Method for Producing Superabsorbent Polymer Particles
The method addresses roll mill cleaning issues in superabsorbent polymer particle production by adjusting feed and gap settings to prevent and remove deposits, enhancing efficiency and drying effectiveness.
Patent Information
- Application Number
- JP2021551574
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-03-01
- Filing Date
- 2020-02-21
- Publication Date
- 2024-09-26
- Estimated Expiration
- 2040-02-21
AI Technical Summary
Existing methods for producing superabsorbent polymer particles face challenges in effectively cleaning roll mills used for grinding dry polymer gels, leading to inefficiencies and increased power consumption due to deposits on the rolls.
A method involving monitoring roll mill deflection and power consumption, adjusting feed rate and gap width to prevent and remove deposits, including reducing feed if deflection and power consumption exceed set values, and optionally changing gap width to facilitate cleaning.
Effectively cleans roll mills by reducing deposits, maintaining efficient operation, and ensuring complete drying of polymer particles, thereby improving the production process.
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing superabsorbent polymer particles, comprising the steps of polymerizing a monomer solution, drying the resulting polymer gel and grinding the dried polymer gel in a roll mill, wherein the rolls of the roll mill are cleaned by reducing the feed to the roll mill and operating the roll mill with reduced feed if the deflection and / or power consumption increases above a set value and by increasing the feed to the roll mill. [Background technology]
[0002] Superabsorbent polymer particles are also used to make diapers, tampons, sanitary napkins, and other hygiene articles, as well as water retention agents in market gardens. Superabsorbent polymer particles are also often referred to as "absorbent resins," "superabsorbents," "superabsorbent polymers," "absorbent polymers," "absorbent gelling materials," "hydrophilic polymers," or "hydrogels."
[0003] Commercially available superabsorbent polymer particles are polymers of partially neutralized acrylic acid, as described in the monograph "Modern Superabsorbent Polymer Technology", FL Buchholz and AT Graham, Wiley-VCH, 1998, pages 69-103. Summary of the Invention [Problem to be solved by the invention]
[0004] It is an object of the present invention to provide an improved method for producing superabsorbent polymer particles, and in particular, improved cleaning of roll mills used in the comminution of dried polymer gels. [Means for solving the problem]
[0005] The object is to provide a method for producing superabsorbent polymer particles, comprising the steps of: a) partially neutralized acrylic acid, b) at least one crosslinker, and c) at least one initiator polymerizing a monomer solution comprising: drying the resulting polymer gel; A process for grinding the dried polymer gel with a roll mill, the rolls of the roll mill being configured to perform the following steps: i) determining the deflection and / or power consumption of the roll mill; ii) reducing the feed rate to the roll mill or stopping the feed to the roll mill if the deflection and / or power consumption increases above a set value; iii) optionally increasing the gap width between the rolls of the roll mill; iv) operating the roll mill at a reduced feed rate or with the feed stopped; v) optionally reducing the gap width between the rolls of the roll mill; vi) optionally operating the roll mill at a reduced gap width until deflection and / or power consumption decrease below set values; vii) optionally increasing the gap width between the rolls of the roll mill to the gap width prior to step ii); and viii) increasing the feed rate to the roll mill to the rate prior to step ii) or resuming feed to the roll mill. and if in step ii) the supply to the roll mill is stopped and in step iii) the gap width between the rolls of the roll mill is increased, then in step v) the gap width between the rolls of the roll mill must be reduced; classifying the resulting polymer particles; This was achieved by a method including:
[0006] The deflection set point is based on the roll vibrations that indicate buildup on the roll. The deflection set point is, for example, 5% higher than the deflection of a clean roll at the same feed rate.
[0007] The power consumption setpoint is based on the power consumption of the roll mill which indicates build-up on the rolls, e.g. 5% higher than the power consumption of the roll mill with a clean roll at the same feed rate.
