Film formation method

A two-step application of top coat materials with varying properties addresses the swelling and staining issues of water-based coatings on elastic films, enhancing durability and appearance.

JP7556704B2Active Publication Date: 2024-09-26BEKKU KK
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2020102139
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-06-18
Filing Date
2020-06-12
Publication Date
2024-09-26
Estimated Expiration
2040-06-12

AI Technical Summary

Technical Problem

Water-based top coat materials applied on elastic films tend to swell and become stained, compromising their aesthetic appearance and durability.

Method used

A film forming method involving two specific types of top coat materials, where the first top coat material has a higher pigment volume concentration and greater elongation rate than the second, applied sequentially to an elastic film to enhance cracking resistance, blistering resistance, and stain resistance.

Benefits of technology

The method results in a film with improved cracking resistance, blistering resistance, and stain resistance, maintaining aesthetic integrity under varying temperatures and environmental conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007556704000002
    Figure 0007556704000002
  • Figure 0007556704000001
    Figure 0007556704000001
Patent Text Reader

Abstract

To provide a coated film formation method which can be applied to an elastic film and can exhibit excellent performance in crack resistance, swelling resistance and stain resistance.SOLUTION: A coated film formation method use a first top coating material and a second top coating material as top coating materials. The first top coating material and the second top coating material each contains an aqueous resin and a coloring pigment, its pigment volume concentration is 1-50%, the pigment volume concentration of the first top coating material is larger than the pigment volume concentration of the second top coating material, the first top coating material forms a coated film having an elongation percentage at -10°C of 20% or more, and the second top coating material forms a coated film having an elongation percentage at -10°C smaller than the elongation percentage at -10°C of the first top coating material.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a novel method for forming a coating. [Background technology]

[0002] Among the substrates constituting the framework of buildings, civil engineering structures, and the like, cement-based substrates such as concrete and mortar may crack over time due to the shrinkage of the substrate itself, the load on the substrate, and the like. In addition, in building materials such as lightweight concrete boards, aerated concrete boards, and siding boards, the joints between the building materials have the property of being easily displaced by changes in temperature, humidity, and the like. For a substrate having such a substrate, it is effective to form an elastic coating. The elastic coating can follow the displacement of the substrate, and can also exert the effect of preventing the intrusion of water, carbon dioxide, and the like into the substrate, and the effect of suppressing the neutralization of the substrate. Such an elastic coating can be formed by various elastic coating materials. Representative elastic coating materials include, for example, waterproof synthetic resin emulsion-based multilayer finishing coating materials (waterproof multilayer coating material E) specified in JIS A6909.

[0003] On the other hand, the topcoat materials used for buildings and civil engineering structures are being converted from solvent-based materials using organic solvents to water-based materials using water as the solvent. This is being done for the purpose of reducing the health damage to painting workers and residents, and reducing air pollution. The water-based topcoat materials are also being developed for the elastic coating materials mentioned above. For example, JP-A-11-35876 describes a water-based topcoat material that can be applied to elastic coating materials, taking into account crack resistance, etc. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 11-35846 Summary of the Invention [Problem to be solved by the invention]

[0005] However, as in the above patent document, when a water-based topcoat material is laminated on an elastic coating, while it exhibits conformity to the elastic coating, the topcoat material film may blister, become dirty, etc., and the original aesthetic appearance may be impaired.

[0006] The present invention has been made in consideration of the above-mentioned problems, and has an object to provide a coating formation method that can be applied to an elastic coating and can exhibit excellent performance in terms of crack resistance, blister resistance, contamination resistance, etc. [Means for solving the problem]

[0007] As a result of intensive research into achieving the above-mentioned object, the inventor came up with the idea of ​​applying two specific types of topcoat material to an elastic coating to form a topcoat material film, and thus completed the present invention.

[0008] That is, the present invention has the following features. 1. For elastic membranes The first and second topcoats are applied in order. A coating method for forming a topcoat coating by coating 、 Above first topcoat material contains an aqueous resin and a color pigment, and the pigment volume concentration is 4 to 25%, The second topcoat material contains a water-based resin and a coloring pigment, and the pigment volume concentration is 3 to 20%. and The pigment volume concentration of the first topcoat material is greater than the pigment volume concentration of the second topcoat material, The first topcoat material forms a coating with an elongation rate of 20% or more at -10°C. The second topcoat material forms a coating whose elongation rate at -10°C is smaller than the elongation rate at -10°C of the first topcoat material. A method for forming a coating comprising the steps of: 2. For elastic membranes Apply the first and second topcoats in order. A topcoat material set for forming a topcoat material film, The above-mentioned topcoat material set consists of a first topcoat material and a second topcoat material, Above first topcoat material contains an aqueous resin and a color pigment, and the pigment volume concentration is 4 to 25%, The second topcoat material contains a water-based resin and a coloring pigment, and the pigment volume concentration is 3 to 20%. and The pigment volume concentration of the first topcoat material is greater than the pigment volume concentration of the second topcoat material, The first topcoat material forms a coating with an elongation rate of 20% or more at -10°C. The second topcoat material forms a coating whose elongation rate at -10°C is smaller than the elongation rate at -10°C of the first topcoat material. A topcoat material set characterized by the above. Effect of the Invention

[0009] The present invention is a method for forming a coating that can be applied to an elastic coating, and can form a coating that exhibits excellent performance in terms of crack resistance, blister resistance, contamination resistance, and the like. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, an embodiment of the present invention will be described.

[0011] The present invention is a coating forming method for forming a coating by applying two specific topcoat materials (a first topcoat material and a second topcoat material) to an elastic coating.

