Manufacturing method of rare earth magnetic material

The described method enhances coercive force and residual magnetism in Nd-Fe-B magnetic materials by using a light rare earth diffusion source alloy, optimizing B and Fe content, and forming μ and δ phases, addressing the inefficiencies and cost issues of heavy rare earth element reliance.

JP7556668B2Active Publication Date: 2024-09-26YANTAI DONGXING MAGNETIC MATERIALS INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023076529
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-05-31
Filing Date
2023-05-08
Publication Date
2024-09-26
Estimated Expiration
2043-05-08

AI Technical Summary

Technical Problem

Existing methods for producing Nd-Fe-B magnetic materials face challenges in achieving high coercive force and residual magnetism while minimizing the use of expensive heavy rare earth elements, often leading to inefficiencies and increased costs.

Method used

A manufacturing method involving a diffusion source alloy with a specific chemical composition (R1 α M1 β B γ Fe 100-α-β-γ) is used, where R1 is Nd, Pr, or Ce, M1 is Al, Cu, or Ga, and the alloy is pulverized and applied to an R-Fe-B magnetic base material, followed by diffusion and aging treatments at controlled temperatures and times, optimizing the content of B and Fe to enhance diffusion efficiency and form μ and δ phases.

Benefits of technology

This method significantly improves coercive force and reduces residual magnetism, allowing for cost-effective mass production of magnetic materials with enhanced magnetic properties by utilizing light rare earth elements effectively.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007556668000005
    Figure 0007556668000005
  • Figure 0007556668000006
    Figure 0007556668000006
Patent Text Reader

Abstract

To provide a rare earth magnetic material with high magnetic properties while using a light rare earth element as a diffusion source without using a heavy rare earth element, and a manufacturing method thereof.SOLUTION: An R-Fe-B system magnetic material containing a main phase, a grain boundary phase and a rare earth rich phase, where the grain boundary phase includes a μ phase and a δ phase, the μ phase has a chemical formula in mass percentage of Rx1Fe100-x1-X2MX2, 58≤x1≤61, 0.3≤x2≤3.5, and the δ phase has a chemical formula in mass percentage of Ry1Fe100-y1-y2My2, 50≤y1≤60, 4≤y2≤16, the R is at least one of Nd, Pr, Ce and La, and the M is at least one of Al, Cu and Ga.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention belongs to the technical field of rare earth magnetic materials, and in particular to light rare earth magnetic materials that can increase the coercive force without using heavy rare earth elements. Manufacturing method Regarding. [Background technology]

[0002] Nd-Fe-B sintered permanent magnets are widely used in the fields of electronic information, medical equipment, new energy vehicles, home appliances, robots, etc. Through research over the past few decades, the performance of Nd-Fe-B magnetic materials has made remarkable progress. In particular, diffusion technology is an excellent technology that can drastically reduce the amount of heavy rare earth elements used while maintaining coercivity performance.

[0003] In this diffusion technique, the heavy rare earth elements Dy and Tb are usually applied (added) to the surface of the Nd-Fe-B sintered permanent magnetic body, which is the base material. However, this method has the problem that the heavy rare earth elements Dy and Tb easily penetrate into the grain boundaries in large quantities, which reduces the remanence of the magnetic body and wastes the heavy rare earth elements. Another method is the grain boundary diffusion method, which uses heat treatment to cause the diffusion source to penetrate into the magnetic body from the grain boundaries and increase the coercive force. This method has attracted widespread attention because it can significantly improve the coercive force of the magnetic body while reducing the amount of heavy rare earth elements used, and is low cost. However, with the recent rise in the price of heavy rare earth elements, it is difficult to solve the high cost problem with the method using Dy and Tb as the diffusion source. The diffusion technique of heavy rare earth elements can effectively reduce the manufacturing cost of magnetic bodies while improving magnetic properties, so the development of the diffusion technique of heavy rare earth elements is particularly important for the manufacturing of Nd-Fe-B sintered permanent magnetic bodies.

