen in the water and create a non-oxidizing atmosphere in the reactor. Next, 7.96M NaOH was added to maintain the pH in the reactor at 11.9.
[0116] Next, the transition metal aqueous solution was added to the reactor at a rate of 510 mL / hr, and a 7.96 M NaOH aqueous solution was added at a rate of 306 mL / hr, and a 5.08 M NH4OH aqueous solution was added at a rate of 204 mL / hr. The coprecipitation reaction was carried out for 40 hours under the conditions of a reaction temperature of 53° C., pH 11.4, and a stirring speed of 300 rpm to obtain Ni with an average particle size of 10 μm. 0.88 Co 0.05 Mn 0.07 A positive electrode active material precursor C represented by (OH)2 was prepared.
[0117] Production Example 4 NiSO4, CoSO4, and MnSO4 were mixed in distilled water in amounts such that the molar ratio of nickel:cobalt:manganese was 88:5:7 to prepare an aqueous transition metal solution with a concentration of 2.4 M.
[0118] Next, deionized water was added to the reactor, and nitrogen gas was purged into the reactor to remove dissolved oxygen in the water and create a non-oxidizing atmosphere in the reactor. Next, 7.96M NaOH was added to maintain the pH in the reactor at 11.9.
[0119] Next, the transition metal aqueous solution was added to the reactor at a rate of 510 mL / hr, and a 7.96 M NaOH aqueous solution was added at a rate of 306 mL / hr, and a 5.08 M NH4OH aqueous solution was added at a rate of 204 mL / hr. The coprecipitation reaction was carried out for 40 hours under the conditions of a reaction temperature of 60° C., pH 11.4, and a stirring speed of 300 rpm to obtain Ni with an average particle size of 10 μm. 0.88 Co 0.05 Mn 0.07 A positive electrode active material precursor D represented by (OH)2 was prepared.
[0120] Production Example 5 NiSO4, CoSO4, and MnSO4 were mixed in distilled water in amounts such that the molar ratio of nickel:cobalt:manganese was 88:5:7 to prepare an aqueous transition metal solution with a concentration of 2.4 M.
[0121] Next, deionized water was added to the reactor, and nitrogen gas was purged into the reactor to remove dissolved oxygen in the water and create a non-oxidizing atmosphere in the reactor. Next, 7.96M NaOH was added to maintain the pH in the reactor at 11.9.
[0122] Next, the transition metal aqueous solution was added to the reactor at a rate of 510 mL / hr, and a 7.96 M NaOH aqueous solution and a 5.08 M NH4OH aqueous solution were added at a rate of 306 mL / hr and 306 mL / hr, respectively, while carrying out a coprecipitation reaction for 40 hours under conditions of a reaction temperature of 60° C., pH 11.4, and a stirring speed of 300 rpm, to obtain Ni with an average particle size of 10 μm. 0.88 Co 0.05 Mn 0.07 A positive electrode active material precursor E represented by (OH)2 was prepared.
[0123] Experimental Example 1: Confirmation of the aspect ratio of the positive electrode active material precursor crystal grains The positive electrode active material precursors produced in Production Examples 1 to 5 were subjected to X-ray diffraction analysis (Empyrean, manufactured by Malvern Panalytical Co., Ltd.) to derive the aspect ratios of the crystal grains, which are shown in the following Table 1. In this case, the conditions for the X-ray diffraction analysis and the method for deriving the aspect ratios of the crystal grains are as described above.
[0124] [Table 1]
[0125] Example 1 The positive electrode active material precursor produced in Production Example 1 was mixed with LiOH in a molar ratio of 1:1.05, and 2 mol% of Al and 0.37 mol% of Zr were added relative to the total moles of the transition metals contained in the positive electrode active material precursor. The mixture was then fired at 780°C for 10 hours to produce a lithium transition metal oxide (composition: Li 1.05 Ni 0.8563 Co0.05 Mn 0.07 Al 0.02 Zr 0.0037 O2) was manufactured.
[0126] Next, the lithium transition metal oxide was mixed with water in a weight ratio of 1:0.8, and washed with water.