[0012] <Substrate surface> In the present invention, the elastic coating provided on the base surface is the subject of painting. Examples of the base surface include exterior surfaces (e.g., outer walls, roofs, etc.) of buildings and civil engineering structures. Examples of the substrate constituting such a base surface include concrete, mortar, and plate-shaped substrates. Among these, examples of the plate-shaped substrate include cement boards, extrusion molding boards, slate boards, PC boards, ALC boards, fiber-reinforced cement boards, metal-based siding boards, ceramic-based siding boards, ceramic boards, calcium silicate boards, plastic boards, hard wood chip cement boards, PVC extrusion siding boards, and plywood. When the base surface is composed of a plurality of plate-shaped substrates, the joints between the plate-shaped substrates may be filled with joint materials such as sealants and dry joint materials.

[0013] The base surface may have an existing coating. Such an existing coating may be formed, for example, by one or more coating agents. Various coating agents may be used, such as colored or uncolored, or opaque or transparent, and examples of such coating agents include those containing one or more resins selected from vinyl acetate resin, alkyd resin, epoxy resin, acrylic resin, urethane resin, acrylic silicone resin, silicone resin, fluororesin, and the like. The existing coating may be a coating of one layer or two or more layers, and may be, for example, an elastic type, a hard type, or the like.

[0014] <Elastic coating> The elastic coating can be formed by applying an elastic coating material to the above-mentioned base surface. Examples of the elastic coating material include, for example, among architectural finishing coating materials specified in JIS A6909:2014, those that exhibit flexibility or waterproofness, architectural coating waterproof materials specified in JIS A6021:2011, etc. Specifically, examples of the elastic coating material include, for example, flexible exterior siliceous thin-applied finishing coating material (flexible exterior thin coating material Si), flexible exterior synthetic resin emulsion thin-applied finishing coating material (flexible exterior thin coating material E), waterproof exterior synthetic resin emulsion thin-applied finishing coating material (waterproof exterior thin coating material E), flexible polymer cement multilayer finishing coating material (flexible multilayer coating material CE), waterproof polymer cement multilayer finishing coating material (waterproof multilayer coating material CE), waterproof synthetic resin emulsion multilayer finishing coating material (waterproof multilayer coating material E), waterproof reactive hardening synthetic resin Examples of such coating materials include emulsion-based multi-layer finishing coating materials (waterproof multi-layer coating material RE), waterproof synthetic resin solution-based multi-layer finishing coating materials (waterproof multi-layer coating material RS), flexible synthetic resin emulsion-based renovation finishing coating materials (flexible renovation coating material E), flexible reaction-hardening synthetic resin emulsion-based renovation finishing coating materials (flexible renovation coating material RE), flexible polymer cement-based renovation finishing coating materials (flexible renovation coating material CE), acrylic rubber-based roof coating waterproof materials, urethane rubber-based roof coating waterproof materials, acrylic rubber-based exterior wall coating waterproof materials, and urethane rubber-based exterior wall coating preventative materials.

[0015] The method of applying the elastic covering material is not particularly limited, and a method suitable for each material can be adopted. Examples of application tools that can be used include a spray, roller, trowel, and brush. The amount of application of the elastic covering material is preferably 0.2 to 5 kg / m. 2 , more preferably 0.3 to 4 kg / m 2 When coating, the elastic coating material can be diluted as needed. Drying after coating of the elastic coating material can be performed at room temperature (preferably 0 to 50°C, more preferably 5 to 45°C), and can be performed with heat if necessary.

[0016] The elastic coating material can be applied directly to the substrate, or it can be applied after treating the substrate with a base coat or a base-conditioning coating material (e.g., sealer, primer, surfacer, filler, putty, etc.).

[0017] The elastic coating is preferably a single coating that forms a coating with an elongation rate of 20% or more at -10°C. Such an elastic coating can exhibit advantageous effects, for example, in terms of the ability to follow the displacement of the substrate and the prevention of the intrusion of water, carbon dioxide, etc. into the substrate. In the present invention, the elongation rate at -10°C is a value measured according to the method specified in the "elongation test" of JIS A6909:2014. The single coating of the elastic coating is subjected to the elongation test with a dry thickness of 1 mm.

[0018] <Top coat material> In the present invention, the first topcoat material and the second topcoat material are applied in order to the elastic coating to form a coating. The first topcoat material and the second topcoat material in the present invention are both so-called aqueous coating materials that contain aqueous resin as a resin component. The common points of such first topcoat material and second topcoat material (hereinafter, both are collectively referred to simply as "topcoat material") will be explained first.

[0019] As the aqueous resin in the topcoat material, a copolymer such as a hard monomer (hereinafter simply referred to as "hard monomer") having a homopolymer glass transition temperature of 50°C or higher and a soft monomer (hereinafter simply referred to as "soft monomer") having a homopolymer glass transition temperature of less than 50°C can be used.

[0020] Among the monomers constituting the aqueous resin, examples of hard monomers include aromatic monomers (s) (hereinafter also referred to as "(s) component"). Such (s) components act advantageously to improve physical properties such as crack resistance, blister resistance, and contamination resistance. It is believed that such effects are achieved by the action of improving the strength of the topcoat material coating. In the present invention, the monomer is a compound having a polymerizable unsaturated double bond. The glass transition temperature of the homopolymer can be measured by DSC (differential scanning calorimetry). The glass transition temperature is also referred to simply as "Tg" hereinafter.

[0021] Examples of the (s) component include styrene (Tg: 100°C), α-methylstyrene (Tg: 168°C), benzyl methacrylate (Tg: 54°C), and phenoxyethyl methacrylate (Tg: 54°C). These can be used alone or in combination of two or more. Among these, styrene is particularly suitable.

[0022] The aqueous resin in the topcoat material can contain, in addition to the (s) component, a (meth)acrylic acid alkyl ester (t) having a cyclic alkyl group (hereinafter also referred to as the "(t) component") and / or a (meth)acrylic acid alkyl ester (u) having a branched alkyl group (hereinafter also referred to as the "(u) component") as a hard monomer constituting the aqueous resin. In the present invention, by using an aqueous resin having such a (t) component and / or a (u) component as a constituent component, it is possible to obtain even more advantageous effects in terms of weather resistance, blister resistance, and contamination resistance. In addition, in the present invention, the acrylic acid alkyl ester and the methacrylic acid alkyl ester are collectively referred to as the (meth)acrylic acid alkyl ester.