[0008] The roll mill is a single-stage or multi-stage roll mill, preferably a two-stage or three-stage roll mill. Each stage of the roll mill consists of a pair of rolls, one of which is fixed and the other is free. If the elastic material, i.e., the incompletely dried polymer particles, sticks onto the rolls and the elastic material is larger than the gap width between the rolls, the free roll may sag in the horizontal direction. The sagging causes the free roll to vibrate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] In a first embodiment of the present invention, the rolls of the roll mill are i) determining the roll deflection and / or the power consumption of the roll mill; ii) reducing the feed rate to the roll mill if the deflection and / or power consumption increases above a set value; iv) operating the roll mill at a reduced feed rate until the deflection and / or power consumption decreases below a set value; viii) increasing the feed rate to the roll mill to the rate prior to step ii). is purified by.
[0010] If the deflection and / or power consumption is above the set value for preferably at least 0.5 seconds, more preferably at least 1 second, most preferably at least 1.5 seconds, the feed rate to the roll mill is reduced in step ii).
[0011] If the deflection and / or power consumption remains below the set value for preferably at least 1.5 seconds, more preferably at least 2.0 seconds, and most preferably at least 2.5 seconds, the feed rate to the roll mill is increased in step viii).
[0012] The feed rate to the roll mill in step ii) may be gradually reduced and / or the feed rate to the roll mill in step vii) may be gradually increased. A gradually reduced feed rate means that the roll mill is operated at a reduced feed rate for a predefined time. If the deflection and / or power consumption is still above the set value, the feed rate is reduced again. A gradually increased feed rate means that the roll mill is operated at an increased feed rate for a predefined time. If the deflection and / or power consumption is still below the set value, the feed rate is increased again.
[0013] The predefined time is preferably 1 to 30 seconds, more preferably 3 to 20 seconds, and most preferably 5 to 15 seconds.
[0014] The amount of feed to the roll mill in step ii) is reduced stepwise, preferably by 2 to 20% per step, more preferably by 5 to 15% per step, and most preferably by 7 to 10% per step, based on the amount of feed before step ii).
[0015] The minimum feed rate to the roll mill in step iv) is preferably at least 25%, more preferably at least 30%, most preferably at least 35% based on the feed rate before step ii).
[0016] The amount of feed to the roll mill in step viii) is increased stepwise, based on the amount of feed before step ii), preferably by 0.5 to 10% per step, most preferably by 1.0 to 5% per step, and most preferably by 1.5 to 5% per step.
[0017] The present invention is based on the discovery that the rolls of a roll mill can be cleaned by reducing the feed rate.
[0018] In a second embodiment of the present invention, the rolls of the roll mill are i) determining the roll deflection and / or the power consumption of the roll mill; ii) stopping the feed to the roll mill if the deflection and / or power consumption increases above a set value; iv) stopping the feed and running the roll mill; v) reducing the gap width between the rolls of the roll mill; vi) operating the roll mill at a reduced gap width until the deflection and / or power consumption decreases below a set value; vii) increasing the gap width between the rolls of the roll mill to the gap width before step ii); and viii) restarting the feed rate to the roll mill is purified by.
[0019] If the deflection and / or power consumption remains above the set value for preferably at least 0.5 seconds, more preferably at least 1 second, most preferably at least 1.5 seconds, the feed to the roll mill is stopped in step ii).
[0020] The roll mill is preferably run with the feed stopped in step iv) for at least 0.5 minutes, more preferably at least 1.0 minutes, and most preferably at least 2.0 minutes.
[0021] The gap width between the rolls of the roll mill in step v) is preferably reduced to less than 0.1 mm, more preferably less than 0.05 mm, most preferably less than 0.02 mm.
[0022] If the deflection and / or power consumption remains below the set value for preferably at least 1.5 seconds, more preferably at least 2.0 seconds, and most preferably at least 2.5 seconds, the feed rate to the roll mill is increased in step viii).