[0004] For example, Chinese Patent Publication No. CN106298219B describes a method for manufacturing an RTB rare earth permanent magnet, which includes: a) using RL as a diffusion source; u RH V Fe 100-u-v-w-z B w M za) preparing a rare earth alloy, wherein RL is at least one of Pr and Nd, RH is at least one of Dy, Tb, and Ho, and M is at least one of Co, Nb, Cu, Al, Ga, Zr, and Ti, the rare earth alloy having a tetragonal main phase structure of R-Fe-B, 0≦u≦10, 35≦v≦70, 0.5≦w≦5, and 0≦z≦5, where u, v, w, and z are mass percents of each element; and b) RL u RH V Fe 100-u-v-w-z B w M z The invention discloses the following: a rare earth alloy is pulverized to prepare an alloy powder; c) the alloy powder and an RTB magnetic body are put into a rotary diffusion device to undergo thermal diffusion treatment, the diffusion temperature being 750-950°C and the diffusion time being 4-72 hours; d) aging treatment is performed, in which an auxiliary substance having a dispersing or buffering effect is added into the rotary diffusion device, the auxiliary substance being one or more of an iron base material and a titanium base material, or one or more of alumina and zirconia, the particle size of the auxiliary substance being less than 10 mm; and an anti-adhesion powder may be further added into the rotary diffusion device, the anti-adhesion powder being one or more of alumina, zirconia, dysprosium oxide, terbium oxide, dysprosium fluoride, and terbium fluoride, the particle size of the anti-adhesion powder being less than 100 μm. The diffusion source alloy used in the above invention is RL u RH V Fe 100-u-v-w-z B w M z It is a rare earth alloy, containing not only light rare earth elements but also heavy rare earth elements. On the other hand, if the content of B in the diffusion source is too high, the melting point will increase, making it difficult to diffuse into the magnetic body. Even though the diffusion source contains valuable heavy rare earth elements, the increase in coercive force after diffusion is slight, and conversely, the residual magnetism is greatly reduced, making it difficult to say that ideal magnetic properties are achieved.

[0005] Furthermore, Chinese Patent Publication No. CN113764147A discloses an invention for a method of improving the coercivity of an Nd-Fe-B magnetic material by mixing and diffusing a low melting point alloy, in which raw materials are mixed and arc-smelted according to the composition of a heavy rare earth-containing low melting point (Dy, Tb)-Al-Cu alloy and a high rare earth-rich low melting point (Pr, Ce)-Ga-Cu alloy, and then powder is produced using a high-energy ball mill, a melt quenching method, and a planetary low-energy ball mill, which are mixed according to the ratio to refine a paste-like solution, which is then uniformly applied to the surface of an Nd-Fe-B magnetic material, and then primary and secondary aging treatments are performed in a nitrogen gas atmosphere and under a low magnetic field to produce an Nd-Fe-B magnetic material with high coercivity. The purpose of using the light rare earth element in the above invention is to increase the diffusion depth of the heavy rare earth element, but since the light rare earth element does not act to improve the coercive force, it is ultimately necessary to use the heavy rare earth element.

[0006] Furthermore, Chinese Patent Publication No. CN113851320A describes a method for producing an Nd-Fe-B magnetic material in which light rare earth is diffused into the grain boundaries of a light rare earth alloy, in which a light rare earth alloy diffusion source is applied to the surface of an Nd-Fe-B sintered magnetic material, a grain boundary diffusion treatment is performed, and an aging treatment is performed. The light rare earth alloy diffusion source contains Pr A Fe 100-A The composition of the light rare earth Nd-Fe-B sintered magnetic material is R x Fe y M a Ga b B c The invention disclosed is (I), in which R is one or more selected from La, Ce, Nd, and Pr, M is one or more selected from Cu, Al, Co, and Zr, x: 28 to 33 wt%, y: 60 to 70 wt%, a: 0 to 0.6 wt%, b: 0.1 to 0.8 wt%, and c: 0.9 to 0.98 wt%. The diffusion source Pr in the above invention A Fe 100-A In the case of a magnetic material having a high iron content, a large amount of iron magnetic phase is formed after diffusion, and although the coercive force of the magnetic material increases, the remanence decreases significantly, and an improvement in the overall magnetic properties cannot be achieved.