[0023] Examples of the (t) component include cyclohexyl methacrylate (Tg: 83°C), isobornyl acrylate (Tg: 94°C), isobornyl methacrylate (Tg: 155°C), dicyclopentanyl acrylate (Tg: 120°C), dicyclopentanyl methacrylate (Tg: 175°C), dicyclopentenyl acrylate (Tg: 120°C), etc. These can be used alone or in combination of two or more. Among these, cyclohexyl methacrylate is particularly suitable.

[0024] Examples of the component (u) include tert-butyl methacrylate (Tg: 107°C), iso-butyl methacrylate (Tg: 53°C), and iso-propyl methacrylate (Tg: 81°C). These can be used alone or in combination of two or more. Among these, tert-butyl methacrylate is particularly preferred.

[0025] The monomers constituting the aqueous resin may include other hard monomers {hard monomers other than the above components (s), (t), and (u)} and / or soft monomers.

[0026] Examples of such monomers (other hard monomers and / or soft monomers) include (meth)acrylic acid alkyl esters other than those mentioned above, carboxyl group-containing monomers, amino group-containing monomers, pyridine-based monomers, hydroxyl group-containing monomers, nitrile group-containing monomers, amide group-containing monomers, epoxy group-containing monomers, carbonyl group-containing monomers, alkoxysilyl group-containing monomers, fluorine-containing monomers, ultraviolet absorbing group-containing monomers, photostable group-containing monomers, etc. These can be used alone or in combination of two or more.

[0027] Specific examples of other hard monomers include methyl methacrylate (Tg: 105° C.), ethyl methacrylate (Tg: 65° C.), acrylic acid (Tg: 106° C.), methacrylic acid (Tg: 185° C.), itaconic acid (Tg: 100° C.), maleic acid (Tg: 130° C.), 2-hydroxyethyl methacrylate (Tg: 55° C.), N,N-dimethylaminopropylacrylamide (Tg: 134° C.), acrylamide (Tg: 179°C), acrylonitrile (Tg: 125°C), γ-methacryloyloxypropyltrimethoxysilane (Tg: 70°C), 2-isopropenyl-2-oxazoline (Tg: 100°C), 2-[2'-hydroxy-5'-methacryloyloxyethylphenyl]-2H-benzotriazole (Tg: 100°C), 4-methacryloyloxy-1,2,2,6,6-pentamethylpiperidine (Tg: 130°C), etc. These can be used alone or in combination of two or more.

[0028] Specific examples of soft monomers include methyl acrylate (Tg: 8° C.), ethyl acrylate (Tg: −20° C.), propyl acrylate (Tg: 3° C.), propyl methacrylate (Tg: 35° C.), isopropyl acrylate (Tg: −3° C.), n-butyl acrylate (Tg: −54° C.), n-butyl methacrylate (Tg: 20° C.), isobutyl acrylate (Tg: −26° C.), tert-butyl acrylate (Tg: −20° C.), and ethyl acrylate (Tg: −20° C.). Amyl acrylate (Tg: 43°C), isoamyl acrylate (Tg: -45°C), 2-ethylhexyl acrylate (Tg: -70°C), 2-ethylhexyl methacrylate (Tg: -10°C), octyl acrylate (Tg: -65°C), iso-octyl methacrylate (Tg: -45°C), iso-octyl acrylate (Tg: -70°C), cyclohexyl acrylate (Tg: 15°C), lauryl acrylate Acrylate (Tg: 10°C), lauryl methacrylate (Tg: -65°C), stearyl acrylate (Tg: 35°C), hexadecyl acrylate (Tg: 35°C), hexadecyl methacrylate (Tg: 15°C), hexyl acrylate (Tg: -57°C), hexyl methacrylate (Tg: -5°C), tetradecyl acrylate (Tg: 24°C), tetradecyl methacrylate (Tg: -72°C), 2-hydroxyethyl acrylate (Tg: -10°C), lauryl methacrylate (Tg: -65°C), stearyl acrylate (Tg: 35°C), hexadecyl acrylate (Tg: -15°C), hexyl acrylate (Tg: -57°C), hexyl methacrylate (Tg: -5°C), tetradecyl acrylate (Tg: 24°C), tetradecyl methacrylate (Tg: -72°C), 2-hydroxyethyl acrylate (Tg: -10°C), lauryl meth ... hydroxyethyl acrylate (Tg: -15°C), 2-hydroxybutyl acrylate (Tg: -7°C), 2-hydroxybutyl methacrylate (Tg: 26°C), 2-methoxyethyl acrylate (Tg: -50°C), 4-hydroxybutyl acrylate (Tg: -80°C), N,N-diethylaminoethyl methacrylate (Tg: 20°C), N,N-dimethylaminoethyl acrylate (Tg: 18°C), N,N-dimethylaminoethyl methacrylate (Tg: 18°C), ethyl carbitol acrylate (Tg: -67°C), ethoxyethyl acrylate (Tg: -50°C), ethoxyethyl methacrylate (Tg: 15°C), ethoxydiethylene glycol acrylate (Tg: -70°C), tetrahydrofurfuryl acrylate (Tg: -12°C), phenoxyethyl acrylate (Tg: -22°C), benzyl acrylate (Tg: 6°C), pentyl acrylate (Tg: 22°C), pentyl methacrylate (Tg: -5°C), carboxyethyl acrylate (Tg: 37°C), methoxyethyl acrylate (Tg: -50°C), methoxy methacrylate (Tg: -16°C), vinyl acetate (Tg: 32°C), etc. can be used alone or in combination of two or more.

[0029] The aqueous resin can be produced, for example, by polymerizing a group of monomers containing the above-mentioned monomers. Examples of the form of the aqueous resin include water-soluble resins and water-dispersible resins, and water-dispersible resins (resin emulsions) are particularly preferred. The water-dispersible resin can be produced, for example, by one-stage or multi-stage (two-stage, three-stage or more) emulsion polymerization methods. These may have crosslinking reactivity and may be one-component or two-component.