[0023] The invention is based on the discovery that the rolls of a roll mill can be cleaned by stopping the feed and reducing the gap width as much as possible. Under these conditions, the incompletely dried polymer particles become completely dried and can be easily removed from the rolls.
[0024] In a third embodiment of the present invention, the rolls of the roll mill are i) determining the roll deflection and / or the power consumption of the roll mill; ii) stopping the feed to the roll mill if the deflection and / or power consumption increases above a set value; iii) increasing the gap width between the rolls of the roll mill; iv) stopping the feed and running the roll mill; v) reducing the gap width between the rolls of the roll mill; vi) operating the roll mill at a reduced gap width until the deflection and / or power consumption decreases below a set value; vii) increasing the gap width between the rolls of the roll mill to the gap width before step ii); and viii) restarting the feed rate to the roll mill is purified by.
[0025] If the deflection and / or power consumption remains above the set value for preferably at least 0.5 seconds, more preferably at least 1 second, most preferably at least 1.5 seconds, the feed to the roll mill is stopped in step ii).
[0026] The gap width between the rolls of the roll mill in step iii) is preferably increased to at least 1.0 mm, more preferably at least 1.5 mm, and most preferably at least 2.0 mm.
[0027] The roll mill is preferably run with the feed stopped in step iv) for at least 0.5 minutes, more preferably at least 1.0 minutes, and most preferably at least 2.0 minutes.
[0028] The gap width between the rolls of the roll mill in step v) is preferably reduced to less than 0.1 mm, more preferably less than 0.05 mm, most preferably less than 0.02 mm.
[0029] If the deflection and / or power consumption remains below the set value for preferably at least 1.5 seconds, more preferably at least 2.0 seconds, and most preferably at least 2.5 seconds, the feed rate to the roll mill is increased in step viii).
[0030] The invention is based on the discovery that the rolls of a roll mill can be cleaned by stopping the feed and reducing the gap width as much as possible. Under these conditions, the incompletely dried polymer particles are completely dried and can be easily removed from the rolls. By increasing the gap width after stopping the feed, the polymer particles are quickly removed from the roll mill, allowing the next step to start sooner.
[0031] The preparation of the superabsorbent polymer particles is described in detail below.
[0032] Superabsorbent polymer particles are made by polymerizing a monomer solution and are typically water-insoluble.
[0033] The acrylic acid typically contains a polymerization inhibitor, preferably a hydroquinone monoether, as a storage stabilizer.
[0034] The monomer solution preferably contains at most 250 ppm by weight, preferably at most 150 ppm by weight, more preferably at most 100 ppm by weight, preferably at least 10 ppm by weight, more preferably at least 30 ppm by weight, in particular around 50 ppm by weight of hydroquinone monoether, in each case based on acrylic acid before neutralization. For example, the monomer solution can be prepared by using acrylic acid with an appropriate content of hydroquinone monoether.
[0035] Suitable crosslinking agents b) are compounds that have at least two groups suitable for crosslinking.Such groups are, for example, ethylenically unsaturated groups that can be polymerized into polymer chains by free radicals, and functional groups that can form covalent bonds with the acid groups of acrylic acid.In addition, polyvalent metal salts that can form coordinate bonds with at least two acid groups of acrylic acid are also suitable as crosslinking agents b).
[0036] The crosslinking agent b) is preferably a compound having at least two polymerizable groups, which can be polymerized by free radicals into a polymer network.Suitable crosslinking agents b) are, for example, ethylene glycol dimethacrylate, diethylene glycol diacrylate, polyethylene glycol diacrylate, allyl methacrylate, trimethylolpropane triacrylate, triallylamine, tetraallyl ammonium chloride, tetraallyloxyethane, as described in EP 0530438 A1, EP 0547847 A1, EP 0559476 A1, EP 0632068 A1, WO 93 / 21237 A1, WO 2003 / 104299 A, etc. 1, di- and triacrylates, as described in WO 2003 / 104300 A1, WO 2003 / 104301 A1, and DE 10331450 A1, mixed acrylates which contain further ethylenically unsaturated groups in addition to acrylate groups, as described in DE 10331456 A1 and DE 10355401 A1, or mixtures of crosslinkers, as described, for example, in DE 19543368 A1, DE 19646484 A1, WO 90 / 15830 A1, and WO 2002 / 032962 A2.