[0007] An analysis of the above-mentioned conventional technologies reveals that there are problems in that (1) heavy rare earth elements are not used as a diffusion method into the crystal grain boundaries, and (2) the magnetic properties of Nd-Fe-B magnetic bodies in which light rare earth elements are diffused are not significantly improved. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Chinese patent CN106298219B publication [Patent Document 2] Chinese patent CN113764147A publication [Patent Document 3] Chinese patent CN113851320A publication DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]

[0009] The present invention aims to solve the problems associated with the above-mentioned conventional techniques and to provide a rare earth magnetic material having high magnetic properties while using a light rare earth element as a diffusion source without using a heavy rare earth element, and a method for producing the same. [Means for solving the problem]

[0010] The present invention is a method for producing a rare earth magnetic material, comprising the steps of: (Step 1) The chemical formula expressed in mass percentage is R1 α M1 β B γ Fe 100-α-β-γ preparing a diffusion source alloy, 10≦α≦80, 15≦β≦90, 0.1≦γ≦3, R1 is at least one of Nd, Pr, Ce, and La; The M1 is at least one of Al, Cu, and Ga, pulverizing the diffusion source alloy to prepare a diffusion source alloy powder; (Step 2) The chemical formula expressed in mass percentage is R2 a M2 b B cFe 100-a-b-c We created an R-Fe-B magnetic base material. 27≦a≦33, 1≦b≦4, 0.8≦c≦1.2, R2 is at least one of Nd and Pr; The M2 is at least one of Al, Cu, Ga, Ti, Zr, and Co; (Step 3) Coating the surface of the R-Fe-B magnetic base material with the diffusion source alloy powder, and performing a diffusion treatment and an aging treatment to obtain the R-Fe-B magnetic material; The diffusion treatment is performed at a temperature of 800 to 910°C for a diffusion time of 6 to 30 hours. The aging treatment is performed in two steps, with a first aging treatment temperature of 700 to 850°C for a first aging treatment time of 2 to 10 hours, a second aging treatment temperature of 450 to 600°C for a second aging treatment time of 3 to 10 hours, The (step 1) and the (step 2) may be performed simultaneously or in reverse order.

[0011] In one embodiment, The R-Fe-B magnetic base material is prepared by mixing a thin piece of the base alloy with a lubricant, subjecting the mixture to hydrogenation treatment, and pulverizing the mixture by a jet mill to prepare a base alloy powder. The diffusion source alloy powder is prepared by spray milling, amorphous alloy ribbon milling or ingot milling; The diffusion source alloy is obtained through a hydrogen absorption treatment and a dehydrogenation treatment, the hydrogen absorption temperature being 50 to 200°C and the dehydrogenation temperature being 450 to 550°C. The average particle size of the base alloy powder is 2 to 5 μm; The average particle size of the diffusion source alloy powder is 3 to 60 μm, The coating method of the diffusion source alloy powder is any one of magnetron sputtering coating, vapor deposition coating, and cover coating; The sintering temperature for producing the R-Fe-B magnetic base material is 980 to 1060°C, and the sintering time is 6 to 15 hours. It is characterized by: Effect of the Invention

[0012] The present invention has the following advantageous effects compared to the prior art. (1) Diffusion source alloy R1 α M1 β B γ Fe 100-α-β-γ Since the content of high melting point element B contained in the magnetic material is reduced, and the magnetic material contains no heavy rare earth elements but a large amount of light rare earth elements, the diffusion efficiency is increased and the light rare earth elements are easily diffused into the magnetic material. By diffusing the light rare earth elements into the magnetic material, more light rare earth layers and crystal grain boundary structures are formed, and the coercive force of the rare earth magnetic material, particularly with a thickness of about 3 to 8 mm, can be effectively increased.

[0013] (2) Diffusion source alloy R1 α M1 β Bγ Fe 100-α-β-γ By reducing the content of B in the material, it is possible to reduce the oxidation problem during the diffusion process and to increase the utilization rate of the rare earth elements during the diffusion process.

[0014] (3) Diffusion source alloy R1 α M1 β B γ Fe 100-α-β-γ By adjusting the contents of B and Fe contained in the magnetic material, a main phase in which the light rare earth elements are diffused is formed, which makes it possible to suppress a decrease in the remanence of the magnetic material, and by forming a μ phase and a δ phase with Al, Ga, and Cu in the magnetic material, the coercivity of the magnetic material can be increased.

[0015] (4) Diffusion source alloy R1 α M1 β B γ Fe 100-α-β-γ By adjusting the content of B and Fe contained in the material (the total weight ratio of B and Fe is up to 20%), the cost of the diffusion source can be significantly reduced, and the manufacturing cost of the magnetic material as a whole can be reduced.