[0030] The composition ratio of the aromatic monomer (s) in the aqueous resin is preferably 40% by weight or less, more preferably 1 to 38% by weight, and even more preferably 3 to 35% by weight, based on the total monomers constituting the aqueous resin. If the (s) component is in such a composition ratio, it is possible to improve the strength, crack resistance, and blister resistance of the topcoat material film while ensuring weather resistance, etc. In the present invention, "α to β" is synonymous with "α or more and β or less".

[0031] The composition ratio of the (t) component and the (u) component in the aqueous resin is preferably 2 to 60% by weight, more preferably 5 to 50% by weight, based on the total weight of the monomers constituting the aqueous resin. If the (t) component and the (u) component are in such a composition ratio, they act advantageously in terms of weather resistance, crack resistance, blister resistance, stain resistance, etc.

[0032] The Tg of the aqueous resin is preferably −30 to 60° C., more preferably −20 to 50° C. In the present invention, the types and ratios of the monomers can be selected so that the Tg of the aqueous resin satisfies such a value. The Tg of the aqueous resin is a value calculated by the FOX formula.

[0033] The topcoat material may contain one or more aqueous resins, and may be used by mixing two or more aqueous resins with different compositions. When two or more aqueous resins are included, it is desirable to adjust the type and ratio of the aqueous resins so as to satisfy the above conditions based on all aqueous resins. Specifically, when two or more aqueous resins are included, for example, an embodiment containing two or more aqueous resins with different monomer compositions, an embodiment containing two or more aqueous resins with different Tg, an embodiment containing two or more aqueous resins with different particle sizes, an embodiment containing two or more aqueous resins with different resin skeletons (e.g., acrylic resin, acrylic silicone resin, urethane resin, fluororesin, etc.), an embodiment containing two or more aqueous resins with different crosslinking forms (e.g., crosslinking reactive, non-crosslinking, etc.), an embodiment containing two or more aqueous resins with different polymerization methods (e.g., one-stage emulsion polymerization, multi-stage emulsion polymerization, etc.), an embodiment containing two or more aqueous resins with different molecular weights, an embodiment containing a water-dispersible resin and a water-soluble resin, etc.

[0034] The topcoat material in the present invention contains a color pigment. As the color pigment, for example, known inorganic color pigments, organic color pigments, etc. can be used. By appropriately using one or more of these color pigments, the topcoat material can be set to the desired color tone, and a topcoat material exhibiting a single color such as glossy synthetic resin emulsion paint (JIS K5660) or synthetic resin emulsion paint (JIS K5663) can be obtained. Furthermore, the use of the color pigment can improve the strength of the topcoat material coating, crack resistance, and blister resistance. The mixing ratio of the color pigment is preferably 1 to 500 parts by weight, more preferably 5 to 200 parts by weight, and even more preferably 10 to 100 parts by weight, relative to 100 parts by weight of the solid content of the aqueous resin.

[0035] Examples of color pigments include titanium oxide, zinc oxide, alumina, carbon black, graphite, black iron oxide, iron-manganese composite oxide, iron-copper-manganese composite oxide, iron-chromium-cobalt composite oxide, copper-chromium composite oxide, copper-manganese-chromium composite oxide, ferric oxide (red oxide), molybdate orange, permanent red, permanent carmine, anthraquinone red, perylene red, quinacridone red, yellow iron oxide, titanium yellow, fast yellow, benzimidazolone yellow, chrome green, cobalt green, phthalocyanine green, ultramarine blue, Prussian blue, cobalt blue, phthalocyanine blue, quinacridone violet, dioxazine violet, aluminum pigments, and pearl pigments. These can be used alone or in combination of two or more. The average particle size of the color pigment is preferably 10 μm or less, more preferably 1 μm or less, and even more preferably 0.01 to 0.9 μm. By using a color pigment with such an average particle size, the above-mentioned effects can be easily obtained. The average particle size of the color pigment is a value measured by a laser diffraction particle size distribution measuring device.

[0036] The topcoat material contains such color pigments, and the pigment volume concentration is 1 to 50%, preferably 2 to 30%, and more preferably 3 to 25%. By having the pigment volume concentration within the above range, advantageous effects can be obtained in terms of improving the strength of the topcoat material coating, crack resistance, and blister resistance. In addition, the pigment volume concentration in the present invention is the volume percentage of the color pigment contained in the dry coating, and is a value calculated from the weight parts and specific gravity of the resin component and pigment constituting the topcoat material. In addition, the specific gravity of the resin component is 1.

[0037] The topcoat material may contain components other than those mentioned above, such as extender pigments, dyes, aggregates, color particles, matting agents, thickeners, wetting agents, leveling agents, antifreeze agents, film-forming aids, preservatives, antifungal agents, anti-algae agents, antibacterial agents, dispersants, surfactants, defoamers, UV absorbers, light stabilizers, antioxidants, adhesion agents, low-staining agents, hydrophilic agents, water repellents, crosslinking agents, hardeners, hardening accelerators, plasticizers, coupling agents, adsorbents, pH adjusters, catalysts, water, solvents, etc.

[0038] <1st top coat material> In the present invention, the first topcoat material is one that forms a coating with an elongation rate of 20% or more (preferably 25 to 100%, more preferably 25 to 75%) at -10 ° C in addition to the above conditions. This allows the formation of a coating that exhibits excellent performance in terms of crack resistance, blister resistance, etc. The elongation rate of the first topcoat material at -10 ° C is a value measured according to the method specified in the "elongation test" of JIS A6909:2014. The test specimen used for the elongation test is a waterproof multi-layer coating material E main material with a dry film thickness of 1 mm (its single coating meets the elongation rate regulation at -10 ° C specified in JIS A6909:2014) on the surface of which the first topcoat coating is coated and laminated with a dry film thickness of 80 μm.