[0037] The amount of crosslinker b) is preferably 0.05 to 1.5% by weight, more preferably 0.1 to 1% by weight, most preferably 0.3 to 0.6% by weight, based in each case on the acrylic acid before neutralization. With increasing crosslinker content, the centrifuge retention capacity (CRC) decreases, reaching 21.0 g / cm 2 The absorbency under pressure passes through a maximum value.
[0038] The initiators c) used may be all compounds which generate free radicals under the polymerization conditions, for example thermal initiators, redox initiators, photoinitiators. Suitable redox initiators are sodium peroxodisulfate / ascorbic acid, hydrogen peroxide / ascorbic acid, sodium peroxodisulfate / sodium bisulfite and hydrogen peroxide / sodium bisulfite. It is preferred to use mixtures of thermal and redox initiators, for example sodium peroxodisulfate / hydrogen peroxide / ascorbic acid. However, the reducing component used is preferably disodium 2-hydroxy-2-sulfonatoacetate or a mixture of disodium 2-hydroxy-2-sulfinatoacetate, disodium 2-hydroxy-2-sulfonatoacetate and sodium bisulfite. Such mixtures are available as Brueggolite® FF6 and Brueggolite® FF7 (Brueggemann Chemicals (Heilbronn; Germany)).
[0039] Typically, an aqueous monomer solution is used. The water content of the monomer solution is preferably 40-75% by weight, more preferably 45-70% by weight, most preferably 50-65% by weight. A monomer suspension, i.e. a monomer solution containing excess sodium acrylate, can also be used. With increasing water content, the energy requirements in the subsequent drying increase, and with decreasing water content, the heat of polymerization may be only insufficiently removed.
[0040] For optimal function, the preferred polymerization inhibitor requires dissolved oxygen. Therefore, the monomer solution may be freed of dissolved oxygen by inertization, i.e., by flushing with an inert gas, preferably nitrogen or carbon dioxide, prior to polymerization. The oxygen content of the monomer solution is preferably reduced to less than 1 ppm by weight, more preferably less than 0.5 ppm by weight, and most preferably less than 0.1 ppm by weight prior to polymerization.
[0041] In order to better control the polymerization reaction, any known chelating agent can be optionally added to the monomer solution or suspension or to its raw materials. Suitable chelating agents are, for example, phosphoric acid, diphosphoric acid, triphosphoric acid, polyphosphoric acid, citric acid, tartaric acid, or salts thereof.
[0042] The monomer solution is polymerized. Suitable reactors are, for example, kneader reactors or belt reactors. In kneaders, the polymer gel formed in the polymerization of aqueous monomer solution or suspension is continuously comminuted by a counter-rotating stirring shaft, for example, as described in WO2001 / 038402A1. Polymerization on a belt is described, for example, in DE3825366A1 and US Pat. No. 6,241,928. Polymerization in a belt reactor forms a polymer gel, which must be comminuted in a further process step, for example, in an extruder or kneader.
[0043] To improve the drying properties, the ground polymer gel obtained by the kneader can be additionally extruded.
[0044] The acid groups of the resulting polymer gel are typically partially neutralized. Neutralization is carried out at the monomer stage. This is typically achieved by mixing in a neutralizing agent, either as an aqueous solution or, preferably, also as a solid. The degree of neutralization is preferably 50-85 mol%, more preferably 60-80 mol%, most preferably 65-75 mol%, and for the neutralization customary neutralizing agents can be used, preferably alkali metal hydroxides, alkali metal oxides, alkali metal carbonates or alkali metal hydrogen carbonates, and mixtures thereof. Instead of the alkali metal salts, ammonium salts can also be used. Particularly preferred alkali metals are sodium and potassium, while sodium hydroxide, potassium hydroxide, and mixtures thereof are very particularly preferred.