[0127] After washing with water, boric acid was mixed so that 100 parts by weight of the lithium transition metal oxide contained 1000 ppm of B, and this was heat-treated at 300°C for 5 hours to produce a positive electrode active material in which a B coating layer was formed on the surface of the lithium transition metal oxide.
[0128] Example 2 A positive electrode active material was produced in the same manner as in Example 1, except that the positive electrode active material precursor produced in Production Example 2 was used instead of the positive electrode active material precursor produced in Production Example 1.
[0129] Comparative Example 1 A positive electrode active material was produced in the same manner as in Example 1, except that the positive electrode active material precursor produced in Production Example 3 was used instead of the positive electrode active material precursor produced in Production Example 1.
[0130] Comparative Example 2 A positive electrode active material was produced in the same manner as in Example 1, except that the positive electrode active material precursor produced in Production Example 4 was used instead of the positive electrode active material precursor produced in Production Example 1.
[0131] Comparative Example 3 A positive electrode active material was produced in the same manner as in Example 1, except that the positive electrode active material precursor produced in Production Example 5 was used instead of the positive electrode active material precursor produced in Production Example 1.
[0132] Experimental Example 2: Analysis of voids contained in secondary particles The positive electrode active materials prepared in Examples 1 and 2 and Comparative Examples 1 to 3 were processed by ion milling, and then SEM images of the cross sections of the secondary particles including voids were obtained using a SEM (FEI, Quanta FEG 250). The SEM images were analyzed using a commercial program, Image J, at an image threshold of 1 to 2%. The area of the closed voids distributed inside the secondary particles was found to be 0.002 μm 2 The minimum area (x) of the rectangle that contains all voids exceeding 0.002 μm 2 The total area (y) of voids exceeding 1000 and the number of voids were obtained, and are shown in Table 2 below. At this time, at least three secondary particles per sample were analyzed, and the average value was used.
[0133] 1 to 5 are diagrams showing cross-sectional SEM images of one secondary particle of the positive electrode active materials produced in Examples 1 and 2 of the present invention and Comparative Examples 1 to 3, and the size and position distribution of voids.
[0134] [Table 2]
[0135] Experimental example 3: Evaluation of capacitance characteristics Lithium secondary batteries were produced using the positive electrode active materials produced in Examples 1 and 2 and Comparative Examples 1 to 3, and the capacity characteristics of each of these batteries were evaluated.
[0136] Specifically, the positive electrode active material, carbon black conductive material, and polyvinylidene fluoride binder of each of Examples 1-2 and Comparative Examples 1-3 were mixed in a weight ratio of 97.5:1:1.5 in N-methylpyrrolidone solvent to prepare a positive electrode active material layer slurry. The positive electrode active material layer slurry was applied to one side of an aluminum current collector having a thickness of 16.5 μm, dried at 130° C., and then rolled to prepare a positive electrode.
[0137] Meanwhile, a negative electrode active material (carbon black) and a polyvinylidene fluoride binder were mixed in a weight ratio of 97.5:2.5 in N-methylpyrrolidone solvent to prepare a slurry for forming a negative electrode active material layer. The slurry for forming a negative electrode active material layer was applied to one side of a copper current collector having a thickness of 16.5 μm, dried at 130° C., and then rolled to prepare a negative electrode.
[0138] A porous polyethylene separator was interposed between the positive and negative electrodes to prepare an electrode assembly, which was then placed inside a battery case, and an electrolyte was injected into the case to prepare a lithium secondary battery. The electrolyte was prepared by dissolving 1M LiPF6 in an organic solvent in which ethylene carbonate (EC): dimethyl carbonate (DMC): ethyl methyl carbonate (EMC) was mixed in a ratio of 3:4:3, and the electrolyte was injected to prepare the lithium secondary batteries according to Examples 1-2 and Comparative Examples 1-3.
[0139] Each of the lithium secondary batteries of Examples 1 and 2 and Comparative Examples 1 to 3 was charged to 4.25 V at a constant current of 0.2 C at 25° C. and discharged to 3.0 V at a constant current of 0.2 C, which constituted one cycle, and the charge capacity and discharge capacity in the first cycle were measured and shown in Table 3 below. The discharge capacity in the first cycle was divided by the charge capacity, and the value multiplied by 100 was taken as the charge / discharge efficiency (%), which is shown in Table 3 below.