[0039] The aqueous resin in the first topcoat material desirably contains at least an aromatic monomer (s) as a hard monomer. And, the composition ratio of the (s) component in the aqueous resin in the first topcoat material is desirably greater than the composition ratio of the (s) component in the aqueous resin in the second topcoat material, and more desirably is 5% by weight or more greater than the composition ratio of the (s) component in the aqueous resin in the second topcoat material. By such an embodiment, it is possible to exert a stable effect in terms of the strength, crack resistance, blister resistance, etc. of the topcoat material coating while ensuring weather resistance, etc. The composition ratio of the (s) component is preferably 1 to 40% by weight, more preferably 5 to 38% by weight, and even more preferably 10 to 35% by weight in the total monomers constituting the aqueous resin in the first topcoat material.

[0040] The aqueous resin in the first topcoat material can contain the (t) component and / or the (u) component as a hard monomer other than the (s) component, and it is particularly desirable to contain the (u) component. The composition ratio of the (u) component is preferably 2 to 60% by weight, more preferably 5 to 50% by weight, and even more preferably 10 to 40% by weight, in the total monomers constituting the aqueous resin. By such an embodiment, it is possible to further improve the blister resistance while ensuring weather resistance, crack resistance, etc.

[0041] The Tg of the aqueous resin in the first topcoat material is preferably -30 to 50°C, more preferably -20 to 40°C, even more preferably -15 to 30°C, and particularly preferably -10 to 25°C.

[0042] In the present invention, the pigment volume concentration of the color pigment in the first topcoat material is greater than the pigment volume concentration of the color pigment in the second topcoat material. The pigment volume concentration of the color pigment in the first topcoat material is preferably 2 to 50%, more preferably 3 to 30%, and even more preferably 4 to 25%. By the pigment volume concentration of the color pigment in the first topcoat material satisfying such conditions, advantageous effects can be obtained in terms of improving the strength of the topcoat material coating, crack resistance, and blister resistance.

[0043] It is desirable to set the color tone of the first topcoat material to the same color as the second topcoat material. This will improve the finish of the topcoat material coating. The color pigment in the first topcoat material can be the same as the color pigment in the second topcoat material.

[0044] <Second top coat material> In the present invention, in addition to the above conditions, the second topcoat material is one that forms a coating whose elongation rate at -10 ° C is smaller than that of the first topcoat material at -10 ° C. The elongation rate of the second topcoat material at -10 ° C is preferably 30% or less, more preferably 1 to 20%, even more preferably 2 to 19%, and particularly preferably 3 to 18%. In the present invention, by using such a second topcoat material, a coating that exhibits excellent performance in terms of blister resistance, stain resistance, etc. can be formed. The elongation rate of the second topcoat material at -10 ° C. is a value measured according to the method specified in the "elongation test" of JIS A6909:2014. The test specimen used for the elongation test is a waterproof multi-layer coating material E main material with a dry film thickness of 1 mm (its single coating meets the elongation rate regulation at -10 ° C. specified in JIS A6909:2014) on the surface of which the second topcoat coating is coated and laminated with a dry film thickness of 80 μm.

[0045] The aqueous resin in the second topcoat material may contain an aromatic monomer (s) as a hard monomer. The composition ratio of the (s) component is preferably 40% by weight or less, more preferably 1 to 35% by weight, even more preferably 3 to 30% by weight, and particularly preferably 5 to 25% by weight, in the total monomers constituting the aqueous resin in the second topcoat material. In addition, the composition ratio of the (s) component in the aqueous resin in the second topcoat material is smaller than the composition ratio of the (s) component in the aqueous resin in the first topcoat material, and is preferably 5% by weight or more smaller than the composition ratio of the (s) component in the aqueous resin in the first topcoat material. By such an embodiment, it is possible to exert a more stable effect in terms of the strength, crack resistance, and blister resistance of the topcoat material coating while ensuring weather resistance, etc.

[0046] The aqueous resin in the second topcoat material can contain the (t) component and / or the (u) component as a hard monomer other than the (s) component, and it is particularly desirable to contain the (t) component. The composition ratio of the (t) component is preferably 2 to 60% by weight, more preferably 10 to 55% by weight, and even more preferably 15 to 50% by weight, in the total monomers constituting the aqueous resin. In this manner, it is possible to further improve weather resistance, blister resistance, etc. while ensuring stain resistance, crack resistance, etc.

[0047] The Tg of the aqueous resin in the second topcoat material is preferably -10 to 60 ° C, more preferably 0 to 50 ° C, and even more preferably 10 to 40 ° C. In addition, the Tg of the aqueous resin in the second topcoat material is preferably higher than the Tg of the aqueous resin in the first topcoat material, and more preferably 3 ° C or higher (even more preferably 5 ° C or higher) than the Tg of the aqueous resin in the first topcoat material. By such an embodiment, it is possible to exert a more stable effect in terms of crack resistance, blister resistance, and contamination resistance.

[0048] In the present invention, the pigment volume concentration of the color pigment in the second topcoat material is set to be smaller than the pigment volume concentration of the first topcoat material. The pigment volume concentration of the color pigment in the second topcoat material is preferably 1 to 30%, more preferably 2 to 25%, and even more preferably 3 to 20%. By making the pigment volume concentration of the color pigment in the second topcoat material satisfy the above conditions, advantageous effects can be obtained in terms of improving the strength of the topcoat material coating, crack resistance, and blister resistance. In addition, the same type of color pigment as the color pigment in the first topcoat material can be used as the color pigment in the second topcoat material, and thereby the color tone of the second topcoat material can be set to the same color as the first topcoat material.

[0049] The second topcoat can be one that forms a coating with a water contact angle (hereinafter simply referred to as the "contact angle") of 70° or less. This makes the second topcoat coating hydrophilic, further improving stain resistance. To measure the contact angle, a test specimen is prepared by applying the second topcoat to the surface of an aluminum plate that has previously been coated with an epoxy resin sealer so that the dry film thickness is 80 μm, and then drying for 7 days under standard conditions (temperature 23°C, relative humidity 50%). The contact angle is measured with a contact angle meter.