[0045] The resulting polymer gel is dried. The dryer is not subject to any restrictions. However, the drying of the polymer gel is preferably carried out by a belt dryer until the residual water content is preferably 0.5-10% by weight, more preferably 1-7% by weight, and most preferably 2-5% by weight, the residual water content being determined by EDANA Recommended Test Method No. WSP230.2(05) "Mass Loss Upon Heating". If the residual water content is too high, the dried polymer gel will have a too low glass transition temperature T g If the residual moisture content is too low, the dried polymer gel will be too brittle and in the subsequent grinding step, a large amount of polymer particles with an excessively small particle size (fines) will be undesirably obtained. The solids content of the gel before drying is preferably 25-90% by weight, more preferably 35-70% by weight, most preferably 40-60% by weight. However, a fluidized bed dryer or a paddle dryer may also be optionally used for drying purposes.
[0046] The dried polymer gel is then crushed and classified.
[0047] The average particle size of the polymer particles taken as product fraction is preferably at least 200 μm, more preferably between 250 and 600 μm, very particularly between 300 and 500 μm. The average particle size of the product fraction may be determined by EDANA Recommended Test Method No. WSP220.2(05) "Particle Size Distribution", in which the mass percentages of the sieved fractions are plotted in cumulative form and the average particle size is determined graphically. The average particle size here is the mesh size value that gives rise to the cumulative 50% by weight.
[0048] To improve the properties, the polymer particles can be subsequently thermally surface crosslinked.Suitable surface crosslinking agents are compounds that contain groups that can form covalent bonds with at least two acid groups of the polymer particles.Suitable compounds are, for example, multifunctional amines, multifunctional amidoamines, multifunctional epoxides, as described in EP0083022A2, EP0543303A1 and EP0937736A2, difunctional or multifunctional alcohols, as described in DE3314019A1, DE3523617A1 and EP0450922A2, or β-hydroxyalkylamides, as described in DE10204938A1 and US Patent No. 6,239,230.
[0049] The amount of surface cross-linking agent is preferably 0.001 to 2% by weight, more preferably 0.02 to 1% by weight, most preferably 0.05 to 0.2% by weight, in each case based on the polymer particles.
[0050] In a preferred embodiment of the present invention, polyvalent cations are applied to the particle surface in addition to the surface postcrosslinking agent before, during or after the surface postcrosslinking.
[0051] The polyvalent cations that can be used in the method according to the invention are, for example, divalent cations, such as zinc, magnesium, calcium, iron and strontium cations, trivalent cations, such as aluminum, iron, chromium, rare earth and manganese cations, tetravalent cations, such as titanium and zirconium cations.Possible counterions are chloride, bromide, hydroxide, sulfate, hydrogen sulfide, carbonate, hydrogen carbonate, nitrate, phosphate, hydrogen phosphate, dihydrogen phosphate and carboxylate ions, such as acetate and lactate.Aluminum hydroxide, sulfate and lactate are preferred.Besides metal salts, polyvalent amines can also be used as polyvalent cations.
[0052] The amount of polyvalent cation used is, for example, 0.001 to 1.5% by weight, preferably 0.005 to 1% by weight, more preferably 0.02 to 0.8% by weight, in each case based on the polymer particles.
[0053] Surface postcrosslinking is typically carried out by spraying the solution of surface postcrosslinking agent onto dry polymer particles.After spray application, the polymer particles coated with surface postcrosslinking agent are dried by heat, and surface postcrosslinking reaction can occur either before or during drying.