[0016] (5) Diffusion source alloy R1 α M1 β B γ Fe 100-α-β-γ can be mass-produced, and after the diffusion source alloy powder is created, it can be applied to the surface of the magnetic base material by a coating method, making it possible to achieve nearly 100% utilization of the diffusion source. In addition, since it does not use heavy rare earth elements, it is possible to provide a large amount of inexpensive diffusion sources for multiple lots of magnetic materials, reducing manufacturing costs and effectively increasing the magnetic energy product of the magnetic materials.

[0017] As described above, according to the present invention, by optimally combining a diffusion source made of a light rare earth element with a magnetic base material whose components have been adjusted to correspond thereto, it is possible to significantly improve the coercive force while minimizing the decrease in remanence. [Brief description of the drawings]

[0018] [Figure 1]Electron microscope photograph of the magnetic material according to Example 10 of the present invention [Diagram 2] Electron microscope photograph of the magnetic material according to Comparative Example 10 DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The rare earth magnetic material and the manufacturing method thereof according to the present invention will be described in detail below. The following examples are used only to interpret the present invention and are not intended to limit the configuration of the present invention.

[0020] As the rare earth magnetic material according to the present invention, Examples 1 to 16 were prepared. The basic manufacturing method of each Example is almost the same, and the differences between each Example are the magnetic material dimensions, the composition of the diffusion source alloy, the temperature and time of the diffusion treatment and aging treatment, and the composition of the magnetic material base material before the diffusion treatment.

[0021] (Creating a diffusion source) The alloy components serving as the diffusion source according to Examples 1 to 16 were prepared. The alloy components and contents (mass%) of each diffusion source according to each Example are as shown in Table 1. The alloy components serving as the diffusion source were put into a vacuum smelting furnace and smelted, then poured into a mold to form diffusion source alloy flakes, and cooled to 50°C. The diffusion source alloy flakes had an average thickness of 0.25 to 1 mm, and the contents of C and O in the diffusion source alloy flakes were 200 ppm or less, and the content of N was 50 ppm or less. The diffusion source alloy flakes were subjected to hydrogen adsorption treatment and dehydrogenation treatment. The hydrogen adsorption temperature was 50 to 200°C, and the dehydrogenation temperature was 450 to 550°C. The diffusion source was then subjected to aging treatment. The aging treatment temperature was 350 to 600°C. The diffusion source alloy flakes after the aging treatment were pulverized to prepare diffusion source alloy powder with an average particle size of 3.0 to 60 μm. The pulverization process can be carried out by spray milling, amorphous melt spun or ingot milling.

[0022] (Creating rare earth magnetic base material) Alloy components for the R-Fe-B magnetic base material according to Examples 1 to 16 were prepared. The specific alloy components and contents (mass%) of each example are as shown in Table 2. The alloy components for the base material were put into a vacuum smelting furnace and smelted, then poured into a mold to form base alloy flakes, and cooled to 50°C. The average thickness of the base alloy flakes was 0.25 mm, and the contents of C and O in the base alloy flakes were 200 ppm or less, and the content of N was 50 ppm or less. The base alloy flakes were subjected to hydrogen adsorption and dehydrogenation treatments. The hydrogen adsorption temperature was 50 to 200°C, and the dehydrogenation temperature was 450 to 550°C.

[0023] The base alloy flakes after hydrogen absorption and dehydrogenation treatment were mixed with a lubricant and subjected to hydrogenation treatment. The mixture was then pulverized in a jet mill using argon gas as the polishing gas to produce base alloy powder with an average particle size of 2 to 5 μm.

[0024] The base alloy powder was put into an automatic press and subjected to magnetic field oriented press molding to form a block base, which was then put into a sintering furnace and sintered at a sintering temperature of 980-1060°C for a sintering time of 6-15 hours, and then machined to the specified size shown in Table 1 to create an R-Fe-B magnetic base material. The magnetic properties of the R-Fe-B magnetic base material before diffusion treatment are shown in Table 2.