[0050] <Film formation method> In the present invention, the topcoat material (first topcoat material and second topcoat material) is applied (painted) to the elastic coating to form the topcoat material coating. That is, the first topcoat material and the second topcoat material are applied in order to the elastic coating to form the topcoat material coating. The elastic coating may be an existing coating or a new coating.

[0051] In the present invention, it is desirable to apply the first topcoat material, dry the coating, and then apply the second topcoat material. The first topcoat material and the second topcoat material can be the above-mentioned. In the present invention, by forming a laminated coating using such two specific topcoat materials, it is possible to exhibit excellent performance in crack resistance, blister resistance, contamination resistance, etc.

[0052] A known painting tool can be used to apply each topcoat material. For example, a spray, roller, brush, etc. can be used as a painting tool. When applying, each topcoat material can be appropriately diluted as necessary. Drying after application of each topcoat material can be performed at room temperature (preferably 0 to 50 ° C, more preferably 5 to 45 ° C), and can also be heated as necessary.

[0053] The amount of the first and second topcoat materials applied is preferably 0.05 to 0.4 kg / m 2 , more preferably 0.08 to 0.3 kg / m 2The dry film thickness of the first topcoat material and the second topcoat material is preferably 20 to 300 μm, more preferably 30 to 200 μm. This makes it possible to form a coating that exhibits excellent performance in crack resistance, blister resistance, and contamination resistance while taking advantage of the texture of the elastic coating.

[0054] The film thickness ratio of the first topcoat coating to the second topcoat coating {(dry film thickness of the first topcoat coating):(dry film thickness of the second topcoat coating)} is preferably 80:20 to 20:80, more preferably 70:30 to 30:70, and even more preferably 65:35 to 35:65. By being in such an embodiment, it is possible to stably obtain better performance in crack resistance, blister resistance, contamination resistance, etc.

[0055] In the coating method of the present invention, for example, an elastic coating material is first applied to the base surface to form an elastic coating, and then the first topcoat material and the second topcoat material can be applied. In this case, a new coating can be formed on the base surface using the elastic coating material, the first topcoat material, and the second topcoat material. It is desirable to apply the first topcoat material after drying the coating of the elastic coating material (preferably after drying for 2 hours or more, more preferably after drying for 3 hours to 10 days), and it is desirable to apply the second topcoat material after drying the coating of the first topcoat material (preferably after drying for 1 hour or more, more preferably after drying for 2 hours or more).

[0056] <Topcoat material set> In the present invention, the above-mentioned first and second topcoat materials can be used as a topcoat material set consisting of these two types. That is, the above-mentioned first and second topcoat materials can be used as a topcoat material set for forming a topcoat material film on an elastic coating.

[0057] <Covering material set> Furthermore, in the present invention, the above-mentioned elastic coating material, the first topcoat material, and the second topcoat material can be used as a coating material set consisting of these three types. That is, the above-mentioned elastic coating material, the first topcoat material, and the second topcoat material can be used as a coating material set for forming a multi-layer coating (laminated coating) on ​​the base surface.

[0058] In such a case, the laminated coating (i) formed by the elastic coating material and the first topcoat material is one that satisfies an elongation rate of 20% or more (preferably 25 to 100%, more preferably 25 to 75%) at -10 ° C., and the laminated coating (ii) formed by the elastic coating material and the second topcoat material is smaller than the elongation rate of the laminated coating (i) at -10 ° C. (furthermore, the elongation rate at -10 ° C. is preferably 30% or less, more preferably 1 to 20%, even more preferably 2 to 19%, particularly preferably 3 to 18%). It is desirable to use a combination of three materials (a combination of an elastic coating material, a first topcoat material, and a second topcoat material). This allows the effects of the present invention to be fully exerted. EXAMPLES

[0059] The following examples will clarify the features of the present invention.

[0060] The following elastic coating materials and topcoat materials were prepared. Elastic covering material a Waterproof multi-layer coating material E that complies with JIS A6909:2014. Main material: {acrylic resin emulsion (Tg-28℃, solid content 50% by weight), titanium dioxide (average particle size 0.3μm, specific gravity 4.2), heavy calcium carbonate (average particle size 12μm, specific gravity 2.6), etc.}. Single film has an elongation rate of 38% at -10℃.

[0061] ·Top coating material a A mixture of 200 parts by weight of water-based resin a {emulsion polymer of styrene, tert-butyl methacrylate, methyl methacrylate, 2-ethylhexyl acrylate, and methacrylic acid (weight ratio 25:20:15:38:2), Tg 12°C, solid content 50% by weight}, 75 parts by weight of titanium oxide (average particle size 0.3 μm, specific gravity 4.2), and other additives (film-forming agent, antifreeze agent, dispersant, thickener, defoamer, water). Pigment volume concentration (hereinafter referred to as "PVC") 15%. Elongation rate is 35% at -10℃.

[0062] ·Top coating material b A mixture of 200 parts by weight of water-based resin b {emulsion polymer of styrene, cyclohexyl methacrylate, methyl methacrylate, 2-ethylhexyl acrylate, and methacrylic acid (weight ratio 10:38:22:28:2), Tg 26°C, solid content 50% by weight}, 58 parts by weight of titanium oxide (same as above), and other additives (film-forming agent, antifreeze agent, dispersant, thickener, defoamer, water). PVC 12%. Elongation rate is 15% at -10℃.

[0063] ·Top coating material c A mixture of 200 parts by weight of water-based resin c {emulsion polymer of styrene, tert-butyl methacrylate, methyl methacrylate, 2-ethylhexyl acrylate, and methacrylic acid (weight ratio 8:20:32:38:2), Tg 13℃, solid content 50% by weight}, 70 parts by weight of titanium oxide (same as above), and other additives (film-forming agent, antifreeze agent, dispersant, thickener, defoamer, water). PVC 14%. Elongation rate is 33% at -10℃.