[0054] The spray application of the solution of the surface postcrosslinker is preferably carried out with a mixer having a moving mixing tool, such as a screw mixer, a disk mixer, and a paddle mixer.Horizontal mixers, such as a paddle mixer, are particularly preferred, and vertical mixers are very particularly preferred.The distinction between horizontal mixers and vertical mixers is made by the position of the mixing shaft, i.e. horizontal mixers have a horizontally mounted mixing shaft, and vertical mixers have a vertically mounted mixing shaft.Suitable mixers are, for example, horizontal Pflugschar® ploughshare mixer (Gebr. Loedige Maschinenbau GmbH; Paderborn; Germany), Vrieco-Nauta continuous mixer (Hosokawa Micron BV; Doetinchem; The Netherlands), Processall Mixmill mixer (Processall Incorporated; Cincinnati; USA), and Schugi Flexomix® (Hosokawa Micron BV; Doetinchem; The Netherlands). However, spraying of the surface postcrosslinker solution can also be carried out in a fluidized bed.
[0055] The surface post-crosslinking agent is typically used in the form of an aqueous solution. The penetration depth of the surface post-crosslinking agent into the polymer particles can be adjusted by the content of the non-aqueous solvent and the total amount of the solvent.
[0056] Surface post-crosslinking by heat is preferably carried out in contact dryer, more preferably in paddle dryer, most preferably in disk dryer.Suitable dryers are, for example, Hosokawa Bepex® Horizontal Paddle Dryer (Hosokawa Micron GmbH; Leingarten; Germany), Hosokawa Bepex® Disc Dryer (Hosokawa Micron GmbH; Leingarten; Germany) and Nara Paddle Dryer (NARA Machinery Europe; Frechen; Germany).Furthermore, fluidized bed dryer can also be used.
[0057] Thermal surface postcrosslinking can be affected in the mixer itself by heating the jacket or blowing in warm air.Downflow dryers, such as tray dryers, rotary tube ovens or heatable screws, are also suitable.It is particularly advantageous to carry out mixing and drying in a fluidized bed dryer.
[0058] The preferred surface postcrosslinking temperature is in the range of 100 to 250° C., preferably 110 to 230° C., more preferably 120 to 210° C., and most preferably 130 to 190° C. The preferred residence time at this temperature in the reaction mixer or dryer is preferably at least 10 minutes, more preferably at least 20 minutes, most preferably at least 30 minutes, and typically up to 60 minutes.
[0059] The surface postcrosslinked polymer particles can then be classified again and excessively small and / or excessively large polymer particles removed and recycled into the process.
[0060] To further improve the properties, the surface postcrosslinked polymer particles can be coated or remoisturized.
[0061] The remoistening is preferably carried out at 30-80°C, more preferably at 35-70°C, most preferably at 40-60°C. At too low a temperature the superabsorbent polymer particles tend to form agglomerates, at high temperatures the water has already evaporated visibly. The amount of water used for the remoistening is preferably 1-10% by weight, more preferably 2-8% by weight, most preferably 3-5% by weight. Remoistening increases the mechanical stability of the polymer particles and reduces their tendency to become electrostatically charged.
[0062] Suitable coatings for improving the free swell rate and saline flow conductivity (SFC) are, for example, inorganic inert substances, such as water-insoluble metal salts, organic polymers, cationic polymers, and divalent or polyvalent metal cations. Suitable coatings for binding dust are, for example, polyols. Suitable coatings for suppressing the undesirable caking tendency of polymer particles are, for example, fumed silica, such as Aerosil® 200, or precipitated silica, such as Sipernat® D17, and surfactants, such as Span® 20.
[0063] The present invention further provides hygiene articles comprising superabsorbent polymer particles prepared by the method of the present invention. EXAMPLES
[0064] Preparation of superabsorbent polymer particles Example 1 An acrylic acid / sodium acrylate solution was prepared by successively mixing deionized water, 48 wt.% sodium hydroxide solution and acrylic acid, with a degree of neutralization corresponding to 72.4 mol.%. The solids content of the monomer solution was 40.0 wt.%.