[0140] [Table 3]
[0141] Referring to Tables 1 to 3, it can be seen that the cathode active material according to the present invention is prepared from a cathode active material precursor having a crystal grain aspect ratio that satisfies a specific range, and the voids contained in the secondary particles satisfy specific conditions, so that the cathode active material according to the present invention has excellent initial discharge capacity and initial charge / discharge efficiency characteristics.
Claims
1. The lithium transition metal oxide contains 60 mol % or more of nickel relative to the total moles of transition metals other than lithium, and is in the form of secondary particles formed by aggregation of primary particles; The lithium transition metal oxide is a positive electrode active material that satisfies the following formula 1: [Formula 1] [0010] In the above formula 1, The x and y are obtained from a cross-sectional SEM image analysis of the secondary particle, and the x is an area of the closed voids distributed inside the secondary particle that is less than 0.002 μm 2 The minimum area of a rectangle that includes all voids exceeding 2 ) and the y is the area of the closed voids distributed inside the secondary particle of 0.002 μm 2 The area of the voids (unit: μm 2 ) is the sum of
2. 2. The positive electrode active material according to claim 1, wherein in formula 1, 20≦x≦400.
3. The positive electrode active material according to claim 1 or 2, wherein in formula 1, 0.01≦y≦5.
0.
4. The area of the closed voids distributed inside the secondary particles is 0.002 μm 2 The average void area of voids exceeding 0.01 μm 2 / piece ~ 0.1μm 2 The positive electrode active material according to claim 1 , wherein the positive electrode active material is a ZnO-based ...
5. The positive electrode active material according to claim 1 , wherein the lithium transition metal oxide has a composition represented by the following chemical formula 1: [Chemical formula 1] Li a Ni x1 Co y1 M1 z1 M2 w1 O 2 In the above Chemical Formula 1, M1 is at least one selected from Mn and Al, M2 is at least one selected from B, Zr, Y, Mo, Cr, V, W, Ta, and Nb, 0.9≦a≦1.2, 0.6≦x1≦1.0, 0≦y1≦0.4, 0≦z1≦0.4, 0≦w1≦0.2, and x1+y1+z1+w1=1.
6. 6. The positive electrode active material of claim 5, wherein, in Formula 1, 0.85≦x1<1.0, 0<y1<0.15, and 0<z1<0.
15.
7. (A) preparing a positive electrode active material precursor containing 60 mol % or more of nickel relative to the total number of moles of transition metals, containing a transition metal hydroxide in the form of secondary particles formed by aggregation of primary particles, and having an aspect ratio of crystal grains of 4.0 to 10.0; and (B) mixing the positive electrode active material precursor and a lithium-containing raw material and baking the mixture to produce a lithium transition metal oxide.
8. The method for producing a positive electrode active material according to claim 7, wherein the transition metal hydroxide has a composition represented by the following chemical formula 2: [Chemical formula 2] Ni x2 Co y2 M1' z2 M2' w2 (OH) 2 In Chemical Formula 2, M1' is at least one selected from Mn and Al, M2' is at least one selected from B, Zr, Y, Mo, Cr, V, W, Ta and Nb, 0.6≦x2≦1.0, 0≦y2≦0.4, 0≦z2≦0.4, 0≦w2≦0.2, and x2+y2+z2+w2=1.
9. 9. The method for producing a positive electrode active material according to claim 8, wherein, in Chemical Formula 1, 0.85≦x2<1.0, 0<y2<0.15, and 0<z2<0.
15.
10. A positive electrode for a lithium secondary battery, comprising the positive electrode active material according to claim 1 .
11. A lithium secondary battery comprising the positive electrode according to claim 10.
Citation Information
Patent Citations
Positive electrode active substance, manufacturing method for same and battery provided with positive electrode active substance
JP2009259605A
Positive electrode active material for nonaqueous electrolyte secondary batteries, manufacturing method thereof, and nonaqueous electrolyte secondary battery arranged by use thereof
JP2015072800A
Method for manufacturing transition metal composite hydroxide particle, transition metal composite hydroxide particle, method for manufacturing nonaqueous electrolyte secondary battery cathode active material and nonaqueous electrolyte secondary battery cathode active material
JP2019149349A