[0064] ·Top coating material d A mixture of 200 parts by weight of aqueous resin d {an emulsion polymer of cyclohexyl methacrylate, methyl methacrylate, 2-ethylhexyl acrylate, and methacrylic acid (weight ratio 38:32:28:2), Tg 27°C, solid content 50% by weight}, 58 parts by weight of titanium oxide (same as above), and other additives (film-forming agent, antifreeze agent, dispersant, thickener, defoamer, water). PVC 12%. Elongation rate at -10℃ is 16%.

[0065] ·Top coating material e A mixture of 200 parts by weight of water-based resin e {emulsion polymer of styrene, cyclohexyl methacrylate, tert-butyl methacrylate, methyl methacrylate, 2-ethylhexyl acrylate, and methacrylic acid (weight ratio 25:20:4:13:36:2), Tg 13℃, solid content 50% by weight}, 70 parts by weight of titanium oxide (same as above), and other additives (film-forming agent, antifreeze agent, dispersant, thickener, defoamer, water). PVC 14%. Elongation rate is 33% at -10℃.

[0066] ·Top coating material f A mixture of 200 parts by weight of water-based resin f {emulsion polymer of styrene, tert-butyl methacrylate, methyl methacrylate, 2-ethylhexyl acrylate, and methacrylic acid (weight ratio 18:25:15:40:2), Tg 9°C, solid content 50% by weight}, 92 parts by weight of titanium oxide (same as above), and other additives (film-forming agent, antifreeze agent, dispersant, thickener, defoamer, water). PVC 18%. Elongation rate is 34% at -10℃.

[0067] ·Top coating material g A mixture of 200 parts by weight of water-based resin g {emulsion polymer of styrene, tert-butyl methacrylate, methyl methacrylate, 2-ethylhexyl acrylate, and methacrylic acid (weight ratio 32:20:8:38:2), Tg 12°C, solid content 50% by weight}, 80 parts by weight of titanium oxide (same as above), and other additives (film-forming agent, antifreeze agent, dispersant, thickener, defoamer, water). PVC 16%. Elongation rate is 34% at -10℃.

[0068] ·Top coating material h A mixture of 200 parts by weight of water-based resin h {emulsion polymer of styrene, cyclohexyl methacrylate, methyl methacrylate, 2-ethylhexyl acrylate, and methacrylic acid (weight ratio 5:30:33:30:2), Tg 24°C, solid content 50% by weight}, 48 parts by weight of titanium oxide (same as above), and other additives (film-forming agent, antifreeze agent, dispersant, thickener, defoamer, water). PVC 10%. Elongation rate is 18% at -10℃.

[0069] ·Top coating material i A mixture of 200 parts by weight of water-based resin i {emulsion polymer of styrene, cyclohexyl methacrylate, methyl methacrylate, 2-ethylhexyl acrylate, and methacrylic acid (weight ratio 13:38:20:27:2), Tg 28°C, solid content 50% by weight}, 48 parts by weight of titanium oxide (same as above), and other additives (film-forming agent, antifreeze agent, dispersant, thickener, defoamer, water). PVC 10%. Elongation rate at -10℃ is 16%.

[0070] ·Top coating material J A mixture of 200 parts by weight of water-based resin b (same as above), 53 parts by weight of titanium oxide (same as above), and other additives (film-forming agent, antifreeze agent, dispersant, thickener, defoamer, water). PVC 11%. Elongation rate at -10℃ is 16%.

[0071] ·Top coating material A mixture of 180 parts by weight of water-based resin b (same as above), 20 parts by weight of water-based resin a (same as above), 53 parts by weight of titanium oxide (same as above), and other additives (film-forming agent, antifreeze agent, dispersant, thickener, defoamer, water). PVC 11%. Elongation rate is 18% at -10℃.

[0072] ·Top coating material A mixture of 200 parts by weight of water-based resin {emulsion polymer of styrene, cyclohexyl methacrylate, methyl methacrylate, 2-ethylhexyl acrylate, and methacrylic acid (weight ratio 4:34:25:35:2), Tg 13℃, solid content 50% by weight}, 80 parts by weight of titanium oxide (same as above), and other additives (film-forming agent, antifreeze agent, dispersant, thickener, defoamer, water). PVC 16%. Elongation rate is 33% at -10℃.

[0073] ·Top coating material m A mixture of 200 parts by weight of water-based resin (same as above), 70 parts by weight of titanium oxide (same as above), and other additives (film-forming agent, antifreeze agent, dispersant, thickener, defoamer, water). PVC 14%. Elongation rate is 34% at -10℃.

[0074] ·Top coating material A mixture of 200 parts by weight of water-based resin b (same as above), 70 parts by weight of titanium oxide (same as above), and other additives (film-forming agent, antifreeze agent, dispersant, thickener, defoamer, water). PVC 14%. Elongation rate at -10℃ is 14%.

[0075] In addition, the elongation rate at -10 ° C. in each topcoat material is a measured value for the laminated coating of the elastic coating material a (dry film thickness 1 mm) and each topcoat material (dry film thickness 80 μm). In addition, all of the topcoat materials a to n form a white coating.

[0076] Example 1 Elastic coating material A was sprayed onto a slate board that had previously been coated with an acrylic resin sealer, and then dried for 24 hours to form an elastic coating (dry film thickness 1.5 mm). Next, topcoat material A was sprayed onto the surface of this elastic coating as the first topcoat material, and after drying for 2 hours, topcoat material B was sprayed onto the surface as the second topcoat material, and then dried and cured for 168 hours. The first and second topcoat coatings were painted so that their dry film thicknesses were 80 μm each. Painting, drying, and curing were all performed under standard conditions (temperature 23°C, relative humidity 50%). The specimens obtained by the above method were subjected to the following tests.