[0065] The monomer solution was further cooled. Then, 3-tuply ethoxylated glycerol triacrylate was added into the monomer solution as a crosslinking agent. The amount of crosslinking agent was 1.43 kg per ton of monomer solution.
[0066] Free radical polymerization was initiated by adding 1.31 kg of 0.25 wt% hydrogen peroxide in water, 3.00 kg of 30 wt% sodium peroxodisulfate in water, and 0.98 kg of 1 wt% ascorbic acid in water (each based on 1 ton of monomer solution). The peroxides were added to the monomer solution.
[0067] The throughput of the monomer solution was 21 t / h. The temperature of the monomer solution was 26° C. when it was fed.
[0068] The components (monomer solution and ascorbic acid solution) were added to 6.3 ml 3 The mixture was continuously metered into a continuous kneader reactor (LIST AG, Arisdorf, Switzerland) having a capacity of 10 ...
[0069] Between the crosslinker and peroxide addition points, the monomer solution was inerted with nitrogen.
[0070] After about 50% of the residence time in the polymerization reactor, fines (1270 kg / h) obtained from the production process by grinding and sieving were further metered into the reactor. The residence time of the reaction mixture in the reactor was 15 min.
[0071] The resulting polymer gel was placed on a belt dryer where an air / gas mixture was continuously flowed around the polymer gel to dry it.
[0072] The dried polymer gel was milled by a two-stage roll mill (model WMC152; Neuhaus Neotec Maschinen und Anlagenbau GmbH; Ganderkesee; Germany). The length of the rolls was 1,500 mm and the diameter was 250 mm. The gap of the upper roll was in the range of 0.3–0.5 mm. The tip speed of the upper roll was in the range of 5.8–8.1 m / s. The gap of the lower roll was in the range of 0.1–0.2 mm. The tip speed of the lower roll was in the range of 7.0–10.0 m / s. The temperature of the feed was 40–60 °C and the moisture content was 1–3 wt.%. The feed rate was 23.9% (DCS reading corresponds to approximately 2,500 kg / h).
[0073] The roll deflection was about 19.1% (100% corresponds to the maximum possible deflection of an unclamped roll) and the power consumption of the roll was about 28.8A.
[0074] The ground polymer was sieved into a particle size fraction of 150-850 μm.
[0075] Roll mill cleaning Example 2 The roll mill of Example 1 was cleaned according to the first embodiment of the present invention. The deflection setting was 21.0%. The power consumption setting was 31.0 A. Both conditions must be met to start the cleaning procedure.
[0076] If the deflection and power consumption were above the set values for 2.0 seconds, the feed rate was reduced in stages, with the feed rate reduced by 2.0% per stage (8.3% based on the feed rate before cleaning of the roll mill), and the time between two stages was 10.0 seconds.
[0077] The minimum feed rate was 10% (based on the feed rate before cleaning of the roll mill: 41.8%).
[0078] When the deflection and power consumption remained below the set values for 3 seconds, the feed rate was increased stepwise to 23.9%, with the feed rate increasing by 0.5% per step (2.1% based on the feed rate before cleaning of the roll mill). The time between two steps was 10.0 seconds.