[0025] (Diffusion processing) The diffusion source alloy powder was made into a slurry, and the diffusion source alloy slurry was applied to the surface of the R-Fe-B magnetic base material by a coating method, and the diffusion treatment was performed. As shown in Table 1, the sintering temperature for the diffusion treatment in each example was 800-910°C, the diffusion time was 6-30 hours, and the aging treatment was performed in two separate steps, with the first aging treatment temperature being 700-850°C, the first aging treatment time being 2-10 hours, the second aging treatment temperature being 450-600°C, and the second aging treatment time being 3-10 hours. The coating method for the diffusion source alloy powder may be any one of magnetron sputtering coating, deposition coating, and coating coating. The diffusion source and the rare earth magnetic base material may be prepared simultaneously, or may be prepared in separate time series.

[0026] The magnetic properties of the R—Fe—B based magnetic materials obtained by the diffusion treatment according to Examples 1 to 16 were measured. The measurement results are shown in Table 1.

[0027] Table 1: Diffusion source components and magnetic properties after diffusion for each example JPEG0007556668000001.jpg21599

[0028] Table 2: Components and magnetic properties of the magnetic base material in each example JPEG0007556668000002.jpg14797

[0029] Fig. 1 is a photograph of the surface of the magnetic body according to Example 10, which is a representative example of each Example, taken by a ZEISS electron microscope, and shows the presence and location of the μ-phase and δ-phase in the grain boundary phase. Table 3 shows the results of component analysis in which the compositions of the μ-phase and δ-phase in Examples 1 to 16 were measured by the EDS method. Note that ZEISS electron microscope photographs of the magnetic bodies other than Example 10 are omitted, but they contain the μ-phase and δ-phase in the grain boundary phase as in Example 10.

[0030] The presence of the μ and δ phases enhances the diamagnetic coupling action in the crystal grain boundaries, and contributes to increasing the coercive force of the magnetic material.

[0031] Table 3: Composition of μ and δ phases in each example JPEG0007556668000003.jpg111110

[0032] (Creating a comparative example) For comparison with the above-mentioned Examples 1 to 16, corresponding Comparative Examples 1 to 16 were prepared. The difference between the Examples and Comparative Examples is that the Comparative Examples do not include B and Fe in the elements constituting the diffusion source alloy, and all other conditions were the same. In addition, the rare earth magnetic base materials before the diffusion treatment in Comparative Examples 1 to 16 were the same as those in the corresponding Examples 1 to 16. Details of Comparative Examples 1 to 16 are as shown in Table 3.

[0033] Table 4: Diffusion source components and magnetic properties after diffusion treatment in each comparative example JPEG0007556668000004.jpg17398

[0034] FIG. 2 is a photograph taken by a ZEISS electron microscope of the surface of the magnetic body according to Comparative Example 10 as a representative example of the comparative examples, and shows the presence and location of the μ phase in the grain boundary phase.

[0035] Hereinafter, the results of comparing the magnetic properties of each of the examples and the corresponding comparative examples shown in Tables 2 and 4 will be described. (Comparison between Example 1 and Comparative Example 1) Example 1 includes both μ and δ phases, and has a remanence Br=14.00 kGs and a coercivity Hcj=21.50 kOe, whereas Comparative Example 1 includes only δ phase, and has Br=13.60 kGs and Hcj=20.00 kOe. The remanence and coercivity of Example 1 are significantly superior to those of Comparative Example 1.

[0036] (Comparison between Example 2 and Comparative Example 2) Example 2 includes both μ and δ phases, and has a remanence Br=14.00 kGs and a coercivity Hcj=23.00 kOe, whereas Comparative Example 2 includes only δ phase, and has Br=13.50 kGs and Hcj=21.00 kOe. The remanence and coercivity of Example 2 are significantly superior to those of Comparative Example 2.

[0037] (Comparison between Example 3 and Comparative Example 3) Example 3 includes both μ and δ phases, and has a remanence Br=13.20 kGs and a coercivity Hcj=24.50 kOe, whereas Comparative Example 3 includes only δ phase, and has Br=12.90 kGs and Hcj=22.50 kOe. The remanence and coercivity of Example 3 are significantly superior to those of Comparative Example 3.

[0038] (Comparison between Example 4 and Comparative Example 4) After the diffusion, Example 4 contained both μ and δ phases, and had a remanence Br=13.30 kGs and a coercivity Hcj=25.00 kOe, whereas Comparative Example 4 contained only δ phase, and had Br=12.80 kGs and Hcj=22.00 kOe. The remanence and coercivity of Example 4 are significantly superior to those of Comparative Example 4.