[0077] Test 1 The specimens obtained by the above method were subjected to a total of five cycles of repeated heating and cooling tests, each cycle consisting of 18 hours of water immersion, 3 hours at -20℃, and 3 hours at 50℃, after which the appearance of the coating was checked and the occurrence of defects (blistering, peeling, cracks, etc.) was evaluated. The evaluation was done on a four-point scale (A>B>C>D: poor), with "A" indicating no defects and "D" indicating obvious defects.

[0078] Test 2 The test specimens obtained using the above method were exposed outdoors for three months, and the appearance of the test specimens was observed for changes in surface dirt. The test specimens were then rated on a four-level scale (A>B>C>D: poor), with "A" indicating that the dirt was slight.

[0079] Example 2 Except for using topcoat material c as the first topcoat material and topcoat material d as the second topcoat material, test specimens were prepared in the same manner as in Example 1, and each test was performed.

[0080] Example 3 Except for using topcoat material e as the first topcoat material and topcoat material b as the second topcoat material, test specimens were prepared in the same manner as in Example 1, and each test was performed.

[0081] Example 4 A test specimen was prepared in the same manner as in Example 1, except that the dry film thickness of the first topcoat material (topcoat material a) was 15 μm, and each test was performed.

[0082] Example 5 Except for using topcoat material f as the first topcoat material, test specimens were prepared in the same manner as in Example 1, and each test was carried out.

[0083] Example 6 Except for using topcoat material g as the first topcoat material, test specimens were prepared in the same manner as in Example 1, and each test was carried out.

[0084] Example 7 Except for using topcoat material h as the second topcoat material, test specimens were prepared in the same manner as in Example 1, and each test was carried out.

[0085] Example 8 Except for using topcoat material i as the second topcoat material, test specimens were prepared in the same manner as in Example 1, and each test was carried out.

[0086] Example 9 Except for using topcoat material j as the second topcoat material, test specimens were prepared in the same manner as in Example 1, and each test was performed.

[0087] Example 10 Except for using topcoat material k as the second topcoat material, test specimens were prepared in the same manner as in Example 1, and each test was carried out.

[0088] Example 11 Except for using topcoat material l as the first topcoat material, test specimens were prepared in the same manner as in Example 1, and each test was carried out.

[0089] Comparative Example 1 Except for using topcoat material m as the first topcoat material and topcoat material n as the second topcoat material, test specimens were prepared in the same manner as in Example 1, and each test was performed.

[0090] Comparative Example 2 Test specimens were prepared in the same manner as in Example 1, except that topcoat material b was used as the first topcoat material and the second coating material, and each test was performed.

[0091] Comparative Example 3 Test specimens were prepared in the same manner as in Example 1, except that topcoat material m was used as both the first topcoat material and the second coating material, and each test was carried out.

[0092] The test results are shown in Table 1. The examples showed excellent performance in each test.

[0093] [Table 1]

[0094] Next, the following tests were carried out on Examples 1 to 10. The test results are shown in Table 2.

[0095] Test 3 The specimens obtained by the above method were subjected to a total of 10 cycles of repeated hot and cold tests, each cycle consisting of 18 hours of water immersion, 3 hours of rest at -20℃, and 3 hours of rest at 50℃, after which the appearance of the coating was checked and the occurrence of defects (blistering, peeling, cracks, etc.) was evaluated. The evaluation was done on a four-level scale (A>B>C>D: poor), with "A" indicating no defects and "D" indicating obvious defects.

[0096] Test 4 The specimens obtained by the above method were subjected to an accelerated weather resistance test using an Eye Super UV Tester (manufactured by Iwasaki Electric Co., Ltd.) as an accelerated weather resistance tester, with 30 cycles of 6 hours of light exposure and 2 hours of condensation (total 8 hours), after which the appearance of the coating was checked and the occurrence of defects (blistering, peeling, cracks, etc.) was evaluated. The evaluation was done on a 4-point scale (A>B>C>D: poor), with "A" indicating no defects and "D" indicating obvious defects.

[0097] Test 5 In the above Test 4, the gloss retention was calculated from the gloss values ​​before and after the accelerated test. The evaluation was as follows: gloss retention of 90% or more was "A", 80% or more but less than 90% was "B", 70% or more but less than 80% was "C", and less than 70% was "D".

[0098] [Table 2]

Claims

1. A coating method for forming a topcoat coating by applying a first topcoat material and a second topcoat material to an elastic coating in sequence, The first topcoat material contains an aqueous resin and a coloring pigment, and the pigment volume concentration is 4 to 25%, The second topcoat material contains an aqueous resin and a coloring pigment, and the pigment volume concentration is 3 to 20%, The pigment volume concentration of the first topcoat material is greater than the pigment volume concentration of the second topcoat material, The first topcoat material forms a coating having an elongation rate of 20% or more at -10 ° C., The second topcoat material forms a coating having an elongation rate at -10 ° C. that is smaller than the elongation rate at -10 ° C. of the first topcoat material. A method for forming a coating comprising the steps of:

2. A topcoat material set for forming a topcoat material film by applying a first topcoat material and a second topcoat material to an elastic coating in sequence, The topcoat material set comprises a first topcoat material and a second topcoat material, The first topcoat material contains an aqueous resin and a coloring pigment, and the pigment volume concentration is 4 to 25%, The second topcoat material contains an aqueous resin and a coloring pigment, and the pigment volume concentration is 3 to 20%, The pigment volume concentration of the first topcoat material is greater than the pigment volume concentration of the second topcoat material, The first topcoat material forms a coating having an elongation rate of 20% or more at -10 ° C., The second topcoat material forms a coating having an elongation rate at -10 ° C. that is smaller than the elongation rate at -10 ° C. of the first topcoat material. A topcoat material set characterized by the above.

Citation Information

Patent Citations

  • Coating composition

    JP1987205169A

  • Method for forming emulsion coating film

    JP1994093226A

  • Active energy ray-curing resin composition and coating film formation using the same

    JP1999035846A

  • Cyclohexyl acrylate water-based resin dispersion composition

    JP2003096261A