Claims
1. 1. A method for producing superabsorbent polymer particles, comprising: a) partially neutralized acrylic acid, b) at least one crosslinker, and c) at least one initiator polymerizing a monomer solution comprising: drying the resulting polymer gel; A process for grinding the dried polymer gel with a roll mill, the rolls of the roll mill being configured to perform the following steps: i) determining the roll deflection and / or the power consumption of the roll mill; ii) reducing the feed rate to the roll mill or stopping the feed to the roll mill if the deflection and / or power consumption increases above a set value; iii) optionally increasing the gap width between the rolls of the roll mill; iv) operating the roll mill at a reduced feed rate or with the feed stopped; v) optionally reducing the gap width between the rolls of the roll mill; vi) optionally operating the roll mill at a reduced gap width until deflection and / or power consumption decrease below set values; vii) optionally increasing the gap width between the rolls of the roll mill to the gap width prior to step ii); and viii) increasing the feed rate to the roll mill to the rate prior to step ii) or resuming feed to the roll mill. and if in step ii) the supply to the roll mill is stopped and in step iii) the gap width between the rolls of the roll mill is increased, then in step v) the gap width between the rolls of the roll mill must be reduced; classifying the resulting polymer particles; A method comprising:
2. The rolls of the roll mill are i) determining the roll deflection and / or the power consumption of the roll mill; ii) reducing the feed rate to the roll mill if the deflection and / or power consumption increases above a set value; iv) operating the roll mill at a reduced feed rate until the deflection and / or power consumption decreases below a set value; viii) increasing the feed rate to the roll mill to the rate prior to step ii). The method of claim 1, wherein the surface is cleaned by
3. 3. The method according to claim 2, wherein the feed rate to the roll mill in step ii) is gradually reduced and / or the feed rate to the roll mill in step viii) is gradually increased.
4. 4. The method according to claim 2 or 3, wherein the feed rate to the roll mill in step ii) is reduced stepwise by 2 to 20% per step based on the feed rate before step ii).
5. 5. The method according to claim 2, wherein the feed to the roll mill in step iv) is at least 25% based on the feed before step ii).
6. The method according to any one of claims 2 to 5, wherein the feed rate to the roll mill in step viii) is increased stepwise by 0.5 to 10% per step based on the feed rate before step ii).
7. The rolls of the roll mill are i) determining the roll deflection and / or the power consumption of the roll mill; ii) stopping the feed to the roll mill if the deflection and / or power consumption increases above a set value; iv) stopping the feed and running the roll mill; v) reducing the gap width between the rolls of the roll mill; vi) operating the roll mill at a reduced gap width until the deflection and / or power consumption decreases below a set value; vii) increasing the gap width between the rolls of the roll mill to the gap width before step ii); and viii) restarting the feed rate to the roll mill The method of claim 1, wherein the surface is cleaned by
8. 8. The method of claim 7, wherein the roll mill is operated with feeding stopped for at least 2.0 minutes in step iv).
9. 9. The method according to claim 7 or 8, wherein the gap width between the rolls of the roll mill in step v) is reduced to less than 0.02 mm.
10. The rolls of the roll mill are i) determining the roll deflection and / or the power consumption of the roll mill; ii) stopping the feed to the roll mill if the deflection and / or power consumption increases above a set value; iii) increasing the gap width between the rolls of the roll mill; iv) stopping the feed and running the roll mill; v) reducing the gap width between the rolls of the roll mill; vi) operating the roll mill at a reduced gap width until the deflection and / or power consumption decreases below a set value; vii) increasing the gap width between the rolls of the roll mill to the gap width before step ii); and viii) restarting the feed rate to the roll mill The method of claim 1, wherein the surface is cleaned by
11. 11. The method according to claim 10, wherein the gap width between the rolls of the roll mill in step iii) is increased to at least 2.0 mm.
12. 12. The method according to claim 10 or 11, wherein the roll mill is operated with the feed stopped for at least 2.0 minutes in step iv).
13. 13. The method according to any one of claims 10 to 12, wherein the gap width between the rolls of the roll mill in step v) is reduced to less than 0.02 mm.
14. 14. The method according to any one of claims 1 to 13, wherein the roll mill is a multi-stage roll mill.
15. A method for producing a hygiene article comprising superabsorbent polymer particles, comprising: Producing superabsorbent polymer particles by the method according to any one of claims 1 to 14; producing a hygiene article comprising said superabsorbent polymer particles; A method comprising:
Citation Information
Patent Citations
Method for operating upright grinder
JP1993329392A
Method of producing polyacrylic acid-based and / or polyacrylate-based water-absorbing resin
JP2013076073A