[0039] (Comparison between Example 5 and Comparative Example 5) Example 5 contains both μ and δ phases, and has a remanence Br=13.25 kGs and a coercivity Hcj=24.00 kOe, whereas Comparative Example 5 does not contain either μ or δ phases, and has Br=12.70 kGs and Hcj=22.00 kOe. The remanence and coercivity of Example 5 are significantly superior to those of Comparative Example 5.

[0040] (Comparison between Example 6 and Comparative Example 6) Example 6 contains both μ and δ phases, and has a remanence Br=13.35 kGs and a coercivity Hcj=25.00 kOe, whereas Comparative Example 6 does not contain either μ or δ phases, and has Br=13.00 kGs and Hcj=21.00 kOe. The remanence and coercivity of Example 6 are significantly superior to those of Comparative Example 6.

[0041] (Comparison between Example 7 and Comparative Example 7) Example 7 contains both μ and δ phases, and has a remanence Br=13.47 kGs and a coercivity Hcj=24.50 kOe, whereas Comparative Example 7 contains only δ phase, and has Br=13.10 kGs and Hcj=21.50 kOe. The remanence and coercivity of Example 7 are significantly superior to those of Comparative Example 7.

[0042] (Comparison between Example 8 and Comparative Example 8) Example 8 contains both μ and δ phases, and has a remanence Br=13.50 kGs and a coercivity Hcj=24.00 kOe, whereas Comparative Example 8 contains only δ phase, and has Br=13.00 kGs and Hcj=20.50 kOe. The remanence and coercivity of Example 8 are significantly superior to those of Comparative Example 8.

[0043] (Comparison between Example 9 and Comparative Example 9) Example 9 contains both μ and δ phases, and has a remanence Br=12.90 kGs and a coercivity Hcj=25.50 kOe, whereas Comparative Example 9 contains only δ phase, and has Br=12.50 kGs and Hcj=23.50 kOe. The remanence and coercivity of Example 9 are significantly superior to those of Comparative Example 9.

[0044] (Comparison between Example 10 and Comparative Example 10) Example 10 contains both μ and δ phases, and has a remanence Br=13.45 kGs and a coercivity Hcj=25.50 kOe, whereas Comparative Example 10 contains only δ phase, and has Br=13.00 kGs and Hcj=23.50 kOe. The remanence and coercivity of Example 10 are significantly superior to those of Comparative Example 10.

[0045] (Comparison between Example 11 and Comparative Example 11) Example 11 contains both μ and δ phases, and has a remanence Br=13.80 kGs and a coercivity Hcj=23.00 kOe, whereas Comparative Example 11 contains only δ phase, and has Br=13.40 kGs and Hcj=21.00 kOe. The remanence and coercivity of Example 11 are significantly superior to those of Comparative Example 11.

[0046] (Comparison between Example 12 and Comparative Example 12) Example 12 contains both μ and δ phases, and has a remanence Br of 13.70 kGs and a coercivity Hcj of 24.00 kOe, whereas Comparative Example 12 does not contain either μ or δ phases, and has a Br of 13.20 kGs and a Hcj of 22.00 kOe. The remanence and coercivity of Example 12 are significantly superior to those of Comparative Example 12.

[0047] (Comparison between Example 13 and Comparative Example 13) Example 13 contains both μ and δ phases, and has a remanence Br=12.30 kGs and a coercivity Hcj=25.00 kOe, whereas Comparative Example 13 after diffusion contains only δ phase, and has Br=12.00 kGs and Hcj=23.00 kOe. The remanence and coercivity of Example 13 are significantly superior to those of Comparative Example 13.

[0048] (Comparison between Example 14 and Comparative Example 14) Example 14 contains both μ and δ phases, and has a remanence Br of 12.50 kGs and a coercivity Hcj of 24.00 kOe, whereas Comparative Example 14 does not contain either μ or δ phases, and has a Br of 12.30 kGs and a Hcj of 22.00 kOe. The remanence and coercivity of Example 14 are significantly superior to those of Comparative Example 14.

[0049] (Comparison between Example 15 and Comparative Example 15) Example 15 contains both μ and δ phases, and has a remanence Br of 13.35 kGs and a coercivity Hcj of 23.00 kOe, whereas Comparative Example 15 does not contain either μ or δ phases, and has a Br of 12.90 kGs and a Hcj of 20.50 kOe. The remanence and coercivity of Example 15 are significantly superior to those of Comparative Example 15.

[0050] (Comparison between Example 16 and Comparative Example 16) Example 16 contains both μ and δ phases, and has a remanence Br=13.25 kGs and a coercivity Hcj=25.50 kOe, whereas Comparative Example 16 contains only δ phase, and has Br=12.80 kGs and Hcj=23.5 kOe. The remanence and coercivity of Example 16 are significantly superior to those of Comparative Example 16.

[0051] As described above, the light rare earth magnetic material is treated with the light rare earth diffusion source alloy R α M β B γ Fe 100-α-β-γ All of the examples according to the present invention in which the magnetic flux was diffused showed clear improvements in magneto-magnetic properties compared to the corresponding comparative examples.

Claims

1. A method for producing a rare earth magnetic material, comprising the steps of: (Step 1) The chemical formula expressed in mass percentage is R1 α M1 β B γ Fe 100-α-β-γ preparing a diffusion source alloy, 10≦α≦80, 15≦β≦90, 0.1≦γ≦3, R1 is at least one of Nd, Pr, Ce, and La; The M1 is at least one of Al, Cu, and Ga, pulverizing the diffusion source alloy to prepare a diffusion source alloy powder; (Step 2) The chemical formula expressed in mass percentage is R2 a M2 b B c Fe 100-a-b-c An R—Fe—B based magnetic base material is prepared, 27≦a≦33, 1≦b≦4, 0.8≦c≦1.2, R2 is at least one of Nd and Pr, The M2 is at least one of Al, Cu, Ga, Ti, Zr, and Co; (Step 3) Coating the surface of the R-Fe-B magnetic base material with the diffusion source alloy powder, and performing a diffusion treatment and an aging treatment to obtain the R-Fe-B magnetic material, the diffusion treatment temperature is 800-910°C, the diffusion time is 6-30 hours, the aging treatment is performed in two steps, the first aging treatment temperature is 700-850°C, the first aging treatment time is 2-10 hours, the second aging treatment temperature is 450-600°C, and the second aging treatment time is 3-10 hours, The steps 1 and 2 may be performed simultaneously or in reverse order.

2. A method for producing a rare earth magnetic material comprising the steps of:

2. The R-Fe-B magnetic base material is prepared by mixing a thin piece of the base alloy with a lubricant, subjecting the mixture to hydrogenation treatment, and pulverizing the mixture by a jet mill to prepare a base alloy powder.

2. The method for producing a rare earth magnetic material according to claim 1.

3. The diffusion source alloy powder is prepared by spray milling, amorphous alloy ribbon milling or ingot milling; 3. The method for producing a rare earth magnetic material according to claim 1 or 2.

4. The diffusion source alloy is obtained through a hydrogen absorption treatment and a dehydrogenation treatment, and the hydrogen absorption temperature is 50 to 200°C and the dehydrogenation temperature is 450 to 550°C.

3. The method for producing a rare earth magnetic material according to claim 1 or 2.

5. The average particle size of the base alloy powder is 2 to 5 μm.

3. The method for producing a rare earth magnetic material according to claim 2.

6. The average particle size of the diffusion source alloy powder is 3 to 60 μm.

3. The method for producing a rare earth magnetic material according to claim 1 or 2.

7. The coating method of the diffusion source alloy powder is any one of magnetron sputtering coating, vapor deposition coating, and cladding coating; 3. The method for producing a rare earth magnetic material according to claim 1 or 2.

8. The sintering temperature for producing the R-Fe-B magnetic base material is 980 to 1060°C, and the sintering time is 6 to 15 hours.

3. The method for producing a rare earth magnetic material according to claim 1 or 2.

Citation Information

Patent Citations

  • A method and apparatus for preparing R-T-B rare earth permanent magnets

    CN106298219B

  • Method for improving coercive force of neodymium-iron-boron magnet through low-melting-point mixed diffusion

    CN113764147A

  • Preparation method of light rare earth alloy grain boundary diffusion enhanced heavy rare earth-free sintered neodymium-iron-boron magnet

    CN113851320A

  • Method of manufacturing r-t-b based sintered magnet

    JP2018029108A

  • METHOD FOR PRODUCING SINTERED Nd-Fe-B MAGNET

    JP2022031605A